The integration of a microcrystalline semiconductor film with an amorphous semiconductor film coverage and impurity element-doped regions in thin film transistors addresses yield and current issues, resulting in high mobility and low off-state current for improved display device performance.

JP2024166329AInactive Publication Date: 2024-11-28SEMICON ENERGY LAB CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024159075
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2007-12-21
Filing Date
2024-09-13
Publication Date
2024-11-28
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Thin film transistors using amorphous semiconductor films have high field effect mobility but complex processing leads to reduced yield and increased cost, while those with microcrystalline films improve on-state current but increase off-state current, affecting display device performance and power consumption.

Method used

A thin film transistor design incorporating a microcrystalline semiconductor film with an amorphous semiconductor film covering its sides and edges, and a specific impurity element-doped semiconductor film, connected through a gate insulating film, reduces off-state current and enhances field effect mobility.

Benefits of technology

This design results in thin film transistors with high field effect mobility, reduced off-state current, and improved image quality in display devices, allowing for efficient power usage and enhanced display performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166329000001_ABST
    Figure 2024166329000001_ABST
Patent Text Reader

Abstract

To reduce a reverse current of a diode as one of the purposes, and improve image quality of a display using a thin-film transistor as one of the purposes.SOLUTION: A thin-film transistor has a microcrystalline semiconductor film that is provided on a gate electrode and in an inside area not reaching the ends of the gate electrode with a gate insulating film therebetween, an amorphous semiconductor film that covers a top face and side faces of the microcrystalline semiconductor film, and an impurity semiconductor film that is on the amorphous semiconductor film and added with one conductive type impurity element forming a source region and a drain region. The microcrystalline semiconductor film contains an impurity element to be a donor.SELECTED DRAWING: Figure 16
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a diode and a display device having the same. [Background technology]

[0002] In recent years, semiconductor thin films (thickness of several tens to several hundreds of nm) formed on substrates with insulating surfaces have been used. The technology for constructing thin-film transistors is attracting attention. It is widely used in electronic devices such as optical devices, especially as a switching element in image display devices. Development is being rushed.

[0003] Thin film transistors using amorphous semiconductor films are used as switching elements for image display devices. Thin film transistors using polycrystalline semiconductor films with crystal grain sizes of 100 nm or more are used. The method for forming a polycrystalline semiconductor film is to use a pulsed excimer laser beam through an optical system. The amorphous silicon film is then irradiated with a linear beam while being scanned to crystallize it. The technology is known.

[0004] In addition, as a switching element for an image display device, a fine crystal grain size of about 1 nm to 100 nm is used. Thin film transistors using a crystalline semiconductor film are used (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 4-242724 [Patent Document 2] JP 2005-49832 A Summary of the Invention [Problem to be solved by the invention]

[0006] A thin film transistor using a polycrystalline semiconductor film is a thin film transistor using an amorphous semiconductor film. The field effect mobility is two orders of magnitude higher than that of the conventional semiconductor display devices. However, the amorphous semiconductor film has the advantage that it can be integrally formed on the same substrate. Compared to the case where a semiconductor film is used, the process is complicated due to the crystallization of the semiconductor film, and the yield is accordingly reduced. However, there are problems with this, such as reduced availability and increased costs.

[0007] In addition, an inverted staggered thin film transistor using a microcrystalline semiconductor film for a channel formation region is Compared with an inverted staggered thin-film transistor that uses an amorphous semiconductor film in the channel formation region, It is possible to improve the on-current, but the off-current also increases. Display devices using high current thin film transistors suffer from poor contrast and high power consumption. There is also the problem of increased power consumption.

[0008] In view of the above problems, one object of the present invention is to reduce the off-current of a thin film transistor. Another object of the present invention is to reduce the reverse current of a diode. One of the objectives is to improve the image quality of the device. [Means for solving the problem]

[0009] One aspect of the present invention is to provide a gate electrode having a gate insulating film therebetween, the gate insulating film being formed on the gate electrode ... A microcrystalline semiconductor film provided in a side region and an amorphous semiconductor film covering an upper surface and a side surface of the microcrystalline semiconductor film. A semiconductor film and a conductive film in which a source region and a drain region are formed on the amorphous semiconductor film. and an impurity semiconductor film to which an impurity element having a conductivity type is added, The thin film transistor is characterized by containing an impurity element.

[0010] The ends of the microcrystalline semiconductor film on the source and drain region sides are made of an amorphous semiconductor film and an impurity semiconductor film. In addition, a part of the end of the microcrystalline semiconductor film may overlap with the source electrode or the drain electrode. The end of the amorphous semiconductor film may be covered with a source electrode and a drain electrode. The conductive layer may be exposed to the outside of the conductive electrode.

[0011] One aspect of the present invention is to provide a gate electrode having a gate insulating film therebetween, the gate insulating film being formed on the gate electrode ... A microcrystalline semiconductor film provided in a side region and to which an impurity element serving as a donor is added, An amorphous semiconductor film covering the top and side surfaces of the semiconductor film; and a source region on the amorphous semiconductor film. Alternatively, a drain region is formed by doping a semiconductor film with one conductivity type impurity element, and The gate electrode and the common line are connected to each other by a conductive film. It is a diode that is used

[0012] One aspect of the present invention is to provide a gate electrode having a gate insulating film therebetween, the gate insulating film being formed on the gate electrode ... A microcrystalline semiconductor film provided in a side region and to which an impurity element serving as a donor is added, An amorphous semiconductor film covering the top and side surfaces of the semiconductor film; and a source region on the amorphous semiconductor film. Alternatively, a drain region is formed by doping a semiconductor film with one conductivity type impurity element, and The gate electrode and the common line are connected to the first conductive film. The amorphous semiconductor film or the microcrystalline semiconductor film and the common line are connected by a second conductive film. It is a diode that can be used

[0013] The end portion of the microcrystalline semiconductor film on the source region or drain region side is made of an amorphous semiconductor film. The amorphous semiconductor film may overlap with the pure semiconductor film. The end of the amorphous semiconductor film may be covered by the source electrode or the drain electrode. The drain electrode may be exposed to the outside.

[0014] In the present invention, an amorphous semiconductor film may be provided so as to overlap the microcrystalline semiconductor film.

[0015] In the present invention, the microcrystalline semiconductor film may be a microcrystalline silicon film, a microcrystalline germanium film, Alternatively, the microcrystalline semiconductor film may be a microcrystalline silicon germanium film. The semiconductor device may have a laminated structure of a silicon film and a microcrystalline germanium film. The structure is composed of crystal grains doped with donor impurity elements and a germanium film covering the crystal grains. Alternatively, an amorphous germanium film or an amorphous silicon film may be used instead of the microcrystalline semiconductor film. A con-germanium film may also be used.

[0016] The impurity element serving as a donor is phosphorus, arsenic, or antimony.

[0017] In addition, a thin film transistor (TFT) using a microcrystalline semiconductor film in the channel formation region is used as a pixel region. The microcrystalline semiconductor film of the present invention is used in a gate insulating film, and further in a driver circuit to manufacture a display device. Since the crystallinity at the interface with the insulating film is high, a thin film transistor using the microcrystalline semiconductor film has a field effect mobility of 2.5 to 10 cm 2 / V·sec and amorphous semiconductor film Since it has a field effect mobility 5 to 20 times that of thin film transistors, it can be used as part of a driving circuit or The entire display can be integrated with the pixel section on the same substrate to form a system-on-panel. do.

[0018] The display device includes a light-emitting device and a liquid crystal display device. A light-emitting device includes a light-emitting element, The liquid crystal display device includes a liquid crystal element. The light-emitting element has a luminance controlled by a current or a voltage. This category includes elements, specifically organic electroluminescence (EL) and inorganic Includes electroluminescence (EL).

[0019] The display device includes a panel in which a display element is sealed, and a controller for the panel. The display device also includes a module in which an IC or the like including the display device is mounted. Regarding an element substrate corresponding to one form before a display element is completed in the process of manufacturing a device, The element substrate includes means for supplying a current to a display element for each of a plurality of pixels. Specifically, the display element may be in a state where only the pixel electrodes of the display element are formed, or the pixel electrodes This is the state after the conductive film to be formed is formed and before the pixel electrode is formed by etching. Any form is acceptable.

[0020] In this specification, the term "display device" refers to an image display device, a light-emitting device, or a light Also refers to connectors, such as FPC (Flexible Printed Circuit). inted circuit) or TAB (Tape Automated Bon ding tape or TCP (Tape Carrier Package) is used. Modules with printed wiring boards attached to the ends of TAB tape or TCP or the display element is mounted with an IC (integrated circuit) by the COG (Chip On Glass) method. The display device also includes all modules in which a display circuit (or other circuit) is directly mounted. Effect of the Invention

[0021] According to the present invention, the off-current of a thin film transistor can be reduced. It is possible to fabricate a thin film transistor having high field effect mobility and reduced off-current. In addition, the reverse current of the diode can be reduced. It is possible to fabricate diodes with high switching speeds, which improves the image quality of display devices. can be improved. [Brief description of the drawings]

[0022] [Figure 1] 1A to 1C are cross-sectional views illustrating a manufacturing process of a thin film transistor of the present invention. [Diagram 2] 1A to 1C are cross-sectional views illustrating a manufacturing process of a thin film transistor of the present invention. [Diagram 3] 1A to 1C are cross-sectional views illustrating a manufacturing process of a thin film transistor of the present invention. [Figure 4] 1A to 1C are cross-sectional views illustrating a manufacturing process of a thin film transistor of the present invention. [Diagram 5] 1A to 1C are plan views illustrating a manufacturing process of a thin film transistor of the present invention. [Figure 6] 1A to 1C are cross-sectional views illustrating a manufacturing process of a thin film transistor of the present invention. [Figure 7] 1A and 1B are diagrams illustrating a multi-tone mask that can be applied to the present invention. [Figure 8] 1A to 1C are cross-sectional views illustrating a manufacturing process of a thin film transistor of the present invention. [Figure 9] 1A to 1C are plan views illustrating a manufacturing process of a thin film transistor of the present invention. [Figure 10] FIG. 2 is a cross-sectional view illustrating a thin film transistor of the present invention. [Figure 11] FIG. 2 is a cross-sectional view illustrating a thin film transistor of the present invention. [Figure 12] 1A and 1B are a plan view and a cross-sectional view illustrating a diode according to the present invention. [Figure 13] 1A and 1B are a plan view and a cross-sectional view illustrating a diode according to the present invention. [Figure 14] FIG. 2 is a plan view illustrating an element substrate of the present invention. [Figure 15] FIG. 2 is a plan view illustrating a diode according to the present invention. [Figure 16] FIG. 2 is a cross-sectional view illustrating a diode according to the present invention. [Figure 17] 1A to 1C are cross-sectional views illustrating a manufacturing process of a diode according to the present invention. [Figure 18] FIG. 2 is a cross-sectional view illustrating a diode according to the present invention. [Figure 19] 1A to 1C are cross-sectional views illustrating a manufacturing process of a diode according to the present invention. [Figure 20] FIG. 2 is a plan view illustrating a diode according to the present invention. [Figure 21] FIG. 2 is a cross-sectional view illustrating a diode according to the present invention. [Figure 22] 1A to 1C are cross-sectional views illustrating a manufacturing process of a diode according to the present invention. [Diagram 23] FIG. 1 is a diagram showing a configuration of a plasma CVD apparatus applicable to the present invention. [Figure 24] FIG. 1 is a diagram showing a configuration of a plasma CVD apparatus applicable to the present invention. [Diagram 25] 1 is a diagram showing the configuration of a plasma CVD apparatus applicable to the present invention and a film formation procedure. [Figure 26] FIG. 1 is a plan view illustrating a display device of the present invention. [Figure 27] FIG. 2 is a cross-sectional view illustrating a terminal portion and a pixel portion of the display device of the present invention. [Figure 28] FIG. 1 is a cross-sectional view illustrating a display device of the present invention. [Figure 29] FIG. 2 is a top view illustrating a display device of the present invention. [Diagram 30] FIG. 2 is a top view illustrating a display device of the present invention. [Diagram 31] 1A and 1B are a cross-sectional view and a top view illustrating a display device of the present invention. [Diagram 32] FIG. 1 is a perspective view illustrating a display panel of the present invention. [Diagram 33] FIG. 1 is a perspective view illustrating an electronic device using a display device of the present invention. [Diagram 34] 1A to 1C are diagrams illustrating electronic devices using a display device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The present invention will be described below with reference to the drawings. The present invention is not limited to the above, and various forms and details may be used without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that the present invention can be modified in various ways. The present invention is not limited to the description of the embodiments. In the drawings, the same reference numerals are used to refer to the same parts.

[0024] (Embodiment 1) In this embodiment, a thin film transistor having high mobility, high on-state current and low off-state current is The manufacturing process is described below. In this embodiment, the element substrate 1 of the display device shown in FIG. In the top view of 300, a thin film transistor formed in each pixel of a pixel portion 1331, The manufacturing steps of the electrodes and the capacitor element will be described below.

[0025] Enlarged view of a region where a thin film transistor and a pixel electrode of one pixel of the pixel section 1331 in FIG. 14 are connected 5, cross-sectional views of QR in FIG. 5 are shown in FIGS. 1 to 3, and a cross-sectional view of ST is shown in FIG. show.

[0026] As shown in FIG. 1A, a gate electrode 51 and a capacitance wiring 56 are formed on a substrate 50. Gate insulating films 52 a and 52 b are formed on the electrode 51 and the capacitance wiring 56 .

[0027] The substrate 50 may be made of barium borosilicate glass, aluminoborosilicate glass, or aluminoborosilicate glass. Non-alkali glass substrates such as silicate glass, produced by the fusion method or float method In addition to ceramic substrates, plastic substrates that are heat-resistant and can withstand the processing temperatures of this manufacturing process are also available. Alternatively, a metal substrate such as a stainless steel alloy may be provided with an insulating film on its surface. A substrate having such a structure may also be used.

[0028] The gate electrode 51 and the capacitance wiring 56 are formed by sputtering, CVD, plating, printing, liquid crystal display, or the like. The conductive film is formed by a droplet discharge method or the like. Here, a molybdenum film is formed on the substrate 50 as a conductive film. The first photomask was used to form a resist mask, and the second photomask was used to form a resist mask. The conductive film formed on the substrate 50 is then etched to form the gate electrode 51 and the capacitance wiring 56. do.

[0029] The gate electrode 51 is made of a metal material. Examples of the metal material include aluminum, chromium, titanium, and the like. The gate electrode 51 is preferably made of aluminum. The barrier metal is a laminated structure of tungsten or aluminum. For the barrier metal, titanium, molybdenum, chromium, and other high melting point metals are used. It is preferable to provide this in order to prevent hillocks and oxidation of the aluminum.

[0030] The gate electrode 51 is formed to a thickness of 50 nm or more and 300 nm or less. By setting the thickness to 50 nm or more and 100 nm or less, the microcrystalline germanium film and wiring that will be formed later can be easily formed. In addition, the thickness of the gate electrode 51 is set to 150 nm or more and 300 nm or less. By making the gate electrode 51 lower, the resistivity of the gate electrode 51 can be reduced, and the area can be increased. It is.

[0031] Since a microcrystalline semiconductor film and wiring are formed on the gate electrode 51, the edge of the gate electrode 51 is cut to prevent a step. It is desirable to process the part so that it has a tapered shape. Wiring lines connected to the port electrodes, capacitance wiring lines, common lines, etc. can also be formed at the same time.

[0032] The gate insulating films 52a and 52b are each formed to a thickness of 1000 nm by using a CVD method, a sputtering method, or the like. Silicon oxide film, silicon nitride film, silicon oxynitride film, or silicon oxynitride film with a thickness of 50 to 150 nm In this embodiment, the gate insulating film 52a is a silicon nitride film or a nitride oxide film. A silicon film is formed, and a silicon oxide film or a silicon oxynitride film is formed as a gate insulating film 52b. The gate insulating film is not a two-layered film, but a silicon oxide film and a silicon nitride film are stacked. The insulating film can be formed of a single layer of a silicon nitride film, a silicon oxynitride film, or a silicon nitride oxide film. Moreover, the gate insulating film can have a three-layer structure using the above insulating films.

