Fired product of pottery, porcelain, glass, or fine ceramics
By crosslinking amorphous thermoplastic resins with metal atoms or oxides in ceramic materials, the stain resistance and antifouling properties of tableware are significantly enhanced, facilitating easy cleaning and environmental conservation.
Patent Information
- Application Number
- JP2024077633
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-05-12
- Publication Date
- 2024-11-28
AI Technical Summary
Existing fired products such as tableware made from earthenware, porcelain, and fine ceramics lack sufficient stain resistance, and existing cost-saving manufacturing methods do not effectively enhance this property.
Incorporating an amorphous thermoplastic resin, such as alkoxysilane, into the base material of earthenware, porcelain, or fine ceramics, crosslinked via bridging metal atoms or metal oxides like aluminum, titanium, copper, palladium, silver, or platinum, to enhance stain resistance.
The resulting products exhibit high stain resistance and antifouling properties, allowing for easy cleaning with minimal water and energy, thus reducing environmental impact.
Smart Images

Figure 2024166116000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a fired product containing a basic material such as earthenware, porcelain, glass or fine ceramics, and relates to, for example, a tableware dish using the fired product and having improved stain resistance. [Background technology]
[0002] There are various types of baked products that contain the basic materials of pottery, porcelain, glass, or fine ceramics. For example, the materials of tableware are diverse, including pottery, porcelain, heat-resistant glass, fine ceramics, metals such as silver and anodized aluminum, heat-resistant plastic resin, paper, and wood. Tableware made of pottery, porcelain, glass, or fine ceramics is particularly widespread. In addition, ceramic tableware can be broadly defined to include pottery, porcelain, and glass, and fine ceramic tableware refers to tableware made from highly refined inorganic solid powder with high purity and uniform particle size.
[0003] Pottery, porcelain, and fine ceramics are generally produced by molding ceramic raw materials such as clay, bisque firing (800-950°C), applying glaze, and firing again (1200-1300°C). Here, it has long been known to apply glaze to ceramics before firing in order to make the surface less susceptible to dirt, increase strength, and enhance aesthetic appeal.
[0004] In the prior art, for example, Patent Document 1 (JP 2019-19007 A) discloses a method for manufacturing ceramics and the like that maintains the stain-resistant properties that make the surface less susceptible to dirt, while eliminating the steps of bisque firing (800-950°C) and applying glazing, and instead completing the product by firing it directly (1200-1300°C).
[0005] Furthermore, in the prior art, for example, the technology disclosed in Patent Document 2 (JP Patent Publication No. 1-133990) is an example of application to tiles, which is a technology that omits the steps of bisque firing and glazing while maintaining the stain-resistant properties that make the surface less susceptible to dirt.The technology disclosed involves forming a clay into a tile shape, spraying water onto the surface at a rate of 0.002 to 0.015 g / cm2 at a high pressure of 1 kg / cm2 or more, and applying the glaze by a curtain application method.
[0006] [Patent Document 1] JP 2019-19007 A [Patent Document 2] Japanese Patent Application Publication No. 1-133990 [Non-Patent Document 1] New Energy and Industrial Technology Development Organization (NEDO): News release "World's first elucidation of the fundamental structure of glass and silicone" DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0007] The above conventional technologies were primarily intended to reduce costs by eliminating processes while maintaining the stain-resistant properties of tableware, and did not improve the stain-resistant properties of tableware itself. In other words, while all tableware manufacturers and tableware suppliers understood that there was a strong need from general users for tableware that was less likely to get dirty and tableware that could be easily washed, development of such tableware progressed very slowly.
[0008] While conducting daily research into cleaning, the inventor, Masaaki Takano, has been actively researching the development of tableware with high stain resistance, since if the stain resistance of the tableware, which is the object of washing, could be improved, the amount of water consumed worldwide every day could be reduced, preserving the global environment, and furthermore, the human energy required to wash the tableware and the electrical energy required for dishwashers could be saved. The inventor, Masaaki Takano, found the clue in the course of intensive research and has been developing tableware with excellent stain resistance. While pondering various physicochemical principles, he came across Non-Patent Document 1, and using the physicochemical principles as a reference, he got the idea for his own development.
