Resin composition

The resin composition, containing a polyether ether ketone compound, epoxy resin, and active ester curing agent, addresses high dielectric properties and low peel strength issues in printed wiring boards, providing improved performance in semiconductor devices.

JP2024166247AActive Publication Date: 2024-11-28AJINOMOTO CO INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024153108
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-28
Estimated Expiration
2040-07-29

AI Technical Summary

Technical Problem

Existing resin compositions used in printed wiring boards for semiconductor devices have high dielectric properties, poor peel strength, and insufficient glass transition temperature, especially when surface roughness is low.

Method used

A resin composition comprising a polyether ether ketone compound with a maleimide group, an epoxy resin, and an active ester curing agent, along with optional components like a resin with a radically polymerizable unsaturated group and an inorganic filler, to form a cured product with low dielectric properties, excellent peel strength, and high glass transition temperature.

Benefits of technology

The composition achieves a cured product with improved dielectric properties, enhanced peel strength, and higher glass transition temperature, suitable for use in insulating layers of printed wiring boards and semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166247000001
    Figure 2024166247000001
  • Figure 2024166247000002
    Figure 2024166247000002
  • Figure 2024166247000003
    Figure 2024166247000003
Patent Text Reader

Abstract

To provide a resin composition or the like that can give a cured product having excellent peel strength and high glass transition temperature despite low dielectric properties and small surface roughness.SOLUTION: A resin composition contains (A) a polyether ether ketone compound having a maleimide group, (B) an epoxy resin, and (C) an active ester-based curing agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition. The present invention further relates to a resin sheet, a printed wiring board, and a semiconductor device obtained by using the resin composition. [Background technology]

[0002] As a manufacturing technique for printed wiring boards, a manufacturing method using a build-up method in which insulating layers and conductor layers are alternately stacked is known. In the manufacturing method using the build-up method, the insulating layer is generally formed by curing a resin composition. As such a resin composition, for example, the resin composition disclosed in Patent Document 1 is known. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-66792 A Summary of the Invention [Problem to be solved by the invention]

[0004] The cured product formed by curing the resin composition can be used as an insulating layer of a printed wiring board of a semiconductor device. Therefore, it is required to reduce the dielectric properties (dielectric constant and dielectric loss tangent) of the cured product. In addition, it is desirable that the insulating layer formed from this cured product has excellent peel strength between the insulating layer and the conductor layer even if the roughness of the insulating layer surface is small, and also has a high glass transition temperature in order to have excellent heat resistance.

[0005] The present invention has been devised in view of the above-mentioned problems, and has an object to provide a resin composition which can give a cured product having low dielectric properties, excellent peel strength even with a small surface roughness, and a high glass transition temperature; a resin sheet having a resin composition layer containing the resin composition; a printed wiring board including an insulating layer formed from a cured product of the resin composition; and a semiconductor device including the printed wiring board. [Means for solving the problem]

[0006] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by using (A) a polyether ether ketone compound having a maleimide group, (B) an epoxy resin, and (C) an active ester-based curing agent, and have thus completed the present invention.

[0007] That is, the present invention includes the following. [1] (A) a polyether ether ketone compound having a maleimide group, (B) an epoxy resin, and (C) a resin composition comprising an active ester-based curing agent. [2] The resin composition according to [1], wherein the number average molecular weight of component (A) is 10,000 or less. [3] The resin composition according to [1] or [2], wherein the component (A) has a maleimide group at a terminal thereof. [4] The resin composition according to any one of [1] to [3], wherein the content of component (A) is 5% by mass or more and 60% by mass or less, when the resin components in the resin composition are taken as 100% by mass. [5] The resin composition according to any one of [1] to [4], wherein the component (B) contains a naphthol-type epoxy resin. [6] The resin composition according to any one of [1] to [5], wherein the component (C) is at least one selected from the group consisting of a dicyclopentadiene-type active ester curing agent and a naphthalene-type active ester curing agent having a naphthalene structure. [7] The resin composition according to any one of [1] to [6], further comprising (D) a resin having a polymerizable unsaturated group. [8] The resin composition according to [7], wherein the component (D) is a resin containing a maleimide group and an aromatic ring. [9] The resin composition according to any one of [1] to [8], further comprising (E) an inorganic filler.

[10] The resin composition according to [9], wherein the content of the (E) component is 40% by mass or more and 65% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass.

[11] The resin composition according to any one of [1] to

[10] , which is for forming an insulating layer.

[12] The resin composition according to any one of [1] to

[11] , which is for forming an insulating layer for forming a conductor layer.

[13] A resin sheet comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of [1] to

[12] .

[14] A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of [1] to

[12] .

[15] A semiconductor device comprising the printed wiring board according to

[14] . Effect of the Invention

[0008] According to the present invention, there can be provided a resin composition which can give a cured product having low dielectric properties, excellent peel strength even with a small surface roughness, and a high glass transition temperature; a resin sheet including a resin composition layer which includes the resin composition; a printed wiring board which includes an insulating layer formed from a cured product of the resin composition; and a semiconductor device which includes the printed wiring board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified as desired without departing from the scope of the claims of the present invention and their equivalents.

[0010] [Resin composition] The resin composition of the present invention contains (A) a polyether ether ketone compound having a maleimide group, (B) an epoxy resin, and (C) an active ester curing agent. With such a resin composition, it is possible to obtain a cured product having low dielectric properties, excellent peel strength even with a small surface roughness, and a high glass transition temperature.

[0011] The resin composition may further contain optional components such as (D) a resin containing a radically polymerizable unsaturated group, (E) an inorganic filler, (F) a curing agent, (G) a curing accelerator, and (H) other additives, as necessary.

[0012] <(A) Polyether ether ketone compound having a maleimide group> The resin composition contains a polyether ether ketone compound having a maleimide group as component (A). The maleimide group is represented by the following formula (A-1). By including component (A) in the resin composition, a cured product having a high glass transition temperature can be obtained. [ka]

[0013] The component (A) may be a compound having a maleimide group and a polyether ether ketone (PEEK) structure. The component (A) preferably has one or more maleimide groups, more preferably has two or more maleimide groups, and preferably has 10 or less maleimide groups, more preferably has 5 or less maleimide groups, and even more preferably has 3 or less maleimide groups, per molecule of the component (A). From the viewpoint of obtaining a cured product with excellent dielectric properties, the maleimide group is preferably present at the terminal of the component (A), and more preferably has maleimide groups at both terminals.

[0014] The component (A) has a polyether ether ketone structure. The polyether ether ketone structure preferably has a structure represented by the following formula (A-2). [ka] In formula (A-2), Ar 1 , Ar 2 , Ar 3 , Ar 4 , and Ar 5 each independently represents a divalent aromatic hydrocarbon group, n represents an integer of 2 to 50, and * represents a bond.

[0015] The aromatic hydrocarbon group refers to a hydrocarbon group containing an aromatic ring. However, the aromatic hydrocarbon group does not necessarily have to be composed of only aromatic rings, and may contain a chain structure or an alicyclic hydrocarbon group as a part thereof, and the aromatic ring may be any one of a monocyclic ring, a polycyclic ring, and a heterocyclic ring.

[0016] Examples of the divalent aromatic hydrocarbon group include an arylene group, an aralkylene group, and a group having an arylene-alkylene-arylene structure.

[0017] The arylene group is preferably an arylene group having 6 to 30 carbon atoms, more preferably an arylene group having 6 to 20 carbon atoms, and further preferably an arylene group having 6 to 10 carbon atoms. Examples of such arylene groups include a phenylene group, a naphthylene group, an anthracenylene group, and a biphenylene group.

[0018] The aralkylene group is preferably an aralkylene group having 7 to 30 carbon atoms, more preferably an aralkylene group having 7 to 20 carbon atoms, and further preferably an aralkylene group having 7 to 15 carbon atoms. Examples of such an aralkylene group include a benzylene group and a group having a biphenylene-methylene structure.

[0019] The arylene in the group having an arylene-alkylene-arylene structure is the same as the arylene group described above. The alkylene is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and even more preferably an alkylene group having 1 to 3 carbon atoms. Examples of such alkylene include methylene, ethylene, and propylene. The alkylene may have a substituent. Examples of the substituent include an alkyl group having 1 to 3 carbon atoms; a halogen atom such as a fluorine atom, a chlorine atom, and a bromine atom; and a halogenated alkyl group. An alkyl group or a halogenated alkyl group having 1 to 3 carbon atoms is preferable, a methyl group or a trifluoromethyl group is more preferable, and a methyl group is even more preferable. Specific examples of the group having such an arylene-alkylene-arylene structure include structures represented by the following formulas (1) and (2). Among them, a group represented by formula (1) is preferable. [ka] In the formula, "*" represents a bond.

[0020] Among these, Ar 1 , Ar 2 , Ar 4 , and Ar 5 is preferably an arylene group or a group having an arylene-alkylene-arylene structure, more preferably an arylene group, and further preferably a phenylene group. 3 As the alkyl group, an arylene group or a group having an arylene-alkylene-arylene structure is preferable, a group having an arylene-alkylene-arylene structure is more preferable, and a group having a phenylene-dimethylmethylene-phenylene structure (a group represented by formula (1)) is even more preferable.

[0021] n represents an integer of 2 to 50, preferably an integer of 3 to 40, more preferably an integer of 4 to 30, and further preferably an integer of 5 to 20.

[0022] Specific examples of the structure represented by formula (A-2) include structures represented by the following formulae (A1) to (A2), but are not limited thereto (in the formulae, * represents a bond). [ka]

[0023] n1 and n2 are the same as n in formula (A-2).

[0024] The component (A) is preferably a compound represented by the following formula (A-3). [ka] In the formula, D 1 and D. 2 each independently represents a single bond or a divalent linking group. 11 , Ar 12 , Ar 14 , and Ar 15 each independently represents Ar 1 , Ar 2 , Ar 4 , and Ar 5 It is the same as Ar 13 each independently represents Ar 3 m is the same as n in formula (A-2).

[0025] D 1 and D. 2 each independently represents a single bond or a divalent linking group. Examples of the divalent linking group include a divalent hydrocarbon group, a divalent heterocyclic group, a carbonyl group, an ether bond, an ester bond, a carbonate bond, an amide bond, an imide bond, and groups in which a plurality of these are linked together. The divalent hydrocarbon group includes a divalent aliphatic hydrocarbon group and a divalent aromatic hydrocarbon group.

[0026] Examples of the divalent aliphatic hydrocarbon group include linear or branched alkylene groups having 1 to 18 carbon atoms, and linear or branched alkenylene groups having 2 to 18 carbon atoms. Examples of the linear or branched alkylene groups having 1 to 18 carbon atoms include methylene, methylmethylene, dimethylmethylene, ethylene, propylene, and trimethylene. Examples of the linear or branched alkenylene groups having 2 to 18 carbon atoms include vinylene, 1-methylvinylene, propenylene, 1-butenylene, and 2-butenylene.

[0027] Examples of the divalent alicyclic hydrocarbon group include divalent alicyclic hydrocarbon groups having 3 to 18 carbon atoms, such as cycloalkylene groups (including cycloalkylidene groups) such as a 1,2-cyclopentylene group, a 1,3-cyclopentylene group, a cyclopentylidene group, a 1,2-cyclohexylene group, a 1,3-cyclohexylene group, a 1,4-cyclohexylene group, and a cyclohexylidene group.

[0028] Examples of the divalent aromatic hydrocarbon group include arylene groups having 6 to 14 carbon atoms, such as a 1,2-phenylene group, a 1,4-phenylene group, a 1,3-phenylene group, a 4,4'-biphenylene group, a 3,3'-biphenylene group, a 2,6-naphthylene group, a 2,7-naphthylene group, a 1,8-naphthylene group, and an anthracenylene group.

[0029] The heterocycle constituting the divalent heterocyclic group includes aromatic heterocycles and non-aromatic heterocycles. Examples of the heterocycle include 3- to 10-membered rings and condensed rings thereof having carbon atoms and at least one heteroatom as atoms constituting the ring. Examples of the heteroatom include an oxygen atom, a sulfur atom, and a nitrogen atom. The heterocycle is preferably a 3- to 10-membered ring, more preferably a 4- to 6-membered ring. Examples of heterocyclic rings constituting the divalent heterocyclic group include three-membered rings such as an oxirane ring; four-membered rings such as an oxetane ring; five-membered rings such as a furan ring, a tetrahydrofuran ring, an oxazole ring, an isoxazole ring, a γ-butyrolactone ring, a thiophene ring, a thiazole ring, an isothiazole ring, a thiadiazole ring, a pyrrole ring, a pyrrolidine ring, a pyrazole ring, an imidazole ring, and a triazole ring; six-membered rings such as a 4-oxo-4H-pyran ring, a tetrahydropyran ring, a morpholine ring, a 4-oxo-4H-thiopyran ring, an isocyanuric ring, a pyridine ring, a pyridazine ring, a pyrimidine ring, a pyrazine ring, a piperidine ring, and a piperazine ring; 4,8 ]Undecane-2-one ring, 3-oxatricyclo[4.2.1.0 4,8 ]nonan-2-one ring and other bridged rings; and condensed rings such as a benzofuran ring, an isobenzofuran ring, a 4-oxo-4H-chromene ring, a chroman ring, an isochroman ring, a benzothiophene ring, an indole ring, an indoline ring, a quinoline ring, an acridine ring, a naphthyridine ring, a quinazoline ring, and a purine ring. A divalent heterocyclic group is a group obtained by removing two hydrogen atoms from the structural formula of the heterocycle described above.

