Biodegradable plastic, and method for producing biodegradable plastic

By integrating fungal mycelium from specific species into biodegradable plastics, the method effectively accelerates and maintains decomposition in marine environments, overcoming the challenges of prolonged persistence.

JP2024166737APending Publication Date: 2024-11-29TOYO SEIKAN GRP HLDG LTD

Patent Information

Application Number
JP2023083050
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

Smart Images

  • Figure 2024166737000001_ABST
    Figure 2024166737000001_ABST
Patent Text Reader

Abstract

To provide a biodegradable plastic that can be optimally degraded in the ocean environment.SOLUTION: A biodegradable plastic contains fungal mycelium capable of degrading biodegradable plastic. Preferably, the fungal mycelium is in a powdered form. Preferably, the biodegradable plastic is at least one synthetic polymer selected from the group consisting of aliphatic polyester, aromatic polyester, and their derivatives and mixtures of them.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plastic decomposition technology, and more particularly to a plastic decomposition technology using microorganisms. [Background technology]

[0002] In recent years, marine pollution by plastics has become a problem. In other words, most plastics that flow into the environment end up in rivers and other bodies of water, eventually ending up in the ocean, causing enormous damage to the marine ecosystem. The impact of plastics on the ocean also damages industry, resulting in huge economic losses. Plastic breaks down into microplastic particles in the ocean, but even when ordinary plastic breaks down into smaller pieces, it does not naturally decompose and is thought to remain for hundreds of years or more.

[0003] In this situation, the use of biodegradable plastics that can decompose naturally is becoming widespread in place of conventional plastics. However, even if biodegradable plastics are used, the marine environment is fluid and the types and amounts of microorganisms change over time, so it takes time for them to decompose naturally, and some types of biodegradable plastics may remain in the ocean for long periods of time. For this reason, it is difficult to solve the problem of marine pollution by biodegradable plastics alone. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 3-179036 [Patent Document 2] JP 2002-356623 A [Patent Document 3] Patent No. 6310843 [Patent Document 4] Patent No. 6985154 Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, the inventors conducted intensive research into methods for efficiently decomposing biodegradable plastics in the marine environment by incorporating biomaterials into the biodegradable plastics, and succeeded in efficiently decomposing biodegradable plastics in the marine environment by incorporating the mycelium of a fungus capable of decomposing biodegradable plastics into the biodegradable plastics, thereby completing the present invention.

[0006] It is also desirable to allow the decomposition effect of the fungal mycelium in such biodegradable plastics to persist for a long period of time. Moreover, in order to make it possible to easily mix fungal mycelium with biodegradable plastics, it is preferable to obtain fungal mycelium having excellent heat resistance. Therefore, the inventors of the present invention have conducted further intensive research and have succeeded in developing a method for producing biodegradable plastics that makes this feasible.

[0007] Here, Patent Documents 1 to 4 disclose biodegradable plastics containing biomaterials. However, these documents do not state or suggest that biodegradable plastics can be decomposed favorably in a marine environment by incorporating mycelium of a fungus capable of decomposing biodegradable plastics into the biodegradable plastics. Furthermore, these documents do not describe or suggest any method for maintaining the decomposition effect of fungal mycelium in biodegradable plastics for a long period of time, or any method for obtaining fungal mycelium with excellent heat resistance.

[0008] The present invention has been made in consideration of the above circumstances, and aims to provide a biodegradable plastic that can be decomposed suitably in a marine environment, and a method for producing a biodegradable plastic. [Means for solving the problem]

[0009] In order to achieve the above object, the biodegradable plastic of the present invention is configured to contain mycelium of a fungus capable of decomposing biodegradable plastic. In addition, it is preferable that the biodegradable plastic of the present invention is configured such that the mycelium of the fungus is in a powdered form.

[0010] In addition, it is preferable that the biodegradable plastic of the present invention is configured such that the biodegradable plastic is at least one synthetic polymer selected from the group consisting of aliphatic polyesters, aromatic polyesters, and derivatives thereof, and mixtures thereof.

