Steel for liquid ammonia transport or storage

A steel material with specific elements and controlled hardness forms strong oxide films to prevent ammonia SCC in liquid ammonia environments, addressing the limitations of conventional methods by enhancing resistance and eliminating the need for heat treatment.

JP2024166605AActive Publication Date: 2024-11-29JFE STEEL CORP

Patent Information

Application Number
JP2023082809
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

Existing steel materials used in liquid ammonia environments struggle with ammonia-induced stress corrosion cracking (SCC), particularly in large structures, as conventional methods like stress relief annealing are impractical and controlling water concentration is difficult, leading to insufficient SCC resistance.

Method used

A steel material composition containing specific elements such as Zr, Hf, Ga, Ta, Te, Sr, Se, Pb, As, Bi, Ba, La, Sm, Pr, Nd, Ce, Sc, Ag, and Au, along with controlled Vickers hardness, forms strong oxide films to prevent new surface formation and crack propagation, enhancing SCC resistance without requiring heat treatment.

Benefits of technology

The steel material exhibits excellent ammonia SCC resistance, suitable for large structures, ensuring long-term use without surface structure alteration and avoiding the need for heat treatment, thus extending the lifespan of equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166605000001
    Figure 2024166605000001
  • Figure 2024166605000002
    Figure 2024166605000002
  • Figure 2024166605000003
    Figure 2024166605000003
Patent Text Reader

Abstract

To provide a steel for ammonia transport or storage, developed in light of current situations, applied to structural members of large structures such as plants and tanks, which are used in liquid ammonia environments and require resistance to ammonia SCC, and demonstrating excellent ammonia SCC resistance.SOLUTION: A steel for liquid ammonia transport or storage contains, in mass%, C: 0.50% or less, Si: 0.01 to 1.00%, Mn: 0.10 to 3.00%, P: 0.030% or less, and S: 0.0100% or less, and further contains a specific amount of one or more kinds selected from Zr, Hf, Ta, Ga, Te, Sr, Se, Pb, As, Bi, Ba, La, Sm, Pr, Nd, Ce, Sc, Ag, Pt, and Au, with the balance being Fe and inevitable impurities.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel material for transporting or storing liquid ammonia that is suitable for structural members of large structures such as pipelines, plants, tanks, etc. that are used in a liquid ammonia environment. [Background technology]

[0002] Ammonia is a compound that is widely manufactured and distributed, mainly as a raw material for basic chemicals such as nitric acid and fertilizers. However, ammonia is difficult to handle, and it is known that ammonia-induced stress corrosion cracking (hereinafter referred to as ammonia SCC) occurs in carbon steel piping, storage tanks, tank cars, and line pipes that handle liquid ammonia. For this reason, conventionally, for structures used in liquid ammonia environments, steel materials with low susceptibility to stress corrosion cracking have been used, and operational measures have been taken to suppress ammonia SCC. For example, it is empirically known that the occurrence of ammonia SCC is correlated with the strength of the material. When using carbon steel, efforts are made to suppress ammonia SCC by setting an upper limit on its strength and by subjecting welds to stress relief annealing. In addition, in a liquid ammonia environment, the presence of water in the liquid ammonia suppresses the occurrence of stress corrosion cracking, so in some cases, a precaution is taken to add water to the liquid ammonia at a level that does not affect its quality. In recent years, the use of liquid ammonia has expanded, and the demand for it has been increasing worldwide, leading to an increase in the size of facilities and a drive to reduce costs in distribution and production. As a result, it has become difficult to implement measures to suppress and prevent ammonia SCC as described above. For example, applying stress relief annealing to welded parts increases the number of manufacturing steps, and therefore its application is not practical, especially in large-scale facilities. In addition, the addition of water to liquid ammonia requires proper management of the water concentration in the liquid ammonia, but as the facility becomes larger, the management of the concentration becomes more difficult. Furthermore, for high-purity liquid ammonia, which has seen an increase in demand in recent years, preventive measures such as adding water cannot be taken in the first place. Therefore, there is a need for the development of steel materials with excellent ammonia SCC resistance suitable for use in structural components of plants and tanks that handle liquid ammonia.

[0003] As a technique relating to steel materials to be used in a liquid ammonia environment, for example, Patent Document 1 discloses a method for producing high tensile steel with excellent ammonia cracking resistance, which is characterized in that after hot rolling a slab, the steel is heated to an austenitizing temperature for structural control and cooled at a cooling rate equal to or slower than air cooling, and then heated and quenched to a two-phase region temperature (Ac1 to Ac3), and then tempered, thereby ensuring the desired properties, i.e., tensile strength and yield strength, and thus achieving ammonia cracking resistance.

