Method for producing manganese-containing pyrochlore oxide powder

JP2024165458APending Publication Date: 2024-11-28DOWA HOLDINGS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023081677
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Benefits of technology

【0009】 本発明によれば、マンガンを含有するパイロクロア酸化物粉体の製造において、原料金属塩の仕込み濃度を、ラボ実験で従来一般的に実施されている仕込み濃度よりも大幅に増大させることができ、かつ不純物相の混在を防止することができる。マンガンの含有は高価なルテニウムの節約につながり、不純物相の混在防止は当該粉体を触媒に用いた二次電池等の装置の性能向上に有利となる。したがって本発明は、マンガンを含有するパイロクロア酸化物粉体の工業的普及に資するものである。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165458000001_ABST
    Figure 2024165458000001_ABST
Patent Text Reader

Abstract

To provide a method for producing manganese-containing pyrochlore oxide powder capable of remarkably suppressing the formation of an impurity phase when the preparation concentration of raw material metal salt is increased.SOLUTION: A method for producing a manganese-containing pyrochlore oxide powder comprises: a first raw material mixing step in which a bismuth-containing salt and a ruthenium-containing salt are mixed in an aqueous solvent; a first pH adjustment step in which an alkali is added to adjust the pH of the liquid within a range of 4.0 or less; a first raw material mixing step in which a manganese-containing salt is mixed; a second pH adjustment step in which an alkali is added to raise the pH to 10.0 or more; an oxidation step in which a solid reaction product is formed while oxygen is supplied to the liquid; a dry solidification step in which the reaction product is dry-solidified to obtain a precursor material; and a calcination step in which the precursor material is calcined to synthesize an oxide powder composed of particles having a crystal structure of a bismuth-ruthenium-oxygen type pyrochlore oxide.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] In this specification, pyrochlore oxides having a crystal structure of bismuth (Bi)-ruthenium (Ru)-oxygen (O) type pyrochlore oxide and containing bismuth and ruthenium, or bismuth, ruthenium and manganese (Mn) as their constituent metal elements, are referred to as "BRO oxides". Among BRO oxides, pyrochlore oxides that contain manganese in particular are referred to as "MBRO oxides". The present invention relates to a method for producing MBRO oxide powder. [Background technology]

[0002] BRO oxides are expected to be used as cathode catalysts in air secondary batteries, hydrogen production processes by water electrolysis, etc. Among them, MBRO oxides containing manganese are considered to have a structure in which a part of the ruthenium sites in BRO oxide is replaced by manganese, and since this can save expensive ruthenium, it is considered promising for the industrial spread of devices using pyrochlore oxide catalysts.

[0003] Patent Document 1 describes a manganese-containing MBRO oxide catalyst (claim 1). It is said that the inclusion of manganese improves catalytic activity. As a method for producing the MBRO oxide, a method is disclosed in which an aqueous NaOH solution is added to an aqueous solution containing raw metal salts at a predetermined ratio, and the solution is stirred for 24 hours while aerating oxygen at 75°C to obtain an oxidation reaction product, which is then dried, calcined at 600°C, suction filtered using distilled water, and then dried (paragraphs 0027 and 0041). In this specification, the mixed amount (mol / L) of raw metals per 1L of liquid medium of the raw material-containing liquid (excluding the addition of an alkaline aqueous solution) to be used in the oxidation reaction is referred to as the "feed concentration". According to the disclosure of Patent Document 1, the feed concentration of raw metal salts is approximately 0.007 mol / L for both bismuth and ruthenium (paragraph 0027). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2020 / 153401 Summary of the Invention [Problem to be solved by the invention]

[0005] When mass-producing MBRO oxides on an industrial scale, it is extremely important to ensure productivity by increasing the concentration of raw metal salt per batch in a reaction tank for generating bismuth-, ruthenium-, and manganese-containing substances (mainly hydroxides and oxyhydroxides) that are the source of the precursor substances to be calcined by a wet reaction process. For example, the concentration of metal salt in the laboratory experiment disclosed in Patent Document 1 is about 0.007 mol / L, but if one tries to ensure a sufficient production volume per batch in a reaction tank at a mass production site with this concentration, the amount of solution required becomes enormous, and it is not easy to carry out on an industrial scale. Considering the productivity at a mass production site, it is desirable to ensure a concentration of at least 10 times that of the example of the laboratory experiment, and if possible, to carry out the process at a concentration of about 50 times or more.

[0006] When the concentration of the raw metal salt is increased, the amount of alkali added must be increased accordingly. In order to perform neutralization uniformly, it is desirable to shorten the time required for adding the alkali as much as possible, but if a large amount of alkali is added to an aqueous solvent, the liquid temperature rises rapidly due to the heat of neutralization, and if the cooling does not keep up, it is likely to become dangerous, such as bumping. In order to prevent this, it is necessary to reduce the rate of addition of the alkali so that the rate of generation of the heat of neutralization does not exceed the cooling capacity of the device. However, according to the study by the inventors, in the production of MBRO oxide, a problem occurred in that when the rate of addition of the alkali is reduced, the MBRO oxide after firing is likely to contain an impurity phase mainly composed of bismuth-manganese composite oxide. The presence of the impurity phase may hinder efforts to improve the performance and durability of devices such as secondary batteries using the MBRO oxide as a catalyst. An object of the present invention is to provide a method for producing an MBRO oxide powder in which the formation of impurity phases is significantly suppressed when the charged concentration of raw metal salts is increased. [Means for solving the problem]

[0007] According to the research of the inventors, when an alkali sufficient to react with the total amount of the anions of bismuth-containing salt, ruthenium-containing salt and manganese-containing salt is added continuously over a long period of time to an aqueous solution in which the concentrations of the bismuth-containing salt, ruthenium-containing salt and manganese-containing salt are increased while suppressing excessive heat generation due to neutralization heat, it is considered that a part of the manganese-containing salt co-precipitates with the neutralization product of bismuth and ruthenium, forming a reaction product in which the form of manganese is heterogeneous, and it is presumed that the manganese-containing salt in the product remains as an impurity phase after firing. Therefore, as a result of detailed investigation, the inventors have found that by adopting a two-stage "metal salt mixing-alkali addition" process in which the manganese-containing salt is not added to the initial raw material solution, but a predetermined amount of alkali is added to the aqueous solution in which the bismuth-containing salt and the ruthenium-containing salt are mixed at an addition rate that does not cause boiling, and then the manganese-containing salt is added and the remaining alkali is added, it is possible to synthesize MBRO oxide without forming an impurity phase even when the concentrations of the raw material metal salts are increased.

