Toner

The toner formulation with a surface-coated wax and inorganic particles addresses resin transfer and dye bleed-out issues in sublimation transfer dyeing, ensuring high fastness and efficient dyeing processes.

JP2024165575AInactive Publication Date: 2024-11-28SHARP KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023081867
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The sublimation transfer dyeing method using electrophotography faces issues with toner binding resin remelting and sticking to fabrics, leading to poor fastness to friction and dye bleed-out, while inkjet methods require drying times and have moisture-related inefficiencies.

Method used

A toner formulation with a binder resin, sublimable dye, and a first wax, featuring a surface-coated second wax with inorganic particles, where the second wax has a melting point of 120°C to 150°C, enhances releasability and prevents resin transfer during high-temperature processing.

Benefits of technology

The toner achieves excellent color fastness to abrasion, reduces resin migration, and maintains dye density on fabrics, improving production efficiency and image quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165575000001_ABST
    Figure 2024165575000001_ABST
Patent Text Reader

Abstract

To provide toner capable of obtaining a material to be dyed excellent in color fastness to friction when used for dyeing by a sublimation transfer method.SOLUTION: With toner in which an external additive is attached to a surface of toner particles, the toner particles contain binder resin, sublimation dye, and first wax. The external additive includes release agents in which a surface of fine particles of second wax is coated with inorganic fine particles. A melting point of the second wax is above 120°C and below 150°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a toner suitable for a dyeing method using a sublimation transfer method (hereinafter also referred to as a sublimation transfer dyeing method). [Background technology]

[0002] In recent years, sublimation transfer dyeing methods using an inkjet system have become widespread. This method involves forming an image on an intermediate recording medium using an inkjet printer with ink containing a sublimation dye, then superimposing the intermediate recording medium on a dyed article such as a fabric and heating the resulting image to utilize the sublimation properties of the dye.

[0003] This method eliminates the plate-making process, which is the biggest problem with conventional textile printing methods, making it possible to produce a wide variety of products in small quantities (high-mix low-volume production) and shortening delivery times (shortening delivery times). Furthermore, this method makes it possible to use electronic file data created on a computer, making it easy to create and modify designs.

[0004] However, problems with sublimation transfer dyeing methods using the inkjet system include the fact that it takes a long time for inkjet printers to print onto the intermediate recording medium, and that the printed intermediate recording medium contains moisture, so a drying process is necessary. Therefore, although production efficiency has improved significantly compared to conventional textile printing methods, there are still challenges to be overcome in further simplifying the process and improving production efficiency.

[0005] In contrast, sublimation transfer dyeing methods using electrophotography are attracting attention as a method that can simplify various processes because image formation on an intermediate recording medium can be performed quickly and there is no need to dry the intermediate recording medium.

[0006] However, when an image is formed on an intermediate recording medium using a dry toner containing a sublimation dye, and then the intermediate recording medium is overlaid on a dyed object such as a resin plate or fabric for sublimation transfer, the image is heated to a high temperature of about 200°C in the heat press process in the sublimation transfer process (see Figs. 3 and 4), so the binder resin of the toner remelts and sticks to the fabric, and some of the molten toner may remain on the surface of the dyed object. In addition, when the intermediate recording medium is peeled off from the dyed object after the sublimation transfer process, pieces of the toner with the remaining sublimation dye may adhere to the dyed object (such as the fibers of the fabric) (see Fig. 6). As a result, there is a problem that the fastness to friction of the image formed by dyeing is deteriorated. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 05-323654 Summary of the Invention [Problem to be solved by the invention]

[0008] Generally, a release agent is added to toner particles to ensure the releasability of the toner (see Figure 2). If the amount of release agent added to the toner particles is increased, the phenomenon in which even the resin of the toner attached to the intermediate recording medium migrates to the dyed object (resin migration, see Figure 6) can be suppressed, and the fastness to friction of the dyed object is improved, but there is a problem that the bleeding out of the sublimation dye deteriorates. Therefore, there was a problem that it was difficult to simultaneously suppress the bleeding out of the sublimation dye (ensuring the heat-resistant storage stability of the toner) and suppress the migration of the resin to the dyed object such as a fabric (ensuring the fastness to friction of the dyed object).

[0009] The toner of the present disclosure has been found in view of the above circumstances, and has as its main object to provide a toner that, in dyeing by a sublimation transfer method, can provide a dyed object having excellent color fastness against friction without a toner layer formed on an intermediate recording medium and the object being strongly attached thereto, and further, can provide a toner that can form an image on the object having sufficient color density, high transparency, and good quality. [Means for solving the problem]

[0010] The toner disclosed herein, which has been made to solve the above problems, is a toner having an external additive attached to the surface of a toner particle, the toner particles containing a binder resin, a sublimable dye, and a first wax, the external additive containing a release agent in which the surface of a second wax particle is coated with inorganic fine particles, and the melting point of the second wax is 120°C or higher and 150°C or lower.

[0011] In the above toner, the binder resin is preferably a styrene-acrylic resin.

[0012] In the above toner, the melting point of the first wax is preferably 70° C. or higher and 110° C. or lower.

[0013] In the above toner, the first wax is preferably at least one selected from the group consisting of paraffin wax, polyethylene wax, and Fischer-Tropsch wax.

[0014] In the above toner, the second wax is preferably a polypropylene wax.

[0015] In the above toner, the median diameter of the fine particles of the second wax is preferably 0.4 μm or more and 1.0 μm or less.

[0016] In the toner, the inorganic fine particles are preferably at least one selected from the group consisting of kaolin, talc, and zinc stearate.

[0017] In the toner, it is preferable that the coverage of the surfaces of the second wax particles with the inorganic fine particles is 60% or more and 90% or less.

[0018] In the toner, the content of the second wax is preferably 0.7 parts by mass or more and 1.4 parts by mass or less with respect to 100 parts by mass of the toner particles.

[0019] In the above toner, when the content of the sublimable dye is X and the total content of the first and second waxes is Y, it is preferable that the mass ratio X / Y is 0.5 or more and 2.5 or less.

[0020] In this specification, "external addition" means that the additive is added (adhered) to the surface of the toner particle, and "internal addition" means that the additive is added to the inside of the toner particle.

