Solid electrolyte battery and method for manufacturing the same

The use of a shape memory resin container for precise alignment and fixation of power generation elements in solid electrolyte batteries addresses misalignment issues, enhancing productivity and reliability by ensuring secure electrode positioning and reducing short circuit risks.

JP2024165722APending Publication Date: 2024-11-28MAXELL LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023082140
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing solid electrolyte batteries face issues with misalignment of power generation elements during manufacturing, affecting productivity and reliability, as the electrodes are simply stacked before sealing, leading to potential misalignment and increased risk of short circuits.

Method used

The battery design incorporates a shape memory resin container that deforms at a specific temperature to facilitate easy insertion of stacked power generation elements, ensuring precise alignment and fixation within the container, using a method that involves deforming the container at a lower temperature and re-transforming it at a higher temperature to secure the electrode body.

Benefits of technology

This approach enhances productivity and reliability by preventing misalignment of electrodes, improving work efficiency, and reducing the risk of short circuits, while maintaining high energy density and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165722000001_ABST
    Figure 2024165722000001_ABST
Patent Text Reader

Abstract

To provide a solid electrolyte battery having good productivity and reliability, and a method for manufacturing the same, a solid electrolyte battery according to the present invention relating to the goals 3, 7, 11, and 12 of the SDGs.SOLUTION: A solid electrolyte battery according to the present invention includes: an electrode body in which a plurality of pellet-shaped power generation elements are laminated; and an exterior body. Each of the plurality of power generation elements is formed by sequentially laminating a positive electrode layer, a solid electrolyte layer, and a negative electrode layer. The electrode body is accommodated in an insulating accommodation body and is included in the exterior body while a side face of the electrode body is fixed to an inner face of the accommodation body. The accommodation body is formed of a shape memory resin that has such a function that a shape of the shape memory resin at a temperature of a predetermined temperature or above is deformed at a temperature less than the predetermined temperature and when the shape memory resin is placed again at a temperature of the predetermined temperature or above, the shape is returned to a shape before the deformation.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid electrolyte battery having good productivity and reliability, and a method for producing the same. [Background technology]

[0002] In recent years, with the development of portable electronic devices such as mobile phones and notebook personal computers, and the practical application of electric vehicles, there has been a demand for small, lightweight batteries with high capacity and high energy density.

[0003] Currently, lithium batteries that can meet this demand, particularly lithium ion batteries, use lithium-containing composite oxides such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2) as the positive electrode active material, graphite or the like as the negative electrode active material, and an organic electrolyte solution containing an organic solvent and a lithium salt as the non-aqueous electrolyte.

[0004] Furthermore, with the further development of devices in which lithium-ion batteries are used, there is a demand for lithium-ion batteries with longer life, higher capacity and higher energy density, as well as a high demand for the reliability of these longer life, higher capacity and higher energy density lithium-ion batteries.

[0005] However, the organic electrolyte used in lithium-ion batteries contains an organic solvent, which is a flammable substance, and therefore the organic electrolyte may generate abnormal heat when an abnormality such as a short circuit occurs in the battery. In addition, with the recent trend toward higher energy density of lithium-ion batteries and an increasing amount of organic solvent in the organic electrolyte, there is a demand for even higher reliability in lithium-ion batteries.

[0006] In the above circumstances, solid electrolyte batteries using a molded body of a solid electrolyte without using an organic solvent instead of an organic solvent-based electrolyte are also being considered. The solid electrolyte of a solid electrolyte battery is highly reliable because it does not generate abnormal heat, unlike an organic solvent-based electrolyte. Therefore, there are high expectations for it, especially in the product field that requires a high-capacity secondary battery.

[0007] In addition, solid electrolyte batteries are not only highly safe, but also highly reliable, highly environmentally resistant, and have a long lifespan, so they are expected to be maintenance-free batteries that can contribute to social development while also continuing to contribute to safety and security. By providing solid electrolyte batteries to society, we can contribute to the achievement of Goal 3 (Ensure healthy lives and promote well-being for all at all ages), Goal 7 (Ensure access to affordable, reliable, sustainable and modern energy for all), Goal 11 (Make cities and human settlements inclusive, safe, resilient and sustainable), and Goal 12 (Ensure sustainable consumption and production patterns) out of the 17 Sustainable Development Goals (SDGs) established by the United Nations.

[0008] Incidentally, in batteries such as solid electrolyte batteries, a pressurizing member that pressurizes power generating elements including electrodes inside an exterior body is sometimes used for the purpose of improving characteristics and productivity.

[0009] For example, Patent Document 1 proposes a sealed storage battery in which a pressure spacer that deforms to increase the volume it occupies within the cell chamber is arranged in the stacking direction of a plate group including the plates (electrodes), thereby improving the adhesion between the plates and the retainer.

[0010] Patent Document 2 proposes a secondary battery in which a member made of a shape-memory material such as a shape-memory alloy or a shape-memory resin that changes shape at a predetermined temperature is placed in a battery case that contains an electrode group and a solid electrolyte or an electrolyte solution, and pressure can be applied or released inside the battery case by heating or cooling. In Patent Document 2, as in Patent Document 1, a member made of a shape-memory material is placed so as to apply pressure to the electrode group in the stacking direction.