[0004] Patent Document 2 also describes a steel slab having a PCM of 0.24% or less when PCM=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B(%), which is rolled to a predetermined plate thickness, and then heated to a temperature of 1100 to 1300°C before quenching heating to form a decarburized layer having a thickness of 0.5 mm or more and having C≦0.05% on the surface of the steel plate, and then quenching and tempering treatment are performed. 2 A method for manufacturing a grade high tensile steel plate is disclosed.

[0005] Furthermore, Patent Document 3 discloses a method for manufacturing a steel plate for an ammonia tank, which comprises a step of surface decarburizing the steel plate material so that the C content within 0.3 mm from the surface becomes 50% or less of the C content of the base material, and a step of heating the surface-decarburized steel plate to a quenching temperature and then cooling the decarburized surface at a cooling rate of 150°C / sec or less in a temperature range of 800 to 500°C. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 5-9571 [Patent Document 2] Japanese Patent Publication No. 61-279631 [Patent Document 3] Japanese Patent Application Publication No. 58-67830 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the steel materials obtained by the manufacturing methods disclosed in Patent Documents 1 to 3 ensure ammonia SCC resistance by controlling the surface structure. Therefore, when the steel materials of Patent Documents 1 to 3 are subjected to heat processing in actual construction, there is a possibility that the surface structure may be altered. For this reason, it cannot be said that sufficient ammonia SCC resistance is necessarily obtained.

[0008] The present invention has been developed in consideration of the above-mentioned current situation, and has an object to provide a steel material for transporting or storing liquid ammonia, which has excellent ammonia SCC resistance and can be applied to structural components of large structures such as plants and tanks that are used in a liquid ammonia environment and require ammonia SCC resistance. [Means for solving the problem]

[0009] The present inventors have conducted extensive research in order to solve the above problems.

[0010] First, the present inventors conducted a detailed study on the mechanism of ammonia SCC occurrence in a liquid ammonia environment and obtained the following findings. In a liquid ammonia environment, the following corrosion reactions occur: Anode reaction: 2Fe → 2Fe 2+ +4e - Cathode reaction: O2 + 2NH4 + +4e - →2OH - +2NH3 However, an inactive oxide film is formed on the steel surface due to the above corrosion reaction. Therefore, the total amount of the above corrosion reaction is usually not large. Therefore, the liquid ammonia environment is not essentially a severe corrosive environment. However, when a new surface is formed on the steel surface due to residual stress in the steel or stress applied from the outside, a selective iron dissolution reaction proceeds with the new surface, where there is no oxide film, as an anode site, forming a crack. The crack becomes a stress concentration area, and the film destruction and corrosion reaction at the crack tip proceed at an accelerated rate, eventually leading to the breakage of the steel. Once a crack is formed by SCC, the life of the steel is determined by the resistance of the steel to SCC crack propagation. Therefore, in order to ensure the ammonia SCC resistance of steel, it is necessary to form a strong oxide film so that a new surface is not formed on the steel surface, thereby preventing the occurrence of SCC and increasing the resistance to SCC crack propagation.

[0011] Based on the above findings, the present inventors have therefore conducted extensive research to develop a steel material that exhibits excellent ammonia SCC resistance in an ammonia environment.

[0012] As a result, they found that containing appropriate amounts of Zr, Hf, Ga, Ta, Te, Sr, Se, Pb, As, Bi, Ba, La, Sm, Pr, Nd, Ce, Sc, Ag, Pt, and Au is effective in improving ammonia SCC resistance, and discovered that it is possible to provide steel material for transporting or storing liquid ammonia that is suitable for structural components of large structures such as pipelines, plants, and tanks used in ammonia environments.

