Lithium ion storage battery
The use of silicon particles coated with a graphene compound and binder in lithium-ion batteries addresses mechanical issues by maintaining electrical conductivity and adhesion, resulting in high-capacity, high-energy-density batteries with extended lifespan and reduced resistance.
Patent Information
- Application Number
- JP2024154561
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2015-07-16
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium-ion storage batteries face issues with mechanical destruction and pulverization of silicon particles due to large volume changes during alloying and dealloying, leading to reduced capacity, conductive path damage, and increased electrical resistance, which affects the battery's reliability and lifespan.
A negative electrode configuration using silicon particles coated with a graphene compound and a binder, featuring voids to accommodate volume changes, maintains electrical conductivity and adhesion, thereby preventing mechanical damage and enhancing the battery's performance.
The configuration results in a power storage device with increased capacity, high energy density, and extended lifespan, while being cost-effective and reliable, with improved electrical conductivity and reduced resistance.
Smart Images

Figure 2024166288000001_ABST
Abstract
Description
[Technical field]
[0001] One embodiment of the present invention relates to an electrode, a storage battery, a power storage device, and an electronic device.
[0002] One embodiment of the present invention is not limited to the above technical fields. The invention relates to a process, a machine, a manual, It is related to the fact or composition of matter. Specifically, the technical field of one embodiment of the present invention disclosed in this specification includes semiconductor devices, display devices, Light emitting device, power storage device, storage device, imaging device, driving method thereof, or manufacturing method thereof can be cited as an example.
[0003] In this specification, the term "electronic device" refers to any device that is driven by electricity, including electro-optical devices. This includes all of the above, including information terminal devices, etc. Electronic devices may have built-in storage batteries. Needless to say, in the specification, "built-in" means having something inside so that it cannot be removed or replaced. This includes devices that are not portable but are carried inside and can be freely removed, such as a battery pack. [Background technology]
[0004] In recent years, various types of storage devices such as lithium-ion batteries, lithium-ion capacitors, and air batteries have become available. In particular, lithium-ion batteries, which have high output and high energy density, are being developed. Batteries are used in mobile phones, smartphones, notebook computers and other portable information terminals, Electronic devices such as players and digital cameras, medical devices, and hybrid vehicles (HEVs) Next-generation cleaners such as electric vehicles (EVs) and plug-in hybrid vehicles (PHEVs) Demand for rechargeable batteries is expanding rapidly along with the development of the semiconductor industry, such as in the case of rechargeable energy vehicles. As a source of energy, it has become indispensable in today's information society.
[0005] The basic structure of a storage battery is that an electrolyte, which can be a liquid electrolyte or a solid electrolyte, is placed between the positive and negative electrodes. The positive and negative electrodes are each a current collector and an active material disposed on the current collector. In the case of lithium-ion batteries, the material is absorbed into the battery. The materials capable of alloying and de-alloying, as well as alloying and dealloying, are used as active materials for the positive and negative electrodes. Used as a substance.
[0006] In order to increase the contact area between the active material and the electrolyte, it is preferable to make the active material particulate. Therefore, a binder, a conductive additive, etc. are mixed with the particulate active material to form an active material. The material layer may be provided on a current collector to form a positive or negative electrode.
[0007] The negative electrode active material is, for example, a carrier ion such as carbon or silicon (hereinafter, The absorption and release of carrier ions (referred to as carrier ions) and the alloying and de-alloying of carrier ions Materials that can be converted to gold are used. For example, silicon is about 10 times more durable per weight than graphite. Since it is possible to alloy with the carrier ions of lithium ions, the theoretical capacity is large and This is advantageous in terms of increasing the capacity of storage batteries.
[0008] In general, the theoretical capacity of carrier ions is large, and the absorption and release reaction of carrier ions is Active materials that undergo alloying and dealloying reactions with carrier ions are For example, when silicon, which has a large theoretical capacity, is used as the active material, The volume of the ions changes significantly as the ions are alloyed with and dealloyed by the carrier ions. The stress caused by the change in the volume of silicon causes the contact area between the current collector and silicon, the active material This reduces the contact area between the electrodes, impairing the conductive path and degrading the battery characteristics. Therefore, a layer made of silicon is formed on the current collector, and then a graphite layer is formed on the layer made of silicon. By providing a layer made of fibrous material, the stress caused by the expansion and contraction of the silicon layer is alleviated. It has been reported that this method reduces the deterioration of battery characteristics (see Patent Document 1).
[0009] In addition, we have developed a composite material in which one or more silicon particles and voids are covered with a carbon film. It has been reported that it is used as a negative electrode active material (see Non-Patent Document 1). [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2001-283834 A [Non-patent literature]
[0011] [Non-Patent Document 1] “A pomegranate-inspired nanoscale design for large-volume-change lithium battery anodes”, Nian Liu, Zhenda Lu, Jie Zhao, Matthew T. McDowell, Hyun-Wook Lee, Wenting Zhao and Yi Cui, Nature Nanotechnology Letters 16, February, 2014. Summary of the Invention [Problem to be solved by the invention]
[0012] In Non-Patent Document 1, one or more silicon particles with a particle diameter of about 80 nm are enclosed with voids. The composite material is made by oxidizing the surface of silicon particles. A silicon oxide film is formed by coating the surface of the silicon oxide film with a carbon film. By removing the carbon film by etching, voids are formed around the silicon particles covered with the carbon film. has been formed.
[0013] However, in the composite material described in Non-Patent Document 1, the grain size is as small as 80 nm. Silicon particles are used. Such small silicon particles are expensive and difficult to mass-produce. From the viewpoint of chemical synthesis, it is not practical to use this as a negative electrode active material in a lithium ion storage battery.
[0014] As described above, silicon particles undergo alloying and dealloying with carrier ions. The volume change of silicon is large. Therefore, alloying and dealloying with carrier ions occurs. During the repetition, mechanical destruction and pulverization may occur. It becomes difficult to maintain the function of the battery as an ion storage battery. This is called "pulverization." The material breaks down into small particles due to repeated cracking caused by mechanical stress and shrinkage. For example, they may peel off from the current collector, the peeled powder may get stuck in the gaps of the separator, or they may adhere to the surface of the positive electrode. In addition, as the material expands and contracts, silicon particles may adhere to the material. This can cause poor contact between the silicon particles or between the silicon particles and the current collector, resulting in loss of conductive paths. The loss of conductive paths leads to a loss of capacity with repeated charge and discharge cycles. .
[0015] In the composite material described in Non-Patent Document 1, the silicon particles are pulverized in this way. In this case, the thickness of the carbon film covering the silicon particles and voids is very thin, less than 10 nm. Therefore, silicon particle fragments break through the carbon film and adhere to the separator voids and the positive electrode surface. In addition, it is difficult to hold the finely pulverized silicon particles in place with such a thin carbon film. To address this issue, the silicon particles and voids are covered. It is desirable to use a film that is physically strong and has excellent electrical conductivity.
[0016] In view of the above, an object of one embodiment of the present invention is to provide a power storage device with large capacity. Another object of one embodiment of the present invention is to provide a power storage device with high energy density. Another object of one embodiment of the present invention is to provide a highly reliable power storage device. Another object of one embodiment of the present invention is to provide a power storage device with a long lifetime. Another object of one embodiment of the present invention is to provide a low-cost power storage device.
[0017] Another object of one embodiment of the present invention is to provide an electrode with large capacitance. An object of one embodiment of the present invention is to provide an electrode with high energy density. Another object of one embodiment of the present invention is to provide a highly reliable electrode. An object of one embodiment of the present invention is to provide an electrode having a long life. One object of the present invention is to provide a low-cost electrode.
[0018] Alternatively, one embodiment of the present invention is a novel material, a novel electrode, a novel storage battery, or a novel One object is to provide a power storage device or the like.
[0019] The description of these problems does not preclude the existence of other problems. It is not necessary for one embodiment to solve all of these problems. The subject matter will be self-evident from the description, drawings, claims, etc. Other issues can be extracted from the drawings, claims, etc. [Means for solving the problem]
[0020] One embodiment of the present invention includes a negative electrode and a positive electrode. The negative electrode includes a current collector and an active material layer, The active material layer includes active material particles, a graphene compound covering the active material particles, and a binder. and having voids in contact with the active material particles, the graphene compound, and the binder. It is a storage device that has the following characteristics.
[0021] Alternatively, one embodiment of the present invention includes a negative electrode and a positive electrode. The negative electrode includes a current collector and an active material layer, The active material layer comprises active material particles, a graphene compound and a binder that cover the active material particles. A first void having an adhesive and contacting the active material particles, the graphene compound, and the binder. and having second voids in contact with the graphene compound and the binder. It is an electricity storage device.
[0022] Alternatively, one embodiment of the present invention includes a negative electrode and a positive electrode. The negative electrode includes a current collector and an active material layer, The active material layer comprises active material particles, a graphene compound covering the active material particles, and a binder. and a plurality of voids in contact with the active material particles, the graphene compound, and the binder. The power storage device is characterized by having
[0023] In the above-mentioned configuration, the graphene compound is a reduced oxide having 2 to 100 layers. The interlayer distance of the reduced graphene oxide is 0.335 nm or more and 0.7 nm. It is preferable that:
[0024] In the above structure, the active material particles are preferably made of silicon.
[0025] In the above structure, the binder is preferably polyimide.
[0026] In the above-mentioned configuration, the active material particles have an average particle size of 0.5 μm or more and 1.5 μm or less. It is preferable that:
[0027] In the above configuration, the active material particles may be produced by crushing a silicon wafer. preferable.
[0028] Another embodiment of the present invention is a power storage device including any one of the above power storage devices, an operation button, and a display. and an electronic device having a display device. Effect of the Invention
[0029] According to one embodiment of the present invention, a power storage device with large capacity can be provided. According to one embodiment of the present invention, a power storage device with high energy density can be provided. According to one embodiment of the present invention, a highly reliable power storage device can be provided. According to another embodiment of the present invention, a power storage device having a long lifetime can be provided. It is possible to provide a power storage device.
[0030] Alternatively, one embodiment of the present invention can provide an electrode having a large capacity. In one embodiment of the present invention, an electrode having a high energy density can be provided. According to one aspect of the present invention, a highly reliable electrode can be provided. It is possible to provide a long electrode. One aspect of the present invention is to provide a low-cost electrode. can.
[0031] Alternatively, one embodiment of the present invention is a novel material, a novel electrode, a novel storage battery, or a novel It is possible to provide a power storage device and the like.
[0032] The description of these effects does not preclude the existence of other effects. An embodiment does not necessarily have to have all of these effects. The above will become apparent from the description in the specification, drawings, claims, etc. It is possible to extract other effects from the descriptions in the claims, etc. [Brief description of the drawings]
[0033] [Figure 1] FIG. [Diagram 2] FIG. [Diagram 3] 3A to 3C illustrate a method for manufacturing an electrode. [Figure 4] 3A to 3C illustrate a method for manufacturing an electrode. [Diagram 5] FIG. [Figure 6] FIG. 1 is a cross-sectional view of a storage battery. [Figure 7] FIG. [Figure 8] FIG. [Figure 9] 1A to 1C are diagrams illustrating a method for manufacturing a storage battery. [Figure 10] 1A to 1C are diagrams illustrating a method for manufacturing a storage battery. [Figure 11] FIG. [Figure 12] FIG. 4 is a diagram for explaining the radius of curvature of a surface. [Figure 13] FIG. 2 is a diagram for explaining the radius of curvature of a film. [Figure 14] FIG. 2 is a cross-sectional view illustrating a portion of a storage battery. [Figure 15] FIG. 2 is a cross-sectional view illustrating a portion of a storage battery. [Figure 16] FIG. 2 is a cross-sectional view illustrating a portion of a storage battery. [Figure 17] FIG. 1 is a diagram illustrating a coin-type storage battery. [Figure 18] FIG. 1 is a diagram illustrating a cylindrical storage battery. [Figure 19] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 20] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 21] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 22] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 23] 1A and 1B are diagrams illustrating examples of power storage devices. [Figure 24] 1A to 1C are diagrams illustrating examples of electronic devices. [Diagram 25] 1A to 1C are diagrams illustrating examples of electronic devices. [Figure 26] 1A to 1C are diagrams illustrating examples of electronic devices. [Figure 27] 1A to 1C are diagrams illustrating examples of electronic devices. [Figure 28] Cross-sectional SEM photograph of the negative electrode active material layer. [Figure 29] Cross-sectional SEM photograph of the negative electrode active material layer. [Diagram 30] FIG. 4 is a graph showing the relationship between the charge / discharge cycle and the discharge capacity of a storage battery. [Diagram 31] FIG. 4 is a graph showing the relationship between the charge / discharge cycle and the discharge capacity of a storage battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following description, and it is understood by those skilled in the art that various changes can be made in form and detail. The present invention is not limited to the description of the following embodiments. It is not something that is done.
[0035] In each of the drawings described in this specification, a positive electrode, a negative electrode, an active material layer, a separator, an outer casing, The size and thickness of each component may be exaggerated for clarity. Therefore, each component is not necessarily limited by its size, and the distance between each component is not necessarily limited by its size. It is not limited to relative size.
[0036] "Electrically connected" means that the device is connected via "something that has some kind of electrical effect." Here, "something that has some electrical effect" refers to the electrical effect between connected objects. There are no particular limitations as long as it is possible to transmit and receive signals.
[0037] The words "membrane" and "layer" may be interchangeable depending on the circumstances. For example, the term "conductive layer" may be replaced with "conductive Alternatively, for example, the term "insulating film" may be used. In some cases, the terminology may be changed to the term "insulating layer."
[0038] In addition, in the configuration of the present invention described in this specification, etc., The same reference numerals are used for the same parts in different drawings, and the repeated explanations are omitted. In addition, when referring to parts having similar functions, the same hatch pattern is used and special symbols are attached. This may not be the case.
[0039] In addition, in this specification, ordinal numbers such as 1st, 2nd, 3rd, etc. are used for convenience. It does not indicate the order of the processes or the hierarchical relationship between the processes. For example, the "first" can be replaced with the "second" or the "third" as appropriate. In addition, the ordinal numbers described in this specification and the like and the ordinal numbers used to specify one aspect of the present invention are The ordinal numbers used may not match.
[0040] In this specification, flexibility refers to the property that an object is flexible and can be bent. It refers to the property of an object being able to deform in response to an external force applied to it, and is called elasticity or deformation. The question is not whether the battery can return to its previous shape. A flexible storage battery can change shape in response to external forces. A flexible storage battery can be used in a deformed state while being fixed in place. It can be repeatedly deformed and used, or it can be used in an undeformed state. In addition, in this specification, the inside of the exterior body refers to the inside of the exterior body of the lithium ion storage battery. This refers to the area enclosed in the box, and includes structures such as the positive electrode, negative electrode, active material layer, and separator, as well as the electrolyte, etc. This is the area where
[0041] In addition, the contents described in the description of the embodiment of the present invention may be used in appropriate combination. can.
[0042] (Embodiment 1) In this embodiment, an electrode according to one embodiment of the present invention will be described.
[0043] In order to extend the life of storage batteries such as lithium-ion batteries, charging and discharging ( When repeated charging and discharging cycles are performed, deterioration of the components of the storage battery, such as electrodes, is minimized. It is important to do so.
[0044] The longer life of the storage battery means that, for example, the frequency of battery replacement can be reduced. The convenience of the equipment equipped with the battery can be improved. For example, the battery has a life of more than 5 years. For example, the battery is designed to have a life of at least 1800 charge / discharge cycles. It is better to have life.
[0045] In addition, considering in-vehicle and outdoor use, the storage battery needs to be able to operate over a wider temperature range. For example, it is more preferable that the device operates stably even in an environment where the temperature exceeds 45°C. It is.
[0046] The electrodes used in lithium-ion batteries contain active materials. Many active materials are As a result, expansion and contraction occur.
[0047] Here, as an example, a case will be considered in which the electrode has a current collector and an active material layer on the current collector. The active material layer contains an active material. The active material layer may also contain a binder and a conductive assistant. .
[0048] There is also a demand for storage batteries that can be installed in wearable devices. It is preferable that the abrasive device has flexibility so that it can be deformed to fit the part of the body where it is worn. If the battery could deform in response to the deformation of the wearable device, This is preferable because it provides a wider range of options for the location of the storage battery, such as on the part or surface.
[0049] In this way, the storage battery installed in the wearable device changes its shape as the wearable device changes. When a battery is deformed, the electrodes may bend, causing the active materials to break apart and the active materials to break apart. This may result in poor contact between the active material and the conductive additive, or between the active material and the binder, etc.
[0050] Therefore, for example, in a storage battery mounted on a wearable device, the electrodes are deformed. Even in this state, the adhesion between active materials, between active materials and conductive additives, between active materials and binders, etc. It is more important to be able to suppress the decrease in
[0051] In addition, a storage battery using an oxidation-reduction reaction of carrier ions, such as a lithium ion storage battery, In this case, carrier ions are inserted into and removed from the active material during charging and discharging, and carrier ions are formed as carrier ions. Alloying and dealloying reactions with metals occur.
[0052] If the electrical resistance of the battery electrodes is high, an overvoltage will occur, for example, on the surface of the active material. Reactions due to overvoltage may occur. For example, the reaction potential may be low at the negative electrode. In many cases, when the electrical resistance of the negative electrode is high, the deposition of metals that become carrier ions occurs on the surface of the active material, etc. Therefore, it is preferable that the resistance of the electrodes of the storage battery is low.
[0053] In addition, for example, the expansion of the active material during charging may cause the individual components of the electrode to expand during or after charging. In some cases, the elements may not make good contact and the conductive path may be lost. Even after discharging, carriers are inserted, absorbed, or alloyed into the active material during charging. Ions may not be able to be released from the active material and may remain inside the active material. Carrier ions remaining in the battery may cause a decrease in the capacity of the battery, and therefore it is preferable to do not have.