[0011] Furthermore, Patent Document 3 proposes a sulfide all-solid-state battery having a pressurizing member made of a material that expands without generating gas when heated, between an electrode body having a sulfide solid electrolyte and an exterior body. Patent Document 3 states that, according to the sulfide all-solid-state battery, the electrode body is housed in an exterior body, sealed, and then heated, so that the pressurizing member can be expanded to obtain a pressurizing force, and therefore the pressurizing member can be efficiently arranged to improve productivity. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Japanese Patent Application Publication No. 6-290805 [Patent Document 2] JP-A-8-64234 (claims, paragraphs

[0040] ,

[0064] , Figure 1, etc.) [Patent Document 3] JP 2022-156220 A Summary of the Invention [Problem to be solved by the invention]

[0013] However, in the case of the batteries described in Patent Documents 1 to 3, before the exterior body (battery case) is sealed, the electrodes (power generating elements) that make up the electrode body are simply stacked. Therefore, there is a risk of the power generating elements that make up the electrode body or the electrodes becoming misaligned during each manufacturing stage of the battery, such as when the electrode body is housed in the exterior body, when wiring is performed after the electrode body is housed in the exterior body, and when the exterior body is sealed. This leaves room for improvement in battery productivity and the reliability of the resulting batteries.

[0014] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a solid electrolyte battery with good productivity and reliability, and a method for producing the same. [Means for solving the problem]

[0015] The solid electrolyte battery of the present invention comprises an electrode body formed by stacking a plurality of pellet-shaped power generating elements, and an outer casing, each of the plurality of power generating elements being formed by stacking a positive electrode layer, a solid electrolyte layer and a negative electrode layer in order, the electrode body being contained within an insulating container and being enclosed within the outer casing with the side of the electrode body fixed to the inner surface of the container, and the container being formed from a shape memory resin that has the function of deforming from a shape it had at a temperature equal to or higher than a predetermined temperature at a temperature below the predetermined temperature, and returning to the shape before deformation when placed again at a temperature equal to or higher than the predetermined temperature.

[0016] In addition, the manufacturing method for a solid electrolyte battery of the present invention is a method for manufacturing a solid electrolyte battery having an electrode body formed by stacking a plurality of pellet-shaped power generating elements, an outer casing, and an insulating container that houses the electrode body and is enclosed in the outer casing, and is characterized by having the steps of: housing the electrode body in the container formed of a shape-memory resin that has a function of deforming from a shape it had at a temperature equal to or higher than a predetermined temperature at a temperature below the predetermined temperature and returning to the shape before deformation when placed again at a temperature equal to or higher than the predetermined temperature; and heating the container housing the electrode body to a temperature equal to or higher than the predetermined temperature to deform it, and fixing the side of the electrode body to the inner surface of the container. Effect of the Invention

[0017] According to the present invention, it is possible to provide a solid electrolyte battery with good productivity and reliability, and a method for producing the same. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a perspective view showing a schematic diagram of an example of a container that can be used for the solid electrolyte battery of the present invention. [Diagram 2] 2 is a perspective view showing a state in which an electrode assembly is housed in the housing of FIG. 1. FIG. [Diagram 3] FIG. 1 is a cross-sectional view illustrating a schematic example of a solid electrolyte battery of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The solid electrolyte battery of the present invention includes an electrode assembly including a plurality of pellet-shaped power generating elements each including a positive electrode layer, a solid electrolyte layer, and a negative electrode layer stacked in that order, and an outer casing. The electrode assembly is housed in an insulating container and enclosed in the outer casing, and the side of the electrode assembly is fixed to the inner surface of the container by, for example, closely contacting the inner surface of the container with the side of the electrode assembly.

[0020] Fig. 1 is a perspective view showing a schematic example of a container that can be used for a solid electrolyte battery. The container 10 shown in Fig. 1 has a bottomed cylindrical shape and is capable of housing an electrode assembly inside. The container 10 is made of a shape-memory resin (hereinafter simply referred to as "shape-memory resin") that has a function of deforming from a shape it had at a temperature equal to or higher than a predetermined temperature at a temperature lower than the predetermined temperature, and returning to the shape before the deformation when placed again at a temperature equal to or higher than the predetermined temperature.

[0021] Fig. 2 is a perspective view showing a schematic state in which the electrode body is accommodated inside the housing 10 of Fig. 1. The electrode body 20 accommodated in the housing 10 is formed by stacking a plurality of pellet-shaped power generating elements. One electrode layer (e.g., positive electrode layer) of each current collecting element constituting the electrode body 20 is conductively connected to each other through a conductive connection terminal (e.g., a positive electrode layer connection terminal) by welding the connection terminal to a lead 43, and the other electrode layers (e.g., negative electrode layer) are conductively connected to each other through a conductive connection terminal (e.g., a negative electrode layer connection terminal) by welding the connection terminal to a lead 54.

[0022] The container 10 for housing the electrode body is formed in advance at a temperature equal to or higher than the predetermined temperature into a shape such that the inner surface will come into close contact with the side surface of the housed electrode body after housing the electrode body at the temperature equal to or higher than the predetermined temperature [Fig. 1(a)], and before housing the electrode body, the container is deformed, for example, so that the opening diameter of the container is enlarged in order to make it easier to house the electrode body at a temperature lower than the predetermined temperature [Fig. 1(b)]. Then, by placing the container 10 after housing the electrode body at a temperature equal to or higher than the predetermined temperature again, the container 10 returns to the shape before deformation [Fig. 1(a)], and the inner surface of the container 10 and the side surface of the electrode body come into close contact with each other, and the container can be in the state shown in Fig. 2.

