Wafer grinding method

The described wafer grinding method forms a ring-shaped reinforcing portion to maintain wafer rigidity post-grinding, addressing deformation issues in large-diameter wafers without a support substrate, ensuring high rigidity and reducing processing errors.

JP2024166668APending Publication Date: 2024-11-29DISCO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023082909
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

Smart Images

  • Figure 2024166668000001_ABST
    Figure 2024166668000001_ABST
Patent Text Reader

Abstract

To provide a grinding method capable of imparting high rigidity to a ground wafer without attaching a support substrate.SOLUTION: A grinding method for a wafer 10 includes a grinding step of grinding the central region of the wafer 10 held on a holding table 110 with a grinding wheel 103 to form a recess 17 and to form a ring-shaped reinforcing portion 18 on the outer periphery of the recess 17. The wafer 10 has a thickness that allows the ring-shaped reinforcing portion 18 to suppress deformation of the wafer 10 on which the recess 17 has been formed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for grinding a wafer. [Background technology]

[0002] It is known that the rigidity of a wafer thinned by grinding decreases, which makes it difficult to handle the wafer in the post-processing. Technologies related to such an issue are described in, for example, Patent Document 1 and Patent Document 2.

[0003] Patent Document 1 proposes TAIKO (registered trademark) grinding, which maintains a certain degree of rigidity of the wafer after grinding by grinding only the central area of ​​the wafer where the device is provided, and leaving the outer peripheral area as it is.

[0004] Even when TAIKO grinding is performed, the rigidity of the wafer is not sufficiently ensured, and deformation of the wafer such as warping or bending may occur in the post-processing. In light of this, Patent Document 2 proposes a technique in which a support substrate is attached to the wafer before TAIKO grinding is performed. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-019461 A [Patent Document 2] JP 2022-044315 A Summary of the Invention [Problem to be solved by the invention]

[0006] As mentioned above, while the issues related to the rigidity of thinned wafers are significantly improved by TAIKO grinding, to address them more reliably, it would require the time and effort of attaching a support substrate to the wafer before grinding.

[0007] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a grinding method capable of imparting high rigidity to a ground wafer without attaching a support substrate. [Means for solving the problem]

[0008] A wafer grinding method according to one embodiment of the present invention includes a grinding step in which a central region of the wafer held on a holding table is ground with a grinding wheel to form a recess and a ring-shaped reinforcement portion is formed on the outer periphery of the recess, and the wafer has a thickness such that deformation of the wafer in which the recess is formed is suppressed by the ring-shaped reinforcement portion. Effect of the Invention

[0009] According to the present invention, it is possible to provide a grinding method capable of imparting high rigidity to a ground wafer without attaching a support substrate. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a perspective view showing an example of a wafer surface. [Diagram 2] FIG. 11 is a perspective view showing an example of a grinding process. [Diagram 3] FIG. 2 is a perspective view showing an example of the back surface of the wafer after a grinding process. [Figure 4] 10A to 10C are cross-sectional views showing an example of a metal film forming step. [Diagram 5] 10A to 10C are cross-sectional views showing an example of a support member fixing step. [Figure 6] FIG. 11 is a perspective view showing an example of a ring-shaped reinforcing portion removing step. [Figure 7] 10A to 10C are cross-sectional views showing an example of a ring-shaped reinforcing portion removing step. [Figure 8] FIG. 11 is a perspective view showing an example of a dividing step. [Figure 9] FIG. 2 is an explanatory diagram showing the relationship between the diameter and thickness of a wafer in the SEMI standard. [Figure 10] FIG. 2 is an explanatory diagram showing the relationship between the diameter, thickness, and diameter-to-thickness ratio of a wafer. [Figure 11] FIG. 13 is an explanatory diagram showing a threshold value of a coefficient which is a ratio between a diameter and a thickness of a wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The method for grinding a wafer according to the present embodiment will be described with reference to the drawings. The wafer to be ground is not particularly limited. It is not limited to a semiconductor wafer or an optical device wafer, and may be any plate-shaped object to be ground.