[0021] Patent Document 1 discloses a toner having a wax with a volume average particle diameter of 0.4 to 1.6 μm that is externally added to the toner particles to provide releasability, and non-magnetic particles with a volume average particle diameter of 0.032 to 0.128 μm that are attached to the surface of the wax, but this toner does not contain a sublimation dye. Therefore, Patent Document 1 does not disclose anything about the configuration of the toner of the present disclosure that contains a sublimation dye. Effect of the Invention

[0022] The toner of the present disclosure exhibits excellent effects, such as the ability to obtain dyed items with excellent color fastness against friction. [Brief description of the drawings]

[0023] [Figure 1] 1 is a cross-sectional view illustrating a schematic example of a toner according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view illustrating a typical example of a conventional toner. [Diagram 3]4 is a cross-sectional view showing a schematic example of a state in which a toner layer has been fixed onto plain paper as an intermediate recording medium; FIG. [Figure 4] 1A to 1C are cross-sectional views each showing a schematic example of a sublimation transfer process. [Diagram 5] FIG. 11 is a cross-sectional view illustrating a state in which resin transfer occurs to a fabric after a sublimation transfer process. [Figure 6] FIG. 11 is a cross-sectional view illustrating how the toner according to the present embodiment suppresses the transfer of resin to the fabric even after the sublimation transfer process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The toner of the present disclosure will be described in detail below.

[0025] 1. Toner particles (toner cores), binder resin The toner particles according to the present embodiment, as illustrated in FIG. 1, contain a binder resin and internal additives such as sublimable dyes and release agents, and the internal additives are dispersed in the binder resin. External additives are attached to the surfaces of the toner particles. If necessary, the toner particles may further contain optional components within a range that does not impair the effects of the present disclosure. The average primary particle diameter of the toner particles can be appropriately selected depending on the purpose, and may be, for example, 4 μm or more and 8 μm or less.

[0026] <Binding resin> Examples of the binder resin of the toner particles include polyester resin, styrene acrylic resin, and the like. Polyester resin has excellent low-temperature fixing property. Styrene acrylic resin has good sublimation transfer efficiency and can form a high-density image on a dyed object such as a fabric. The toner particles according to the present embodiment preferably contain a styrene acrylic resin as a binder resin. According to the toner of the present disclosure, even in the case of a toner configuration that can form a high-density image by using a styrene acrylic resin as a binder resin, a dyed object having excellent color fastness against friction can be obtained.

[0027] The polyester resin used for the binder resin is usually obtained by polycondensation reaction of one or more selected from a dihydric alcohol component and a trihydric or higher polyhydric alcohol component with one or more selected from a divalent carboxylic acid and a trivalent or higher polycarboxylic acid by a known method via an esterification reaction or an ester exchange reaction.

[0028] The conditions for the polycondensation reaction may be appropriately set depending on the reactivity of the monomer components, and the reaction may be terminated when the polymer has suitable physical properties. For example, the reaction temperature is about 170 to 250° C., and the reaction pressure is about 5 mmHg to normal pressure.

[0029] Examples of the dihydric alcohol component include alkylene oxide adducts of bisphenol A such as polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(3.3)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(2.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(2.0)-polyoxyethylene(2.0)-2,2-bis(4-hydroxyphenyl)propane, and polyoxypropylene(6)-2,2-bis(4-hydroxyphenyl)propane; Examples of the diols include glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; bisphenol A; propylene adducts of bisphenol A; ethylene adducts of bisphenol A; and hydrogenated bisphenol A.

[0030] Examples of trihydric or higher polyhydric alcohol components include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, sucrose (cane sugar), 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene.

[0031] In the toner according to the present embodiment, one of the dihydric alcohol components and the trihydric or higher polyhydric alcohol components may be used alone, or two or more of them may be used in combination.

[0032] Examples of divalent carboxylic acids include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, cyclohexanedicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, n-dodecenylsuccinic acid, n-dodecylsuccinic acid, n-octylsuccinic acid, isooctenylsuccinic acid, isooctylsuccinic acid, and acid anhydrides and lower alkyl esters thereof.

[0033] Examples of trivalent or higher polyvalent carboxylic acids include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empol trimer acid, and acid anhydrides and lower alkyl esters thereof.

[0034] In the toner according to the present embodiment, one of the divalent carboxylic acids and trivalent or higher polyvalent carboxylic acids may be used alone, or two or more of them may be used in combination.

[0035] The styrene-acrylic resin is not particularly limited, but may be, for example, a resin obtained by polymerizing a styrene-based monomer and a monofunctional (meth)acrylic monomer. Note that "(meth)acrylic" is a concept that includes both "acrylic" and "methacrylic".

[0036] The styrene monomer is not particularly limited, but examples thereof include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, 4,α-dimethylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, 2,4,6-trimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-pentylstyrene, pn-hexylstyrene, pn-heptylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decanylstyrene, pn-dodecylstyrene, p-phenylstyrene, 3,4-dicyclosilstyrene, etc. Among these, styrene is preferable for the toner according to the present embodiment.

[0037] In the toner according to the present embodiment, among the above styrene-based monomers, one type may be used alone, or two or more types may be used in combination.

[0038] The monofunctional (meth)acrylic monomer is not particularly limited, but examples thereof include: Acrylic monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, n-octadecyl acrylate, methyl α-chloroacrylate, and ethyl α-chloroacrylate; Methacrylic monomers such as methacrylic acid, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-cyclohexyl methacrylate, n-dodecyl methacrylate, n-tridecyl methacrylate, and n-octadecyl methacrylate; In the toner according to the present embodiment, among these, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, and tert-butyl methacrylate are preferred, and n-butyl acrylate and n-butyl methacrylate are particularly preferred.

[0039] In the toner according to the present embodiment, one of the above monofunctional (meth)acrylic monomers may be used alone, or two or more of them may be used in combination.

[0040] The binder resin of the toner according to this embodiment may be a styrene-acrylic resin having a glass transition temperature (Tg) of 50° C. or more and 110° C. or less. The glass transition temperature of the styrene-acrylic resin is preferably 52° C. or more and 68° C. or less, and more preferably 55° C. or more and 65° C. or less.