[0033] The gate insulating film 52a is formed using a silicon nitride film or a silicon oxynitride film. The adhesion between the gate insulating film 52a and the substrate 50 is increased. When a glass substrate is used as the substrate 50, It is possible to prevent impurities from the substrate 50 from diffusing into the microcrystalline semiconductor film, and further In addition, it is possible to prevent the gate electrode 51 from being oxidized. This can improve the electrical characteristics of the thin film transistor that will be formed later. When the insulating films 52a and 52b each have a thickness of 50 nm or more, the gate electrode 51 is not easily damaged due to its unevenness. This is preferable because it is possible to alleviate the reduction in coverage caused by the above-mentioned method.

[0034] Here, the silicon oxynitride film is a film whose composition contains more oxygen than nitrogen. Rutherford Backscattering (RBS) Scattering Spectrometry (HSS) and Hydrogen Forward Scattering Spectroscopy (HFS) n Forward Scattering (FSc) measurement, the composition range is Oxygen 50-70 atomic %, Nitrogen 0.5-15 atomic %, Silicon 25-35 atomic %, Water The term "silicon oxynitride film" refers to a film containing 0.1 to 10 atomic percent of silicon. The composition is such that the nitrogen content is greater than the oxygen content, and the measured values ​​are When the composition is determined, the oxygen content is 5 to 30 atomic percent, the nitrogen content is 20 to 55 atomic percent, and the silicon content is 10 to 15 atomic percent. The atomic percentage of oxygen is 25-35% and the atomic percentage of hydrogen is 10-30%. When the total atoms constituting silicon nitride or silicon oxynitride is taken as 100 atomic % The content ratios of nitrogen, oxygen, silicon and hydrogen are within the above ranges.

[0035] Next, a microcrystalline semiconductor film 45 containing an impurity element serving as a donor is formed on the gate insulating film 52b. The microcrystalline semiconductor film 58 containing an impurity element serving as a donor may include phosphorus, arsenic, tantalum, etc. Microcrystalline silicon film, microcrystalline germanium film, which contain impurity elements such as tungsten as donors, Examples include microcrystalline silicon germanium.

[0036] The microcrystalline semiconductor film here is an intermediate structure between amorphous and crystalline structures (including single crystal and polycrystalline). The semiconductor has a third state that is stable in terms of free energy. It is a semiconductor that has a short-range order and lattice distortion and is crystalline, with a grain size of 0. Columnar or needle-like crystals of 5 to 20 nm are grown in the normal direction to the substrate surface. A non-single-crystal semiconductor exists between multiple microcrystalline semiconductors. This is a typical example of a microcrystalline semiconductor. Microcrystalline silicon has a Raman spectrum of 520 cm, which is indicative of single-crystalline silicon. -1 than The wave number shifts to the lower side. That is, the wave number at 520 cm indicates single crystal silicon. -1 and Amorpha Silicone showing 480cm -1 The Raman spectrum of microcrystalline silicon has a peak between In addition, hydrogen or halogen is reduced to terminate dangling bonds. Each of these elements contains 1 atomic percent or more of helium, argon, krypton, By adding rare gas elements such as neon, the lattice distortion is further promoted, resulting in increased stability and good performance. Such a microcrystalline semiconductor film can be obtained by, for example, This is disclosed in Japanese Patent No. 4,409,134.

[0037] The thickness of the microcrystalline semiconductor film 58 containing the impurity element serving as a donor is 1 nm or more and 200 nm or less. , preferably 1 nm or more and 100 nm or less, preferably 1 nm or more and 50 nm or less, The thickness of the microcrystalline semiconductor film containing an impurity element serving as a donor is 10 nm or more and 25 nm or less. By setting the thickness of 58 to 1 nm or more and 50 nm or less, a fully depleted thin film transistor can be created. It can be manufactured.

[0038] The concentration of the impurity element serving as a donor contained in the microcrystalline semiconductor film is 6×10 15 cm -3 End 3×10 18 cm -3Less than or equal to 1×10 16 cm -3 More than 3×10 18 cm -3 Less than or equal to 3×10 16 cm -3 More than 3×10 17 cm -3 The following is a description of the microcrystalline By setting the concentration of the impurity element that serves as a donor contained in the conductive film 58 within the above range, It is possible to improve the crystallinity at the interface between the insulating film 52b and the microcrystalline semiconductor film 58. Since the resistivity of the microcrystalline semiconductor film 58 can be reduced, the field effect mobility is high. In addition, a thin film transistor having a high on-state current can be manufactured. The peak concentration of donor impurity elements in the 15 cm -3 If it is less than that, Donna The amount of impurity elements that act as a barrier is insufficient, and an increase in field effect mobility and on-current cannot be expected. In addition, the peak concentration of the impurity element serving as a donor contained in the microcrystalline semiconductor film is set to 3×10 18 c m -3 If the gate voltage is set to be larger than 100V, the threshold voltage will shift to the negative side of the gate voltage, In order to prevent transistor operation, the donor impurity concentration is 6×10 15 cm -3 More than 3×10 18 cm -3 Less than or equal to 1×10 16 cm -3 More than 3×10 18 cm -3 Less than or equal to 3×10 16 cm -3 More than 3×10 17 cm -3 Below It is preferable that

[0039] The oxygen concentration and the nitrogen concentration of the microcrystalline semiconductor film 58 including the impurity element serving as a donor are Less than 10 times the concentration of the donor impurity element, typically 3×10 19 atoms / cm 3 less than 3×10 18 atoms / cm 3 Less than 3×10 carbon concentration 1 8 atoms / cm 3 It is preferable that oxygen, nitrogen, and carbon are contained in the microcrystalline semiconductor. By reducing the concentration of impurity elements mixed in the film, the microcrystalline semiconductor film 58 containing the impurity elements serving as donors can be formed. Furthermore, the generation of defects in the microcrystalline semiconductor film can be suppressed. Therefore, the crystallization of the microcrystalline semiconductor containing the impurity element that acts as a donor is difficult. The oxygen concentration or nitrogen concentration in the film 58 is relatively low, and impurity elements that act as donors are included. By this, the crystallinity of the microcrystalline semiconductor film 58 containing the impurity element serving as a donor can be improved. can.

[0040] In addition, the microcrystalline semiconductor film 58 containing the impurity element serving as a donor in this embodiment mode has a Since the microcrystalline semiconductor film 58 containing the impurity element serving as a donor is By adding an impurity element that acts as an acceptor to the film during or after the film formation, It is possible to control the threshold voltage. The typical impurity elements that act as acceptors are The most preferred is boron, and impurity gases such as B2H6 and BF3 are preferably in the range of 1 ppm to 1000 ppm. It is advisable to mix boron into silicon hydride at a ratio of 1 to 100 ppm. The concentration of boron is , about one tenth of the donor impurity element, for example, 1×10 14 ~6×10 16 ato ms / cm3 It would be better to say:

[0041] In a reaction chamber of a plasma CVD apparatus, a deposition gas containing silicon or germanium is and hydrogen are mixed, and the microcrystalline semiconductor film 45 is formed by glow discharge plasma. The flow rate of hydrogen is set to 10 to 2000 times the flow rate of deposition gas containing cation or germanium. The solution is diluted 50 to 200 times to form a microcrystalline semiconductor film. The reaction is carried out at 100° C. to 300° C., preferably 120° C. to 220° C. In addition, By mixing gases containing phosphorus, arsenic, antimony, etc., impurity elements that act as donors are added. Here, a microcrystalline semiconductor film containing silane, hydrogen, and / or rare gas can be formed. The mixture of silicon and phosphine was used to produce phosphorus-containing microcrystalline silicon by glow discharge plasma. A silicon film can be formed.

[0042] In the process of forming the microcrystalline semiconductor film 45 containing the impurity element serving as a donor, The generation of 3MHz to 30MHz, typically 13.56MHz, 27.12MHz High-frequency power in the VHF band, or high-frequency power in the VHF band from 30 MHz to about 300 MHz This is done by applying a power of, for example, 60 MHz. Alternatively, a high frequency plasma of 2.45 GHz can be used.

[0043] Representative examples of deposition gases containing silicon or germanium include SiH4, Si 2H6, GeH4, Ge2H6, etc.

[0044] Instead of forming the semiconductor film 47 containing the impurity element serving as a donor, A semiconductor film not containing pure elements is formed, and an impurity source serving as a donor is formed as the gate insulating film 52b. For example, an insulating film containing an impurity element (such as phosphorus, arsenic, or Silicon oxide film, silicon nitride film, silicon oxynitride film, or silicon nitride oxide film containing antimony In addition, when the gate insulating film 52b has a laminated structure, An impurity element that serves as a donor is added to the layer in contact with the crystalline semiconductor film 45 or the layer in contact with the substrate 50. You may do so.

[0045] As a method for forming the insulating film containing an impurity element serving as a donor as the gate insulating film 52b, If an insulating film is formed using a gas containing an impurity element that acts as a donor together with the raw material gas for the insulating film, For example, a plasma CVD method using silane, ammonia, and phosphine can be used. It is possible to form silicon nitride containing phosphorus. It is also possible to form silicon nitride containing phosphorus by using silane, nitrous oxide, and ammonia. Silicon oxynitride films containing phosphorus were fabricated by plasma CVD using niobium and phosphine. can be formed.

[0046] In addition, before the gate insulating film 52b is formed, an impurity source serving as a donor is placed in the reaction chamber of the film forming apparatus. A gas containing impurities is flowed to adsorb the impurity elements acting as donors onto the surface of the substrate 50 and the inner wall of the reaction chamber. Thereafter, the gate insulating film 52b is formed to remove the impurity element serving as a donor. Since the insulating film is deposited while the gate insulating film is being etched, it forms a gate insulating film containing impurity elements that act as donors. It is possible.

[0047] In addition, before the microcrystalline semiconductor film 45 containing the impurity element serving as a donor is formed, A gas containing an impurity element that serves as a donor is fed into the reaction chamber to form a gate insulating film 52b and a wall of the reaction chamber. An impurity element serving as a donor may be adsorbed on the semiconductor layer. Since the microcrystalline semiconductor film is deposited while incorporating the impurity element that becomes the donor, A microcrystalline semiconductor film 45 containing an impurity element can be formed.

[0048] In order to form a microcrystalline semiconductor film containing an impurity element serving as a donor, silicon or A fluoride gas containing silicon or germanium together with a deposition gas containing germanium In this case, the flow rate of silane fluoride is set to 0.1 to 50% of the flow rate of silane. The microcrystalline semiconductor film 45 containing an impurity element serving as a donor is To form a silicon or germanium oxide film, a deposition gas containing silicon or germanium is added to the silicon or germanium oxide film. By using a fluoride gas containing germanium, the crystal growth of the microcrystalline semiconductor film can be improved. The fluorine radicals etch the amorphous semiconductor components, resulting in high crystallinity and crystal growth. That is, a microcrystalline semiconductor film with high crystallinity can be formed.

[0049] In addition, germanium hydrides such as GeH4 and GeF4, and germanium fluorides, etc., are mixed in gases such as silane. Silicon germanium mixed to adjust the energy band width to 0.9-1.1 eV. Adding germanium to silicon improves the temperature characteristics of thin-film transistors. You can change your gender.

[0050] In addition, in the microcrystalline semiconductor film containing the impurity element serving as a donor in this embodiment mode, Because it contains impurity elements, the microcrystals function as the channel formation region of thin film transistors. For semiconductor films, impurity elements that become acceptors are added simultaneously with or after film formation. By adding impurity elements, it becomes possible to control the threshold voltage. The typical example is boron, and impurity gases such as B2H6 and BF3 are used at 1 ppm to 10 00 ppm, preferably 1 to 100 ppm, of silicon or germanium. The boron concentration is 10% of the donor impurity element. For example, 1×10 14 ~6×10 16 atoms / cm 3 It would be better to say:

[0051] In addition, in the deposition process of a microcrystalline semiconductor film containing an impurity element serving as a donor, silane and In addition to hydrogen, helium can be added to the reaction gas. Helium has an energy of 24.5 eV, which is higher than all other gases. It has the highest ionization energy of any of the four, about 2 Since there is a metastable state at the 0 eV level, the difference in ionization during the discharge is about 4 Therefore, the discharge start voltage is the lowest among all gases. Due to these characteristics, helium can maintain a stable plasma. Since it is possible to form a sma, a microcrystalline semiconductor film containing an impurity element that acts as a donor is deposited. Even if the area of ​​the substrate to be heated is large, the plasma density can be made uniform.

[0052] Next, the first buffer layer 54 is formed. The first buffer layer 54 is made of an amorphous The first buffer layer 54 is formed of a silicon film, an amorphous silicon germanium film, or the like. The thickness is 10 to 100 nm, preferably 30 to 50 nm.

[0053] The first buffer layer 54 is a plasma deposition layer using a deposition gas containing silicon or germanium. Amorphous semiconductor films can be formed by the Zuma CVD method. The deposition gas containing germanium is selected from helium, argon, krypton, and neon. The amorphous semiconductor film can be formed by diluting the gas with one or more rare gas elements. Alternatively, the flow rate of the silane gas is 1 to 10 times, more preferably 1 to 5 times. The hydrogen can be used to form an amorphous semiconductor film containing hydrogen. The semiconductor film may be doped with a halogen, such as fluorine, chlorine, bromine, or iodine.

[0054] The first buffer layer 54 is formed by ionizing the target with hydrogen, germanium, etc. Alternatively, an amorphous semiconductor film can be formed by sputtering with a rare gas.

[0055] A first buffer layer 54 is formed on a surface of the microcrystalline semiconductor film 45 containing an impurity element serving as a donor. By this method, an amorphous semiconductor film, and further an amorphous semiconductor film containing hydrogen, nitrogen, or halogen, can be formed. By this, the surface of the crystal grains included in the microcrystalline semiconductor film 45 containing the impurity element serving as a donor is It is possible to prevent natural oxidation, especially in the region where the amorphous semiconductor and the microcrystalline grains come into contact. When the cracks come into contact with oxygen, the grains are oxidized, and the However, the microcrystalline semiconductor film 45 containing the impurity element serving as a donor By forming the first buffer layer 54 on the surface, oxidation of the microcrystal grains can be prevented.

[0056] In addition, after forming the microcrystalline semiconductor film 45 containing the impurity element serving as a donor, plasma CVD It is preferable to form the first buffer layer 54 at a temperature of 300° C. to 400° C. by the method. By this film formation process, hydrogen is supplied to the microcrystalline semiconductor film 45, and the microcrystalline semiconductor film 45 is heated to 10 ... In other words, the effect is the same as that of a microcrystalline semiconductor that contains impurity elements that act as donors. By depositing a first buffer layer 54 on the semiconductor film 45, a semiconductor layer containing an impurity element that serves as a donor is formed. Hydrogen can be diffused into the microcrystalline semiconductor film 45 to terminate the dangling bonds. do.

[0057] Next, a resist is applied onto the first buffer layer 54 and the gate insulating film 52b, and a second photoresist is formed. The resist is exposed and developed in a photolithography process using a photomask to form a resist Next, the first buffer layer 54 and the dopant are formed using the resist mask. The microcrystalline semiconductor film 45 containing the impurity element serving as the donor is etched to obtain a semiconductor layer as shown in FIG. As shown in FIG. 1, the first buffer layer 62 and the microcrystalline semiconductor film 58 containing the impurity element serving as a donor are At this time, as shown in FIG. 4(A), a gate electrode 51 (gate wiring) and The area where the source wiring intersects is also made of a microcrystalline semiconductor containing an impurity element that acts as a donor. 5A. A solid film 59 and a first buffer layer 64 are formed. 4(A) corresponds to a cross-sectional view of ST in FIG. 5(A).

[0058] Next, as shown in FIG. 1C, a second layer is formed on the first buffer layer 62 and the gate insulating film 52b. The buffer layer 41 and the impurity semiconductor film 55 to which an impurity element imparting one conductivity type is added are Form.

[0059] The second buffer layer 41 can be formed in the same manner as the first buffer layer 54. The second buffer layer 41 at this time is used in the subsequent process of forming the source region and the drain region. In some cases, the second buffer layer 41 may be partially etched away, but at that time, a part of the second buffer layer 41 remains. It is preferable to form the film to a thickness of 30 nm or more and 500 nm or less. It is preferable to form the film with a thickness of 50 nm or more and 200 nm or less.