[0008] The above object can be achieved by the following invention. [1] A method for producing a powder of a "manganese-containing pyrochlore oxide" in which a part of the ruthenium constituting the bismuth-ruthenium-oxygen pyrochlore oxide is replaced with manganese, comprising the steps of: A "first raw material mixing step" of mixing raw materials, bismuth-containing salt and ruthenium-containing salt, with an aqueous solvent to obtain a bismuth-ruthenium-containing liquid; A "first pH adjustment step" of increasing the pH of the liquid obtained in the first raw material mixing step by adding an alkali to obtain a liquid having a pH of 4.0 or less; A "second raw material mixing step" of mixing a manganese-containing salt, which is a raw material, with the liquid obtained in the first pH adjustment step to obtain a bismuth-, ruthenium-, and manganese-containing liquid; A "second pH adjustment step" of adding an alkali to the liquid obtained in the second raw material mixing step to obtain a liquid having a pH of 10.0 or more; An "oxidation step" in which a solid reaction product is formed while supplying oxygen to the liquid obtained in the second pH adjustment step; a "drying step" of recovering the reaction product and then drying it to obtain a precursor material; A "calcination step" of synthesizing an oxide powder composed of particles having a crystal structure of a bismuth-ruthenium-oxygen pyrochlore oxide by calcining the precursor material; A method for producing a manganese-containing pyrochlore oxide powder, comprising: [2] The method for producing a manganese-containing pyrochlore oxide powder according to the above item [1], wherein the mixing ratio of the raw materials to be mixed into the liquid in the first raw material mixing step and the second raw material mixing step is set to a mixing ratio such that the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is 0.05 or more and 0.35 or less. [3] The method for producing a manganese-containing pyrochlore oxide powder according to the above [1] or [2], wherein the mixing ratio of the raw materials to be mixed into the liquid in the first raw material mixing step and the second raw material mixing step is a mixing ratio in which the Bi / (Ru+Mn) atomic ratio, which represents the atomic ratio of bismuth to the total amount of ruthenium and manganese, is 0.700 or more and 0.990 or less. [4] The method for producing a manganese-containing pyrochlore oxide powder according to any one of the above [1] to [3], wherein the liquid subjected to the oxidation step has a bismuth content of 0.3 mol / L or more per 1 L of liquid medium excluding the added alkaline aqueous solution. [5] The method for producing a manganese-containing pyrochlore oxide powder according to any one of the above [1] to [4], wherein the time required for adding the alkali in the second pH adjustment step is within 300 seconds. Effect of the Invention

[0009] According to the present invention, in the production of manganese-containing pyrochlore oxide powder, the concentration of raw metal salt can be significantly increased compared to the concentration generally used in conventional laboratory experiments, and the inclusion of impurity phases can be prevented. The inclusion of manganese leads to saving expensive ruthenium, and the prevention of the inclusion of impurity phases is advantageous for improving the performance of devices such as secondary batteries that use the powder as a catalyst. Therefore, the present invention contributes to the industrial spread of manganese-containing pyrochlore oxide powder. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 illustrates the X-ray diffraction patterns for the MBRO oxide powders obtained in each example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Pyrochlore oxide] The typical formula for pyrochlore oxides is A2B2O xwhere x is 7 or a value close to it. "Bismuth-ruthenium-oxygen pyrochlore oxide" means a pyrochlore oxide in which the A site is bismuth (Bi) and the B site is ruthenium (Ru). The manganese-containing pyrochlore oxide (MBRO oxide) targeted in the present invention has a crystal structure in which diffraction peaks from each crystal plane of "bismuth-ruthenium-oxygen pyrochlore oxide" are observed in the X-ray diffraction pattern. MBRO oxides containing manganese as a metal element are generally considered to have an atomic arrangement in which a part of the ruthenium atom occupying the B site is replaced by a manganese atom. In addition, an atomic arrangement in which an atom other than bismuth, ruthenium, or manganese replaces a part of the bismuth atom occupying the A site or a part of the ruthenium atom or manganese atom occupying the B site, or enters an interstitial position, is also permitted as long as it does not impair the effects of the present invention. For example, sodium (Na) atoms, which may be introduced into the liquid during the manufacturing process, may exist in the crystal lattice by replacing some of the bismuth atoms occupying the A site or by entering interstitial positions. Note that, since manganese exists in the crystal lattice in the MBRO oxide targeted by the present invention, some variation in the crystal plane spacing may occur compared to a pure "bismuth-ruthenium-oxygen pyrochlore oxide."

[0012] [MBRO oxide powder manufacturing process] In the present invention, MBRO oxide powder is produced by a production process including, in the above order, a first raw material mixing step, a first pH adjustment step, a second raw material mixing step, a second pH adjustment step, an oxidation step, a drying step, and a calcination step.

[0013] (raw material) As raw materials, a bismuth-containing salt (e.g., bismuth (III) nitrate hydrate), a ruthenium-containing salt (e.g., ruthenium (III) chloride hydrate), and a manganese-containing salt (e.g., manganese (II) nitrate hydrate) are prepared. In the conventional method for producing MBRO oxide, all of these raw materials are generally mixed in an aqueous solvent to prepare an initial raw material solution. However, it has become clear that this method makes it easier to synthesize MBRO oxide containing impurity phases when the raw material concentration is significantly increased. In the present invention, a multi-stage metal salt mixing method is adopted in which the bismuth-containing salt and the ruthenium-containing salt are first mixed in an aqueous solvent to prepare an initial raw material solution, and the manganese-containing salt is mixed in a later process. An aqueous solvent is a liquid medium whose main component is water (i.e., the mass ratio of water is 50% or more).

[0014] The quantitative ratio of the bismuth-containing salt, ruthenium-containing salt, and manganese-containing salt used is a blending ratio that synthesizes a bismuth-ruthenium-oxygen pyrochlore oxide having a composition in which a portion of the ruthenium is replaced by manganese.