[0054] The remaining carrier ions in the active material can be evaluated, for example, by elemental analysis. For example, elemental analysis can be performed using inductively coupled plasma mass spectrometry (ICP-MS). ively Coupled Plasma Mass Spectrometry) X-ray Photoelectron Spectroscopy (XPS) scopy) etc.
[0055] In order to reduce the resistance of the electrodes of the storage battery, for example, the adhesion between the current collector and the active material layer is increased. It is preferred.
[0056] Alternatively, in order to reduce the resistance of the electrodes of the storage battery, for example, the adhesion between active materials can be increased, It is preferable to increase the contact area between the active material and the conductive assistant.
[0057] In this embodiment, first, a negative electrode of a lithium storage battery and a method for manufacturing the same will be described with reference to FIG. This is explained below.
[0058] <Negative electrode structure 1> Here, FIG. 1A shows a cross-sectional view of a negative electrode 101. In the negative electrode 101, a negative electrode active material layer 107 is formed in contact with the negative electrode current collector 109. A close-up of the enclosed area is shown.
[0059] The negative electrode active material layer 107 is made of a negative electrode active material 121 and a dispersed negative electrode active material 122 that covers the negative electrode active material 121. and a graphene compound 123 formed by the above-mentioned method, and a graphene compound 124 dispersed in contact with the graphene compound. The graphene compound 1 has a binder 122 and voids 124 and 125. It is preferable to use a conductive graphene compound as 23. For example, Graphene oxide may be used. The graphene compound 123 has a sheet shape. In addition, the graphene compound 123 is preferably a compound having a plurality of reduced graphene oxides. The sheets may be partially overlapped.
[0060] As shown in FIG. 1(B), the inside of the negative electrode active material layer 107 is generally uniformly filled with sheet-like grit. The graphene compound 123 is dispersed. Although the thin film is shown in bold, it is actually a thin film having a thickness of a single layer or multiple layers of carbon molecules. The graphene compounds 123 and the binder 122 are arranged in a negative electrode active material 121 and in voids 124, The negative electrode active material 121 is disposed so as to surround, enclose, or cover the void 125 and the surface of the negative electrode active material 121. Therefore, the graphene compound 123 and the negative electrode active material The graphene compounds 121 are in surface contact with each other. The graphene compounds 123 are also in surface contact with each other. By doing so, multiple graphene compounds 123 form a three-dimensional electrically conductive network. For these reasons, it is believed that a conductive graphene compound can be used as a conductive additive. preferable.
[0061] The formation of the graphene compound 123 will be described in detail later. In this embodiment, The graphene compound used is a material obtained by reducing graphene oxide. The reason why a three-dimensional conductive network is formed by 123 is that the graphene compound This is because graphene oxide, which has extremely high dispersibility in polar dispersion media, is used to form 123. The graphene compound 123 remaining in the negative electrode active material layer 107 partially overlaps with one another. Then, the graphene compound 123 is separated from a dispersion containing uniformly dispersed graphene oxide. The dispersion medium is removed by volatilization, and the graphene oxide is reduced to obtain a graphene containing reduced graphene oxide. The graphene compound 123 is a graphene compound that is in surface contact with each other. The dispersion of the graphene oxide forms a path for electrical conduction. For example, it may be carried out by heat treatment or by using a reducing agent.
[0062] The method for producing the negative electrode active material layer will be described later in detail. In addition, when graphene oxide is mixed, the graphene oxide is further subjected to a kneading process. The electrodes are dispersed in the electrode active material layer 107 to form a good three-dimensional electrical conductive network. can be done.
[0063] Therefore, unlike granular conductive additives such as acetylene black, which come into point contact with the active material, Since the phenyl compound 123 enables surface contact with low contact resistance, it is possible to use a small amount of conductive additive. The amount of the graphene compound 123 is increased to improve electrical conductivity between the granular negative electrode active material 121 and the graphene compound 123. Therefore, the ratio of the negative electrode active material 121 in the negative electrode active material layer 107 can be increased. This makes it possible to increase the discharge capacity of the power storage device.
[0064] In addition, graphene compounds bond together to form a mesh-like graphene compound (hereinafter A graphene net or a graphene compound net can be formed. When a substance is covered with a graphene compound net, the graphene compound net connects the particles. Therefore, the amount of binder can be reduced. The ratio of active material to the electrode volume and weight can be adjusted to suit the needs of the application. In other words, the capacity of the power storage device can be increased.
[0065] The binder 122 may be present in a layer form on the surface of the negative electrode active material 121. It is preferable that the binder 123 has a region in contact with the surface of the binder 122. For example, it is located between the negative electrode active material 121 and the graphene compound 123. A binder 122 is provided on the negative electrode active material 121, and a graphene-formed film is formed on the binder 122. A mixture 123 is provided.
[0066] In addition, the structure shown in FIG. 1B does not need to be uniformly formed on the negative electrode active material layer 107. For example, the negative electrode active material layer 107 may have a region in which the above structure is partially formed. That would be good.
[0067] <Negative electrode structure 2> In addition, Figure 2 shows a negative electrode structure that is partially different from the negative electrode structure described above. FIG. 2A shows a cross-sectional view of the negative electrode 101, and FIG. 2B shows the structure of the negative electrode 101 shown in FIG. An enlarged view of the area enclosed by the dashed line is shown.
[0068] The negative electrode active material layer 107 is made of a negative electrode active material 121 and a dispersed negative electrode active material 122 that covers the negative electrode active material 121. and a graphene compound 123 formed by the above-mentioned method, and a graphene compound 124 dispersed in contact with the graphene compound. The graphene compound 123 has a binder 122 and voids 125. For example, reduced graphene oxide may be used. In addition, the graphene compound 123 preferably has a shape of a tube. The graphene oxide may be partially overlapped to form a sheet.
[0069] In FIG. 2B, the negative electrode active material layer 107 is roughly uniformly shattered in the same manner as in FIG. 1B. The graphene compound 123 is dispersed in the form of a binder 1. 22 is disposed so as to encase, surround, or cover the negative electrode active material 121 and the void 125. The graphene is formed so as to be attached to the surface of the negative electrode active material 121. The compound 123 and the negative electrode active material 121 are in surface contact with each other. The graphene compounds 123 also contact each other on their surfaces, forming a three-dimensional electrical field. It forms a conduction network.
[0070] Also, in FIG. 2(C), the area of the void is larger than that of the void 125 shown in FIG. 2(B). 2C shows an enlarged view of the negative electrode active material layer 107. In FIG. The graphene compounds 123 and the binder 122 have a size approximately equal to that of the graphene compounds 123. The negative electrode active material 121 and the voids 125 are wrapped, surrounded, or covered, or the negative electrode It is formed so as to be attached to the surface of the active material 121 .
[0071] In addition, the structure shown in FIG. 2(B) or FIG. 2(C) is formed uniformly in the negative electrode active material layer 107. For example, the above structure may be partially formed in the negative electrode active material layer 107. It is sufficient that the area has a certain area.
[0072] The binder 122 may be present in a layer form on the surface of the negative electrode active material 121. It is preferable that the binder 123 has a region in contact with the surface of the binder 122. For example, it is located between the negative electrode active material 121 and the graphene compound 123. A binder 122 is provided on the negative electrode active material 121, and a graphene-formed film is formed on the binder 122. A mixture 123 is provided.
[0073] A negative electrode whose volume expands due to alloying with carrier ions or absorption of carrier ions The active material expands and contracts during charging and discharging, causing stress between the current collector and the negative electrode active material. This can cause wrinkles in the current collector, which can lead to the negative electrode active material being separated from the current collector. This can cause the negative electrode active material to peel off from the current collector, resulting in poor contact between the negative electrode active material and the current collector, and the conductive path The loss of the conductive path can cause the capacity to decrease with charging and discharging cycles. The amount may decrease.
[0074] However, in one embodiment of the present invention, as shown in FIG. 1 and FIG. 2, the negative electrode active material 121 Even if the volume of the negative electrode repeatedly expands and contracts due to charging and discharging, the void 124 and the negative electrode active material Since the porous layer 107 has voids 125 distributed throughout, the stress caused by the expansion and contraction of the volume is resistant to the As a result, the negative electrode active material is prevented from peeling off from the current collector, and the electrical conductivity is improved. By maintaining the path, it is possible to prevent the capacity from decreasing due to charge / discharge cycles.
[0075] In addition, the volume of the material expands due to alloying with carrier ions or absorption of carrier ions. In the case of negative electrode active materials, cracks occur in the negative electrode active material itself during charging and discharging, making the negative electrode active material layer brittle. This may cause the negative electrode active material layer to collapse. During charging and discharging, some of the negative electrode active material layer may collapse or the negative electrode active material may become pulverized. When the negative electrode is charged, the conductive path between the negative electrode active materials is cut off, and the negative electrode active materials cannot participate in the electrochemical reaction. This causes the capacity to decrease with the charge / discharge cycle. The powdered negative electrode active material peels off from the current collector, and the peeled powder gets stuck in the voids of the separator. This can lead to phenomena such as adhesion to the surface of the electrodes, which can reduce the capacity of the battery. There may be cases where it falls.
[0076] However, in one embodiment of the present invention, as shown in FIG. 1 and FIG. 2, the negative electrode active material layer 10 The graphene compound 123 and the binder 122 dispersed in the negative electrode active material 121 are coated on the negative electrode active material 121. Therefore, the graphene compound 123 and the binder 122 may cause the negative electrode active material layer 107 to collapse or It is possible to prevent the phenomenon in which the finely powdered negative electrode active material 121 adheres to the separator or the positive electrode. Even if the negative electrode active material layer 107 collapses, the finely powdered negative electrode active material 121 will remain in the void. The negative electrode active material 121 can be kept in the gap 125. That is, the volume of the negative electrode active material 121 changes with charging and discharging. Even if the expansion and contraction are repeated, the graphene compound 123 and the binder 122 are bonded to the negative electrode active material 121. can be kept inside the negative electrode active material layer 107, and a conductive path between the negative electrode active materials 121 can be formed can be maintained.
[0077] In addition, the negative electrode active material layer 107 has a porous structure due to the voids 124 and voids 125. As a result, the negative electrode active material layer 107 is formed by the voids 124 and 125. In addition, the space is secured in advance to accommodate the increase in volume due to the expansion of the glass. The phene compound 123 has a structure in which multiple reduced graphene oxides are stacked together. Therefore, the negative electrode active material 121 is flexible due to the voids 124 and 125. Even if the graphene compound 123 expands to a different shape, the graphene compound 123 can be formed according to the shape of the negative electrode active material 121. Therefore, the stress caused by the expansion can be dispersed, and a part of the negative electrode active material layer 107 can be deformed. can be prevented from collapsing.
[0078] <Negative electrode active material> The negative electrode active material 121 is, for example, silicon (Si) or the like, which is alloyed with carrier ions. Materials that can be easily and dealloyed are used. Silicon is about 10 times stronger by weight than graphite. Since it is possible to alloy with the carrier ions of other elements, the theoretical capacity is large and it is possible to increase the size of the power storage device. It is excellent in terms of capacity.
[0079] In addition to Si, the negative electrode active material 121 may be, for example, Mg, Ca, Ga, Al, or G. At least one of the following elements: e, Sn, Pb, Sb, Bi, Ag, Zn, Cd, As, Hg, and In It is preferable that the negative electrode active material 121 has one of Mg2Si, M g2Ge, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2 , Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb3, InSb, SbSn, etc. may be used. The material 121 is titanium dioxide (TiO2), lithium titanium oxide (Li4Ti5O 12 ), lithium-graphite intercalation compound (Li x C6), niobium pentoxide (Nb2O5), titanium oxide oxides such as tungsten (WO2), molybdenum oxide (MoO2), and oxides of lithium and transition metals. Lithium nitride with Li3N type structure 3-x M x N (M = Co, Ni, Cu) It is possible.
[0080] In this embodiment, silicon particles are used as the particulate negative electrode active material 121. The silicon particles are made by crushing silicon wafers, so they are very different from commercially available silicon particles. It can be produced inexpensively. The average particle size of the silicon particles is 0.5 μm to 3 μm. It is preferable that the average particle size is 0.5 μm or more and 1.5 μm or less. Here, the particle size is, for example, calculated by converting the volume of the particle into a sphere and taking the diameter of the sphere as the particle size. Alternatively, for example, the cross section of the particle can be observed, its area converted into a circle, and its diameter calculated as the particle diameter. The average particle size can be calculated by SEM (scanning electron microscope) or TEM. It can be measured by observation or with a particle size distribution analyzer using a laser diffraction / scattering method.
[0081] In addition, the active material is a material that undergoes insertion and desorption of ions, or alloying and dealloying. For example, when making electrodes that are positive or negative, or both, In the active material layer, a mixture of active materials and other materials such as conductive additives, binders, and dispersion media is formed. Therefore, the active material and the active material layer are distinguished. A distinction is made between positive and negative active material layers, and negative and positive active material layers.
[0082] Although not shown, the negative electrode active material 121 has a surface layer formed of The negative electrode active material may have a layer containing a compound having an element common to the main component. The surface layer of the material 121 may contain an oxide of the main component element of the negative electrode active material 121. For example, a nitride of a main component element of the negative electrode active material 121 is formed on the surface layer of the negative electrode active material 121. It may contain sulfides, phosphides, fluorides, and the like.
[0083] For example, the negative electrode active material 121 may contain Si, Mg, Ca, Ga, Al, Ge, Sn, Pb, Sb, Bi, Ag, Zn, Cd, As, Hg and In The negative electrode active material 121 may have at least one element, and the surface layer of the negative electrode active material 121 may have an oxide of the element. For example, the negative electrode active material of one embodiment of the present invention includes a negative electrode active material 121 containing Si as a main component element. For example, the negative electrode active material according to one embodiment of the present invention may have a silicon oxide layer. The material may have Sn as a main component element of the negative electrode active material 121 and have tin oxide in the surface layer. good.
[0084] <Void> The shape of the voids is maintained by the graphene compound 123 and the binder 122. The voids are formed by the difference in volume between before and after the expansion of the negative electrode active material 121 during charging. Also, the voids may be formed so as to cover the negative electrode active material as shown by the voids 124 in FIG. 1(B). Specifically, for example, when silicon is used as the negative electrode active material, The resulting expansion theoretically doubles or even quadruples the volume of silicon before expansion. The volume of the battery expands to more than twice its original volume. In order to relieve the stress caused by the volume expansion of the silicon particles, the volume of the voids is increased to the It is preferable that the volume of the negative electrode be four or more times larger than the volume of the negative electrode. Therefore, if the volume of the voids is too large, the capacity per volume of the negative electrode active material decreases. Therefore, it is more preferable that the volume of the voids is 5 times or less the volume of the silicon particles. In addition, the void 125 in FIG. 1B has a volume smaller than the volume of the silicon particle. As shown in FIG. 2B or FIG. 2C, the periphery of the negative electrode active material 121 may be Here, the volume of the void may be calculated by, for example, calculating the diameter of the void from the void volume. Alternatively, for example, the cross section of the void can be observed and its area converted into a circle, The volume can be calculated from the diameter. The diameter of the voids was measured using a scanning electron microscope (SEM). Alternatively, it can be measured by observation with a TEM.
[0085] Regarding the voids 125 in FIG. 2(B), the diameter of the voids is the average particle diameter of the negative electrode active material 121. It is preferable that the volume of the void is smaller than the diameter. 00 nm or less, and more preferably 200 nm or more and 400 nm or less. In addition, the total volume of the plurality of voids 125 provided around the negative electrode active material 121 is preferably When the negative electrode active material 121 expands during charging, the expansion volume is equal to the difference between the volume before and after the expansion. Specifically, when the negative electrode active material 121 is silicon, the silicon particles are surrounded by The total volume of the plurality of voids 125 is set to be four times or more the volume of the silicon particle. In this way, it is preferable that a plurality of voids 125 are provided around the negative electrode active material 121. This can relieve the stress caused by the expansion of the negative electrode active material 121 during charging.
[0086] Regarding the voids 125 in FIG. 2(C), the diameter of the voids is the average particle diameter of the negative electrode active material 121. Specifically, the diameter of the void is preferably 0.5 μm or more and 3 μm or less. It is preferable that the thickness is 0.5 μm or less and more preferable that the thickness is 0.5 μm or more and 1.5 μm or less. In addition, the total volume of the plurality of voids 125 provided around the negative electrode active material 121 increases with charging. When the negative electrode active material 121 expands, the expansion volume is preferably equal to the difference in volume between before and after the expansion. Specifically, when the negative electrode active material 121 is silicon, the negative electrode active material 121 is provided around the silicon particles. The total volume of the plurality of voids 125 is preferably four times or more the volume of the silicon particle. In this way, by providing a plurality of voids 125 around the negative electrode active material 121, This can relieve the stress caused by the expansion of the negative electrode active material 121 due to the voids. The diameter can be measured by observation with a SEM (scanning electron microscope) or a TEM. do.
[0087] <Binding material> The binders include polyimide, polyvinyl chloride, polytetrafluoroethylene, and polyethylene. ethylene, polypropylene, isobutylene, polyethylene terephthalate, nylon, poly Polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyvinyl chloride ethylene propylene diene polymer, polyvinyl acetate, nitrocellulose, polystyrene Polymethyl acrylate, Polymethyl methacrylate (Polymethyl methacrylate PM MA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide It is preferable to use materials such as poly(ethylene oxide) (PEO) and polypropylene oxide. Adhesives include styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, Rubber, Acrylonitrile-Butadiene Rubber, Butadiene Rubber, Ethylene-Propylene-Diene For example, diene-based rubber materials such as olefin copolymers and fluororubbers can be used.