[0011] Furthermore, it is preferable that the biodegradable plastic of the present invention is configured such that the synthetic polymer is selected from the group consisting of polycaprolactone (PCL), polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polylactic acid (PLA), polyhydroxyalkanoate (PHA), polyglycolic acid (PGA), polyethylene terephthalate succinate (PETS), starch polyester, and polybutylene succinate terephthalate (PBST).

[0012] In the biodegradable plastic of the present invention, the fungus is preferably a filamentous fungus. In addition, it is preferable that the biodegradable plastic of the present invention is configured so that the filamentous fungus is an imperfect fungus or an Ascomycete fungus, and it is also preferable that the filamentous fungus is a fungus belonging to the genus Aspergillus, Fusarium, or Glomerella.

[0013] The biodegradable plastic of the present invention preferably contains 0.001% to 10% by mass of powder of the mycelium of the fungus. Furthermore, it is also preferable that the biodegradable plastic of this embodiment has a configuration in which the configurations of the biodegradable plastics described above are combined in various ways.

[0014] The method for producing a biodegradable plastic according to this embodiment is a method for incorporating mycelium of a fungus capable of decomposing the biodegradable plastic into the biodegradable plastic. In addition, the method for producing a biodegradable plastic of this embodiment is preferably a method in which the mycelium of the fungus is powdered and added to the biodegradable plastic.

[0015] In addition, it is preferable that the manufacturing method of biodegradable plastic of this embodiment is a method including the steps of inoculating a liquid culture medium with the filamentous fungus of the fungus, culturing the filamentous fungus in a stationary or agitated state for a predetermined period of time to create a mycelium mat of the filamentous fungus, harvesting the mycelium mat, drying the mycelium mat for a predetermined period of time, and powdering the dried mycelium mat.

[0016] Furthermore, the method for producing a biodegradable plastic of this embodiment is preferably a method for improving the resistance of the mycelium of the fungus by adding glucose, trehalose, and / or sucrose to the liquid medium, and the resistance is preferably storage resistance or heat resistance.

[0017] In addition, in the method for producing biodegradable plastics of this embodiment, it is preferable that the filamentous fungus is selected from the genus Fungi Imperfecti or the genus Ascomycota, and it is also preferable that the filamentous fungus is selected from the genus Aspergillus, the genus Fusarium, or the genus Glomerella.

[0018] In addition, the method for producing a biodegradable plastic of this embodiment is preferably a method in which the powder of the mycelium is dispersed in a biodegradable plastic dissolved in an organic solvent, and molding is performed by a solution casting method. It is also preferable that the method for producing a biodegradable plastic of this embodiment is a method in which the powder of the mycelium is dispersed in a heat-melted biodegradable plastic and molded by a melt kneading method. Furthermore, in the manufacturing method of biodegradable plastics of this embodiment, it is also preferable that the molding step is a method in which the powder of mycelium is molded into a film, thin film, or block. Effect of the Invention

[0019] According to the present invention, it is possible to provide a biodegradable plastic that can be decomposed suitably in a marine environment, and a method for producing a biodegradable plastic. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a diagram showing the results of a degradation test (PCL) in artificial seawater of a biodegradable plastic according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing the results of a degradation test (PBAT) in artificial seawater of a biodegradable plastic according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a diagram showing the results of a decomposition test in artificial seawater (PBSA) of a biodegradable plastic according to an embodiment of the present invention. [Figure 4] FIG. 1 is a diagram showing the results of a test to confirm the effect of the bioactivity of encapsulated microorganisms on decomposition of a biodegradable plastic according to an embodiment of the present invention. [Diagram 5] FIG. 1 is a diagram showing the results of a degradation test (PCL) in natural seawater of a biodegradable plastic according to an embodiment of the present invention. [Figure 6] FIG. 2 is a diagram showing the results of a degradation test (PBAT) in natural seawater of a biodegradable plastic according to an embodiment of the present invention. [Figure 7] FIG. 1 is a diagram showing the results of a decomposition test in natural seawater (PBSA) of a biodegradable plastic according to an embodiment of the present invention. [Figure 8] FIG. 1 is a diagram showing the results of a test to confirm the preservation of fungal mycelium contained in a biodegradable plastic according to an embodiment of the present invention. [Figure 9] FIG. 2 is a diagram showing the results of a test to confirm the heat resistance of fungal mycelium contained in a biodegradable plastic according to an embodiment of the present invention. [Figure 10]FIG. 1 is a diagram showing the results of a decomposition test on an artificial seawater agar medium of a biodegradable plastic produced by a melt-kneading method according to an embodiment of the present invention. [Figure 11] FIG. 1 is a diagram showing the results of a decomposition test on a natural seawater agar medium of a biodegradable plastic produced by a melt-kneading method according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the embodiments of the biodegradable plastic and the method for producing the biodegradable plastic of the present invention will be described in detail. However, the present invention is not limited to the specific contents of the following embodiments and examples described later.

