Evaluation-purpose method of stress corrosion crack resistance in liquid ammonia

A method using a small pressure vessel with controlled impurities and a reference test piece promotes SCC in liquid ammonia, addressing inefficiencies in current SCC evaluation methods by stabilizing the test environment and enabling accurate SCC susceptibility assessment.

JP2024165864AActive Publication Date: 2024-11-28NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2023082420
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

Current methods for evaluating stress corrosion cracking (SCC) in liquid ammonia are inefficient, require large pressure vessels, and lack precise control over test environment purity and impurity concentrations, making it difficult to accurately reproduce SCC phenomena in steel materials.

Method used

A method using a small pressure vessel with controlled impurities and a reference test piece to promote SCC through catalytic corrosion of different metals, involving a bending test jig, ammonium carbamate, and oxygen gas to stabilize the test environment, allowing for SCC evaluation in high-strength steel.

Benefits of technology

Enables stable and accelerated reproduction of SCC in a laboratory setting, facilitating efficient evaluation of SCC susceptibility in steel materials under controlled conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165864000001_ABST
    Figure 2024165864000001_ABST
Patent Text Reader

Abstract

To provide an evaluation-purpose method of stress corrosion crack resistance in liquid ammonia, capable of evaluating a SCC sensitivity through accelerating and reproducing a SCC generated in a steel material by liquid ammonia in a laboratory, utilizing a small pressure vessel.SOLUTION: An evaluation-purpose method includes: a step of installing, respectively in different pressure containers, reference-purpose and evaluation-purpose test pieces to which a surface strain is applied by a test jig, introducing carbamic acid ammonium, liquid ammonia and an oxygen gas of prescribed purity or higher to the respective pressure containers, and compressing and holding for one hour or more; and a step of confirming an existence / nonexistence of a stress corrosion crack after an elapse of testing time. In the reference test piece, a Vickers hardness is 230 HV or more. Each test piece is electrically conducted to the test jig. In a test environment, the evaluation-purpose test piece is baser than stainless steel. When an occurrence of a stress corrosion crack is recognized in the reference-purpose test piece, an evaluation of a stress corrosion crack to the evaluation-purpose test piece is regarded valid.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating stress corrosion cracking properties in liquid ammonia. [Background technology]

[0002] Ammonia has been widely used for various purposes, such as raw material for fertilizers and refrigerant. In recent years, the need for global warming countermeasures has increased, and ammonia has attracted attention as a next-generation energy source due to its characteristic of not emitting CO2 when burned. It is expected that CO2 emissions will be reduced through the co-firing and exclusive combustion of ammonia in thermal power generation, industry, engines, etc. In order to supply huge amounts of ammonia for these purposes, efficient storage and transportation of ammonia is necessary, and there is a demand for the construction of large ammonia tanks made of high-strength steel.

[0003] However, ammonia is corrosive to steel, and steel may undergo stress corrosion cracking (hereinafter sometimes referred to as "SCC") in liquid ammonia. For this reason, the strength of steel used in ammonia tanks is currently limited. However, if high-strength steel is used to manufacture large ammonia tanks in the future, the welding residual stress of the welded joints will increase, and the design stress will also increase, increasing the SCC susceptibility. Therefore, it is necessary to properly evaluate the SCC properties of high-strength steel and its welds in liquid ammonia, and then design and manufacture large ammonia tanks made of high-strength steel under conditions where SCC does not occur.

[0004] SCC of steel in liquid ammonia is said to be active path corrosion type SCC, and when a corrosion film is formed on the inner surface of the tank that comes into contact with ammonia during long-term use of the liquid ammonia tank, and the film is locally destroyed by welding residual stress or hoop stress due to internal pressure, a new surface is exposed, and the new surface corrodes and dissolves preferentially, leading to cracks. If we try to accurately reproduce this type of SCC phenomenon, it will take an enormous amount of time (several years to several decades) equivalent to SCC in an actual tank, which makes the test efficiency extremely poor.