[0088] In this embodiment, polyimide is used for the binder 122. In particular, polyimide has high heat resistance. Since the negative electrode active material has a high resistance and high strength, it can withstand the expansion and contraction of the negative electrode active material caused by charging and discharging. In the electrode preparation process, the material to be mixed is a polyimide precursor. The precursor is imidized in a subsequent heat treatment to form a polyimide.
[0089] The content of the binder 122 with respect to the total amount of the negative electrode active material layer 107 is 10 wt % or more and 40 wt % or less. wt% or less is preferable, 20wt% to 40wt% is more preferable, and 25wt% or more is more preferable. It is more preferable that the content is 35 wt % or less.
[0090] <Conductive assistant> In this embodiment, a conductive graphene compound is used as a conductive assistant. Examples of the conductive assistant include fibrous carbon materials, metal materials, conductive ceramic materials, etc. The content of the conductive assistant with respect to the total amount of the negative electrode active material layer 107 is 5 wt. % or more and 40 wt % or less is preferable, and 10 wt % or more and 20 wt % or less is more preferable.
[0091] The conductive additive can form an electrically conductive network in the electrode. By this, it is possible to maintain a path of electrical conduction between the active materials. By adding the above, an active material layer having high electrical conductivity can be realized.
[0092] As the conductive assistant, in addition to the graphene compound, for example, carbon fiber can be used. Examples of carbon fibers include mesophase pitch-based carbon fibers and isotropic pitch-based carbon fibers. Carbon fibers such as carbon nanofibers can be used. Carbon nanotubes and the like can be used. Also, vapor grown carbon fibers can be used as carbon fibers. Fiber (VGCF (registered trademark): Vapor-Grown Carbon Fiber) Also, for example, metal powders such as copper, nickel, aluminum, silver, and gold can be used. Powder, metal fibers, conductive ceramic materials, etc. can be used.
[0093] Graphene and graphene compounds are explained below. Graphene is a carbon Atoms are arranged in one atomic layer, with π bonds between the carbon atoms.
[0094] Compounds that have graphene as the basic skeleton are called "graphene compounds" ("graphene compacts"). The compound is called "Graphene Compound".
[0095] The graphene compound will be described in detail below.
[0096] Among graphene compounds, those with 2 to 100 layers of graphene are called multi-layered. Graphene and multi-graphene are, for example, The length is 50 nm or more and 100 μm or less, or 800 nm or more and 50 μm or less.
[0097] For example, a graphene compound may include a graphene or multi-graphene having an atom other than carbon, Alternatively, the compound may be a compound in which an atomic group having an atom other than carbon is modified. Compounds in which an atomic group mainly consisting of carbon, such as an alkyl group, is modified on graphene or multi-graphene. The atomic group may be called a substituent, a functional group, a characteristic group, or the like. Here, the graphene compound also includes graphene modified with the above-mentioned atoms or atomic groups. .
[0098] Here, even if the front and back surfaces of the graphene compound are modified with different atoms or atomic groups, In addition, when the graphene compound has multi-layer graphene, each layer may have different Atoms or atomic groups may be modified.
[0099] As an example of graphene modified with the above-mentioned atomic groups, oxygen-modified graphene or Multi-graphene may also be used. For example, graphene modified with a functional group containing oxygen may also be used. Alternatively, graphene or multi-graphene may be used. Here, the oxygen-containing functional group may be, for example, ethylene. Examples of the oxygen-modified groups include carbonyl groups such as epoxy groups and carboxyl groups, and hydroxyl groups. Decorated graphene is sometimes called graphene oxide.
[0100] An example of a method for producing graphene oxide will be described. Graphene oxide can be obtained by oxidizing multi-graphene. Graphite oxide can be obtained by oxidizing graphite. Here, the graphene oxide can be further modified with the above-mentioned atoms or atomic groups. Good too.
[0101] In addition, highly conductive graphene compounds can be obtained by reducing graphene oxide. In addition, the graphene compound obtained by reducing graphene oxide is When called "RGO (Reduced Graphene Oxide)" In addition, reduced graphene oxide or RGO has the following properties: Not all oxygen is eliminated, and some oxygen or atomic groups containing oxygen remain bonded. For example, RGO may have carbonyl groups such as epoxy groups, carboxyl groups, or It may have a functional group such as a hydroxyl group.
[0102] Graphene compounds are composed of multiple graphene compounds that overlap partially to form a single sheet. Such a graphene compound may be called a graphene compound sheet. The graphene compound sheet may have a thickness of, for example, 0.33 nm or more and 50 μm or less. More preferably, the graphene compound has a region larger than 0.34 nm and smaller than 10 μm. The group may contain an atom other than carbon, an atomic group having an atom other than carbon, or carbon such as an alkyl group. The main atomic group or the like may be modified. In addition, the multiple layers of the graphene compound sheet may be In each of the formulas, different atoms or groups of atoms may be modified.
[0103] Graphene compounds are composed of not only six-membered rings made of carbon, but also five-membered rings made of carbon and In this case, the vicinity of the poly-membered ring other than the six-membered ring may be In this case, there may be an area through which lithium ions can pass.
[0104] For example, a plurality of graphene compounds may be gathered together to form a sheet shape. .
[0105] The graphene compound has a planar shape, which allows for surface contact.
[0106] Highly conductive graphene compounds, such as graphene or multi-graphene, are thin but It has high electrical conductivity and provides surface contact between graphene and between graphene and active material. The contact area can be increased. Therefore, even if the amount per volume is small, the electrical conductivity is high. A path can be formed.
[0107] Some graphene compounds can be used as insulators. For example, The graphene oxide sheet can be used as a sheet-shaped insulator. In some cases, graphene has higher insulating properties than graphene. The insulating properties of a compound may be improved depending on the type of modifying atomic group.
[0108] The graphene compound according to one embodiment of the present invention may have a graphene precursor. The graphene precursor may include, for example, the above-mentioned graphene oxide or graphite oxide. good.
[0109] In addition, graphene containing alkali metals and graphene containing elements other than carbon, such as oxygen, The graphene compound according to one embodiment of the present invention includes a graphene analogue. Also includes laphene analogues.
[0110] In addition, the graphene compound according to one embodiment of the present invention has atoms, atomic groups, and their interlayer structures. For example, a lithium compound or a lithium ion may be inserted between the graphene layers. In addition, the graphene compound may have atoms, atomic groups, and ions thereof between the layers. The physical properties of graphene, such as electrical conductivity and ionic conductivity, may change when the In addition, the interlayer distance may be larger than that of, for example, multi-graphene.
[0111] Graphene compounds also have excellent electrical properties, such as high electrical conductivity, and are highly flexible and In addition, the glass may have excellent physical properties such as high mechanical strength. The phenanthroline compound has a planar shape, which allows for surface contact with low contact resistance. Even though they are thin, they can be very conductive, and even a small amount can be used to efficiently form a conductive path within the active material layer. Therefore, a conductive graphene compound is used as a conductive assistant. This is preferable because it is possible to increase the contact area between the active material and the conductive assistant. In addition, it is preferable because the electrical resistance can be reduced in some cases. It is particularly preferable to use reduced graphene oxide as the graphene compound.
[0112] In addition, when using an active material with a small particle size, for example an active material with an average particle size of 1 μm or less, In this case, the specific surface area of the active material is large, and more conductive paths are required to connect the active materials together. In such cases, graphene compounds that can efficiently form conductive paths even in small amounts are used. It is particularly preferred to use
[0113] In addition, when the graphene compound is reduced graphene oxide, adjacent reduced graphene oxides The interlayer distance with graphene is preferably 0.335 nm or more and 0.7 nm or less.
[0114] The interlayer distance of reduced graphene oxide can be measured by, for example, observing the cross section of reduced graphene oxide through a transmission microscope. It can be evaluated by observing it with a transmission electron microscope (TEM). The interlayer distance of graphene oxide is calculated as the interplanar distance using, for example, X-ray diffraction (XRD). It is possible.
[0115] The graphene compound according to one embodiment of the present invention uses reduced graphene oxide. For the entire graphene oxide, the oxygen concentration measured by XPS (X-ray photoelectron spectroscopy) is For example, preferably 0.3 atomic % or more and 20 atomic % or less, more preferably 1a % or more and 11 atomic % or less, and more preferably 3 atomic % or more and 10 atomic % or less. It is less than atomic percent.
[0116] In addition, when graphene compounds were measured by XPS, the binding energy corresponding to the C1s of carbon was By analyzing the energy spectrum through waveform separation, And sp 2 The proportion of the peaks that indicate this can be estimated as an area ratio. The graphene compound according to one embodiment of the present invention is sp 2 The percentage of C1s in the entire spectrum It is preferable that the ratio is 50% or more and 90% or less. 2 By increasing the proportion of For example, the electrical conductivity of the graphene compound can be increased.
[0117] Note that the physical properties such as the interplanar spacing and oxygen concentration shown above are merely examples. The graphene compound is not limited thereto.
[0118] <Negative electrode current collector> The negative electrode current collector 109 may be made of a metal such as copper, stainless steel, gold, platinum, aluminum, or titanium. The negative electrode current collector 109 may be made of a material having high electrical conductivity, such as a material selected from the group consisting of tungsten, arsenic, tantalum, tungsten, tantalum, fluorine, arsenic ... The current collector material used in the present invention is preferably a material that does not form an alloy with carrier ions such as lithium. In addition, the heat resistance of silicon, titanium, neodymium, scandium, molybdenum, etc. has been improved. Aluminum alloys containing elements that react with silicon can be used. Alternatively, the insulating layer may be formed of a metal element that reacts with silicon to form a silicide. The metal elements that form the alloy include zirconium, titanium, hafnium, vanadium, niobium, Tantalum, chromium, molybdenum, tungsten, cobalt, nickel, etc. Negative electrode current collector The body 109 may be in the form of a foil, a plate (sheet), a net, a punched metal, an expanded metal, or the like. The negative electrode current collector 109 may have a thickness of 5 μm to 30 μm. The following may be used:
[0119] Furthermore, a carbon material may be used as the negative electrode current collector.
[0120] <Method 1 for making negative electrode> A method for manufacturing a negative electrode according to one embodiment of the present invention will be described below with reference to FIGS.
[0121] FIG. 3 is a flow diagram of a method for producing the negative electrode shown in FIG.
[0122] <Step S101> In step S101, a silicon wafer is crushed to obtain silicon particles that will become a negative electrode active material. Prepare the following:
[0123] For example, cut an 8-inch round silicon wafer into pieces with a glass cutter or other cutter. After cutting into pieces between 0.5cm and 1.5cm, grind them further in a mortar or pestle until they are 1mm in diameter or less. The silicon powder is obtained by further crushing the silicon dioxide particles into a ball mill. The silicon powder is further pulverized. Specifically, for example, the silicon powder, the dispersion medium, the metal The mixture is placed in a container along with metal or ceramic balls and the container is rotated. The grinding process is carried out at a speed of 200 rpm to 500 rpm for 3 hours to 6 hours. It is preferable to perform ball milling to finely pulverize silicon powder. This makes it possible to microparticulate the electrode material after fabrication. In addition, a material in which the raw material is not dissolved can be used as the dispersion medium. In addition, after the ball milling process, small silicon particles can be separated using a sieve. Here, it is preferable to use a sieve having a hole diameter of 10 μm or more and 100 μm or less. In this way, silicon particles having an average particle size of 0.5 μm or more and 5 μm or less can be obtained. Cut.
[0124] Generally, commercially available silica with small particle size (for example, average particle size of 100 nm or less) Silicon particles are expensive. On the other hand, in one embodiment of the present invention, silicon wafers are crushed to produce silicon. By using silicon wafers, silicon particles can be produced very cheaply. In addition, it is preferable that the silicon particles serving as the negative electrode active material have a low resistance value. In the present invention, a low resistance semiconductor containing impurities (e.g., boron, phosphorus, antimony, etc.) is used. A silicon wafer with low resistivity can be used, and silicon particles with low resistivity are used as the negative electrode active material. However, in one embodiment of the present invention, the silicon particles may be formed by forming a silicon wafer. It is not limited to silicon particles produced by pulverization.
[0125] <Step S102> The silicon particles obtained by the crushing process in step S101 are heat-treated to form silicon particles. A silicon oxide film is formed on the surface.
[0126] For example, the silicon particles produced in step S101 are heated to 700° C. or higher in an air atmosphere. It is preferable to carry out the heat treatment at 1000° C. or less for 0.5 to 5 hours. According to this theory, the surface of silicon particles is covered with a silicon oxide film with a thickness of 100 nm to 900 nm. It is preferable that a film having a thickness of 150 nm or more and 450 nm or less is formed. It is also preferable that the radius of the silicon particles is smaller than the thickness of the silicon oxide film. In some cases, the silicon atoms formed in this step are completely oxidized to silicon oxide. The silicon oxide film is removed by etching in a step described later, leaving voids. The volume of this void is equal to or greater than the volume of the negative electrode active material when the volume expands during charging. This allows the silicon particles to expand in volume during charging. Stress can be relieved.
[0127] <Step S103> Next, the graphene oxide, the binder, and the silicon particles obtained in S102 are mixed. Prepare mixture A.
[0128] For example, the silicon particles obtained in step S102 may be mixed with a graphene compound, a binder, or a separator. Add the mixture containing the dispersion medium, knead it (knead it at high viscosity) and then ventilate it. The dispersion medium is evaporated and removed using a dryer. By performing a kneading process, silicon particles and graphite particles are The graphene compound and the binder can be uniformly mixed. It is preferable to use graphene oxide as the material.
[0129] In this embodiment, graphene oxide is used as a conductive additive, and a precursor of polyimide is used as a binder. , and N-methylpyrrolidone (NM By this kneading process, the graphene oxide is uniformly dispersed and a single layer or two layers are formed. Graphene oxide with 100 or more layers is attached to the surface of silicon particles. By removing the graphene oxide, the graphene oxide and the binder are fixed to the surface of the silicon particles. The content of silicon particles in the total amount of mixture A is preferably 40 wt% or more and 80 wt% or less. The content of the mixture A in the total amount of the mixture B is preferably 50 wt% or more and 70 wt% or less. The content of the conductive additive is preferably 10wt% or more and 30wt% or less, and more preferably 15wt% or more and 25wt% or less. The content of the binder in the total amount of mixture A is preferably 10 wt% or less. The content is preferably from 15 wt % to 30 wt %, and more preferably from 15 wt % to 25 wt %.
[0130] As the dispersion medium, a material in which the raw material is not dissolved can be used. The dispersion medium is water, methanol, ethanol, acetone, tetrahydrofuran (THF), Dimethylformamide (DMF), N-methylpyrrolidone (NMP) and dimethylsulfonate A mixture of two or more of these, including dimethyl sulfoxide (DMSO), can be used.
[0131] The polyimide precursor is imidized in a subsequent heat treatment to become polyimide.
[0132] Here, a method for manufacturing graphene oxide will be described. Graphene oxide is used as the compound. Graphene oxide is, for example, single crystal graphite. The powder is oxidized by adding a solution of potassium permanganate in sulfuric acid, hydrogen peroxide, etc. The graphite oxide can be prepared by using a method for preparing a dispersion liquid containing graphite. Phito is formed by oxidation of carbon in graphite into epoxy groups, carbonyl groups, and carboxyl groups. It has functional groups such as aryl groups and hydroxyl groups.
[0133] In addition, since the graphite oxide has the above-mentioned functional groups, multiple graphene layers can be formed. The distance between the electrodes is longer than that of graphite.
[0134] Next, ultrasonic vibration was applied to the dispersion liquid containing graphite oxide to form graphite particles with a long interlayer distance. Graphite oxide is cleaved to separate graphene oxide, and the graphene oxide-containing particles are A dispersion liquid can be prepared. Then, the dispersion medium is removed from the dispersion liquid containing graphene oxide. By this, graphene oxide can be obtained.
[0135] In a polar solution, graphene oxide is negatively charged due to its functional groups. Therefore, different graphene oxides are less likely to aggregate with each other. This makes it easier for graphene oxide to be dispersed uniformly.
[0136] The length of one side of the graphene oxide used (also called the flake size) is 1 μm or more. It is preferable that the thickness is 0 μm or less.
[0137] <Step S104> The silicon particles included in the mixture A prepared in step S103 are The silicon oxide film is removed by etching to prepare mixture B. The substrate is washed, dried, and then heated.
[0138] The area of the silicon oxide film removed by the etching process becomes a gap 124. For example, the volume of the void 124 is the same as that of the silicon particle when the volume expands due to charging. It is sufficient that the volume is equal to or larger than that of the particle diameter of 1.0 μm. When the silicon particle is charged and its volume is increased by four times, the diameter of the void 124 is 1.6 μm or less. The diameter of the silicon particles is preferably 100 nm or less. is also removed by etching to form a gap 125. Although there is no particular limitation, for example, a fluorine-based aqueous solution can be used. Specifically, for example, ammonium hydrogen fluoride is added to the mixture A prepared in step S103. A mixture containing 7.13% ammonium fluoride (NH4HF2) and 15.4% ammonium fluoride (NH4F) The etching can be performed by dripping a mixture solution (manufactured by Stella Chemifa, product name LAL500) on the surface. The etching time is preferably 1 minute or more and 10 minutes or less. By controlling the etching treatment time, the silicon oxide film on the surface of the silicon particles can be completely removed. It is also possible to leave the silicon oxide film without removing the silicon oxide film.
[0139] In addition, after the etching process, the substrate was washed with pure water several times for cleaning and drying. After that, it is preferable to perform vacuum drying. The processing temperature in the vacuum drying is 100°C or more for 1 The temperature is preferably 50° C. or lower and the treatment time is preferably 10 hours or longer.