[0009] This non-patent document 1 clarifies the basic structure of glass and silicone, and although it is not the same as the content of the present invention, it clarifies the existence of precursors leading to the formation of glass. The inventor, Masaaki Takano, has found that by applying these precursors, a composition that improves the stain-resistant performance of tableware can be formed. Through the above process, this patent application was invented regarding a fired product containing basic materials such as pottery, porcelain, glass or fine ceramics. In particular, a promising application is tableware with excellent stain resistance. [Means for solving the problem]
[0010] In order to achieve the above-mentioned object of the present invention, the present invention provides a fired product made of pottery, porcelain, glass or fine ceramics, which comprises a base of pottery, porcelain, glass or fine ceramics containing an inorganic silicon compound as a basic material, and a non-crystalline thermoplastic resin, in which the non-crystalline thermoplastic resin is metal-bridged to the base via a bridging metal atom or a bridging metal oxide.
[0011] Here, the thermoplastic resin is preferably an alkoxysilane having an alkyl group. It is also preferred that the metal bridge formed by a bridge metal atom or a bridge metal oxide is a bridge to orthosilicic acid, which is a precursor formed from the base inorganic silicon compound and silanol generated by hydrolysis of alkoxysilane. The thermoplastic resin is preferably an acrylic hydrophilic monomer resin. More specifically, the thermoplastic resin is preferably acrylamide. The bridging metal atom or bridging metal oxide is preferably selected from the group consisting of aluminum, titanium, copper, palladium, silver and platinum.
[0012] With the above-mentioned structure, a thermoplastic resin having antifouling properties can be stably added to the basic material of pottery, porcelain, glass or fine ceramics by metal bridging via bridging metal atoms or bridging metal oxides, and the fired product can have excellent antifouling properties. Promising applications include tableware. Promising applications also include sanitary ware including ceramic fixtures such as toilets, wash basins and bathtubs. Effect of the Invention
[0013] The fired earthenware, porcelain, glass or fine ceramic product of the present invention can be applied to tableware, sanitary ware and the like having excellent stain-resistant properties. The tableware as the baked product of the present invention can exhibit high antifouling properties even when washed by general washing methods for tableware, i.e., washing with running water only, washing with detergent, and washing with a dishwasher and dryer, and in addition to such general washing methods, by washing with a faucet that applies the washing technology developed by the present inventor, Masaaki Takano, i.e., a faucet equipped with the technology of Patent No. 5961733, Patent No. 4369993, Patent No. 4860781, Patent No. 5762420, etc., a sufficiently high washing effect and antifouling effect can be exhibited even without using detergent. In other words, by combining the faucet developed by the present inventor, Masaaki Takano, with the tableware of the present invention, excellent water-saving effect, excellent washing effect, and excellent antifouling effect can be obtained synergistically, and the water environment and working environment of the earth can be improved. [Brief description of the drawings]
[0014] [Figure 1] This is a diagram summarizing the differences in atomic percentage:molar ratio of elements between a prototype dishware dish 100 (test piece 1) of Example 1 of the present invention used in an experiment on anti-stain properties, and a commercially available dishware dish (test piece 2) made by Company A, which is considered to have high anti-stain properties. [Diagram 2] FIG. 13 is a photograph of a test piece when hand washing checker lotion was used as a pigmented stain. [Diagram 3] This figure summarizes the results of a sensory test when hand washing checker lotion was used as a pigmented stain. [Figure 4] FIG. 13 is a photograph of a test piece in the case where lip balm was used as a high-viscosity stain. [Diagram 5] FIG. 11 is a diagram summarizing the results of a sensory test in which lip balm was used as a high-viscosity stain. [Figure 6] FIG. 13 is a photograph of a test piece in the case where a permanent marker was used as a fixed stain. [Figure 7] FIG. 13 is a diagram summarizing the results of a sensory test in which a permanent marker was used as the fixed stain. [Figure 8] FIG. 13 is a diagram summarizing the results of repeated cleaning and the numerical conversion of color difference of remaining stains. [Figure 9] FIG. 13 is a diagram showing the results of a durability test of the antifouling performance of Example 2. BEST MODE FOR CARRYING OUT THEINVENTION
[0015] Examples of the fired product of the present invention will be described below. However, it goes without saying that the scope of the present invention is not limited to the specific uses, shapes, numbers, etc. shown in the following examples.