[0060] A display device that applies a high voltage (for example, about 15V) to a thin-film transistor, typically a liquid crystal display. In the display device, when the first buffer layer 54 and the second buffer layer 41 are formed thick, The source-drain breakdown voltage has increased, so even if a high voltage is applied to the gate voltage of a thin-film transistor, Therefore, the deterioration of the thin film transistor can be reduced.

[0061] The first buffer layer 54 and the second buffer layer 41 are formed using an amorphous semiconductor film. Alternatively, since the semiconductor film is formed of an amorphous semiconductor film containing hydrogen or halogen, the energy gap is The gap is larger than that of the microcrystalline semiconductor film 45 containing an impurity element, and the resistivity is high. The degree of the lattice structure is as low as 1 / 5 to 1 / 10 of that of the microcrystalline semiconductor film 45. In a transistor, a source region, a drain region, and a microcrystal containing an impurity element that acts as a donor are The first buffer layer and the second buffer layer formed between the crystalline semiconductor film 45 are high resistance regions. The microcrystalline semiconductor film 45 including the impurity element serving as a donor serves as a channel formation region. Therefore, the off-current of the thin film transistor can be reduced. When a thin-film transistor is used as a switching element of a display device, the contrast of the display device is This can improve performance.

[0062] The impurity semiconductor film 55 to which an impurity element that imparts one conductivity type is added is an n-channel thin film. When forming a transistor, phosphorus may be added as a typical impurity element. An impurity gas such as PH3 may be added to a deposition gas containing silicon or germanium. In addition, when forming a p-channel thin film transistor, a typical impurity element is Boron can be added to deposition gas containing silicon or germanium, such as B2H6. The impurity gas containing phosphorus or boron at a concentration of 1×10 19 ~1×10 21 cm -3 By doing so, ohmic contact with the wirings 71a to 71c is achieved. It is possible to provide a single conductivity type, which functions as a source region and a drain region. The impurity semiconductor film 55 to which the impurity element is added is a microcrystalline semiconductor film or an amorphous semiconductor film. The semiconductor film can be formed of an impurity semiconductor film to which an impurity element that imparts one conductivity type is added. The layer 55 is formed to a thickness of 2 nm to 50 nm. By thinning the thickness of the doped semiconductor film, the throughput can be improved. .

[0063] Next, a resist mask is formed on the impurity semiconductor film 55 to which an impurity element that imparts one conductivity type is added. The resist mask is formed by photolithography. Using a third photomask, a semiconductor doped with an impurity element that gives one conductivity type is The resist applied on the film 55 is exposed and developed to form a resist mask.

[0064] Next, the second buffer layer 41 and the impurity imparting one conductivity type are formed using a resist mask. The doped impurity semiconductor film 55 is etched and separated to form island-like The second buffer layer 42 and the impurity semiconductor film doped with an impurity element that imparts one conductivity type At this time, as shown in FIG. 4(B), the gate electrode (gate wiring) and the rear The second buffer layer 44 and the one-conductivity type are also formed in the region where the source wiring intersects with the first buffer layer 44. The impurity semiconductor film 65 is formed by adding the impurity element. FIG. 2(A) corresponds to a cross-sectional view of QR in FIG. 5(B), and FIG. corresponds to a cross-sectional view of ST in FIG.

[0065] The second buffer layer 42 covers the microcrystalline semiconductor film 58 containing the impurity element serving as a donor. As a result, the microcrystalline semiconductor film 58 including the impurity element serving as a donor is connected to a wiring to be formed later. Therefore, the wiring formed on the first buffer layer 62 and the microcrystalline semiconductor film 58 are not formed. It is possible to reduce the leakage current.

[0066] Next, as shown in FIG. 2(B), an impurity semiconductor is formed by doping an impurity element that gives one conductivity type. Conductive films 65a to 65c are formed on the body film 63 and the gate insulating film 52b. 65c is formed by using a sputtering method, a CVD method, a printing method, a droplet ejection method, a deposition method, or the like. do.

[0067] The conductive films 65a to 65c are made of aluminum, copper, silicon, titanium, neodymium, or tin. Addition of heat-resistant elements such as candium and molybdenum or hillock prevention elements It is preferable to form the conductive layer by a single layer or a multilayer of an aluminum alloy. The film on the side in contact with the source region and drain region 72 to which the impurity element is added is made of titanium, tantalum, etc. The material is made of tantalum, molybdenum, tungsten, or a nitride of these elements, and aluminum is then applied to the surface. A laminated structure of aluminum or an aluminum alloy may be used. The upper and lower surfaces of aluminum or aluminum alloy are coated with titanium, tantalum, molybdenum, tungsten, The conductive film may have a laminated structure in which the conductive film is sandwiched between a conductive film and a nitride of the conductive film. The wiring 71a and 71c are laminated in three layers. The structure uses an aluminum film for the conductive film 71b, and titanium for the wiring 71a and 71c. 7 shows a structure in which an aluminum film is used for the conductive film 71b.

[0068] Next, a photolithography process is performed using a fourth photomask on the conductive film 65c. Forms a gyst mask.

[0069] Next, the conductive films 65a to 65c are etched using a resist mask to form the conductive films 65a to 65c shown in FIG. As shown in FIG. 1, a pair of wirings 71a to 71c (functioning as a source electrode and a drain electrode) , forming capacitance electrodes 71d to 71f.

[0070] At this time, as shown in FIG. 4C, the second buffer layer 44 and the non-insulating layer for imparting one conductivity type are An impurity semiconductor film 65 to which a pure element is added, a microcrystalline semiconductor containing an impurity element serving as a donor The gate electrode 51 (gate wiring) and the wiring 71a are connected via the film 59 and the first buffer layer 64. Therefore, the gate electrode 51 (gate wiring) and the wirings 71a to 71c intersect. This can reduce the parasitic capacitance in the intersecting region.

[0071] Next, a resist mask is used to form a semiconductor layer doped with an impurity element that provides one conductivity type. The film 63 is etched and separated. As a result, a pair of source regions are formed as shown in FIG. In this etching process, the first and second regions 72 can be formed. A part of the buffer layer 42 of the second substrate 41 is also etched. The second buffer layer is referred to as a second buffer layer 43. The step of forming the recess in the second buffer layer and the step of forming the recess in the second buffer layer can be performed in the same step. The depth of the recess of 43 is set to 1 / 2 to 1 / 3 of the thickness of the thickest region of the second buffer layer 43. By doing so, it is possible to separate the source and drain regions. The leakage current between the gate and drain regions can be reduced. Remove.

[0072] Next, the exposed second buffer layer 43 is subjected to a heat treatment so that the exposed second buffer layer 43 is not damaged and the second buffer layer Dry etching may be performed under conditions where the etching rate for 43 is low. As a result, the etching residue on the second buffer layer 43 between the source region and the drain region, the resist Residues from resist masks and contamination sources in the equipment used to remove resist masks can be removed. This makes it possible to ensure the insulation between the source and drain regions. As a result, it is possible to reduce the leakage current of the thin film transistor and the off-current is small. It is possible to fabricate a thin film transistor with high breakdown voltage. For example, chlorine gas may be used.

[0073] Through the above steps, a channel-etch type thin film transistor 74 can be formed.

[0074] FIG. 2(C) corresponds to a cross-sectional view of QR in FIG. 5(C), and FIG. 4(C) corresponds to a cross-sectional view of QR in FIG. 5(C). As shown in FIG. 5C, the source and drain regions 72 It can be seen that the end of the wiring 71c is located outside the end of the wiring 71c. The microcrystalline semiconductor film, the first buffer layer 64, the second buffer layer 44, and the first conductive type are Since the wiring is overlapped with the impurity semiconductor film 65 to which the impurity element is added, The effect of unevenness on the gate electrode is small, and the coverage rate and leakage current can be reduced.

[0075] Next, as shown in FIG. 3A, the wirings 71a to 71c, the source region and the drain region 72 A protective insulating film 76 is formed on the second buffer layer 43 and the gate insulating film 52b. The insulating film 76 can be formed in the same manner as the gate insulating films 52a and 52b. The insulating film 76 prevents the intrusion of contaminating impurities such as organic matter, metal matter, and water vapor suspended in the air. In order to prevent this, a dense film is preferable. As a result, the oxygen concentration in the second buffer layer 43 is set to 5×10 19 atoms / cm 3 The following are the preferred Or 1×10 19 atoms / cm 3 The second buffer layer 43 may be It is possible to prevent oxidation.

[0076] Next, an insulating film 101 is formed on the protective insulating film 76. Here, a photosensitive organic resin is used. Then, the insulating film 101 is exposed to light using a fifth photomask. Then, development is performed to form the insulating film 102 that exposes the protective insulating film 76. 2 to etch the protective insulating film 76, so that one of the wirings 71c is A contact hole 111 exposing the capacitor electrode 71f and a contact hole 112 exposing the capacitor electrode 71f Form 12.

[0077] Next, as shown in FIG. 3C, the wiring 71c and the capacitor are inserted into the contact holes 111 and 112. A pixel electrode 77 is formed in contact with the capacitance electrode 71f. The capacitance electrodes 71d to 71f and the pixel electrode 77 form a capacitance element 106. In this example, after a conductive film is formed on the insulating film 102, a photolithography process is performed using a sixth photomask. The conductive film is etched using a resist mask formed by a lithography process to form a pixel electrode. Forming pole 77.

[0078] The pixel electrode 77 is made of indium oxide containing tungsten oxide, indium oxide containing tungsten oxide, Indium zinc oxide, Indium oxide with titanium oxide, Indium with titanium oxide Tin oxide, indium tin oxide, indium zinc oxide, indium doped with silicon oxide A light-transmitting conductive material such as tin oxide can be used.

[0079] The pixel electrode 77 is made of a conductive composition containing a conductive polymer. The pixel electrode formed by using the conductive composition can be formed by using a sheet resistor. It is preferable that the resistance is 10,000Ω / □ or less and the light transmittance at a wavelength of 550 nm is 70% or more. It is preferable that the resistivity of the conductive polymer contained in the conductive composition is 0.1 Ω cm or less. It is preferable that

[0080] As the conductive polymer, a so-called π-electron conjugated conductive polymer can be used. For example, polyaniline or its derivatives, polypyrrole or its derivatives, polythiophene or or a derivative thereof, or a copolymer of two or more of these.

[0081] Here, the pixel electrode 77 is formed by forming an ITO film by a sputtering method, and then the ITO A resist is applied on the top. Next, the resist is exposed and developed using a sixth photomask. Then, a resist mask is formed. Next, the ITO is etched using the resist mask to form a pattern. The element electrodes 77 are formed.

[0082] In this manner, a thin film transistor can be formed. A device substrate capable of being formed can be formed.

[0083] The channel formation region of the thin film transistor manufactured in this embodiment mode is formed using a microcrystalline semiconductor film. Therefore, it is possible to increase the driving frequency of the display device, and the panel size can be increased. It can also be used to increase the area and density of pixels. The thin film transistor can be fabricated.

[0084] In addition, a buffer layer is provided between the microcrystalline semiconductor film containing the impurity element serving as a donor and the wiring. Therefore, leakage current between the microcrystalline semiconductor film containing the impurity element serving as a donor and the wiring is reduced. The current can be reduced. Also, the source and drain regions and impurities acting as donors can be A buffer layer formed of an amorphous semiconductor film is provided between the microcrystalline semiconductor films containing an organic element. Therefore, the buffer layer becomes a high resistance region, and the leakage current can be reduced. Therefore, a thin film transistor having excellent electrical characteristics and high reliability can be manufactured.

[0085] In this embodiment mode, a channel-etched thin film transistor is used. This embodiment mode can be applied to a panel-protected thin film transistor.

[0086] (Embodiment 2) In the present embodiment, the number of photomasks can be reduced compared to the first embodiment. The process for manufacturing a thin film transistor will be described.

[0087] As in the first embodiment, as shown in FIG. 6(A), a conductive film is formed on a substrate 50. A resist is applied on the top and formed by a photolithography process using a first photomask. The conductive film is partially etched using the resist mask to form the gate electrode 51 and the capacitance wiring Next, on the gate electrode 51, gate insulating films 52a and 52b are formed. Next, a photolithography process using a second photomask is performed on the gate insulating film 52b. The microcrystalline semiconductor film 58 containing an impurity element serving as a donor and the first buffer layer 62 are formed using the above-mentioned method. Next, a second buffer layer 41, which is a first conductive type, is formed on the first buffer layer 62. The impurity semiconductor film 55 to which the impurity element to be added is added and the conductive films 65a to 65c are formed in order. Next, a resist is applied onto the conductive film 65a.

[0088] The resist may be a positive resist or a negative resist. This is shown using a di-type resist.

[0089] Next, a multi-tone mask is used as a third photomask to irradiate the resist with light. The photoresist is exposed to light to form a resist mask 81.

[0090] Here, exposure using a multi-tone mask will be described with reference to FIG.

[0091] A multi-tone mask has three exposure levels for the exposed, intermediate and unexposed parts. This is a mask that can produce multiple (typically two types) It is possible to form a resist mask having a region of thickness of 100 nm or more. By using this mask, it is possible to reduce the number of photomasks.

[0092] A typical example of a multi-tone mask is a gray-tone mask 159a as shown in FIG. There is a half-tone mask 159b as shown in FIG.

[0093] As shown in FIG. 7A, the gray-tone mask 159a is made of a light-transmitting substrate 163 and The light shielding portion 164 and the diffraction grating 165 are formed on the light shielding portion 164. On the other hand, the diffraction grating 165 has slits, dots, meshes, etc. By making the intervals between the light transmitting portions such as the slits equal to or less than the resolution limit of the light used for exposure, The diffraction grating 165 can control the light transmittance of the slits and dots. , meshes, or non-periodic slits, dots, meshes can be used. .

[0094] The light-transmitting substrate 163 may be a light-transmitting substrate such as quartz. The portion 164 and the diffraction grating 165 are made of a light-shielding material that absorbs light, such as chromium or chromium oxide. It can be formed.

[0095] When the gray-tone mask 159a is irradiated with exposure light, as shown in FIG. In the case of 164, the light transmittance 166 is 0%, and the light shielding portion 164 and the diffraction grating 165 are provided. In the unshaded area, the light transmittance 166 is 100%. The light transmittance 166 of the diffraction grating 165 can be adjusted in the range of 10 to 70%. The adjustment can be achieved by adjusting the spacing and pitch of the slits, dots, or meshes of the diffraction grating. It is Noh.

[0096] As shown in FIG. 7C, the half-tone mask 159b is disposed on a light-transmitting substrate 163 and The semi-transmitting portion 167 and the light-shielding portion 168 are formed on the semi-transmitting portion 167. MoSiN, MoSi, MoSiO, MoSiON, CrSi, etc. can be used. The light shielding portion 168 is formed using a light shielding material that absorbs light, such as chromium or chromium oxide. It is possible.

[0097] When the halftone mask 159b is irradiated with exposure light, as shown in FIG. In the case of 168, the light transmittance 169 is 0%, and the light shielding portion 168 and the semi-transmitting portion 167 are provided. In the unshaded area, the light transmittance 169 is 100%. The light transmittance 169 of the semi-transparent portion 167 can be adjusted in the range of 10 to 70%. The adjustment is possible by adjusting the material of the semi-transmissive portion 167 .

[0098] By exposing the film using a multi-tone mask and then developing it, the film thickness can be varied as shown in FIG. 6(A). A resist mask 81 having a region can be formed.

[0099] Next, the second buffer layer 41 and the impurity source for imparting one conductivity type are formed by using a resist mask 81. The impurity semiconductor film 55 to which oxygen is added and the conductive films 65a to 65c are etched and separated. As a result, as shown in FIG. 6B, the second buffer layer 42 is formed of impurities that impart one conductivity type. The impurity semiconductor film 63 to which an impurity element is added and the conductive films 85a to 85c can be formed. FIG. 6A (excluding the resist mask 81) shows the same structure as that shown in FIG. 9A in the UV light. This corresponds to a cross-sectional view.