[0140] It is preferable to use a vacuum furnace for the heat treatment. The temperature is preferably 300° C. or higher and 500° C. or lower, and more preferably 350° C. or higher and 450° C. or lower. The heating time is preferably from 30 minutes to 2 hours. The polyimide precursor is imidized to form polyimide. The treatment reduces the graphene compound contained in the mixture B. In this embodiment, In step S103, graphene oxide is used as the graphene compound to be mixed. The heat treatment reduces the graphene oxide to form reduced graphene oxide. This can increase the electrical conductivity of the graphene compound.
[0141] <Step S105> The mixture B obtained in step S104 is used to prepare a slurry.
[0142] Mixture B with a binder and a dispersion medium to form a slurry. The dispersion medium is added and mixed by stirring in a stirrer. The processing time should be between 3 and 10 minutes and the speed should be between 000 rpm and 3000 rpm. It is more preferable to carry out a kneading treatment after the stirring treatment.
[0143] The content of mixture B in the total amount of the slurry is preferably 70 wt% or more and 95 wt% or less. The content of the slurries in the total amount of the slurry is preferably 80 wt % or more and more preferably 90 wt % or less. The content of the binder is preferably 5 wt% or more and 30 wt% or less, and more preferably 10 wt% or more and 20 wt% or less. The following is more preferred:
[0144] In addition, the above-mentioned binders can be used as the binder, but the binder used in step S103 can be used as the binder. It is preferable to use the same binder as the adhesive. In this embodiment, polyimide is used as the binder. A precursor of the tetrahydrofuran is used.
[0145] In addition, the dispersion medium may be the same as that described in step S103. It is preferable to use the same dispersion medium as that used in S103. As a solvent, N-methylpyrrolidone (NMP) ) is used.
[0146] <Step S106> The slurry prepared in step S105 is applied onto the negative electrode current collector 109. Apply the coating.
[0147] First, the slurry is applied onto the negative electrode current collector 109. Here, before applying the slurry, In addition, a surface treatment may be performed on the negative electrode current collector 109. For example, the surface treatment may be a corona discharge treatment. Examples of the treatment include a coating process, a plasma treatment, and an undercoat treatment. Before applying the slurry onto the current collector, the active material layer is coated with a fluorine-containing layer to reduce the interface resistance between the active material layer and the current collector. This refers to a film formed on the current collector to improve the adhesion between the active material layer and the current collector. The coating does not necessarily have to be in the form of a film, but may be formed in the form of islands. The undercoat may be an active material and may exert a capacitance. Carbon materials can be used. Examples of carbon materials include graphite and acetylene black. , carbon black such as Ketjen Black (registered trademark), carbon nanotubes, etc. It can be used.
[0148] The slurry can be applied by the slot die method, gravure method, blade method, or a combination of these methods. A continuous coater or the like may be used for coating.
[0149] Next, the dispersion medium contained in the slurry is volatilized. The reaction is preferably carried out at a temperature in the range of 50° C. to 200° C., preferably 60° C. to 150° C. stomach.
[0150] For example, heat the battery on a hot plate in an air atmosphere at 30°C to 70°C for 10 minutes or more. After the heat treatment, for example, the temperature is increased to 100°C and the temperature is increased to 1 hour or more and 10 hours or less. In this case, the heat treatment may be carried out in a reduced pressure environment.
[0151] Alternatively, the heat treatment may be performed using a drying oven or the like. When a drying oven is used, for example, Heat treatment may be performed at a temperature of 30° C. or higher and 120° C. or lower for 30 seconds or longer and 20 minutes or shorter.
[0152] Alternatively, the temperature may be increased stepwise. For example, heat treatment at 60°C or less for 10 minutes or less may be performed. After that, a further heat treatment may be carried out at a temperature of 65° C. or higher for 1 minute or more.
[0153] The thickness of the active material layer thus formed is preferably, for example, 5 μm to 300 μm. The thickness may be equal to or less than 10 μm, and more preferably equal to or more than 150 μm.
[0154] When the dispersion medium is evaporated from the slurry, the active material, the conductive additive, and the binder move. For example, the concentration of the binder in the active material layer may decrease. The higher the viscosity of the slurry, the greater the dispersion medium. In some cases, the change in dispersibility after the evaporation of the dispersion medium is small, which is preferable. The slower the speed, the smaller the change in dispersibility will be, and this may be preferable.
[0155] The slurry may be applied to both sides of the negative electrode current collector 109 or only one side of the negative electrode current collector 109 . Alternatively, the substrate may have regions where the slurry is partially applied on both sides.
[0156] <Step S107> Next, the negative electrode current collector 109 coated with the slurry is subjected to a heat treatment.
[0157] The heat treatment is preferably performed using a vacuum furnace. The temperature is preferably 0°C or higher and 500°C or lower, and more preferably 350°C or higher and 450°C or lower. The time is preferably from 30 minutes to 2 hours. The polyimide precursor is imidized to form a polyimide. As a result, the graphene compound is further thermally reduced. Form.
[0158] In this embodiment, the heat treatment in steps S104 and S107 The thermal reduction of the graphene compound progresses, and the electrical conductivity of the graphene compound can be increased. In this embodiment, graphene oxide is added to the graphene compound to be mixed in step S103. Since graphene oxide is used, the heat treatment reduces the graphene oxide. The conductivity of the fen can be increased.
[0159] In this embodiment, the heating process for firing the slurry and reducing the graphene oxide is performed as follows: A temperature at which the binder is not decomposed, for example, a temperature of 300°C or higher and 500°C or lower, preferably 350°C or lower The heating temperature is from 0° C. to 450° C. This makes it possible to prevent the binder from being decomposed. Furthermore, by heating at a temperature at which the binder is not decomposed, damage to the negative electrode can be suppressed. Since the battery is not destroyed, it is possible to prevent the reliability of the lithium-ion battery from being reduced. be.
[0160] As described above, in this embodiment, the graphene compound to be added is graphene oxide. Graphene oxide is formed by oxidizing graphite. The functional groups formed by the oxidation contribute to the dispersibility of graphene oxide, making it highly dispersible. However, in the process of reducing graphene oxide, the functional group that contributes to the dispersibility is The dispersibility of reduced graphene oxide is low because the groups are reduced and reduced.
[0161] An electrode (negative electrode) formed by mixing graphene oxide and an active material and then heating the mixture. In the case of the graphene oxide, the functional groups are dispersed before being reduced and decreased, so the reduction The graphene oxide is uniformly dispersed. The lithium ion battery used has good electrical characteristics.
[0162] <Step S108> The negative electrode active material layer 107 formed on the negative electrode current collector 109 by the above-described manufacturing process is The negative electrode 101 is formed.
[0163] Another method for manufacturing a negative electrode according to one embodiment of the present invention will be described below with reference to FIGS.
[0164] <Method 2 for producing negative electrode> FIG. 4 is a flow diagram of a method for producing the negative electrode shown in FIG.
[0165] <Step S201> The silicon wafer is crushed to produce silicon particles that will become the negative electrode active material. Step S201 is similar to the process described in step S101.
[0166] <Step S202> Next, silicon particles, silicon oxide particles, graphene compounds, and The mixture A is prepared by mixing the powder and the binder.
[0167] For example, silicon particles are mixed with silicon oxide particles, graphene compounds, binders, and dispersion media. The mixture is then mixed and kneaded (mixed at high viscosity) and then placed in a forced air dryer. The dispersion medium is removed by volatilization. The silicon particles and silicon oxide are removed by the kneading process. The particles, the graphene compound, and the binder can be uniformly mixed. As the compound, it is preferable to use graphene oxide.
[0168] In the negative electrode active material layer 107 shown in FIG. 2(B), the silicon oxide particles have an average The particle size is preferably 100 nm or more and 500 nm or less, and more preferably 200 nm or more and 300 nm or less. m or less. In particular, the silicon oxide particles preferably have an average particle size of 0.5 μm or more and 3.0 μm or less. The silicon oxide particles are preferably 0.5 μm or more and 1.5 μm or less. The method for producing the above-mentioned is not particularly limited, but may be, for example, a method using silicon tetrachloride, oxygen, and The high-temperature hydrolysis method produces silicon oxide by simultaneously reacting hydrogen with silicon and metals. The raw material is vaporized by thermal energy and oxidized in an oxygen atmosphere to produce oxide particles. Physical Vapor Synthesis Method to Generate The method is not particularly limited and may be made by using a method such as silicon oxide. The particles used may be commercially available.
[0169] The binder and the dispersion medium are the same as those described in step S103. As for the mixing method, the same as described in step S103 can be used. The process is similar.
[0170] <Step S203> The silicon oxide particles contained in the mixture A prepared in step S202 are etched. Mixture B is then washed and dried, and heated. Perform processing.
[0171] The etching process removes the silicon oxide particles, forming voids 125. The etching process is the same as that described in step S104. It is a process.
[0172] <Step S204> The mixture B obtained in step S203 is used to prepare a slurry. The process is similar to that described in step S105.
[0173] <Step S205> The slurry prepared in step S204 is applied onto the negative electrode current collector 109. The slurry coating process is the same as that described in step S106. be.
[0174] <Step S206> Next, the negative electrode current collector 109 coated with the slurry is subjected to a heat treatment. This is the same as the process described in step S107.
[0175] <Step S207> The negative electrode active material layer 107 formed on the negative electrode current collector 109 by the above-described manufacturing process is The negative electrode 101 is formed.
[0176] Note that one embodiment of the present invention has been described in this embodiment. In the following, one embodiment of the present invention will be described. However, the embodiment of the present invention is not limited to these. That is, various inventive aspects are described in this and other embodiments. Therefore, one embodiment of the present invention is not limited to a specific embodiment. For example, one embodiment of the present invention As an example of the application of the present invention to a lithium ion battery, In some cases, or depending on the situation, one aspect of the present invention is to Batteries, lead-acid batteries, lithium-ion polymer batteries, nickel-metal hydride batteries, nickel-ca Domium batteries, nickel-iron batteries, nickel-zinc batteries, silver oxide-zinc batteries, solid A solid-state battery, an air battery, a zinc-air battery, a lithium-air battery, a primary battery, a capacitor, or Electric double layer capacitor, ultracapacitor, supercapacitor, lithium ion For example, in some cases or depending on the situation, Therefore, one embodiment of the present invention does not necessarily need to be applied to a lithium-ion battery. In one embodiment, the graphene, the graphene compound, or the graphene oxide is included. However, one embodiment of the present invention is not limited to this. Depending on the circumstances, an embodiment of the present invention may have various materials. Depending on the circumstances, one aspect of the present invention is to provide a graphene, a graphene compound, Alternatively, graphene oxide or the like may not be included.
[0177] (Embodiment 2) In this embodiment, an example of a power storage device using an electrode which is one embodiment of the present invention will be described.
[0178] In this specification and the like, the term "electricity storage device" refers to elements and devices in general that have an electricity storage function. For example, lithium-ion batteries, lithium-ion capacitors, and electric double-layer capacitors Includes Pacita etc.
[0179] <Thin storage battery> FIG. 5 shows a thin storage battery as an example of a power storage device. Here is an example. If a thin storage battery is made flexible, it can be made with fewer flexible parts. If the battery is mounted on an electronic device that has at least some of the battery, the battery can be bent according to the deformation of the electronic device. It is also possible.
[0180] FIG. 5 shows an external view of a thin storage battery 500. Also, FIG. 6(A) and FIG. 6(B) show 5 shows the A1-A2 cross section and the B1-B2 cross section indicated by the dashed line. 503 having a positive electrode current collector 501 and a positive electrode active material layer 502; and and a negative electrode 506 having a negative electrode active material layer 505, a separator 507, and an electrolyte solution 508. The battery has a positive electrode 503 and a negative electrode 506 provided in the exterior body 509. A separator 507 is placed between the electrodes. The inside of the exterior body 509 is filled with an electrolyte 508. It has been done.
[0181] The negative electrode 506 may be formed using the negative electrode 101 described in Embodiment 1 as appropriate.
[0182] The positive electrode current collector 501 and the positive electrode active material layer 502 in the positive electrode 503 are as follows: The positive electrode current collector and the positive electrode active material layer shown below can be used appropriately.
[0183] <Positive electrode current collector> The positive electrode current collector 501 is made of a metal such as stainless steel, gold, platinum, aluminum, or titanium, Materials such as these alloys that are highly conductive and do not dissolve at the potential of the positive electrode can be used. In addition, the heat resistance of silicon, titanium, neodymium, scandium, molybdenum, etc. has been improved. Aluminum alloys containing elements that react with silicon can be used. It may be formed of a metal element that forms a silicide. It reacts with silicon to form a silicide. The metal elements that are used are zirconium, titanium, hafnium, vanadium, niobium, and titanium. talc, chromium, molybdenum, tungsten, cobalt, nickel, etc. Positive electrode current collector 5 01: foil, plate (sheet), net, punched metal, expanded metal, etc. The positive electrode current collector 501 has a thickness of 5 μm or more and 30 μm or less. It is also preferable to use a material such as graphite on the surface of the positive electrode current collector 501. An undercoat layer may be provided.
[0184] <Cathode active material layer> The positive electrode active material layer 502 contains, in addition to the positive electrode active material, a binder ( The positive electrode active material layer 502 may contain a binder, a conductive assistant for increasing the conductivity of the positive electrode active material layer 502, and the like.
[0185] The positive electrode active material used for the positive electrode active material layer 502 may have an olivine type crystal structure, a layered rock salt type The positive electrode active material is a composite oxide having a crystalline structure of 0.1 to 1.0 μm or a spinel type crystalline structure. For example, LiFeO2, LiCoO2, LiNiO2, LiMn2O4, V2O5, Compounds such as Cr2O5 and MnO2 are used.
[0186] In particular, LiCoO2 has a large capacity and is more stable in air than LiNiO2. It is preferable because it has the advantages of being thermally stable compared to LiNiO2.
[0187] In addition, lithium-containing materials with a spinel-type crystal structure containing manganese, such as LiMn2O4, A small amount of lithium nickel oxide (LiNiO2 or LiNi 1-x MO2(0 <x<1) (M=Co, Al, etc.) can improve the characteristics of the storage device using this material. This is preferable.
[0188] In addition, the positive electrode active material is Li a Mn b M c O d Lithium ion can be expressed as In this case, the element M is any element other than lithium or manganese. It is preferable to use a metal element selected from the group consisting of silicon and phosphorus, and nickel is preferably used. It is more preferable to measure the entire particle of the lithium manganese composite oxide. When the voltage is applied <a / (b+c)<2、かつc>, the value is 0.0 and 0.26≦(b+c) / d<0.5. It is preferable that the metal and silicon content of the entire lithium manganese composite oxide particle is The composition of phosphorus, etc. is measured, for example, using an ICP-MS (inductively coupled plasma mass spectrometer). The oxygen composition of the entire lithium manganese oxide particle can be, for example, E It can be measured using DX (energy dispersive X-ray analysis). -Used in conjunction with MS analysis, fusion gas analysis and XAFS (X-ray absorption fine structure) analysis to evaluate the charge The lithium manganese composite oxide can be determined by using at least It refers to an oxide containing lithium and manganese, and also contains chromium, cobalt, aluminum, nickel , iron, magnesium, molybdenum, zinc, indium, gallium, copper, titanium, niobium, It may contain at least one element selected from the group consisting of silicon, phosphorus, etc. good.
[0189] In order to realize high capacity, the crystal structure, crystal orientation, or oxygen It is preferable to use a lithium manganese composite oxide having regions with different contents. In order to obtain such a lithium manganese composite oxide, the composition formula is Lia Mn b Ni c O d (1. 6≦a≦1.848, 0.19≦c / b≦0.935, 2.5≦d≦3) Further, Li 1.68 Mn 0.8062 Ni 0.318 The formula for O3 is It is particularly preferable to use a lithium manganese composite oxide having a high molecular weight. Li 1.68 Mn 0.8062 Ni 0.318 Lithium with the formula O3 Manganese composite oxide is a material whose molar ratio is Li2CO3:MnCO3:N Lithium manganese formed by adjusting iO=0.84:0.8062:0.318 Therefore, the lithium manganese composite oxide has the composition formula Li 1.68 Mn 0.8062 Ni 0.318 It is represented by O3, but the composition can deviate from this.
[0190] Here, the lithium manganese has regions with different crystal structures, crystal orientations, or oxygen contents. An example of a cross-sectional view of a composite oxide particle is shown in FIG.
[0191] As shown in FIG. 7(A), the crystal structure, crystal orientation, or oxygen content of the region may be different. The lithium manganese composite oxide has a first region 331, a second region 332, and a third region. The second region 332 is preferably at least an area outside the first region 331. The outer side of the particle is closer to the surface of the particle. The region 333 corresponds to the surface of the particle having the lithium manganese composite oxide. It is preferable that
[0192] Also, as shown in FIG. 7B, the first region 331 is not covered by the second region 332. The second region 332 may have an area that is not covered by the third region 333. For example, the first region 331 may have a region where the third region 333 is in contact with the first region 331. In addition, the first region 331 may be either the second region 332 or the third region 333. It may have areas that are not covered by the
[0193] The second region 332 preferably has a different composition than the first region 331 .
[0194] For example, the compositions of the first region 331 and the second region 332 are measured separately, and the composition of the first region 33 The first region 331 has lithium, manganese, the element M and oxygen, and the second region 332 has lithium, manganese, the element M and oxygen. The first region 331 has lithium, manganese, the element M, and oxygen. The atomic ratio of lithium, ma, and oxygen in the second region 332 is represented by a1:b1:c1:d1. The atomic ratio of the elements N, M, and oxygen is expressed as a2:b2:c2:d2. The composition of each of the first region 331 and the second region 332 is, for example, T Measurements are made using EDX (energy dispersive X-ray analysis) with an EM (transmission electron microscope). It is sometimes difficult to measure the lithium composition using EDX. Therefore, in the following, the difference in composition between the first region 331 and the second region 332 is the amount of elements other than lithium. Here, d1 / (b1+c1) is preferably 2.2 or more, and 2.3 or less. More preferably, the ratio is 2.35 or more and even more preferably 2.35 or more and 3 or less. d2 / (b2+c2) is preferably less than 2.2, and more preferably less than 2.1. It is preferable that the ratio is 1.1 or more and 1.9 or less. The composition of the entire lithium manganese composite oxide particle including the first region 331 and the second region 332 is It is preferable that the above-mentioned condition 0.26≦(b+c) / d<0.5 is satisfied.