[0030] Among them, D 1 and D. 2 From the viewpoint of achieving the effects of the present invention remarkably, preferably represents a divalent aromatic hydrocarbon group, more preferably represents an arylene group having 6 to 16 carbon atoms, further preferably represents a 1,2-phenylene group, a 1,4-phenylene group, a 1,3-phenylene group, a 4,4'-biphenylene group, a 3,3'-biphenylene group, a 2,6-naphthylene group, a 2,7-naphthylene group, a 1,8-naphthylene group, or an anthracenylene group, and particularly preferably represents a 1,2-phenylene group, a 1,4-phenylene group, or a 1,3-phenylene group.

[0031] Specific examples of the component (A) include the following, but the invention is not limited to these: In the following formula, na and nb each independently represent an integer of 2 to 50. [ka]

[0032] The component (A) may be a commercially available product or may be synthesized by a known method. The component (A) may be synthesized, for example, by utilizing the synthesis method described in Polymer 1989, p. 978. The component (A) may be used alone or in combination of two or more types.

[0033] From the viewpoint of obtaining a cured product having low dielectric properties and excellent adhesion to copper foil, the weight average molecular weight of component (A) is preferably 1,000 or more, more preferably 1,200 or more, and even more preferably 1,400 or more, and is preferably 10,000 or less, more preferably 7,500 or less, and even more preferably 5,000 or less. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0034] The number average molecular weight of component (A) is preferably 1,000 or more, more preferably 1,200 or more, and even more preferably 1,400 or more, from the viewpoint of obtaining a cured product having low dielectric properties and excellent adhesion to copper foil, and is preferably 10,000 or less, more preferably 7,500 or less, and even more preferably 5,000 or less. The number average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene equivalent value.

[0035] From the viewpoint of obtaining a cured product having low dielectric properties and excellent adhesion to copper foil, the content of component (A) is preferably 1 mass % or more, more preferably 3 mass % or more, and even more preferably 5 mass % or more, and is preferably 25 mass % or less, more preferably 20 mass % or less, and even more preferably 15 mass % or less, based on 100 mass % of the non-volatile components in the resin composition. In the present invention, the content of each component in the resin composition is a value when the non-volatile components in the resin composition are taken as 100 mass %, unless otherwise specified.

[0036] From the viewpoint of obtaining a cured product having low dielectric properties and excellent adhesion to copper foil, the content of the (A) component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 60% by mass or less, preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less, when the resin component in the resin composition is taken as 100% by mass. The resin component refers to the non-volatile components in the resin composition excluding the (E) inorganic filler.

[0037] <(B) Epoxy resin> The resin composition contains an epoxy resin as component (B). By including the epoxy resin (B) in the resin composition, it is possible to obtain a cured product having low dielectric properties and excellent peel strength.

[0038] Examples of the (B) component include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, cresol novolac type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, etc. Among them, naphthol type epoxy resin is preferable as the (B) component from the viewpoint of obtaining the effect of the present invention remarkably.

[0039] The resin composition preferably contains, as component (B), an epoxy resin having two or more epoxy groups in one molecule. From the viewpoint of significantly obtaining the desired effects of the present invention, the ratio of the epoxy resin having two or more epoxy groups in one molecule to 100% by mass of the non-volatile components of component (B) is preferably 20% by mass or more, more preferably 30% by mass or more, and particularly preferably 40% by mass or more.

[0040] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only a liquid epoxy resin, only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin as component (B), but from the viewpoint of significantly obtaining the desired effects of the present invention, it is preferable to contain only a solid epoxy resin.

[0041] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0042] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and naphthol type epoxy resin is more preferred.

[0043] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", and "HP-7200H" (dicyclopentadiene epoxy resin) manufactured by DIC Corporation. ene type epoxy resins); "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", and "HP6000" (naphthylene ether type epoxy resins) manufactured by DIC; "EPPN-502H" (trisphenol type epoxy resins) manufactured by Nippon Kayaku; "NC7000L" (naphthol novolac type epoxy resins) manufactured by Nippon Kayaku; "NC3000H", "NC3000", and "NC3000L" manufactured by Nippon Kayaku ","NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX4000HK" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; " Examples of epoxy resins include "YX8800" (anthracene type epoxy resin), "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals, "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical, "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical, "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical, and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical. These may be used alone or in combination of two or more.

[0044] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0045] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, glycidyl amine type epoxy resin, and epoxy resin having a butadiene structure are preferred, and naphthalene type epoxy resin is more preferred.

[0046] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation. ); "ZX1059" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation; "PB-3600" (epoxy resin having a butadiene structure) manufactured by Daicel Corporation; "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd. These may be used alone or in combination of two or more types.

[0047] When a liquid epoxy resin and a solid epoxy resin are used in combination as the (B) component, the ratio by mass (liquid epoxy resin:solid epoxy resin) is preferably 1:1 to 1:20, more preferably 1:1.5 to 1:15, and particularly preferably 1:2 to 1:10. When the ratio by mass of the liquid epoxy resin and the solid epoxy resin is within such a range, the desired effects of the present invention can be significantly obtained. Furthermore, when used in the form of a resin sheet, appropriate adhesion is usually obtained. Furthermore, when used in the form of a resin sheet, sufficient flexibility is usually obtained, and handling is improved. Furthermore, a cured product having sufficient breaking strength can usually be obtained.

[0048] The epoxy equivalent of the (B) component is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. When it is in this range, the crosslink density of the cured product of the resin composition layer becomes sufficient, and an insulating layer with small surface roughness can be obtained. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.

[0049] The weight average molecular weight (Mw) of the component (B) is preferably 100 to 5,000, more preferably 200 to 3,000, and even more preferably 250 to 1,500, from the viewpoint of significantly achieving the desired effects of the present invention.

[0050] The content of the (B) component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, when the non-volatile components in the resin composition are taken as 100% by mass, from the viewpoint of obtaining an insulating layer exhibiting good mechanical strength and insulating reliability. The upper limit of the epoxy resin content is preferably 30% by mass or less, more preferably 25% by mass or less, and particularly preferably 20% by mass or less, from the viewpoint of significantly obtaining the desired effects of the present invention.

[0051] From the viewpoint of obtaining an insulating layer exhibiting good mechanical strength and insulating reliability, the content of the (B) component, relative to 100 mass% of the resin component in the resin composition, is preferably 20 mass% or more, more preferably 25 mass% or more, even more preferably 30 mass% or more, and is preferably 50 mass% or less, more preferably 45 mass% or less, even more preferably 40 mass% or less.

[0052] <(C) Active ester curing agent> The resin composition contains (C) an active ester-based curing agent. By using the active ester-based curing agent, the dielectric properties can be improved, and the peel strength becomes excellent. The (C) component may be used alone or in combination of two or more kinds.

[0053] As the (C) active ester curing agent, generally, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferably used. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0054] Specifically, the (C) component may be a dicyclopentadiene-type active ester curing agent, a naphthalene-type active ester curing agent containing a naphthalene structure, an active ester curing agent containing an acetylated product of phenol novolac, or an active ester curing agent containing a benzoylated product of phenol novolac. Among them, the (C) component is more preferably one or more selected from a dicyclopentadiene-type active ester curing agent and a naphthalene-type active ester curing agent containing a naphthalene structure, and is even more preferably a naphthalene-type active ester curing agent containing a naphthalene structure. As the dicyclopentadiene-type active ester curing agent, an active ester curing agent containing a dicyclopentadiene diphenol structure is preferred. The "dicyclopentadiene diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.

[0055] (C) Commercially available active ester curing agents include "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "EXB-8000L-65TM" (manufactured by DIC Corporation) as active ester curing agents containing a dicyclopentadiene-type diphenol structure; and "EXB9416-70BK", "EXB-8100L-65T", "EXB-8150L-65T", "EXB-8150-65T", "HPC-8150-60T", "HPC-8150-62T" (manufactured by DIC Corporation) and "PC1300-02-65T" (manufactured by DIC Corporation) as naphthalene-type active ester curing agents containing a naphthalene structure. Examples of such active ester curing agents include "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester curing agent containing an acetylated product of phenol novolac; "YLH1026" (manufactured by Mitsubishi Chemical Corporation) as an active ester curing agent containing a benzoylated product of phenol novolac; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester curing agent which is an acetylated product of phenol novolac; "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester curing agents which are benzoylated products of phenol novolac; and "EXB-8500-65T" (manufactured by DIC Corporation).

[0056] From the viewpoint of being able to reduce the dielectric tangent and obtaining a cured product with excellent adhesion, the active ester group equivalent of the (C) active ester curing agent is preferably 50 g / eq. to 500 g / eq., more preferably 50 g / eq. to 400 g / eq., and even more preferably 100 g / eq. to 300 g / eq. The active ester group equivalent is the mass of the active ester curing agent containing one equivalent of active ester group.

[0057] The ratio of the amount of the epoxy resin (B) to the active ester curing agent (C) is preferably 0.01 or more, more preferably 0.3 or more, and even more preferably 0.5 or more, and is preferably 5 or less, more preferably 3 or less, and even more preferably 2 or less, in terms of the ratio of [total number of active groups of the active ester curing agent] / [total number of epoxy groups of the epoxy resin]. Here, the "epoxy group number of the epoxy resin" is the total value obtained by dividing the mass of the non-volatile components of the epoxy resin present in the resin composition by the epoxy equivalent. In addition, the "active ester curing number" is the total value obtained by dividing the mass of the non-volatile components of the active ester curing agent present in the resin composition by the active ester group equivalent. By setting the ratio of the amount of the epoxy resin to the active ester curing agent within this range, it is possible to obtain the effects of the present invention remarkably.

[0058] From the viewpoint of obtaining a cured product having low dielectric properties and excellent peel strength, the content of the (C) active ester curing agent is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less.

[0059] The content of the (C) active ester curing agent, from the viewpoint of being able to reduce the dielectric properties and obtaining a cured product with excellent peel strength, is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, and is preferably 50% by mass or less, more preferably 45% by mass or less, even more preferably 40% by mass or less, based on 100% by mass of the resin component in the resin composition.

[0060] <(D) Resin containing radically polymerizable unsaturated group> In addition to the above-mentioned components, the resin composition may contain (D) a resin containing a radically polymerizable unsaturated group as an optional component. By including (D) a resin containing a radically polymerizable unsaturated group in the resin composition, a cured product having low dielectric properties and excellent peel strength can be obtained. The (D) component does not include components (A) to (C).

[0061] The radical polymerizable unsaturated group contained in the (D) component represents a group containing an unsaturated bond exhibiting radical polymerizability. Examples of the radical polymerizable unsaturated group include a group containing an ethylenic double bond. The (D) component containing such a radical polymerizable unsaturated group can cause radical polymerization by heat or active energy rays, and can cure the resin composition.

[0062] Examples of the radically polymerizable unsaturated group include a maleimide group, a vinyl group, a vinylphenyl group, an acryloyl group, a methacryloyl group, a fumaroyl group, a maleoyl group, a benzocyclobutene group, and an allyl group. Among them, the maleimide group is preferable as the component (D) from the viewpoint of obtaining the effect of the present invention remarkably. The number of radically polymerizable unsaturated groups contained in the component (D) is usually 1 or more, preferably 2 or more. When the component (D) contains two or more radically polymerizable unsaturated groups, the two or more radically polymerizable unsaturated groups may be the same or different.

[0063] The (D) component is preferably a resin containing an aromatic ring in the molecule. Therefore, the (D) component is preferably a resin containing an aromatic ring and a radically polymerizable unsaturated group. The aromatic ring contained in the (D) component may be an aromatic carbon ring or an aromatic heterocycle. The aromatic ring may be a monocyclic aromatic ring, a condensed aromatic ring in which two or more monocyclic aromatic rings are condensed, or a condensed aromatic ring in which one or more monocyclic non-aromatic rings are condensed to one or more monocyclic aromatic rings. Examples of these aromatic rings include monocyclic aromatic rings such as a benzene ring and a pyridine ring; and condensed aromatic rings such as an indane ring, a fluorene ring, and a naphthalene ring. Among them, the aromatic ring is preferably an aromatic carbon ring. The number of carbon atoms in the aromatic carbon ring is preferably 6 or more and 10 or less.

[0064] The aromatic ring contained in component (D) may have a substituent bonded thereto. The number of substituents bonded to one aromatic ring may be 1 or 2 or more. When the number of substituents is 2 or more, the 2 or more substituents may be the same or different.

[0065] Examples of the substituent include an alkyl group, an alkyloxy group, an alkylthio group, an aryl group, an aryloxy group, an arylthio group, a cycloalkyl group, a halogen atom, a hydroxyl group, and a mercapto group.