[0013] The present invention has been completed based on the above findings and further investigations. That is, the gist and configuration of the present invention are as follows. [1] In weight percent: C: 0.50% or less, Si: 0.01 to 1.00%, Mn: 0.10-3.00%, P: 0.030% or less, S: 0.0100% or less, and Zr: 0.001 to 0.100%, Hf: 0.001~0.100%, Ta: 0.001 to 0.200%, Ga: 0.001 to 0.300%, Te: 0.001 to 0.500%, Sr: 0.001 to 0.500%, Se: 0.001 to 0.500%, Pb: 0.001~0.500%, As: 0.001 to 0.500%, Bi: 0.001 to 0.500%, Ba: 0.001~0.500%, La: 0.001 to 0.100%, Sm: 0.001~0.100%, Pr: 0.001~0.100%, Nd: 0.001~0.100%, Ce: 0.001 to 0.100%, Sc: 0.001 to 0.100%, Ag: 0.001~0.010%, Pt: 0.001 to 0.010%, Au: 0.001 to 0.010% A steel material for transporting or storing liquid ammonia, characterized in that it has a composition containing one or more selected from the following, with the balance consisting of Fe and unavoidable impurities. [2] The steel material for transporting or storing liquid ammonia according to [1], characterized in that the composition further contains, in mass %, one or more elements selected from the following groups A to G: Note Group A: Ti: 0.100% or less, Group B: Sb: 0.50% or less, Sn: 0.50% or less, Cu:3.00% or less, Ni: 3.00% or less, Cr:3.00% or less, One or more selected from the following: Group C: Ca: 0.0100% or less, Y: 0.100% or less, Mg: 0.0200% or less, One or more selected from the following: Group D: Co: 0.50% or less, Mo: 1.00% or less W: 1.00% or less, V: 0.200% or less, Nb: 0.200% or less, One or more selected from the following: Group E: Al: 0.300% or less, Group F: B: 0.0300% or less, Group G: N: 0.0100% or less [3] A steel material for transporting or storing liquid ammonia according to [1] or [2], characterized in that the maximum Vickers hardness HV0.1 in the surface layer of the steel material is 265 or less. Effect of the Invention

[0014] According to the present invention, it is possible to obtain a steel material for transporting or storing liquid ammonia, which is suitable for use as a structural member of a large structure such as a pipeline, a plant, or a tank used in a liquid ammonia environment and has excellent ammonia SCC resistance. In addition, since the steel material of the present invention ensures ammonia SCC resistance by containing an appropriate amount of specific components, there is no risk of the ammonia SCC resistance being impaired by the alteration of the surface structure, and surface structure control is not required, and the steel material can be manufactured without performing heat treatment such as tempering after hot rolling. Furthermore, when the steel material of the present invention is applied to, for example, a storage tank for liquid ammonia, it can be used for a longer period of time than before without performing stress relief annealing on the welded portion, which is extremely advantageous from an industrial standpoint. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of the present invention will be described. Note that the unit for the composition of the steel material is "mass %", and hereinafter, unless otherwise specified, it will be simply indicated as "%".

[0016] C: 0.50% or less C is an element effective in ensuring the strength of steel. Therefore, in the present invention, it is preferable that C content is 0.01% or more. More preferably, it is 0.02% or more. On the other hand, if the C content exceeds 0.50%, the workability and weldability are significantly deteriorated, and the ammonia SCC resistance decreases with the increase in strength. For this reason, the C content is set to 0.50% or less. It is preferably 0.40% or less, more preferably 0.30% or less, and even more preferably 0.20% or less.

[0017] Silicon: 0.01 to 1.00% Silicon is an element that acts as a deoxidizer for molten steel. In order to ensure this effect, a content of 0.01% or more is required. The Si content is preferably 0.02% or more, more preferably 0.03% or more, and even more preferably 0.05% or more. On the other hand, if the Si content exceeds 1.00%, ductility decreases, toughness deteriorates, and inclusions increase, so that the inclusions become the starting point of cracks and the risk of SCC occurring increases. For this reason, the Si content is set to 1.00% or less, preferably 0.80% or less, more preferably 0.70% or less, and even more preferably 0.60% or less.

[0018] Mn: 0.10-3.00% Mn is an element that improves strength and toughness. If the Mn content is less than 0.10%, the effect is insufficient, so the Mn content is set to 0.10% or more, preferably 0.20% or more, and more preferably 0.50% or more. On the other hand, if the Mn content exceeds 3.00%, the weldability deteriorates and the strength increases, increasing the risk of ammonia SCC occurring, so the Mn content is set to 3.00% or less. Preferably, it is 2.00% or less.

[0019] P:0.030% or less Since P is a harmful element that deteriorates toughness and weldability, the P content is set to 0.030% or less, and preferably 0.025% or less. Although there is no particular lower limit, the P content is preferably set to 0.001% or more because excessive dephosphorization leads to increased costs.

[0020] S: 0.0100% or less S is a harmful element that deteriorates the toughness and weldability of steel, so it is desirable to reduce it as much as possible. In particular, if the S content exceeds 0.0100%, the deterioration of the base material toughness and the weld toughness increases. Therefore, the S content is set to 0.0100% or less. It is preferably 0.0080% or less, and more preferably 0.0060% or less. Although there is no particular lower limit, it is preferable that the S content be 0.0001% or more because excessive desulfurization leads to increased costs.