[0005] In order to reproduce the SCC phenomenon in a laboratory, for example, Patent Document 1 describes a method for producing a mixture of liquid ammonia at 25°C, saturated CO2 (a sufficient amount of ammonium carbamate: NH4CO2NH2) and 1 kgf / cm3 as an SCC accelerator. 2 A technology has been disclosed that reproduces SCC in 168 hours by adding 100 MPa of O2 and then applying a constant potential (2 V against a platinum electrode, polarization toward the anode side) to a four-point bending test piece in liquid ammonia via a constant potential generator (potentiostat).

[0006] Furthermore, Patent Document 2 discloses a technique in which, although the test specimen is not anodically polarized, the test specimen is bent into a U shape to impart plastic strain, thereby promoting film destruction, and furthermore, by adding CO2 (ammonium carbamate) and oxygen as environmental acceleration factors, the specimen is immersed in liquid ammonia at 25°C for 1,000 hours to reproduce SCC.

[0007] Furthermore, Non-Patent Document 1 discloses a technique for reproducing SCC by electrically connecting a carbon steel test piece to a stainless steel container and polarizing the carbon steel test piece through dissimilar metal contact. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 57-137096 [Patent Document 2] Japanese Patent Application Publication No. 11-131178 [Non-patent literature]

[0009] [Non-Patent Document 1] Hiroyuki Imagawa, Anodic Polarization and Corrosion Cracking Behavior of High Tensile Steel in Liquid Ammonia, Journal of the Japan Institute of Metals, Vol. 40, No. 12, 1976, pp. 1256-1263 Summary of the Invention [Problem to be solved by the invention]

[0010] Incidentally, the SCC of steel in liquid ammonia is temperature dependent, with the SCC susceptibility being higher at room temperature (20-25°C) than at low temperatures. However, in order to keep ammonia in a liquid state at room temperature, high pressure (e.g., 0.86 MPa or more at 20°C) is required. Therefore, to perform SCC evaluation tests of steel in liquid ammonia under strict conditions, such as room temperature, a pressure vessel (autoclave) is required, which imposes experimental constraints. In addition, care must be taken to prevent ammonia from leaking during testing, making handling extremely cumbersome.

[0011] In the technology described in Patent Document 1, multiple test pieces are simultaneously placed in a pressure vessel for evaluation, aiming at the efficiency of the test. When multiple test pieces are placed inside, the dimensions of the pressure vessel become large, but it is desirable to use a smaller pressure vessel in order to suppress leakage of ammonia. However, when the pressure vessel is made small, it is not possible to place a reference electrode or a counter electrode required for applying a constant potential or a constant current to the test piece in the narrow pressure vessel, and it becomes impossible to use a potentiostat that applies a constant potential or a galvanostat that passes a constant current.

[0012] Furthermore, neither Patent Document 1 nor Patent Document 2, nor Non-Patent Document 1, specifies whether the test environment in the same SCC test was appropriately and strictly controlled, and there is a possibility that the test conditions are not strictly controlled in the techniques described therein.

[0013] The SCC of steel in liquid ammonia is easily affected by trace amounts of impurities mixed into the liquid ammonia, and if the trace amounts of impurities in the test environment are not appropriately controlled, the SCC will not be reproduced, resulting in an inappropriate evaluation. However, it is extremely complicated and unrealistic to analyze the types and concentrations of impurities in the environment with high precision for each test. Therefore, a test method is required that shows that the test environment including the evaluation material is appropriately performed to reproduce liquid ammonia SCC, with the ammonia purity and the concentrations of added substances appropriately limited in advance. However, neither Patent Document 1 nor Patent Document 2 specifies the purity or concentration of each substance used to reproduce the test environment, and the type and concentration of impurities in the test environment are unclear in the current evaluation of SCC in liquid ammonia. Although Non-Patent Document 1 specifies the purity of ammonia, the purity or concentration of each of the other substances is not specified. In Non-Patent Document 1, ammonium chloride (NH4Cl) and ammonium sulfate ((NH4)2SO4) are added to liquid ammonia, the purity of which is unclear, and nitrogen gas is used for pressurization.