[0100] Next, the resist mask 81 is ashed. As a result, the area of ​​the resist is reduced and the thickness At this time, the resist in the thin region (the region overlapping a part of the gate electrode 51) The resist mask 86 is then removed to form a separate resist mask 86, as shown in FIG. 6(C). This can be done.

[0101] Next, the conductive films 85a to 85c are etched and separated using the resist mask 86. As a result, a pair of wirings 92a to 92c as shown in FIG. 8(A) can be formed. When the conductive films 89a to 89c are wet-etched using the resist mask 86, As a result, the areas 89a to 89c are etched away from the resist mask 86. Narrow wirings 92a to 92c can be formed.

[0102] Next, as shown in FIG. 8B, a resist mask 86 is used to remove impurities that impart one conductivity type. The impurity semiconductor film 63 to which the impurity element is added is etched to form a pair of source and drain regions. In this etching process, a portion of the second buffer layer 42 is The partially etched second buffer layer is then removed to form second buffer layer 87. The second buffer layer 87 has a recess formed therein. The step of forming the region and the recess of the second buffer layer can be performed in the same step. In this case, a part of the second buffer layer 87 is a resist mask having a reduced area compared to the resist mask 81. Since the mask 86 is partially etched, the source and drain regions 88 are not exposed. The second buffer layer 87 has a protruding shape. The ends of the source region and the drain region 88 are not aligned but are shifted. On the outside, the ends of the source and drain regions 88 are formed. After this, a resist mask 86 is removed. Note that FIG. 8B corresponds to a UV cross-sectional view of FIG. 9B.

[0103] Next, the exposed buffer layer is etched without being damaged and without being etched. This step may be performed by dry etching under low grade conditions. Etching residues on the buffer layer between the rain regions, resist mask residues, and resist It is possible to remove the contamination sources in the equipment used to remove the mask, and the source and drain regions As a result, the lead of the thin film transistor can be prevented from being damaged. It is possible to reduce the off-state current, and to create a thin film transistor with a small off-state current and high voltage resistance. It is possible to fabricate the semiconductor device using the above-mentioned method. For example, chlorine gas may be used as the etching gas.

[0104] Through the above steps, a channel-etch type thin film transistor 83 can be formed. Moreover, a thin film transistor can be formed using two photomasks.

[0105] After that, through the same process as in the first embodiment, the wirings 92a to 92b are formed as shown in FIG. c, the source region and drain region 88, the second buffer layer 87, and the gate insulating film 52b A protective insulating film and an insulating film are formed on top, and a photolithography process is performed using a fourth photomask. In this case, the protective insulating film is formed as a protective insulating film 76a. This indicates that.

[0106] At this time, the gate insulating film 52b and the protective insulating film 76a are formed of films having different etching selectivity. For example, the gate insulating film 52b is formed of a silicon oxynitride film, and the protective insulating film 76a is formed of a silicon nitride film. The protective insulating film 76a is formed of a base film. Etching for forming a contact hole on the capacitance wiring 56 is stopped at the gate insulating film 52b. Therefore, the capacitance element is formed by the capacitance wiring 56, the gate insulating films 52a and 52b, and and pixel electrode 77.

[0107] In addition, the gate insulating film 52b and the protective insulating film 76a are formed of the same material. a and the gate insulating film 52b are formed with films having different etching selectivity (for example, the gate insulating film The film 52b and the protective insulating film 76a are formed of a silicon nitride film, and the gate insulating film 52a is formed of a silicon oxynitride film. The protective insulating film 76a and the gate insulating film 52b are selectively etched. By using the conditions for forming the contact hole on the capacitance wiring 56, the etching is performed in the gate Therefore, the capacitance element can be formed by the capacitance wiring 56, the gate insulating film 52a, and the like. The capacitance element can be formed of two conductive layers. An insulating film (here, a gate insulating film) between a film (here, a capacitance wiring 56 and a pixel electrode 77) The thinner the film thickness of 52a), the higher the capacity that can be carried, and therefore, it is preferable.

[0108] Next, a pattern is formed on the insulating film 102 by a photolithography process using a fifth photomask. The element electrode 77 can be formed. Note that FIG. 8(C) is a UV cross-sectional view of FIG. 9(C). is equivalent to.

[0109] In the above manner, a thin film transistor can be manufactured. A device substrate capable of being formed can be formed.

[0110] By the above process, it is possible to reduce the number of photomasks by one compared to the first embodiment. By the above process, an element substrate having a thin film transistor and capable of being used in a display device is formed. It is possible.

[0111] (Embodiment 3) In this embodiment, a thin film transistor different from those in the first and second embodiments will be described. The following are the reasons for this:

[0112] FIG. 10 is a diagram showing an impurity serving as a donor in the thin film transistor shown in the first embodiment and the second embodiment. Instead of the microcrystalline semiconductor film containing the element, an impurity element serving as a donor is formed on the gate insulating film 52b. The crystal grains 60 containing the impurity element serving as a donor and the gate insulating A thin film transistor having a semiconductor film 61 mainly composed of germanium covering the film 52b. The shape of the semiconductor film 61 is also shown. The germanium layer 43 is formed. Since the semiconductor film 61 mainly made of germanium has a higher mobility, the carriers are mainly made of germanium. Therefore, the gate insulating film 52b is formed on the semiconductor film 61. The semiconductor film 61 mainly composed of ruthenium is used as a channel forming region of a thin film transistor. It works.

[0113] The buffer layer 43 covers the upper and side surfaces of the semiconductor film 61 mainly made of germanium. Therefore, the semiconductor film 61 mainly composed of germanium is not in contact with the wirings 71a to 71c. This allows the leakage current to be reduced. As a result, the on-state current and field effect mobility are high, and the on-state current is This results in a thin film transistor with low off-state current.

[0114] The crystal grains 60 containing the impurity element serving as a donor are formed in the gate insulating film 52 in the same manner as in the first embodiment. A microcrystalline semiconductor film or an amorphous semiconductor film containing an impurity element serving as a donor is formed on b. Next, a plasma is applied to the microcrystalline semiconductor film or the amorphous semiconductor film containing the impurity element serving as a donor. The crystal grains 60 are formed by exposing the substrate to a plasma of any one of hydrogen, fluorine, and fluoride. One or more of these are introduced into the reaction chamber of the plasma CVD apparatus, and a high frequency power source is applied to generate plasma. To generate.

[0115] At least one of fluorine, fluoride gas, and hydrogen is introduced and a high-frequency power source is applied. Hydrogen plasma and fluorine plasma are generated by introducing hydrogen into the reaction chamber. Fluorine plasma is generated by introducing fluorine or fluoride into the reaction chamber. The fluorides are HF, SiF4, SiHF3, and S. iH2F2, SiH3F, Si2F6, GeF4, GeHF3, GeH2F2, GeH3 F, Ge2F6, etc. In addition to fluorine, fluoride gas, or hydrogen, rare gases can also be used for the reaction. It may be introduced into the reaction chamber to generate a rare gas plasma.

[0116] Hydrogen plasma, fluorine plasma, etc. generate hydrogen radicals, fluorine radicals, etc. in the plasma. Hydrogen radicals are generated in a microcrystalline semiconductor film or an amorphous semiconductor film containing an impurity element that serves as a donor. The reaction with the amorphous components of the amorphous semiconductor film crystallizes a part of the semiconductor film and causes the amorphous components to form. The fluorine radicals also etch away the microcrystalline semiconductor that contains the impurity element that acts as a donor. The amorphous components of the conductive film or the amorphous semiconductor film are etched. In addition, the crystal grains can be left on the gate insulating film 52b. In the case where an amorphous semiconductor film containing Therefore, the interface with the gate insulating film can be crystallized to form crystal grains. Since the amorphous components are also etched by the plasma, crystal grains are formed on the gate insulating film. It is possible.

[0117] The plasma generation method is the HF band (3MHz to 30MHz, typically 13.56MHz, 27.12MHz), or high VHF band from 30MHz to about 300MHz This is done by applying a frequency power, typically 60 MHz. GHz or 2.45GHz high frequency plasma can be used. By using high frequency power of 60 Hz, it is possible to improve the uniformity of the plasma. Even on large-area substrates of the 20th to 10th generation, highly uniform plasma is exposed to the germanium film. This is preferable for mass production.

[0118] Next, a semiconductor film 61 containing germanium as a main component is formed on the crystal grains 60. The adhesion of the semiconductor film 61 mainly composed of silicon can be improved. The crystals are grown using 0 as crystal nuclei, and the result is a semiconductor film 61 mainly composed of germanium. A crystalline germanium film can be formed.

[0119] When the semiconductor film 61 mainly composed of germanium is formed by the CVD method, germanium Hydrogen is introduced into the reaction chamber of the plasma CVD apparatus together with a deposition gas containing hydrogen, and high frequency power is applied. A plasma is generated by applying a gas to the semiconductor film 61 containing germanium as a main component. Form a germanium film or a microcrystalline germanium film. By using a deposition gas containing silicon together with gas and hydrogen, amorphous silicon germanium can be formed. A silicon germanium film or a microcrystalline silicon germanium film is formed.

[0120] In addition, an amorphous germanium film is formed as the semiconductor film 61 containing germanium as a main component. In one embodiment, a glow discharge plasma is used in a reaction chamber to deposit germanium-containing deposition gas. By using ZnO, an amorphous germanium film can be formed. The deposition gas is one or more selected from the group consisting of helium, argon, krypton, and neon. The amorphous germanium film is formed by diluting the germanium with rare gas elements of Alternatively, the flow rate of the deposition gas containing germanium is 1 to 10 times, and more preferably 1 to 10 times, ... Preferably, the amorphous gel is formed by glow discharge plasma using hydrogen at a flow rate of 1 to 5 times. A germanium film can be formed. Furthermore, a deposition gas containing germanium, hydrogen At the same time, by using a deposition gas containing silicon, a semiconductor mainly composed of germanium can be The film 61 may be an amorphous silicon germanium film.

[0121] In addition, a microcrystalline germanium film is formed as the semiconductor film 61 mainly composed of germanium. In one embodiment, a deposition gas containing germanium, here germanium, is introduced into the reaction chamber. The germanium oxide is mixed with hydrogen and / or rare gas, and the microcrystalline germanium oxide is produced by glow discharge plasma. Germane is diluted 10 to 2000 times with hydrogen and / or rare gases. Therefore, a large amount of hydrogen and / or rare gas is required. The heating temperature of the substrate is 100℃ to 4 The deposition temperature is 00° C., preferably 250° C. to 350° C. Furthermore, the deposition gas containing germanium is By using a deposition gas containing silicon along with hydrogen and silicon dioxide, a germanium-based The semiconductor film 61 is made of microcrystalline silicon germanium (Si y Ge 1-y , 0 <y<0.5 ) film can be formed.

[0122] Generation of glow discharge plasma in the process of forming a semiconductor film 61 mainly composed of germanium High frequency bands from 3MHz to 30MHz, typically 13.56MHz and 27.12MHz Power, or high-frequency power in the VHF band from 30 MHz to about 300 MHz, representative Typically, this is done by applying a 60 MHz frequency.

[0123] The microcrystalline semiconductor film 45 including the impurity element serving as a donor shown in Embodiment 1 and the first buffer Instead of the GaN layer 54, the GaN layer 54 is made of crystal grains containing the above-mentioned impurity element as a donor and germanium. After forming the semiconductor film as the component, the same process as in the first embodiment is performed to form the semiconductor film as shown in FIG. In addition, a thin film transistor can be manufactured by the same process as in the embodiment 2. A film transistor can be formed.

[0124] FIG. 11 shows a different embodiment from the first embodiment. As in the first embodiment, the gate insulating film After forming a microcrystalline semiconductor film 45 containing an impurity element serving as a donor on 52, germanium Next, a second photomask is applied in the same manner as in the first embodiment. The resist mask formed by the photolithography process is used to form a donor. The microcrystalline semiconductor film 45 containing a pure element and the semiconductor film mainly containing germanium are etched. The microcrystalline semiconductor film 69 containing an impurity element serving as a donor and the germanium-based Next, a semiconductor film 61 is formed by the same process as in the first embodiment. A microcrystalline semiconductor film 69 containing an impurity element serving as a donor is formed on the gate insulating film 52b. A semiconductor film 61 mainly composed of germanium is formed thereon, and a donor impurity Sides of the microcrystalline semiconductor film 69 containing a pure element and the semiconductor film 61 containing germanium as a main component A thin film transistor having a buffer layer 73 covering the thin film transistor can be fabricated. A thin film transistor can be formed by the same process as in the second embodiment.

[0125] The semiconductor film 61 mainly made of germanium is a microcrystalline semiconductor mainly made of silicon. Since the insulating film 69 is in contact with the insulating film 69, the adhesion between the insulating film 69 and the insulating film 69 is improved. It is possible to increase the density.

[0126] In addition, the microcrystalline semiconductor film 69 containing the impurity element serving as a donor has microcrystals formed on the film surface. Therefore, the surface of the microcrystalline semiconductor film 69 containing the impurity element serving as a donor has high crystallinity. When a semiconductor film 61 mainly made of germanium is formed on this, Since the crystals grow from the crystals on the surface of the microcrystalline semiconductor film 69, which is a crystal nucleus, the crystals have high crystallinity. A semiconductor film 61 mainly made of germanium, typically a fine crystal of germanium A crystalline semiconductor film is formed. The semiconductor film 61 mainly composed of germanium has a low resistivity. Carriers preferentially flow through the semiconductor film 61 containing germanium as a main component. The thin film transistor described in this embodiment has high field-effect mobility and high on-state current.

[0127] In addition, the buffer layer 73 covers the upper surface and the side surface of the semiconductor film 61 mainly composed of germanium. Therefore, the semiconductor film 61 containing germanium as a main component is not in contact with the wirings 71a to 71c. Therefore, the occurrence of leakage current can be suppressed. It is possible to manufacture a thin film transistor having high conductivity and low off-state current.

[0128] (Embodiment 4) In this embodiment mode, the structure of the thin film transistor shown in the above embodiment mode will be described below. .

[0129] FIG. 12A shows a top view of a thin film transistor in which the source electrode and the drain electrode are parallel. FIG. 12B shows a cross-sectional view of EF in FIG. 12A.

[0130] FIG. 12B shows a gate electrode 51 and a gate insulating film formed on a substrate 50. A microcrystalline semiconductor film 58 containing an impurity element serving as a donor and a first buffer layer 62 are provided on the inside of the In addition, the microcrystalline semiconductor film 58 containing the impurity element serving as a donor and the first buffer A second buffer layer 43 is formed to cover the silicon layer 62. The source region 72S and the drain region 72D facing each other, and the source electrode 71S and the drain electrode 71D is formed.

[0131] In FIG. 12B, an overlapping region 441 of the gate electrode 51 and the drain region 72D, The microcrystalline semiconductor film 58 containing the impurity element serving as a donor and the overlapping region 4 of the drain region 72D 42. In addition, overlapping regions 441 and 442 also overlap.

[0132] The thin film transistor, gate electrode 51 and drain region 72 shown in FIGS. D, and the microcrystalline semiconductor film 58 containing the impurity element serving as a donor and the drain region 72D. Since the layers are overlapped, the thin film transistor has a high on-current and a high field effect mobility. can be done.

[0133] FIG. 12C shows the top structure of a thin film transistor, and FIG. 12D shows the top structure of FIG. A cross-sectional view of EF is shown.

[0134] FIG. 12C shows a gate electrode 51 and a gate insulating film formed on a substrate 50. A microcrystalline semiconductor film 58 containing an impurity element serving as a donor and a first buffer layer 59 are formed so as to cover the end portions of the first buffer layer 58 and the first buffer layer 59. A microcrystalline semiconductor film 58 containing an impurity element serving as a donor and a A second buffer layer 43 is formed to cover the first buffer layer 62. 43, a source region 72S and a drain region 72D, and a source electrode 71S and a drain electrode A rain electrode 71D is formed.

[0135] In FIG. 12D, the edge of the gate electrode 51 and the edge of the drain electrode 71D are aligned. The microcrystalline semiconductor film 58 including the impurity element serving as a donor and the drain region 72D overlap each other. Has 444.

[0136] In FIG. 12B, the edge of the gate electrode 51 and the edge of the drain electrode 71D are aligned. On the other hand, the microcrystalline semiconductor film 58 containing the impurity element serving as a donor and the drain region 72 D overlapping region 444.