[0066] The number of carbon atoms in the alkyl group is preferably 1 to 10. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an n-butyl group, and a t-butyl group.

[0067] The number of carbon atoms in the alkyloxy group is preferably 1 to 10. Examples of the alkyloxy group include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group.

[0068] The number of carbon atoms in the alkylthio group is preferably 1 to 10. Examples of the alkylthio group include a methylthio group, an ethylthio group, a propylthio group, and a butylthio group.

[0069] The number of carbon atoms in the aryl group is preferably 6 to 10. Examples of the aryl group include a phenyl group and a naphthyl group.

[0070] The number of carbon atoms in the aryloxy group is preferably 6 to 10. Examples of the aryloxy group include a phenyloxy group and a naphthyloxy group.

[0071] The number of carbon atoms in the arylthio group is preferably 6 to 10. Examples of the arylthio group include a phenylthio group and a naphthylthio group.

[0072] The number of carbon atoms in the cycloalkyl group is preferably 3 to 10. Examples of the cycloalkyl group include a cyclopentyl group, a cyclohexyl group, and a cycloheptyl group.

[0073] Examples of the halogen atom include a fluorine atom, a chlorine atom, and an iodine atom.

[0074] In particular, it is preferable that the aromatic ring contained in component (D) has no substituent bonded thereto or has an alkyl group bonded thereto.

[0075] The number of aromatic rings contained in component (D) is usually at least 1, and preferably at least 2. When component (D) contains two or more aromatic rings, those two or more aromatic rings may be the same or different.

[0076] The component (D) may be used alone or in combination of two or more types.

[0077] A preferred embodiment of component (D) is a resin containing a maleimide group. The resin containing a maleimide group preferably further contains an aromatic ring. Since the resin containing a maleimide group is a resin belonging to component (D), those corresponding to component (A) are excluded. The resin containing a maleimide group may be used alone or in combination of two or more types.

[0078] Examples of resins containing maleimide groups include (D-1) a maleimide compound containing an aliphatic group having 5 or more carbon atoms directly bonded to a nitrogen atom of a maleimide group, (D-2) a maleimide compound having an aromatic ring directly bonded to the nitrogen atom of a maleimide group, and (D-3) Maleimide compounds containing a trimethylindane skeleton, It is preferable that the compound is one or more selected from the following:

[0079] The term "directly" used herein means that, in the case of component (D-1), there is no other group between the nitrogen atom of the maleimide group and the aliphatic group having 5 or more carbon atoms, and in the case of component (D-2), there is no other group between the nitrogen atom of the maleimide and the aromatic ring.

[0080] The component (D-1) is a maleimide compound containing an aliphatic group having 5 or more carbon atoms directly bonded to a nitrogen atom of the maleimide. The component (D-1) can be obtained, for example, by subjecting a component containing an aliphatic amine compound (such as a diamine compound having a dimer acid skeleton), maleic anhydride, and, if necessary, tetracarboxylic dianhydride to an imidization reaction.

[0081] Examples of the aliphatic group having 5 or more carbon atoms include an alkyl group, an alkylene group, and an alkenylene group.

[0082] The number of carbon atoms of the alkyl group having 5 or more carbon atoms is preferably 6 or more, more preferably 8 or more, preferably 50 or less, more preferably 45 or less, and even more preferably 40 or less. The alkyl group may be linear, branched, or cyclic, and linear is preferred. Examples of such alkyl groups include pentyl, hexyl, heptyl, octyl, nonyl, and decyl groups. The alkyl group having 5 or more carbon atoms may be a substituent of an alkylene group having 5 or more carbon atoms.

[0083] The number of carbon atoms of the alkylene group having 5 or more carbon atoms is preferably 6 or more, more preferably 8 or more, preferably 50 or less, more preferably 45 or less, and even more preferably 40 or less. The alkylene group may be linear, branched, or cyclic, and linear is preferred. Here, the cyclic alkylene group is a concept that includes the case where it is composed of only a cyclic alkylene group and the case where it contains both a linear alkylene group and a cyclic alkylene group. Examples of such alkylene groups include pentylene, hexylene, heptylene, octylene, nonylene, decylene, undecylene, dodecylene, tridecylene, heptadecylene, hexatriacontylene, a group having an octylene-cyclohexylene structure, a group having an octylene-cyclohexylene-octylene structure, and a group having a propylene-cyclohexylene-octylene structure.

[0084] The number of carbon atoms in the alkenylene group having 5 or more carbon atoms is preferably 6 or more, more preferably 8 or more, preferably 50 or less, more preferably 45 or less, and even more preferably 40 or less. The alkenylene group may be linear, branched, or cyclic, and linear is preferred. Here, the cyclic alkenylene group is a concept that includes a case where the alkenylene group is composed only of a cyclic alkenylene group and a case where the alkenylene group contains both a linear alkenylene group and a cyclic alkenylene group. Examples of such alkenylene groups include a pentynylene group, a hexynylene group, a heptylenylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, a dodecynylene group, a tridecynylene group, a heptadecynylene group, a hexatriacontinylene group, a group having an octynylene-cyclohexynylene structure, a group having an octynylene-cyclohexynylene-octynylene structure, and a group having a propynylene-cyclohexynylene-octynylene structure.

[0085] The component (D-1) is preferably a compound represented by the following formula (D-1-1). [ka] In the general formula (D-1-1), M represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent, and L represents a single bond or a divalent linking group.

[0086] M represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent. The number of carbon atoms of the divalent aliphatic group having 5 or more carbon atoms is preferably 6 or more, more preferably 8 or more, preferably 50 or less, more preferably 45 or less, and still more preferably 40 or less. This aliphatic group may be linear, branched, or cyclic, and among them, a linear one is preferred. Here, the cyclic aliphatic group is a concept including both the case consisting only of a cyclic aliphatic group and the case including both a linear aliphatic group and a cyclic aliphatic group. Examples of the divalent aliphatic group include an alkylene group and an alkenylene group. The alkylene group and the alkenylene group are as described above.

[0087] Examples of the substituent of M include a halogen atom, -OH, -O-C 1-10 alkyl group, -N(C 1-10 alkyl group)2, C 1-10 alkyl group, C 2-30 alkenyl group, C 2-30 alkynyl group, C 6-10 aryl group, -NH2, -CN, -C(O)O-C 1-10 alkyl group, -COOH, -C(O)H, -NO2, etc. Here, the term "C x-y " (x and y are positive integers and satisfy x < y) represents that the number of carbon atoms of the organic group described immediately after this term is x to y. For example, the expression "C 1-10 alkyl group" indicates an alkyl group having 1 to 10 carbon atoms. These substituents may be bonded to each other to form a ring, and the ring structure includes a spiro ring and a condensed ring. The substituent is preferably an alkyl group having 5 or more carbon atoms.

[0088] L represents a single bond or a divalent linking group. Examples of the divalent linking group include an alkylene group, an alkenylene group, an alkynylene group, an arylene group, -C(=O)-, -C(=O)-O-, -NR 0-(R 0 is a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, an oxygen atom, a sulfur atom, or C(=O)NR 0 -, a divalent group derived from phthalimide, a divalent group derived from pyromellitic diimide, and a group consisting of a combination of two or more of these divalent groups. The alkylene group, alkenylene group, alkynylene group, arylene group, divalent group derived from phthalimide, divalent group derived from pyromellitic diimide, and a group consisting of a combination of two or more of these divalent groups may have an alkyl group having 5 or more carbon atoms as a substituent. The divalent group derived from phthalimide represents a divalent group derived from phthalimide, specifically a group represented by general formula (D-1-2). The divalent group derived from pyromellitic diimide represents a divalent group derived from pyromellitic diimide, specifically a group represented by general formula (D-1-3). In the formula, "*" represents a bond. [ka]

[0089] The alkylene group as the divalent linking group in L is preferably an alkylene group having 1 to 50 carbon atoms, more preferably an alkylene group having 1 to 45 carbon atoms, and particularly preferably an alkylene group having 1 to 40 carbon atoms. This alkylene group may be linear, branched, or cyclic. Examples of such alkylene groups include a methylethylene group, a cyclohexylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tridecylene group, a heptadecylene group, a hexatriacontylene group, a group having an octylene-cyclohexylene structure, a group having an octylene-cyclohexylene-octylene structure, and a group having a propylene-cyclohexylene-octylene structure.

[0090] The alkenylene group as the divalent linking group in L is preferably an alkenylene group having 2 to 50 carbon atoms, more preferably an alkenylene group having 2 to 45 carbon atoms, and particularly preferably an alkenylene group having 2 to 40 carbon atoms. This alkenylene group may be linear, branched, or cyclic. Examples of such alkenylene groups include a methylethylenylene group, a cyclohexenylene group, a pentenylene group, a hexenylene group, a heptenylene group, and an octenylene group.

[0091] The alkynylene group as the divalent linking group in L is preferably an alkynylene group having 2 to 50 carbon atoms, more preferably an alkynylene group having 2 to 45 carbon atoms, and particularly preferably an alkynylene group having 2 to 40 carbon atoms. This alkynylene group may be linear, branched, or cyclic. Examples of such alkynylene groups include a methylethynylene group, a cyclohexynylene group, a pentynylene group, a hexynylene group, a heptynylene group, and an octynylene group.

[0092] The arylene group as the divalent linking group in L is preferably an arylene group having 6 to 24 carbon atoms, more preferably an arylene group having 6 to 18 carbon atoms, still more preferably an arylene group having 6 to 14 carbon atoms, and even more preferably an arylene group having 6 to 10 carbon atoms. Examples of the arylene group include a phenylene group, a naphthylene group, and an anthracenylene group.

[0093] The alkylene group, alkenylene group, alkynylene group, and arylene group, which are the divalent linking groups in L, may have a substituent. The substituent is the same as the substituent of M in general formula (B2-1-1), and is preferably an alkyl group having 5 or more carbon atoms.

[0094] Examples of the group consisting of a combination of two or more divalent groups in L include a divalent group consisting of a combination of an alkylene group, a divalent group derived from phthalimide, and an oxygen atom; a divalent group consisting of a combination of a divalent group derived from phthalimide, an oxygen atom, an arylene group, and an alkylene group; a divalent group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide; and the like. The group consisting of a combination of two or more divalent groups may form a ring such as a condensed ring by the combination of the respective groups. In addition, the group consisting of a combination of two or more divalent groups may be a repeating unit having a repeating unit number of 1 to 10.

[0095] Among these, L in the general formula (D-1-1) is preferably an oxygen atom, an arylene group having 6 to 24 carbon atoms which may have a substituent, an alkylene group having 1 to 50 carbon atoms which may have a substituent, an alkyl group having 5 or more carbon atoms, a divalent group derived from phthalimide, a divalent group derived from pyromellitic diimide, or a divalent group consisting of a combination of two or more of these groups. Among these, as L, an alkylene group; a divalent group having the structure of an alkylene group-phthalimide-derived divalent group-oxygen atom-phthalimide-derived divalent group; a divalent group having the structure of an alkylene group-phthalimide-derived divalent group-oxygen atom-arylene group-alkylene group-arylene group-oxygen atom-phthalimide-derived divalent group; a divalent group having the structure of an alkylene-pyromellitic diimide-derived divalent group; a divalent group having the structure of an alkynylene group-phthalimide-derived divalent group-oxygen atom-phthalimide-derived divalent group; a divalent group having the structure of an alkynylene group-phthalimide-derived divalent group-oxygen atom-arylene group-alkynylene group-arylene group-oxygen atom-phthalimide-derived divalent group; or a divalent group having the structure of an alkynylene-pyromellitic diimide-derived divalent group is more preferred.

[0096] The maleimide resin represented by general formula (D-1-1) is preferably a maleimide resin represented by general formula (D-1-4). [ka] In general formula (D-1-4), M 1 each independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent, each Z independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent or a divalent group having an aromatic ring which may have a substituent, and t represents an integer of 1 to 10.

[0097] M 1 Each of M independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent. 1 is the same as M in general formula (D-1-1).

[0098] Each Z independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent, or a divalent group having an aromatic ring which may have a substituent. Examples of the divalent aliphatic group in Z include an alkylene group and an alkenylene group. The divalent aliphatic group may be linear, branched, or cyclic, and among these, a cyclic divalent aliphatic group having 5 or more carbon atoms which may have a substituent is preferred.

[0099] The number of carbon atoms in the alkylene group is preferably 6 or more, more preferably 8 or more, and preferably 50 or less, more preferably 45 or less, and even more preferably 40 or less. Examples of such alkylene groups include groups having an octylene-cyclohexylene structure, groups having an octylene-cyclohexylene-octylene structure, and groups having a propylene-cyclohexylene-octylene structure.