[0014] As described above, the current evaluation of SCC in liquid ammonia lacks sufficient control of the test environment and impurities, and when a small pressure vessel is used, it is not possible to install the reference electrode and counter electrode required to apply a constant potential or pass a constant current to the test specimen inside the pressure vessel.

[0015] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for evaluating stress corrosion cracking properties in liquid ammonia, which uses a small pressure vessel to accelerate and stably reproduce SCC caused by liquid ammonia in a laboratory, and enables evaluation of SCC susceptibility. [Means for solving the problem]

[0016] The inventors have come up with the idea of ​​appropriately managing the test environment and impurities, something that has not been done before, and furthermore, placing a reference test piece, which has been confirmed to develop SCC, in a pressure vessel different from that of the evaluation test piece, and promoting SCC through galvanic corrosion, thereby downsizing the pressure vessel. By conducting a test under conditions that would cause SCC in the reference test piece and by confirming that SCC has developed in the reference test piece, it is guaranteed that the test environment is appropriately set up to reproduce liquid ammonia SCC.

[0017] The gist of the present invention is as follows. [1] A method for evaluating stress corrosion cracking properties in liquid ammonia according to one embodiment of the present invention includes the steps of: placing a reference test piece and an evaluation test piece, each of which has been given a surface strain by a bending test jig, in different pressure vessels; filling each of the pressure vessels with an ammonia solution containing 3 mass % or more of ammonium carbamate; pressurizing each of the pressure vessels by introducing oxygen gas into the pressure vessels; maintaining the pressurized state for a test time during which stress corrosion cracking occurred in the reference test piece in a previously performed test; and confirming whether or not stress corrosion cracking occurred after the test time has elapsed. The material of the reference test piece has a Vickers hardness of 23. the reference test piece and the evaluation test piece are electrically connected to each of the bending test jigs; the purity of the liquid ammonia constituting the ammonia solution is 99.9% or more, the purity of the ammonium carbamate is 97.0% or more, and the purity of the oxygen gas is 99.9% or more; and if the occurrence of stress corrosion cracking is confirmed in the reference test piece in the confirmation process, the evaluation of stress corrosion cracking of the evaluation test piece is valid. [2] In the method for evaluating stress corrosion cracking properties in liquid ammonia described in [1] above, in the pressurizing step and the testing step, the O2 partial pressure in the pressure vessel is set to 0.5 kgf / cm 2 More than 5.0kgf / cm 2The following may also be used. [3] In the method for evaluating stress corrosion cracking properties in liquid ammonia according to the above [1] or [2], the surface strain may be 0.6 times or more the yield strain. [4] In the method for evaluating stress corrosion cracking properties in liquid ammonia according to any one of [1] to [3] above, the bending test jig may be a four-point bending test jig, and the reference test piece and the evaluation test piece may be supported at a constant displacement via stainless steel pins. Effect of the Invention

[0018] According to the present invention, it is possible to provide a method for evaluating stress corrosion cracking properties in liquid ammonia, which uses a small pressure vessel to accelerate and stably reproduce SCC caused by liquid ammonia in a laboratory and enables evaluation of SCC susceptibility. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a schematic diagram showing an example of a test device that can be used in a method for evaluating stress corrosion cracking properties in liquid ammonia according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] <Evaluation method for stress corrosion cracking properties in liquid ammonia> The method for evaluating the stress corrosion cracking property in liquid ammonia according to the embodiment of the present invention will be described. The method for evaluating the stress corrosion cracking property in liquid ammonia according to the present embodiment includes an installation step of installing a reference test piece and an evaluation test piece, each of which has been given a surface strain by a bending test jig, in different pressure vessels, a filling step of filling each pressure vessel with an ammonia solution containing 3 mass % or more of ammonium carbamate, a pressurizing step of introducing oxygen gas into each pressure vessel to pressurize it, a testing step of maintaining the pressurized state for a test time during which stress corrosion cracking occurred in the reference test piece in a test carried out in advance, and a confirmation step of confirming whether or not stress corrosion cracking occurred after the test time has elapsed.