[0016] The base of the fired product of the present invention is earthenware, porcelain, glass or fine ceramics containing an inorganic silicon compound as a basic material. The base of the fired product may basically contain clay derived from earth and inorganic silicon compounds such as feldspar and quartz. It is important that the base of the fired product contains inorganic silicon compounds as a basic material, and the ratio can vary widely.
[0017] For example, the weight ratio of clay to inorganic silicon compounds (feldspar or silica) may be 90%:10% to 40:60%. A typical ratio here may be 50% clay, 20% feldspar, and 30% silica. Furthermore, even when a glaze is used as the base of the fired product of the present invention, since the glaze contains feldspar or silica, which are inorganic silicon compounds, the base of the fired product of the present invention may be glazed or may be glazed and then pre-fired, and this may serve as the base for the fired product that contains inorganic silicon compounds as a basic material.
[0018] The baked product of the present invention contains a non-crystalline thermoplastic resin in the base of the baked product described above. Then, in order to compound the amorphous thermoplastic resin with the base containing the inorganic silicon compound, metal bridging is carried out using a bridging metal atom or a bridging metal oxide. The base containing an inorganic silicon compound provides orthosilicic acid, a precursor formed from silanols having glassy hydroxyl groups (-OH), as one of the crosslinking groups.
[0019] In addition, the non-crystalline thermoplastic resin that is the other of the crosslinks may be an alkoxysilane having an alkyl group. Alkoxysilanes are compounds that have one or more alkoxy groups on the silicon atom. The alkoxy group is -OR, where R is an alkyl group. Alkoxysilane, a non-crystalline thermoplastic resin, has thermoplastic properties and is hydrolyzed in the presence of a small amount of water to produce silanol, which then supplies orthosilicic acid, a precursor formed from silanol.
[0020] Orthosilicic acid is cross-linked by metal bridges using bridging metal atoms or bridging metal oxides, but the origins of the two are different, and the compounds supplied are different. In other words, the base containing the inorganic silicon compound of the fired material is an inorganic material, and the alkoxysilane, which is a non-crystalline thermoplastic resin, is an organic material, and the metal bridges using bridging metal atoms or bridging metal oxides form an inorganic-organic metal bridge. Inorganic-organic metal bridges can exhibit properties that cannot be achieved by either component alone due to the complexation of each component. It was designed to exhibit the following characteristics. The following explanation will be given using tableware as an example of the application of the baked product, but other applicable objects such as sanitary ware including ceramic fixtures such as toilets, wash basins, and bathtubs can also be considered in the same way.
[0021] <Hydrophilicity> The more hydrophilic the surface of the dish, that is, the smaller the static contact angle between the surface and water molecules, the stronger the interaction between the water molecules and the surface. In other words, it becomes easier for water to penetrate between the surface of the dish and the dirt on the surface of the dish (food residue, seasoning residue), making it easier for the dirt on the surface of the dish to float, and we can expect the so-called "sticking" to be weakened.
[0022] The alkoxysilane used in this embodiment has an alkyl group, and if the alkyl group is present as a functional group on the surface of the tableware dish, the number of hydroxyl groups (OH groups) on the surface of the baked tableware dish increases, making it more hydrophilic. In other words, although the alkoxy group is hydrophobic, in the process of metal bridging by the bridging metal atom or bridging metal oxide, the alkoxy group is replaced by a hydroxyl group (OH group), and the hydroxyl group (OH group) derived from the alkyl group gives the tableware dish of the present invention a hydrophilic property, so that the tableware dish of the present invention can have a hydrophilic property. As will be described later, the static contact angle of water in the prototype was about 8°. Generally, a static contact angle of water of about 37° is considered hydrophilic, but since the static contact angle of water was about 8°, a sufficiently high level of hydrophilicity was obtained.