[0041] The content of the binder resin in the toner particles according to the present embodiment can be appropriately selected depending on the purpose, but is usually 60% by mass or more and 99% by mass or less, and preferably 65% ​​by mass or more and 95% by mass or less. If the content of the binder resin is less than the lower limit, the dispersion of the dye in the toner may be poor, which may lead to a deterioration in the electrical properties of the toner. If the content of the binder resin is more than the upper limit, the color density may be reduced.

[0042] <Sublimable dye> The toner particles according to the present embodiment contain a sublimation dye. The sublimation dye is not particularly limited, but is preferably a dye suitable for sublimation transfer.

[0043] The term "dye suitable for sublimation transfer" refers to a dye whose staining (polyester) test result in the heat-sensitive treatment test (C method) in "Testing method for color fastness to dry heat treatment [JIS L 0879:2005] (revised on January 20, 2005, published by the Japan Standards Association)" is usually 3 to 4 or less, preferably 3 or less. Among such dyes, examples of known dyes include the following dyes.

[0044] Yellow dyes include CI Disperse Yellow 3, 7, 8, 23, 39, 51, 54, 60, 71, 86; CI Solvent Yellow 114, 163, and the like.

[0045] Orange dyes include CI Disperse Orange 1, 1:1, 5, 20, 25, 25:1, 33, 56, 76, and the like.

[0046] Brown dyes include CI Disperse Brown 2 and the like.

[0047] Red dyes include CI Disperse Red 11, 50, 53, 55, 55:1, 59, 60, 65, 70, 75, 93, 146, 158, 190, 190:1, 207, 239, 240; CI Bat Red 41, and the like.

[0048] Violet dyes include CI Disperse Violet 8, 17, 23, 27, 28, 29, 36, 57, and the like.

[0049] Blue dyes include CI Disperse Blue 19, 26, 26:1, 35, 55, 56, 58, 64, 64:1, 72, 72:1, 81, 81:1, 91, 95, 108, 131, 141, 145, 359, 360; CI Solvent Blue 3, 63, 83, 105, 111, and the like.

[0050] In the toner according to the present embodiment, one of the above dyes may be used alone, or two or more may be used in combination. By combining two or more dyes, it is possible to obtain a hue that is completely different from the original dye. For example, a black dye can be obtained by appropriately blending a blue dye with a yellow dye and a red dye. In addition, by combining two or more dyes, it is possible to finely adjust the color tone of blue, yellow, orange, red, violet, black, etc. to a more preferred color tone, or to obtain an intermediate color.

[0051] The content of the sublimation dye in the toner particles according to the present embodiment can be appropriately selected according to the purpose, but is usually 1% by mass or more and 40% by mass or less, preferably 2% by mass or more and 20% by mass or less, and more preferably 5% by mass or more and 15% by mass or less. If the content of the sublimation dye in the toner particles is less than the lower limit, the dyeing density may decrease. If the content of the sublimation dye in the toner particles exceeds the upper limit, the dye may not disperse well in the toner, which may cause the electrical properties of the toner to deteriorate.

[0052] <Charge control agent> The toner particles according to the present embodiment may contain a charge control agent. As the charge control agent, charge control agents commonly used in the art for controlling positive charge and negative charge can be used.

[0053] Examples of charge control agents for controlling positive charges include nigrosine dyes, basic dyes, quaternary ammonium salts, quaternary phosphonium salts, aminopyrine, pyrimidine compounds, polynuclear polyamino compounds, aminosilanes, nigrosine dyes and derivatives thereof, triphenylmethane derivatives, guanidine salts, and amidine salts.

[0054] Examples of charge control agents for negative charge control include oil-soluble dyes such as oil black and spiron black, metal-containing azo compounds, azo complex dyes, metal naphthenates, metal complexes and metal salts of salicylic acid and its derivatives (metals include chromium, zinc, zirconium, etc.), boron compounds, fatty acid soaps, long-chain alkyl carboxylates, and resin acid soaps.

[0055] In the toner according to the present embodiment, among the above charge control agents, one type may be used alone, or two or more types may be used in combination.

[0056] The content of the charge control agent in the toner according to the present embodiment is not particularly limited, but is preferably 0.5 parts by mass or more and 3.0 parts by mass or less, and more preferably 1 part by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the binder resin. By having the content of the charge control agent within the above range, it is possible to form an image having high image density and good image quality without impairing various physical properties of the toner. In terms of conversion, the content of the charge control agent in the toner particles is preferably 0.5% by mass or more and 2.0% by mass or less, and more preferably 0.7% by mass or more and 1.5% by mass or less.

[0057] <Releasing agent in toner particles (first wax)> The toner particles according to the present embodiment contain a first wax in the toner particles as a release agent. In other words, the first wax is an internally added wax. As the first wax, waxes used in the electrophotographic field can be used, for example, petroleum waxes such as paraffin wax and its derivatives; hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene wax and its derivatives; carnauba wax, rice wax, candelilla wax, etc. These waxes may be used alone or in combination of two or more.

[0058] Among these waxes, the first wax is preferably at least one selected from the group consisting of paraffin wax, polyethylene wax, and Fischer-Tropsch wax. For example, comparing these three types of wax with ester wax, these three types of wax are preferable because they have better sublimation transfer efficiency than ester wax. This is thought to be because the sublimation transfer efficiency of ester wax is slightly worsened due to the ester group. Also, comparing these three types of wax with polypropylene wax, when polypropylene wax is added to toner particles, it becomes necessary to increase the fixing temperature of the toner, and when the toner is fixed to an intermediate recording medium such as plain paper, the sublimation dye also sublimes partially, which may cause contamination inside the machine. In addition, since the sublimation dye is reduced by the time of the sublimation transfer process, there is a risk of insufficient dye concentration on the dyed material such as fabric. Therefore, the above three types of wax are preferable to polypropylene wax.

[0059] The melting point of the first wax is preferably 70° C. or more and 110° C. or less, more preferably 75° C. or more and 105° C. or less. If the melting point is less than the lower limit, the toner may have low resistance to stress and may easily cause filming on the photoconductor. If the melting point is more than the upper limit, low-temperature offset may easily occur.