[0021] FIG. 1 is a schematic diagram showing an example of a test apparatus that can be used in the method for evaluating stress corrosion cracking properties in liquid ammonia according to one embodiment of the present invention. FIG. 1 shows a state in which a test piece 2 to which surface strain is applied by a bending test jig 3 is placed inside a pressure vessel 1, and powdered ammonium carbamate 4 and an ammonia solution 5 in which ammonium carbamate is dissolved are placed. The test piece 2 corresponds to a reference test piece or an evaluation test piece. A plurality of test apparatuses are prepared, a reference test piece is placed in one apparatus, and evaluation test pieces are placed in the remaining test apparatuses. The pressure vessel 1 is provided with a connection pipe 6 to a gas cylinder for introducing liquid ammonia and O2, and a connection pipe 7 to a pressure gauge for measuring the internal pressure.

[0022] [Installation process] In the installation step, the reference test piece and the evaluation test piece to which surface strain has been applied by the bending test jig 3 are installed in different pressure vessels 1, respectively.

[0023] The reference test piece is a test piece for determining whether or not the test environment is appropriate in an evaluation test of stress corrosion cracking properties in liquid ammonia. The reference test piece is a steel plate, or a welded joint including a steel plate and a welded heat-affected zone. The shape of the reference test piece is a shape corresponding to the bending test jig 3. The bending test jig 3 is not particularly limited as long as it can impart surface strain to the reference test piece and the evaluation test piece, and examples thereof include a four-point bending test jig, a three-point bending test jig, and a U-bend test jig.

[0024] The material of the reference test piece is a steel material having a Vickers hardness of 230HV or more, or a welded joint having a Vickers hardness of 230HV or more in the heat affected zone (sometimes called HAZ). High-strength steel is required for a large tank for storing a large volume of liquid ammonia. The reference test piece is required to generate SCC because it is used to ensure that the test environment is appropriately performed to reproduce liquid ammonia SCC. If the Vickers hardness is 230HV or more, SCC in liquid ammonia is likely to occur, so the Vickers hardness of the steel material from which the reference test piece is taken, or the Vickers hardness of the HAZ of the welded joint is 230HV or more. In order to make the SCC generation condition more severe, it is preferable that the Vickers hardness of the reference test piece is 240HV or more, or 260HV or more. Examples of the material for the reference test piece include low-alloy steel with a total content of alloy elements of 5% or less, and medium-alloy steel with a total content of alloy elements of more than 5% and 10% or less. The Vickers hardness is a value obtained by applying a load of, for example, 9.8 N (1 kgf) in accordance with JIS Z 2244-1:2020.

[0025] The method for evaluating stress corrosion cracking properties in liquid ammonia according to this embodiment is basically carried out under conditions under which stress corrosion cracking occurs in the reference test specimen. The conditions under which stress corrosion cracking occurs in the reference test specimen are determined in advance by confirming the test time and pressurization state under which stress corrosion cracking occurs using the reference test specimen. Then, in the final confirmation step of the series of steps described below, if the occurrence of stress corrosion cracking is confirmed in the reference test specimen, the evaluation of stress corrosion cracking of the evaluation test specimen can be judged to be valid.

[0026] The evaluation test piece is a test piece to be evaluated for stress corrosion cracking properties in liquid ammonia. The evaluation test piece has the same shape as the reference test piece. Examples of the material of the evaluation test piece include low-alloy steel with a total content of alloying elements of 5% or less, and medium-alloy steel with a total content of alloying elements of more than 5% and 10% or less. In one evaluation, the material of the evaluation test piece 22 may be the same as the material of the reference test piece 21, or may be different from each other.