[0023] As described above, due to the hydrophilicity of the dishware plate of the present invention, water is interposed between the surface of the dishware plate and the dirt on the surface, making the dirt easier to float and reducing the so-called "sticking" effect.Furthermore, due to the sliding properties of water in the dishware plate of the present invention, the floating dirt slides right off, making the dishware plate of the present invention highly stain-resistant. Example 1
[0024] As a prototype tableware of the present invention, a prototype in which the bridging metal atom or bridging metal oxide is aluminum was used, and it was confirmed through experiments that the antifouling performance was excellent. Figure 1 shows the differences in atomic percentage:molar ratio of elements between a prototype dishware plate 100 (test piece 1) of Example 1 of the present invention used in an experiment on stain resistance, and a commercially available dishware plate (test piece 2) made by Company A, which is considered to have high stain resistance. In Figure 1, C, O, and Si have various origins, so the results cannot be generalized, but the presence or absence of Al is a clear difference between the two. The prototype dish 100 of the present invention in Example 1 clearly contains a lot of Al, while the comparison dish made by Company A does not contain any (the value of Al is not zero, but this may be due to an error). Thus, the difference between the presence or absence of Al was confirmed to be that the prototype tableware dish 100 of the present invention in Example 1 has a chemical structure of metal bridges that are bridging metal atoms or bridging metal oxides (aluminum in this example).
[0025] Next, the difference in stain-resistant performance between the prototype dishware dish 100 (test piece 1) of Example 1 of the present invention and a commercially available dishware dish (test piece 2) manufactured by Company A, which is said to have high stain-resistant properties, was examined. First, the following items were selected as targets for contamination: There are two main types of dirt: oily and non-oily. Oily dirt is particularly difficult to remove, and among these, there are pigmented dirt, high viscosity dirt, and fixed dirt. The following dirt types were selected as representatives of these three types.
[0026] Hand-washing checker lotion was selected as the pigment stain, which contains the oily stain of lotion and fine fluorescent pigments that cause pigment stains. Lip balm was selected as an example of a highly viscous stain. It contains petrolatum and is a highly viscous oil stain. Permanent marker was selected as the type of stain that would stick to the surface. This is an oil stain that contains organic solvents and dries quickly, so it can be considered a stain that will stick to the surface as soon as it dries. In order to evaluate the condition in which dirt is formed by cooking or the like and then the dirt is cleaned, the following two-step procedure was repeated: the heat load procedure and the dirt adhesion / cleaning procedure.
[0027] [Heat Load Procedure] 1. The test piece is immersed in 100℃ warm water and subjected to a thermal load. 2. One cycle is 90℃ x 30 minutes. 3. After one cycle, evaluate the following antifouling performance of the test piece. 4. The point at which the stain-resistant performance has deteriorated and stains can no longer be removed is regarded as the stain-resistant durability period.
[0028] [Soil adhesion and cleaning procedure] 1. Apply dirt to the test piece. 2. The test piece with the dirt attached is cleaned. 3. Cleaning procedures should be performed in accordance with the test conditions. 4. First, the soiled test piece is immersed in the water of the tank for 30 seconds and the amount of remaining soil is evaluated. 5. If dirt remains, remove the item from the water in the tank and re-immerse it, repeating this process up to 15 times, and then evaluate the amount of dirt remaining. If dirt remains after step 6.5, rub the surface with a sponge up to five times and evaluate the remaining dirt. 7. When 50% or more of the stain remains on the surface twice, the stain-resistant performance is deemed to have been lost. In addition, since the tableware of the present invention is a highly hydrophilic dish, the evaluation is for hydrophilicity, not for stain-resistant performance due to wettability.
[0029] Evaluation of antifouling performance at each stage The evaluation consisted of visual sensory testing and numerical evaluation using a color difference meter. The evaluation criteria for the visual sensory test were as follows. S: The dirt has been completely removed A: There is a small amount of dirt remaining, but it is barely visible. B: There is some dirt remaining, but it is not noticeable. C: Dirt remains D: The dirt has spread E: The surface is rough and dirt is raised.
[0030] Figure 2 is a photograph of a test piece when hand-washing checker lotion was used as a pigment stain. The image is taken under ultraviolet light, capturing the fluorescent pigment. Figure 3 summarizes the results of the sensory test when hand-washing checker lotion was used as a pigmented stain. 2 and 3, a prototype dish 100 according to the first embodiment of the present invention is shown side-by-side for comparison with a comparative dish made by company A.
[0031] FIG. 4 is a photograph of a test piece in which lip balm was used as the high-viscosity stain. Figure 5 summarizes the results of the sensory test when lip balm was used as the high-viscosity stain. Both Figs. 4 and 5 show a prototype dish 100 of the first embodiment of the present invention and a comparative dish made by company A side by side for comparison.