[0022] The biodegradable plastic of this embodiment is characterized by containing the mycelium of a fungus capable of decomposing biodegradable plastics. In this embodiment, the biodegradable plastic is preferably at least one synthetic polymer selected from the group consisting of aliphatic polyesters, aromatic polyesters, and derivatives thereof, and mixtures thereof.

[0023] Also, the synthetic polymer is preferably selected from the group consisting of polycaprolactone (PCL), polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polylactic acid (PLA), polyhydroxyalkanoate (PHA), polyglycolic acid (PGA), polyethylene terephthalate succinate (PETS), starch polyester, and polybutylene succinate terephthalate (PBST).

[0024] In the biodegradable plastic of this embodiment, the fungal mycelium is preferably a filamentous fungus, and the filamentous fungus is preferably a fungus imperfecti or an ascomycete. In addition, it is preferable to use, as the filamentous fungus, a fungus belonging to the genus Aspergillus, Fusarium, Glomerella, Penicillium, or Pacillomyces.

[0025] In the biodegradable plastic of this embodiment, the fungal mycelium is preferably contained in a powdered form. Furthermore, in the biodegradable plastic of this embodiment, the fungal mycelium powder is preferably contained in an amount of 0.001% to 10% by mass, and more preferably 0.001% to 5% by mass.

[0026] The method for producing a biodegradable plastic according to this embodiment is characterized in that mycelium of a fungus capable of decomposing a biodegradable plastic is added to the biodegradable plastic to be contained therein. In addition, in the method for producing a biodegradable plastic according to this embodiment, it is preferable that the mycelium of the fungus is powdered and added to the biodegradable plastic.

[0027] Furthermore, the method for producing a biodegradable plastic according to this embodiment preferably includes the following steps. (1) Inoculating a liquid medium with a fungal filamentous fungus (2) A step of culturing the filamentous fungus for a predetermined period of time under static or agitated conditions to produce a mycelium mat of the filamentous fungus. (3) Harvesting mycelium mat (4) A process of drying the mycelium mat for a specified period of time. (5) A process for powdering the dried mycelium mat

[0028] Specifically, as described later in the Examples, for example, a colony obtained by pre-culture can be cut into pieces of approximately 5 mm square using a spatula or the like, and the pieces can be inoculated into Czapek liquid medium or the like and cultured statically in a dark place at 25°C to create a mycelium mat consisting of filamentous fungi on the surface of the liquid medium. After the static culture period, the mycelium mat formed on the surface of the liquid medium can be harvested and dried at room temperature for a certain period of time. The dried mycelium mat can then be powdered by sealing it together with zirconia balls in a screw-cap tube and shaking it with a mini bead beater.

[0029] In the method for producing a biodegradable plastic according to the present embodiment, it is preferable to improve the resistance of the fungal mycelium by adding glucose, trehalose, and / or sucrose to the liquid medium. In addition, it is preferable that the resistance is storage stability or heat resistance.

[0030] In addition, in the method for producing biodegradable plastics of this embodiment, it is preferable to select the filamentous fungus from the Deuteromycetes or Ascomycetes, and it is also preferable to select the filamentous fungus from the genera Aspergillus, Fusarium, Glomerella, Penicillium, or Pacillomyces.