[0012] The wafer grinding method according to this embodiment includes a grinding step of performing TAIKO (registered trademark) grinding. TAIKO grinding is a grinding process that forms a ring-shaped protrusion by thinning the wafer while leaving the peripheral region. According to TAIKO grinding, the thinned wafer is reinforced by the ring-shaped protrusion, so that deformation of the wafer is suppressed compared to the case where the protrusion is not formed. Hereinafter, the ring-shaped protrusion formed in the peripheral region of the wafer is referred to as a ring-shaped reinforcing portion.

[0013] However, in conventional grinding methods, the effect of suppressing wafer deformation obtained by the ring-shaped reinforcing portion is not necessarily perfect, and wafer deformation is likely to occur especially when thinning large-diameter wafers having a diameter of about 300 mm (12 inches) or more.

[0014] As a result of thorough investigation into the above-mentioned problems, the inventors of the present application have discovered a new grinding method that can sufficiently suppress deformation of the wafer, even for large-diameter wafers, without using a support substrate as described in Patent Document 2.

[0015] First, with reference to Figs. 1 to 8, a wafer processing procedure including a grinding step in which TAIKO grinding is performed will be described together with the necessity of suppressing deformation of the wafer.

[0016] 1 is a perspective view showing an example of a front surface 11 of a wafer 10. The front surface 11 of the wafer 10 to be ground is provided with a device region 12 in which a plurality of devices 14 are formed. This device region 12 is partitioned by a plurality of planned division lines 15. In addition, on the outer periphery side of the device region 12, an outer periphery excess region 13 in which no devices 14 are formed is provided.

[0017] That is, the surface 11 of the wafer 10 has a device region 12 and a peripheral excess region 13 surrounding the device region 12 .

[0018] Fig. 2 is a perspective view showing an example of a grinding process. The grinding process is performed, for example, by a grinding device shown in Fig. 2. The grinding device shown in Fig. 2 includes a grinding mechanism 100 and a holding table 110. The holding table 110 is a chuck table that suction-holds the front surface 11 of the wafer 10, and the wafer 10 is held on the holding table 110 with its back surface 16 facing the grinding mechanism 100.

[0019] A mount 102 is provided at the lower end of a spindle 101 of the grinding mechanism 100, and a small grinding wheel 103 for TAIKO grinding, which has multiple grinding stones 104 arranged in a ring shape, is attached to the lower surface of the mount 102. The ring-shaped grinding stone 104 is formed by bonding diamond abrasive grains with a bonding agent such as a metal bond or a resin bond, and has an outer diameter that is, for example, larger than the radius of the device region 12 and smaller than the radius of the wafer 10.

[0020] In the grinding process, the holding table 110 holding the wafer 10 is rotated at a low speed by a motor or the like (not shown). Furthermore, the grinding mechanism 100 descends while the grinding wheel 103 on which the annular grinding stone 104 is arranged rotates at high speed in the same direction as the holding table 110. At this time, the annular grinding stone 104 is controlled so as to be constantly in contact with the center of rotation of the back surface 16 of the wafer 10 which rotates together with the rotation of the holding table 110, thereby performing TAIKO grinding to thin the wafer 10 while leaving the outer peripheral region of the wafer 10.

[0021] Fig. 3 is a perspective view showing an example of the back surface 16 of the wafer 10 after the grinding process. In the TAIKO grinding, the central region of the wafer 10 held on the holding table 110 is ground and thinned by a grinding wheel 103 provided with a grinding stone 104, so that a recess 17 is formed on the back surface 16 of the wafer 10 as shown in Fig. 2 and Fig. 3. In addition to the formation of the recess 17, a ring-shaped reinforcing part 18 that maintains the thickness before grinding is formed on the outer periphery side of the recess 17 (the outer periphery region of the wafer 10).