[0195] The manganese contained in the second region 332 is different from the manganese contained in the first region 331. The element M in the second region 332 may have a valence of 1 to 100 . may have a different valence from that of the element M.
[0196] More specifically, the first region 331 is made of lithium manganese having a layered rock-salt type crystal structure. The second region 332 is preferably a silicon composite oxide having a spinel type crystal structure. It is preferable that the lithium manganese composite oxide has the above structure.
[0197] Here, when there is a spatial distribution in the composition of each region or the valence of an element, for example, The composition and valence of each area are evaluated, and the average value is calculated. good.
[0198] There may also be a transition layer between the second region 332 and the first region 331. A transition layer is, for example, a region where the composition changes continuously or stepwise. A layer is a region where the crystal structure changes continuously or stepwise. , the region in which the lattice constant of the crystal changes continuously or stepwise. A mixed layer may be provided between the first region 332 and the second region 331. Here, the mixed layer may be, for example, This refers to a mixture of two or more crystals with different crystal orientations. Alternatively, a mixed layer is, for example, For example, it refers to a mixture of two or more crystals with different crystal structures. For example, this refers to a mixture of two or more crystals with different compositions.
[0199] The third region 333 can be made of carbon or a metal compound. Examples of such metals include cobalt, aluminum, nickel, iron, manganese, titanium, zinc, and lithium. Examples of metal compounds include oxides and fluorides of these metals. Some examples include:
[0200] Of the above, it is particularly preferable that the third region 333 contains carbon. Carbon is conductive. Therefore, by using carbon-coated particles in the electrodes of a power storage device, In addition, since the third region 333 contains carbon, the third region The second region 332 adjacent to the third region 333 can be oxidized. The graphene compound may have a conductive property (described later). The compound has excellent physical properties such as high flexibility and mechanical strength as well as excellent electrical properties. In addition, the lithium manganese composite oxide particles can be efficiently coated.
[0201] The third region 333 contains carbon, such as a graphene compound, having electrical conductivity. This improves the cycle characteristics of the energy storage device that uses lithium manganese composite oxide as the positive electrode material. It can be done.
[0202] The thickness of the carbon-containing layer is preferably 0.4 nm or more and 40 nm or less.
[0203] In addition, the lithium manganese composite oxide has, for example, an average particle size of the primary particles of 5 nm or more. It is preferably 50 μm or less, and more preferably 100 nm or more and 500 nm or less. In addition, the specific surface area is 5m 2 / g or more 15m 2 / g or less. The average particle size of the secondary particles is preferably 5 μm or more and 50 μm or less. The diameter was measured by SEM (scanning electron microscope) or TEM observation, or by laser diffraction / scattering method. The specific surface area can be measured by a particle size distribution meter using a gas adsorption method. It can be measured.
[0204] Alternatively, a composite material (general formula LiMPO4 (M is Fe(II), M The general formula L can be used. Representative examples of iMPO4 include LiFePO4, LiNiPO4, LiCoPO4, and Li MnPO4, LiFe a Ni b PO4, LiFe a Co b PO4, LiFe a Mn b PO 4. LiNi a Co b PO4, LiNi a Mn b PO4(a+b is less than 1, 0 <a<1、 0 <b<1)、LiFe c Ni d Co e PO4, LiFe c Ni d Mn e PO4, LiN i c Co d Mn e PO4(c+d+e is less than 1, 0 <c<1、0<d<1、0<e<1) , Life f Ni g Co h Mn iPO4 (where f + g + h + i is 1 or less, 0 < f < 1, 0 < g <1, 0 < h < 1, 0 < i < 1), etc., lithium compounds can be used.
[0205] In particular, LiFePO4 satisfies well the requirements for a cathode active material, such as safety, stability, high capacity density, and the presence of lithium ions that are initially oxidized, i.e., extracted during charging. Therefore, it is preferable.
[0206] Or, a composite material of the general formula Li (2-j) MSiO4 (M is one or more of Fe(II), Mn(II), Co (II), Ni(II), 0 ≤ j ≤ 2), etc., can be used. General formula Li (2-j) MSiO4 representative examples include Li (2-j) FeSiO4, Li ( 2-j) NiSiO4, Li (2-j) CoSiO4, Li (2-j) MnSiO4, L i (2-j) Fe k Ni l SiO4, Li (2-j) Fe k Co l SiO4, Li (2- j) Fe k Mn l SiO4, Li (2-j) Ni k Co l SiO4, Li (2-j) Ni k Mn l SiO4 (where k + l is 1 or less, 0 < k < 1, 0 < l < 1), Li (2-j) Fe m Ni n Co q SiO4, Li (2-j) Fe m Ni n Mn q SiO4, Li(2-j) N i m Co n Mn q SiO4 (where m + n + q is 1 or less, 0 < m < 1, 0 < n < 1, 0 < q < 1 )、Li (2-j) Fe r Ni s Co t Mn u SiO4 (where r + s + t + u is 1 or less, 0 < r < 1, 0 < s < 1, 0 < t < 1, 0 < u < 1) and other lithium compounds can be used ).
[0207] Also, as the positive electrode active material, A x M2(XO4)3 (A = Li, Na, Mg, M = Fe, Mn, Ti, V, Nb, X = S, P, Mo, W, As, Si) represented by the general formula of NASICON type compounds can be used. NASICON type compounds include Fe2(MnO4)3, Fe2(SO4)3, Li3Fe2(PO4)3, etc. Also, as the positive electrode active material, L i2MPO4F, Li2MP2O7, Li5MO4 (M = Fe, Mn) represented by the general formula of compounds, perovskite type fluorides such as NaFeF3, FeF3, metal chalcogenides (sulfides, selenides, tellurides) such as TiS2, MoS2 , oxides having an inverse spinel type crystal structure such as LiMVO4 (M = Mn , Co, Ni), vanadium oxide systems (V2 O5, V6O 13 8, LiV3O8, etc.), manganese oxides, organic sulfur compounds, etc. can be used .
[0208] In addition, when the carrier ion is an alkali metal ion other than lithium ion or an alkaline earth metal ion, as the positive electrode active material, instead of lithium, an alkali metal (for example, Na thorium, potassium, etc.), alkaline earth metals (e.g. calcium, strontium, barium, etc.), For example, NaFeO2 or Na 2 / 3 [Fe 1 / 2 Mn 1 / 2 ]O2 and other sodium-containing layered oxides are used as the positive electrode active material. It can be used.
[0209] Although not shown, a conductive material such as a carbon layer may be provided on the surface of the positive electrode active material. By providing a conductive material such as a base layer, the conductivity of the electrode can be improved. For example, The carbon layer is coated on the positive electrode active material by mixing carbohydrates such as glucose during the firing of the positive electrode active material. It can be formed by
[0210] The average particle size of the primary particles of the granular positive electrode active material is 50 nm to 100 μm. It would be good to do so.
[0211] <Conductive assistant> The conductive assistant may be, for example, a carbon material, a metal material, or a conductive ceramic material. In addition, a fibrous material may be used as the conductive assistant. The content of the conductive assistant with respect to the total amount of 2 is preferably 1 wt% or more and 10 wt% or less, and 1 wt % or more and 5 wt % or less is more preferable.
[0212] The conductive additive can form an electrically conductive network in the electrode. By this, it is possible to maintain a path of electrical conduction between the active materials. By adding the above, an active material layer having high electrical conductivity can be realized.
[0213] The conductive additive is the same as the conductive additive used in the negative electrode active material layer 107 described in the first embodiment. Such conductive additives can be used.
[0214] In particular, graphene compounds that have electrical conductivity have excellent electrical properties, as well as flexibility and functionality. In some cases, graphene has excellent physical properties such as mechanical strength. By using a conductive compound as a conductive additive, the contact points and contact area between active materials are increased. It can be done.
[0215] In addition, the graphene compound has a low contact resistance because of its planar shape. Surface contact is possible. In addition, the graphene compound has excellent electrical conductivity even when it is thin. Even a small amount of the active material can efficiently form a conductive path in the active material layer.
[0216] When using an active material with a small average particle size, for example, an active material with a particle size of 1 μm or less, the ratio of the active material The surface area is large, and more conductive paths are required to connect the active materials together. Graphene has extremely high electrical conductivity and can efficiently form conductive paths even in small amounts. It is particularly preferred to use a compound.
[0217] In the following, similarly to the negative electrode active material layer 107 in the first embodiment, the positive electrode active material layer 502 is provided with a conductive An example of a cross-sectional configuration in the case where a conductive graphene compound is used as the auxiliary will be described.
[0218] 8A shows a vertical cross-sectional view of the positive electrode active material layer 502. The positive electrode active material layer 502 is made of granular A positive electrode active material 322, a graphene compound 123 as a conductive additive, and a binder ( Here, the graphene compound 123 includes a graphene having electrical conductivity. Preferably, it is a phene compound, reduced graphene oxide.
[0219] In the vertical cross section of the positive electrode active material layer 502, as shown in FIG. The sheet-like graphene compound 123 is dispersed approximately uniformly inside the substrate 2. In the figure, the graphene compound 123 is shown in bold as a schematic diagram, but in reality, the carbon molecules The graphene compounds 123 are thin films having a thickness of a single layer or multiple layers. The positive electrode active material 322 is wrapped, surrounded, or covered by a plurality of granular positive electrode Since they are formed so as to be attached to the surface of the active material 322, they are in surface contact with each other. In addition, the graphene compounds 123 also come into surface contact with each other, forming a multi-graphene compound. 123 forms a three-dimensional electrical conduction network.
[0220] This is because the formation of graphene compound 123 was achieved by using oxidized graphene, which has extremely high dispersibility in polar dispersion media. The graphene oxide is dispersed in a dispersion liquid containing uniformly dispersed graphene oxide. The catalyst is removed by evaporation, and the graphene oxide is reduced to form reduced graphene oxide. The graphene compound 123 remaining on the active material layer 502 partially overlaps with each other and is in surface contact with each other. The graphene oxide is dispersed to such an extent that it forms a path for electrical conduction. The reduction may be carried out, for example, by heat treatment or by using a reducing agent.
[0221] Therefore, unlike granular conductive additives such as acetylene black, which come into point contact with the positive electrode active material, The laphene compound 123 enables surface contact with low contact resistance, so that the low electrical conductivity The amount of the auxiliary agent improves the electrical conductivity between the granular positive electrode active material 322 and the graphene compound 123. Therefore, the ratio of the positive electrode active material 322 in the positive electrode active material layer 502 can be increased. This makes it possible to increase the discharge capacity of the power storage device.
[0222] In addition, graphene compounds bond together to form a mesh-like graphene compound (hereinafter The graphene net is formed by covering the positive electrode active material with the graphene net. In this case, the graphene net can also function as a binder between particles. This allows the amount of binder to be reduced or even eliminated. Therefore, the ratio of the positive electrode active material to the electrode volume and weight can be improved. Therefore, the capacity of the power storage device can be increased.
[0223] FIG. 8B shows an enlarged view of the area surrounded by the dashed line in FIG. 8A. The graphene compound 123 may be present in a layer form on the surface of the electrode active material 322. It is preferable that the binder 323 has a region in contact with the surface of the positive electrode active material 32. 2 and the graphene compound 123. A binder 323 is provided on the graphene compound 123. do.
[0224] <Electrolyte> The solvent of the electrolytic solution 508 is preferably an aprotic organic solvent, for example, ethylene carbonate. Carbonate (EC), Propylene Carbonate (PC), Butylene Carbonate, Chloro Ethylene carbonate, vinylene carbonate, gamma-butyrolactone, gamma-valerolactone Dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl Carbonate (EMC), methyl formate, methyl acetate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ethane ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, One of these, ruforan, sultone, etc., or any combination and ratio of two or more of these It can be used at a rate.
[0225] In addition, by using a polymer material that gels as a solvent for the electrolyte, the resistance to leakage, etc. This improves safety. It also makes it possible to make the storage battery thinner and lighter. Representative examples of materials are silicone gel, acrylic gel, acrylonitrile gel, and polyethylene gel. Styrene oxide gel, polypropylene oxide gel, fluorine polymer gel, etc. There is.
[0226] In addition, a flame-retardant and non-volatile ionic liquid (room-temperature molten salt) is used as the solvent for the electrolyte. By using one or more, the internal temperature of the storage device can be increased due to an internal short circuit or overcharging. Even if the battery is heated, it can prevent the battery from bursting or catching fire. The electrolyte solution is made of cations and anions. Ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations Aliphatic onium cations such as imidazolium cations and pyridinium cations The aromatic cations are also used as anions in the electrolyte. Anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkyl sulfonic acid anion, tetrafluoroborate anion, perfluoroalkyl borate anion phosphate anion, hexafluorophosphate anion, or perfluoroalkyl phosphate anion anions, etc.
[0227] In addition, when lithium ions are used as a carrier for the electrolyte to be dissolved in the above-mentioned solvent, For example, LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, L iSCN, LiBr, LiI, Li2SO4, Li2B 10 Cl 10 , Li2B 12 Cl 12 , LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C 2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO 2) One or more lithium salts such as LiN(C2F5SO2)2 can be used in any combination and ratio.
[0228] In addition, the electrolyte used in the electricity storage device is free of granular waste and elements other than the constituent elements of the electrolyte (hereinafter referred to as It is preferable to use a highly purified electrolyte solution with a low content of impurities. Specifically, the weight ratio of impurities to the electrolyte is 1% or less, preferably 0.1% or less. More preferably, it is set to 0.01% or less.
[0229] In addition, the electrolyte contains vinylene carbonate, propane sultone (PS), and tert-butyl Benzene (TBB), Fluoroethylene carbonate (FEC), Lithium bis(oxalate) Additives such as lithium borate (LiBOB) may be added. The concentration of the additives may be adjusted by, for example, The content should be between 0.1wt% and 5wt% of the total.
[0230] Alternatively, a polymer gel electrolyte may be used in which a polymer is swollen with an electrolytic solution.
[0231] The polymer may be, for example, a polyalkylene oxide such as polyethylene oxide (PEO). Polymers with side structures, PVDF, polyacrylonitrile, etc., and their For example, a copolymer containing PVDF and hexafluoropropylene ( PVDF-HFP, a copolymer of PVDF and HFP, can be used. It may have a porous shape.
[0232] In addition, instead of the electrolyte solution, a solid electrolyte having an inorganic material such as a sulfide or oxide is used. It is possible to use a solid electrolyte containing a polymer material such as PEO (polyethylene oxide). When a solid electrolyte is used, the installation of a separator or spacer becomes unnecessary. Since the entire storage battery can be made solid-state, there is no risk of leakage, and safety is dramatically improved.
[0233] The separator 507 may be made of, for example, paper, nonwoven fabric, glass fiber, ceramics, nylon, etc. Polyamide, vinylon or polyvinyl alcohol fiber, polyester, acrylic The material used must be synthetic fibers such as olefin, polyolefin, and polyurethane. The separator 507 is processed into a bag shape, and is connected to either the positive electrode 503 or the negative electrode 506. For example, as shown in FIG. 9(A), the positive electrode 503 is preferably arranged so as to wrap around the positive electrode 503. The separator 507 is folded in half so as to sandwich the positive electrode 503, and the outside of the area where it overlaps with the positive electrode 503 is sealed. By sealing with the stopper 514, the positive electrode 503 is securely supported within the separator 507. Then, as shown in FIG. 9(B), the positive electrode 503 wrapped in the separator 507 is and a negative electrode 506 are alternately stacked and placed inside an exterior body 509 to form a thin storage battery. It is advisable to form 500.
[0234] FIG. 10 shows an example of welding a current collector to a lead electrode. As shown in FIG. 10(A), The positive electrode 503 wrapped in the palladium plate 507 and the negative electrode 506 are stacked alternately. 03 is welded to the positive electrode lead electrode 510, and the negative electrode 506 is welded to the negative electrode lead electrode 511. FIG. 10B shows an example in which the positive electrode 503 is welded to the positive electrode lead electrode 510. is welded to the positive electrode lead electrode 510 at a weld area 512 using ultrasonic welding or the like. The positive electrode 503 has a curved portion 513 as shown in FIG. 10(B), thereby forming a thin storage battery 5 After the fabrication of the battery 500, the stress caused by the application of external force can be alleviated, and a thin storage battery 500 can be fabricated. This can increase the reliability of 00.
[0235] In the thin storage battery 500 shown in FIGS. 5 and 6, a positive electrode lead electrode 510 and a negative electrode The lead electrode 511 is ultrasonically bonded to the positive electrode 503 or the negative electrode 506 to form a positive electrode lead. The electrode 510 and the negative lead electrode 511 are exposed to the outside. The positive electrode 503 and the negative electrode 506 can also serve as terminals for receiving contact. In that case, Without using lead electrodes, a part of the positive electrode 503 and the negative electrode 506 are exposed to the outside from the exterior body 509. It may be arranged so that
[0236] In addition, in FIG. 5, the positive electrode lead electrode 510 and the negative electrode lead electrode 511 are arranged on the same side. However, as shown in FIG. 11, the positive electrode lead electrode 510 and the negative electrode lead electrode 511 are arranged on different sides. In this way, the storage battery according to one embodiment of the present invention allows the lead electrodes to be freely arranged. Therefore, the design freedom is high. In addition, the productivity of a product using the storage battery according to one embodiment of the present invention can be improved. can be increased.