[0100] The number of carbon atoms in the alkenylene group having 5 or more carbon atoms is preferably 6 or more, more preferably 8 or more, preferably 50 or less, more preferably 45 or less, and even more preferably 40 or less. The alkenylene group may be linear, branched, or cyclic, and linear is preferred. Here, the cyclic alkenylene group is a concept that includes a case where the alkenylene group is composed only of a cyclic alkenylene group and a case where the alkenylene group contains both a linear alkenylene group and a cyclic alkenylene group. Examples of such alkenylene groups include a pentynylene group, a hexynylene group, a heptylenylene group, an octynylene group, a nonynylene group, a decynylene group, an undecynylene group, a dodecynylene group, a tridecynylene group, a heptadecynylene group, a hexatriacontinylene group, a group having an octynylene-cyclohexynylene structure, a group having an octynylene-cyclohexynylene-octynylene structure, and a group having a propynylene-cyclohexynylene-octynylene structure.

[0101] Examples of the aromatic ring in the divalent group having an aromatic ring represented by Z include a benzene ring, a naphthalene ring, an anthracene ring, a phthalimide ring, a pyromellitic diimide ring, and an aromatic heterocycle, and the like are mentioned, with a benzene ring, a phthalimide ring, and a pyromellitic diimide ring being preferred. That is, the divalent group having an aromatic ring is preferably a divalent group having a benzene ring which may have a substituent, a divalent group having a phthalimide ring which may have a substituent, or a divalent group having a pyromellitic diimide ring which may have a substituent. Examples of the divalent group having an aromatic ring include a group consisting of a combination of a divalent group derived from phthalimide and an oxygen atom; a group consisting of a combination of a divalent group derived from phthalimide, an oxygen atom, an arylene group, and an alkylene group; a group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide; a divalent group derived from pyromellitic diimide; a group consisting of a combination of a divalent group derived from phthalimide and an alkylene group; and the like. The arylene group is the same as the arylene group in the divalent linking group represented by L in general formula (D-1-1).

[0102] The alkylene group and the divalent group having an aromatic ring represented by Z may have a substituent. The substituent is the same as the substituent that may be possessed by M in the general formula (D-1-1).

[0103] Specific examples of the group represented by Z include the following groups: In the formula, "*" represents a bond. [ka] [ka]

[0104] The compound represented by general formula (D-1-1) is preferably any one of a compound represented by general formula (D-1-5) and a compound represented by general formula (D-1-6). [ka] In general formula (D-1-5), M 2 and M 3 each independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent, R 40 each independently represents an oxygen atom, an arylene group, an alkylene group, or a divalent group consisting of a combination of two or more of these groups. t1 represents an integer of 1 to 10. In general formula (D-1-6), M 4 , M 6 and M 7 each independently represents an aliphatic group having 5 or more carbon atoms which may have a substituent; M 5 each independently represents a divalent group having an aromatic ring which may have a substituent; R 41 and R 42 each independently represents an alkyl group having 5 or more carbon atoms. t2 represents an integer of 0 to 10, and u1 and u2 each independently represent an integer of 0 to 4.

[0105] M 2 and M 3Each of M independently represents a divalent aliphatic group having 5 or more carbon atoms which may have a substituent. 2 and M 3 is the same as the divalent aliphatic group having 5 or more carbon atoms represented by M in general formula (D-1-1), and a hexatriacontinylene group or a hexatriacontylene group is preferred.

[0106] R 40 R each independently represents an oxygen atom, an arylene group, an alkylene group, or a group consisting of a combination of two or more of these divalent groups. The arylene group and the alkylene group are the same as the arylene group and the alkylene group in the divalent linking group represented by L in the general formula (D-1-1). 40 is preferably an oxygen atom or a group formed from a combination of two or more divalent groups.

[0107] R 40 In the formula, examples of the group consisting of a combination of two or more divalent groups include a combination of an oxygen atom, an arylene group, and an alkylene group. Specific examples of the group consisting of a combination of two or more divalent groups include the following groups. In the formula, "*" represents a bond. [ka]

[0108] M 4 , M 6 and M 7 Each of M independently represents an aliphatic group having 5 or more carbon atoms which may have a substituent. 4 , M 6 and M 7 is the same as the aliphatic group having 5 or more carbon atoms which may have a substituent represented by M in general formula (D-1-1), and is preferably a hexylene group, a heptylene group, an octylene group, a nonylene group, or a decylene group, and more preferably an octylene group.

[0109] M 5 Each of M independently represents a divalent group having an aromatic ring which may have a substituent. 5is the same as the divalent group having an aromatic ring which may have a substituent represented by Z in general formula (D-1-4), and is preferably a group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide; a group consisting of a combination of a divalent group derived from phthalimide and an alkylene group, and more preferably a group consisting of a combination of an alkylene group and a divalent group derived from pyromellitic diimide. The arylene group and alkylene group are the same as the arylene group and alkylene group in the divalent linking group represented by L in general formula (D-1-1).

[0110] M 5 Specific examples of the group represented by the formula include the following groups: In the formula, "*" represents a bond. [ka]

[0111] R 41 and R 42 R each independently represents an alkyl group having 5 or more carbon atoms. 41 and R 42 is the same as the above-mentioned alkyl group having 5 or more carbon atoms, and is preferably a hexyl group, a heptyl group, an octyl group, a nonyl group, or a decyl group, and more preferably a hexyl group or an octyl group.

[0112] Each of u1 and u2 independently represents an integer of 1 to 15, and an integer of 1 to 10 is preferable.

[0113] Specific examples of the component (D-1) include the following compounds (Di) to (D-iii), but are not limited to these specific examples. In the formula, v represents an integer of 1 to 10. [ka] [ka]

[0114] Specific examples of the (D-1) component include "BMI1500" (compound of formula (Di)), "BMI1700" (compound of formula (D-ii)), and "BMI689" (compound of formula (D-iii)), all of which are manufactured by Designor Molecules.

[0115] The weight average molecular weight (Mw) of the component (D-1) is preferably 150 to 5,000, and more preferably 300 to 2,500.

[0116] From the viewpoint of significantly obtaining the desired effects of the present invention, the maleimide group equivalent of the (D-1) component is preferably 50 g / eq. to 2000 g / eq., more preferably 100 g / eq. to 1000 g / eq., and even more preferably 150 g / eq. to 500 g / eq. The maleimide group equivalent is the mass of the (D-1) component containing one equivalent of a maleimide group.

[0117] The component (D-2) is a maleimide compound having an aromatic ring directly bonded to the nitrogen atom of the maleimide. The component (D-2) can be obtained, for example, by imidization of a component containing an aromatic amine compound (such as an aromatic diamine compound) and maleic anhydride.

[0118] The aromatic ring may be a carbocyclic ring or a heterocyclic ring. Examples of the aromatic ring include monocyclic aromatic rings such as benzene ring, furan ring, thiophene ring, pyrrole ring, pyrazole ring, oxazole ring, isoxazole ring, thiazole ring, imidazole ring, pyridine ring, pyridazine ring, pyrimidine ring, and pyrazine ring; condensed rings in which two or more monocyclic aromatic rings are condensed, such as naphthalene ring, anthracene ring, benzofuran ring, isobenzofuran ring, indole ring, isoindole ring, benzothiophene ring, benzimidazole ring, indazole ring, benzoxazole ring, benzisoxazole ring, benzothiazole ring, quinoline ring, isoquinoline ring, quinoxaline ring, acridine ring, quinazoline ring, cinnoline ring, and phthalazine ring; condensed rings in which one or more monocyclic aromatic rings are condensed, such as indane ring, fluorene ring, and tetralin ring, and one or more monocyclic non-aromatic rings are condensed. Among these, the aromatic ring is preferably a monocyclic aromatic ring, and more preferably a benzene ring.

[0119] The component (D-2) is preferably a compound represented by the following formula (D-2-1). [ka]

[0120] In the formula, R c each independently represents a substituent; X c each independently represents a single bond, an alkylene group, an alkenylene group, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, -NHCO-, -COO-, or -OCO- (preferably a single bond or an alkylene group); Z ceach independently represents a non-aromatic ring which may have a substituent, or an aromatic ring which may have a substituent (preferably an aromatic ring which may have a substituent, particularly preferably an aromatic ring which may have a substituent); s represents an integer of 1 or more (preferably an integer of 1 to 100, more preferably an integer of 1 to 50, and even more preferably an integer of 1 to 20); t1 each independently represents 0 or an integer of 1 or more; and u each independently represents an integer of 0 to 2 (preferably 0).], and particularly preferably the maleimide compounds represented by the formulae (D-2-2) to (D-2-5):

[0121] [ka] In the formula, R c1 , R c2 and R c3 each independently represents an alkyl group; X c1 and X c2 each independently represents a single bond or an alkylene group; s represents an integer of 1 or more (preferably an integer of 1 to 100, more preferably an integer of 1 to 50, and even more preferably an integer of 1 to 20); t' represents an integer of 1 to 5; and v1, v2, and v3 each independently represent an integer of 0 to 2 (preferably 0). Note that the s unit, t unit, t' unit, v unit, v1 unit, v2 unit, and v3 unit may be the same or different for each unit.

[0122] In another embodiment, the component (D-2) preferably has a structure represented by the following formula (D-2-6): [ka] In the formula, R 31 and R 36 represents a maleimide group, and R 32 , R 33 , R 34 and R 35Each independently represents a hydrogen atom, an alkyl group, or an aryl group, and each D independently represents a divalent aromatic group. m1 and m2 each independently represent an integer from 1 to 10, and a represents an integer from 1 to 100.

[0123] R in formula (D-2-6) 32 , R 33 , R 34 and R 35 each independently represents a hydrogen atom, an alkyl group, or an aryl group, and a hydrogen atom is preferred.

[0124] As the alkyl group, an alkyl group having 1 to 10 carbon atoms is preferred, an alkyl group having 1 to 6 carbon atoms is more preferred, and an alkyl group having 1 to 3 carbon atoms is even more preferred. The alkyl group may be linear, branched, or cyclic. Examples of such an alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, an isopropyl group, and the like.

[0125] The aryl group preferably has 6 to 20 carbon atoms, more preferably 6 to 15 carbon atoms, and even more preferably 6 to 10 carbon atoms. The aryl group may be a monocyclic ring or a condensed ring. Examples of such an aryl group include a phenyl group, a naphthyl group, an anthracenyl group, and the like.

[0126] The alkyl group and the aryl group may have a substituent. The substituent is not particularly limited, and examples thereof include a halogen atom, -OH, -O-C 1-6 alkyl group, -N(C 1-10 alkyl group)2, C 1-10 alkyl group, C 6-10 aryl group, -NH2, -CN, -C(O)O-C 1-10 alkyl group, -COOH, -C(O)H, -NO2, and the like. Here, the term "C p-q "(p and q are positive integers and satisfy p < q.) represents that the number of carbon atoms of the organic group described immediately after this term is p to q. For example, "C 1-10The expression "alkyl group" refers to an alkyl group having 1 to 10 carbon atoms. These substituents may be bonded to each other to form a ring, and the ring structure also includes a spiro ring and a fused ring.

[0127] The above-mentioned substituents may further have a substituent (hereinafter, sometimes referred to as a "secondary substituent"). Unless otherwise specified, the secondary substituent may be the same as the above-mentioned substituent.

[0128] D in formula (D-2-6) represents a divalent aromatic group. Examples of the divalent aromatic group include a phenylene group, a naphthylene group, an anthracenylene group, an aralkyl group, a biphenylene group, and a biphenylaralkyl group. Among them, a biphenylene group and a biphenylaralkyl group are preferred, and a biphenylene group is more preferred. The divalent aromatic group may have a substituent. As the substituent, R in formula (D-2-6) may be used. 32 The substituents are the same as those that the alkyl group represented by the formula (I) may have.

[0129] m1 and m2 each independently represent an integer of 1 to 10, preferably 1 to 6, more preferably 1 to 3, even more preferably 1 or 2, and still more preferably 1.

[0130] "a" represents an integer of 1 to 100, preferably 1 to 50, more preferably 1 to 20, and further preferably 1 to 5.

[0131] The component (D-2) is preferably a resin represented by formula (D-2-7). [ka] In the formula, R 37 and R 38 represents a maleimide group. a1 represents an integer of 1 to 100.

[0132] a1 is the same as a in formula (D-2-6), and the preferred range is also the same.

[0133] Examples of commercially available products of component (D-2) include "MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd.; "BMI-50P" manufactured by KI Chemical Industry Co., Ltd.; "BMI-1000", "BMI-1000H", "BMI-1100", "BMI-1100H", "BMI-4000", and "BMI-5100" manufactured by Yamato Chemical Industry Co., Ltd.; "BMI-4,4'-BPE", "BMI-70", and "BMI-80" manufactured by KI Chemical Industry Co., Ltd.

[0134] The weight average molecular weight (Mw) of the component (D-2) is preferably 150 to 5,000, and more preferably 300 to 2,500.

[0135] The functional group equivalent of the maleimide group in the component (D-2) is preferably 50 g / eq. to 2000 g / eq., more preferably 100 g / eq. to 1000 g / eq., still more preferably 150 g / eq. to 500 g / eq., and particularly preferably 200 g / eq. to 300 g / eq.

[0136] The component (D-3) is a maleimide compound containing a trimethylindane skeleton, which is represented by the following formula (D-3-1).