[0060] The content of the first wax in the toner particles is not particularly limited, but is preferably 0.5% by mass or more and 10% by mass or less. If the content is less than the lower limit, the toner may have insufficient releasability and may easily cause offset. If the content is more than the upper limit, the toner may have insufficient heat-resistant storage stability.

[0061] 2.External additives <Wax external additive> The toner according to this embodiment has an external additive attached to the surface of the toner particles, and this external additive includes a release agent in which the surface of second wax particles is coated with inorganic fine particles. Therefore, the second wax is an externally added wax. In this specification, the "release agent in which the surface of second wax particles is coated with inorganic fine particles" is also referred to as a "wax external additive."

[0062] In the toner according to the present embodiment, the melting point of the second wax is 120°C or more and 150°C or less, more preferably 130°C or more and 140°C or less. As shown in FIG. 4, in the sublimation transfer process, heating (heat pressing) is performed at about 200°C to 210°C, so it is preferable to use a wax having a melting point within the above range in order to ensure releasability during sublimation transfer. In addition, it is preferable that the melting point of the second wax is 50°C to 80°C lower than the heat pressing temperature in the sublimation transfer process. By using a wax having a melting point within the above range, resin migration during sublimation transfer (the phenomenon shown in FIG. 6) can be suppressed, and a dyed product in which resin migration is suppressed as shown in FIG. 5 can be obtained, in other words, a dyed product having excellent color fastness to friction can be obtained.

[0063] Typical waxes having a melting point within the above range include polypropylene wax and amide wax, but in the toner according to the present embodiment, it is preferable to use polypropylene wax as the second wax. Since the amide group of the amide wax has a positive (+) chargeability, there is a risk of fogging occurring due to poor charging.

[0064] In the wax external additive, the second wax microparticles preferably have a median diameter of 0.4 μm to 1.0 μm, more preferably 0.6 μm to 0.8 μm. If the median diameter is less than the lower limit, the effect of improving the fastness to friction of the dyed object may not be obtained. This is because if the dispersion diameter of the second wax microparticles is small, the melt viscosity is low, and the transfer of the toner to the resin during sublimation transfer cannot be prevented. If the median diameter exceeds the upper limit, the fluidity of the toner may deteriorate, resulting in a decrease in the amount of development.

[0065] In the wax external additive, the inorganic fine particles that cover the surface of the second wax fine particles are preferably at least one selected from the group consisting of kaolin, talc, and zinc stearate. The reason why these inorganic fine particles are preferable is that inorganic fine particles having a flat crystal structure such as kaolin and talc (layered or flat inorganic fine particles) have a lower adhesion to the photoreceptor drum than spherical or cubic inorganic fine particles such as silica, titanium oxide, strontium titanate, etc. In addition, silica, titanium oxide, strontium titanate, etc., which are often used in general external additives, have a large effect on the chargeability of the toner, so inorganic fine particles that can reduce the effect on the chargeability are preferable.

[0066] In the wax additive, the coverage of the second wax particle surface by the inorganic fine particles is preferably 60% to 90%, more preferably 65% ​​to 80%. If the coverage is below the lower limit, the second wax has a high melting point, so there is no problem with the heat-resistant storage stability of the toner, but there is a risk of insufficient fluidity of the toner, resulting in a decrease in the amount of development. If the coverage is above the upper limit, the inorganic fine particles may affect the charging property of the toner, causing poor charging, which may even affect the amount of development.

[0067] In the toner according to the present embodiment, the content of the second wax is preferably 0.7 parts by mass or more and 1.4 parts by mass or less, and more preferably 1.0 parts by mass or more and 1.3 parts by mass or less, relative to 100 parts by mass of the toner particles. If the content of the second wax is less than the lower limit, there is a risk of development failure due to insufficient charging of the toner. If the content of the second wax is more than the upper limit, there is a risk of development failure due to insufficient fluidity of the toner.

[0068] In the toner according to the present embodiment, the content of the sublimation dye is X, and the total content of the first and second waxes is Y. The mass ratio X / Y is preferably 0.5 to 2.5, more preferably 1.5 to 2.2. If X / Y is less than the lower limit, the dyeing of the substrate such as fabric may not be possible with sufficient image density. If X / Y is more than the upper limit, the sublimation dye may bleed out, deteriorating the heat-resistant storage stability of the toner.

[0069] <Other external additives> The toner according to the present embodiment may contain an external additive other than the wax external additive described above. The functions of the external additive include a function of improving the powder fluidity, triboelectric charging property, heat-resistant storage stability, and cleaning property of the toner, a function of controlling the wear property of the photoreceptor surface, and the like.

[0070] Examples of external additives other than the wax external additive include inorganic fine particles having an average particle size of 5 nm to 200 nm, such as silica, titanium oxide, alumina, etc. These inorganic fine particles are more suitable for use in treating the surfaces of the inorganic fine particles with a silane coupling agent, a titanium coupling agent, or silicone oil to impart hydrophobicity, since this reduces the decrease in electrical resistance and charge amount under high humidity conditions.

[0071] The content of the external additive is preferably 0.2 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the toner particles. If the content of the external additive is less than the lower limit, it becomes difficult to impart the effect of improving the fluidity. If the content of the external additive is more than the upper limit, the fixing property may decrease.

[0072] As a method for adding an external additive to toner particles, a method in which the toner particles and the external additive are mixed in an air flow mixer such as a Henschel mixer can be mentioned.

[0073] The toner according to the present embodiment may be used as a one-component developer as it is, or may be mixed with a carrier and used as a two-component developer.

[0074] 3. Toner manufacturing method The toner manufacturing method according to the present embodiment includes a kneading step S1 in which a kneaded mixture is produced by kneading toner materials including a binder resin, a release agent, and a sublimable dye, and a pulverization step S2 in which the kneaded mixture produced in the kneading step S1 is pulverized to produce toner particles. The toner manufacturing method according to the present embodiment further includes a classification step S3 in which the toner particles produced in the pulverization step S2 are classified, and an external addition step S4 in which an external additive is added to the toner particles classified in the classification step S3.