[0237] In the thin storage battery 500, the exterior body 509 is made of, for example, polyethylene, polypropylene, Aluminum is coated on a membrane made of a material such as polycarbonate, ionomer, or polyamide. A thin metal film made of a material having excellent flexibility, such as aluminum, stainless steel, copper, or nickel, is then formed on the thin metal film. The outer surface of the exterior body is covered with an insulating synthetic resin film such as polyamide resin or polyester resin. A film having a three-layer structure can be used.
[0238] In FIG. 6, as an example, the number of pairs of the positive electrode active material layers and the negative electrode active material layers facing each other is set to five. However, the number of electrode active material layers is not limited to five, and may be more or less. When the number of electrode active material layers is large, a storage battery having a larger capacity can be obtained. In addition, when the number of electrode active material layers is small, the battery can be made thin and has excellent flexibility. It is possible.
[0239] In the above configuration, the exterior body 509 of the thin storage battery 500 has a minimum curvature radius of, for example, The deformation is from 3 mm to 30 mm, and more preferably from 3 mm to 10 mm. The film that is the exterior of the storage battery is made up of one or two sheets, and the In the case of a layered storage battery, the cross-sectional structure of the curved storage battery is The structure is sandwiched between two curves.
[0240] The radius of curvature of the surface will be described with reference to FIG. 12. A part of a curve 1702 included in a surface 1700 is drawn as a circle on a plane 1701 cutting the surface 1700. The radius of the circle is taken as the radius of curvature 1703, and the center of the circle is taken as the center of curvature 1704. FIG. 12B shows a top view of a curved surface 1700. FIG. 12C shows a curved surface 1701. A cross-sectional view of a surface 1700 is shown. When a curved surface is cut by a plane, the angle of the plane to the curved surface is The radius of curvature of the curve that appears in the cross section will differ depending on the cutting angle and cutting position. Now, the smallest radius of curvature is taken as the radius of curvature of the surface.
[0241] When a storage battery with two sheets of film as the exterior body and 1805 sandwiching electrodes and electrolyte is bent, In this case, the radius of curvature 1802 of the film 1801 on the side closer to the center of curvature 1800 of the storage battery is It is smaller than the radius of curvature 1804 of the film 1803 on the side farther from the center of curvature 1800 (FIG. 1 3(A)). If the battery is bent to make the cross section an arc, the film will be close to the center of curvature 180°. The surface of the film far from the center of curvature 1800 is under compressive stress, and the surface of the film far from the center of curvature 1800 is under tensile stress. Force is applied (Figure 13(B)). A pattern formed by concave or convex parts is formed on the surface of the exterior body. This means that even if compressive or tensile stress is applied, the effects of strain can be tolerated. Therefore, the battery can be kept within the minimum range of the exterior body on the side closer to the center of curvature. The radius of curvature is, for example, 3 mm or more and 30 mm or less, more preferably 3 mm or more and 10 mm or less. It can be transformed to become
[0242] The cross-sectional shape of the storage battery is not limited to a simple arc shape, and may be a shape that includes a partial arc. For example, the shape shown in FIG. 13(C), a wavy shape (FIG. 13(D)), an S-shape, etc. In the case where the curved surface of the storage battery has a shape having a plurality of centers of curvature, Among the radii of curvature at the centers of curvature, the surface with the smallest radius of curvature is the surface with two For example, the minimum radius of curvature of the exterior body closest to the center of curvature of the exterior body is 3 mm or more and 30 mm or less. More preferably, the deformation can be within a range of 3 mm to 10 mm.
[0243] Next, various examples of lamination of the positive electrode, the negative electrode and the separator are shown.
[0244] FIG. 14A shows another configuration of a thin storage battery 500, in which a positive electrode 111 and a negative electrode 115 are arranged. The positive electrode 111 has a positive electrode current collector 151 on one side thereof. An active material layer 152 is provided on one surface of a negative electrode current collector 155 of the negative electrode 115. A negative electrode active material layer 156 is provided.
[0245] In the configuration shown in FIG. 14(A), the positive electrode 111 does not have a positive electrode active material layer 152. The positive electrode 115 is placed on the positive electrode 11 so that the surfaces of the negative electrode 115 that do not have the negative electrode active material layer 156 are in contact with each other. 1 and the negative electrode 115 are laminated in this order. The surfaces of the negative electrodes 115 that do not have the negative electrode active material layer 152 are called the surfaces of the negative electrodes 115 that do not have the negative electrode active material layer 156. The contact surface between the metals can be created by the active material and the separator. The coefficient of friction can be reduced compared to the contact surface of the other surface.
[0246] Therefore, when the thin storage battery 500 is curved, the positive electrode active material layer 152 of the positive electrode 111 is The surfaces of the negative electrodes 115 that do not have the negative electrode active material layer 156 slide against each other, so that the curve It is possible to release the stress caused by the difference between the inner diameter and the outer diameter. Here, the inner diameter of the curve is, for example, When the thin storage battery 500 is curved, the exterior body of the thin storage battery 500 has a curved portion. This refers to the radius of curvature of the surface located on the inside of the thin storage battery 500. In addition, the storage battery 500 can be made thin and highly reliable.
[0247] FIG. 14(B) shows an example of lamination of a positive electrode 111 and a negative electrode 115 different from that shown in FIG. 14(A). In the configuration shown in FIG. 14(B), a positive electrode active material layer 152 is provided on both sides of a positive electrode current collector 151. As shown in FIG. 14(B), the positive electrode current collector By providing the positive electrode active material layers 152 on both sides of the positive electrode active material layer 151, the thin storage battery 500 can be formed with a thickness of 100 μm per unit volume. This allows for a larger capacity.
[0248] FIG. 14(C) shows an example of lamination of a positive electrode 111 and a negative electrode 115 different from that shown in FIG. 14(B). In the configuration shown in FIG. 14(C), a negative electrode active material layer 156 is provided on both sides of a negative electrode current collector 155. As shown in FIG. 14(C), the negative electrode current collector By providing the negative electrode active material layers 156 on both sides of the negative electrode active material layer 155, the thin storage battery 500 can be formed with a thickness of 100 μm per unit volume. The capacity can be further increased.
[0249] In the configuration shown in FIG. 14, the separator 153 wraps the positive electrode 111 in a bag shape. However, the present invention is not limited to this. An example having a separator 153 with a different structure is shown. In the structure shown in FIG. 15(A), the positive electrode active A sheet-like separator 153 is provided between each of the material layers 152 and the negative electrode active material layers 156. The configuration shown in FIG. 15(A) differs from the configuration shown in FIG. Six layers of electrodes 111 and six layers of negative electrodes 115 are laminated, and six layers of separators 153 are provided.
[0250] FIG. 15B shows an example in which a separator 153 different from that in FIG. 15A is provided. In the configuration shown in FIG. 15(B), one separator 153 is provided between the positive electrode active material layer 152 and the negative electrode active material layer 153. The point where the insulating film 152 is folded back multiple times so as to be sandwiched between the layers 156 is shown in FIG. The structure shown in FIG. 15(B) is different from the structure shown in FIG. 15(A). It can also be said that the layer is connected by extending the connector 153. In the configuration, six layers of positive electrodes 111 and six layers of negative electrodes 115 are laminated, and a small number of separators 153 are used. The separator 153 must be folded at least five times. The negative electrode active material layer 156 is not only sandwiched between the negative electrode active material layers 156 but also extends to form a plurality of positive electrodes 111. and the negative electrode 115 may be bound together.
[0251] Alternatively, the positive electrode, the negative electrode, and the separator may be laminated as shown in FIG. FIG. 16(A) is a cross-sectional view of the first electrode assembly 130, and FIG. 16(B) is a cross-sectional view of the second electrode assembly 131. FIG. 16(C) shows an example having a separator 153 having a different configuration from that shown in FIG. In FIG. 16(C), for the sake of clarity, the first electrode assembly 130 and the second electrode assembly 13 1 and separator 153 are shown.
[0252] As shown in FIG. 16C, the thin storage battery 500 includes a plurality of first electrode assemblies 130 and and a plurality of second electrode assemblies 131.
[0253] As shown in FIG. 16A, in the first electrode assembly 130, the positive electrode current collector 151 has a A positive electrode 111a having a positive electrode active material layer 152, a separator 153, and both sides of a negative electrode current collector 155 The negative electrode 115a having the negative electrode active material layer 156 on both sides of the separator 153 and the positive electrode current collector 151 The positive electrode 111a having the positive electrode active material layer 152 on the surface is laminated in this order. As shown in FIG. 1B, in the second electrode assembly 131, a negative electrode active material is applied to both sides of the negative electrode current collector 155. The negative electrode 115a has a layer 156, a separator 153, and a positive electrode current collector 151. A positive electrode 111a having a porous layer 152, a separator 153, and a negative electrode current collector 155 are provided on both sides thereof. A negative electrode 115a having a material layer 156 is laminated in this order.
[0254] Further, as shown in FIG. 16(C), a plurality of first electrode assemblies 130 and a plurality of second The electrode assembly 131 is covered by a wound separator 153 .
[0255] <Coin-type battery> Next, as an example of the power storage device, an example of a coin-type storage battery will be described with reference to FIG. FIG. 17(A) is an external view of a coin-type (single-layer flat) storage battery, and FIG. 17(B) is , a cross-sectional view thereof.
[0256] The coin-type storage battery 300 has a positive electrode can 301 that also serves as a positive electrode terminal and a negative electrode can 302 that also serves as a negative electrode terminal. 302 is insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is composed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector 305. It is formed by:
[0257] The negative electrode 307 is made up of a negative electrode current collector 308 and a negative electrode active material It is formed by layer 309 .
[0258] The positive electrode 304 may be the same as that described for the positive electrode 503. The positive electrode active material layer 306 is For the negative electrode 307, see negative electrode 506. The layer 309 may be described with reference to the negative electrode active material layer 505. For the electrolyte, see the description of electrolyte 508.
[0259] The positive electrode 304 and the negative electrode 307 used in the coin-type storage battery 300 are each an active material. The barrier layer need only be formed on one side.
[0260] The positive electrode can 301 and the negative electrode can 302 are made of nickel or aluminum, which are resistant to corrosion by the electrolyte. Metals such as titanium, or alloys of these and other metals, such as stainless steel In order to prevent corrosion by the electrolyte, nickel or aluminum may be used. The positive electrode can 301 is for covering the positive electrode 304, and the negative electrode can 302 is for covering the negative electrode 304. 7 and electrically connected to each other.
[0261] The negative electrode 307, the positive electrode 304 and the separator 310 are impregnated with an electrolyte, and the negative electrode 307, the positive electrode 304 and the separator 310 are impregnated with an electrolyte. As shown in Fig. 2B, the positive electrode can 301 is placed downward, and the positive electrode 304, the separator 310, and the negative electrode 307 are placed in the same position. The positive electrode can 301 and the negative electrode can 302 are stacked in this order, and the positive electrode can 301 and the negative electrode can 302 are secured together with a gasket 303. The coin-shaped storage battery 300 is manufactured by crimping the wires through a wire cutout.
[0262] <Cylindrical storage battery> Next, a cylindrical storage battery will be shown as an example of a power storage device. The cylindrical storage battery 600 has a positive electrode on the upper surface as shown in FIG. It has a cap (battery cover) 601 and a battery can (outer can) 602 on the side and bottom. The positive electrode cap 601 and the battery can (outer can) 602 are connected with a gasket (insulating packing). The device is insulated by 610.
[0263] FIG. 18(B) is a schematic diagram showing a cross section of a cylindrical storage battery. Inside the can 602, a strip-shaped positive electrode 604 and a negative electrode 606 are sandwiched between a separator 605. A wound storage battery element is provided. Although not shown, the storage battery element is wound around a center pin. The battery can 602 is closed at one end and open at the other end. 2 is made of metals such as nickel, aluminum, titanium, etc. that are resistant to corrosion by the electrolyte, or Alloys of these and alloys of these with other metals (e.g., stainless steel, etc.) can be used. In addition, to prevent corrosion by the electrolyte, it is possible to coat it with nickel, aluminum, etc. In the inside of the battery can 602, a positive electrode, a negative electrode, and a separator are wound to form a battery. The battery element is sandwiched between a pair of opposing insulating plates 608 and 609. The inside of the battery can 602 in which the non-aqueous electrolyte is provided is filled with a non-aqueous electrolyte (not shown). The solution used can be the same as that used in coin-type storage batteries.
[0264] The positive electrode 604 may be referred to as the positive electrode 503. The negative electrode 606 may be referred to as the negative electrode 506. The negative electrode 606 can be formed by referring to the method for forming a negative electrode described in Embodiment 1, for example. The positive and negative electrodes used in cylindrical storage batteries are wound, so that active electrodes are placed on both sides of the current collector. A positive electrode terminal (positive electrode current collecting lead) 603 is connected to the positive electrode 604. The negative electrode 606 is connected to a negative electrode terminal (negative electrode current collecting lead) 607. Both the negative electrode terminal 607 and the negative electrode terminal 606 can be made of a metal material such as aluminum. The positive terminal 603 is connected to a safety valve mechanism 612, and the negative terminal 607 is connected to the bottom of the battery can 602. The safety valve mechanism 612 is a PTC (Positive Temperature Coefficient) element. The positive electrode cap 601 is electrically connected to the positive electrode cap 601 via a current collector (current collector) 611. The safety valve mechanism 612 is a mechanism that releases the positive electrode cap when the internal pressure of the storage battery increases beyond a predetermined threshold. The cap 601 and the positive electrode 604 are electrically disconnected. 11 is a thermal resistor whose resistance increases when the temperature rises. The PTC element contains barium titanate (Ba TiO3) based semiconductor ceramics, etc. can be used.
[0265] When winding electrodes in a cylindrical storage battery as shown in Figure 18, large amounts of In addition, when the electrode winding body is housed in a housing, the electrode always has a winding shaft. Even if a large stress acts on the electrode, the active material This can prevent the material from cleaving.
[0266] In this embodiment, the storage battery is a coin type, a cylindrical type, and a thin type. However, other types of batteries, such as sealed batteries and rectangular batteries, can be used. In addition, a structure in which a positive electrode, a negative electrode, and a separator are laminated in multiple layers, For example, other examples of the storage battery are shown in Figs. vinegar.
[0267] (Example of a thin storage battery configuration) 19 and 20 show an example of the configuration of a thin storage battery. The battery 3 has a negative electrode 994 , a positive electrode 995 , and a separator 996 .
[0268] The wound body 993 has a negative electrode 994 and a positive electrode 995 overlapped with a separator 996 sandwiched therebetween. The laminated sheet is then wound. The wound body 993 is placed in a rectangular sealed container or the like. By covering the battery with a material such as aluminum, a rectangular storage battery is created.
[0269] The number of layers of the negative electrode 994, the positive electrode 995, and the separator 996 may be as large as necessary. The negative electrode 994 is connected to the lead electrode 997 and the The positive electrode 995 is connected to a negative electrode collector (not shown) via one of the leads 998. The other of the electrode 997 and the lead electrode 998 is connected to a positive electrode collector (not shown). .
[0270] The storage battery 990 shown in FIG. 19(B) and FIG. 19(C) is a film 981 that serves as an exterior body. The film 982 having the recess is bonded to the film 982 by thermocompression or the like to form a space. The winding body 993 includes a lead electrode 997 and a lead The film 981 and the film 982 having the recesses are electrically connected to each other. It is impregnated with liquid.
[0271] The film 981 and the film 982 having the recesses are made of a metal material such as aluminum. The film 981 and the film 982 having the recesses can be made of a metal or resin material. If a resin material is used as the material for the recess 981, when an external force is applied, the recess 981 and the film 982 are The film 982 having the above structure can be deformed to produce a flexible storage battery. can be done.
[0272] In addition, although Fig. 19(B) and Fig. 19(C) show examples using two films, A space is formed by folding one sheet of film, and the above-mentioned wound body 9 is inserted into the space. 93 may also be accommodated.
[0273] In addition, the exterior body of the power storage device and the sealing container are made of a resin material, etc., so that the device has flexibility. However, when the exterior body or the sealing container is made of a resin material, The parts that are connected to the outside are made of conductive material.
[0274] For example, another example of a thin storage battery having flexibility is shown in FIG. 20. The wound body 9 in FIG. 93 is the same as that shown in FIG. 19(A), so detailed description will be omitted. .
[0275] The storage battery 990 shown in FIG. 20(B) and FIG. 20(C) has the above-described The winding body 993 includes a lead electrode 997 and a lead The electrode 998 is impregnated with an electrolyte inside the exterior bodies 991 and 992. The outer casing 992 can be made of a metal material such as aluminum or a resin material. If resin material is used as the material of 991 and 992, the exterior body 9 91, 992 can be deformed to produce a thin storage battery having flexibility. do.
[0276] By using an electrode including an active material according to one embodiment of the present invention in a flexible thin storage battery, This means that even if stress is applied to the electrodes by repeatedly bending a thin storage battery, the battery will remain active. This can prevent the material from being cleaved.
[0277] As a result, the active material having at least a part of the cleavage plane covered with graphene can be used for an electrode. This makes it possible to suppress a decrease in the voltage of the storage battery and a decrease in the discharge capacity. This makes it possible to improve the cycle characteristics of the storage battery during charging and discharging.
[0278] <Example of energy storage system structure> A structural example of the power storage system will be described with reference to Figs. 21 to 23. The power system refers to, for example, a device equipped with a power storage device.
[0279] 21(A) and 21(B) are diagrams showing the external appearance of the power storage system. The system includes a circuit board 900 and a storage battery 913. The storage battery 913 is provided with a label 91. 21B, the power storage system has a terminal 951 and , a terminal 952 , an antenna 914 , and an antenna 915 .