[0021] In addition to the above components, the following elements (Zr: 0.001-0.100%, Hf: 0.001-0.100%, Ta: 0.001-0.200%, Ga: 0.001-0.300%, Te: 0.001-0.500%, Sr: 0.001-0.500%, Se: 0.001-0.500%, Pb: 0.001-0.500%, As: 0.001-0.500%, Bi:0.001~0.500%, Ba:0.001~0.500%, La:0.001~0.100%, Sm:0.001~0.100%, Pr:0.001~0.100%, Nd:0.001~0.100%, Ce:0.001~0.100%, Sc:0.001~0.100%, Ag:0.001~0.010%, Pt:0.001~0.010%, Au: 0.001~0.010%) should be added to one or more. The steel material of the present invention is not particularly limited in terms of the combination of contained components, but may be one or more elements selected from Zr: 0.001-0.100%, Hf: 0.001-0.100%, and Ta: 0.001-0.200%, Te: 0.001-0.500%, Sr: 0.001-0.500%, Se: 0.001-0.500%, Pb: 0.001-0.500%, As: 0.001-0.500%, Bi: 0.001-0.500%, and Ba: 0.001-0.500%, Further improvement in ammonia SCC resistance can be expected by simultaneously containing one or more of the following elements: La: 0.001-0.100%, Sm: 0.001-0.100%, Pr: 0.001-0.100%, Nd: 0.001-0.100%, Ce: 0.001-0.100%, and Sc: 0.001-0.100%.

[0022] Zr:0.001~0.100%, Hf:0.001~0.100%, Ta:0.001~0.200% Zr, Hf and Ta are important elements for obtaining sufficient ammonia SCC resistance. That is, all of these elements have the function of forming a strong oxide film on the surface of the steel material in a liquid ammonia environment. This suppresses the occurrence of local corrosion that is the starting point of stress corrosion cracking, as well as suppressing the progress of selective anodic dissolution reaction at the crack tip, thereby reducing the ammonia SCC susceptibility of the steel material. Such effects are manifested by containing these elements at 0.001% or more, so they are contained at 0.001% or more. On the other hand, if the content of Zr and Hf exceeds 0.100%, the effect saturates and costs increase, so the Zr content and the Hf content are each set to 0.100% or less, and preferably 0.080% or less. If the content of Ta exceeds 0.200%, the effect saturates and costs increase, so the Ta content is set to 0.200% or less, and preferably 0.180% or less.

[0023] Examples of the strong oxide film in a liquid ammonia environment include Zr(OH)4, Hf(OH)4, and Ta(OH)5, and the thickness of these oxide films is preferably 5 nm or more and 500 nm or less.

[0024] Ga: 0.001 to 0.300% Ga is an important element for obtaining sufficient ammonia SCC resistance. 3+ It has the property of being easily liberated as an ion. 3+ The ions are hydroxide ions (OH -) to form Ga(OH)3. When the crack becomes deep, Ga(OH)3 is formed in the crack and Ga(OH)3 is deposited. This protects the crack and inhibits the progress of the selective anodic dissolution reaction in the crack, thereby improving the ammonia SCC resistance. Such an effect is achieved by including 0.001% or more of Ga, so the content is set to 0.001% or more. On the other hand, if Ga is included in excess, the toughness of the weld metal part decreases and the cost increases. Therefore, the Ga content is set to 0.300% or less, and preferably 0.200% or less. The thickness of the Ga(OH)3 film is preferably 5 nm or more and 500 nm or less.

[0025] Te:0.001~0.500%, Sr:0.001~0.500%, Se:0.001~0.500%, Pb:0.001~0.500%, As:0.001~0.500%, Bi:0.001~0.500%, Ba:0.001~0.500% Te, Sr, Se, Pb, As, Bi and Ba are important elements for obtaining sufficient ammonia SCC resistance. That is, all of these elements are elements that increase the corrosion resistance of steel materials, and have the function of suppressing the corrosion reaction that progresses at an accelerated rate when the pH drops excessively as a result of selective anodic dissolution at the crack tip. In order to suppress the corrosion reaction that progresses at an accelerated rate, it is preferable that the steel material is enriched in a range of 1 mm from the surface, that is, that there is at least one range in which these elements are present (enriched) in a composition of 0.01% or more. The presence of these elements in a composition of 0.01% or more refers to a range of 1 μm x 1 μm or more. Such an effect is manifested by containing these elements at 0.001% or more, so when they are contained, they are contained at 0.001% or more. However, if any of the elements is contained in a large amount, it deteriorates weldability and toughness and leads to an increase in costs. The content of these elements is 0.500% or less, preferably 0.400% or less, and more preferably 0.350% or less.