[0022] The ring-shaped reinforcing portion 18 is formed in a region of the back surface 16 corresponding to the outer peripheral surplus region 13 of the front surface 11. In the grinding process according to this embodiment, such a positional relationship between the ring-shaped reinforcing portion 18 and the outer peripheral surplus region 13 is realized by constantly contacting an annular grinding wheel 104 having an outer diameter larger than the radius of the device region 12 and smaller than the radius of the wafer 10 with the center of rotation of the wafer 10.

[0023] Although the reduction in the rigidity of the wafer 10 thinned by grinding is suppressed by the presence of the ring-shaped reinforcing portion 18, the rigidity of the thinned wafer 10 is reduced compared to that before grinding. If the rigidity of the wafer 10 thinned by grinding is insufficient, deformation such as warping will occur in the wafer 10.

[0024] Such deformation of the wafer 10 can cause various errors in the subsequent processes or damage to the wafer 10. In order to avoid the occurrence of these undesirable events, it is necessary to sufficiently secure the rigidity of the wafer 10 after grinding to suppress deformation of the wafer 10.

[0025] 4 is a cross-sectional view showing an example of a metal film forming process. In the metal film forming process performed after the grinding process, a metal film 19 of gold, silver, titanium, or the like is formed in the recesses 17 on the back surface 16 of the wafer 10. The metal film 19 formed on the back surface 16 (recesses 17) is provided for the purpose of performing electrical tests on each device 14 formed on the front surface 11 (device region 12).

[0026] There is no particular limitation on the method for forming the metal film 19 on the wafer 10. Any method such as sputtering, evaporation, chemical vapor deposition (CVD), etc. may be used.

[0027] Since the metal film 19 formed on the back surface 16 of the metal film 19 has a different thermal shrinkage rate from that of the wafer 10, the difference in thermal shrinkage rate makes the wafer 10 more susceptible to warping and the like after the formation of the metal film 19 than before the formation of the metal film 19. Therefore, if the rigidity of the wafer 10 after grinding to be thinned is insufficient, deformation such as warping will occur in the wafer 10, and the magnitude of the deformation that occurs may be larger than that before the formation of the metal film.

[0028] Large deformation of the wafer 10 is likely to cause the above-mentioned errors or damage to the wafer 10. For this reason, when a metal film is formed during the processing of the wafer 10, it is extremely important to ensure sufficient rigidity of the wafer 10 after grinding to suppress deformation of the wafer 10.

[0029] After the metallization process, each device 14 is tested for electrical characteristics.

[0030] 5 is a cross-sectional view showing an example of a support member fixing step. In the support member fixing step performed after testing of the device 14, a frame set is formed in which the wafer 10 and a ring frame 21, which is a support member, are integrated by a dicing tape 20.

[0031] There is no particular limitation on the method for forming the frame set. For example, a frame set may be formed by pressing a dicing tape 20 pulled out from a roll tape (not shown) against the ring frame 21 and the wafer 10 with an application roller 202 shown in FIG. 5 while rotating the application roller 202, thereby adhering the dicing tape 20 to the ring frame 21 and the wafer 10.

[0032] The dicing tape 20 is applied while the wafer 10 is held by suction on the table 201. However, if the wafer 10 is deformed, such as warped, due to insufficient rigidity of the wafer 10 after grinding, a gap will be generated between the holding surface of the table 201 and the front surface 11 of the wafer 10, making it difficult to hold the wafer 10 firmly by suction.

[0033] If the wafer 10 cannot be held securely by suction, it will be difficult to attach the dicing tape 20, which will increase the occurrence of errors in the support member fixing process. In order to avoid the occurrence of such errors, it is necessary to ensure sufficient rigidity of the wafer 10 after grinding to suppress deformation of the wafer 10.

[0034] Fig. 6 is a perspective view showing an example of the ring-shaped reinforcement portion removing step. Fig. 7 is a cross-sectional view showing an example of the ring-shaped reinforcement portion removing step. After the frame set is formed, the frame set is placed in a cutting device equipped with a cutting mechanism 300 (see Figs. 6 and 7).