[0075] In addition, before the external addition step S4, the process includes steps for producing the wax external additive, namely, a "wax fine-pulverizing step" S11 for preparing second wax microparticles, a "coating step with inorganic microparticles" S12 for coating the surfaces of the second wax microparticles with inorganic microparticles, and a "drying step" S13 for drying the wax slurry obtained in the coating step S12 to obtain the wax external additive.

[0076] In the kneading step S1, toner materials such as a binder resin, a release agent, and a sublimable dye are mixed in a mixer such as a Henschel mixer, and then kneaded using a kneader to obtain a kneaded mixture.

[0077] Mixing is preferably a dry type, and the mixer may be a known device commonly used in the technical field, such as Henschel type mixers such as Henschel Mixer (trade name, manufactured by Nippon Coke & Engineering Co., Ltd.), Super Mixer (trade name, manufactured by Kawata Corporation), and Mechano Mill (trade name, manufactured by Okada Seiko Co., Ltd.), Ang Mill (trade name, manufactured by Hosokawa Micron Corporation), Hybridization System (trade name, manufactured by Nara Machinery Works, Ltd.), and Cosmo System (trade name, manufactured by Kawasaki Heavy Industries, Ltd.).

[0078] The kneader may be a known device commonly used in the technical field, and examples of the kneader include general kneaders such as a twin-screw extruder, a triple roll, and a lab blast mill. Specific examples include single-screw or twin-screw extruders such as TEM-100B (trade name, manufactured by Toshiba Machine Co., Ltd.), PCM-65 / 87, and PCM-30 (all of which are trade names, manufactured by Ikegai Corporation), and open-roll type kneaders such as Kneadex (trade name, manufactured by Nippon Coke and Engineering Co., Ltd.). Among these, open-roll type kneaders are preferred in that they have a strong shear during kneading and can highly disperse the toner materials.

[0079] In the pulverization step S2, the kneaded material obtained in the kneading step S1 is finely pulverized using a pulverizer. As the pulverizer, a known device commonly used in the technical field can be used, and examples thereof include a jet pulverizer that pulverizes using a supersonic jet stream, and an impact pulverizer that introduces a solidified material into the space formed between a rotor and a stator (liner) rotating at high speed and pulverizes it.

[0080] In the classification step S3, the finely pulverized toner particles obtained in the pulverization step S2 are classified using a classifier. A known device commonly used in the art can be used for classification. A classifier capable of removing excessively pulverized toner particles by centrifugal force and wind force, such as a rotary wind classifier (rotary wind classifier), is suitable.

[0081] In the external addition step S4, the toner particles obtained in the classification step S3, the wax external additive, and hydrophobic silica fine particles as an optional external additive are mixed using a mixer to attach the external additive to the toner particles. The mixer may be a known device commonly used in the technical field. For example, a Henschel type mixer such as Henschel Mixer (trade name, manufactured by Nippon Coke & Engineering Co., Ltd.), Super Mixer (trade name, manufactured by Kawata Corporation), Mechano Mill (trade name, manufactured by Okada Seiko Co., Ltd.), Ang Mill (trade name, manufactured by Hosokawa Micron Corporation), Hybridization System (trade name, manufactured by Nara Machinery Works, Ltd.), Cosmo System (trade name, manufactured by Kawasaki Heavy Industries, Ltd.), etc. may be mentioned.

[0082] The following steps from wax fine pulverization step S11 to drying step S13 are steps for producing a wax external additive, and therefore are carried out before the above-mentioned external addition step S4.

[0083] In the wax fine pulverization step S11, a wax slurry is obtained by pulverizing the wax using a bead mill. As the pulverization device, a known device commonly used in the technical field can be used. In this embodiment, either a dry type or a wet type may be used as the bead mill treatment, but it is preferable to use a wet bead mill treatment. In this case, in addition to water, an alcohol solvent such as methanol, ethanol, isopropanol, or butanol can be used as the solvent. As the device to be used, for example, a wet bead mill Labostar (product name, manufactured by Ashizawa Finetech Co., Ltd.) can be used.

[0084] In the inorganic fine particle coating step S12, inorganic fine particles are added to the wax slurry obtained in the wax fine pulverization step S11 and suspended to obtain a wax slurry in which the surfaces of the wax fine particles are coated with inorganic fine particles. The suspension device used may be a known device commonly used in the technical field, such as an aluminum air motor vertical stirrer (Bernoulli flow stirrer BEAG E type, manufactured by Nitto Metal Industries Co., Ltd.).

[0085] In the drying step S13, the wax slurry obtained in the inorganic fine particle coating step S12 is continuously dried to obtain a wax external additive (a release agent in which the surface of wax fine particles is coated with inorganic fine particles). Examples of the drying device used include a flash jet dryer (product name, manufactured by Seishin Enterprise Co., Ltd.).

[0086] 4. Two-component developer When performing two-component development, the toner according to the present embodiment and the carrier are mixed to prepare a two-component developer. As a mixer for mixing the toner and the carrier, for example, a powder mixer such as a V-type mixer (product name: V-5, manufactured by Tokuju Machinery Co., Ltd.) can be used.

[0087] The blending ratio of the toner and the carrier is preferably within the range of 10:90 to 5:95 by mass ratio. As the carrier, a carrier that is normally used in the technical field can be used. In addition, a coated carrier can also be used. EXAMPLES

[0088] The toner and the method for producing the toner according to the present disclosure will be specifically described below based on examples and comparative examples. First, various measurement methods and evaluation methods will be described.

[0089] 1. Measurement and evaluation methods <Measuring the melting point of wax> The melting point was determined as the temperature at which the heat of absorption peak of the wax constituting the toner was measured by differential scanning calorimetry (DSC). Measurements were performed in accordance with ASTM D3418-82, in which 10 mg of a measurement sample was heated from 20°C to 150°C at a heating rate of 10°C / min using a differential scanning calorimetry measuring device DSC8230 (manufactured by Rigaku Corporation) at room temperature and normal humidity.

[0090] <Evaluation item 1: Evaluation of photoconductor filming> The toners of the examples and comparative examples were filled into a commercially available copier (product name: MX-5111FN, manufactured by Sharp Corporation) having a developing device, and a predetermined print pattern with a print rate of 1% was continuously printed on A4 paper in a high temperature and high humidity environment (temperature 28°C, humidity 80%). After continuously printing 5,000 sheets, the photoconductor and the solid image were visually observed to evaluate the photoconductor filming.