[0027] The pressure vessel according to this embodiment is small, and the counter electrode and the reference electrode connected to the potentio / galvanostat cannot be installed inside. In this embodiment, in order to promote SCC, the portion of the bending test jig 3 that contacts the reference test piece or the evaluation test piece is made of stainless steel. The stainless steel is not particularly limited, and may be general-purpose SUS304, SUS316, etc. In addition, the reference test piece and the evaluation test piece are electrically conductive with each of the bending test jig 3. For example, when a surface strain is applied by a four-point bending test jig, the reference test piece and the evaluation test piece are supported at a constant displacement via a stainless steel pin. The reference test piece and the evaluation test piece have a lower corrosion potential than stainless steel in an ammonia solution containing ammonium carbamate and O2, so they are easily corroded and SCC is promoted. A reference electrode or a counter electrode for anodically polarizing the test piece 2 at a constant potential or constant current is not installed inside the pressure vessel 1, and the configuration is relatively simple, so that the test environment inside the pressure vessel 1 can be stably maintained for a long time.

[0028] The surface strain applied to the reference test piece and the evaluation test piece by the bending test jig 3 is preferably 0.6 times or more of the yield strain. If the applied surface strain is 0.6 times or more of the yield strain, the SCC evaluation can be accelerated and the test time can be shortened. On the other hand, in order to set the surface strain applied to the test piece 2 almost uniformly on the test surface, it is necessary to avoid applying a large strain that causes a local portion of the test piece to bulge or shrink significantly. From this viewpoint, the surface strain applied to the reference test piece and the evaluation test piece by the bending test jig 3 is preferably 10 times or less of the yield strain, which corresponds to a U-bend bending test. In the case of a four-point bending test, the surface strain is preferably 1.0 times or less of the yield strain. Moreover, the surface strain applied to the evaluation test piece may be larger than the surface strain applied to the reference test piece. The yield strain is a value converted into strain using the yield stress previously measured in a tensile test, and for example, the upper yield point or 0.2% proof stress obtained at room temperature in accordance with JIS Z2241: 2022 may be used. When the yield strain differs in the base material, the welded heat-affected zone, and the weld metal, the value of a representative portion may be used, for example, the value of the base material.

[0029] The method for measuring the surface strain in the reference test piece and the evaluation test piece is not limited, but the surface strain in the reference test piece and the evaluation test piece is, for example, a value measured by the following method. That is, a strain gauge connected to a strain measuring device is attached to the surface of the test piece, and the value of the surface strain can be measured by the strain measuring device. In this case, after the surface strain is set to a target value, it is preferable to peel off the strain gauge, wipe off the adhesive used to attach the strain gauge with an organic solvent, and then polish the surface with fine-grained (e.g., #1000) emery paper until there is no trace of the attached strain gauge.

[0030] The pressure vessel 1 can accommodate either a reference test piece with the bending test jig 3 attached thereto or an evaluation test piece with the bending test jig 3 attached thereto, and can maintain a high pressure inside. The pressure vessel 1 may be a pressure-resistant vessel capable of creating a high pressure inside, a so-called autoclave. The pressure vessel 1 may preferably be made of stainless steel like the bending test jig 3, and may be in contact with the bending test jig 3 inside.

[0031] The reference test piece and the evaluation test piece are placed in different pressure vessels 1. By placing each test piece in a different pressure vessel 1, each pressure vessel 1 can be made smaller. The dimensions of the pressure vessel 1, for example, the inner diameter and the internal height, may be equal to or greater than the minimum dimensions that the reference test piece or the evaluation test piece attached to the bending test jig 3 can accommodate, and may be equal to or less than twice these minimum dimensions. By increasing the number of pressure vessels 1 in which the evaluation test pieces are placed, the test can be performed more efficiently.

[0032] [Filling process] In the filling step, an ammonia solution containing 3% by mass or more of ammonium carbamate is filled into the pressure vessel. If the concentration of ammonium carbamate in the ammonia solution is 3% by mass or more, SCC in liquid ammonia can be promoted. The concentration of ammonium carbamate in the ammonia solution may be 4% by mass or more or 5% by mass or more. If the concentration of ammonium carbamate is too high, the effect of promoting SCC in liquid ammonia is saturated. Therefore, there is no particular upper limit on the concentration of ammonium carbamate in the ammonia solution. The concentration of ammonium carbamate in the ammonia solution may be, for example, 10% by mass or less in order to save the amount of ammonium carbamate used.