[0023] The housing 10 is also provided with slits 11, 11 for exposing the positive electrode layer connection terminal and the negative electrode layer connection terminal of the contained electrode body to the outside of the housing 10. That is, as shown in Fig. 2, the lead 43 and the electrode layer connection terminal attached to the lead 43, and the lead 54 and the electrode layer connection terminal attached to the lead 54 are exposed to the outside of the housing 10 from the slits 11, 11.

[0024] Next, an example of a solid electrolyte battery will be described with reference to the drawings. Fig. 3 is a cross-sectional view that shows a schematic diagram of an example of a solid electrolyte battery of the present invention. The cross section shown in Fig. 3 corresponds to the cross section of line II of the housing 10 housing the electrode assembly 20 shown in Fig. 2.

[0025] 3 has an electrode assembly 20 formed by stacking four pellet-shaped power generating elements 30, and an exterior body made up of a cylindrical metal exterior can 70 with a bottom and a metal lid 80. The exterior can and the lid can be made of aluminum, stainless steel, or the like.

[0026] A metal terminal 90 is attached to the lid 80 via an insulating packing 100 made of resin (such as polypropylene), glass hermetic, ceramic hermetic, or the like. When using an electrolyte that decomposes due to moisture in the air, such as a sulfide or hydride, it is desirable to use a more airtight glass hermetic or ceramic hermetic. The lid 80 is then inserted into the opening of the exterior can 70, and the opening of the exterior can 70 is sealed by welding the joint between the two, or the like, to hermetically seal the inside of the battery.

[0027] Each power generating element 30 of the electrode body 20 is formed by sequentially stacking a positive electrode layer 40, a solid electrolyte layer 60, and a negative electrode layer 50. The electrode body 20 is formed by stacking four power generating elements 30 in the vertical direction in the figure and connecting them in parallel to each other as described below.

[0028] The electrode body 20 is formed by stacking each power generating element 30 so that the electrode layers of the same polarity of adjacent power generating elements 30 face each other (for example, the power generating element 30 located at the top and the power generating element 30 adjacent thereto are stacked so that their positive electrode layers 40, 40 face each other).

[0029] Furthermore, a positive electrode layer connection terminal 41 for conducting electric power to the positive electrode layers 40, 40 is disposed between the positive electrode layer 40 of the power generating element 30 located at the top and the positive electrode layer 40 of the power generating element 30 adjacent thereto below. A positive electrode layer connection terminal 42 for conducting electric power to the positive electrode layers 40, 40 is disposed between the positive electrode layer 40 of the power generating element 30 located at the bottom and the positive electrode layer 40 of the power generating element 30 adjacent thereto above. Although not shown in Fig. 3, each of the positive electrode layer connection terminals 41, 42 is conductively connected to a lead (lead 43 in Fig. 2) by welding or the like, and for example, this lead is conductively connected to the inner surface of the exterior can 70 that also serves as the positive electrode terminal by welding or the like.

[0030] Moreover, a negative electrode layer connection terminal 51 for conducting with the negative electrode layer 50 and deriving electric power is disposed above the negative electrode layer 50 of the power generating element 30 located at the top. Furthermore, a negative electrode layer connection terminal 52 for conducting with the negative electrode layers 50, 50 and deriving electric power is disposed between the negative electrode layer 50 of the power generating element 30 located second from the top and the negative electrode layer 50 of the power generating element 30 adjacent thereto below. Moreover, a negative electrode layer connection terminal 53 for conducting with the negative electrode layer 50 and deriving electric power is disposed below the negative electrode layer 50 of the power generating element 30 located at the bottom. Although not shown in FIG. 3, the negative electrode layer connection terminals 51, 52, 53 are conductively connected to a lead (lead 54 in FIG. 2) by welding or the like. For example, the lead is conductively connected to the lower surface of the terminal 90 functioning as a negative electrode terminal by welding or the like.

[0031] Although FIG. 3 shows a solid electrolyte battery in an embodiment in which the outer can 70 also functions as a positive electrode terminal and the terminal 90 functions as a negative electrode terminal, if necessary, the outer can 70 may also function as a negative electrode terminal and the terminal 90 may function as a positive electrode terminal.

[0032] As shown in FIG. 3, in the solid electrolyte battery of the present invention, an electrode body formed by stacking a plurality of pellet-shaped power generating elements is housed in a container formed of a shape memory resin, and the side of the electrode body is fixed to the inner surface of the container by, for example, contacting the inner surface of the container with the side of the electrode body (i.e., the position of the power generating element constituting the electrode body in the container). Therefore, when the container containing the electrode body is housed in an exterior body (exterior can) and wiring is performed, the positional deviation between the power generating elements does not occur, improving the workability. As a result, high productivity can be ensured in the solid electrolyte battery of the present invention, and high reliability can also be ensured because the positional deviation between the power generating elements constituting the electrode body does not occur even in the battery state. Furthermore, the container can suppress contact between the electrode constituting the power generating element of the electrode body and the inner surface of the exterior can which also serves as the terminal of the counter electrode, so that the occurrence of a short circuit can also be effectively prevented. The electrode body can be fixed in the container by contacting the side of the electrode body with the inner surface of the container, but as long as the position of the electrode body in the container can be fixed, for example, the side of the electrode body and the inner surface of the container may be only partially in contact with each other.

[0033] Furthermore, by forming the container from a shape-memory resin, when the electrode body is contained, for example, the opening diameter can be made large to improve workability, and the container can be returned to its shape before deformation by a simple operation such as heating thereafter, thereby tightly adhering the container and the electrode body, and thus the electrode body can be fixed within the container. As a result, in the solid electrolyte battery of the present invention, a decrease in production efficiency due to an increase in the number of manufacturing steps due to operations such as containing the electrode body in the container and fixing the electrode body within the container is suppressed as much as possible.