[0091] The evaluation criteria for the photoreceptor filming are as follows. ⊚ (Excellent): No filming occurs on the photoconductor, and there are no problems at all. ◯ (Good): There are fine scratches on the photoconductor, but no filming occurs and there are no problems with the image. △ (Fair): Some filming has occurred on the photoconductor, but there is no problem with the image. × (Fail): A lot of filming has occurred on the photoconductor, and there are problems with the image.

[0092] <Evaluation item 2: Evaluation of low temperature offset> The toners of the examples and comparative examples were filled into a commercially available copying machine (product name: MX-5111FN, manufactured by Sharp Corporation), and an A4 test document having a rectangular solid image of 20 mm length and 50 mm width was printed on a recording paper (product name: PPC paper SF-4AM3, manufactured by Sharp Corporation) to check whether low-temperature offset occurred on the recording paper. At this time, the amount of toner attached to the solid image area was 0.5 mg / cm 2 The temperature of the fixing roller was set to 135° C. Low-temperature offset refers to the phenomenon in which toner is not fixed to the recording paper during fixing, but remains attached to the fixing roller and re-adheres to the recording paper after the fixing roller makes one revolution.

[0093] The evaluation criteria for low temperature offset are as follows: ◯ (Good): No re-adhesion of toner to the recording paper was observed. Δ (fairly good): Some redeposition of toner onto the recording paper was observed, but the reflection density (ID) of the redeposited image was less than 0.1. × (unacceptable): Toner redeposition onto the recording paper was clearly observed, and the reflection density (ID) of the redeposition image was 0.1 or more.

[0094] <Evaluation item 3: Evaluation of sublimation transfer efficiency> The toners of the examples and comparative examples were loaded into a commercially available copying machine (product name: MX-5111FN, manufactured by Sharp Corporation), and an A4 test document having a rectangular solid image measuring 20 mm in length and 50 mm in width was printed on a recording paper (product name: PPC paper SF-4AM3, manufactured by Sharp Corporation) as an intermediate recording medium. At this time, the amount of toner adhered to the solid image area was set to 0.5 mg / cm. 2 The temperature of the fixing roller was set to 135°C.

[0095] For the intermediate recording medium obtained by the above two-component development, the magenta dye density was measured using a spectrophotometer (product name: Spectroeye, manufactured by GretagMacbeth) for a portion of the intermediate recording medium corresponding to 100% of the print output before and after sublimation transfer by heat press processing. The sublimation transfer efficiency was calculated from the dye concentration attached to the intermediate recording medium before and after transfer using the following formula. Sublimation transfer efficiency = (dye concentration after transfer - dye concentration before transfer) / (dye concentration before transfer) x 100%

[0096] Based on the calculated sublimation transfer efficiency, evaluation was performed according to the following criteria. ◎ (Excellent): Sublimation transfer efficiency is 50% or more. ◯ (Good): Sublimation transfer efficiency is 45% or more and less than 50%. △(Fair): Sublimation transfer efficiency is 40% or more and less than 45%. × (Fail): Sublimation transfer efficiency is less than 40%.

[0097] <Evaluation item 4: Evaluation of fogging> A whiteness meter (product name: ZE6000, manufactured by Nippon Denshoku Industries Co., Ltd.) was used to measure the difference in whiteness between the paper before printing and the whiteness of the non-image area of ​​the paper after printing, and the fogging was evaluated according to the following criteria.

[0098] ◎ (Excellent): The difference in whiteness is 0.5 or less. ◯ (Good): The difference in whiteness is more than 0.5 and 1.0 or less. △(Acceptable): The difference in whiteness is more than 1.0 and 1.5 or less. × (Fail): The difference in whiteness is more than 1.5.

[0099] <Evaluation item 5: Evaluation of color fastness to friction> The toners of the examples and comparative examples were loaded into a commercially available copying machine (product name: MX-5111FN, manufactured by Sharp Corporation) and images were formed on an intermediate recording medium. The intermediate recording medium and fabric were superimposed and then heat-pressed to dye the fabric by sublimation transfer. Specifically, the following three types of fabric were heat-pressed at 180°C for 35 seconds to dye the fabric by sublimation transfer, and three types of test fabric were prepared. Fabric 1: PET tromat (a thick polyester fabric with eyelets and bag stitching) Fabric 2: T / C blend (polyester and cotton blend) Fabric 3: Cotton Brode (a plain weave fabric with high density and luster)

[0100] For each test cloth obtained as described above, a color fastness test against rubbing was carried out using a type II (Gakushin type) testing machine according to the method specified in JIS L0849. Dry rubbing was tested according to the dry test specified in JIS L0849, and wet rubbing was tested according to the wet test specified in JIS L0849, and the results were evaluated according to the following criteria using the stain gray scale.

[0101] ◎ (Excellent): Dye fastness is grade 4-5 or above. ○ (Good): Dye fastness is grade 4. △(Acceptable): Dye fastness is grade 3-4. × (Fail): Dye fastness is grade 3 or lower.

[0102] <Evaluation item 6: Evaluation of toner development amount> A 1 cm x 1 cm square template was attached to three locations on the OPC (organic photoconductor), two locations 3 cm from both ends in the width direction and one location in the center in the width direction, and the toner on the OPC was sucked up using a Q / m meter (product name: 210HS, manufactured by Trek Corporation). The amount of toner per unit area on the OPC, calculated by dividing the amount of toner sucked up by the area sucked up, was used as the amount of developed toner.

[0103] The evaluation criteria for the amount of toner development are as follows. ◎ (Excellent): Development amount is 0.2mg / cm 2 More than 0.25mg / cm 2 is less than. ○(Good): Development amount is 0.25mg / cm 2 More than 0.3mg / cm 2 is less than. △(Acceptable): Developing amount is 0.3mg / cm 2 Or the amount of development is 0.2 mg / cm 2 is less than.

[0104] 2. Manufacture of toner and two-component developer [Example 1] <Toner particle manufacturing process> The following toner materials were used to prepare the toner particles (toner cores).