[0015] Specifically, the Mn / (Ru+Mn) atomic ratio, which represents the atomic ratio of manganese to the total amount of ruthenium and manganese, is preferably 0.05 or more. This provides a significant economic benefit of saving expensive ruthenium. It is more effective for the Mn / (Ru+Mn) atomic ratio to be 0.20 or more, and even more effective for the Mn / (Ru+Mn) atomic ratio to be 0.25 or more. It is preferable to adjust the Mn / (Ru+Mn) atomic ratio to be within the range of 0.35 or less.

[0016] In addition, the atomic ratio of Bi / (Ru+Mn), which represents the atomic ratio of bismuth to the total amount of ruthenium and manganese, is preferably 0.990 or less. By slightly reducing the atomic ratio of bismuth to the total number of atoms of ruthenium and manganese, the effect of preventing the inclusion of impurity phases containing bismuth is enhanced. However, if the atomic ratio of Bi / (Ru+Mn) is too low, the amount of surplus ruthenium increases, which may adversely affect the economic efficiency. Usually, the atomic ratio of Bi / (Ru+Mn) may be set in the range of 0.700 or more, and may be controlled in the range of 0.940 or more.

[0017] [First raw material mixing process] The raw materials, bismuth-containing salt and ruthenium-containing salt, are mixed in an aqueous solvent to prepare an initial raw material solution, which is a bismuth-ruthenium-containing liquid. At this stage, the manganese-containing salt is not mixed in yet. Since the solubility of the bismuth-containing salt and the ruthenium-containing salt in water is low, when they are mixed in water, most of them do not dissolve and remain in the water as a solid, resulting in a slurry-like liquid. Therefore, in the present invention, it is preferable to use an aqueous solvent in which an organic substance that serves as a dispersant is dissolved as a secondary component other than water. An example of the dispersant is tetra-n-propylammonium bromide.

[0018] In this specification, the amount (mol / L) of the raw material mixed per 1 L of the liquid medium of the raw material-containing liquid (excluding the addition of the alkaline aqueous solution) to be used in the oxidation step is called the "feed concentration" of the raw material. The amount of the raw material mixed in the first raw material mixing step is preferably set so that the feed concentration of bismuth, that is, the bismuth content as the number of atoms per 1 L of the liquid medium of the liquid (excluding the addition of the alkaline aqueous solution) to be used in the oxidation step described below, is 0.3 mol / L or more from the viewpoint of productivity. It is more effective to set the feed concentration of bismuth to 0.5 mol / L or more. If the feed concentration of the raw material metal becomes too high, the amount of alkali added to the reaction tank increases, and the cooling load of the equipment increases and the rate of alkali addition is greatly restricted in order to suppress the heat generation at that time. The amount of the raw material metal mixed in this step is preferably set so that the feed concentration of bismuth is 1.0 mol / L or less, and may be controlled so that it is 0.8 mol / L or less. When a dispersant is used, for example tetra-n-propylammonium bromide, the dispersant concentration per 1 L of liquid medium in the raw material-containing liquid (not including the added alkaline aqueous solution) to be subjected to the oxidation step may be adjusted to a range of 0.05 to 0.50 mol / L.

[0019] An aqueous solvent is placed in a reaction tank, and a predetermined amount of bismuth-containing salt and ruthenium-containing salt are mixed into the aqueous solvent to produce a bismuth-ruthenium-containing liquid. A dispersant is also mixed as necessary. This is thoroughly stirred to produce a slurry. Due to the free acid, this liquid (slurry) will be acidic, with a pH of, for example, 0.5 or less, if the bismuth concentration is about 0.6 mol / L.

[0020] [First pH adjustment step] An alkali is added to the bismuth and ruthenium-containing liquid (slurry) obtained in the first raw material mixing step to increase the pH of the liquid. As the alkali, for example, sodium hydroxide can be used. In the first pH adjustment step, the pH of the liquid is increased by adding an alkali to obtain a liquid having a pH of 4.0 or less. In other words, it is necessary to stop adding the alkali before the pH of the liquid exceeds 4.0. The manganese-containing salt added later has different properties from the bismuth-containing salt and the ruthenium-containing salt, and when the pH becomes higher than near the neutral range, it becomes more stable in the state of a solid compound salt than in the state dissociated into ions (dissolved in the liquid), and is more likely to precipitate as a salt. As a result of the investigation, if the pH exceeds 4.0 at this stage, there is a risk of coprecipitation of the manganese-containing salt occurring when an alkali is added in the second pH adjustment step after the addition of the manganese-containing salt. In that case, it becomes difficult to prevent the impurity phase from remaining in the end. In the first pH adjustment step, it is more preferable to obtain a liquid having a pH of 3.0 or less, and even more preferable to obtain a liquid having a pH of 2.0 or less, and it may be controlled to obtain a liquid having a pH of 1.0 or less. However, in order to prevent bumping when the alkali is added in the second pH adjustment step, when the bismuth charge concentration is, for example, about 0.6 mol / L, it is preferable to control the pH to 0.5 or more in the first pH adjustment step. If bumping can be avoided when the alkali is added in the second pH adjustment step by improving the cooling capacity of the reaction apparatus, it is also possible to lower the pH to below 0.5 when the bismuth charge concentration is about 0.6 mol / L. The pH may be adjusted by a method of measuring and monitoring the pH of the liquid at appropriate times, or by adding an appropriate amount of alkali that is determined in advance in a preliminary experiment.

[0021] The amount of alkali added in the first pH adjustment step is, for example, when the concentration of bismuth added is 0.4 to 0.8 mol / L, preferably 40% or more of the amount of alkali required to react with all of the anions supplied from the bismuth-containing salt, the ruthenium-containing salt, and the manganese-containing salt, and may be 50% or more.

[0022] (Example of a method for calculating the amount of alkali required to react with all of the anions provided by the bismuth-containing salt, the ruthenium-containing salt, and the manganese-containing salt) For example, if NaOH is used as the alkali, in a liquid containing 0.95 mol of Bi(NO3)3·5H2O, 0.7 mol of RuCl3·nH2O, and 0.3 mol of Mn(NO3)2·6H2O, the Na ions, NO3 ions, and Cl ions are all monovalent, so the amount of alkali required to react with all of the anions supplied by the bismuth-containing salt, ruthenium-containing salt, and manganese-containing salt is 3×0.95+3×0.7+2×0.3=5.55 mol.