[0137] The thin film transistor shown in FIG. 12(C) and (D) has a gate electrode 51 and a drain region 7 Since the 2D does not overlap, the parasitic capacitance can be reduced. Therefore, the thin film transistor using this structure can reduce the voltage drop on the side of the transistor. In particular, the pixel response speed of a liquid crystal display device can be improved. In the case of thin-film transistors formed in the liquid crystal, the voltage drop in the drain voltage can be reduced. It is possible to increase the response speed of the material.

[0138] FIG. 13(A) shows a case where the opposing regions of the source electrode and the drain electrode are curved. The top view structure of a thin film transistor when the drain electrode is C-shaped or U-shaped is shown in FIG. FIG. 13(B) shows a cross-sectional view of GH in FIG. 13(A), and FIG. 13(C) shows a cross-sectional view of EF in FIG. 13(A). A cross-sectional view of the above is shown.

[0139] 13B and 13C show a structure in which a gate electrode 51 and a gate insulating film are formed on a substrate 50. A microcrystalline semiconductor film 58 containing an impurity element serving as a donor and a first A buffer layer 62 is formed. In addition, the microcrystalline semiconductor film 58 containing an impurity element serving as a donor A second buffer layer 43 is formed to cover the first buffer layer 62. The source and drain regions 72 and the source electrode 71S and the drain electrode 71C are disposed on the first layer 43. An inner electrode 71D is formed.

[0140] In FIG. 13B and FIG. 13C, the gate electrode 51 and the drain region 72D overlap. The microcrystalline semiconductor film 58 containing the impurity element serving as a donor and the drain region 7 The overlapping regions 449 and 450 are also overlapping. One of the wirings is shaped to surround the other of the source and drain regions (specifically, U-shaped or C-shaped). This makes it possible to increase the area of ​​the region through which carriers move. Therefore, it is possible to increase the amount of current and reduce the area of ​​the thin film transistor. .

[0141] (Embodiment 5) In this embodiment, in an element substrate 1300 shown in FIG. 14, a pixel portion 1331 and an input terminal The configuration and fabrication of the protection circuits 1334 and 1336 formed between 1332 and 1333 The protection circuit shown in this embodiment is a schottky junction diode. It is formed using an iodide.

[0142] An input terminal 1332 on the scanning line side and an input terminal 1333 on the signal line side formed on a substrate 1330 3 and the pixel section 1331 are connected by wiring extending vertically and horizontally, and the wiring is a protection circuit Connected to 1334~1337.

[0143] The pixel section 1331 and the input terminal 1332 are connected by a wiring 1339. The line 1334 is disposed between the pixel section 1331 and the input terminal 1332 and is connected to the wiring 1339. The protection circuit 1334 protects the thin film transistor of the pixel portion 1331. It is possible to protect various semiconductor elements such as those described above and to prevent them from being deteriorated or destroyed. Although the line 1339 indicates one wiring in the figure, it is provided in parallel with the wiring 1339. All of the wirings have the same connection relationship as the wiring 1339. functions as a scanning line (gate wiring).

[0144] In addition, a protection circuit 1334 on the scanning line side is provided between the input terminal 1332 and the pixel portion 1331. In addition to the protection circuit 1334, the pixel section 1331 is sandwiched between the input terminal 1332 and the It may also be provided on the opposite side (see protection circuit 1335 in FIG. 14).

[0145] The pixel portion 1331 and the input terminal 1333 are connected by a wiring 1338 . The protection circuit 1336 is disposed between the pixel portion 1331 and the input terminal 1333. 38. The protection circuit 1336 protects the thin film transistor of the pixel section 1331. It is possible to protect various semiconductor elements such as resistors and the like, and prevent deterioration or destruction. Although 1338 indicates one wiring in the figure, it is provided in parallel with wiring 1338. All of the wirings have the same connection relationship as the wiring 1338. , which functions as a signal line (source wiring).

[0146] A protection circuit 1336 on the signal line side is provided between the input terminal 1333 and the pixel portion 1331. In addition to the protection circuit 1336, the pixel section 1331 is sandwiched between the input terminal 1333 and the inverted It may also be provided on the opposite side (see protection circuit 1337 in FIG. 14).

[0147] It is not necessary to provide all of the protection circuits 1334 to 1337, but at least the protection circuit 13 34 is required. If an excessive current is generated in the wiring 1339, which is the scanning line, the pixel The gate insulating film of the thin film transistor in the portion 1331 may be destroyed, resulting in point defects. It is.

[0148] Furthermore, by providing not only the protection circuit 1334 but also the protection circuit 1336, the wiring Therefore, the generation of an excessive current in the protection circuit 1338 can be prevented. The reliability and yield are improved compared to the case where only the protection circuit 133 is provided. By providing the above-mentioned 6, it is possible to prevent electrostatic damage that may occur during the rubbing process after the formation of a thin film transistor. It is also possible to prevent destruction.

[0149] Furthermore, the provision of the protection circuit 1335 and the protection circuit 1337 further improves reliability. The protection circuit 1335 and the protection circuit 1337 are connected to the input Since the terminal 1332 and the input terminal 1333 are provided on the opposite side, these are This contributes to preventing deterioration or damage to various semiconductor elements that occurs during the manufacturing process.

[0150] Next, specific circuits of the protection circuits 1334 to 1337 in FIG. An example configuration is described below.

[0151] The protection circuit shown in FIG. 15 includes a plurality of diodes. 1c (the wiring 1338 which is the signal line shown in FIG. 14) 2. Here, a cross-sectional view of IJ in FIG. 15 is shown in FIG. 16(A), and A cross-sectional view is shown in FIG.

[0152] As shown in FIG. 16A, the signal lines 271a to 271c of the diode 311 are formed of a conductive film 2 01 and is connected to the gate electrode 251 and the source or drain region 26 The second buffer layer 242a of the diode 311 is in contact with the conductive film 202. Here, the common line 256 is connected to the common line 256 via the conductive film 202. The second buffer layer is formed of an amorphous semiconductor film to which an impurity element serving as a donor is not added. It contacts the Fab layer 242a, forming a Schottky junction.

[0153] As shown in FIG. 16B, the gate electrode of the diode 312 is connected to the common line 256. The common line 256 is connected to the second buffer of the diode 312 via the conductive film 203. The signal lines 271a to 271c of the diode 312 are connected to the source layer 242b. The common line 256 is in contact with the source region or drain region 263b. The first semiconductor film is formed of an amorphous semiconductor film to which no impurity element serving as a donor is added through the third semiconductor film. Since the second buffer layer 242a is in contact with the second buffer layer 242a, a Schottky junction is formed.

[0154] When a positive voltage with a large absolute value is applied to the input terminals of the signal lines 271a to 271c, the A positive potential is applied to the gate electrode 251 of the diode 311 and the signal lines 271a to 271c of FIG. When pressure is applied, carriers are generated in the microcrystalline semiconductor film 258a containing the impurity element serving as a donor. A current flows through the common line 256. In addition, absolute current is supplied from the input terminals of the signal lines 271a to 271c. When a large negative voltage is applied, the signal line 271a of the diode 312 in FIG. A negative voltage is applied to the gate electrodes and the signal lines 271a to 271c, and a threshold voltage is applied to the gate electrodes and the signal lines 271a to 271c. Since a potential difference higher than the voltage occurs, the microcrystalline semiconductor film 258b containing the impurity element serving as a donor Carriers are generated and a current flows through the common line 256. Electrostatic damage to the transistor can be prevented.

[0155] Next, a manufacturing process of the diode 311 shown in FIG. 16(A) will be described with reference to FIG. Here, the method of manufacturing the diode 311 will be described using the first embodiment. 2 can be used as appropriate.

[0156] By the same process as in the first embodiment, a gate electrode is formed on a substrate 50 as shown in FIG. Next, a gate electrode 251 and a common line 256 are formed. Port insulating films 52a and 52b are formed.

[0157] Next, in the same manner as in the first embodiment, a micro-implant containing an impurity element serving as a donor is formed on the gate insulating film 52b. A crystalline semiconductor film 258a and a first buffer layer 262a are formed.

[0158] Next, similarly to the first embodiment, a second insulating film 52b is formed on the first buffer layer 262a and the gate insulating film 52b. A second buffer layer 242a is formed.

[0159] Next, in the same manner as in the first embodiment, the source or drain region 263a and the signal line 271a In this case, the second barrier 271a to 271c that is not covered by the signal lines 271a to 271c is formed. The thickness of the buffer layer 242a is partially reduced.

[0160] Next, in the same manner as in the first embodiment, the protective insulating film 76 and the insulating film 101 are formed.

[0161] Next, as shown in FIG. 17(B), a contact hole 21 exposing the gate insulating film 52b is formed. 1, 214, a contact hole 212 exposing the signal line 271c, a second buffer layer 24 A contact hole 213 is formed to expose 2a.

[0162] Next, as shown in FIG. 17(C), the gate insulating films 52a and 52b are selectively etched. The gate insulating films 52a and 52b are etched under the conditions described above to form the gate electrode 251 and Contact holes 215 and 216 that expose the common line 256 are formed.

[0163] Next, as shown in FIG. 17(D), the pixel electrode 77 is formed and at the same time, the gate electrode 251 is formed. and the conductive film 201 connecting the signal line 271c, the second buffer layer 242a and the common A conductive film 202 that connects the wiring 256 is formed.

[0164] By the above steps, the diode 311 can be formed. The protection circuit can be formed using the same number of masks as the thin film transistor shown in Embodiment 3. can.

[0165] (Embodiment 6) In this embodiment mode, a structure and a manufacturing method of a protection circuit different from those in Embodiment Mode 5 will be described below. In this embodiment, a microcrystalline semiconductor film including an impurity element serving as a donor, a first buffer A Schottky diode is formed between the first buffer layer and the common line. Shown below.

[0166] Here, a cross-sectional view of IJ in FIG. 15 is shown in FIG. 18(A), and a cross-sectional view of KL in FIG. Shown in Figure 8(B).

[0167] As shown in FIG. 18A, the signal lines 271a to 271c of the diode 313 are formed of a conductive film 2 01 and is connected to the gate electrode 251 and the source or drain region 26 In addition, a microcrystalline semiconductor film containing an impurity element serving as a donor of the diode 313 is in contact with the semiconductor layer 312. 258a, the first buffer layer 262a, and the second buffer layer 242a are formed on the conductive film 222. Here, the common line 256 is connected to the common line 256 via the conductive film 222. The first barrier layer is formed of an amorphous semiconductor film to which an impurity element serving as a donor is not added. The first buffer layer 262a and the second buffer layer 242a, and the impurity source serving as a low concentration donor Since the silicon-containing microcrystalline semiconductor film 258a is in contact with the silicon-containing microcrystalline semiconductor film 258a, a Schottky junction is formed between the silicon-containing microcrystalline semiconductor film 258a and the silicon-containing microcrystalline semiconductor film 258a.

[0168] As shown in FIG. 18B, the gate electrode of the diode 314 is connected to the common line 256. The common line 256 is connected to the diode 314 via the conductive film 221 as a donor. The microcrystalline semiconductor film 258b containing the impurity element, the first buffer layer 262b, and the second buffer layer 262c are The signal lines 271a to 271c of the diode 314 are connected to the buffer layer 242b. , contacts the source region or drain region 263b. Here, the common line 256 is a conductive The semiconductor layer 221 is made of an amorphous semiconductor film to which no impurity element serving as a donor is added. The first buffer layer 262b and the second buffer layer 242b are formed by the low concentration of donors. Since the microcrystalline semiconductor film 258b containing the impurity element is in contact with the do.

[0169] In the case of a protective circuit provided for the wiring 1339 that is a scan line shown in FIG. The signal lines 271a to 271c in FIG. 18 function as common lines, and the common line 256 in FIG. It functions as:

[0170] When a positive high voltage is applied to the input terminals of the signal lines 271a to 271c, the double-ended signal line shown in FIG. A positive voltage is applied to the gate electrode 251 of the diode 313 and the signal lines 271a to 271c. Carriers are generated in the microcrystalline semiconductor film 258a containing the impurity element serving as a donor, and the common line 2 A current flows through the input terminals of the signal lines 271a to 271c. When the voltage is applied, the signal lines 271a to 271c of the diode 314 in FIG. A negative voltage is applied, and a potential equal to or higher than the threshold voltage is applied to the gate electrodes and the signal lines 271a to 271c. Due to the difference, carriers are generated in the microcrystalline semiconductor film 258b including the impurity element serving as a donor. This generates a current flowing through the common line 256. This can prevent electrostatic damage.

[0171] Next, a manufacturing process of the diode 313 shown in FIG. 18(A) will be described with reference to FIG. Here, a method for manufacturing the diode 313 will be described using the first embodiment. 2 can be used as appropriate.

[0172] As in the fifth embodiment, as shown in FIG. 19(A), a gate electrode 251 and a The common line 256 is formed. Next, a gate insulating film is formed on the gate electrode 251 and the common line 256. Next, a dopant layer containing an impurity element that serves as a donor is formed on the gate insulating film 52b. A microcrystalline semiconductor film 258a including the first buffer layer 262a is formed. A second buffer layer 242a is formed on the layer 262a and the gate insulating film 52b. The lines 271a to 271c and the source or drain region 263a are formed. In this case, the second buffer layer 242a that is not covered by the signal lines 271a to 271c has a thickness Next, the protective insulating film 76 and the insulating film 101 are formed. It is preferable to use a non-photosensitive resin as the material 101 .

[0173] Next, a resist is applied onto the insulating film 101. Next, a multi-tone mask as shown in the second embodiment is applied. The resist is irradiated with light using a mask, and the resist is exposed and developed to have multiple thicknesses. In this example, the gate electrode 251, the signal lines 271a to In the region where the contact hole exposing the common line 256 is formed, the resist It is possible to expose 100% of the sample, and the microcrystals containing the donor impurity element are The semiconductor film 258a, the first buffer layer 262a, and the second buffer layer 242a are exposed. In the contact hole formation area, the resist is exposed in the range of 10 to 70%. By using a multi-tone mask capable of performing the above, a resist mask 223 with different thicknesses is formed. It is possible.

[0174] Next, as shown in FIG. 19(B), the insulating film 101 is etched using the resist mask 223. Next, the protective insulating film 76 is etched. Next, the gate insulating films 52a and 52b are As a result, the gate electrode 251 and the common line 256 are exposed. The contact holes 224 and 226 and the contact hole 225 exposing the signal line 271c are It can be formed.

[0175] Next, the resist mask 223 is removed by ashing, and the thin film region is separated. Next, the insulating film 101 and the protective film 231 are formed using the mask. The protective insulating film 76 is etched. Next, the microcrystalline semiconductor film 2 containing the impurity element serving as a donor is 58a, and a part of each of the first buffer layer 262a and the second buffer layer 242a. Then, as shown in FIG. 19(C), a contact hole is formed to expose the gate insulating film 52b. At this time, the insulating film 234 is formed under the condition that the gate insulating film 52b is not etched. the film 101, the protective insulating film 76, the microcrystalline semiconductor film 258a including the impurity element serving as a donor, The first buffer layer 262a and the second buffer layer 242a are partially etched. In addition, the etching process is preferably performed to form a contact hole as shown in FIG. In the regions 224 to 226, the insulating film 102 and the protective insulating film 76 are also partially etched. Contact holes 232, 234, and 235 are formed with a double top surface shape.

[0176] Thereafter, in the same manner as in the fifth embodiment, a pixel electrode is formed, and at the same time, a gate electrode 251 and a signal The conductive film 201 connecting the common line 271c, the second buffer layer 242a, and the common line 2 A conductive film 222 connecting 56 is formed.

[0177] By the above steps, a diode can be formed. A protection circuit can be formed using the same number of masks as the thin film transistor shown in Form 3. .

[0178] (Embodiment 7) In this embodiment mode, a structure and a manufacturing method of a protection circuit different from those in Embodiments 5 and 6 will be described. In this embodiment, a method for forming a microcrystalline semiconductor film containing an impurity element that serves as a donor is described below. A diode having a Schottky junction between a semiconductor film, a first buffer layer, and a second buffer layer is used. Shown below.