[0031] In addition, in the method for producing a biodegradable plastic according to this embodiment, it is preferable to disperse powder of mycelium in a biodegradable plastic dissolved in an organic solvent and mold the resulting product by a solution casting method. In addition, in the method for producing a biodegradable plastic according to this embodiment, it is also preferable to disperse powder of mycelium in heat-melted biodegradable plastic and mold the plastic by a melt kneading method. In these molding processes, it is preferable to mold the mycelium powder into a film, thin film, or block shape.

[0032] Specifically, as described later in the Examples, in the solution casting method, for example, a predetermined amount of resin pellets is added to a glass vial, and while stirring the pellets, a solution capable of dissolving the biodegradable resin (e.g., chloroform) is added and stirred until completely dissolved. Then, a predetermined amount of mycelium powder is added to the stirred chloroform solution in which the resin has completely dissolved, and after stirring, the mixture is immediately poured into a glass petri dish and air-dried in a draft environment until the chloroform disappears, thereby producing a film containing mycelium powder. Furthermore, when mass-producing the biodegradable plastic of this embodiment using a solution casting method, it is possible to obtain the plastic by, for example, adding mycelium powder to a solution in which a resin is dissolved in a solvent, and then applying, spraying, or impregnating the resulting solution onto a support.

[0033] In the melt kneading method, for example, a predetermined amount of resin pellets is added to a microtube, which is then placed in a block heater set at a predetermined temperature and heated for a certain period of time until the pellets lose their shape and become candy-like. A predetermined amount of mycelium powder is then added to the candy-like resin, which is then kneaded with a spatula or the like to produce resin pieces containing mycelium powder. Furthermore, when mass-producing the biodegradable plastic of this embodiment using the melt kneading method, it is possible to obtain the plastic by, for example, feeding mycelium powder together with resin pellets into a continuous extruder using a screw or the like, and cutting the extruded resin or injecting it into a mold for molding.

[0034] According to the biodegradable plastic and the method for producing the biodegradable plastic of this embodiment, it is possible to decompose the biodegradable plastic favorably in a marine environment. EXAMPLES

[0035] Tests conducted to confirm the effects of the biodegradable plastic and the method for producing the biodegradable plastic according to the embodiment of the present invention will be described below.

[0036] [Test 1] A test was carried out on the decomposition promoting effect of the biodegradable plastic produced according to this embodiment in artificial seawater.

[0037] First, the fungal mycelium to be contained in the biodegradable plastic was prepared as follows. 1. Preculture Stock strains that had been frozen (-80°C) were inoculated into PDA medium (Potato Dextrose Agar) and cultured in the dark at 25°C for approximately 1 to 2 weeks. The following three types of stock strains were used: Strain A: Aspergillus flavus NBRC6343 Strain B: Fusarium oxysporum NBRC9971 Strain C: Glomerella cingulata NBRC107004

[0038] 2. Inoculation into liquid medium and preparation of mycelium mat The formed colonies were cut into pieces of about 5 mm square using a spatula, and the pieces were inoculated into Czapek liquid medium (0.3% NaNO3, 0.1% K2HPO4, 0.05% MgSO4·7H2O, 0.05% KCl, 0.001% FeSO4·7H2O) containing 3% (w / v) glucose, and cultured statically in the dark at 25°C. This produced a mycelium mat consisting of filamentous fungi on the surface of the liquid medium.

[0039] The static culture periods for each strain are as follows. Note that there is no special significance to the length of these periods. The same applies to the static culture periods and drying periods for each strain in the following tests. Strain A: 192 days Strain B: 101 days Strain C: 101 days

[0040] 3. Mycelium Mat Collection After a period of static cultivation, the mycelial mat that formed on the surface of the liquid medium was harvested.

[0041] 4. Drying the Mycelium Mat The mycelium mat was allowed to dry at room temperature for a period of time. The drying periods for each strain were as follows: Strain A: 126 days Strain B: 31 days Strain C: 31 days

[0042] 5. Powderization of Mycelial Mat The dried mycelium mat and two zirconia balls (approximately 3.0 mm in diameter) were placed in a 2 ml screw-cap tube and shaken at 2500 rpm for 120 seconds using a mini bead beater BSP-3110BX to powderize the dried mycelium mat and obtain a powdered form of fungal mycelium (mycelium powder).