[0026] La:0.001~0.100%, Sm:0.001~0.100%, Pr:0.001~0.100%, Nd:0.001~0.100%, Ce:0.001~0.100%, Sc:0.001~0.100% La, Sm, Pr, Nd, Ce and Sc are important elements for obtaining sufficient ammonia SCC resistance. That is, they have the function of preventing the occurrence of large subsurface inclusions by controlling the sulfide morphology and enhancing the resistance to SCC crack propagation. By controlling the sulfide morphology, the grain size of all large subsurface inclusions can be reduced to 100 μm or less. Such an effect is manifested by containing 0.001% or more of these elements, so they are contained at 0.001% or more. However, if any of the elements is contained in large amounts, it deteriorates the toughness of the weld and increases the cost. Therefore, the content of these elements is 0.100% or less, and preferably 0.080% or less. These elements are part of the elements called REM (rare earth elements).

[0027] Ag:0.001~0.010%, Pt:0.001~0.010%, Au:0.001~0.010% Ag, Pt and Au are important elements for obtaining sufficient ammonia SCC resistance. That is, all of these elements dissolve in a liquid ammonia environment as the steel corrodes, and form an inactive film on the steel surface. This suppresses the progress of the selective anodic dissolution reaction at the crack tip, and reduces the ammonia SCC susceptibility of the steel. Such an effect is manifested by containing 0.001% or more of these elements, so if they are contained, they should be contained at 0.001% or more. However, if any of these elements is contained in a large amount, it deteriorates toughness and increases costs. Therefore, the content of these elements is set to 0.010% or less.

[0028] Examples of the inactive film formed in the liquid ammonia environment include AgOH, Au(OH)3, and Pt(OH)2, and the thickness of these inactive films is preferably 5 nm or more and 500 nm or less.

[0029] Although the basic essential components have been described above, the following elements may be appropriately contained as necessary. That is, one or more elements selected from the following groups A to G may be appropriately contained.

[0030] Group A: Ti: 0.100% or less Ti is an element that further improves ammonia SCC resistance, and may be contained as necessary. That is, Ti has the function of forming a strong oxide film on the surface of the steel material in a liquid ammonia environment. This suppresses the occurrence of local corrosion that is the starting point of stress corrosion cracking, and also suppresses the progress of selective anodic dissolution reaction at the crack tip, thereby reducing the ammonia SCC susceptibility of the steel material. In order to obtain such an effect, when Ti is contained, it is preferable to contain Ti at 0.001% or more, and more preferably to contain Ti at 0.020% or more. On the other hand, when Ti is contained, the effect is saturated when it exceeds 0.100%, so when Ti is contained, the Ti content is 0.100% or less, and preferably 0.080% or less.

[0031] An example of the strong oxide film in a liquid ammonia environment is Ti(OH)4, and the thickness of the oxide film is preferably 5 nm or more and 500 nm or less.

[0032] Group B: One or more selected from Sb: 0.50% or less, Sn: 0.50% or less, Cu: 3.00% or less, Ni: 3.00% or less, Cr: 3.00% or less Sb, Sn, Cu, Ni and Cr are elements that further improve ammonia SCC resistance, and one or more of these may be contained. All of these elements are elements that increase the corrosion resistance of steel materials, and have the function of suppressing the corrosion reaction that accelerates when the pH drops excessively as a result of selective anodic dissolution at the crack tip. In order to obtain such an effect, it is preferable to contain these elements at 0.01% or more, and more preferably at 0.02% or more. However, if any of the elements is contained in a large amount, it deteriorates weldability and toughness, and leads to an increase in cost. Therefore, when these elements are contained, the Sb content is 0.50% or less, and preferably 0.35% or less. The Sn content is 0.50% or less, and preferably 0.35% or less. The Cu content is 3.00% or less, and preferably 2.00% or less. The Ni content is 3.00% or less, and preferably 2.00% or less. The Cr content is set to 3.00% or less, and preferably to 2.00% or less.

[0033] Group C: Ca: 0.0100% or less, Y: 0.100% or less, Mg: 0.0200% or less, one or more selected from the following Ca, Y, and Mg may be contained in one or more kinds in order to secure the toughness of the welded portion. In order to obtain such an effect, it is preferable to contain Ca at 0.0001% or more, Y at 0.001% or more, and Mg at 0.001% or more. However, if a large amount of each element is contained, it leads to a deterioration in the toughness of the welded portion and an increase in cost. Therefore, when these elements are contained, the Ca content is 0.0100% or less, the Y content is 0.100% or less, and the Mg content is 0.0200% or less. Preferably, the Ca content is 0.0080% or less, the Y content is 0.080% or less, and the Mg content is 0.0180% or less.