[0032] FIG. 6 is a photograph of a test piece when permanent marker was used as the fixed stain. FIG. 7 shows the results of the sensory test when permanent marker was used as the fixed stain. 6 and 7, the prototype dish 100 of the first embodiment of the present invention is shown side-by-side for comparison with a comparative dish made by company A. From the above verification experiments, it can be seen that the prototype dish 100 of Example 1 of the present invention has sufficiently high stain-resistant performance when compared with the dish made by Company A for comparison.
[0033] Next, the high stain-resistant performance of the prototype tableware plate 100 of Example 1 of the present invention was further quantified. An experiment was carried out to remove stains using lip balm as a highly viscous stain and oil-based marker as a hardened stain. The cleaning operation was carried out according to the test conditions described above. The degree to which the dirt was removed was measured using a spectrophotometer (fiber type) and quantified. The measurements were conducted at the Izumi Center of the Osaka Industrial Technology Research Institute, a local independent administrative institution. The measuring equipment used was a fiber-type spectrophotometer at the same center.
[0034] The color difference between two samples (color stimuli) was measured, defined by ΔL*, Δa*, and Δb*, which are the differences in the coordinates L*, a*, and b* in the L*a*b* color space. The numerical value is expressed as ΔE*ab, which is calculated using the following formula 1.
number
[0035] Figure 8 shows the results of repeated cleaning and the numerical analysis of the color difference of the remaining stains. As shown in Fig. 8, in the case of the prototype tableware plate 100 of Example 1 of the present invention, the lip balm stain was completely removed even after the heat load procedure and the stain attachment / cleaning procedure were repeated 10 times. In the case of the oil-based marker stain, the stain was completely removed even after the heat load procedure and the stain attachment / cleaning procedure were repeated 9 times.
[0036] The tableware made by Company A, which was used for comparison, already exceeded a color difference of 1.0 in the first cycle. In other words, on tableware that is sold as a highly stain-resistant product on the market, lip balm stains and oil-based marker stains were still visible to the naked eye even after the first wash. From these demonstration experiments, it was verified that the prototype dish 100 of Example 1 of the present invention has higher stain-resistant performance than the dish made by Company A, which was used for comparison. Example 2
[0037] In Example 2, it was experimentally confirmed that the durability of the stain-resistant performance is excellent for the bridging metal atoms or bridging metal oxides in the prototype tableware of the present invention, other than the aluminum in Example 1. In Example 2, the durability of the stain-resistant performance was experimentally confirmed for aluminum, titanium, copper, palladium, silver, and platinum as the bridging metal atoms or bridging metal oxides. As in Example 1, oil-based marker was used as the stain for the durability of the stain-resistant performance. This is an oil stain containing an organic solvent, and can be considered as a stain that dries quickly and adheres immediately after drying. In order to evaluate the condition of stains caused by cooking, etc., and then cleaning the stains, the following two-step procedure was repeated: the heat load procedure and the stain attachment / cleaning procedure.
[0038] [Heat Load Procedure] 1. The test piece is immersed in 100℃ warm water and subjected to a thermal load. 2. One cycle is 90℃ x 30 minutes. 3. After one cycle, evaluate the following antifouling performance of the test piece. 4. The point at which the stain-resistant performance has deteriorated and stains can no longer be removed is regarded as the stain-resistant durability period.
[0039] [Soil adhesion and cleaning procedure] 1. Apply dirt to the test piece. 2. The test piece with the dirt attached is cleaned. 3. Cleaning procedures should be performed in accordance with the test conditions. 4. First, the soiled test piece is immersed in the water of the tank for 30 seconds and the amount of remaining soil is evaluated. 5. If dirt remains, remove the item from the water in the tank and re-immerse it, repeating this process up to 15 times, and then evaluate the amount of dirt remaining. If dirt remains after step 6.5, rub the surface with a sponge up to five times and evaluate the remaining dirt. 7. When 50% or more of the stain remains on the surface twice, the stain-resistant performance is deemed to have been lost. In addition, since the tableware of the present invention is a highly hydrophilic dish, the evaluation is for hydrophilicity, not for stain-resistant performance due to wettability.