[0043] Next, a biodegradable plastic was prepared by solution casting as follows. 6. Dissolving the resin with chloroform A given amount of resin pellets was added to a glass vial (size: capacity 19 ml), and 2 ml of chloroform was added while stirring the pellets, followed by stirring for about 2 to 3 hours until the pellets were completely dissolved. The following resin pellets were used: ·PCL (Polycaprolactone): PLACCEL H8C Lot.H8C-AJ-D01 (Daicel Corporation)

[0044] 7.Completion of biodegradable plastic A predetermined amount of mycelium powder was added to the stirred chloroform solution in which the resin had been completely dissolved, and after stirring for about 40 seconds, the powder was immediately poured into a glass petri dish (diameter 50 mm x height 30 mm) and air-dried in a draft environment for about 2 hours until the chloroform had disappeared, creating a film containing the mycelium powder and obtaining the biodegradable plastic of this embodiment.

[0045] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A: PCL 208.1 mg + Strain A 10.0 mg (mycelium concentration 4.6%) Strain B: PCL 202.0mg + Strain B 9.2mg (4.4%) Strain C: PCL 194.1 mg + Strain C 9.7 mg (4.8%)

[0046] Next, the decomposition of the biodegradable plastic was confirmed as follows. 8. Preparation of Artificial Seawater NaNO3 was added to Daigo Artificial Seawater SP for Marine Microalgae Cultivation at a ratio of 36g / L to make it 0.3% (w / v). Then, 25ml of artificial seawater was dispensed per flask and autoclaved. NaNO3 was added to promote the growth of mycelium by introducing a nitrogen source into the artificial seawater. [Table 1]

[0047] 9. Exposure of biodegradable plastics to an artificial seawater environment Using scissors disinfected with ethanol, the biodegradable plastic film was cut into approximately 10-20 mm squares, and 2-4 pieces of the film were placed in each flask so that the amount of biodegradable plastic was approximately the same. In this way, the mycelium powder on the cut surface was exposed to water to promote mycelium growth. The blank in this test was artificial seawater into which a film slice not containing mycelium powder was placed. The same was true for tests 2-4 and 10. In this manner, the biodegradable plastic was exposed to an artificial seawater environment for 88 days under shaking conditions of 25°C and 130 rpm.

[0048] 10. Calculation of weight loss rate of biodegradable plastics After exposure to the above artificial seawater environment, only those that were visually confirmed to be films or parts of films were collected and weighed, and the weight loss rate was calculated using the following formula. Weight reduction rate (%) = (film weight before insertion - film weight at time of recovery) / film weight before insertion × 100

[0049] 11. Calculation of growth section rate In order to confirm the bioactivity of the fungal mycelium in the biodegradable plastic of this embodiment used in the exposure to the above-mentioned artificial seawater environment, the growth slice rate was calculated as follows.

[0050] On the day of preparation, the film containing the mycelium powder was cut to an appropriate size (approximately 5 x 5 mm square), immediately placed on PDA medium, and left in a dark place at 25°C. After 1 to 2 weeks, the percentage of slices in which mycelium contained in the film was found to have grown was calculated. At this time, the growth of mycelium contained in the film was confirmed for all 9 sections. In addition, blank films containing no mycelium were similarly placed on PDA medium for all 6 sections to confirm the absence of mycelium growth.

[0051] FIG. 1 shows the weight loss rate of biodegradable plastic for each strain obtained as described above, as well as the encapsulation concentration of mycelium and the rate of growing pieces in each biodegradable plastic. As shown in Figure 1, the weight loss rates of biodegradable plastics using strains A, B, and C were 20.1%, 90.7%, and 100.0%, respectively.

[0052] In addition, the encapsulation concentrations of strain A, strain B, and strain C in biodegradable plastics were 4.6%, 4.4%, and 4.8%, respectively, and the growth intercept rates were 100.0% (9 / 9), 66.7% (6 / 9), and 100.0% (9 / 9), respectively. As described above, it has been found that the biodegradable plastic and the method for producing the biodegradable plastic of this embodiment can promote the decomposition of the biodegradable plastic in an artificial seawater environment.