[0034] Group D: One or more selected from Co: 0.50% or less, Mo: 1.00% or less, W: 1.00% or less, V: 0.200% or less, Nb: 0.200% or less Co, Mo, W, V, and Nb are elements that improve the hardenability of steel. For the purpose of ensuring the desired strength of the steel, one or more of these elements may be contained as necessary. In order to obtain such an effect, Co is preferably contained at 0.01% or more, Mo is preferably contained at 0.01% or more, W is preferably contained at 0.01% or more, V is preferably contained at 0.001% or more, and Nb is preferably contained at 0.001% or more. However, if Co, Mo, and W are contained in large amounts, the toughness and weldability of the steel material are deteriorated, leading to an increase in cost. Therefore, when these elements are contained, the Co content is 0.50% or less, and the Mo content and the W content are 1.00% or less. Furthermore, the effect of V and Nb is saturated when the content exceeds 0.200%. Preferably, the Co content is 0.40% or less, and the Mo content and the W content are 0.90% or less. Furthermore, the effect of V and Nb is saturated when the content exceeds 0.200%. Therefore, when these elements are contained, the V content and the Nb content are 0.200% or less. The V content and Nb content are preferably 0.180% or less.

[0035] Group E: Al: 0.300% or less Al is an effective element as a deoxidizer, and may be contained as necessary to improve the deoxidizing efficiency. To obtain such an effect, it is preferable to contain 0.010% or more. However, if the Al content exceeds 0.300%, the toughness of the steel material is reduced. Therefore, when Al is contained, the content is 0.300% or less, and preferably 0.250% or less.

[0036] Group F: B: 0.0300% or less B is an element that improves the hardenability of steel material, and may be contained as necessary for the purpose of ensuring the desired strength of the steel material. In order to obtain such an effect, it is preferable to contain 0.0001% or more of B, and more preferably 0.0003% or more of B. However, if the B content exceeds 0.0300%, the toughness of the steel material will be significantly deteriorated. Therefore, when B is contained, its content is 0.0300% or less, and preferably 0.0200% or less.

[0037] Group G: N: 0.0100% or less Since N is a harmful element that reduces toughness, it is desirable to reduce it as much as possible. In particular, if the N content exceeds 0.0100%, the toughness of the steel material is significantly reduced. Therefore, if N is contained, the N content is 0.0100% or less, preferably 0.0080% or less, and more preferably 0.0070% or less. On the other hand, in order to avoid an excessive increase in refining costs in the steelmaking process, the N content is preferably 0.0005% or more, and more preferably 0.0010% or more.

[0038] Components other than those mentioned above are Fe and unavoidable impurities, and unavoidable impurities refer to less than 0.01% O (oxygen) or less than 0.001% of the above components.

[0039] From the viewpoint of further improving ammonia SCC resistance, it is effective to make the maximum value of Vickers hardness HV0.1 in the surface layer of the steel material 265 or less.

[0040] Maximum Vickers hardness HV0.1 in the surface layer of the steel: 265 or less The hardening phases in the surface layer of steel, which are caused by dislocations and precipitates, 1) promote the formation of coarse slip planes, and 2) act as priority areas for anodic dissolution, thus promoting ammonia SCC. This is true even for minute hardening phases in the surface layer of steel.

[0041] In other words, in order to further improve the ammonia SCC resistance of steel, it is effective to suppress the increase in hardness at the surface layer of the steel due to the localized hardening phase. By suppressing the increase in hardness at the surface layer of the steel, it is possible to suppress the progress of the selective iron dissolution reaction with the steel surface as the anode site, and to suppress the initiation and propagation of cracks.

[0042] For this reason, the maximum value of Vickers hardness HV0.1 in the surface layer of the steel material is preferably 265 or less, more preferably 250 or less, even more preferably 230 or less, and most preferably 210 or less. There is no particular restriction on the lower limit, but it is preferably 140 or more. Here, the maximum value of Vickers hardness HV0.1 in the surface layer of the steel material is the maximum value of Vickers hardness measured at 10 points in the rolling direction of the steel material at a depth of 0.5 mm from the steel material surface in the rolling direction cross section of the steel material, under conditions of a test force of 0.1 kgf (0.9807 N) and a pitch of 1 mm, in accordance with JIS Z 2244 (2009).

[0043] By using a steel material having the above-described compositional components and hardness, it is possible to prevent the generation and propagation of cracks caused by the progress of a selective iron dissolution reaction with the steel material surface, which does not have an oxide film, acting as an anode site when stress is applied in ammonia.

[0044] The liquid ammonia mentioned above may also contain a portion of gaseous ammonia.

[0045] The structure of the steel material of the present invention is not particularly limited, but since SCC resistance decreases as the strength of the surface layer increases, it is preferable that martensite accounts for 50% or less of the entire structure within a range of 1 mm from the steel material surface.