[0040] [Test conditions] ● Water temperature: 30°C ● Dirt: Oil-based marker 1.2mm thick (dirt area: 24mm 2 degree) ● Sponge load: 100g ● Test piece 1: Commercially available product (test control) ● Test piece 2: DGPT-030 Cross-linked metal Al(OH)3 ● Test piece 3: DGPT-030 Cross-linked metal Ag ● Test piece 4: DGPT-030 Cross-linked metal Cu ● Test piece 5: DGPT-030 Cross-linked metal Pd ● Test piece 6: DGPT-030 Cross-linked metal Pt ● Test piece 7: DGPT-030 Cross-linked metal TiO2 ● Test piece 8: DGPT-030 Cross-linked metal Water-soluble TiO2
[0041] Evaluation of antifouling performance at each stage The evaluation consisted of visual sensory testing and numerical evaluation using a color difference meter. The evaluation criteria for the visual sensory test were as follows. The clear level in the visual sensory test using the comparison standard color was set to 19 levels (1 to 19). The stain remaining after 19 steps was broadly categorized into three levels: S, A, and B. S and A levels were evaluated as having stain-resistant properties, while B was evaluated as having lost stain-resistant properties. S: The dirt has completely come off. (9 levels from 1 to 9 based on visual sensory test pass level) A: There is a small amount of dirt remaining, but it is barely visible. (Five levels from 10 to 14 based on visual sensory test results) B: There is some dirt remaining, but it is not noticeable. (Five levels from 15 to 19 based on visual sensory test results)
[0042] FIG. 9 is a diagram showing the results of a durability test of the antifouling performance according to Example 2. The values entered in FIG. 9 are the clear levels in a visual sensory test using the above 19-level comparison standard colors. If level B appeared twice consecutively in the repeated experiment, the repeated experiment was terminated at that point since further accumulation of dirt would occur. As shown in Figure 9, the stain-resistant performance of test piece 1 (a commercially available control dish) in the far left column was not durable, and once stains were adhered to the plate, the stains could not be removed by simply immersing the plate in water. On the other hand, in the tableware of the present invention, although the durability of the stain-resistant performance differed depending on the type of metal used in the bridging metal atom or bridging metal oxide, it was confirmed that high stain-resistant performance was generally exhibited regardless of the bridging metal. Even the dish with the least durability (silver as the bridging metal) was able to exhibit stain-resistant properties even after 12 repetitions, and the dish with the most durability (copper as the bridging metal) was able to exhibit stain-resistant properties even after 18 repetitions. Thus, it was confirmed that high durability of the antifouling performance was obtained regardless of whether the bridging metal was aluminum, titanium, copper, palladium, silver, or platinum. It was confirmed that the dish of the present invention exhibited significantly higher durability than the control dish on the market.
[0043] Although the preferred embodiment of the present invention has been described above, it will be understood that various modifications can be made without departing from the technical scope of the present invention, which is therefore limited only by the scope of the appended claims.
Claims
1. A fired product made of pottery, porcelain, glass or fine ceramics, A base of pottery, porcelain, glass or fine ceramics containing inorganic silicon compounds as a basic material; Contains a non-crystalline thermoplastic resin, A fired product, characterized in that the amorphous thermoplastic resin is metal-bridged to the base via a bridging metal atom or a bridging metal oxide.
2. The fired product according to claim 1 , wherein the thermoplastic resin is an alkoxysilane having an alkyl group.
3. The fired product according to claim 2, characterized in that the metal bridge by the bridged metal atom or bridged metal oxide is a bridge to orthosilicic acid, which is a precursor formed from the inorganic silicon compound of the base and silanol generated by hydrolysis of the alkoxysilane.
4. The fired product according to claim 3 , wherein the thermoplastic resin is an acrylic hydrophilic monomer resin.
5. The baked product according to claim 4, wherein the thermoplastic resin is acrylamide.
6. 2. The fired product according to claim 1, wherein said bridging metal atom or bridging metal oxide is selected from the group consisting of aluminum, titanium, copper, palladium, silver and platinum.
7. 7. A tableware using the fired product according to claim 1, which is a tableware.
8. 7. Sanitary ware using the fired product according to claim 1, which is a sanitary ware including ceramic appliances such as a toilet bowl, a wash basin, and a bathtub.