[0280] The circuit board 900 has a terminal 911 and a circuit 912. The terminal 911 is connected to the terminal 95. 1, terminal 952, antenna 914, antenna 915, and circuit 912. A plurality of terminals 911 are provided, and each of the plurality of terminals 911 is connected to a control signal input terminal, a power supply terminal, It may also be a terminal.
[0281] The circuit 912 may be provided on the back surface of the circuit board 900. The antenna 915 is not limited to a coil shape, but may be, for example, a wire or plate shape. Planar antennas, aperture antennas, traveling wave antennas, EH antennas, magnetic field antennas, induction Alternatively, an antenna such as an electric antenna may be used. 5 may be a flat conductor. This flat conductor functions as one of the conductors for electric field coupling. In other words, one of the two conductors of the capacitor is The antenna 914 or the antenna 915 may be activated. Not only that, but it is also possible to exchange power using an electric field.
[0282] The line width of antenna 914 is preferably larger than the line width of antenna 915. This allows the amount of power received by the antenna 914 to be increased.
[0283] The storage system includes a layer 9 between the antenna 914 and the antenna 915 and the storage battery 913. The layer 916 has a function of shielding the electromagnetic field caused by the battery 913, for example. The layer 916 may be made of, for example, a magnetic material.
[0284] The structure of the power storage system is not limited to the structure shown in FIG.
[0285] For example, as shown in Figs. 22(A-1) and 22(A-2), In the storage battery 913 shown in FIG. 21(B), an antenna is provided on each of a pair of opposing surfaces. FIG. 22(A-1) is an external view seen from one side of the pair of faces. 2(A-2) is an external view seen from the other side of the pair of surfaces. 21(A) and 21(B) are the same as those in the storage system shown in FIG. The explanation of the power storage system shown in FIG. 1(B) can be used as appropriate.
[0286] As shown in FIG. 22(A-1), a layer 916 is sandwiched between one of a pair of surfaces of a storage battery 913. As shown in FIG. 22(A-2), an antenna 914 is provided on one side of the storage battery 913, and the other side of the storage battery 913 is provided on the other side of the storage battery 913. An antenna 915 is provided on the opposite side of the layer 917. The layer 917 is, for example, a storage battery 913. The layer 917 has a function of blocking electromagnetic fields caused by the electromagnetic waves. There can be.
[0287] By adopting the above structure, the size of both antenna 914 and antenna 915 can be increased. It can be heard.
[0288] Or, as shown in FIG. 22(B-1) and FIG. 22(B-2), In the storage battery 913 shown in FIG. 21(B), a separate antenna is attached to each of a pair of opposing surfaces. FIG. 22(B-1) is an external view of the pair of surfaces as viewed from one side, FIG. 22(B-2) is an external view seen from the other side of the pair of faces. The same parts as those in the storage system shown in FIG. 21(A) and FIG. 21(B) are shown in FIG. The description of the power storage system shown in FIG. 21B can be used as appropriate.
[0289] As shown in FIG. 22(B-1), a layer 916 is sandwiched between one of the pair of surfaces of a storage battery 913. An antenna 914 and an antenna 915 are provided, and as shown in FIG. An antenna 918 is provided on the other of the pair of surfaces of the antenna 913 with a layer 917 sandwiched therebetween. The antenna 91 has a function of performing data communication with an external device, for example. 8, for example, an antenna having a shape applicable to antenna 914 and antenna 915 is applied. As a communication method between the power storage system and other devices via the antenna 918, The system applies a response method such as NFC that can be used between the energy storage system and other devices. It is possible.
[0290] 23(A), the storage battery 91 shown in FIG. 21(A) and FIG. 21(B) A display device 920 may be provided on the input side of the input terminal 911 via a terminal 919. The label 910 is electrically connected to the display device 920. It is not necessary to use the same parts as those in the power storage system shown in FIG. 21(A) and FIG. 21(B). For this purpose, the description of the power storage system shown in FIG. 21(A) and FIG. 21(B) can be used as appropriate.
[0291] The display device 920 displays, for example, an image indicating whether charging is in progress, an image indicating the amount of stored power, etc. The display device 920 may be, for example, an electronic paper, a liquid crystal display device, an electronic For example, electroluminescence (EL) display devices can be used. By using the polarizer, the power consumption of the display device 920 can be reduced.
[0292] 23(B), the storage battery 91 shown in FIG. 21(A) and FIG. 21(B) A sensor 921 may be provided on the terminal 911 via a terminal 922. Note that the same parts as the power storage system shown in FIG. 21(A) and FIG. 21(B) are used. For this, the explanation of the power storage system shown in FIG. 21(A) and FIG. 21(B) can be used as appropriate. Cut.
[0293] The sensor 921 may be, for example, a sensor for detecting force, displacement, position, velocity, acceleration, angular velocity, rotation speed, distance, etc. Distance, light, liquid, magnetic, temperature, chemicals, sound, time, hardness, electric field, current, voltage, power, radiation Use devices that include the function of measuring line, flow rate, humidity, gradient, vibration, odor, or infrared rays. By providing the sensor 921, for example, Data indicative of the temperature can be detected and stored in the memory of the circuit 912. .
[0294] The battery and the power storage system described in this embodiment include an electrode according to one embodiment of the present invention. This allows the capacity of storage batteries and power storage systems to be increased. It is possible to increase the energy density. It is also possible to improve reliability. It is also possible to extend the life. It can be made easier.
[0295] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0296] (Embodiment 3) In this embodiment, an example in which a flexible storage battery is mounted in an electronic device will be described.
[0297] FIG. 24 shows an example in which the flexible storage battery described in Embodiment 2 is mounted in an electronic device. As an example of an electronic device to which a flexible storage battery is applied, a television set (television, (also called television receivers), computer monitors, digital cameras, digital digital video cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices) (hereinafter referred to as "computer games"), portable game machines, personal digital assistants, audio playback devices, large game machines such as pachinko machines etc.
[0298] In addition, the flexible storage battery can be mounted on the inner or outer walls of houses or buildings, or on the interior or exterior of automobiles. It is also possible to install it along the curved surface of the exterior.
[0299] FIG. 24A shows an example of a mobile phone. A mobile phone 7400 includes a housing 740. In addition to the display unit 7402 incorporated in the 1, the operation buttons 7403, the external connection port 7404, The mobile phone 7400 includes a speaker 7405, a microphone 7406, and the like. The device has an electrical device 7407.
[0300] FIG. 24B shows the mobile phone 7400 in a curved state. When the 00 is deformed by an external force and curved, the storage battery installed inside The storage device 7407 is also bent. At this time, the bent state of the storage device 7407 is shown in FIG. The power storage device 7407 is a thin storage battery. The power storage device 7407 is fixed in a resistor connected electrically to the current collector 7409. It has a gate electrode 7408.
[0301] FIG. 24D shows an example of a bangle-type display device. The portable display device 7100 is 7101, a display unit 7102, operation buttons 7103, and a power storage device 7104. FIG. 24E shows the bent state of the power storage device 7104. When the device is bent and worn on the user's arm, the housing may deform and cause a part of the power storage device 7104 or The total curvature changes. The degree of curvature at any point on the curve is expressed as the radius of the corresponding circle. The value expressed as the radius of curvature is called the curvature, and the reciprocal of the radius of curvature is called the curvature. A part of the main surface of the housing or the power storage device 7104 within a range of 40 mm to 150 mm in diameter Or the entire surface of the power storage device 7104 changes. High reliability can be maintained if the deviation is within the range of 0 mm or less.
[0302] FIG. 24F shows an example of a wristwatch-type portable information terminal. The housing 7201, the display unit 7202, the band 7203, the buckle 7204, the operation button 7 205, an input / output terminal 7206, etc.
[0303] The portable information terminal 7200 is capable of carrying out mobile phone calls, e-mails, viewing and creating documents, playing music, and internet connections. It can run various applications such as internet communication and computer games. Cut.
[0304] The display unit 7202 has a curved display surface, and displays information along the curved display surface. The display unit 7202 is equipped with a touch sensor, and the screen can be operated by touching it with a finger or a stylus. For example, the icon 7 displayed on the display unit 7202 can be operated by touching the By touching 207, the application can be launched.
[0305] The operation button 7205 is used to set the time, turn the power on and off, and turn wireless communication on and off. It supports various functions such as auto-start, silent mode and power saving mode. For example, an operating system built into the portable information terminal 7200 can be Depending on the system, the functions of the operation buttons 7205 can be freely set.
[0306] In addition, the mobile information terminal 7200 is capable of performing short-distance wireless communication according to a communication standard. For example, by communicating with a wireless headset, a hands-free You can also make calls.
[0307] The portable information terminal 7200 also includes an input / output terminal 7206 and is connected to other information terminals via a connector. Data can be exchanged directly through the input / output terminal 7206. The charging operation can be performed by wireless power supply without going through the input / output terminal 7206. You may go.
[0308] The display portion 7202 of the portable information terminal 7200 includes an electrode according to one embodiment of the present invention. For example, the power storage device 7104 shown in FIG. It can be installed in a curved state or in a curved state inside the band 7203. do.
[0309] The portable information terminal 7200 preferably has a sensor. For example, a fingerprint sensor may be used as the sensor. Human body sensors such as sensors for measuring body temperature, touch sensors, pressure sensors, and acceleration sensors. It is preferable that the sensor, etc. be mounted.
[0310] FIG. 24G shows an example of a wristband-type display device. The display device 7300 has a display unit The display device 7300 includes a power storage device of one embodiment of the present invention. The display portion 7304 may be provided with a touch sensor, and may function as a portable information terminal. It is also possible.
[0311] The display surface of the display unit 7304 is curved, and the display is performed along the curved display surface. In addition, the display device 7300 can display the image by short-distance wireless communication according to a communication standard. You can change the situation.
[0312] The display device 7300 also has an input / output terminal, and can directly connect to other information terminals via a connector. It is possible to exchange data. It is also possible to charge the device via the input / output terminal. The charging operation may be performed by wireless power supply without using the input / output terminals.
[0313] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0314] (Embodiment 4) In this embodiment, an example of an electronic device in which a power storage device can be mounted will be described.
[0315] FIG. 25(A) and FIG. 25(B) show an example of a tablet terminal that can be folded in two. The tablet terminal 9600 shown in FIG. 25(A) and FIG. 25(B) includes a housing 9630a, A housing 9630b, a movable part 9640 connecting the housings 9630a and 9630b, and a display unit 9 A display unit 9631 having a display unit 9631a and a display unit 9631b, a display mode changeover switch 96 26, power switch 9627, power saving mode switch 9625, fastener 9629 25(A) shows the tablet terminal 9600 in an open state. 25(A) shows a state in which the tablet terminal 9600 is opened, and FIG. 25(B) shows a state in which the tablet terminal 9600 is closed.
[0316] The tablet terminal 9600 also includes a housing 9630a and a housing 9630b. The power storage unit 9635 is connected to the housing 9630a through the movable portion 9640. It is provided across the body 9630b.
[0317] A part of the display unit 9631a can be used as a touch panel area 9632a. By touching the operation keys 9638 displayed on the display unit 96, data can be input. In 31a, as an example, half of the area has a display function only, and the other half The display unit 96 has a touch panel function, but is not limited to this. The entire area of the display unit 931a may have a touch panel function. The entire surface of 631a is made to display keyboard buttons to serve as a touch panel, and the display section 9631b is made to display It can be used as a display screen.
[0318] In addition, in the display unit 9631b, as in the display unit 9631a, The part of the touch panel can be the area 9632b of the touch panel. Touch the area where the mode display switch button 9639 is displayed with your finger or a stylus. A keyboard button can be displayed on the display portion 9631b.
[0319] In addition, the touch panel area 9632a and the touch panel area 9632b are simultaneously You can also use touch input.
[0320] A display mode changeover switch 9626 is used to change the display orientation, such as vertical or horizontal. You can choose between black and white and color display. The switch 9625 detects the usage of the light detected by the light sensor built into the tablet terminal 9600. The display brightness can be optimized according to the amount of external light at the time. In addition to optical sensors, other sensors such as gyros and acceleration sensors that detect tilt are also used. An ejection device may be built in.
[0321] FIG. 25A shows an example in which the display area of the display portion 9631b is the same as that of the display portion 9631a. However, there is no particular limitation, and one size may be different from the other size. The quality of the display may also be different. For example, one display panel may provide a higher resolution display than the other. It may also be used as a rule.
[0322] FIG. 25(B) shows the tablet terminal in a closed state. The tablet terminal includes a housing 9630 and a solar cell 9 633, a charge / discharge control circuit 9634 including a DCDC converter 9636. The power storage unit according to one embodiment of the present invention is used as the power storage unit 9635.
[0323] In addition, since the tablet terminal 9600 can be folded in two, when not in use, The housing 9630b can be folded so that the housing 9630b and the housing 9630b overlap each other. Since the display units 9631a and 9631b can be protected, the tablet terminal 9600 The durability can be improved. In addition, the power storage unit 9635 using the power storage unit of one embodiment of the present invention It has flexibility and the charge / discharge capacity does not decrease easily even if it is repeatedly bent and stretched. Therefore, it has high reliability. It can provide an excellent tablet device.
[0324] In addition, the tablet terminals shown in Fig. 25(A) and Fig. 25(B) are used in various Functions that display useful information (still images, videos, text images, etc.), calendars, dates, or times A function to display the information on the display unit, and a function to input or edit the information displayed on the display unit. It has a function to input data, a function to control processing by various software (programs), etc. It is possible.
[0325] The solar cell 9633 attached to the surface of the tablet device supplies power to the touch panel. The solar cell 9633 can supply the solar cell 9633 with the following components: The battery 9635 can be efficiently charged by providing the battery on one or both sides of the housing 9630. The power storage unit 9635 can be a lithium ion battery. This has the advantage of enabling miniaturization.
[0326] The configuration and operation of the charge / discharge control circuit 9634 shown in FIG. A block diagram is shown in FIG. 25C. A solar cell 9633 and a power storage unit 96 35, DCDC converter 9636, converter 9637, switch SW1 to switch SW3, a display unit 9631, a power storage unit 9635, and a DC-DC converter 96 36, the converter 9637, and the switches SW1 to SW3 are shown in FIG. This corresponds to the charge / discharge control circuit 9634 .
[0327] First, an example of operation in which power is generated by the solar cell 9633 using external light will be described. The power generated by the solar cell is converted to a voltage to charge the storage battery 9635. The converter 9636 increases or decreases the voltage. When power from the battery 9633 is used, the switch SW1 is turned on, and the converter 963 7, the voltage is increased or decreased to a voltage required for the display unit 9631. When not displaying in 1, turn SW1 off and SW2 on to turn on the power storage unit 9635. It is sufficient to configure the device so as to perform charging.
[0328] The solar cell 9633 is shown as an example of a power generating means, but is not limited thereto. Storage by other power generation means such as piezoelectric elements and thermoelectric conversion elements For example, the power may be transmitted and received wirelessly (contactlessly). The configuration is a non-contact power transmission module that charges the battery by connecting the battery to the battery, or by combining it with other charging means. You may do so.
[0329] Another example of electronic equipment is shown in FIG. 26. In FIG. 26, a display device 8000 is a display device according to the present invention. 8 is an example of an electronic device including a power storage device 8004 according to one embodiment. 8000 corresponds to a display device for receiving TV broadcasts, and includes a housing 8001, a display unit 8002, a speaker, The power storage device 8004 according to one embodiment of the present invention includes: The display device 8000 is provided inside a housing 8001. The display device 8000 is supplied with power from a commercial power source. It is also possible to use the power stored in the power storage device 8004. Therefore, even when power cannot be supplied from a commercial power source due to a power outage or the like, the present invention according to one aspect of the present invention can be used. The display device 8000 can be used by using the power storage device 8004 as an uninterruptible power supply. become.
[0330] The display unit 8002 is a display device having a light emitting element such as a liquid crystal display device or an organic EL element in each pixel. Optical devices, electrophoretic displays, DMD (Digital Micromirror Devices) ice), PDP (Plasma Display Panel), FED (Field A semiconductor display device such as a 3D Emission Display can be used.
[0331] In addition, display devices are used for TV broadcast reception, personal computers, advertising displays, etc. This includes all display devices for displaying information, such as
[0332] In FIG. 26, a stationary lighting device 8100 includes a power storage device 8 according to one embodiment of the present invention. 8101 is an example of an electronic device using the lighting device 8100. The light source 8102 and the power storage device 8103 are included. In FIG. For example, the light source 101 and the light source 8102 are installed inside a ceiling 8104. 8, the power storage device 8103 may be provided inside the housing 8101. The device 8100 can receive power from a commercial power source, or can store power in a power storage device 8103. The stored power can also be used. Therefore, in the event of a power outage, the supply of power from the commercial power source is not possible. Even when power cannot be received, the power storage device 8103 of one embodiment of the present invention can be used as an uninterruptible power source. This enables the lighting device 8100 to be used.
[0333] In addition, FIG. 26 illustrates a lighting device 8100 that is installed on a ceiling 8104. However, in the power storage device of one embodiment of the present invention, in addition to the ceiling 8104, for example, the side wall 8105, the floor The present invention can be applied to a lighting device installed in a fixed position such as a desk 8106 or a window 8107. It can also be used in upper lighting devices.
[0334] In addition, the light source 8102 can be an artificial light source that artificially obtains light using electricity. Specifically, this applies to incandescent lamps, discharge lamps such as fluorescent lamps, and light-emitting diodes and organic electroluminescence (EL) elements. An example of the artificial light source is a light element.