[0033] The purity of ammonium carbamate is 97.0% or more. The purity of the liquid ammonia constituting the ammonia solution is 99.9% or more. This limits the amount of impurities to a small amount, and the effect of impurities on SCC can be suppressed. The purity of ammonium carbamate is preferably 99.5% or more. The purity of the liquid ammonia constituting the ammonia solution is preferably 99.999% or more.

[0034] The method for filling the pressure vessel with an ammonia solution containing 3% by mass or more of ammonium carbamate is not particularly limited, and can be, for example, the following method: For example, after placing ammonium carbamate powder in the pressure vessel, liquid ammonia is added to the pressure vessel to dissolve the ammonium carbamate in the liquid ammonia, thereby preparing an ammonia solution.

[0035] [Pressure process] In the pressurizing step, oxygen gas (O2 gas) is introduced into the pressure vessel 1 to apply pressure. In the pressurizing step, the reference test piece and the evaluation test piece are immersed in an ammonia solution containing 3 mass % or more of ammonium carbamate and O2.

[0036] The temperature of the ammonia solution is not particularly limited, but is preferably room temperature in consideration of the promotion of SCC and ease of handling of the test environment. The temperature of the ammonia solution may be, for example, 5° C. or higher and 35° C. or lower.

[0037] The purity of the oxygen gas is 99.9% or more. By making the purity of the oxygen gas 99.9% or more, the amount of impurities is limited to a small amount, and the effect of the impurities on SCC can be suppressed. The purity of the oxygen gas is preferably 99.999% or more.

[0038] The O2 partial pressure in pressure vessel 1 is 0.5kgf / cm 2 More than 5.0kgf / cm 2It is preferable that the O2 partial pressure in the pressure vessel 1 is 0.5 kgf / cm or less. The O2 gas in the gas phase dissolves in the ammonia solution at the interface with the ammonia solution and forms a film on the surface of the test piece. In order to form a film that reproduces actual use, the O2 partial pressure in the pressure vessel 1 is 0.5 kgf / cm or less. 2 More preferably, the O2 partial pressure in the pressure vessel 1 is 0.7 kgf / cm or more. 2 More preferably, it is 0.8 kgf / cm 2 Above 0.9kgf / cm 2 Above 1.0kgf / cm 2 That's all. The O2 partial pressure in the pressure vessel 1 is 1.1 kgf / cm 2 It may be 1.2kgf / cm or more. 2 On the other hand, if the coating becomes too thick, cracks are less likely to occur. Therefore, the O2 partial pressure in the pressure vessel 1 is 5.0 kgf / cm 2 The O2 partial pressure in the pressure vessel 1 is preferably 1.5 kgf / cm or less. 2 More preferably, it is 1.2 kgf / cm or less. 2 Below, 1.1kgf / cm 2 The O2 partial pressure in the pressure vessel 1 is 1.0 kgf / cm 2 It may be less than 0.9kgf / cm 2 The pressure inside the pressure vessel 1 can be measured by a pressure gauge and adjusted by introducing oxygen gas from a gas cylinder as necessary.

[0039] [Testing process] In the test process, the pressurized state is maintained for a test time during which stress corrosion cracking occurs in the reference test piece in a previously performed test. The time during which stress corrosion cracking occurs in the reference test piece varies depending on the shape of the test piece 2, the type of bending test jig 3, and the environment (temperature, pressure, ammonia solution components, etc.) inside the pressure vessel 1, but the test time can be, for example, 720 hours or more, for example, 1000 hours.

[0040] [Confirmation process] In the confirmation process, the occurrence of stress corrosion cracking is confirmed after the test time has elapsed. During the confirmation, the reference test piece and the evaluation test piece are removed from the pressure vessel 1. In the confirmation process, the occurrence of SCC is confirmed for the reference test piece and the evaluation test piece after they have been immersed in the ammonia solution for a specified test time.