[0023] The temperature of the liquid (slurry) when the alkali is added is preferably 50 to 99°C. The alkali can be added in the first pH adjustment step while stirring the liquid, at an addition rate that does not cause the liquid temperature to exceed the above-mentioned temperature range according to the cooling capacity of the reaction vessel. The alkali can be added by intermittent addition, continuous addition, or, if the cooling capacity of the reaction vessel allows, a method of adding the entire amount at once. Usually, the alkali addition can be completed within the required time of one hour, but depending on the cooling capacity of the reaction vessel, it may be added over a longer period of time.

[0024] In this specification, the pH is measured using a pH meter calibrated with an appropriate buffer solution according to the pH range to be measured based on JIS Z8802: 2011. The pH value described in this specification is the measurement value indicated by the pH meter compensated by a temperature compensation electrode, which is directly read under the temperature conditions of the liquid. In the examples described later, pH was measured using a HORIBA portable pH / ORP / ion meter D-73 and a pH measurement electrode 9615S-10D.

[0025] [Second raw material mixing process] The manganese-containing salt, which is a raw material, is mixed with the liquid whose pH has been adjusted to the above-mentioned predetermined range in the first pH adjustment step to obtain a liquid containing bismuth, ruthenium, and manganese. The manganese-containing salt may be added in a state of being dissolved in an aqueous solvent in advance.

[0026] [Second pH adjustment process] Next, an alkali is added to the liquid while stirring it. The same kind of substance (e.g., sodium hydroxide) as that used in the first pH adjustment step can be used as the alkaline substance. In the second pH adjustment step, the pH of the liquid is adjusted to 10.0 or more by adding an alkali. If a liquid with a lower pH is subjected to the oxidation step, the effect of significantly preventing the generation of an impurity phase may not be fully exerted. It is more preferable to adjust the pH to 11.0 or more, and even more preferable to adjust the pH to 11.5 or more.

[0027] In the second pH adjustment step, the amount of alkali added is preferably equal to or more than the amount obtained by subtracting the amount of alkali added in the first pH adjustment step from the amount of alkali (described above) required to react with all the anions supplied from all the metal salts (bismuth-containing salt, ruthenium-containing salt, manganese-containing salt) mixed in the liquid. That is, it is preferable to ensure that the ratio of the total amount of alkali added in the first pH adjustment step and the amount of alkali required to react with all the anions supplied from the raw metal salts (hereinafter, this may be referred to as the "anion equivalent ratio") is 1.00 or more. It is more preferable to ensure that the anion equivalent ratio is 1.02 or more. However, since excessive alkali addition is uneconomical, the amount of alkali added may be set in a range where the anion equivalent ratio is 1.10 or less. In the second pH adjustment step, the bismuth-containing salt and a part of the ruthenium-containing salt have already finished reacting with the alkali, and the addition of the alkali starts in the low pH range (pH 4.0 or less) where the manganese-containing salt is stable as an ion, so that all of the manganese ions present in the liquid can be reacted with the alkali quickly. Therefore, precipitation as a manganese-containing salt is avoided, and all of the anion components supplied from the raw metal salt can be dissolved in the liquid as a water-soluble alkali salt.

[0028] In the second pH adjustment step, the liquid temperature is preferably maintained at 50 to 99° C. The alkali addition rate in the second pH adjustment step is preferably as fast as possible depending on the temperature adjustment capacity of the reaction vessel, which leads to improved productivity. For example, the alkali addition time is preferably within 300 seconds, and it is more preferable to add the alkali all at once (for example, within 30 seconds).

[0029] [Oxidation process] Next, the liquid (slurry) obtained in the second pH adjustment step is stirred continuously while oxygen is being supplied to form a solid reaction product. The liquid temperature is preferably maintained at 50 to 99°C. Oxygen can be supplied by blowing (bubbling) oxygen gas or air into the liquid. The stirring time under oxygen supply is preferably 1 to 36 hours. In this way, the wet oxidation reaction is progressed to form a solid reaction product containing bismuth, ruthenium, and manganese. It is believed that this reaction product is mainly composed of oxyhydroxides of the above metals.

[0030] [Drying process] The reaction product is dried. It is efficient to carry out a pretreatment to remove as much liquid component as possible from the liquid (reaction liquid) after the oxidation step, and then dry out the solid content (reaction product). For example, the pretreatment may involve leaving the reaction liquid for a predetermined time and then removing the supernatant. The leaving time is preferably, for example, 24 hours or more. In this case, the amount of the supernatant removed is preferably 70% or more by volume of the reaction liquid after the oxidation step. If necessary, a centrifuge may be used to promote sedimentation of the reaction product.

[0031] Drying can be performed by exposing the reaction product (solid content) to which the liquid component is attached to air at, for example, 80 to 140°C. In this way, a precursor substance is formed. Thereafter, if necessary, a crushing treatment or an additional drying treatment at a temperature of, for example, about 180 to 250°C can be performed to remove chemically adsorbed water. In addition, the particle size distribution of the powder to be subjected to the firing step can be optimized, for example, by using a sieve.

[0032] [Firing process] The obtained precursor material is fired by heating in an oxidizing gas atmosphere to synthesize an oxide powder composed of particles having a crystal structure of a bismuth-ruthenium-oxygen pyrochlore oxide. In the present invention, a precursor material containing manganese is used, so that a pyrochlore oxide containing manganese (MBRO oxide) is obtained. In addition, since the precursor material is produced through the above-mentioned wet process that can avoid the inclusion of unnecessary metal salts, this process can produce an MBRO oxide powder with very little impurity phase. The firing temperature is preferably 400 to 700°C, and the firing time (retention time in the above temperature range) is preferably 0.5 to 3.0 hours. Air under atmospheric pressure can be used as the above-mentioned oxidizing gas atmosphere.