[0034] A spacer 110 is disposed between the electrode body 20 and the terminal 90, and the electrode body 20 (each stacked power generation element 30) is pressed toward the bottom of the exterior can 70 by this spacer 110. As described below, the connection terminals connecting the electrode layers of each power generation element 30 may or may not be fixed to the adjacent electrode layers. Even if the connection terminals are not fixed to the electrode layers, the action of the spacer 110 can satisfactorily connect the connection terminals and the electrode layers, resulting in a solid electrolyte battery with superior characteristics. The spacer 110 can be made of a rubber plate, a metal spring (such as a leaf spring), or the like.

[0035] Next, the solid electrolyte battery of the present invention will be described in detail. The solid electrolyte battery of the present invention includes a primary battery and a secondary battery.

[0036] <Containment Unit> The container may be made of a shape-memory resin, and the predetermined temperature (the temperature at which the deformed shape returns to the original shape) of the shape-memory resin is preferably equal to or higher than the maximum temperature to which the battery is exposed during processing or use, and more specifically, is preferably 80 to 150°C. Examples of shape-memory resins that satisfy this requirement include polynorbornene, trans-polyisoprene, styrene-butadiene copolymer, and polyurethane. The thickness of the container (the thickness of the shape-memory resin that constitutes the container in a state in which it is in close contact with the contained electrode body) is preferably 10 to 1000 μm. If the container is too thin, the force that holds the container is weak and there is a risk that the shape cannot be maintained, and if the container is too thick, the volume of the container that occupies the internal volume of the battery becomes too large, and the energy density of the battery decreases.

[0037] As shown in FIG. 3, the housing may have a slit for exposing the connection terminal for connecting the positive electrode layers to each other or the connection terminal for connecting the negative electrode layers to each other to the outside of the housing if necessary, and may not have a slit if not necessary, for example, when the electrode body is formed by connecting the power generating elements to each other in series. When the power generating elements are connected in parallel to each other to form the electrode body as shown in FIG. 3, as described above, when the connection terminal for connecting the positive electrode layers to each other or the negative electrode layers to each other is connected to the lead, the work can be performed at the slit with each power generating element housed in the housing. Therefore, each power generating element can be housed in the housing, and each power generating element can be connected to each other in a state in which the housing is deformed by heating to fix each power generating element. Since it is possible to prevent the power generating elements from being misaligned during this connection, it is possible to further increase the productivity of the electrode body and, in turn, the productivity of the solid electrolyte battery.

[0038] The width of the slits in the container may be such that the electrode layer connection terminals and the leads to which these connection terminals are attached can be sufficiently exposed from each slit, but if the width is too wide, there is a risk that the container will not have sufficient strength, so it is preferable that the width (the total width, if there are multiple slits) be 30% or less of the outer periphery of the container when viewed in a plane.

[0039] <Positive electrode layer> The positive electrode layer of the solid electrolyte battery can be formed, for example, by molding a positive electrode mixture containing a positive electrode active material and the like.

[0040] When the solid electrolyte battery is a primary battery, the positive electrode active material can be the same as the positive electrode active material used in conventionally known non-aqueous electrolyte primary batteries. Specifically, for example, manganese dioxide, lithium-containing manganese oxide (e.g., LiMn3O6, or a composite oxide having the same crystal structure as manganese dioxide (e.g., β-type, γ-type, or a structure in which β-type and γ-type are mixed) and a Li content of 3.5 mass% or less, preferably 2 mass% or less, more preferably 1.5 mass% or less, and particularly preferably 1 mass% or less), Li a Ti 5 / 3Lithium-containing composite oxides such as O4 (4 / 3 ≤ a < 7 / 3); vanadium oxides; niobium oxides; titanium oxides; sulfides such as iron disulfide; graphite fluoride; silver sulfides such as Ag2S; nickel oxides such as NiO2; and the like can be mentioned.

[0041] When the solid electrolyte battery is a secondary battery, the positive electrode active material is not particularly limited as long as it is a positive electrode active material conventionally used in non-aqueous electrolyte secondary batteries, that is, an active material capable of occluding and releasing Li ions. Specific examples of the positive electrode active material include LiM r Mn 2-r O4 (where M is at least one element selected from the group consisting of Li, Na, K, B, Mg, Ca, Sr, Ba, Ti, V, Cr, Zr, Fe, Co, Ni, Cu, Zn, Al, Sn, Sb, In, Nb, Ta, Mo, W, Y, Ru, and Rh, and 0 ≤ r ≤ 1), a spinel-type lithium manganese composite oxide represented by r Mn (1-s-r) Ni s M t O (2-u) F v (where M is at least one element selected from the group consisting of Co, Mg, Al, B, Ti, V, Cr, Fe, Cu, Zn, Zr, Mo, Sn, Ca, Sr, and W, 0.8 ≤ r ≤ 1.2, 0 < s < 0.5, 0 ≤ t ≤ 0.5, u + v < 1, -0.1 ≤ u ≤ 0.2, 0 ≤ v ≤ 0.1), a layered compound represented by LiCo 1-r M r O2 (where M is at least one element selected from the group consisting of Al, Mg, Ti, V, Cr, Zr, Fe, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≤ r ≤ 0.5), a lithium cobalt composite oxide represented by 1-r M r O2 (where M is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Fe, Co, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≤ r ≤ 0.5), a lithium nickel composite oxide represented by 1+s M 1-r N r PO4F s(wherein M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0≦r≦0.5, 0≦s≦1), an olivine-type composite oxide represented by Li2M 1-r N r Examples of such compounds include pyrophosphate compounds represented by the formula: P2O7 (wherein M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0≦r≦0.5). Among these compounds, only one may be used, or two or more may be used in combination.