[0035] In the cutting device, the back surface 16 of the wafer 10 is held by a holding table 310 shown in Fig. 7, and the ring frame 21 is held by a clamp (not shown). As a result, the frame set is held in the cutting device with the front surface 11 facing the cutting mechanism 300.

[0036] The holding table 310 is a chuck table equipped with a porous plate 312 embedded in a recess of a frame 311. The wafer 10 is sucked and held on the holding table 310 by using a negative pressure generated on the surface of the porous plate 312 by the suction operation of a suction source (not shown).

[0037] When the frame set is held on the holding table 310, the cutting device performs a circle cut on the wafer 10. Specifically, as shown in Figures 6 and 7, the cutting mechanism 300 lowers toward the wafer 10 while rotating the spindle 302, thereby pressing the cutting blade 301 against the boundary between the device region 12 and the outer peripheral excess region 13 on the front surface 11 of the wafer 10 to cut the wafer 10. At this time, the frame set rotates together with the holding table 310 as a result of the rotation of a spindle (not shown) of the holding table 310, which has a rotation axis in a direction perpendicular to the spindle 302 of the cutting mechanism 300.

[0038] As a result, the cutting blade 301 of the cutting mechanism 300 cuts the wafer 10 in a circular shape along the boundary between the device region 12 and the peripheral surplus region 13 of the wafer 10, separating the device region 12 from the peripheral surplus region 13. This removes the ring-shaped reinforcing portion 18 formed in the region corresponding to the peripheral surplus region 13 from the wafer 10 (device region 12).

[0039] 8 is a perspective view showing an example of the dividing process. In the dividing process performed after the circle cut, a cutting mechanism 300 cuts and dices the wafer 10 along the dividing lines 15, thereby dividing the wafer 10 into chips on which individual devices 14 are formed.

[0040] Specifically, the cutting mechanism 300 rotates the spindle 302 while descending toward the wafer 10, thereby pressing the cutting blade 301 against the division lines 15 to cut the wafer 10. At this time, the base of the holding table 310 is moved in a direction parallel to the division lines 15, thereby dividing the wafer 10 along the division lines 15. By performing such processing for each division line 15, the wafer 10 is divided into chips on which individual devices 14 are formed.

[0041] Next, a wafer grinding method for suppressing a decrease in rigidity of the thinned, ground wafer 10 will be described in detail with reference to FIGS.

[0042] As a result of intensive research, the inventors of the present application have concluded that the reason why deformation of a wafer is likely to occur when a large-diameter wafer is thinned is that the ring-shaped reinforcing part does not sufficiently support the thinned wafer after grinding, that is, due to insufficient support by the ring-shaped reinforcing part.The inventors have also found that, in a wafer grinding method, by forming a ring-shaped reinforcing part that sufficiently supports the thinned wafer after grinding, it is possible to make it difficult for deformation of the wafer to occur even when a large-diameter wafer is thinned.

[0043] Considering that the thickness of the ring-shaped reinforcing part formed in TAIKO grinding corresponds to the original thickness of the wafer, in the wafer grinding method, the wafer should have a thickness (original thickness) that suppresses the deformation of the wafer with the recess formed therein by the ring-shaped reinforcing part. In the grinding method according to the present embodiment, a wafer that satisfies such a condition is used.

[0044] In the following, an example will be described in which a grinding method is used for a silicon wafer having devices formed thereon, in which the wafer has an original thickness such that deformation of the wafer is suppressed by a ring-shaped reinforcing portion.

[0045] Figure 9 is an explanatory diagram showing the relationship between wafer diameter and thickness in the SEMI standard. The SEMI standard is a standard established by SEMI (Semiconductor Equipment and Materials International), an international industry organization of semiconductor manufacturing equipment manufacturers, material manufacturers, etc.

[0046] In the SEMI standard, the relationship between diameter and thickness is defined as the standard specification for silicon wafer dimensions as shown in Figure 9. For this reason, it is believed that the relationship between diameter and thickness of most silicon wafers on the market also satisfies the relationship shown in Figure 9.