[0041] Stress corrosion cracking is confirmed by observing the surface of the evaluation test piece. For example, the occurrence of stress corrosion cracking may be confirmed by visual observation, or the occurrence of stress corrosion cracking may be confirmed by observing the surface of the evaluation test piece at an arbitrary magnification, for example, 500 times, using an optical microscope. At this time, if the occurrence of stress corrosion cracking is confirmed in the reference test piece, it can be determined that an appropriate evaluation has been performed. Therefore, if the occurrence of stress corrosion cracking is confirmed in the reference test piece, the evaluation of stress corrosion cracking of the evaluation test piece is considered to be valid.

[0042] The method for evaluating stress corrosion cracking properties in liquid ammonia has been described above. However, the technical scope of the present invention is not limited to the above-mentioned embodiment, and various modifications can be made without departing from the spirit of the present invention.

[0043] For example, the number of evaluation test pieces, the bending test jig for applying bending strain to the evaluation test pieces, and the pressure vessel in which they are installed is not limited to one, and may be multiple. If there are multiple evaluation test pieces, bending test jig for applying bending strain to the evaluation test pieces, and the pressure vessel in which they are installed, it is possible to evaluate the stress corrosion cracking properties of different evaluation test pieces, improving the evaluation efficiency.

[0044] In the confirmation step, the evaluation test piece may be embedded in a resin, polished, and then the surface of the evaluation test piece may be observed. EXAMPLES

[0045] Next, examples of the present invention will be described, although the technical scope of the present invention is not limited to the following examples.

[0046] Reference test pieces were taken from the arc welded parts of high-strength steel HT80 (maximum hardness of the welded heat-affected zone is greater than 260HV), pressure vessel steel plate SPV315 (maximum hardness of the welded heat-affected zone is 210HV) specified in JIS G3115:2022, or HT60 (maximum hardness of the welded heat-affected zone is 230HV), which is stronger than that. Evaluation test pieces were also taken from the arc welded parts of pressure vessel steel plate SPV315 or high-strength steel HT60. For each of the reference test and evaluation test pieces, a stainless steel four-point bending test jig was used to set the surface strain between the two central points to the magnitude shown in Table 1. In the bending test jig, the reference test piece and the evaluation test piece were brought into contact with a stainless steel pin, and each test piece was made conductive with the pin. For comparison, a test was also conducted using a ceramic insulating pin instead of a stainless steel conductive pin. The evaluation test specimen and the reference test specimen fixed to the bending test fixture were placed in different pressure vessels. Liquid ammonia, ammonium carbamate, and O2 gas with different purities were prepared, and the SCC test was performed by changing the partial pressure of O2. The test temperature was controlled at 20°C (±2°C). After immersion, O2 gas was introduced into the pressure vessel. Each test specimen was naturally immersed in the ammonia solution. After the test time shown in Table 1 had elapsed, the test specimens were removed from each pressure vessel, and if SCC was found in the reference test specimen, the presence or absence of SCC was investigated for the evaluation test specimen placed in a separate vessel under the same test conditions as the reference test specimen. The presence or absence of SCC was confirmed specifically by visual observation and by observing the surfaces of the reference test specimen and the evaluation test specimen at 500 times magnification using an optical microscope. Table 1 shows a list of SCC test conditions and results.

[0047] [Table 1]

[0048] In all of the inventive examples Nos. 1 to 6, SCC occurred in the reference specimens, which indicates that the conditions for reproducing SCC were appropriate, and it was possible to evaluate the presence or absence of SCC susceptibility in the evaluation specimens.

[0049] In the comparative example, No. 7, the SCC susceptibility of the reference test piece was low, so SCC was not reproduced in the reference test piece, and it was inappropriate as an SCC test environment in liquid ammonia. The test conditions set for No. 7 were the same as those for No. 2, an example of the present invention, except that SPV315 (maximum hardness of the weld heat affected zone is 210 HV) was used as the reference test piece. However, if SCC was not reproduced in the reference test piece, it would be impossible to determine whether the SCC reproduction conditions in the test process were appropriate, so No. 7 was an inappropriate example.