[0335] In FIG. 26, an air conditioner having an indoor unit 8200 and an outdoor unit 8204 is 8 is an example of an electronic device including a power storage device 8203 according to one embodiment of the present invention. The indoor unit 8200 includes a housing 8201, an air outlet 8202, a power storage device 8203, and the like. In the example shown in FIG. 1, the power storage device 8203 is provided in the indoor unit 8200. The electric device 8203 may be provided in an outdoor unit 8204. The power storage device 8203 may be provided in both the outdoor units 8204. The power supply can be supplied from a commercial power source, or the power stored in the power storage device 8203 can be used. In particular, both the indoor unit 8200 and the outdoor unit 8204 are provided with a power storage device 8 If 203 is installed, when power cannot be supplied from the commercial power source due to a power outage, etc. However, by using the power storage device 8203 of one embodiment of the present invention as an uninterruptible power supply, The use of conditioners will be possible.
[0336] In addition, in Figure 26, a separate type air conditioner consisting of an indoor unit and an outdoor unit is shown. However, an integrated air conditioner that has both the indoor and outdoor functions in a single housing is also shown. The power storage device of one embodiment of the present invention can also be used for the conditioner.
[0337] In FIG. 26 , an electric refrigerator-freezer 8300 includes a power storage device 8304 according to one embodiment of the present invention. Specifically, an electric refrigerator-freezer 8300 includes a housing 8301, The door for a refrigerator 8302, the door for a freezer 8303, a power storage device 8304, and the like are included. A power storage device 8304 is provided inside a housing 8301. The power supply can be received from a commercial power source, or the power stored in the power storage device 8304 can be used. Therefore, when power cannot be supplied from commercial power sources due to a power outage, etc. Even in such a case, the power storage device 8304 of one embodiment of the present invention can be used as an uninterruptible power supply. It will be possible to use 8300 refrigerators / freezers.
[0338] Among the above-mentioned electronic devices, high-frequency heating devices such as microwave ovens and electric rice cookers The child devices require high power for a short period of time. Therefore, the power that cannot be supplied by the commercial power supply is supplemented. By using a power storage device according to one embodiment of the present invention as an auxiliary power source for supporting This can prevent the commercial power breaker from tripping when using the device.
[0339] In addition, during periods when electronic devices are not in use, the total amount of power that can be supplied by commercial power suppliers is also During periods when the ratio of the amount of electricity actually used (called the electricity usage rate) is low, By storing electricity in the electrical equipment, it is possible to prevent the power usage rate from increasing outside the above-mentioned time periods. For example, in the case of the electric refrigerator-freezer 8300, when the temperature is low, the refrigerator compartment door 83 02, during the night when the freezer door 8303 is not opened or closed, power is supplied to the power storage device 8304. Then, as the temperature rises, the refrigerator door 8302 and the freezer door 8303 open and close. During the daytime, when the electricity is consumed, the power storage device 8304 is used as an auxiliary power source. The rate can be kept low.
[0340] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0341] (Embodiment 5) In this embodiment, an example in which a power storage device is mounted on a vehicle will be described.
[0342] In addition, by installing a power storage device in a vehicle, it can be used as a hybrid vehicle (HEV) or electric vehicle (EV). or next-generation clean energy vehicles such as plug-in hybrid vehicles (PHEVs) It can be realized.
[0343] 27A and 27B show examples of vehicles using one embodiment of the present invention. The 8400 is an electric vehicle that uses an electric motor as a power source for running. The vehicle can be powered by either an electric motor or an engine. A hybrid vehicle. By using one embodiment of the present invention, a vehicle with a long driving range can be realized. The automobile 8400 also has a power storage device. The power storage device can be an electric motor. It not only drives the 8406, but also the headlights 8401 and room lights (not shown). It is possible to supply power to the light emitting device.
[0344] In addition, the power storage device can be used to store information such as a speedometer and a tachometer of the automobile 8400. The power storage device can supply power to the navigation device of the automobile 8400. The present invention can provide power to semiconductor devices such as gating systems.
[0345] The automobile 8500 shown in FIG. 27B is a power storage device that is plugged in to the automobile 8500. It is possible to charge the battery by receiving power from an external charging facility using a contactless charging method or other methods. FIG. 27(B) shows a case where a charging device mounted on a vehicle 8500 is connected to a ground-mounted charging device 8021. The power storage device 8024 is shown being charged via a cable 8022. For charging methods and connector specifications, please refer to the specifications of CHAdeMO (registered trademark) and Combo. The charging device 8021 is a charging station installed in a commercial facility. For example, plug-in technology can be used to connect the power source to the outside. The power storage device 8024 mounted on the automobile 8500 can be charged by the power supply. Charging is performed by converting AC power to DC power via a converter such as an AC / DC converter. It is possible to do so.
[0346] Although not shown, a power receiving device is mounted on the vehicle and receives power from a ground power transmitting device in a non-contact manner. In this case, the power transmission device is installed on the road or on the exterior wall. By incorporating this, charging can be done not only when the vehicle is stopped but also while the vehicle is moving. In addition, the vehicle exterior may be provided with a power supply. A solar cell may be provided in the vehicle so that the power storage device can be charged when the vehicle is stopped or traveling. To supply power in the above, an electromagnetic induction method or a magnetic resonance method can be used.
[0347] According to one embodiment of the present invention, the cycle characteristics of a power storage device can be improved, and the reliability can be improved. Furthermore, according to one embodiment of the present invention, the characteristics of the power storage device can be improved, Therefore, the power storage device itself can be made smaller and lighter. This contributes to reducing the weight of the vehicle, which can improve the cruising distance. The on-board power storage device can also be used as a power supply source for something other than the vehicle. This allows avoiding the use of commercial power during peak hours.
[0348] This embodiment mode can be implemented in appropriate combination with other embodiment modes. EXAMPLES
[0349] In this example, a negative electrode of one embodiment of the present invention will be described with reference to the flow shown in FIG.
[0350] Based on steps S101 to S105 of FIG. 3, a slurry to be used for coating the electrodes is prepared. Ta.
[0351] In step S101 of FIG. 3, a silicon wafer (p-type, surface orientation (100)) is crushed. The silicon particles used for the negative electrode active material 121 were prepared by the following grinding conditions for the ball mill treatment: Put 4g of silicon powder, a 3mm diameter ball, and acetone into a container and rotate at 400 rpm for 5 hours. The sieve used had a hole diameter of 75 μm.
[0352] In step S102 of FIG. 3, the surface of the silicon particles is oxidized to form a silicon oxide film. The heat treatment conditions were 900°C in air and 1.5 hours.
[0353] FIG. 28 is a cross-sectional SEM image of the silicon particle produced in step S102 as described above. In the cross-sectional SEM photograph of FIG. 28, a silicon oxide film 126 is formed on the surface of a silicon particle. It has also been shown that small-sized silicon particles are easily broken down by heat treatment. The whole becomes the silicon oxide film 126.
[0354] In step S103 of FIG. 3, the graphene compound and the binder produced in step S102 are mixed. The graphene compound used here was graphene oxide. The mixture ratio of silicon particles, graphene oxide, and polyimide precursor was 60:20:20 ( % by weight. Specifically, 1.0 g of silicon particles and 0.0 g of graphene oxide were mixed. The mixture was mixed with 2.33 g of ethylenediaminetetraacetate and 2.4 g of a polyimide precursor. After the heating process, 13.7% of the whole material is imidized to become polyimide. The weight of the polyimide after oxidation is 0.33 g (2.4 g × 0.137).
[0355] In addition, as the above mixing procedure, graphene oxide, polyimide precursor and NMP ( A mixture was made by mixing 6.0 ml of the dispersion medium with the 1.0 ml of ... ) was mixed with silicon particles, kneaded, and the dispersion medium was removed by volatilization. The procedure of removing the dispersion medium by evaporation was repeated several times until the mixture was completely used up. The time for the evaporation was 40 minutes, and the dispersion medium was removed by evaporation at 110°C for 10 hours.
[0356] In step S104, the silicon oxide film formed on the surface of the silicon particles is etched. The etching was performed using ammonium hydrogen fluoride (NH4HF 2) 7.13% and ammonium fluoride (NH4F) 15.4% mixed solution (Stella The above mixture was dropped onto the silicon particles, and then 5 The substrate was left for 10 minutes and then washed several times with pure water. The heating was performed at 110°C for 10 hours in a vacuum furnace at 400°C for 1 Here, the graphene oxide mixed in step S103 is heated to The precursor of polyimide is thermally reduced to graphene, and the precursor of polyimide is imidized to polyimide by heat treatment. It becomes a reimide.
[0357] FIG. 29 is a cross-sectional SEM photograph of the mixture produced in step S104 as described above. In the cross-sectional SEM photograph of FIG. 29, silicon particles, which are negative electrode active material 121, and silicon particles The gap 124 around the substrate is covered with a mixture of graphene 127 and polyimide 128. It has also been shown that even in areas where silicon particles are not present, voids 1 25 is shown covered by graphene 127 and polyimide 128. Here, the graphene 127 has a thickness of about 100 nm and is therefore formed of multiple layers. This suggests that the graphene oxide is reduced.
[0358] In step S105, the polyimide precursor and the mixture prepared in step S104 are The mixture and polyimide precursor were mixed in a ratio of 85:1 to prepare a slurry. 5 (wt%). 0.3504 g of precursor was mixed, 1.21 g of NMP (dispersion medium) was added, and the mixture was kneaded. The time for hard kneading was 40 minutes.
[0359] According to steps S106 to S108 of FIG. 3, the slurry is applied to the negative electrode current collector. The dispersion medium was removed by volatilization, and a heat treatment was then performed to prepare a negative electrode.
[0360] In step S106, the slurry is applied to the negative electrode current collector, and the dispersion medium is removed by volatilization. The negative electrode current collector was copper with a thickness of 18 μm. The blade method was used for coating. The blade had a gap of 100 μm with respect to the surface of the current collector. To remove the dispersion medium by evaporation, a forced-air dryer was used at 80°C for 2 hours.
[0361] In step S107, a heat treatment was performed. The heat treatment was performed in a vacuum furnace at 400° C. , one hour.
[0362] FIG. 30 shows the cycle of a lithium ion storage battery using the negative electrode prepared as described above. The characteristics are shown in the figure, and the results are shown for a half cell. To evaluate the characteristics of the half cell, metallic lithium was used as the positive electrode. The battery used is a CR2032 type (diameter 20 mm, height 3.2 mm) coin-type battery. The charge / discharge rate was 1C.
[0363] The electrolyte contains ethylene carbonate (EC) and diethyl carbonate (DEC). In a mixed solution of lithium hexafluorophosphate (LiPF6 The separator was made of polypropylene. Used.
[0364] In FIG. 30, the vertical axis indicates the capacity (mAh / g) and the horizontal axis indicates the number of cycles. The battery was charged and discharged 200 times. The solid line indicates the charge and the dashed line indicates the discharge.
[0365] <Reference example 1> The negative electrode active material layer in the negative electrode of this reference example was made of crushed silicon wafers. Silicon particles are used, but the voids around the silicon particles provided in one embodiment of the present invention are Not set.
[0366] The negative electrode active material of the negative electrode of the reference example was prepared by the steps S102 and S103 shown in the above embodiment. Specifically, the silicon in step S102 was A step of subjecting the particles to a heat treatment to form a silicon oxide film on the surface of the silicon particles; The step of removing the silicon oxide film in S104 was omitted.
[0367] FIG. 31 shows the cycle of a lithium ion storage battery using the negative electrode prepared as described above. The characteristics are shown in the figure, and the results are shown for a half cell. To evaluate the characteristics of the half cell, metallic lithium was used as the positive electrode. The battery used is a CR2032 type (diameter 20 mm, height 3.2 mm) coin-type battery. The charge / discharge rate was 1C.
[0368] The electrolyte contains ethylene carbonate (EC) and diethyl carbonate (DEC). In a mixed solution of lithium hexafluorophosphate (LiPF6 The separator was made of polypropylene. Used.
[0369] In FIG. 31, the vertical axis indicates the capacity (mAh / g) and the horizontal axis indicates the number of cycles. The battery was subjected to 39 charge / discharge cycles. The solid line indicates the charge and the dashed line indicates the discharge.
[0370] As shown in FIG. 31, the cycle characteristics of the negative electrode of the reference example were such that the number of cycles exceeded 10. The capacity drops rapidly when the battery is turned on, and the capacity cannot be maintained before the number of cycles reaches 20. In this reference example, the sudden decrease in capacity was caused by the increase in silicon particles due to charging and discharging. The stress caused by the expansion and contraction of the volume of the negative electrode causes the contact area between the negative electrode current collector and the silicon particles, This is because the contact area between the materials is reduced. This phenomenon damages the conductive path inside the anode. This was because the battery characteristics had deteriorated.
[0371] On the other hand, as shown in FIG. 30, the cycle of the negative electrode prepared according to one embodiment of the present invention The characteristics are that the capacity gradually decreases with the number of cycles, but after 200 cycles This is because the silicon particles are able to expand and contract in volume during charging and discharging. Even if the number of times is repeated, the voids around the silicon particles or distributed in the negative electrode active material layer will expand in volume. This is because it relieves the stress caused by the shrinkage of the battery. This maintains the conductive path inside the anode. This makes it possible to prevent the capacity from decreasing due to charge / discharge cycles. [Explanation of symbols]
[0372] 101 Negative electrode 107 Negative electrode active material layer 109 Negative electrode current collector 111 Positive electrode 111a positive electrode 115 Negative electrode 115a negative electrode 121 Negative electrode active material 122 Binding material 123 Graphene Compounds 124 void 125 void 126 Silicon oxide film 127 Graphene 128 Polyimide 130 Electrode assembly 131 Electrode assembly 151 Positive electrode current collector 152 Cathode active material layer 153 Separator 155 Negative electrode current collector 156 Negative electrode active material layer 157 Exterior body 300 Battery 301 Positive electrode can 302 Anode can 303 Gasket 304 Positive electrode 305 Positive electrode current collector 306 Positive electrode active material layer 307 Negative electrode 308 Negative electrode current collector 309 Negative electrode active material layer 310 Separator 322 Cathode active material 323 Binding material 331 First Area 332 Second Area 333 The Third Region 500 Battery 501 Positive electrode current collector 502 Positive electrode active material layer 503 Positive electrode 504 Negative electrode current collector 505 Negative electrode active material layer 506 negative electrode 507 Separator 508 Electrolyte 509 Exterior body 510 Positive lead electrode 511 Negative lead electrode 512 Welding Area 513 Curved section 514 Sealing part 600 Battery 601 Positive electrode cap 602 Battery Can 603 Positive terminal 604 Positive electrode 605 Separator 606 negative electrode 607 Negative terminal 608 Insulating plate 609 Insulating plate 611 PTC element 612 Safety valve mechanism 900 Circuit Board 910 Label 911 Terminal 912 Circuit 913 Storage battery 914 Antenna 915 Antenna 916 layers 917 layers 918 Antenna 919 Terminal 920 Display device 921 Sensor 922 Terminal 951 Terminal 952 Terminal 981 Film 982 Film 990 Battery 991 Exterior body 992 Exterior body 993 Wound body 994 negative electrode 995 positive electrode 996 Separator 997 Lead Electrode 998 Lead Electrode 1700 curved surface 1701 Plane 1702 Curve 1703 Radius of curvature 1704 Center of curvature 1800 Center of curvature 1801 Film 1802 radius of curvature 1803 Film 1804 radius of curvature 7100 Portable display devices 7101 Case 7102 Display section 7103 Operation button 7104 Energy storage devices 7200 Portable Information Terminal 7201 Case 7202 Display section 7203 Band 7204 Buckle 7205 Operation button 7206 Input / output terminal 7207 Icon 7300 display device 7304 Display section 7400 Mobile Phone 7401 Case 7402 Display section 7403 Operation button 7404 External connection port 7405 Speaker 7406 Mike 7407 Energy storage devices 7408 Lead electrode 7409 Current collector 8000 display device 8001 Case 8002 Display section 8003 Speaker section 8004 Electricity storage device 8021 Charging device 8022 Cable 8024 Electricity storage device 8100 Lighting equipment 8101 Case 8102 Light source 8103 Energy storage devices 8104 Ceiling 8105 Side wall 8106 Bed 8107 Window 8200 indoor unit 8201 Case 8202 Ventilator 8203 Energy storage devices 8204 Outdoor unit 8300 Electric refrigerator-freezer 8301 Case 8302 Refrigerator door 8303 Freezer door 8304 Energy storage devices 8400 Automobiles 8401 Headlight 8406 Electric Motor 8500 Automobiles 9600 Tablet PC 9625 Switch 9626 Switch 9627 Power Switch 9628 Operation Switch 9629 Fastener 9630 Case 9630a Case 9630b Case 9631 Display section 9631a Display section 9631b Display section 9632a area 9632b area 9633 Solar Cells 9634 Charge / discharge control circuit 9635 Electric storage unit 9636 DC-DC Converter 9637 Converter 9638 Operation key 9639 Button 9640 Moving parts
Claims
[Claim 1] A negative electrode and a positive electrode, the negative electrode has a current collector and a negative electrode active material layer on the current collector, The negative electrode active material layer includes a negative electrode active material, a conductive assistant, and a binder, The negative electrode active material has silicon particles, The conductive assistant has a first graphene and a second graphene, the binder comprises a first polyimide and a second polyimide; In cross section, the negative electrode active material layer has a first void in a region surrounding the silicon particle, the first void is a region surrounded by the silicon particle, the first graphene, and the first polyimide having a region in contact with the first graphene, the negative electrode active material layer has second voids in regions where the silicon particles are not present, the second void is a region surrounded by the second graphene and the second polyimide having a region in contact with the second graphene.
Citation Information
Patent Citations
Negative electrode for power storage device, power storage device, and electrical machine
JP2015118924A
Secondary battery
JP2001283834A