[0047] Fig. 10 is an explanatory diagram showing the relationship between the diameter, thickness, and diameter / thickness ratio of a wafer. The white background indicates the specifications of a wafer that is unlikely to deform after TAIKO grinding, and the black background indicates the specifications of a wafer that is likely to deform after TAIKO grinding or is not suitable for practical use.

[0048] In Fig. 10, the specifications within the range of the SEMI standard for 12-inch wafers are shown with a black background because, when thinning large-diameter wafers with a diameter of about 300 mm (12 inches) or more, the wafers are likely to deform even if TAIKO grinding is performed. In addition, the specifications for wafers that are too thick (diameter 300 mm, thickness 10 mm) are also shown with a black background because they are judged to be impractical from the perspective of grinding costs.

[0049] The inventors of the present application noticed that when 12-inch wafers are thinned, the wafers are prone to deformation even when TAIKO grinding is performed. When they checked 12-inch wafers that had been ground using TAIKO, they discovered that the ring-shaped reinforcement portion had been deformed along with the recessed portion, and concluded that the insufficient thickness (original thickness) of 12-inch wafers that meet the standard specifications was causing insufficient support for the wafer by the ring-shaped reinforcement portion.

[0050] According to the SEMI standard 12-inch wafer specifications, 12-inch wafers with a maximum thickness of 795 μm are thought to be distributed on the market, and wafers with a thickness of 800 μm or more, which exceeds the thickness (original thickness) of 12-inch wafers that meet the standard specifications, are not distributed on the market. By using such uncommon wafers with a thickness of 800 μm or more, the thickness of the ring-shaped reinforcing portion is also thicker than conventional ones, making it possible to suppress deformation of the wafer after grinding more than conventionally.

[0051] Therefore, in the wafer grinding method, it is desirable that the thickness of the wafer is 800 μm or more. By deliberately using such a wafer that does not meet the SEMI standard, it is possible to impart high rigidity to the wafer after grinding without attaching a support substrate, and therefore it is possible to obtain the effect of suppressing deformation of the wafer.

[0052] Furthermore, as a result of examining the relationship shown in FIG. 10, the inventors of the present application have noticed that the ratio of the original thickness to the diameter of a standard specification wafer defined by the SEMI standard shown in FIG. 9 becomes smaller as the diameter of the wafer increases, as shown below, and have concluded that the decrease in the ratio of thickness to diameter is the cause of the tendency of the wafer to become deformed when a large diameter wafer is thinned. 4 inch wafer: 0.0052 5 inch wafer: 0.005 6 inch wafer: 0.0045 8 inch wafer: 0.00363 12 inch wafer: 0.00258

[0053] Furthermore, since wafer deformation is unlikely to occur after TAIKO grinding for wafers up to 8 inches, but is relatively likely to occur after TAIKO grinding for 12 inches, it was concluded that as long as the thickness-to-diameter ratio of 8-inch wafers is maintained, wafer deformation can be suppressed after TAIKO grinding regardless of wafer size.

[0054] Therefore, in the wafer grinding method, it is desirable that the wafer satisfies the following formula (1). Wafer thickness >= wafer diameter × 0.725 / 200 (1)

[0055] By using a wafer that satisfies formula (1), regardless of the wafer size (inches, diameter), high rigidity can be imparted to the ground wafer without attaching a support substrate, making it possible to suppress deformation of the wafer after TAIKO grinding. In particular, when using wafers with a diameter of 300 mm or more, it is desirable to satisfy formula (1). This makes it possible to suppress deformation of the wafer after grinding, which was likely to occur when using 12-inch wafers that meet the standard specifications of the SEMI standard.