[0137] [ka]

[0138] The benzene ring contained in the trimethylindane skeleton may have a substituent bonded thereto, for example, an alkyl group, an alkyloxy group, an alkylthio group, an aryl group, an aryloxy group, an arylthio group, a cycloalkyl group, a halogen atom, a hydroxyl group, and a mercapto group. The number of carbon atoms in the alkyl group is preferably 1 to 10. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an n-butyl group, and a t-butyl group. The number of carbon atoms in the alkyloxy group is preferably 1 to 10. Examples of the alkyloxy group include a methoxy group, an ethoxy group, a propoxy group, and a butoxy group. The number of carbon atoms in the alkylthio group is preferably 1 to 10. Examples of the alkylthio group include a methylthio group, an ethylthio group, a propylthio group, and a butylthio group. The number of carbon atoms in the aryl group is preferably 6 to 10. Examples of the aryl group include a phenyl group and a naphthyl group. The number of carbon atoms in the aryloxy group is preferably 6 to 10. Examples of the aryloxy group include a phenyloxy group and a naphthyloxy group. The number of carbon atoms in the arylthio group is preferably 6 to 10. Examples of the arylthio group include a phenylthio group and a naphthylthio group. The number of carbon atoms in the cycloalkyl group is preferably 3 to 10. Examples of the cycloalkyl group include a cyclopentyl group, a cyclohexyl group, and a cycloheptyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, and an iodine atom.

[0139] Among the above-mentioned substituents, the hydrogen atoms of the alkyl group, the alkyloxy group, the alkylthio group, the aryl group, the aryloxy group, the arylthio group and the cycloalkyl group may be substituted with a halogen atom.

[0140] The number of substituents bonded to one benzene ring contained in the trimethylindane skeleton may be 1 or 2 or more. The number of substituents bonded to a benzene ring contained in the trimethylindane skeleton is usually 0 to 3. When the number of substituents is 2 or more, the 2 or more substituents may be the same or different. In particular, it is preferable that no substituents are bonded to the benzene ring contained in the trimethylindane skeleton.

[0141] The number of trimethylindane structures contained in one molecule of the component (D-3) may be 1, or may be equal to or greater than 2. The upper limit can be, for example, 10 or less, 8 or less, 7 or less, or 6 or less.

[0142] The component (D-3) preferably further contains an aromatic ring skeleton in addition to the above-mentioned trimethylindane skeleton. The number of ring-constituting carbon atoms of the aromatic ring skeleton is preferably 6 to 10. Examples of aromatic ring skeletons include a benzene ring skeleton and a naphthalene ring skeleton. The number of the aromatic ring skeletons contained in one molecule of the component (D-3) is preferably 1 or more, more preferably 2 or more, and preferably 6 or less, more preferably 4 or less, and particularly preferably 3 or less. When the component (D-3) contains two or more aromatic ring skeletons in addition to the trimethylindane skeleton, the aromatic ring skeletons may be the same or different.

[0143] The aromatic ring contained in the aromatic ring skeleton may have a substituent bonded thereto. Examples of the substituent include the above-mentioned substituents that may be bonded to the benzene ring contained in the trimethylindane skeleton, and a nitro group. The number of substituents bonded to one aromatic ring may be 1 or 2 or more. The number of substituents bonded to an aromatic ring is usually 0 to 4. When the number of substituents is 2 or more, the 2 or more substituents may be the same or different.

[0144] The (D-3) component preferably further contains a divalent aliphatic hydrocarbon group in addition to the above-mentioned trimethylindane skeleton. In particular, when the (D-3) component contains an aromatic ring skeleton other than the benzene ring contained in the trimethylindane skeleton, the (D-3) component preferably contains a divalent aliphatic hydrocarbon group. In this case, the divalent aliphatic hydrocarbon group preferably connects between the benzene ring and the aromatic ring skeleton contained in the trimethylindane skeleton. In addition, the divalent aliphatic hydrocarbon group preferably connects between the aromatic ring skeletons.

[0145] The number of carbon atoms in the divalent aliphatic hydrocarbon group is preferably 1 or more, preferably 12 or less, more preferably 8 or less, and particularly preferably 5 or less. As the divalent aliphatic hydrocarbon group, an alkylene group as a saturated aliphatic hydrocarbon group is more preferable. As the divalent aliphatic hydrocarbon group, linear alkylene groups such as methylene group, ethylene group, trimethylene group, tetramethylene group, pentamethylene group, and hexamethylene group; branched alkylene groups such as ethylidene group (-CH(CH3)-), propylidene group (-CH(CH2CH3)-), isopropylidene group (-C(CH3)2-), ethylmethylmethylene group (-C(CH3)(CH2CH3)-), and diethylmethylene group (-C(CH2CH3)2-); and the like. (B2-3) When the maleimide compound containing a trimethylindane skeleton contains two or more divalent aliphatic hydrocarbon groups in addition to the trimethylindane skeleton, those divalent aliphatic hydrocarbon groups may be the same or different.

[0146] The component (D-3) preferably contains a structure represented by the following formula (D-3-2): The entire component (D-3) may have the structure represented by formula (D-3-2), or a portion of the component (D-3) may have the structure represented by formula (D-3-2). [ka]

[0147] (In the formula, Ar a1 represents a divalent aromatic hydrocarbon group which may have a substituent; R a1 each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; R a2each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group, or a mercapto group; R a3 each independently represents a divalent aliphatic hydrocarbon group; a1 represents a positive integer; n a2 each independently represents an integer of 0 to 4; a3 R each independently represents an integer of 0 to 3. a1 The hydrogen atoms of the alkyl group, alkyloxy group, alkylthio group, aryl group, aryloxy group, arylthio group, and cycloalkyl group of R may be substituted with halogen atoms. a2 The hydrogen atoms of the alkyl group, alkyloxy group, alkylthio group, aryl group, aryloxy group, arylthio group, and cycloalkyl group may be substituted with halogen atoms. a2 If is between 2 and 4, R a1 may be the same or different in the same ring. a3 If is 2-3, R a2 may be the same or different in the same ring.

[0148] In formula (D-3-2), Ar a1represents a divalent aromatic hydrocarbon group which may have a substituent. The number of carbon atoms in this divalent aromatic hydrocarbon group is preferably 6 or more, preferably 20 or less, more preferably 16 or less. Examples of the divalent aromatic hydrocarbon group include a phenylene group and a naphthylene group. Examples of the substituent that the divalent aromatic hydrocarbon group may have include an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group, and a mercapto group. The hydrogen atom of each substituent may be further substituted with a halogen atom. Specific examples of these substituents include the same examples as the substituents which may be bonded to the benzene ring contained in the trimethylindane skeleton. When the divalent aromatic hydrocarbon group has a substituent, the number of the substituents is preferably 1 to 4. When the divalent aromatic hydrocarbon group has two or more substituents, the two or more substituents may be the same or different. a1 is preferably an unsubstituted divalent aromatic hydrocarbon group.

[0149] In formula (D-3-2), R a1 each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group. The hydrogen atoms of the alkyl group, the alkyloxy group, the alkylthio group, the aryl group, the aryloxy group, the arylthio group, and the cycloalkyl group may be substituted with a halogen atom. Specific examples of these groups include the same examples as the substituents that can be bonded to the benzene ring contained in the trimethylindane skeleton. Among them, R a1is more preferably one or more groups selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 10 carbon atoms, and is particularly preferably an alkyl group having 1 to 4 carbon atoms.

[0150] In formula (D-3-2), R a2 each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group, or a mercapto group. The hydrogen atoms of the alkyl group, alkyloxy group, alkylthio group, aryl group, aryloxy group, arylthio group, and cycloalkyl group may be substituted with a halogen atom. Specific examples of these groups include the same examples as the substituents that can be bonded to the benzene ring contained in the trimethylindane skeleton. Among them, R a2 is more preferably one or more groups selected from the group consisting of an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 10 carbon atoms.

[0151] In formula (D-3-2), R a3 each independently represents a divalent aliphatic hydrocarbon group. The preferred range of the divalent aliphatic hydrocarbon group is as described above.

[0152] In formula (D-3-2), n a1 represents a positive integer. a1 is preferably 1 or more, and preferably 10 or less, more preferably 8 or less.

[0153] In formula (D-3-2), n a2 Each independently represents an integer of 0 to 4. a2 is preferably 2 or 3, more preferably 2. a2 may be different, but are preferably the same.a2 If is 2 or more, multiple R a1 may be the same or different within the same ring.

[0154] In formula (D-3-2), n a3 Each independently represents an integer of 0 to 3. a3 may be different, but are preferably the same. a3 is preferably 0.

[0155] It is particularly preferred that the component (D-3) contains the structure shown in formula (D-3-3) below: The entire component (D-3) may have the structure shown in formula (D-3-3), or a portion of the component (D-3) may have the structure shown in formula (D-3-3). [ka] (In the formula, R b1 each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; R b2 each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group, or a mercapto group; b1 represents a positive integer; n b2 each independently represents an integer of 0 to 4; b3 R each independently represents an integer of 0 to 3. b1 The hydrogen atoms of the alkyl group, alkyloxy group, alkylthio group, aryl group, aryloxy group, arylthio group, and cycloalkyl group of R may be substituted with halogen atoms. b2The hydrogen atoms of the alkyl group, alkyloxy group, alkylthio group, aryl group, aryloxy group, arylthio group, and cycloalkyl group may be substituted with halogen atoms. b2 If is between 2 and 4, R b1 may be the same or different in the same ring. b3 If is 2-3, R b2 may be the same or different in the same ring.

[0156] In formula (D-3-3), R b1 , R b2 , n b1 , n b2 and n b3 are R in formula (D-3-2), a1 , R a2 , n a1 , n a2 and n a3 is the same as:

[0157] The component (D-3) may further contain a structure represented by the following formula (D-3-4). [ka] In formula (D-3-4), R c1 , R c2 , n c2 and n c3 are R in formula (D-3-2), a1 , R a2 , n a2 and n a3 In addition, in formula (D-3-4), n c1 is the number of repeating units and is an integer of 1 to 20. Furthermore, in formula (D-3-4), * represents a bond. For example, the (D-3) component is a compound represented by formula (D-3-2), a2 is 3 or less, and R is present at two or more of the ortho and para positions relative to the maleimide group of the benzene ring to which the maleimide group is bonded. a1When no bond is bonded, the structure represented by formula (D-3-2) may be combined with the structure represented by formula (D-3-4). b2 is 3 or less, and R is present at two or more of the ortho and para positions relative to the maleimide group of the benzene ring to which the maleimide group is bonded. b1 When is not bonded, the structure represented by formula (D-3-3) may include the structure represented by formula (D-3-4) in combination with the structure represented by formula (D-3-3).

[0158] The component (D-3) may be used as a single type, or as a combination of two or more types in any desired ratio.

[0159] The maleimide group equivalent of the (D-3) component is preferably 50 g / eq. or more, more preferably 100 g / eq. or more, particularly preferably 200 g / eq. or more, and is preferably 2000 g / eq. or less, more preferably 1000 g / eq. or less, particularly preferably 800 g / eq. or less. The maleimide group equivalent represents the mass of the maleimide compound per equivalent of maleimide group. When the maleimide group equivalent of the (D-3) component is within the above range, the effects of the present invention can be significantly obtained.

[0160] The method for producing the component (D-3) is not particularly limited. The component (D-3) can be produced, for example, by the method described in the Japan Institute of Invention and Innovation's Technical Journal No. 2020-500211. According to the production method described in the Japan Institute of Invention and Innovation's Technical Journal No. 2020-500211, a maleimide compound having a distribution in the number of repeating units of the trimethylindane skeleton can be obtained. The maleimide compound obtained by this method contains a structure represented by the following formula (D-3-5). Therefore, the component (D-3) may contain a maleimide compound containing a structure represented by formula (D-3-5).

[0161] [ka]

[0162] (In the formula, R1 each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group, or a mercapto group; R 2 each independently represents an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group, or a mercapto group; n1 represents the average number of repeating units of 0.95 to 10.0; each independently represents an integer of 0 to 4; and each independently represents an integer of 0 to 3. R 1 The hydrogen atoms of the alkyl group, alkyloxy group, alkylthio group, aryl group, aryloxy group, arylthio group, and cycloalkyl group of R may be substituted with halogen atoms. 2 The hydrogen atoms of the alkyl group, alkyloxy group, alkylthio group, aryl group, aryloxy group, arylthio group, and cycloalkyl group may be substituted with halogen atoms. 1 may be the same or different in the same ring. When n3 is 2 to 3, R 2 may be the same or different in the same ring.