[0053] [Test 2] The decomposition-promoting effect of the biodegradable plastic produced according to this embodiment in artificial seawater was examined by changing the plastic used.

[0054] The fungal mycelium to be contained in the biodegradable plastic was the same as that prepared in Test 1. Moreover, the biodegradable plastic of this embodiment was prepared in the same manner as in Test 1, except for the following points. The following resin pellets were used: PBAT (Polybutylene Adipate Terephthalate): ECOFLEX F BLEND C1200 Lot.67510 624UO (BASF)

[0055] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A: PBAT 199.7 mg + Strain A 10.0 mg (mycelium concentration 4.8%) Strain B: PBAT 195.1 mg + Strain B 10.1 mg (4.9%) Strain C: PBAT 198.6 mg + Strain C 10.0 mg (4.8%)

[0056] Next, the decomposition of the biodegradable plastic was confirmed as follows. As in Test 1, artificial seawater was dispensed into flasks and autoclaved. Using scissors sterilized with ethanol, the biodegradable plastic film was cut into pieces of approximately 10 to 20 mm square, and 2 to 4 pieces of the film were placed into each of the above flasks so that the amount of biodegradable plastic was approximately the same.

[0057] The biodegradable plastic was then exposed to an artificial seawater environment for 88 days at 25°C and with shaking at 130 rpm. In addition, similarly to Test 1, the weight loss rate of the biodegradable plastic and the growth slice rate were calculated.

[0058] FIG. 2 shows the weight loss rate of the biodegradable plastic for each strain obtained as described above, as well as the encapsulation concentration of mycelium and the rate of growing pieces in each biodegradable plastic. As shown in Figure 2, the weight loss rates of biodegradable plastics using strain A, strain B, and strain C were 0.0%, 4.6%, and 1.8%, respectively.

[0059] In addition, the encapsulation concentrations of strains A, B, and C in biodegradable plastics were 4.8%, 4.9%, and 4.8%, respectively, and the growth intercept rates were 100.0% (9 / 9), 66.7% (6 / 9), and 100.0% (9 / 9), respectively. As described above, according to the biodegradable plastic and the method for producing the biodegradable plastic of this embodiment, it was confirmed that when the plastic used is changed, strains B and C can promote the decomposition of biodegradable plastic in an artificial seawater environment.

[0060] [Test 3] The decomposition-promoting effect of the biodegradable plastic produced according to this embodiment in artificial seawater was examined by changing the plastic used.

[0061] The fungal mycelium to be contained in the biodegradable plastic was the same as that prepared in Test 1. Moreover, the biodegradable plastic of this embodiment was prepared in the same manner as in Test 1, except for the following points. The following resin pellets were used: ·PBSA (Polybutylene succinate adipate): BioPBS TM FD92 (Mitsubishi Chemical Corporation)

[0062] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A: PBSA 206.2mg + Strain A 9.8mg (mycelium concentration 4.5%) Strain B: PBSA 206.8mg + Strain B 9.3mg (4.3%) Strain C: PBSA 202.0 mg + Strain C 10.0 mg (4.7%)

[0063] Next, the decomposition of the biodegradable plastic was confirmed as follows. As in Test 1, artificial seawater was dispensed into flasks and autoclaved. Using scissors sterilized with ethanol, the biodegradable plastic film was cut into pieces of approximately 10 to 20 mm square, and 2 to 4 pieces of the film were placed into each of the above flasks so that the amount of biodegradable plastic was approximately the same.

[0064] The biodegradable plastic was then exposed to an artificial seawater environment for 88 days at 25°C and with shaking at 130 rpm. In addition, similarly to Test 1, the weight loss rate of the biodegradable plastic and the growth slice rate were calculated.

[0065] FIG. 3 shows the weight loss rate of the biodegradable plastic for each strain obtained as described above, as well as the encapsulation concentration of mycelium and the rate of growing pieces in each biodegradable plastic. As shown in Figure 3, the weight loss rates of biodegradable plastics using strain A, strain B, and strain C were 8.3%, 52.2%, and 100.0%, respectively.