[0179] Here, a cross-sectional view of MN in FIG. 20 is shown in FIG. 21(A), and a cross-sectional view of OP in FIG. 20 is shown in FIG. 1(B).

[0180] As shown in FIG. 20, the diode 315 of the present embodiment includes a common line 256, a donor, and The microcrystalline semiconductor film 231a containing the impurity element, the first buffer layer 232a, and the second The contact hole 245 in contact with the buffer layer 233a contains an impurity element that serves as a donor. A microcrystalline semiconductor film 231a, a first buffer layer 232a, and a second buffer layer 233a The difference from the sixth embodiment is that the diode 316 is formed at the end of the common The first buffer layer 231b includes a first impurity element serving as a donor. The contact hole 246 where the first buffer layer 232b and the second buffer layer 233b contact each other is a donor. a microcrystalline semiconductor film 231b containing an impurity element serving as a first buffer layer 232b, The second embodiment differs from the sixth embodiment in that the second buffer layer 233b is formed at an end of the second buffer layer 233b.

[0181] As shown in FIG. 21A, the signal lines 271a to 271c of the diode 315 are formed of a conductive film 2 41 and is connected to the gate electrode 251 via the source region or drain region 26 In addition, a microcrystalline semiconductor film containing an impurity element serving as a donor of the diode 315 is in contact with the semiconductor layer 312. The first buffer layer 231a, the first buffer layer 232a, and the second buffer layer 233a are formed on the conductive film 242. Here, the common line 256 is connected to the common line 256 via the conductive film 242. The first barrier layer is formed of an amorphous semiconductor film to which an impurity element serving as a donor is not added. The first buffer layer 232a and the second buffer layer 233a, and the impurity source serving as a low concentration donor Since the silicon-containing microcrystalline semiconductor film 231a is in contact with the silicon-containing microcrystalline semiconductor film 231a, a Schottky junction is formed between the silicon-containing microcrystalline semiconductor film 231a and the silicon-containing microcrystalline semiconductor film 231a.

[0182] The gate electrode of the diode 316 is formed from the common line 256. The microcrystalline semiconductor containing the impurity element serving as a donor of the diode 316 is The insulating film 231b, the first buffer layer 232b, and the second buffer layer 233b are connected to each other. In addition, the signal lines 271a to 271c of the diode 316 are connected to the source region or the drain region. Here, the common line 256 is in contact with the region 263b via the conductive film 243. The first buffer layer 232b is formed of an amorphous semiconductor film to which no impurity element is added. , the second buffer layer 233a, and a microcrystal containing a low concentration of an impurity element serving as a donor. It contacts the semiconductor film 231b and forms a Schottky junction.

[0183] In the case of a protective circuit provided for the wiring 1339 that is a scan line shown in FIG. The signal lines 271a to 271c in FIG. 21 function as common lines, and the common line 256 in FIG. It functions as:

[0184] When a positive high voltage is applied to the input terminals of the signal lines 271a to 271c, the double-ended signal line shown in FIG. A positive voltage is applied to the gate electrode 251 of the diode 315 and the signal lines 271a to 271c. Carriers are generated in the microcrystalline semiconductor film 231a containing the impurity element serving as a donor, and the common line 2 A current flows through the input terminals of the signal lines 271a to 271c. When the voltage is applied, the signal lines 271a to 271c of the diode 316 in FIG. A negative voltage is applied, and a voltage equal to or higher than the threshold voltage is applied to the common line 256 and the signal lines 271a to 271c. Due to the occurrence of a potential difference, the carriers are transferred to the microcrystalline semiconductor film 231b including the impurity element serving as a donor. This generates a current flowing through the common line 256. This can prevent electrostatic damage to the capacitor.

[0185] Next, a manufacturing process of the diode 315 shown in FIG. 21(A) will be described with reference to FIG. Here, a method for manufacturing the diode 315 will be described using the first embodiment. 2 can be used as appropriate.

[0186] As in the fifth embodiment, as shown in FIG. 22(A), a gate electrode 251 and a The common line 256 is formed. Next, a gate insulating film is formed on the gate electrode 251 and the common line 256. Next, a dopant layer containing an impurity element that serves as a donor is formed on the gate insulating film 52b. A microcrystalline semiconductor film 258a including the first buffer layer 262a is formed. A second buffer layer 41 is formed on the layer 262a and the gate insulating film 52b. An impurity semiconductor film 55 to which an impurity element imparting one conductivity type is added is formed on the buffer layer 41. Form.

[0187] Next, a resist is applied onto the impurity semiconductor film 55 to which an impurity element that imparts one conductivity type is added. After the deposition, a resist mask is formed by a photolithography process using a photomask. Next, the resist mask is used to form an impurity film having an impurity element that imparts one conductivity type. The semiconductor film 55, the second buffer layer 44, the first buffer layer 262a, and the impurities acting as donors Each of the microcrystalline semiconductor films 258a containing an organic element is partially etched to obtain a structure shown in FIG. As shown in FIG. 1, a microcrystalline semiconductor film 235 including an impurity element serving as a donor, a first buffer layer 2 36, the second buffer layer 237, and the impurity layer having an impurity element that imparts one conductivity type added thereto A semiconductor film 238 is formed. Here, a microcrystalline semiconductor film 2 35 and the side of the first buffer layer 236 are covered with a second buffer layer 237, The second buffer layer 237 has a side surface that generally coincides with the side surface of the second buffer layer 237 .

[0188] Next, in the same manner as in the sixth embodiment, the signal lines 271a to 271c and the source region or the drain region are In this case, the second region 263a that is not covered by the signal lines 271a to 271c is formed. The thickness of the buffer layer 239 is partially reduced. Next, the protective insulating film 76 and the insulating film 101 are formed. do.

[0189] Next, in the same manner as in the sixth embodiment, a process using a multi-tone mask is performed to form a gate electrode 251 and a common Contact holes are formed to expose the data line 256 and the signal line 271c. The microcrystalline semiconductor film 231a containing an impurity element serving as a donor, the first buffer layer 232a, and the second buffer layer 232b are The buffer layer 233a is partially etched to form a layer including an impurity element serving as a donor. The side surfaces of the microcrystalline semiconductor film 235, the first buffer layer 236, and the second buffer layer 237 are At the same time, a contact hole 245 is formed that exposes the gate insulating film 52b.

[0190] Thereafter, in the same manner as in the fifth embodiment, a pixel electrode is formed, and at the same time, a gate electrode 251 and a signal The conductive film 241 connecting the wiring 271c and the microcrystalline semiconductor containing the impurity element serving as a donor The main body 231a, the first buffer layer 232a, the second buffer layer 233a, and the common A conductive film 242 that connects the lines 256 is formed.

[0191] Through the above steps, the diode 315 can be formed. The protection circuit can be formed using the same number of masks as the thin film transistor shown in Embodiment 3. can.

[0192] (Embodiment 8) In this embodiment, a film formation apparatus that can be used in the film formation process in the above embodiment and a method for forming a film therein will be described. The flow of the boards at is shown below.

[0193] Next, as an example of a plasma CVD apparatus applicable to the film forming process of this embodiment, An insulating film, a microcrystalline semiconductor film containing an impurity element serving as a donor, a buffer layer, and a single conductivity type are provided. An example of a structure suitable for forming an impurity semiconductor film to which an impurity element is added will be described.

[0194] Figure 23 shows an example of a multi-chamber plasma CVD apparatus equipped with multiple reaction chambers. The apparatus includes a common chamber 423, a load / unload chamber 422, a first reaction chamber 400a, a second reaction chamber 400b, and a The reactor is configured with a first reaction chamber 400b, a second reaction chamber 400c, and a fourth reaction chamber 400d. The substrates loaded into the cassette in the load / unload chamber 422 are transported by a transport mechanism 426 in the common chamber 423. The reactor is configured as a single wafer type, with the wafer being transported in and out of each reactor by a gate between the common chamber 423 and each reactor. The reaction chambers are provided with a valve 425 so that the processes carried out in the reaction chambers do not interfere with each other. It is being done.

[0195] Each reaction chamber is classified according to the type of thin film to be formed. For example, the first reaction chamber 400a is The second reaction chamber 400b is a reaction chamber for forming an insulating film such as a gate insulating film. The third reaction chamber 400c is used as a high resistance region of a thin film transistor. The fourth reaction chamber 400d is a one-conductivity type substrate for forming the source and drain. The chamber is used as a reaction chamber for forming an impurity semiconductor film to which the impurity element is added. Of course, the number of reaction chambers is not limited to this, and can be increased or decreased as needed. Cut.

[0196] A turbo molecular pump 419 and a dry pump 420 are connected to each reaction chamber as exhaust means. The exhaust means is not limited to the combination of these vacuum pumps, and may be any combination of approximately 10 -1 Pa to 10 -5 Other vacuum pumps can be used if they can evacuate to a vacuum level of 100 Pa. A butterfly valve 417 is provided between the exhaust means and each reaction chamber. This allows the vacuum pumping to be shut off, and the conductance valve 418 By controlling the exhaust speed, the pressure in each reaction chamber can be adjusted.

[0197] The second reaction chamber 400b for forming a microcrystalline semiconductor film containing an impurity element serving as a donor is a super A cryopump 421 may be connected to evacuate the chamber to a high vacuum. The pressure in the reaction chamber is increased by 10 -5 Ultra-high vacuum at pressures below Pa In this embodiment, the reaction chamber is -5 Ultra-high accuracy with pressures below Pa By making the semiconductor film empty, the oxygen concentration and the nitrogen concentration in the microcrystalline semiconductor film containing the impurity element serving as a donor are As a result, the microcrystalline semiconductor film 45 containing the impurity element serving as a donor is effectively The concentration of oxygen in 16 atoms / cm 3 It can be: Donna By reducing the oxygen concentration and the nitrogen concentration in the microcrystalline semiconductor film containing the impurity element, It is possible to reduce defects in the film and increase crystallinity, improving carrier mobility. It is possible.

[0198] The gas supply means 408 supplies semiconductor material gases such as silane and germane, or rare gases. A cylinder 410 filled with the gas used in the process, stop valves 411 and 412, The gas supply means 408g is configured with a first reaction chamber 400a and supplies gas for forming a gate insulating film. 8i is connected to the second reaction chamber 400b, and is for forming a microcrystalline semiconductor film containing an impurity element serving as a donor. The gas supply means 408b is connected to the third reaction chamber 400c, and supplies the gas The gas supply means 408n is connected to the fourth reaction chamber 400d, and The gas for the semiconductor film is supplied. It is also one of the gases containing impurity elements that act as donors. The phosphine gas is also connected to the first reaction chamber 400a and the second reaction chamber 400b. The gas supply means 408a supplies argon, and the gas supply means 408f supplies This is a system that supplies the etching gas used for cleaning. It is configured as an in.

[0199] Each reaction chamber is connected to a high-frequency power supply means 403 for generating plasma. The high frequency power supply means includes a high frequency power source 404 and a matching box 406 .

[0200] Each reaction chamber can be used depending on the type of thin film to be formed. Since there is an optimal film formation temperature, the film formation temperature can be controlled by separating the reaction chambers. Furthermore, since the same film type can be repeatedly formed, there is no residual information related to the film formation history. In particular, the influence of residual impurities can be eliminated by using microcrystalline semiconductors that contain donor impurity elements. In the case of a conductive film, it is necessary to avoid mixing the impurity element that will become the donor into the buffer layer. As a result, it is possible to reduce the concentration of impurity elements in the buffer layer, The off-state current of the film transistor can be reduced.

[0201] Next, in the same reaction chamber, a gate insulating film and a microcrystalline semiconductor containing an impurity element that acts as a donor are The semiconductor film, the buffer layer, and the impurity semiconductor film doped with an impurity element that gives one conductivity type are successively formed. One embodiment of a plasma CVD apparatus for forming the above-mentioned structure is shown in FIG.

[0202] This device includes a common chamber 423, a load / unload chamber 422, a waiting chamber 401, and a reaction chamber 400. The substrates loaded into the cassette in the load / unload chamber 422 are is a single-wafer type configuration in which the wafer is transported to and from each reaction chamber by a transport mechanism 426 in the common chamber 423. A gate valve 425 is provided between the common chamber 423 and each chamber, and the process in each reaction chamber is controlled by the gate valve 425. are configured so as not to interfere with each other.

[0203] A turbo molecular pump 419 and a dry pump 420 are connected to the reaction chamber 400a as exhaust means. The exhaust means is not limited to the combination of these vacuum pumps, but generally about 10 -1 Pa to 10 -5 If it can evacuate to a vacuum level of 100 Pa, it is suitable for other vacuum pumps. A butterfly valve 417 is provided between the exhaust means 430 and the reaction chamber. This allows the vacuum exhaust to be shut off, and the conductance valve The pumping speed can be controlled by 418 to adjust the pressure in each reaction chamber. In addition, a cryopump 421 may be connected to the reaction chamber 400a.

[0204] The gas supply means 408 supplies semiconductor material gases such as silane and germane, or rare gases. A cylinder 410 filled with the gas used in the process, stop valves 411 and 412, The gas supply means 408g, 408i, and a gas flow controller 413 are included. 408b, 408n, and 408f are connected to the reaction chamber 400a.

[0205] A high-frequency power supply means 403 for generating plasma is connected to the reaction chamber. The radio frequency power supply means 403 includes a radio frequency power source 404 and a matching box 406 .

[0206] Next, a process for continuously depositing multiple films using the plasma CVD apparatus shown in FIG. This is shown in FIG.

[0207] FIG. 25(A) is a simplified diagram of the plasma CVD apparatus shown in FIG. 24. (B) shows a gate insulating film and a donor impurity element on a substrate on which a gate electrode is formed. A microcrystalline semiconductor film containing - The process of continuously forming a film of The dashed arrows indicate the flow of the substrate, and the solid arrows indicate the flow of the film forming process. vinegar.

[0208] As shown in FIG. 25(B), the inner wall of the reaction chamber 400a is cleaned with fluorine radicals or the like ( S461) to remove residual impurities from the reaction chamber 400a. Next, the inner wall of the reaction chamber 400a is Then, a film similar to the gate insulating film is coated on the semiconductor substrate (S462). This prevents the metal constituting the reaction chamber 400a from being mixed into the gate insulating film as an impurity. This can be done.

[0209] Next, the substrate to be loaded into the cassette in the load / unload chamber 422 is moved as shown by the arrow a1. Then, the substrate is transported to the reaction chamber 400a by the transport mechanism 426 of the common chamber 423. At step 0a, a gate insulating film, here a silicon oxynitride film, is formed on the substrate (S463).

[0210] Next, the substrate on which the gate insulating film has been formed is transferred to the transfer mechanism of the common chamber 423 as shown by the arrow a2. The substrate is transported to the waiting chamber 401 by the mechanism 426, and is made to wait (S464). The inner wall of the reaction chamber 400a is cleaned with fluorine radicals or the like (S465). After removing the remaining impurities, the inner wall of the reaction chamber 400a is coated with an amorphous semiconductor film ( By this cleaning and coating, a film is formed on the inner wall of the reaction chamber 400a. The components of the gate insulating film (oxygen, nitrogen, etc.) and the metals that make up the reaction chamber act as impurities and are later It is possible to prevent the impurity element that becomes a donor from being mixed into the microcrystalline semiconductor film that contains the impurity element. As a result, the crystallinity of the microcrystalline semiconductor film can be improved. The donor is transported to the reaction chamber 400a by the transport mechanism 426 of the common chamber 423. A microcrystalline semiconductor film containing an impurity element that serves as a donor is formed (S467). As a microcrystalline semiconductor film containing an impurity element, silane, hydrogen, and phosphine are used as raw material gas. A phosphorus-containing microcrystalline silicon film is formed using the phosphorus-containing microcrystalline silicon film as a source.