[0163] In formula (D-3-5), R 1 , R 2 , n2 and n3 are R in formula (D-3-2), a1 , R a2 , n a2 and n a3 is the same as:

[0164] In formula (D-3-5), n1 represents the average number of repeating units, and its range is 0.95 to 10.0. According to the manufacturing method described in the Japan Institute of Invention and Innovation Disclosure Technical Bulletin No. 2020-500211, a group of maleimide compounds containing a structure represented by formula (D-3-5) can be obtained. As can be seen from the fact that the average number of repeating units n1 in formula (D-3-5) can be smaller than 1.00, the maleimide compound containing the structure represented by formula (D-3-5) thus obtained can contain a maleimide compound having a trimethylindane skeleton repeating unit number of 0. Therefore, the maleimide compound containing the structure represented by formula (D-3-5) can be purified to remove the maleimide compound having a trimethylindane skeleton repeating unit number of 0 to obtain the (D-3) component, and the resin composition may contain only the obtained (D-3) component. However, even if a maleimide compound having a trimethylindane skeleton repeating unit number of 0 is contained in the resin composition, the effect of the present invention can be obtained. In addition, when purification is omitted, it is possible to reduce costs. Therefore, it is preferable that the resin composition contains a maleimide compound having a structure represented by formula (D-3-5) without excluding a maleimide compound having a trimethylindane skeleton with a repeating unit number of 0.

[0165] In formula (D-3-5), the average number of repeating units n1 is preferably 0.95 or more, more preferably 0.98 or more, even more preferably 1.0 or more, particularly preferably 1.1 or more, and is preferably 10.0 or less, more preferably 8.0 or less, even more preferably 7.0 or less, particularly preferably 6.0 or less. When the average number of repeating units n1 is within the above range, the effects of the present invention can be significantly obtained. In particular, the glass transition temperature of the resin composition can be effectively increased.

[0166] Examples of the structure represented by formula (D-3-5) include the following.

[0167] [ka]

[0168] The maleimide compound containing the structure represented by formula (D-3-5) may further contain the structure represented by formula (D-3-4) above. For example, the maleimide compound containing the structure represented by formula (D-3-5) is a compound in which n2 is 3 or less and R is present at two or more of the ortho and para positions relative to the maleimide group of the benzene ring to which the maleimide group is bonded. 1 When is not bonded, the structure represented by formula (D-3-5) may include a structure represented by formula (D-3-4) in combination.

[0169] The maleimide compound containing the structure represented by formula (D-3-5) preferably has a molecular weight distribution Mw / Mn calculated by gel permeation chromatography (GPC) measurement in a specific range. The molecular weight distribution is a value obtained by dividing the weight average molecular weight Mw by the number average molecular weight Mn, and is expressed as "Mw / Mn". Specifically, the molecular weight distribution Mw / Mn of the maleimide compound containing the structure represented by formula (D-3-5) is preferably 1.0 to 4.0, more preferably 1.1 to 3.8, even more preferably 1.2 to 3.6, and particularly preferably 1.3 to 3.4. When the molecular weight distribution Mw / Mn of the maleimide compound containing the structure represented by formula (D-3-5) is in the above range, the effects of the present invention can be significantly obtained.

[0170] Of the maleimide compounds containing the structure represented by formula (D-3-5), the amount of the maleimide compound having an average repeating unit number n1 of 0 is preferably within a specific range. When the GPC measurement of the maleimide compound containing the structure represented by formula (D-3-5) is performed, the amount of the maleimide compound having an average repeating unit number n1 of 0 can be expressed in area % based on the results of the GPC measurement. In detail, the amount of the maleimide compound having an average repeating unit number n1 of 0 can be expressed by the ratio (area %) of the peak area of ​​the maleimide compound having the structure represented by formula (D-3-5) to the total area of ​​the peaks of the maleimide compound containing the structure represented by formula (D-3-5) in the chromatogram obtained by the GPC measurement. Specifically, the amount of the maleimide compound having an average repeating unit number n1 of 0 is preferably 32 area % or less, more preferably 30 area % or less, and even more preferably 28 area % or less, based on the total amount of the maleimide compound containing the structure represented by formula (D-3-5) (100 area %). When the amount of the maleimide compound having an average repeating unit number n1 of 0 is within the above range, the effects of the present invention can be significantly obtained.

[0171] The maleimide group equivalent of the maleimide compound containing the structure represented by formula (D-3-5) is preferably in the same range as the maleimide group equivalent of the above-mentioned component (D-3). When the maleimide group equivalent of the maleimide compound containing the structure represented by formula (D-3-5) is in the above range, the effects of the present invention can be significantly obtained.

[0172] From the viewpoint of obtaining a cured product having low dielectric properties and excellent peel strength, the content of the (D) component is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, and even more preferably 1 mass % or more, and is preferably 10 mass % or less, more preferably 8 mass % or less, and even more preferably 5 mass % or less, based on 100 mass % of the non-volatile components in the resin composition.

[0173] From the viewpoint of obtaining a cured product with low dielectric properties and excellent peel strength, the content of the (D) component, relative to 100 mass% of the resin component in the resin composition, is preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, and is preferably 20 mass% or less, more preferably 15 mass% or less, even more preferably 10 mass% or less.

[0174] <(E) Inorganic filler> In addition to the above-mentioned components, the resin composition may contain an inorganic filler (E) as an optional component. By including the inorganic filler (E) in the resin composition, it is possible to obtain a cured product having excellent dielectric properties.

[0175] As the material of the inorganic filler, an inorganic compound is used. Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Moreover, as the silica, spherical silica is preferable. (E) The inorganic filler may be used alone or in combination of two or more types.

[0176] (E) Commercially available inorganic fillers include, for example, "UFP-30" manufactured by Denka Chemical Industry Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumitomo Metal Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd.; "UFP-30" manufactured by Denka Company, Ltd.; "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation; and "SC2500SQ", "SO-C4", "SO-C2", "SO-C1", and "SC2050-SXF" manufactured by Admatechs Co., Ltd.

[0177] From the viewpoint of significantly obtaining the desired effects of the present invention, the average particle size of the (E) inorganic filler is preferably 0.01 μm or more, more preferably 0.05 μm or more, particularly preferably 0.1 μm or more, and is preferably 5 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less.

[0178] (E) The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample is measured using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, and the volume-based particle size distribution of the inorganic filler is measured using a flow cell method, and the average particle size is calculated as the median diameter from the particle size distribution obtained. Examples of laser diffraction particle size distribution measuring devices include the "LA-960" manufactured by Horiba, Ltd. and the "SALD-2200" manufactured by Shimadzu Corporation.

[0179] The specific surface area of ​​the (E) inorganic filler is preferably 1 m or less from the viewpoint of remarkably obtaining the desired effects of the present invention. 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 3m 2 / g or more. There is no particular upper limit, but it is preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2 The specific surface area is measured by using a BET fully automatic specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) to adsorb nitrogen gas onto the surface of the sample, and then calculating the specific surface area using the BET multipoint method.

[0180] (E) The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include fluorine-containing silane coupling agents such as 3,3,3-trifluoropropyltrimethoxysilane; aminosilane coupling agents such as 3-aminopropyltriethoxysilane, N-phenyl-8-aminooctyl-trimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane; epoxysilane coupling agents such as 3-glycidoxypropyltrimethoxysilane; mercaptosilane coupling agents such as 3-mercaptopropyltrimethoxysilane; silane coupling agents; alkoxysilanes such as phenyltrimethoxysilane; organosilazane compounds such as hexamethyldisilazane, and titanate coupling agents. The surface treatment agent may be used alone or in any combination of two or more.

[0181] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0182] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100 parts by mass of the inorganic filler is preferably surface-treated with 0.2 parts by mass to 5 parts by mass of the surface treatment agent, more preferably 0.2 parts by mass to 3 parts by mass, and even more preferably 0.3 parts by mass to 2 parts by mass.

[0183] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the form of a sheet, it is more preferable that the content is 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0184] (E) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0185] From the viewpoint of significantly obtaining the effects of the present invention, the content of the (E) inorganic filler is preferably 40% by mass or more, more preferably 45% by mass or more, even more preferably 50% by mass or more, and is preferably 75% by mass or less, preferably 70% by mass or less, preferably 65% ​​by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass.

[0186] <(F) Hardener> The resin composition may further contain a (F) curing agent as an optional component in addition to the above-mentioned components. However, the (C) active ester-based curing agent is not included in the (F) curing agent. Examples of the (F) curing agent include a phenol-based curing agent, a naphthol-based curing agent, a benzoxazine-based curing agent, a cyanate ester-based curing agent, and a carbodiimide-based curing agent. Among them, from the viewpoint of improving insulation reliability, the (F) curing agent is preferably one or more of a phenol-based curing agent, a naphthol-based curing agent, a cyanate ester-based curing agent, and a carbodiimide-based curing agent, more preferably one of a phenol-based curing agent and a naphthol-based curing agent, and further preferably includes a phenol-based curing agent. The (F) curing agent may be used alone or in combination of two or more.

[0187] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferable. Also, from the viewpoint of adhesion to the conductor layer, a nitrogen-containing phenol-based curing agent is preferable, and a triazine skeleton-containing phenol-based curing agent is more preferable.

[0188] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", "SN375", and "SN395" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA3018-50P", and "EXB-9500" manufactured by DIC Corporation.

[0189] Specific examples of benzoxazine-based curing agents include "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0190] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0191] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.

[0192] When the curing agent is contained as the (F) component, the ratio of the amount of the epoxy resin to the (B) active ester curing agent and the (F) curing agent is preferably in the range of 1:0.01 to 1:5, more preferably 1:0.3 to 1:3, and even more preferably 1:0.5 to 1:2, in terms of the ratio of [total number of epoxy groups in the epoxy resin]:[total number of active groups in the (B) active ester curing agent and the (F) curing agent]. Here, the "number of epoxy groups in the epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile components of the epoxy resin present in the resin composition by the epoxy equivalent. In addition, the "number of active groups in the (B) active ester curing agent and the (F) curing agent" refers to the total value obtained by dividing the mass of the non-volatile components of the active ester curing agent and the curing agent present in the resin composition by the active group equivalent. By setting the ratio of the amount of the epoxy resin to the (B) component and the (F) component within such a range, the effects of the present invention can be obtained remarkably.

[0193] When the curing agent is contained as the (F) component, the ratio of the amount of the epoxy resin to all the (F) curing agents is preferably in the range of 1:0.01 to 1:1, more preferably 1:0.03 to 1:0.5, and even more preferably 1:0.05 to 1:0.3, in terms of the ratio of [total number of epoxy groups in the epoxy resin]:[total number of active groups in the (F) curing agent]. Here, the "number of active groups in the (F) curing agent" refers to the total value of all values ​​obtained by dividing the mass of the non-volatile components of the (F) curing agent present in the resin composition by the active group equivalent. By setting the ratio of the amount of the epoxy resin to the curing agent as the (F) component within this range, the effects of the present invention can be obtained significantly.

[0194] From the viewpoint of obtaining the desired effect of the present invention remarkably, the content of the (F) curing agent is preferably 1% by mass or more, more preferably 1.5% by mass or more, and more preferably 2% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less.

[0195] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (F) curing agent is preferably 1 mass % or more, more preferably 2 mass % or more, and even more preferably 3 mass % or more, and is preferably 10 mass % or less, more preferably 8 mass % or less, and even more preferably 5 mass % or less, based on 100 mass % of the resin component in the resin composition.

[0196] <(G) Curing accelerator> In addition to the above-mentioned components, the resin composition may further contain, as an optional component, a curing accelerator as component (G).

[0197] Examples of the (G) component include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, etc. The (G) component may be used alone or in combination of two or more types.

[0198] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.

[0199] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.

[0200] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.

[0201] As the imidazole-based curing accelerator, a commercially available product may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0202] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of such biguanide include o-[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.

[0203] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0204] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (G) component, relative to 100 mass% of the non-volatile components in the resin composition, is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and is preferably 3 mass% or less, more preferably 1.5 mass% or less, even more preferably 1 mass% or less.

[0205] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (G) component, relative to 100 mass% of the resin component in the resin composition, is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, even more preferably 0.5 mass% or more, and is preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 1 mass% or less.

[0206] <(H) Other Additives> The resin composition may further contain other additives as optional components in addition to the above-mentioned components. Examples of such additives include thermoplastic resins, elastomers, organic fillers, thickeners, defoamers, leveling agents, adhesion promoters, flame retardants, etc. These may be used alone or in combination of two or more at any ratio.

[0207] The resin composition can be produced, for example, by mixing the above-mentioned components in any order. In addition, in the process of mixing each component, heating and / or cooling may be performed by appropriately adjusting the temperature. In addition, during or after mixing of each component, stirring may be performed using a stirring device such as a mixer to uniformly disperse each component. Furthermore, if necessary, the resin composition may be subjected to a degassing treatment.

[0208] <Physical properties and applications of resin compositions> Since the resin composition contains a combination of the (A) component, the (B) component, and the (C) component, it is possible to obtain a cured product that has low dielectric properties, excellent peel strength even with a small surface roughness, and a high glass transition temperature.

[0209] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes has a low dielectric constant Dk. Therefore, when an insulating layer is formed with this cured product, an insulating layer with a low dielectric constant can be obtained. For example, the dielectric constant Dk of the cured product obtained by curing the resin composition under the conditions described in the examples described below is preferably 3.0 or less, more preferably 2.9 or less, and even more preferably 2.8 or less. The lower limit of the dielectric constant Dk of the cured product is not particularly limited, but may be 0.1 or more. The dielectric constant of the cured product can be measured by the method described in the examples.