[0066] In addition, the encapsulation concentrations of strain A, strain B, and strain C in biodegradable plastics were 4.5%, 4.3%, and 4.7%, respectively, and the growth intercept rates were 100.0% (9 / 9), 77.8% (7 / 9), and 100.0% (9 / 9), respectively. As described above, it has been found that the biodegradable plastic and the method for producing the biodegradable plastic of this embodiment can promote the decomposition of the biodegradable plastic in an artificial seawater environment when the plastic used is changed.

[0067] [Test 4] A test was carried out to confirm the influence of the bioactivity of the encapsulated microorganisms (rate of growing pieces of mycelium) in the biodegradable plastic produced according to this embodiment on the decomposition promotion effect. Specifically, the decomposition promotion effect was compared between when the mycelium growth slice rate was high (Experiment 1) and when the mycelium growth slice rate was extremely low (Experiment 2).

[0068] Specifically, the biodegradable plastics in Experiment 2 were prepared in the same manner as in Test 1, except for the following points: The strain was the same as that in Test 1; and the results of Experiment 1 were the same as those of Strain C in Test 1. The mixing ratio of mycelium powder and resin in the biodegradable plastic in Experiment 2 was as follows: · Strain C: PCL211.1mg + Strain C9.7mg (4.4%)

[0069] Next, the decomposition of the biodegradable plastic in Experiment 2 was confirmed as follows. As in Test 1, artificial seawater was dispensed into flasks and autoclaved. Using scissors disinfected with ethanol, the film was cut into pieces of approximately 10 to 20 mm square, and 2 to 4 pieces of the film were placed in the above flask so that the amount of biodegradable plastic was approximately the same.

[0070] The biodegradable plastic was then exposed to an artificial seawater environment for 96 days at 25°C with shaking at 130 rpm. In addition, the weight loss rate of the biodegradable plastic and the rate of grown sections were calculated in the same manner as in Test 1. However, in Experiment 2, the growth of mycelium contained in the film was confirmed in all 22 sections. Of these, mycelium growth was confirmed in only one section.

[0071] As a result, as shown in Figure 4, the weight loss rate of the biodegradable plastic by strain C in experiment 1 was 100.0%. In addition, the encapsulation concentration of strain C in the biodegradable plastic was 4.8%, and the growth slice rate was 100.0% (9 / 9). On the other hand, the weight loss rate of the biodegradable plastic by strain C in experiment 2 was 0.0%. The encapsulation concentration of strain C in the biodegradable plastic was 4.4%, and the growth slice rate was 4.5% (1 / 22). These results confirmed that the greater the biological activity (rate of growing mycelium fragments) of the encapsulated microorganisms in biodegradable plastics, the greater the effect of promoting the decomposition of the biodegradable plastics.

[0072] [Test 5] A test was carried out on the decomposition promoting effect of the biodegradable plastic produced according to this embodiment in natural seawater.

[0073] The fungal mycelium to be incorporated into the biodegradable plastic was prepared as follows. First, pre-culture and inoculation into liquid medium were performed in the same manner as in Test 1. However, only strain C was inoculated into PDA liquid medium (containing 2% (w / v) glucose). The static culture periods for each strain were as follows: Strain A: 152 days Strain B: 152 days Strain C: 101 days

[0074] After the static culture period, the mycelium mat formed on the surface of the liquid medium was collected and dried for a certain period under the following conditions. The drying period for each strain was as follows: Strain A: 92 days at 4°C Strain B: 92 days at 4°C Strain C: 17 days at room temperature, 38 days at 4°C, total 55 days

[0075] The dried mycelium mat was then powdered in the same manner as in Test 1 to obtain a powdered form of fungal mycelium (mycelium powder).

[0076] Next, a biodegradable plastic was prepared as follows. The following resin pellets were used: ·PCL (Polycaprolactone): PLACCEL H8C Lot.H8C-AJ-D01 (Daicel Corporation)

[0077] As in Test 1, the resin (PCL) was dissolved using chloroform, and a specified amount of mycelium powder was added to the stirred chloroform solution in which the resin had been completely dissolved. After stirring for approximately 40 seconds, the powder was immediately poured into a glass petri dish (diameter 50 mm x height 30 mm) and air-dried in a draft environment for approximately 2 hours until the chloroform had disappeared, creating a film containing the mycelium powder.