[0033] The MBRO oxide powder obtained by calcination can be subjected to a crushing process or a process for adjusting the particle size distribution using a sieve, if necessary. In addition, the powder obtained can be subjected to a process for removing water-soluble adhering salts by a method of stirring the powder obtained in water and then recovering the solid components. In this manner, by using a method in which the charged concentrations of the raw materials are increased, it is possible to obtain MBRO oxide powder in which the generation of impurity phases is significantly suppressed. EXAMPLES

[0034] [Control Example 1] Here, we present an example in which the concentrations of the raw materials were increased to the extent that it was known that MBRO oxides with fewer impurity phases could be obtained without applying the two-stage "metal salt mixing-alkali addition" process according to the present invention, but the concentrations were significantly higher than those in conventional laboratory experiments.

[0035] (Preparation of liquid to be used in oxidation process) A 1L separable beaker (manufactured by Asahi Seisakusho) was set on a mantle heater (manufactured by Asahi Seisakusho), and 150g of pure water was added and heated to 75°C while stirring. An anchor blade was used for stirring, and the stirring speed was set to 300 rpm. 0.0521 mol (14.15g) of tetra-n-propylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 50g of pure water and added while stirring. Furthermore, 0.2083 mol (101.5g) of bismuth (III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.1535 mol (34.36g) of ruthenium (III) chloride n-hydrate (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) were prepared as a uniformly turbid slurry in 200g of pure water and added. Furthermore, 0.0658 mol (18.88 g) of manganese (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 100 g of pure water and added. The total amount of pure water used was 700 g.

[0036] After each substance was added, the mixture was stirred at 75°C for 1 hour. Since bismuth(III) nitrate pentahydrate and ruthenium(III) chloride n-hydrate have low solubility in water, they could not be dissolved completely even at 75°C, and a slurry-like raw solution was obtained. The pH of the raw solution after stirring was approximately 0.3. The Bi / (Ru+Mn) atomic ratio in this raw solution was 0.950, and the Mn / (Ru+Mn) atomic ratio was 0.30. The concentration of the raw metal salts was 0.2976 mol / L in terms of the bismuth content as the number of atoms. This concentration was calculated without considering the volume of the salt, and was calculated using the volume of the pure water used, 0.7 L. Specifically, the concentration of bismuth added = molar amount of bismuth 0.2083 mol / volume of pure water 0.7 L = 0.2976 mol / L.

[0037] A sodium hydroxide solution with a concentration of 18 mol / L was prepared and added to the above raw material solution. The amount of sodium hydroxide added was set to an amount that would supply 1.08 times the amount of sodium required to react with the total amount of anions supplied from bismuth (III) nitrate pentahydrate, ruthenium (III) chloride n-hydrate, and manganese (II) nitrate hexahydrate in atomic ratio. Here, the total amount of sodium hydroxide was added over 7.5 minutes. At this time, the liquid temperature rose to over 95°C. Therefore, if the concentration of the raw material metal salts is further increased and sodium hydroxide is added at the same rate as in this example, the liquid temperature will exceed 100°C, and there is a risk of bumping. In Table 1, this alkali addition is shown in the column "first pH adjustment step" for convenience (the same applies to Comparative Examples 1 and 2 below).

[0038] (oxidation process) Next, while blowing pure oxygen gas into the liquid in the reaction vessel, the temperature was maintained at 75°C and stirring was continued for 18 hours to form a solid reaction product. The pure oxygen gas supply rate was set to about 100 mL / min per 1 L of liquid in the reaction vessel, calculated as a gas volume at room temperature and atmospheric pressure.

[0039] (Drying process) After the above stirring, the liquid in the reaction tank (slurry in which the reaction product was suspended) was left to stand for 5 days, the supernatant was removed, and then the liquid was centrifuged to finally remove 70% or more of the supernatant relative to the volume of the "liquid in the reaction tank" and recover the reaction product. The recovered reaction product was dried together with the remaining liquid components by holding them in air at 120°C for 18 hours to form a precursor substance.

[0040] This precursor material was broken into powder and then further dried by being kept in air at 200° C. for 2 hours, and then crushed in a mortar to prepare a precursor material for firing.

[0041] (Firing process) The above precursor material was calcined in air at 600°C for 1 hour to synthesize MBRO oxide.

[0042] The synthesized MBRO oxide was stirred and washed in pure water with a volume of 0.5 L per 100 g of oxide to remove adhering salts, and then the solid matter was recovered by suction filtration and dried in air at 120°C to obtain MBRO oxide powder.

[0043] (X-ray diffraction pattern measurement) The X-ray diffraction pattern of the obtained MBRO oxide powder was measured using an X-ray diffractometer (Rigaku, Ultima IV) under the conditions of Cu-Kα radiation, tube voltage of 40 kV, tube current of 40 mA, measurement step of 0.02 degrees, and scan speed of 0.5 degrees / min. The X-ray diffraction patterns of the MBRO oxide powders obtained in this example and in each of the examples described below are shown in Figure 1. The X-ray diffraction patterns were analyzed by the RIR (Reference Intensity Ratio) method, and no impurity phases containing bismuth or manganese were detected in the MBRO oxide powders obtained in this example.

[0044] (Composition analysis by SEM-EDX) The composition of the obtained MBRO oxide powder was analyzed by SEM (FE-SEM JSM-7200F, manufactured by JEOL Ltd.) and EDX (X-Max20, manufactured by Oxford Instruments). As a result, the Bi / (Ru+Mn) atomic ratio of the MBRO oxide powder obtained in this example was 0.93, and the Mn / (Ru+Mn) atomic ratio was 0.32. Tables 1 and 2 show the production conditions and results (the same applies to each of the following examples).

[0045] [Comparative Example 1] This example is an example in which the charged concentration of the raw metal salt was significantly higher than that of Control Example 1, but the two-stage "metal salt mixing-alkali addition" process according to the present invention was not applied.

[0046] (Preparation of liquid to be used in oxidation process) A 1L separable beaker (manufactured by Asahi Seisakusho) was set on a mantle heater (manufactured by Asahi Seisakusho), and 150g of pure water was added and heated to 75°C while stirring. An anchor blade was used for stirring, and the stirring speed was set to 300 rpm. 0.0521 mol (14.15g) of tetra-n-propylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), a dispersant, was dissolved in 50g of pure water and added while stirring. Furthermore, 0.4166 mol (203.1g) of bismuth (III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.3070 mol (68.72g) of ruthenium (III) chloride n-hydrate (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) were prepared as slurries in which they were uniformly mixed in 200g of pure water and added. Furthermore, 0.1316 mol (37.77 g) of manganese (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 100 g of pure water and added. The total amount of pure water used was 700 g.