[0050] In the comparative example, No. 8, the purity of the liquid ammonia was low and it contained impurities that reduced cracking susceptibility, so SCC could not be reproduced in the reference test specimen, making it unsuitable as an SCC test environment in liquid ammonia.

[0051] In the comparative example, No. 9, the purity of the ammonium carbamate was low and it contained impurities that reduced cracking susceptibility, so SCC could not be reproduced in the reference test specimen, making it unsuitable as an SCC test environment in liquid ammonia.

[0052] In the comparative example, No. 10, the concentration of ammonium carbamate in the ammonia solution was low, and the SCC promotion effect in liquid ammonia was not obtained, so SCC was not reproduced in the reference test piece, making it unsuitable as an SCC test environment in liquid ammonia.

[0053] In the comparative example, No. 11, the purity of O2 was low and impurities that reduced cracking susceptibility were contained, so SCC could not be reproduced in the reference test specimen, making it unsuitable as an SCC test environment in liquid ammonia.

[0054] Comparative example No. 12 is an example in which a ceramic pin was used. Since each test specimen was insulated from the four-point bending test fixture and the test specimen was not anodically polarized, SCC was not reproduced in the reference test specimen, making it unsuitable as an SCC test environment in liquid ammonia. [Explanation of symbols]

[0055] 1. Pressure vessel (autoclave) 2. Test specimens 3 Bending test fixture (stainless steel 4-point bending test fixture) 4. Ammonium carbamate 5. Ammonia solution 6. Connection piping for gas cylinders (liquid ammonia, O2) 7. Piping for connecting to pressure gauge

Claims

1. An installation step of installing the reference test piece and the evaluation test piece to which the surface strain is applied by the bending test jig in different pressure vessels, respectively; a filling step of filling each of the pressure vessels with an ammonia solution containing 3% by mass or more of ammonium carbamate; a pressurizing step of introducing oxygen gas into each of the pressure vessels to pressurize them; A test step of maintaining a pressurized state for a test time during which stress corrosion cracking occurs in the reference test piece in a previously performed test; A confirmation step of confirming whether or not stress corrosion cracking occurs after the test time has elapsed; Including, The material of the reference test piece is a steel material having a Vickers hardness of 230 HV or more, or a welded joint including a weld heat affected zone having a Vickers hardness of 230 HV or more, a portion of the bending test jig that comes into contact with the reference test piece and the evaluation test piece is made of stainless steel; the reference test piece and the evaluation test piece are electrically connected to the bending test fixtures, The purity of the liquid ammonia constituting the ammonia solution is 99.9% or more, The purity of the ammonium carbamate is 97.0% or more, The purity of the oxygen gas is 99.9% or more, When occurrence of stress corrosion cracking is confirmed in the reference test piece in the confirmation step, the evaluation of the stress corrosion cracking of the evaluation test piece is validated. Evaluation method for stress corrosion cracking properties in liquid ammonia.

2. In the pressurizing step and the testing step, the O 2 Partial pressure 0.5 kgf / cm 2 More than 5.0 kgf / cm 2 The following shall apply: The method for evaluating stress corrosion cracking properties in liquid ammonia according to claim 1.

3. The surface strain is 0.6 times or more the yield strain; The method for evaluating stress corrosion cracking properties in liquid ammonia according to claim 1 or 2.

4. The bending test jig is a four-point bending test jig, and supports the reference test piece and the evaluation test piece at a constant displacement via a stainless steel pin. The method for evaluating stress corrosion cracking properties in liquid ammonia according to claim 1 or 2.

Citation Information

Patent Citations

  • Low hydrogen type coated electrode

    JP1982137096A

  • The titanium or titanium alloy stress corrosion cracking test jig

    JP1986040653U

  • System for evaluation of sensitization degree of material by accelerated stress corrosion crack test

    JP1999173970A

  • Stress corrosion crack testing device and stress corrosion crack testing method

    JP2014020873A

  • Low yield ratio and high-strength steel having excellent stress corrosion cracking resistance and low temperature toughness

    US20180371588A1

Cited By

  • Ammonia compatibility evaluation using slow strain rate test

    WO2026182551A1