[0211] Next, a substrate on which a microcrystalline semiconductor film containing an impurity element serving as a donor is formed is shown by an arrow a2. As shown in FIG. 1, the transfer mechanism 426 in the common room 423 transfers the sample to the waiting room 401 and waits there (S47 0). After that, the inner wall of the reaction chamber 400a is cleaned with fluorine radicals or the like (S468 ), and after removing the remaining impurities in the reaction chamber 400a, an amorphous semiconductor film is formed on the inner wall of the reaction chamber 400a. By this cleaning and coating, the reaction chamber 4 is coated with The microcrystalline semiconductor film containing impurities that act as donors formed on the inner wall of the 00a is composed of phosphorus and antimony. Prevents the metal constituting the chamber from being mixed as an impurity into the amorphous semiconductor film to be formed later. Therefore, the amorphous semiconductor film can function as a high resistance region. Next, as shown by the arrow a3, the reaction chamber 400a is transported by the transport mechanism 426 of the common chamber 423. The substrate is transported to the reaction chamber 400a, where an amorphous semiconductor film is formed as a first buffer layer (S4 71) In this study, silane and hydrogen were used as source gases to form an amorphous semiconductor film. An amorphous silicon film is formed.

[0212] Next, the substrate on which the first buffer layer has been formed is transferred to the common chamber 423 as indicated by the arrow a4. The wafer is loaded into the cassette in the load / unload chamber 422 by the transport mechanism 426. A gate insulating film and fine crystals containing impurity elements that act as donors are formed on a substrate on which a gate electrode is formed. The crystalline semiconductor film and the first buffer layer can be formed successively. The inner wall of the reaction chamber 400a is cleaned with fluorine radicals or the like (S472), and the remaining After removing impurities, the inner wall of the reaction chamber 400a is coated with a film similar to that of the gate insulation. Next, another substrate loaded in a cassette in the load / unload chamber 422 is The substrate is transported to the reaction chamber 400a, and the gate insulating film is formed (S463) and the process is the same as that described above. a gate insulating film, a microcrystalline semiconductor film containing an impurity element serving as a donor, and a first buffer layer are continuously formed.

[0213] All the substrates loaded in the cassette of the load / unload chamber 422 were coated with a gate insulating film, a donor and After the microcrystalline semiconductor film containing the impurity element and the first buffer layer are formed, the cassette is The substrate is then unloaded from the load / unload chamber 422 and sent to the next process.

[0214] In this case, the gate insulating film, n ― The substrate on which the μc-Si film is formed is placed on standby in standby chamber 401. However, it may be allowed to wait in the load / unload chamber 422. The CVD equipment can be simplified, which allows for cost reduction.

[0215] Also, n ― The method for forming the μc-Si film is as follows: Instead, phosphine was poured into the reaction chamber after coating S466. After phosphorus is adsorbed to the inner wall of the reaction chamber, the substrate that has been waiting in the waiting chamber 401 is transferred to the reaction chamber 400a. The microcrystalline silicon film is formed by using silane and hydrogen as raw gases. The film is formed while absorbing phosphorus adsorbed in the chamber, so it contains impurity elements that act as donors. A microcrystalline semiconductor film can be formed.

[0216] In addition, when forming a gate insulating film using S463, phosphine is mixed into the source gas to form phosphorus. After forming a gate insulating film containing silane, a micro-silane was deposited in S467 using silane and hydrogen as source gases. By depositing crystalline silicon, a microcrystalline silicon film containing phosphorus can be formed.

[0217] Next, referring to FIG. 25(B), a microcrystalline semiconductor containing an impurity element that will be a donor and is formed in an island shape is A second buffer layer and an impurity element imparting one conductivity type are formed on the conductive film and the first buffer layer. A semiconductor film doped with impurities (here, n + The a-Si film is continuously formed. The process is shown below. The dashed arrows indicate the flow of the substrate, and the solid arrows indicate the flow of the film formation process. vinegar.

[0218] As shown in FIG. 25(C), the inner wall of the reaction chamber 400a is cleaned with fluorine radicals or the like ( S481) to remove residual impurities from the reaction chamber 400a. Next, the inner wall of the reaction chamber 400a is The second buffer layer is coated on the amorphous silicon (S482). This coating process forms a silicon film. This can prevent the gate insulating film from being contaminated as an impurity.

[0219] Next, the substrate to be loaded into the cassette in the load / unload chamber 422 is moved as shown by the arrow a1. Then, the substrate is transported to the reaction chamber 400a by the transport mechanism 426 of the common chamber 423. At step S483, a second buffer layer, an amorphous silicon film in this case, is formed on the substrate. )do.

[0220] Next, an impurity element that imparts one conductivity type is added to the substrate on which the second buffer layer is formed. The impurity semiconductor film (here, n + Here, a film of a-Si is formed. Rufus silicon film and n + The main components of the a-Si film are the same, and the amorphous silicon For n, + It does not contain any contaminants that can cause a-Si films, so + a-Si film There is no need to perform a coating step before forming the film.

[0221] Next, n + The substrate on which the a-Si film is formed is transported to the common chamber 423 as shown by the arrow a4. The cassette in the load / unload chamber 422 is loaded by the mechanism 426. , island n ― A second buffer layer is formed on the substrate on which the μc-Si film and the first buffer layer are formed. Layer and n + Next, the inner wall of the reaction chamber 400a is The reaction chamber 400a is cleaned with fluorine radicals or the like (S485) to remove residual impurities. After that, the inner wall of the reaction chamber 400a is coated with a film similar to the second buffer layer (S4 86). Next, another substrate loaded in a cassette in the load / unload chamber 422 is transferred to the reaction chamber 400a, and the second buffer layer is formed (S483) and the process is the same as that described above. The second buffer layer and + The a-Si film is continuously formed.

[0222] All the substrates loaded in the cassette of the load / unload chamber 422 are coated with the second buffer layer and n + After the a-Si film is formed, the cassette is removed from the load / unload chamber 422 and the next Put it into the process.

[0223] By the above process, multiple films can be continuously formed without being exposed to the atmosphere. Films can be formed without introducing contaminants.

[0224] (Embodiment 9) In this embodiment, a thin film transistor and a diode having a structure different from those in the above embodiment will be described. The following are the reasons for this:

[0225] In the first to eighth embodiments, a microcrystalline semiconductor including an impurity element serving as a donor A first buffer layer 62 is provided on the film 58, but the first buffer layer 62 is not provided. That is, the top surface and the side surface of the microcrystalline semiconductor film 58 containing the impurity element serving as a donor may be The second buffer layer 42 covers the gate insulating film 52b and the donor. The microcrystalline semiconductor film 58 containing the impurity element may be in contact with the semiconductor layer 56 at its outer edge. This makes it possible to reduce the number of film formation steps, thereby enabling cost reduction.

[0226] (Embodiment 10) In this embodiment, the scanning line (gate wiring) insertion hole provided on the periphery of the substrate 50 shown in FIG. The structure of the input terminal and the signal line (source wiring) input terminal is shown below with reference to Figure 27. FIG. 27 shows a scanning line input terminal section and a signal line input terminal section, which are provided on the periphery of the substrate 50, 1A and 1B are cross-sectional views of a thin film transistor in a pixel portion.

[0227] A display device 300 shown in FIG. 26 is provided with a pixel section 301. The pixel section 301 and the periphery of a substrate 50 Between the portions, protective circuits 302 and 322, a signal line 303, and a scanning line 323 are provided. Although not shown, a signal line 303 and a scanning line 304 are connected from the pixel section 301 and the protection circuits 302 and 322 to the peripheral section. The signal line 303 and the scanning line 323 are provided at their ends with signal line input terminals 306. , and a scanning line input terminal section 326 are provided. The 26 terminals are connected to FPC304 and 324, respectively, and the FPC304 and 324 have signal A scanning line driver circuit 305 and a scanning line driver circuit 325 are provided in the pixel portion 301. However, pixels 327 are arranged in a matrix.

[0228] In FIG. 27A, the scanning line input terminal 306a is connected to the gate of the thin film transistor 330. It is connected to a scanning line 323 formed in the same layer as the electrode 331. A gate electrode 331 of the transistor 330 may be formed. a is formed in the same layer as the source electrode or drain electrode 337 of the thin film transistor 330. The signal line 303 is connected to the source of the thin film transistor 330. A source or drain electrode 337 may be formed.

[0229] The scanning line input terminal 306a and the signal line input terminal 316a are thin-film transistors in the pixel area. The pixel electrodes 340 of the pixel electrodes 330 are formed in the same layer. The line input terminal 316a is formed on an insulating film 339 formed on the signal line 303. On the insulating film 339, the scanning line input terminal 306a and the signal line input terminal 316a are anisotropically Conductive adhesive 307, 327 and conductive particles 308, 328 are bonded to FPC 304, 324. are connected to the wiring 309 and 329.

[0230] In this example, the scanning line 323 and the scanning line input terminal 306a are connected. Between the scanning line input terminal 306a and the signal line 303, a conductive film formed in the same layer as the signal line 303 is provided. Also, the signal line 303 and the signal line input terminal 316a are connected, but A conductive film formed of the same layer as the scanning line 323 may be provided between the signal line input terminal 316a and the signal line input terminal 316b. good.

[0231] In FIG. 27B, the scanning line input terminal 306b is connected to the gate of the thin film transistor 330. It is connected to a scanning line 323 formed in the same layer as the electrode 331. A gate electrode 331 of the transistor 330 may be formed. b is formed in the same layer as the source electrode or drain electrode 337 of the thin film transistor 330. The signal line 303 is connected to the source of the thin film transistor 330. A source or drain electrode 337 may be formed.

[0232] The scanning line input terminal 306b and the signal line input terminal 316b are thin-film transistors in the pixel area. The pixel electrodes 340 of the pixel electrodes 330 are formed in the same layer. The line input terminal 316b is formed on the insulating film 339 and the protective insulating film 338. On the substrate 50, the scanning line input terminal 306b and the signal line input terminal 316b are formed by anisotropic conductive adhesive. The wiring 30 of the FPC 304, 324 is connected via the conductive particles 308, 328 of the adhesive 307, 327. 9, 329.

[0233] In this example, the scanning line 323 is connected to the scanning line input terminal 306b. A conductive film formed in the same layer as the signal line 303 may be provided between the scanning line input terminal 306b and the scanning line input terminal 306b. In addition, the signal line 303 and the signal line input terminal 316b are connected. A conductive film formed in the same layer as the scanning line 323 may be provided between the signal line input terminals 316b. .

[0234] In FIG. 27C, the scanning line input terminal 306c is connected to the gate of the thin film transistor 330. It is connected to a scanning line 323 formed in the same layer as the electrode 331. A gate electrode 331 of the transistor 330 may be formed. c is formed in the same layer as the source electrode or drain electrode 337 of the thin film transistor 330. The signal line 303 is connected to the source of the thin film transistor 330. A source or drain electrode 337 may be formed.

[0235] The scanning line input terminal 306c and the signal line input terminal 316c are connected to thin film transistors in the pixel area. The pixel electrodes 340 of the pixel electrodes 330 are formed in the same layer. The line input terminal 316b is formed on the insulating film 339. In FIG. The openings in the insulating film 339 are the scanning line input terminal 306b and the signal line input terminal 316b. The end of the scanning line 323 is exposed. In the opening of 39, conductive particles 308, 328 of the anisotropic conductive adhesive 307, 327 are The wiring 309 and 329 of the FPC 304 and 324 are connected via the same.

[0236] In this example, the scanning line 323 is connected to the scanning line input terminal 306b. A conductive film formed in the same layer as the signal line 303 may be provided between the scanning line input terminal 306b and the scanning line input terminal 306b. In addition, the signal line 303 and the signal line input terminal 316b are connected. A conductive film formed in the same layer as the scanning line 323 may be provided between the signal line input terminals 316b. .

[0237] (Embodiment 11) In this embodiment mode, the thin film transistor described in the above embodiment mode is used as one mode of a display device. The following describes a liquid crystal display device having a VA (Vertical Ali A VA type liquid crystal display device will be described with reference to Figs. 28 to 30. The VA type is a type of liquid crystal display device that controls the arrangement of liquid crystal molecules in the liquid crystal panel. In the liquid crystal display device of the present invention, the liquid crystal molecules are aligned vertically to the panel surface when no voltage is applied. In this embodiment, the pixel is divided into several regions (sub-pixels). The structure is designed to split the molecules into small cubes (called "multi-dome") and tilt them in different directions. In the following explanation, multi-domain design is taken into consideration. The liquid crystal display device will now be described.

[0238] 28 and 29 show the pixel structure of a VA type liquid crystal panel. FIG. 28 is a plan view of the semiconductor device, and shows a cross-sectional structure corresponding to the cutting line YZ shown in the figure. The explanation will be given with reference to both figures.

[0239] In this pixel structure, one pixel has multiple pixel electrodes 624 and 626. Thin film transistors 628 and 629 are connected to electrodes 624 and 626 via a planarizing film 622. The thin film transistors 628 and 629 are configured to be driven by different gate signals. That is, in a pixel with a multi-domain design, each pixel electrode 624 , 626 are configured to be independently controlled.

[0240] The pixel electrode 624 is connected to the thin film transistor 618 through the contact hole 623 . The pixel electrode 626 is connected to a wiring 628 through a contact hole 627. The thin film transistor 628 is connected to the thin film transistor 629 through the gate line 619. Different gate signals are applied to the gate wiring 602 of the thin film transistor 629 and the gate wiring 603 of the thin film transistor 629. On the other hand, the wiring 616 that functions as a data line is made of a thin film. This is commonly used for the transistor 628 and the thin film transistor 629. The thin film transistor 628 and the thin film transistor 629 are manufactured by the method shown in the above embodiment mode. can be done.

[0241] The pixel electrodes 624 and 626 have different shapes and are separated by a slit 625. A pixel electrode 626 is formed so as to surround the outside of the pixel electrode 624 that spreads in a V shape. The timing of the voltage applied to the pixel electrodes 624 and 626 is controlled by a thin-film transistor. The alignment of the liquid crystal is controlled by changing the polarity of the pixel electrode 628 and the thin film transistor 629. The gate wiring 602 and the gate wiring 603 are provided with different gate signals, The operation timing of the transistor 628 and the thin film transistor 629 can be made different. In addition, an alignment film 648 is formed on the pixel electrodes 624 and 626 .

[0242] On the counter substrate 601, a light-shielding film 632, a colored film 636, and a counter electrode 640 are formed. In addition, a flattening film 637 is formed between the colored film 636 and the counter electrode 640, and the alignment of the liquid crystal is prevented from being disturbed. In addition, an alignment film 646 is formed on the counter electrode 640. The structure of the plate side is shown. The counter electrode 640 is an electrode shared between different pixels, but The slit 641, the pixel electrode 624, and the pixel electrode 6 By arranging the slits 625 on the 26 side so that they interdigitate with each other, the oblique electric field can be effectively This allows the liquid crystal to be oriented in a specific direction. This allows the display to be adjusted to different viewing angles, thereby expanding the viewing angle.

[0243] In this embodiment, the substrate, the colored film, the light-shielding film, and the planarizing film constitute a color filter. Either or both of the light-shielding film and the planarizing film may not be formed on the substrate.

[0244] In addition, the colored film preferentially transmits light components in a certain wavelength range within the visible light wavelength range. Usually, it has the function of dividing light into three groups: light in the red wavelength range, light in the blue wavelength range, and light in the green wavelength range. By combining colored films that transmit light preferentially, they can be used as color filters. However, the combination of the colored films is not limited to this.

[0245] The pixel electrode 624, the liquid crystal layer 650, and the counter electrode 640 are overlapped to form a first liquid crystal element. In addition, the pixel electrode 626, the liquid crystal layer 650, and the counter electrode 640 are overlapped. The first liquid crystal element and the second liquid crystal element are formed in one pixel. It is a multi-domain structure in which children are provided.

[0246] In this example, a VA (Vertical Alignment) liquid crystal display device is used. The liquid crystal display device shown in FIG. 1 is a FFS type liquid crystal display device. Liquid crystal display devices, IPS type liquid crystal display devices, TN type liquid crystal display devices, other liquid crystal display devices can be used.

[0247] Through the above steps, a liquid crystal display device can be manufactured. The off-state current is small and the inverted staggered thin film transistor with excellent electrical characteristics is used. Therefore, a liquid crystal display device with high contrast and high visibility can be manufactured.

[0248] (Embodiment 12) In this embodiment mode, the thin film transistor described in the above embodiment mode is used as one mode of a display device. The structure of a pixel in a light-emitting device is described below. FIG. 31(A) shows one mode of a top view of a pixel, and FIG. 31(B) shows a top view of the pixel shown in FIG. 4 shows one form of a cross-sectional structure of a pixel corresponding to AB in FIG.