[0056] Fig. 11 is an explanatory diagram showing thresholds of coefficients which are the ratios of the diameter and thickness of a wafer. In Fig. 11, the ratios (coefficients) of the diameter and thickness of a wafer in the above-mentioned two specific examples are shown as thresholds. The threshold THa is the ratio (coefficient) of the thickness and diameter of a 12-inch wafer having a thickness of 800 μm, and is 0.00267. The threshold THb is the ratio (coefficient) of the thickness and diameter of a 12-inch wafer that meets the standard specifications of the SEMI standard, and is 0.00363.

[0057] In the wafer grinding method, by using a wafer having a ratio (coefficient) equal to or greater than the threshold value THa, it is possible to increase the rigidity of the wafer after TAIKO grinding more than conventionally, particularly for 12-inch wafers, and thus to suppress deformation of the wafer. In addition, by using a wafer having a ratio (coefficient) equal to or greater than the threshold value THb, it is possible to ensure sufficient rigidity of the wafer after TAIKO grinding regardless of the wafer size, and thus to more reliably suppress deformation of the wafer.

[0058] Therefore, by using a wafer having a ratio at least equal to or greater than the threshold value THa, it is possible to suppress the occurrence of various errors, including wafer breakage, in the process after TAIKO grinding. Also, by using a wafer having a ratio equal to or greater than the threshold value THb, it is possible to further suppress the occurrence of various errors in the process after TAIKO grinding.

[0059] Various errors that occur in processes after TAIKO grinding due to wafer deformation include transport errors in processes after the grinding process, errors in which the wafer bends and breaks while being stored in a cassette after the grinding process, and errors in which the wafer cannot be sucked and held on the holding table in the support member fixing process.

[0060] The embodiments of the present invention are not limited to the above-mentioned embodiments, and may be variously changed, substituted, or modified within the scope of the spirit of the technical idea of ​​the present invention. Furthermore, if the technical idea of ​​the present invention can be realized in a different way due to the progress of technology or another derived technology, it may be implemented using that method. Therefore, the claims cover all embodiments that can be included within the scope of the technical idea of ​​the present invention. [Industrial Applicability]

[0061] As described above, according to the wafer grinding method of the present invention, it is possible to impart high rigidity to the ground wafer without attaching a support substrate, which is extremely useful in grinding large-diameter wafers that tend to lack rigidity after grinding. [Explanation of symbols]

[0062] 10: Wafer 11: Surface 12: Device area 13: Surplus outer area 14: Device 15: Planned division line 16: Back side 17: Recess 18: Ring-shaped reinforcement section 19: Metal film 20: Dicing tape 21: Ring frame 100: Grinding mechanism 101: Spindle 102: Mount 103: Grinding wheel 104: Grinding wheel 110: Holding table 201: Table 202: Adhesive roller 300: Cutting mechanism 301: Cutting blade 302: Spindle 310: Holding table 311: Frame 312:Porous plate THa, THb: Threshold

Claims

1. A method for grinding a wafer, comprising the steps of: a grinding step of grinding a central region of the wafer held on a holding table with a grinding wheel to form a recess and to form a ring-shaped reinforcing portion on an outer periphery of the recess; The wafer has a thickness such that deformation of the wafer in which the recess is formed is suppressed by the ring-shaped reinforcing portion. The wafer grinding method is characterized by the above.

2. On the surface of the wafer, a device region having a plurality of devices formed therein; a peripheral excess area surrounding the device area; The ring-shaped reinforcing portion is formed in a region corresponding to the outer peripheral excess region.

2. The method for grinding a wafer according to claim 1,

3. The thickness of the wafer is 800 μm or more.

3. The method for grinding a wafer according to claim 1 or 2, characterized in that

4. The wafer is The thickness of the wafer >= the diameter of the wafer × 0.725 / 200 Satisfy the formula 3. The method for grinding a wafer according to claim 1 or 2, characterized in that

5. The diameter of the wafer is 300 mm or more.

3. The method for grinding a wafer according to claim 1 or 2, characterized in that

Citation Information

Patent Citations

  • Method for processing wafer and wafer

    JP2007019461A

  • Grinding method

    JP2022044315A