[0047] After each substance was added, the mixture was stirred at 75°C for 1 hour. Since bismuth(III) nitrate pentahydrate and ruthenium(III) chloride n-hydrate have low solubility in water, they could not be completely dissolved even at 75°C, and a slurry-like raw solution was obtained. The atomic ratio of Bi / (Ru+Mn) in this raw solution was 0.950, and the atomic ratio of Mn / (Ru+Mn) was 0.30. The concentration of the raw metal salts was 0.5952 mol / L in terms of the bismuth content as the number of atoms. This concentration was calculated without considering the volume of the salt, and was taken as 0.7 L, which is the volume of the pure water used.

[0048] A sodium hydroxide solution with a concentration of 18 mol / L was prepared and added to the above raw material solution. The amount of sodium hydroxide added was set to provide an atomic ratio of 1.04 times the amount of sodium required to react with the total amount of anions provided by bismuth (III) nitrate pentahydrate, ruthenium (III) chloride n-hydrate, and manganese (II) nitrate hexahydrate. The entire amount of sodium hydroxide was added over 30 minutes to prevent excessive temperature rise. The temperature of the solution during the addition of sodium hydroxide was maintained at approximately 75°C using a temperature controller.

[0049] The liquid (slurry) in the reaction tank after the above alkali addition was subjected to the "oxidation step" and subsequent steps described in Comparative Example 1 in the same manner as in Comparative Example 1 to produce MBRO oxide powder. The obtained MBRO oxide powder was subjected to X-ray diffraction pattern measurement and composition analysis by SEM-EDX in the same manner as in Comparative Example 1 (the same applies to each of the following examples). The results of X-ray diffraction measurements showed that the MBRO oxide powder obtained in this study contained Bi-Ru oxide (Bi3Ru3O 11 ), and impurity phases thought to be Bi-Mn oxides were detected. Analysis by the RIR method revealed that the proportion of these impurity phases was approximately 14 mass%. Furthermore, SEM-EDX analysis revealed that the Bi / (Ru+Mn) atomic ratio was 0.97, and the Mn / (Ru+Mn) atomic ratio was 0.33.

[0050] [Comparative Example 2] This example is an example in which the concentration of the raw metal salts was increased further than in Comparative Example 1 above, but the two-stage "metal salt mixing-alkali addition" process according to the present invention was not applied.

[0051] (Preparation of liquid to be used in oxidation process) A 1L separable beaker (manufactured by Asahi Seisakusho) was set on a mantle heater (manufactured by Asahi Seisakusho), and 150g of pure water was added and heated to 75°C while stirring. An anchor blade was used for stirring, and the stirring speed was set to 300 rpm. 0.0521 mol (14.15g) of tetra-n-propylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), a dispersant, was dissolved in 50g of pure water and added while stirring. Furthermore, 0.8333 mol (406.2g) of bismuth (III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.6140 mol (137.4g) of ruthenium (III) chloride n-hydrate (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) were prepared as slurries in which they were uniformly mixed in 200g of pure water and added. Furthermore, 0.2631 moles (75.53 g) of manganese (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 100 g of pure water and added. The total amount of pure water used was 700 g.

[0052] After each substance was added, the mixture was stirred at 75°C for 1 hour. Since bismuth(III) nitrate pentahydrate and ruthenium(III) chloride n-hydrate have low solubility in water, they could not be completely dissolved even at 75°C, and a slurry-like raw solution was obtained. The atomic ratio of Bi / (Ru+Mn) in this raw solution was 0.950, and the atomic ratio of Mn / (Ru+Mn) was 0.30. The concentration of the raw metal salts was 1.190 mol / L in terms of the bismuth content as the number of atoms. This concentration was calculated without considering the volume of the salt, and was 0.7 L, which was the volume of the pure water used.

[0053] A sodium hydroxide solution with a concentration of 18 mol / L was prepared and added to the above raw material solution. The amount of sodium hydroxide added was set to provide an atomic ratio of 1.02 times the amount of sodium required to react with the total amount of anions provided by bismuth (III) nitrate pentahydrate, ruthenium (III) chloride n-hydrate, and manganese (II) nitrate hexahydrate. The total amount of sodium hydroxide was added over 180 minutes to prevent excessive temperature rise. The temperature of the solution during the addition of sodium hydroxide was maintained at approximately 75°C using a temperature controller.

[0054] The liquid (slurry) in the reaction tank after the above-mentioned alkali addition was subjected to the "oxidation step" and subsequent steps described in Comparative Example 1 in the same manner as in Comparative Example 1 to produce MBRO oxide powder. The results of X-ray diffraction measurements showed that the MBRO oxide powder obtained in this study contained Bi-Ru oxide (Bi3Ru3O 11 ), and impurity phases thought to be Bi-Mn oxides were detected. Analysis by the RIR method revealed that the proportion of these impurity phases was approximately 19 mass%. Furthermore, SEM-EDX analysis revealed that the atomic ratio of Bi / (Ru+Mn) was 0.83, and the atomic ratio of Mn / (Ru+Mn) was 0.40. It is believed that the atomic ratios from the SEM-EDX analysis include elements of impurity phases that do not constitute an MBRO crystal lattice, and a large discrepancy was observed between the composition from the SEM-EDX analysis and that of the raw material solution.

[0055] [Comparative Example 3] This is an example in which the two-stage process of "mixing metal salts and adding alkali" according to the present invention was not applied when the concentration of the raw metal salts was significantly higher than that of Control Example 1. However, an attempt was made to apply a method of switching the rate of alkali addition when the pH rose to 2.0.

[0056] (Preparation of liquid to be used in oxidation process) A 1L separable beaker (manufactured by Asahi Seisakusho) was set on a mantle heater (manufactured by Asahi Seisakusho), and 150g of pure water was added and heated to 75°C while stirring. An anchor blade was used for stirring, and the stirring speed was set to 300 rpm. 0.0521 mol (14.15g) of tetra-n-propylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), a dispersant, was dissolved in 50g of pure water and added while stirring. Furthermore, 0.4166 mol (203.1g) of bismuth (III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.3070 mol (68.72g) of ruthenium (III) chloride n-hydrate (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) were prepared as slurries in which they were uniformly mixed in 200g of pure water and added. Furthermore, 0.1316 mol (37.77 g) of manganese (II) nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 100 g of pure water and added. The total amount of pure water used was 700 g.