[0210] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes has a low dielectric loss tangent. Therefore, when an insulating layer is formed with this cured product, an insulating layer with a low dielectric loss tangent can be obtained. For example, the dielectric loss tangent Df of the cured product obtained by curing the resin composition under the conditions described in the examples described later is preferably 0.010 or less, more preferably 0.005 or less, and even more preferably 0.004 or less. The lower limit of the dielectric loss tangent Df of the cured product is not particularly limited, but may be 0.001 or more. The dielectric loss tangent of the cured product can be measured by the method described in the examples.

[0211] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes can increase the plating peel strength between the resin composition and the plating. Therefore, when an insulating layer is formed from this cured product, an insulating layer with high peel strength between the insulating layer and the conductor layer can be obtained. For example, when an insulating layer and a plated conductor layer are formed by the method described in the examples below, the peel strength between the insulating layer and the conductor layer can be preferably 0.2 kgf / cm or more, more preferably 0.3 kgf / cm or more, and particularly preferably 0.4 kgf / cm or more. The upper limit of the adhesion is not particularly limited, but can be, for example, 10.0 kgf / cm or less. The peel strength can be measured by the method described in the examples.

[0212] A cured product obtained by thermally curing the resin composition at 200°C for 90 minutes exhibits the characteristic of being able to reduce the arithmetic mean roughness (Ra) of the cured product surface after roughening treatment. Therefore, an insulating layer having a small arithmetic mean roughness (Ra) of the surface after roughening treatment can be obtained. The arithmetic mean roughness (Ra) is preferably 100 nm or less, more preferably 80 nm or less, and even more preferably 50 nm or less. The lower limit is not particularly limited, but may be 1 nm or more. The arithmetic mean roughness (Ra) can be measured according to the method described in the examples below.

[0213] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes exhibits the characteristic of a high glass transition temperature. Therefore, when an insulating layer is formed from this cured product, an insulating layer having a high glass transition temperature and excellent heat resistance can be obtained. The glass transition temperature is preferably 140°C or higher, more preferably 145°C or higher, and even more preferably 150°C or higher. The upper limit is not particularly limited, but may be 300°C or lower. The glass transition temperature can be measured according to the method described in the examples below.

[0214] The resin composition according to one embodiment of the present invention is suitable as a resin composition for insulating applications, and is particularly suitable as a resin composition for forming an insulating layer. Thus, for example, the resin composition is suitable as a resin composition for forming an insulating layer of a printed wiring board (a resin composition for forming an insulating layer of a printed wiring board). In addition, the resin composition is suitable as a resin composition for forming an insulating layer (a resin composition for forming an insulating layer for forming a conductor layer) for forming a conductor layer (including a rewiring layer) formed on the insulating layer. The resin composition can also be used in a wide range of applications in which the resin composition can be used, such as a resin sheet, a sheet-like laminate material such as a prepreg, a solder resist, an underfill material, a die bonding material, a semiconductor encapsulant, a hole filling resin, a component embedding resin, a multi-chip package, a package-on-package, a wafer-level package, a panel-level package, a system-in-package, etc.

[0215] Furthermore, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition according to the present embodiment is also suitable as a resin composition for forming a rewiring formation layer as an insulating layer for forming a rewiring layer (resin composition for forming a rewiring formation layer) and as a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When a semiconductor chip package is manufactured, a rewiring layer may be further formed on the sealing layer. (1) A step of laminating a temporary fixing film onto a substrate; (2) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (3) forming an encapsulation layer on the semiconductor chip; (4) peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; and (6) A process of forming a rewiring layer as a conductor layer on the rewiring formation layer.

[0216] The above-mentioned resin composition can also be used when the printed wiring board is a circuit board with built-in components.

[0217] [Resin sheet] The resin sheet of the present invention includes a support and a resin composition layer formed from the resin composition of the present invention provided on the support.

[0218] The thickness of the resin composition layer is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less, from the viewpoint of making the printed wiring board thinner and being able to provide a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 5 μm or more.

[0219] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0220] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0221] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0222] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0223] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0224] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0225] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.

[0226] The resin sheet can be produced, for example, by preparing a resin varnish by dissolving a resin composition in an organic solvent, applying this resin varnish onto a support using a die coater or the like, and then drying the same to form a resin composition layer.

[0227] Examples of organic solvents include ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone; acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbons such as toluene and xylene; and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. The organic solvents may be used alone or in combination of two or more.

[0228] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0229] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0230] [Printed wiring board] A printed wiring board according to one embodiment of the present invention includes an insulating layer formed of a cured product obtained by curing the above-described resin composition.

[0231] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet by a method including the following steps (I) and (II). (I) A step of laminating a resin sheet on an inner layer substrate such that a resin composition layer of the resin sheet is bonded to the inner layer substrate. (II) A step of curing the resin composition layer to form an insulating layer

[0232] The "inner layer substrate" used in step (I) is a member that becomes the substrate of the printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a printed wiring board is also included in the "inner layer substrate". When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.

[0233] The lamination of the inner layer substrate and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (such as a SUS roll). It is preferable to press the thermocompression member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.

[0234] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination may be performed under reduced pressure conditions, preferably at a pressure of 26.7hPa or less.

[0235] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0236] After lamination, the laminated resin sheet may be smoothed under atmospheric pressure, for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0237] The support may be removed between step (I) and step (II) or after step (II).

[0238] In step (II), the resin composition layer is cured to form an insulating layer made of a cured product of the resin composition. The curing conditions for the resin composition layer are not particularly limited, and the conditions employed for forming an insulating layer of a printed wiring board may be used. The resin composition layer may be cured by irradiation with active energy rays such as ultraviolet rays, but is usually thermally cured by heating.

[0239] For example, the thermal curing conditions for the resin composition layer vary depending on the type of resin composition, but in one embodiment, the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.

[0240] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. to 120° C., preferably 60° C. to 115° C., more preferably 70° C. to 110° C. for 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.

[0241] The method for producing a printed wiring board may further include the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer. When the support is removed after step (II), the removal of the support may be performed between steps (II) and (III), between steps (III) and (IV), or between steps (IV) and (V). In addition, the steps (I) to (V) of forming the insulating layer and the conductor layer may be repeated to form a multilayer wiring board, as necessary.

[0242] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.

[0243] Step (IV) is a step of roughening the insulating layer. Usually, smears are also removed in this step (IV). The procedure and conditions of the roughening treatment are not particularly limited. For example, the insulating layer can be roughened by carrying out a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order.

[0244] Examples of the swelling liquid used in the roughening treatment include an alkaline solution and a surfactant solution, and an alkaline solution is preferred. As the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferred. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using the swelling liquid is not particularly limited, but can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferred to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.

[0245] An example of an oxidizing agent used in the roughening treatment is an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.

[0246] The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Solution Securigant P" manufactured by Atotech Japan. Treatment with a neutralizing solution can be performed by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30°C to 80°C for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40°C to 70°C for 5 to 20 minutes is preferred.

[0247] In one embodiment, the arithmetic mean roughness Ra of the insulating layer surface after the roughening treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc. The root mean square roughness (Rq) of the insulating layer surface after the roughening treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc. The arithmetic mean roughness (Ra) and root mean square roughness (Rq) of the insulating layer surface can be measured using a non-contact surface roughness meter.

[0248] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0249] The conductor layer may be a single-layer structure, or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0250] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.

[0251] The conductor layer is preferably formed by plating. For example, the surface of the insulating layer can be plated by a semi-additive method, a full-additive method, or the like to form a conductor layer having a desired wiring pattern. From the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.

[0252] A plating seed layer is formed on the surface of the insulating layer by electroless plating. Then, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.

[0253] [Semiconductor Devices] A semiconductor device according to an embodiment of the present invention includes the above-mentioned printed wiring board. This semiconductor device can be manufactured using the above-mentioned printed wiring board.

[0254] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft). EXAMPLES

[0255] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples. In the following description, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Furthermore, the operations described below were performed in an environment of normal temperature and pressure, unless otherwise specified.

[0256] <Preparation of Maleimide Resin A> An MEK solution (non-volatile content 70% by mass) of maleimide resin A synthesized by the method described in Synthesis Example 1 of the Japan Institute of Invention and Innovation's Technical Journal Publication No. 2020-500211 was prepared. This maleimide resin A has a structure represented by the following formula.

[0257] [ka]

[0258] When the FD-MS spectrum of maleimide resin A is measured, peaks at M+=560, 718, and 876 are confirmed. These peaks correspond to the cases where n1 is 0, 1, and 2, respectively. When maleimide resin A is analyzed by GPC, the value of the number of repeating units n1 of the indane skeleton portion is calculated based on the number average molecular weight, and n1=1.47, and the molecular weight distribution (Mw / Mn)=1.81. Furthermore, the content of maleimide resins with an average number of repeating units n1 of 0 in the total amount of maleimide resin A (100 area %) is 26.5 area %.

[0259] The FD-MS spectrum of the maleimide resin A was measured using the following measuring device and under the following measuring conditions. (FD-MS spectrum measuring device and measuring conditions) Measurement equipment: JMS-T100GC AccuTOF Measurement conditions Measurement range: m / z=4.00~2000.00 Rate of change: 51.2mA / min Final current value: 45mA Cathode voltage: -10kV Recording interval: 0.07 sec

[0260] The GPC of the maleimide resin A was measured using the following measuring device and under the following measuring conditions. Measurement equipment: Tosoh Corporation "HLC-8320 GPC" Columns: Tosoh guard column "HXL-L", Tosoh "TSK-GEL G2000HXL", Tosoh "TSK-GEL G2000HXL", Tosoh "TSK-GEL G3000HXL", and Tosoh "TSK-GEL G4000HXL" Detector: RI (differential refractometer) Data processing: Tosoh Corporation's "GPC Workstation EcoSEC-WorkStation" Measurement conditions: Column temperature 40℃ Developing solvent: Tetrahydrofuran Flow rate 1.0ml / min Standard: Use monodisperse polystyrene with a known molecular weight in accordance with the measurement manual of the "GPC Workstation EcoSEC-WorkStation". Sample: A 1.0 mass% tetrahydrofuran solution of the maleimide compound in terms of non-volatile components, filtered through a microfilter (50 μl).

[0261] The molecular weight distribution (weight-average molecular weight (Mw) / number-average molecular weight (Mn)) of maleimide resin A and the average number of repeating units "n1" contributing to the indane skeleton in the maleimide resin are represented by those calculated from the GPC chart obtained by the above GPC measurement. Also, the average number of repeating units "n1" is represented by that calculated based on the number-average molecular weight (Mn). Specifically, for compounds with n1 ranging from 0 to 4, the theoretical molecular weight and the measured molecular weight in GPC are plotted on a scatter diagram, and an approximate straight line is drawn. Then, the number-average molecular weight (Mn) is determined from the point indicated by the measured Mn(1) on this straight line, and further the average number of repeating units "n1" is calculated. Furthermore, based on the results of the GPC measurement, the content ratio (area%) of the maleimide resin with an average number of repeating units n1 of 0 in 100 area% of the total amount of maleimide resin A is calculated. For details, reference can be made to the Invention Association Public Technical Report Public Technical Number 2020-500211.

[0262] <Synthesis of PEEK (Polyetheretherketone) Compound A> Into a 500 mL flask (three-necked) equipped with a stirrer, an argon inlet tube, and a Dean-Stark apparatus, put 31.443 g of 4,4'-difluorobenzophenone, 27.419 g of bisphenol A, 29.894 g of potassium carbonate anhydrous, 180 mL of N-methylpyrrolidone, and 90 mL of toluene, heat with stirring under an argon atmosphere, and reflux toluene at 130 - 140 °C for 4 hours. Then, heat further to distill off toluene at 170 - 180 °C. Furthermore, continue stirring at 170 - 180 °C for 10 hours, then return to room temperature to obtain Product 1.

[0263] To the flask containing the product 1, 5.233 g of 4-aminophenol, 6.628 g of anhydrous potassium carbonate, 18 mL of N-methylpyrrolidone, and 90 mL of toluene were added, and the mixture was heated again under an argon atmosphere while stirring, and the toluene was refluxed at 130-140°C for 3 hours. After that, the mixture was heated to 170-180°C to distill off the toluene, and stirring was continued for 4 hours while maintaining the temperature. After that, the mixture was cooled to room temperature, and the reaction solution was added to 5000 mL of methanol and filtered to obtain a powdery solid. This powdery solid was repeatedly washed with methanol and water, and then dried at 100°C for 8 hours to obtain 37.461 g of a powdery solid (Diamine-A).