[0042] When the solid electrolyte battery is a secondary battery, the average particle size of the positive electrode active material is preferably 0.1 μm or more, more preferably 0.5 μm or more, and more preferably 25 μm or less, more preferably 10 μm or less, from the viewpoint of reducing side reactions that cause capacity deterioration of the battery and increasing the density of the positive electrode. The positive electrode active material may be primary particles or secondary particles formed by agglomeration of primary particles. When the positive electrode layer contains a solid electrolyte, using a positive electrode active material having an average particle size in the above range can provide a large interface with the solid electrolyte, thereby further improving the load characteristics of the battery.

[0043] The average particle diameter of the positive electrode active material and the average particle diameter of other particles (such as solid electrolytes) in this specification are the 50% diameter value (D) in the volume-based integrated fraction when calculating the integral volume from small particles using a particle size distribution measurement device (such as the Microtrac particle size distribution measurement device "HRA9320" manufactured by Nikkiso Co., Ltd.). 50 )

[0044] When the positive electrode layer contains a solid electrolyte, the positive electrode active material preferably has a reaction suppression layer on its surface for suppressing reaction with the solid electrolyte contained in the positive electrode layer.

[0045] In the positive electrode layer, if the positive electrode active material and the solid electrolyte come into direct contact with each other, the solid electrolyte may oxidize to form a resistance layer, which may reduce the ionic conductivity in the layer. By providing a reaction suppression layer that suppresses the reaction with the solid electrolyte on the surface of the positive electrode active material and preventing direct contact between the positive electrode active material and the solid electrolyte, it is possible to suppress the reduction in the ionic conductivity in the positive electrode layer due to the oxidation of the solid electrolyte.

[0046] The reaction suppression layer may be made of a material that has ion conductivity and can suppress the reaction between the positive electrode active material and the solid electrolyte. Examples of materials that can form the reaction suppression layer include oxides containing Li and at least one element selected from the group consisting of Nb, P, B, Si, Ge, Ti, Zr, Ta, and W, more specifically, Nb-containing oxides such as LiNbO3, Li3PO4, Li3BO3, Li4SiO4, Li4GeO4, LiTiO3, LiZrO3, Li2WO4, and the like. The reaction suppression layer may contain only one of these oxides, or may contain two or more of them, and further, a plurality of these oxides may form a composite compound. Among these oxides, it is preferable to use an Nb-containing oxide, and it is more preferable to use LiNbO3.

[0047] The reaction suppression layer is preferably present on the surface in an amount of 0.1 to 2.0 parts by mass per 100 parts by mass of the positive electrode active material, in order to effectively suppress the reaction between the positive electrode active material and the solid electrolyte.

[0048] Methods for forming a reaction suppression layer on the surface of a positive electrode active material include the sol-gel method, the mechanofusion method, the CVD method, the PVD method, and the ALD method.

[0049] The content of the positive electrode active material in the positive electrode layer is preferably 20 to 95 mass %.

[0050] Examples of the conductive assistant for the positive electrode include carbon materials such as carbon black (thermal black, furnace black, channel black, ketjen black, acetylene black, etc.), graphite (natural graphite, artificial graphite), graphene, vapor-grown carbon fiber, carbon nanofiber, and carbon nanotube; powders of Cu, Ni, Al, Au, and Pd alone or alloys thereof, or porous bodies thereof; and these may be used alone or in combination of two or more. The content of the conductive assistant in the positive electrode layer is preferably 0.1 to 15 mass%.

[0051] The positive electrode layer can contain a solid electrolyte. The solid electrolyte used in the positive electrode layer is not particularly limited as long as it has Li-ion conductivity, and examples of the solid electrolyte that can be used include sulfide-based solid electrolytes, hydride-based solid electrolytes, halide-based solid electrolytes, and oxide-based solid electrolytes.

[0052] Examples of sulfide-based solid electrolytes include particles of Li2S-P2S5, Li2S-SiS2, Li2S-P2S5-GeS2, and Li2S-B2S3-based glass. In addition, thio-LISICON-type electrolytes [Li 10 GeP2S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 Li 12-12a-b+c+6d-e M 1 3+a-b-c-d M 2 b M 3 c M 4 d M 5 12-e X e (However, M 1 is Si, Ge or Sn, M 2 is P or V, M 3 is Al, Ga, Y or Sb, M 4 is Zn, Ca, Ba, M 5is either S or S and O, X is F, Cl, Br or I, 0 ≦ a < 3, 0 ≦ b + c + d ≦ 3, 0 ≦ e ≦ 3), or an argyrodite type (such as Li6PS5Cl, Li 7-f+g PS 6-x Cl x+y (where 0.05 ≦ f ≦ 0.9, -3.0f + 1.8 ≦ g ≦ -3.0f + 5.7), Li 7-h PS 6-h Cl i Br j (where h = i + j, 0 < h ≦ 1.8, 0.1 ≦ i / j ≦ 10.0), etc.) can also be used.