[0046] Next, a method for producing a steel material according to the present invention will be described. Note that the method for producing a steel material according to the present invention is not limited to the method described below.

[0047] [Steel manufacturing method] The steel material of the present invention can be produced by melting steel adjusted to the above-mentioned component composition using a known refining process such as a converter, an electric furnace, or vacuum degassing, forming a steel material (slab) using a continuous casting method or an ingot casting-blooming rolling method, and then reheating this steel material as necessary and hot rolling it to form a steel plate, a shaped steel, or the like.

[0048] Here, when the above-mentioned steel material (slab) is hot-rolled to a desired size and shape, it is preferable to reheat the slab at a temperature of 900 to 1350° C. If the slab reheating temperature is less than 900° C., the deformation resistance is large, making hot rolling difficult. On the other hand, if the slab reheating temperature exceeds 1350° C., a partially molten phase is generated on the steel material surface, causing surface marks, scale loss, and an increase in fuel consumption.

[0049] In the method for producing a steel material according to the present invention, instead of the process of reheating and hot rolling the steel material (slab), it is possible to hot roll the steel material (slab) produced by the continuous casting method or the ingot making-blooming rolling method without cooling it to a temperature range below 900° C., and without reheating it. In addition, the hot-rolled steel sheet obtained after the hot rolling may be subjected to reheating treatment, pickling, and cold rolling to produce a cold-rolled steel sheet of a predetermined thickness.

[0050] In hot rolling, the finish rolling end temperature is preferably 650°C or higher. If the finish rolling end temperature is less than 650°C, the rolling load increases due to an increase in deformation resistance, making it difficult to carry out rolling. The finish rolling end temperature is preferably 950°C or lower. If the rolling end temperature exceeds 950°C, the reduction rate in the non-recrystallization temperature range cannot be sufficiently ensured, and the strength and toughness of the finally obtained steel plate are reduced.

[0051] Cooling after hot rolling may be performed by either air cooling or accelerated cooling, but it is preferable to perform accelerated cooling when higher strength is desired. When performing accelerated cooling, it is preferable to set the average cooling rate to 2 to 100°C / s and the cooling stop temperature to 700 to 400°C. That is, if the average cooling rate is less than 2°C / s and / or the cooling stop temperature is more than 700°C, the effect of accelerated cooling is small and sufficient strength may not be achieved. On the other hand, if the average cooling rate is more than 100°C / s and / or the cooling stop temperature is less than 400°C, the toughness of the steel material may decrease or distortion may occur in the shape of the steel material. The average cooling rate here refers to the average cooling rate from the cooling start temperature to the cooling stop temperature in accelerated cooling.

[0052] In the present invention, from the viewpoint of ammonia SCC resistance, it is not necessary to perform heat treatment on the steel sheet cooled after rolling. If distortion occurs in the steel sheet, it is possible to perform heat treatment for the purpose of correcting the distortion, and in this case, it is preferable to heat the steel sheet to 200 to 700°C. In this case, it is preferable to hold the steel sheet during heating for 300 seconds or more.

[0053] In the present invention, the temperatures in the manufacturing conditions are all the average steel sheet temperature. The average steel sheet temperature is obtained by simulation calculation or the like from the sheet thickness, surface temperature, cooling conditions, etc. For example, the average steel sheet temperature is obtained by calculating the temperature distribution in the sheet thickness direction using a finite difference method.

[0054] The steel material of the present invention obtained as described above can be used as a steel material for transporting or storing liquid ammonia, and can be applied to structural components of large structures such as plants and tanks that are used in a liquid ammonia environment and require ammonia SCC resistance. EXAMPLES

[0055] Next, examples of the present invention will be described, but the present invention is not limited to these examples.

[0056] Steels having the chemical compositions shown in Tables 1-1, 1-2, 1-3, and 1-4 (the balance being Fe and unavoidable impurities) were melted in a converter and made into steel slabs by continuous casting. These steel slabs were reheated, hot rolled, and immediately after hot rolling, water-cooled. Test pieces were taken from the obtained steel plates and the following ammonia SCC resistance evaluation test was performed.