[0249] The light-emitting device in this embodiment is a display having a light-emitting element that utilizes electroluminescence. The device is used to demonstrate this. Light-emitting elements that utilize electroluminescence are made of organic light-emitting materials. Generally, the former are organic EL elements, the latter are inorganic compounds, and the latter are inorganic compounds. The latter is called an inorganic EL element. The above embodiment can be used.

[0250] In an organic EL element, electrons and holes are released from a pair of electrodes by applying a voltage to the light-emitting element. are injected into layers containing light-emitting organic compounds, causing a current to flow. The rears (electrons and holes) recombine to form an excited state in the light-emitting organic compound. When the excited state returns to the ground state, light is emitted. Such a light-emitting element is called a current-excitation type light-emitting element.

[0251] Inorganic EL elements are divided into dispersion-type inorganic EL elements and thin-film-type inorganic EL elements according to their element structure. Dispersion-type inorganic EL elements have a light-emitting layer in which particles of a light-emitting material are dispersed in a binder. The emission mechanism is a donor-acceptor reaction that utilizes the donor and acceptor levels. Thin-film inorganic EL elements are made by sandwiching a light-emitting layer between dielectric layers. The structure is sandwiched between electrodes, and the light emission mechanism utilizes the inner shell electron transition of metal ions. In this example, the light-emitting element is an organic EL element. In addition, a thin-film transistor for switching is provided to control the input of a signal to the first electrode. As a driving thin film transistor for controlling the driving of the light emitting element, a channel etch type However, a channel protection type thin film transistor may be used as appropriate. This can be done.

[0252] In FIG. 31(A) and FIG. 31(B), the first thin film transistor 74a has a first electrode A switching thin film transistor for controlling the input of a signal, and a second thin film transistor The transistor 74b is a driving thin film for controlling the supply of current or voltage to the light emitting element 94. It corresponds to a membrane transistor.

[0253] The gate electrode of the first thin film transistor 74a is connected to the scanning line 51a, and the source or drain One of the terminals is connected to the wirings 71a to 71c which function as signal lines, and the other terminal is connected to the source or drain. The other end is connected to the gate electrode 51b of the second thin film transistor 74b. Either the source or the drain of the transistor 74b is connected to the power supply lines 93a to 93c. Or the other of the drains is connected to the first electrode 79 of the display device. The gate electrode of the first capacitor 74b, the gate insulating film, and the power supply line 93a constitute a capacitance element 96. The other of the source and the drain of the thin film transistor 74 a is connected to a capacitance element 96 .

[0254] The capacitance element 96 is connected to the second thin film transistor 74a when the first thin film transistor 74a is turned off. The gate-source voltage or gate-drain voltage of the transistor 74b (hereinafter, the gate voltage This corresponds to a capacitance element for holding a capacitance value (assuming that the capacitance is a capacitance value of 1 / 2) and is not necessarily required.

[0255] In this embodiment, the first thin film transistor 74a and the second thin film transistor 74b are The first thin film transistor can be used. The first thin film transistor 74a and the second thin film transistor 74b are n-channel thin film transistors. The first thin film transistor 74a is an n-channel thin film transistor. The second thin film transistor 74b is formed of a p-channel thin film transistor. Furthermore, the first thin film transistor 74a and the second thin film transistor 74b may be It may be formed of a p-channel thin film transistor.

[0256] A protective insulating film 76 is formed on the first thin film transistor 74a and the second thin film transistor 74b. A planarization film 78 is formed on the protective insulating film 76, and the planarization film 78 and the protective insulating film 67 are In the contact hole, a first electrode 79 is formed to connect to the wiring 93f. The planarization film 78 is made of an organic resin such as acrylic, polyimide, or polyamide, or a silicone resin. It is preferable to form the contact hole using a polymer. Since the electrode 79 has projections and recesses, a partition wall 91 is provided to cover the projections and recesses and to have an opening. An EL layer 92 is formed in the opening of the wall 91 so as to contact the first electrode 79. A second electrode 93 is formed so as to cover the partition wall 92, and a second electrode 93 and a partition wall 91 are formed so as to cover the partition wall 92. A protective insulating film 95 is formed.

[0257] Here, a light emitting element 94 having a top emission structure is shown as the light emitting element. 94 also emits light on the first thin film transistor 74a and the second thin film transistor 74b. Therefore, the light emitting area can be increased. If the undercoat film of the second electrode 93 has unevenness, the film thickness distribution becomes non-uniform at the unevenness. The first electrode 79 is shorted, resulting in a display defect. It is preferable to provide such a function.

[0258] The region where the EL layer 92 is sandwiched between the first electrode 79 and the second electrode 93 corresponds to the light emitting element 94. In the case of the pixel shown in FIG. 31(B), the light emitted from the light emitting element 94 is indicated by a white arrow. As shown by the mark, the light is emitted toward the second electrode 93 side.

[0259] The first electrode 79 functioning as a cathode is a conductive film that has a small work function and reflects light. Any known material can be used. For example, Ca, Al, CaF, MgAg, Al Li, etc. The EL layer 92 may be composed of a single layer or a plurality of layers may be laminated. If it is made up of multiple layers, it functions as a cathode. The first electrode 79 is provided with an electron injection layer, an electron transport layer, a light emitting layer, a hole transport layer, and a hole injection layer. It is not necessary to provide all of these layers. The electrode 93 is formed using a conductive material that transmits light, such as tungsten oxide. Indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, titanium oxide Indium oxide containing titanium, indium tin oxide containing titanium oxide, ITO, indium A light-transmitting conductive film such as indium zinc oxide or indium tin oxide with silicon oxide added is used. You may use it.

[0260] Here, we have shown a light-emitting element with a top emission structure that emits light from the surface opposite the substrate. However, there are light emitting devices with a bottom emission structure that emits light from the surface on the substrate side, and light emitting devices that emit light from the substrate side or the opposite side to the substrate. It is possible to appropriately use a light emitting element having a dual emission structure in which light is emitted from the side surface.

[0261] In addition, although organic EL elements have been described as light-emitting elements here, inorganic EL elements may also be used as light-emitting elements. It is also possible to provide an L element.

[0262] In this embodiment, a thin film transistor (a driving thin film transistor) that controls driving of a light emitting element is used. In the above example, the driving thin film transistor and the light emitting element are electrically connected. A current control thin film transistor may be connected between the light emitting element and the light emitting element.

[0263] Through the above steps, a light emitting device can be manufactured. The use of inverted staggered thin-film transistors with low current and excellent electrical characteristics allows A light-emitting device with high reliability and high visibility can be manufactured.

[0264] (Embodiment 13) Next, a structure of a display panel, which is one embodiment of a display device of the present invention, will be described below.

[0265] In FIG. 32, only a signal line driver circuit 6013 is formed separately, and a pixel 6 shows a form of a display panel connected to a pixel portion 6012. 6014 is formed using a thin film transistor in which a microcrystalline semiconductor film is used for the channel formation region. The field effect is higher than that of a thin film transistor using a microcrystalline semiconductor film in a channel formation region. By forming a signal line driver circuit using a transistor that can obtain mobility, This makes it possible to stabilize the operation of the signal line driver circuit, which requires a very high driving frequency. The signal line driver circuit 6013 is a transistor using a single crystal semiconductor for a channel formation region, A thin-film transistor that uses a polycrystalline semiconductor for the channel formation region, or a thin-film transistor that uses SOI for the channel The pixel portion 6012 and the signal line driver circuit 60 may be the same transistor as that used in the pixel portion 6012. The potential of the power supply, various signals, etc. are respectively connected to the FPC 6013 and the scanning line driver circuit 6014. 15. Furthermore, between the signal line driver circuit 6013 and the FPC 6015, Alternatively, a protective circuit may be provided between the signal line driver circuit 6013 and the pixel portion 6012. The circuit is made of one or more elements selected from a thin film transistor, a diode, a resistor, a capacitor, etc. The diode is composed of a plurality of elements. A diode with a Kettke junction may also be used.

[0266] In addition, both the signal line driver circuit and the scanning line driver circuit may be formed on the same substrate as the pixel portion. .

[0267] In addition, when a driver circuit is formed separately, the substrate on which the driver circuit is formed is not necessarily the substrate on which the pixel portion is formed. It is not necessary to attach it to a substrate that has already been fabricated. For example, it can be attached to an FPC. In FIG. 32B, only a signal line driver circuit 6023 is formed separately and formed on a substrate 6021. The shape of the display panel connected to the formed pixel portion 6022 and the scanning line driver circuit 6024 The pixel portion 6022 and the scanning line driver circuit 6024 are formed of a microcrystalline semiconductor film in a channel form. The signal line driver circuit 6023 is formed using the thin film transistors used in the FPC The pixel portion 6022 is connected to the signal line driver circuit 6025. The potential of the power supply, various signals, etc. are respectively connected to the FPC 6023 and the scanning line driver circuit 6024. Further, between the signal line driver circuit 6023 and the FPC 6025 Alternatively, a protective circuit may be provided between the signal line driver circuit 6023 and the pixel portion 6022 .

[0268] In addition, only a part of the signal line driver circuit or a part of the scanning line driver circuit is formed of a microcrystalline semiconductor film. The thin film transistors used in the panel formation area are formed on the same substrate as the pixel area, and the rest is formed on a separate substrate. The signal line driving circuit may be formed in the signal line driving circuit so as to be electrically connected to the pixel section. The analog switch 6033a of the circuit is connected to the pixel section 6032 and the scanning line driver circuit 6034. A shift register 6033b of the signal line driver circuit is formed on the same substrate 6031. The display panel is formed on different substrates and bonded together. The scanning line driver circuit 6034 is a thin film transistor using a microcrystalline semiconductor film in a channel formation region. The shift register 6033b of the signal line driver circuit is formed using FPC 603 5. The pixel portion 6032 is connected to the signal line driver circuit and the driving circuit. The power supply potential and various signals are supplied to the scanning line driving circuit 6034 via the FPC 6035. Furthermore, between the signal line driver circuit 6033 and the FPC 6035 or between the signal line A protective circuit may be provided between the driver circuit 6033 and the pixel portion 6032 .

[0269] As shown in FIG. 32, in the display device of this embodiment, a part or the whole of the driver circuit is provided in the pixel section. A thin film transistor using a microcrystalline semiconductor film in a channel formation region is used on the same substrate as the It can be formed.

[0270] The method for connecting the separately formed substrate is not particularly limited, and may be a known COG method. For example, a wire bonding method or a TAB method can be used. The position is not limited to the position shown in FIG. 28 as long as electrical connection is possible. The controller, CPU, memory, etc. may be formed separately and connected.

[0271] The signal line driver circuit used in the present invention has a shift register and an analog switch. In addition to shift registers and analog switches, buffers, level shifters, source The shift register and analog switch must be included. For example, instead of a shift register, there is no need to provide a decoder circuit or other circuit for the signal line. You can use another circuit that can select, or use a latch instead of an analog switch. is also good.

[0272] (Embodiment 14) The display device obtained by the present invention can be used for an active matrix display panel. In other words, the present invention can be applied to all electronic devices that incorporate such a display unit. do.

[0273] Such electronic devices include cameras such as video cameras and digital cameras, head-mounted displays (goggle-type displays), car navigation systems, projectors, car Stereos, personal computers, personal digital assistants (mobile computers, mobile phones, etc.) An example of such a device is shown in FIG. 33.

[0274] FIG. 33(A) shows a television device. As shown in FIG. 33(A), the display panel is enclosed in a housing. The display panel can be used to display the main screen. 2003 was formed, and other auxiliary equipment such as a speaker unit 2009 and an operation switch were installed. In this manner, the television device can be completed.

[0275] As shown in FIG. 33(A), a display panel 2002 using a display element is mounted on a housing 2001. The receiver 2005 receives general television broadcasts, and the modem 2004 By connecting to a wired or wireless communication network via It is also possible to communicate information one-to-one (between a sender and a receiver, or between receivers themselves) or two-way (between a sender and a receiver, or between receivers themselves). The television set is operated by a switch built into the housing or a separate remote control. 2006, and the remote control device also has a display that displays the information to be output. A display unit 2007 may be provided.

[0276] In addition to the main screen 2003, the television device also has a sub-screen 2008 as a second display panel. The display may be formed of a digital camera and may be added with a configuration for displaying the channel, volume, etc. The main screen 2003 is formed of a liquid crystal display panel, and the sub-screen 2008 is formed of a light-emitting display panel. Alternatively, the main screen 2003 may be formed of a light-emitting display panel, and the sub-screen 2008 may be formed of a light-emitting display panel. It may be formed of a light-emitting display panel, and the sub-screen may be configured to be able to blink.

[0277] FIG. 34 is a block diagram showing the main components of a television device. A pixel portion 921 is formed on the display panel 921. A signal line driver circuit 922 and a scanning line driver circuit 923 are provided on the display panel 921. The display panel 900 may be mounted using the COG method.

[0278] As for the configuration of other external circuits, on the input side of the video signal, a signal received by a tuner 924 Among these, a video signal amplifier circuit 925 amplifies the video signal, and a signal output from the video signal amplifier circuit 925 is fed to a red, A video signal processing circuit 926 converts the video signal into a color signal corresponding to each color of green and blue, The control circuit 927 converts the input specifications of the driver IC. The control circuit 927 outputs signals to the scanning line side and the signal line side. In this case, a signal division circuit 928 is provided on the signal line side to divide the input digital signal into m parts. It may be configured to supply the

[0279] Of the signals received by the tuner 924, the audio signal is sent to an audio signal amplifier circuit 929, The output is supplied to a speaker 933 via an audio signal processing circuit 930. The control information for the receiving station (receiving frequency) and the volume is received from the input unit 932, and the tuner 924 and the audio The signal is sent to the voice signal processing circuit 930.

[0280] Of course, the present invention is not limited to television devices, but may be used in a variety of applications, including personal computer monitors. Therefore, it is suitable for large-area displays such as information display boards at train stations and airports, and advertising display boards on the street. It can also be used for various purposes as a display medium.

[0281] The display device described in the above embodiment is applied to the main screen 2003 and the sub-screen 2008. This will improve the mass production of television sets with improved image quality, such as contrast. can.

[0282] FIG. 33B shows an example of a mobile phone 2301. This mobile phone 2301 has a display The display unit 2302 includes an operation unit 2303. By applying the display device described in the above embodiment, image quality such as contrast can be improved. This will enable the mass production of mobile phones with improved performance.

[0283] A portable computer shown in FIG. 33C includes a main body 2401, a display unit 2402, etc. By applying the display device described in the above embodiment to the display portion 2402, The mass productivity of computers with improved image quality such as contrast can be improved.

[0284] FIG. 33(D) shows a table lamp, which includes a lighting unit 2501, a shade 2502, and an adjustable arm 2503. 2501, a support 2504, a base 2505, and a power source 2506. The lighting fixtures are either ceiling-mounted or wall-mounted. By applying the display device shown in the above embodiment, This improves productivity and provides an inexpensive desk lighting fixture.

Claims

[Claim 1] a first conductive layer over a substrate; a second conductive layer above the substrate; a first insulating layer over the first conductive layer and over the second conductive layer; a semiconductor layer above the first insulating layer; a third conductive layer above the semiconductor layer; a fourth conductive layer above the semiconductor layer; a second insulating layer over the third conductive layer and over the fourth conductive layer; a fifth conductive layer above the second insulating layer; the third conductive layer has an area intersecting with the second conductive layer; the first conductive layer has a region that functions as a gate electrode; the second conductive layer has a region that functions as a wiring; the second insulating layer has a first opening; the second insulating layer has a second opening; the fifth conductive layer has a region that functions as a pixel electrode, the fifth conductive layer has a region electrically connected to the fourth conductive layer through the first opening, the fifth conductive layer has a region overlapping with the second conductive layer through the first insulating layer in the second opening.

Citation Information

Patent Citations

  • Liquid crystal display device and method of manufacture

    JP2001324725A

  • Thin-film transistor array, manufacturing method therefor and liquid crystal display using the same

    JP2003297850A

  • Thin-film transistor display board manufacturing method

    JP2006190967A

  • Wiring for display device, thin film transistor display panel and its manufacturing method

    JP2006221162A

  • Liquid crystal display device

    JP1992242724A