[0053] Examples of the hydride-based solid electrolyte include LiBH4, a solid solution of LiBH4 and the following alkali metal compound (for example, those with a molar ratio of LiBH4 to the alkali metal compound of 1:1 to 20:1). Examples of the alkali metal compound in the solid solution include lithium halides (such as LiI, LiBr, LiF, LiCl), rubidium halides (such as RbI, RbBr, RbF, RbCl), cesium halides (such as CsI, CsBr, CsF, CsCl), lithium amide, rubidium amide, and at least one selected from the group consisting of cesium amide.

[0054] Examples of the halide-based solid electrolyte include monoclinic LiAlCl4, defective spinel-type or layered-structured LiInBr4, monoclinic Li 6-3m Y m X6 (where 0 < m < 2 and X = Cl or Br), etc., and in addition, for example, those known from International Publication No. 2020 / 070958 and International Publication No. 2020 / 070955 can be used.

[0055] Examples of the oxide-based solid electrolyte include Li2O - Al2O3 - SiO2 - P2O5 - TiO2 - based glass ceramics, Li2O - Al2O3 - SiO2 - P2O5 - GeO2 - based glass ceramics, garnet-type Li7La3Zr2O 12 , NASICON-type Li 1+O Al1+O Ti 2-O (PO4)3, Li 1+p Al 1+p Ge 2-p (PO4)3, perovskite-type Li 3q La 2 / 3-q Examples include TiO3.

[0056] Among these solid electrolytes, sulfide-based solid electrolytes are preferred due to their high Li-ion conductivity, sulfide-based solid electrolytes containing Li and P are more preferred, and argyrodite-type sulfide-based solid electrolytes, which have particularly high Li-ion conductivity and high chemical stability, are even more preferred.

[0057] The content of the solid electrolyte in the positive electrode layer is preferably 4 to 80 mass %.

[0058] The positive electrode layer may contain a binder, or may not contain a binder when good moldability can be ensured without using a binder, such as in the case of a positive electrode in which a sulfide-based solid electrolyte is contained and powder of the positive electrode mixture is charged into a molding die and compacted.

[0059] The binder contained in the positive electrode layer may be a fluororesin such as PVDF.

[0060] When the positive electrode layer requires a binder, the content is preferably 15% by mass or less, and more preferably 0.5% by mass or more. On the other hand, when the positive electrode layer requires no binder from the viewpoint of formability, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).

[0061] The positive electrode layer may have a current collector. Examples of the current collector for the positive electrode layer include metal foils such as aluminum and stainless steel; sheet-shaped conductive porous substrates such as punched metal, net, expanded metal, and foamed metal; and carbon sheets. As the sheet-shaped conductive porous substrate, it is preferable to use a foamed metal porous body. A specific example of the foamed metal porous body is "Celmet (registered trademark)" by Sumitomo Electric Industries, Ltd.

[0062] The positive electrode layer can be formed, for example, by compressing a positive electrode mixture prepared by mixing a positive electrode active material, a conductive assistant, a solid electrolyte, and further a binder added as necessary, by pressure molding or the like.

[0063] In the case of a positive electrode layer having a current collector, the layer can be formed by, for example, pressing a current collector onto a pressed molded body of the positive electrode mixture obtained as described above.

[0064] The thickness of the positive electrode layer is usually 50 μm or more, but from the viewpoint of increasing the capacity of the battery, it is preferably 200 μm or more, and the thickness of the positive electrode layer is usually 2000 μm or less.

[0065] The thickness of the current collector for the positive electrode layer is preferably 0.01 to 0.1 mm.

[0066] <Negative electrode layer> The negative electrode layer of the solid electrolyte battery can be formed, for example, by molding a negative electrode mixture containing a negative electrode active material and the like.

[0067] When the solid electrolyte battery is a primary battery, examples of the negative electrode active material include metallic lithium and lithium alloys (lithium-aluminum alloys, lithium-indium alloys, etc.).

[0068] When the solid electrolyte battery is a secondary battery, the negative electrode active material may be, for example, one or a mixture of two or more carbonaceous materials capable of absorbing and releasing lithium, such as graphite, pyrolytic carbons, cokes, glassy carbons, fired organic polymer compounds, mesocarbon microbeads (MCMB), and carbon fibers. In addition, simple substances, compounds and alloys thereof containing elements such as Si, Sn, Ge, Bi, Sb, and In; compounds capable of charging and discharging at a low voltage close to that of lithium metal, such as lithium-containing nitrides or lithium-containing oxides; lithium metal; and lithium / aluminum alloys. For example, Li4Ti5O 12 , TiO2, NbO 2.5-δ (0≦δ≦0.5), MoO 3-δ (0≦δ≦1), WO 3-δ (0≦δ≦1), a metal oxide such as TiNb2O7; or a metal sulfide such as WS2 or MoS2; or a mixture of two or more of these may also be used as the negative electrode active material.

[0069] The content of the negative electrode active material in the negative electrode layer is preferably 50 to 95 mass %.

[0070] The negative electrode layer can contain a solid electrolyte. The solid electrolyte contained in the negative electrode layer can be one or more of the sulfide-based solid electrolyte, hydride-based solid electrolyte, and oxide-based solid electrolyte exemplified above as the solid electrolyte that can be contained in the positive electrode layer. Among the above-mentioned solid electrolytes, it is more preferable to use a sulfide-based solid electrolyte because it has high Li-ion conductivity and has a function of enhancing the negative electrode layer, and it is even more preferable to use an argyrodite-type sulfide-based solid electrolyte.