[0105] ·Binding resin Styrene acrylic resin (product name: CPR-190, manufactured by Mitsui Chemicals, Inc.) 82.0% by mass ·Sublimable dye Disperse Yellow 54 (product name: Plast Yellow 8040, Arimoto Chemical Industry Co., Ltd.) 3.0% by mass Disperse Red 60 (product name: Plast Red 8375-N, Arimoto Chemical Industry Co., Ltd.) 5.0% by mass Disperse Blue 56 (product name: KP Plast Blue BG, Kiwa Chemical Industry Co., Ltd.) 5.0% by mass Charge control agent Salicylic acid compound (product name: Bontron E-84, Orient Chemical Industry Co., Ltd.) 1.0% by mass Release agent (first wax) Polyethylene wax (product name: Sanwax 161-P, manufactured by Sanyo Chemical Industries, Ltd.) 4.0% by mass

[0106] The above materials were premixed for 5 minutes using an airflow mixer (Henschel mixer, model: FM20C, manufactured by Nippon Coke & Engineering Co., Ltd.), and then melt-kneaded using a twin-screw extruder (model: PCM30, manufactured by Ikegai Co., Ltd.) under conditions of cylinder setting temperature 110°C, barrel rotation speed 200 rpm, and material supply rate 15 kg / hour to obtain a molten kneaded product. [Mixing and kneading process]

[0107] The obtained molten kneaded product was cooled in a drum flaker, and then coarsely pulverized using a cutting mill (model: VM-16, manufactured by Orient Co., Ltd.) to obtain a coarsely pulverized product. [Coarse pulverization process]

[0108] The resulting coarsely pulverized product was then finely pulverized using a jet pulverizer (model: IDS-2, manufactured by Nippon Pneumatic Mfg. Co., Ltd.) to obtain a finely pulverized product. [Finely pulverizing process]

[0109] The resulting finely pulverized product was classified using an elbow jet classifier (model: EJ-LABO, manufactured by Nittetsu Mining Co., Ltd.) to obtain toner particles having an average primary particle size of 5.5 μm [classification step].

[0110] <Preparation process of wax external additive> (1) Preparation of wax dispersion A dispersion liquid in which Viscol 660P (manufactured by Sanyo Chemical Industries, Ltd., melting point 136° C.) was dispersed in a solvent was prepared as follows.

[0111] 450 g of this wax powder was added to 1,050 g of ion-exchanged water, and the resulting mixture was milled in a wet bead mill, Labostar (model: LMZ06, manufactured by Ashizawa Finetech Co., Ltd.), at an agitator peripheral speed of 12 m / s and a processing time of 25 minutes to obtain a dispersion containing fine wax particles (wax slurry). [Wax fine grinding process]

[0112] (2) Wax particle size measurement The volume-based median diameter (D50) of the wax fine particles in the obtained wax slurry was measured with a Microtrac (model: UPA-150, manufactured by Nikkiso Co., Ltd.) and was found to be 100 nm.

[0113] (3) Coating of the wax particle surface with inorganic particles 1,500 mL of the obtained wax slurry and 600 g of talc (Microace SG-2000, manufactured by Nippon Talc Kogyo Co., Ltd.) were placed in a tank and stirred with an aluminum air motor stirrer at 900 rpm for 30 minutes to mix so that the coverage rate of the wax particle surface with the inorganic fine particles was 85%. [Inorganic fine particle coating process]

[0114] (4) Drying process The wax slurry that had been subjected to the above step (3) was dried in an airflow dryer (flash jet dryer, manufactured by Seishin Enterprise Co., Ltd.) to obtain a wax external additive (a release agent containing a second wax). The drying conditions were a blowing temperature of 60°C, a temperature at the outlet of the dryer of 30°C, and the supply rate of the wax slurry was adjusted so that the outlet temperature did not deviate from 30°C. [Drying step]

[0115] <External addition process> 100 parts by mass of the toner particles obtained in the above "Toner particle manufacturing process", 1.0 part by mass of hydrophobic silica fine particles (product name: fumed silica R976S, average primary particle diameter 7 nm, manufactured by Nippon Aerosil Co., Ltd.), and 2.5 parts by mass of the wax external additive obtained in the above "Wax external additive preparation process" were put into an air flow mixer (Henschel mixer, model: FM20C, manufactured by Nippon Coke and Engineering Co., Ltd.), and the peripheral speed at the outermost circumference of the stirring blade tip was set to 40 m / sec, and the mixture was stirred and mixed for 1 minute to obtain about 2,000 g of the toner of Example 1 (volume average particle size 5.9 μm, coefficient of variation 24%). [External Addition Process]

[0116] <Preparation of two-component developer> The obtained toner and a coated carrier (genuine carrier for MX-5111FN manufactured by Sharp Corporation) were mixed for 20 minutes in a V-type mixer (product name: V-5, manufactured by Tokuju Kogyosho Co., Ltd.) so that the toner concentration was 7% by mass, to prepare a two-component developer.

[0117] [Examples 2 to 28, Comparative Examples 1 to 6] Table 1 shows a list of waxes used in the examples and comparative examples. Table 2 shows a list of the types of first wax (internal wax), second wax (external wax as external wax additive), and inorganic fine particles used as the wax external additive, all of which were used in the examples and comparative examples. The amount of second wax added in Table 2 is the amount [parts by mass] added relative to 100 parts by mass of toner particles.

[0118] A toner and a two-component developer were obtained in the same manner as in Example 1, except that the type of the first wax, the type and amount of the second wax, the type of inorganic fine particles, and the coverage rate by the inorganic fine particles were changed as shown in Table 2.

[0119] [Table 1]

[0120] [Table 2]

[0121] [Table 3]

[0122] Table 3 shows the evaluation results of the examples and comparative examples. As is clear from the evaluation results, the toners of Examples 1 to 28, which are toners having an external additive attached to the surface of the toner particles, the toner particles containing a binder resin, a sublimable dye, and a first wax, the external additive containing a release agent in which the surface of the second wax particles is coated with inorganic fine particles (referred to as "wax external additive" in Table 2), and the melting point of the second wax is 120°C or higher and 150°C or lower, were excellent in color fastness to friction when used for dyeing by sublimation transfer. In addition, the occurrence of photoconductor filming, low-temperature offset, and fogging could be suppressed, and the sublimation transfer efficiency was also excellent.