[0057] After each substance was added, the mixture was stirred at 75°C for 1 hour. Since bismuth(III) nitrate pentahydrate and ruthenium(III) chloride n-hydrate have low solubility in water, they could not be completely dissolved even at 75°C, and a slurry-like raw solution was obtained. The atomic ratio of Bi / (Ru+Mn) in this raw solution was 0.950, and the atomic ratio of Mn / (Ru+Mn) was 0.30. The concentration of the raw metal salts was 0.5952 mol / L in terms of the bismuth content as the number of atoms. This concentration was calculated without considering the volume of the salt, and was taken as 0.7 L, which is the volume of the pure water used.

[0058] A sodium hydroxide solution with a concentration of 18 mol / L was prepared and added to the above raw material solution. The total amount of sodium hydroxide added was set to an amount that was 1.04 times the amount of sodium required to react with the total amount of anions supplied from bismuth (III) nitrate pentahydrate, ruthenium (III) chloride n-hydrate, and manganese (II) nitrate hexahydrate in atomic ratio. Here, while measuring the pH of the solution at appropriate times, sodium hydroxide was added continuously until the pH reached 2.0 without causing excessive temperature rise. The addition took about 30 minutes.

[0059] Next, the remaining amount of sodium hydroxide was added all at once. The time required for the addition was about a few seconds. The pH of the liquid after the addition of sodium hydroxide was confirmed to be 11.5 or higher. The temperature of the liquid was kept below 95°C until the addition of sodium hydroxide was completed using a temperature controller.

[0060] After the addition of sodium hydroxide, the liquid (slurry) in the reaction tank was subjected to the "oxidation step" and subsequent steps described in Comparative Example 1 in the same manner as in Comparative Example 1 to produce MBRO oxide powder. As a result of X-ray diffraction measurement, impurity phases thought to be Bi-Mn oxides were detected in the MBRO oxide powder obtained in this example. As a result of analysis by the RIR method, the proportion of the impurity phase was about 2 mass%. Furthermore, as a result of SEM-EDX analysis, the atomic ratio of Bi / (Ru+Mn) was 0.93, and the atomic ratio of Mn / (Ru+Mn) was 0.34.

[0061] [Example 1] This example is an example in which the two-stage "metal salt mixing-alkali addition" process according to the present invention was applied in a case where the charged concentration of the raw metal salt was significantly higher than that of Control Example 1.

[0062] (First raw material mixing process) A 1L separable beaker (manufactured by Asahi Seisakusho) was set on a mantle heater (manufactured by Asahi Seisakusho), and 150g of pure water was added and heated to 75°C while stirring. An anchor blade was used for stirring, and the stirring speed was set to 300 rpm. 0.0521 mol (14.15g) of tetra-n-propylammonium bromide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 50g of pure water and added while stirring. Furthermore, 0.4166 mol (203.1g) of bismuth (III) nitrate pentahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 0.3070 mol (68.72g) of ruthenium (III) chloride n-hydrate (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) were prepared as a uniformly turbid slurry in 200g of pure water and added. After each substance was added, stirring was performed for 1 hour at a liquid temperature of 75°C. Since bismuth(III) nitrate pentahydrate and ruthenium(III) chloride n-hydrate have low solubility in water, they could not be completely dissolved even at 75°C, and a slurry-like raw solution was obtained. The pH of the raw solution after stirring was approximately 0.2.

[0063] (1st pH adjustment step) A sodium hydroxide solution with a concentration of 18 mol / L was prepared and added to the raw material solution. Here, while measuring the pH of the liquid at appropriate times, sodium hydroxide was continuously added until the pH reached 2.0, without excessively increasing the temperature. The time required for the addition was about 30 minutes. The amount of alkali added to the liquid in this first pH adjustment step was 55% of the amount of alkali required to react with all of the anions supplied from the added bismuth-containing salt, the ruthenium-containing salt, and the manganese-containing salt to be added later. The temperature of the liquid during the addition of sodium hydroxide could be kept at about 75°C by a temperature controller.

[0064] (Second raw material mixing process) Manganese nitrate (II) hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1316 mol (37.77 g) was dissolved in 100 g of pure water to obtain an aqueous manganese nitrate solution. The aqueous manganese nitrate solution was mixed with the liquid whose pH had been adjusted to 2.0 after the first pH adjustment step, and the mixture was stirred at a liquid temperature of 75° C. for 30 minutes.

[0065] (2nd pH adjustment step) Thereafter, an amount of alkali, which is 1.04 times the amount of alkali required to react with all the anions supplied from all the metal salts (the bismuth-containing salt, the ruthenium-containing salt, and the manganese-containing salt) mixed in the liquid, minus the amount of alkali added in the first pH adjustment step, was added to the liquid all at once using an aqueous sodium hydroxide solution with a concentration of 18 mol / L. The time required for the all at once addition is about several seconds. It was confirmed that the pH of the liquid after the addition of sodium hydroxide was completed was 11.5 or higher. The temperature of the liquid was able to be kept below 95°C until the addition of sodium hydroxide was completed by the temperature regulator. The Bi / (Ru+Mn) atomic ratio in this liquid (slurry) was 0.950, and the Mn / (Ru+Mn) atomic ratio was 0.30. The concentration of the raw metal salt (concentration relative to the total amount of the liquid medium excluding the amount of the aqueous alkali solution added) was 0.595 mol / L in terms of the bismuth content as the number of atoms. This concentration was calculated without taking into account the volume of the salt, assuming the volume to be 0.7 L, which is the volume of the pure water used.

[0066] The liquid (slurry) in the reaction tank after the second pH adjustment step was subjected to the "oxidation step" and subsequent steps described in Comparative Example 1 in the same manner as in Comparative Example 1 to produce MBRO oxide powder. X-ray diffraction measurements showed that no impurity phases containing bismuth or manganese were detected in the MBRO oxide powder obtained in this example. SEM-EDX analysis showed that the Bi / (Ru+Mn) atomic ratio was 0.95 and the Mn / (Ru+Mn) atomic ratio was 0.34. In this example, even though the charged concentration of the raw metal salt was significantly increased compared to Control Example 1, an MBRO oxide powder was obtained in which no impurity phase was detected.