[0071] The content of the solid electrolyte in the negative electrode layer is preferably 4 to 70 mass %.

[0072] The negative electrode layer may contain a conductive assistant. Specific examples of the conductive assistant include carbon materials such as graphite (natural graphite, artificial graphite), graphene, carbon black, vapor-grown carbon fiber, carbon nanofiber, and carbon nanotube. The content of the conductive assistant in the negative electrode layer is preferably 1 to 10 mass %.

[0073] The negative electrode layer may or may not contain a binder. Specific examples thereof include the same binders as those exemplified above as those that may be contained in the positive electrode layer. Note that, for example, in the case where the negative electrode layer contains a sulfide-based solid electrolyte, if good moldability can be ensured in forming the negative electrode layer without using a binder, the negative electrode layer may not contain a binder.

[0074] When the negative electrode layer requires a binder, the content is preferably 15% by mass or less, and more preferably 0.5% by mass or more. On the other hand, when good moldability can be obtained without the binder in the negative electrode layer, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).

[0075] The negative electrode layer may have a current collector. As the current collector for the negative electrode layer, a sheet-like conductive porous substrate such as copper or nickel foil, punched metal, net, expanded metal, foamed metal, etc.; a carbon sheet; etc. can be used. As the sheet-like conductive porous substrate, it is preferable to use a foamed metal porous body. A specific example of the foamed metal porous body is "Celmet (registered trademark)" by Sumitomo Electric Industries, Ltd.

[0076] The negative electrode layer can be formed, for example, by compressing, by pressure molding, a negative electrode mixture prepared by mixing a negative electrode active material, a conductive assistant, a solid electrolyte, and further a binder added as necessary.

[0077] In the case of a negative electrode layer having a current collector, the layer can be formed by, for example, pressing a current collector onto a pressed molded product of the negative electrode mixture obtained as described above.

[0078] The thickness of the negative electrode layer is usually 100 μm or more, but from the viewpoint of increasing the capacity of the battery, it is preferably 200 μm or more, and the thickness of the negative electrode layer is usually 3000 μm or less.

[0079] The thickness of the current collector for the negative electrode layer is preferably 0.01 to 0.1 mm.

[0080] <Solid electrolyte layer> The solid electrolyte layer in the solid electrolyte battery can use one or more of the sulfide-based solid electrolyte, hydride-based solid electrolyte, and oxide-based solid electrolyte exemplified above as the solid electrolyte that can be contained in the positive electrode layer. Among the above-mentioned solid electrolytes, it is more preferable to use a sulfide-based solid electrolyte, and it is even more preferable to use an argyrodite-type sulfide-based solid electrolyte, in order to improve the battery characteristics.

[0081] The solid electrolyte layer can be formed by a method of compressing a solid electrolyte by pressure molding or the like; a method of applying a composition for forming a solid electrolyte layer, which is prepared by dispersing a solid electrolyte in a solvent, onto a substrate, a positive electrode, or a negative electrode, drying the composition, and, if necessary, performing pressure molding such as pressing.

[0082] The solid electrolyte layer may have a porous body such as a resin nonwoven fabric as a support.

[0083] It is preferable to select a solvent that does not deteriorate the solid electrolyte for use in the composition for forming the solid electrolyte layer. In particular, since sulfide-based solid electrolytes and hydride-based solid electrolytes undergo chemical reactions due to a small amount of water, it is preferable to use a non-polar aprotic solvent represented by a hydrocarbon solvent such as hexane, heptane, octane, nonane, decane, decalin, toluene, or xylene. In particular, it is more preferable to use an ultra-dehydrated solvent with a water content of 0.001 mass% (10 ppm) or less. In addition, fluorine-based solvents such as "Vertrel (registered trademark)" manufactured by Mitsui DuPont Fluorochemicals, "Zeorolla (registered trademark)" manufactured by Nippon Zeon Co., Ltd., and "Novec (registered trademark)" manufactured by Sumitomo 3M Co., Ltd., as well as non-aqueous organic solvents such as dichloromethane and diethyl ether can also be used.

[0084] The thickness of the solid electrolyte layer is preferably 10 to 500 μm.

[0085] <Power generating element and electrode body> The power generating element is in the form of a pellet, and is formed by sequentially stacking a positive electrode layer, a solid electrolyte layer, and a negative electrode layer. To obtain the power generating element, for example, a method can be adopted in which a positive electrode layer (or a negative electrode layer) is formed in advance by pressure molding, and the solid electrolyte layer and a negative electrode layer (or a positive electrode layer) are sequentially formed by pressure molding using the positive electrode layer as a base material, or a positive electrode layer is formed by pressure molding on one side of a solid electrolyte layer previously formed by pressure molding, and a negative electrode layer is formed by pressure molding on the other side of the solid electrolyte layer.

[0086] The shape of the power generating element in a plan view is not particularly limited, and may be a circle, an ellipse, or a polygon such as a rectangle.

[0087] The electrode body is formed by stacking a plurality of power generating elements and connecting adjacent power generating elements in parallel or in series. When connecting power generating elements in parallel, for example, a method of stacking adjacent power generating elements so that their electrode layers of the same polarity face each other as shown in Fig. 3 can be used.

[0088] When the power generating elements are connected in series, for example, a method can be employed in which adjacent power generating elements are stacked such that their electrode layers of opposite polarity face each other.