[0264] In a 500mL flask (three-necked) equipped with a stirrer and an argon inlet tube, 0.878g of Diamine-A, 4.943g of maleic anhydride, and 240mL of N-methylpyrrolidone were placed and stirred at room temperature for 18 hours under an argon atmosphere. Then, 8.576g of acetic anhydride and 0.689g of sodium acetate were added and stirred at 60°C for 6 hours. After the reaction solution was returned to room temperature, the reaction solution was added to 5000mL of methanol to obtain a powdery solid. This powdery solid was repeatedly washed with methanol and water, and then dried at 100°C for 8 hours to obtain 28.434g of PEEK compound A represented by the following formula. The number average molecular weight of PEEK compound A calculated by GPC measurement was 2230. [ka]

[0265] [Example 1] A mixture of 14 parts of PEEK compound A, 20 parts of naphthalene-type epoxy resin ("ESN475V" manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd., epoxy equivalent of approximately 332 g / eq.), 30 parts of active ester-based curing agent ("HPC-8000-65T" manufactured by DIC Corporation, active group equivalent of 223, toluene solution with solid content of 65% by mass), and inorganic filler (spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with an amine-based alkoxysilane compound ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.) 2The mixture was mixed with 60 parts of ethyl acetate / g and 0.5 parts of a curing accelerator ("1B2PZ", 2-phenyl-1-benzyl-1H-imidazole, manufactured by Shikoku Kasei Co., Ltd.) and dispersed uniformly using a high-speed rotating mixer to obtain a resin varnish.

[0266] A polyethylene terephthalate film with a release layer ("AL5" manufactured by Lintec Corporation, thickness 38 μm) was prepared as a support. The resin varnish was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 40 μm. The resin varnish was then dried at 80°C to 100°C (average 90°C) for 4 minutes to obtain a resin sheet including a support and a resin composition layer.

[0267] [Example 2] In Example 1, 30 parts of an active ester curing agent (DIC Corporation's "HPC-8000-65T", active group equivalent 223, toluene solution with solid content of 65 mass %) was changed to 30 parts of an active ester curing agent (DIC Corporation's "HPC-8150-62T", active group equivalent 229, toluene solution with solid content of 62 mass %). A resin varnish and a resin sheet were obtained in the same manner as in Example 1 except for the above.

[0268] [Example 3] In Example 2, The amount of PEEK compound A was changed from 14 parts to 10.5 parts. Furthermore, 5 parts of a radical polymerizable compound (biphenylaralkyl-type maleimide compound ("MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd., maleimide group equivalent: 275 g / eq., MEK / toluene mixed solution with non-volatile content of 70%) was used. A resin varnish and a resin sheet were obtained in the same manner as in Example 2 except for the above.

[0269] [Example 4] In Example 2, The amount of PEEK compound A was changed from 14 parts to 12.6 parts. Furthermore, 2 parts of a radical polymerizable compound ("BMI-1500" manufactured by Designor Molecular Systems, Inc., maleimide group equivalent weight 750 g / eq.) was used. A resin varnish and a resin sheet were obtained in the same manner as in Example 2 except for the above.

[0270] [Example 5] In Example 2, The amount of active ester curing agent (DIC "HPC-8150-62T", active group equivalent 229, toluene solution with solid content of 62% by mass) was changed from 30 parts to 25 parts. The amount of hardening accelerator (Shikoku Kasei's "1B2PZ", 2-phenyl-1-benzyl-1H-imidazole) was changed from 0.5 parts to 0.1 parts. Furthermore, 5 parts of a triazine skeleton-containing cresol novolac-based curing agent (DIC Corporation's "LA3018-50P", hydroxyl equivalent 151, 1-methoxy-2-propanol solution with 50% non-volatile components) was used. A resin varnish and a resin sheet were obtained in the same manner as in Example 2 except for the above.

[0271] [Example 6] In Example 2, The amount of PEEK compound A was changed from 14 parts to 10.5 parts. Furthermore, 5 parts of a MEK solution of maleimide resin A (70% by mass of non-volatile components) was used. A resin varnish and a resin sheet were obtained in the same manner as in Example 2 except for the above.

[0272] [Example 7] In Example 1, 30 parts of the active ester curing agent (DIC Corporation's "HPC-8000-65T", active group equivalent 223, toluene solution with solid content of 65% by mass) was changed to 30 parts of an active ester curing agent containing a naphthalene structure (Air Water Corporation's "PC1300-02-65MA", active group equivalent 200, methyl amyl ketone solution with solid content of 65% by mass). A resin varnish and a resin sheet were obtained in the same manner as in Example 1 except for the above.

[0273] [Comparative Example 1] In Example 2, Without using 14 parts of PEEK compound A, Spherical silica (Admatechs' "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with an inorganic filler (amine-based alkoxysilane compound (Shin-Etsu Chemical's "KBM573") 2 / g) was changed from 60 parts to 45 parts. A resin varnish and a resin sheet were obtained in the same manner as in Example 2 except for the above.

[0274] [Comparative Example 2] In Example 3, Without using 10.5 parts of PEEK compound A, The amount of the radical polymerizable compound (biphenylaralkyl-type maleimide compound ("MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd., maleimide group equivalent: 275 g / eq., MEK / toluene mixed solution with 70% nonvolatile content)) was changed from 5 parts to 20 parts. A resin varnish and a resin sheet were obtained in the same manner as in Example 3 except for the above.

[0275] [Comparative Example 3] In Example 4, Without using 12.6 parts of PEEK compound A, The amount of the radical polymerizable compound ("BMI-1500" manufactured by Designor Molecular Systems, Inc., maleimide group equivalent: 750 g / eq.) was changed from 2 parts to 14 parts. A resin varnish and a resin sheet were obtained in the same manner as in Example 4 except for the above.

[0276] [Measurement of dielectric properties (dielectric constant and dielectric tangent)] The resin sheets prepared in the examples and comparative examples were heated at 200°C for 90 minutes to thermally cure the resin composition layer. The support was then peeled off to obtain "resin composition cured product A". The resin composition cured product A was cut into a test piece having a width of 2 mm and a length of 80 mm. The dielectric constant Dk and dielectric loss tangent Df of the test piece were measured at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C using an Agilent Technologies "HP8362B" by a cavity resonance perturbation method. Measurements were performed on three test pieces, and the average values ​​are shown in the table below.

[0277] [Measurement of plating peel strength] (1) Surface preparation for inner layer circuit boards: A glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, board thickness 0.4 mm, Panasonic "R1515A") with inner layer circuits (copper foil) on both sides was prepared as an inner layer circuit board. Both sides of this inner layer circuit board were etched by 1 μm using MEC's ​​"CZ8101" to roughen the copper surface.

[0278] (2) Lamination of resin sheet: The resin sheet was laminated on both sides of the inner layer circuit board using a batch type vacuum pressure laminator (Nikko Materials Co., Ltd., 2-stage build-up laminator, CVP700). This lamination was performed so that the resin composition layer of the resin sheet was in contact with the inner layer circuit board. This lamination was also performed by reducing the pressure for 30 seconds to 13 hPa or less, and pressing at 130°C and a pressure of 0.74 MPa for 45 seconds. Next, a heat press was performed at 120°C and a pressure of 0.5 MPa for 75 seconds.

[0279] (3) Curing of the resin composition: The laminated resin sheet and the inner layer circuit board were heated at 130° C. for 30 minutes, and then heated at 170° C. for 30 minutes to harden the resin composition and form an insulating layer. The support was then peeled off to obtain a laminated substrate having an insulating layer, an inner layer circuit board, and an insulating layer in this order.

[0280] (4) Roughening treatment: The laminated substrate was immersed in a swelling solution (Atotech Japan's Swelling Dip Securigant P (aqueous solution of glycol ethers and sodium hydroxide) containing diethylene glycol monobutyl ether). The laminated substrate was then immersed in a roughening solution (Atotech Japan's Concentrate Compact P (aqueous solution of KMnO4: 60 g / L and NaOH: 40 g / L)) at 80°C for 20 minutes. The laminated substrate was then immersed in a neutralizing solution (Atotech Japan's Reduction Shalusin Securigant P (aqueous solution of sulfuric acid)) at 40°C for 5 minutes. The laminated substrate was then dried at 80°C for 30 minutes to obtain "Evaluation Substrate A."

[0281] (5) Semi-additive plating: Evaluation substrate A was immersed in an electroless plating solution containing PdCl2 at 40°C for 5 minutes, and then immersed in an electroless copper plating solution at 25°C for 20 minutes. It was then heated at 150°C for 30 minutes and annealed. An etching resist was then formed, and a pattern was formed by etching. Copper sulfate electrolytic plating was then performed to form a conductor layer with a thickness of 20 μm. An annealing process was then performed at 200°C for 60 minutes to obtain "evaluation substrate B."

[0282] (6) Measurement of plating peel strength: A cut was made in the conductor layer of evaluation board B, surrounding a rectangular portion 10 mm wide and 100 mm long. One end of the rectangular portion was peeled off and held with a gripper (Autocom type testing machine "AC-50C-SL" manufactured by TSE Corporation). The rectangular portion was peeled off vertically at room temperature at a speed of 50 mm / min using the gripper, and the load (kgf / cm) when 35 mm had been peeled off was measured as the plating peel strength.

[0283] [Measurement of surface roughness Ra] The arithmetic mean roughness Ra of the surface of the insulating layer of evaluation board A was measured. The measurement was performed using a non-contact surface roughness meter (WYKO NT3300 manufactured by B-CO Instruments) in VSI mode with a 50x lens, with the measurement range set to 121μm x 92μm. This measurement was performed at 10 measurement points, and the average values ​​are shown in the table below.

[0284] [Measurement of glass transition temperature] The cured resin composition A was cut into a test piece with a width of about 5 mm and a length of about 15 mm, and a thermomechanical analysis was performed by a tensile load method using a dynamic viscoelasticity measuring device (EXSTAR6000, manufactured by SII Nano Technology Co., Ltd.). After mounting the test piece on the device, the measurement was performed under the measurement conditions of a load of 200 mN and a heating rate of 2°C / min. The peak top of the obtained tan δ was calculated as the glass transition temperature (°C).

[0285] [Table 1] *In the table, the content of component (A) represents the content of component (A) when the resin component in the resin composition is 100% by mass. The content of component (E) represents the content of component (E) when the non-volatile components in the resin composition are 100% by mass. Component (C) / component (B) represents the ratio of [total number of active groups in active ester curing agent] / [total number of epoxy groups in epoxy resin], where [total number of epoxy groups in epoxy resin] refers to the total value obtained by dividing the mass of the non-volatile components of the epoxy resin present in the resin composition by the epoxy equivalent, and [total number of active groups in active ester curing agent] refers to the total value obtained by dividing the mass of the non-volatile components of the active ester curing agent present in the resin composition by the active ester group equivalent.

Claims

1. (A) a polyether ether ketone compound having a maleimide group, (B) an epoxy resin, and (C) an active ester curing agent, The content of the component (A) is 1% by mass or more and 25% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass, The content of the (B) component is 5% by mass or more and 30% by mass or less, when the non-volatile components in the resin composition are taken as 100% by mass, A resin composition, wherein the content of the component (C) is 1% by mass or more and 30% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass.

2. The resin composition according to claim 1, wherein the number average molecular weight of the component (A) is 10,000 or less.

3. The resin composition according to claim 1 or 2, wherein the component (A) has a maleimide group at a terminal thereof.

4. The content of the component (A) is 5 mass% or more and 60 mass% or less, when the resin component, which is a component excluding inorganic fillers among non-volatile components in the resin composition, is 100 mass%. The resin composition according to any one of claims 1 to 3.

5. The resin composition according to any one of claims 1 to 4, wherein the component (B) comprises a naphthol-type epoxy resin.

6. The resin composition according to any one of claims 1 to 5, wherein the component (C) is at least one selected from the group consisting of dicyclopentadiene-type active ester-based curing agents and naphthalene-type active ester-based curing agents containing a naphthalene structure.

7. the quantitative ratio of the component (B) to the component (C) is, as a ratio of the total number of active groups in the component (C) to the total number of epoxy groups in the component (B), 0.01 or more and 5 or less; The total number of epoxy groups in the component (B) is a value obtained by dividing the mass of the non-volatile components of the component (B) present in the resin composition by the epoxy equivalent, and The total number of active groups of the component (C) is a value obtained by dividing the mass of the non-volatile component (C) present in the resin composition by the active ester group equivalent. The resin composition according to any one of claims 1 to 6.

8. The resin composition according to any one of claims 1 to 7, further comprising (D) a resin having a polymerizable unsaturated group different from the component (A).

9. The resin composition according to claim 8, wherein the component (D) is a resin containing a maleimide group and an aromatic ring.

10. The resin composition according to any one of claims 1 to 9, further comprising (E) an inorganic filler.

11. The resin composition according to claim 10, wherein the content of the component (E) is 40% by mass or more and 75% by mass or less, based on 100% by mass of non-volatile components in the resin composition.

12. The resin composition according to any one of claims 1 to 11, which is for forming an insulating layer.

13. The resin composition according to any one of claims 1 to 12, which is a resin composition for forming an insulating layer when a conductor layer is formed on an insulating layer.

14. A resin sheet comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of claims 1 to 13.

15. A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of claims 1 to 13.

16. A semiconductor device comprising the printed wiring board according to claim 15.

Citation Information

Patent Citations

  • Loss reducing device used for partial feed-in turbine, and partial feed-in turbine

    JP2020128706A

  • Resin composition

    JP2022025704A

  • Resin composition

    JP7552124B2

  • Photosensitive resin composition, photosensitive element, and printed wiring board and method for manufacturing the same

    JP2019066792A