[0057] [Ammonia SCC resistance evaluation test] A test piece with a width of 20 mm, length of 120 mm, and thickness of 3.0 mm was taken from the steel material obtained as described above. Next, the above test piece was bent into a U-shape in the length direction with an inner radius of 15 mm, and then immersed in a solution of 12.5 g of ammonium carbamate and 1 L of liquid ammonia for 168 hours while applying an anode voltage of 2.0 V (vs. Pt). After immersion, a cross section of the test piece was cut out, and the maximum crack depth of the crack present in the cross section (the distance from the surface of the test piece to the tip of the crack) was measured, and the ammonia SCC resistance was evaluated according to the following criteria. It was determined that the ammonia SCC resistance was sufficient if it was rated as ◯ or ◎. The results are shown in Tables 2-1 and 2-2. ◎ (Pass, especially excellent): Maximum crack depth is less than 100 μm ○ (Pass): Maximum crack depth is 100 μm or more and less than 300 μm × (Fail): Maximum crack depth is 300 μm or more or breakage occurs Among the examples of the invention, steels Nos. 22 to 24, 26 to 28, 30 to 32, 35, and 38 to 42, which simultaneously contained one or more elements selected from Zr, Hf, and Ta, one or more elements selected from Te, Sr, Se, Pb, As, Bi, and Ba, and one or more elements selected from La, Sm, Pr, Nd, Ce, and Sc, had further improved ammonia SCC resistance (rated as ⊚).

[0058] [Vickers hardness measurement test] The Vickers hardness HV0.1 of the surface layer of the steel material is measured by the following procedure. The steel material is cut so that the target surface is a surface parallel to the rolling direction and perpendicular to the steel material surface. Next, at a position 0.5 mm deep from the surface of the cut steel material on the cross section (rolling direction cross section (L cross section)), Vickers hardness is measured at 10 points in the rolling direction of the steel material under the conditions of a test force of 0.1 kgf (0.9807 N) and a pitch of 1 mm in accordance with JIS Z 2244 (2009). The results are shown in Tables 2-1 and 2-2.

[0059] [Table 1-1]

[0060] [Table 1-2]

[0061] [Table 1-3]

[0062] [Table 1-4]

[0063] [Table 2-1]

[0064] [Table 2-2]

[0065] As shown in Tables 2-1 and 2-2, all of the inventive examples had excellent ammonia SCC resistance even without heat treatment such as tempering after hot rolling. In contrast, all of the comparative examples did not have sufficient ammonia SCC resistance.

Claims

1. In mass%, C: 0.50% or less, Si: 0.01-1.00%, Mn: 0.10-3.00%, P: 0.030% or less, S: 0.0100% or less, and Zr: 0.001 to 0.100%, Hf: 0.001-0.100%, Ta: 0.001-0.200%, Ga: 0.001-0.300%, Te: 0.001 to 0.500%, Sr: 0.001-0.500%, Se: 0.001 to 0.500%, Pb: 0.001 to 0.500%, As: 0.001 to 0.500%, Bi: 0.001-0.500%, Ba: 0.001-0.500%, La: 0.001 to 0.100%, Sm: 0.001-0.100%, Pr: 0.001 to 0.100%, Nd: 0.001 to 0.100%, Ce: 0.001 to 0.100%, Sc:0.001~0.100%, Ag: 0.001-0.010%, Pt: 0.001-0.010%, Au: 0.001-0.010% 1. A steel material for transporting or storing liquid ammonia, characterized in that it has a chemical composition containing one or more selected from the following:

2. 2. The steel material for transporting or storing liquid ammonia according to claim 1, wherein the component composition further contains, in mass %, one or more elements selected from the following groups A to G: Note Group A: Ti: 0.100% or less, Group B: Sb: 0.50% or less, Sn: 0.50% or less, Cu: 3.00% or less, Ni: 3.00% or less, Cr: 3.00% or less, One or more selected from the following: Group C: Ca: 0.0100% or less, Y: 0.100% or less, Mg: 0.0200% or less, One or more selected from the following: Group D: Co: 0.50% or less, Mo: 1.00% or less, W: 1.00% or less, V: 0.200% or less, Nb: 0.200% or less, One or more selected from the following: Group E: Al: 0.300% or less, Group F: B: 0.0300% or less, Group G: N: 0.0100% or less

3. 3. A steel material for transporting or storing liquid ammonia according to claim 1, wherein the maximum value of Vickers hardness HV0.1 in the surface layer of the steel material is 265 or less.

Citation Information

Patent Citations

  • High-strength and high-toughness container steel plate for hydrogen-corrosion-resistant normalizing mobile tank car and manufacturing method of high-strength and high-toughness container steel plate

    CN115558865A

  • Steel material

    JP2019094563A

  • Preparation of tempered steel excellent in ammonia crack resistant characteristics

    JP1983067830A

  • Manufacture of tempered 60kgf / mm2 class high tension steel plate superior in sulfide and ammonia stress corrosion cracking resistance

    JP1986279631A

  • Production of high tensile strength steel excellent in ammonia crack resistance

    JP1993009571A

Cited By

  • Steel plates, ammonia tanks, and line pipes

    JP7853636B1

  • Steel sheet, ammonia tank, and line pipe

    WO2026154735A1