[0067] [Example 2] In this example, MBRO oxide powder was prepared and various measurements were performed in the same manner as in Example 1, except that the Mn / (Ru+Mn) atomic ratio in the feed composition was changed from 0.30 to 0.35, and the liquid pH at the end of the alkali addition in the first pH adjustment step was changed from 2.0 to 1.0.

[0068] (First raw material mixing process) Under the same conditions as in Example 1, a slurry-like raw material solution was obtained.

[0069] (1st pH adjustment step) An aqueous sodium hydroxide solution with a concentration of 18 mol / L was prepared and added to the raw material solution. Here, while measuring the pH of the solution at appropriate times, sodium hydroxide was continuously added until the pH reached 1.0, without excessively increasing the temperature. The time required for the addition was about 30 minutes. The amount of alkali added to the solution in this first pH adjustment step was 50% of the amount of alkali required to react with all of the anions supplied from the added bismuth-containing salt, the ruthenium-containing salt, and the manganese-containing salt to be added later. The temperature of the solution during the addition of sodium hydroxide could be kept at about 75°C by a temperature controller.

[0070] (Second raw material mixing process) Manganese nitrate (II) hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1535 mol (44.06 g) was dissolved in 100 g of pure water to obtain an aqueous manganese nitrate solution. The aqueous manganese nitrate solution was mixed with the liquid whose pH had been adjusted to 1.0 after the first pH adjustment step, and the mixture was stirred at a liquid temperature of 75° C. for 30 minutes.

[0071] (2nd pH adjustment step) Thereafter, an amount of alkali, which is 1.04 times the amount of alkali required to react with all the anions supplied from all the metal salts (the bismuth-containing salt, the ruthenium-containing salt, and the manganese-containing salt) mixed in the liquid, minus the amount of alkali added in the first pH adjustment step, was added to the liquid all at once using an aqueous sodium hydroxide solution with a concentration of 18 mol / L. The time required for the all at once addition is about several seconds. It was confirmed that the pH of the liquid after the addition of sodium hydroxide was completed was 11.5 or higher. The temperature of the liquid could be kept below 95°C until the addition of sodium hydroxide was completed by the temperature regulator. The atomic ratio of Bi / (Ru+Mn) in this liquid (slurry) was 0.950, and the atomic ratio of Mn / (Ru+Mn) was 0.35. The concentration of the raw metal salt (concentration relative to the total amount of the liquid medium excluding the amount of the aqueous alkaline solution added) was 0.595 mol / L in terms of the bismuth content as the number of atoms. This concentration was calculated without taking into account the volume of the salt, assuming the volume to be 0.7 L, which is the volume of the pure water used.

[0072] The liquid (slurry) in the reaction tank after the second pH adjustment step was subjected to the "oxidation step" and subsequent steps described in Comparative Example 1 in the same manner as in Comparative Example 1 to produce MBRO oxide powder. X-ray diffraction measurements showed that no impurity phases containing bismuth or manganese were detected in the MBRO oxide powder obtained in this example. SEM-EDX analysis showed that the Bi / (Ru+Mn) atomic ratio was 0.88 and the Mn / (Ru+Mn) atomic ratio was 0.39. In this example, even though the Mn / (Ru+Mn) atomic ratio was increased from that in Example 1, an MBRO oxide powder was obtained in which no impurity phase was detected.

[0073] [Table 1]

[0074] [Table 2]

Claims

1. A method for producing a powder of a "manganese-containing pyrochlore oxide" in which a part of the ruthenium constituting the bismuth-ruthenium-oxygen pyrochlore oxide is replaced with manganese, comprising: A "first raw material mixing step" of mixing raw materials, bismuth-containing salt and ruthenium-containing salt, with an aqueous solvent to obtain a bismuth-ruthenium-containing liquid; A "first pH adjustment step" of increasing the pH of the liquid obtained in the first raw material mixing step by adding an alkali to obtain a liquid having a pH of 4.0 or less; A "second raw material mixing step" of mixing a manganese-containing salt, which is a raw material, with the liquid obtained in the first pH adjustment step to obtain a bismuth-, ruthenium-, and manganese-containing liquid; A "second pH adjustment step" of adding an alkali to the liquid obtained in the second raw material mixing step to obtain a liquid having a pH of 10.0 or more; an "oxidation step" in which a solid reaction product is formed while supplying oxygen to the liquid obtained in the second pH adjustment step; a "drying step" of recovering the reaction product and then drying it to obtain a precursor material; A "calcination step" in which the precursor material is calcined to synthesize an oxide powder composed of particles having a crystal structure of a bismuth-ruthenium-oxygen pyrochlore oxide; A method for producing a manganese-containing pyrochlore oxide powder, comprising:

2. 2. The method for producing a manganese-containing pyrochlore oxide powder according to claim 1, wherein a mixing ratio of the raw materials mixed into the liquid in the first raw material mixing step and the second raw material mixing step is a mixing ratio in which an atomic ratio of Mn / (Ru+Mn), which represents an atomic ratio of manganese to a total amount of ruthenium and manganese, is 0.05 or more and 0.35 or less.

3. 2. The method for producing a manganese-containing pyrochlore oxide powder according to claim 1, wherein a mixing ratio of the raw materials mixed into the liquid in the first raw material mixing step and the second raw material mixing step is a mixing ratio in which a Bi / (Ru+Mn) atomic ratio, which represents an atomic ratio of bismuth to a total amount of ruthenium and manganese, is 0.700 or more and 0.990 or less.

4. 2. The method for producing a manganese-containing pyrochlore oxide powder according to claim 1, wherein the liquid subjected to the oxidation step has a bismuth content of 0.3 mol / L or more per 1 L of liquid medium excluding the added alkaline aqueous solution.

5. The method for producing a manganese-containing pyrochlore oxide powder according to claim 1 , wherein the time required for adding the alkali in the second pH adjustment step is 300 seconds or less.

Citation Information

Patent Citations

  • Oxygen catalyst and electrode using said oxygen catalyst

    WO2020153401A1