[0123] In contrast, Comparative Examples 1 to 6, which did not satisfy these requirements, were inferior to the Examples at least in the evaluation of color fastness to rubbing.

[0124] Examples 2 to 6 are examples in which waxes with different melting points are used. Examples 4 and 5, in which the melting point of the first wax is 70°C or more and 110°C or less, are found to be superior in the evaluation of photoreceptor filming to Example 3, in which the melting point is below the lower limit. Also, it is found to be superior in the evaluation of low-temperature offset to Example 6, in which the melting point exceeds the upper limit. Also, among the examples in which the melting point of the second wax is in the range of 120°C or more and 150°C or less, Example 1, in which the melting point is in the range of 130°C or more and 140°C or less, is found to be the most superior in the evaluation of color fastness to friction and also superior in various other evaluations.

[0125] Example 7 is an example in which an amide wax was used as the second wax. It can be seen that Example 2 and the like in which the second wax is a polypropylene wax are particularly superior in the evaluation of fogging to Example 7 in which the second wax is an amide wax.

[0126] Examples 4 and 8 are examples in which an ester wax was used as the first wax. Examples 1, 2, 9, etc. in which the first wax was paraffin wax, polyethylene wax, or Fischer-Tropsch wax were found to be particularly superior in the evaluation of sublimation transfer efficiency to Examples 4 and 8 in which the first wax was an ester wax.

[0127] Examples 10 to 13 are examples in which the median diameter of the second wax particles (particle diameter of the wax particles in the wax external additive) is changed. It can be seen that Example 11 and the like in which the median diameter of the second wax particles is 0.4 μm or more is particularly superior in the evaluation of low-temperature offset than Example 10 in which the median diameter is less than 0.4 μm. It can also be seen that Example 12 and the like in which the median diameter of the second wax particles is 1.0 μm or less is particularly superior in the evaluation of the development amount than Example 13 in which the median diameter exceeds 1.0 μm.

[0128] Examples 14 to 16 are examples in which the inorganic fine particles contained in the wax external additive were changed. It can be seen that Example 1 and the like in which the inorganic fine particles used were kaolin, talc, or zinc stearate were particularly superior in the evaluation of photoreceptor filming and fogging to Examples 14 to 16 in which the inorganic fine particles were titanium oxide, silica, or strontium titanate.

[0129] Examples 17 to 20 are examples in which the coverage of the second wax particle surface by the inorganic particles in the wax external additive was changed. It can be seen that Examples 18 and 19, in which the coverage was 60% or more and 90% or less, were particularly superior in the evaluation of the development amount to Examples 17 and 19, in which the coverage was outside the above range.

[0130] Examples 21 to 24 are examples in which the amount of the second wax added per 100 parts by mass of toner particles was changed. It can be seen that Examples 22 and 23, in which the amount of the second wax added per 100 parts by mass of toner particles is 0.7 parts by mass or more and 1.4 parts by mass or less, are particularly superior in terms of the evaluation of the development amount compared to Examples 21 and 24, in which the amount added is outside the above range.

[0131] Examples 25 to 28 are examples in which the mass ratio X / Y was changed when the content of the sublimable dye was X and the total content of the first and second waxes was Y. In Example 25, where the mass ratio X / Y was less than 0.5, sufficient image density could not be obtained for the fabric to be dyed. In Example 28, where the mass ratio X / Y was more than 2.5, bleeding out of the dye occurred and the durability of the toner was deteriorated.

[0132] The embodiments disclosed herein are illustrative in all respects and are not intended to be limiting. Therefore, the technical scope of the present disclosure is not interpreted solely by the above-described embodiments, but is defined based on the claims. Also, all modifications within the scope and meaning equivalent to the claims are included. [Explanation of symbols]

[0133] 1. Binder resin 2 Sublimable dye 3. Charge control agent 4. Wax 41 Second wax (external wax) 42 First wax (internal wax) 51 Inorganic fine particles (coating the surface of the second wax fine particles) 52 Inorganic fine particles (additives other than wax additives) 53 Large inorganic particles 54 Small inorganic particles 6. Wax Additives A Toner according to this embodiment A' Conventional toner B Toner layer C Plain paper (intermediate recording medium) D Fabric (material to be dyed)

Claims

1. A toner having an external additive attached to the surface of a toner particle, the toner particles include a binder resin, a sublimable dye, and a first wax; the external additive includes a release agent in which the surfaces of second wax particles are coated with inorganic particles, The toner according to the present invention is characterized in that the melting point of the second wax is 120° C. or more and 150° C. or less.

2. 2. The toner according to claim 1, The toner is characterized in that the binder resin is a styrene-acrylic resin.

3. The toner according to claim 1 or 2, The toner according to the present invention is characterized in that the melting point of the first wax is 70° C. or more and 110° C. or less.

4. The toner according to claim 3, The toner, wherein the first wax is at least one wax selected from the group consisting of paraffin wax, polyethylene wax, and Fischer-Tropsch wax.

5. The toner according to claim 1 or 2, The toner, wherein the second wax is a polypropylene wax.

6. The toner according to claim 1 or 2, The toner, wherein the median diameter of the second wax particles is 0.4 μm or more and 1.0 μm or less.

7. The toner according to claim 1 or 2, The toner, wherein the inorganic fine particles are at least one selected from the group consisting of kaolin, talc, and zinc stearate.

8. The toner according to claim 1 or 2, The toner according to claim 1, wherein the coverage of the surfaces of the second wax particles with the inorganic fine particles is 60% or more and 90% or less.

9. The toner according to claim 1 or 2, The toner, wherein the content of the second wax is 0.7 parts by mass or more and 1.4 parts by mass or less with respect to 100 parts by mass of the toner particles.

10. The toner according to claim 1 or 2, The toner according to claim 1, wherein the content of the sublimable dye is X and the total content of the first and second waxes is Y, and the mass ratio X / Y is 0.5 or more and 2.5 or less.

Citation Information

Patent Citations

  • Toner, production of toner and image forming device

    JP1993323654A