[0089] In both cases of connecting the power generating elements in parallel and in series, the opposing electrode layers may be electrically connected by interposing a conductive connection terminal between them. The connection terminal that electrically connects the electrode layers may be fixed to either one of the opposing electrode layers, or may not be fixed to either of the electrode layers. When fixing the connection terminal to the electrode layer, for example, the current collector of an electrode layer having a metal current collector may be welded to the connection terminal.

[0090] The number of power generating elements in the electrode body is not particularly limited as long as it is multiple (two or more), and it is possible to have 10, 20 or more depending on the characteristics required of the solid electrolyte battery.

[0091] <Connection terminals and leads> The connection terminals for extracting electricity from the electrode layer of the power generation element (connection terminals that connect the electrode layers of adjacent power generation elements) and the leads for connecting the connection terminals together can be made of metallic foils (plates) such as stainless steel, nickel, aluminum, iron, copper, clad materials that combine these, and materials made from these materials that have been plated with nickel, chromium, nickel chromium, etc.

[0092] The thickness of the connection terminals and leads made of metal foil (plate) is preferably 10 to 100 μm. There are no particular limitations on the size of the connection terminals and leads, but when they are exposed to the outside of the housing through a slit in the housing, their width is made shorter than the width of the slit.

[0093] <Exterior body> The exterior body of the solid electrolyte battery is not particularly limited, but since the electrode body contained therein is formed by stacking a plurality of power generating elements, a configuration having a bottomed tubular exterior can (rectangular tubular can, cylindrical can) and a lid body as shown in Fig. 3 is preferably used. The exterior can and the lid body can be connected by welding or crimping with a gasket.

[0094] <Solid electrolyte battery manufacturing method> The solid electrolyte battery can be manufactured, for example, by the following method. First, a container made of a shape-memory resin is molded into a shape that will adhere to the side of the electrode body after accommodation at a temperature equal to or higher than a predetermined temperature at which the shape-memory resin memorizes the shape, and then the container is deformed into a shape that makes it easy to insert the electrode body at a temperature lower than the predetermined temperature. The electrode body with the power generation element stacked thereon is inserted into the container, and the container is returned to its original shape at a temperature equal to or higher than the predetermined temperature, and the side of the electrode body is fixed to the inner surface of the container by adhering the container and the electrode body to each other. The connection between the power generation elements in the electrode body can be performed after fixing each power generation element in the container by using a container having a slit as described above, for example, in the case of an electrode body that connects the power generation elements in parallel.

[0095] The housing with the electrode assembly fixed inside is housed in an outer can, and after necessary wiring is provided, the opening of the outer can is sealed with a lid to form an outer casing, completing the solid electrolyte battery. [Industrial Applicability]

[0096] The solid electrolyte battery of the present invention can be used in the same applications as conventionally known primary batteries and secondary batteries, but since it has excellent heat resistance as described above, it can be preferably used in applications where it is exposed to high temperatures. [Explanation of symbols]

[0097] 1 Solid electrolyte battery 10 Containment Unit 20 Electrode body 30 Power generation elements 40 Positive electrode layer 41, 42 Positive electrode layer connection terminal 43 Lead 50 Negative electrode layer 51, 52, 53 Negative electrode layer connection terminals 54 Lead 60 Solid electrolyte layer 70 Outer can 80 Lid 90 Terminal 100 Insulating packing 110 Spacer

Claims

1. The battery has an electrode assembly formed by stacking a plurality of pellet-shaped power generating elements, and an exterior body, Each of the plurality of power generating elements is formed by sequentially stacking a positive electrode layer, a solid electrolyte layer, and a negative electrode layer, The electrode body is accommodated in an insulating container, and is enclosed in the exterior body in a state where a side surface of the electrode body is fixed to an inner surface of the container, a solid electrolyte battery characterized in that the container is formed from a shape-memory resin that has a function of being deformed from a shape it has at a temperature equal to or higher than a predetermined temperature at a temperature lower than the predetermined temperature, and returning to the shape before the deformation when placed again at a temperature equal to or higher than the predetermined temperature.

2. 2. The solid electrolyte battery according to claim 1, wherein adjacent power generating elements are connected in series.

3. a conductive positive electrode layer connection terminal that is electrically connected to the positive electrode layer and capable of drawing out electric power from the positive electrode layer, and a conductive negative electrode layer connection terminal that is electrically connected to the negative electrode layer and capable of drawing out electric power from the negative electrode layer, 2. The solid electrolyte battery according to claim 1, wherein adjacent power generating elements are connected in parallel via the positive electrode layer connecting terminal and the negative electrode layer connecting terminal.

4. 4. The solid electrolyte battery according to claim 3, wherein a side surface of the container has slits for exposing the positive electrode layer connection terminal and the negative electrode layer connection terminal to the outside of the container.

5. A method for producing a solid electrolyte battery having an electrode assembly formed by stacking a plurality of pellet-shaped power generating elements, an outer casing, and an insulating container that houses the electrode assembly and is enclosed in the outer casing, comprising the steps of: a step of housing the electrode assembly in the housing formed of a shape-memory resin having a function of being deformed from a shape that it had at a temperature equal to or higher than a predetermined temperature at a temperature lower than the predetermined temperature, and returning to the shape before the deformation when it is placed again at a temperature equal to or higher than the predetermined temperature; a step of heating the housing containing the electrode body to a predetermined temperature or higher to deform the housing, and fixing a side surface of the electrode body to an inner surface of the housing.

Citation Information

Patent Citations

  • Sealed storage battery

    JP1994290805A

  • Secondary battery and its manufacture