[0078] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A: PCL 200.4mg + Strain A 11.3mg (mycelium concentration 5.3%) Strain B: PCL 206.2mg + Strain B 10.5mg (4.8%) · Strain C: PCL211.1mg + Strain C9.7mg (4.4%)

[0079] Next, the decomposition of the biodegradable plastic was confirmed as follows. The natural seawater used was collected from the beach in front of Enoshima Aquarium on the morning of June 16, 2022. The pH of the collected seawater was 8.1, and the number of microorganisms contained was 1.3 × 10 4 The microbial count was measured using a standard agar medium (Nissui Co., Ltd.) prepared with artificial seawater.

[0080] The natural seawater was dispensed in 40 ml portions per flask for testing. The natural seawater was not autoclaved. Using scissors disinfected with ethanol, the biodegradable plastic film was cut into approximately 10-20 mm squares, and 2-4 pieces of the film were placed in each flask so that the amount of biodegradable plastic was approximately the same. The blank in this test was natural seawater into which a piece of film not containing mycelium powder was placed. The same was true for tests 6, 7, and 11.

[0081] The biodegradable plastic was then exposed to a natural seawater environment for 96 days at 25°C and with shaking at 130 rpm. In addition, the weight loss rate of the biodegradable plastic and the rate of viable slices were calculated in the same manner as in Test 1. However, in this test, the growth of mycelium contained in the film was confirmed based on various numbers of slices, and the rate of viable slices was calculated.

[0082] FIG. 5 shows the weight loss rate of the biodegradable plastic for each strain obtained as described above, as well as the encapsulation concentration of mycelium and the rate of growing pieces in each biodegradable plastic. As shown in Figure 5, the weight loss rates of biodegradable plastics using strain A, strain B, strain C, and the blank were 26.6%, 19.3%, 3.9%, and 12.5%, respectively. The weight loss rate of the biodegradable plastic in the blank is presumed to be due to the microorganisms contained in natural seawater. The same was true for Tests 6 and 7.

[0083] In addition, the encapsulation concentrations of strains A, B, and C in biodegradable plastics were 5.3%, 4.8%, and 4.4%, respectively, and the growth intercept rates were 100.0% (10 / 10), 0.0% (0 / 22), and 4.5% (1 / 22), respectively. It is presumed that the reason for the low weight loss rate of the biodegradable plastic when using strain C is that it may be antagonistic to the microorganisms contained in the natural seawater. Also, although the growth slice rate of strain B was 0.0%, it is possible that slices placed in the natural seawater environment contained slices that maintained their bioactivity, which is why it is presumed that the weight loss rate of the biodegradable plastic was greater than that of the blank. As described above, it has been confirmed that the biodegradable plastic and the method for producing a biodegradable plastic of this embodiment can promote the decomposition of biodegradable plastic in a natural seawater environment, at least with strain A.

[0084] [Test 6] The decomposition-promoting effect of the biodegradable plastic produced according to this embodiment in natural seawater was examined by changing the plastic used.

[0085] The fungal mycelium to be contained in the biodegradable plastic was the same as that prepared in Test 5. Moreover, a biodegradable plastic was prepared as follows. The following resin pellets were used: PBAT (Polybutylene Adipate Terephthalate): ECOFLEX F BLEND C1200 Lot.67510 624UO (BASF)

[0086] As in Test 1, the resin (PBAT) was dissolved using chloroform, and a specified amount of mycelium powder was added to the stirred chloroform solution in which the resin had been completely dissolved. After stirring for approximately 40 seconds, the powder was immediately poured into a glass petri dish (diameter 50 mm x height 30 mm) and air-dried in a draft environment for approximately 2 hours until the chloroform had disappeared, creating a film containing the mycelium powder.

[0087] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A: PBAT 205.8mg + Strain A 11.6mg (mycelium concentration 5.3%) Strain B: PBAT 198.4 mg + Strain B 10.1 mg (4.8%) Strain C: PBAT 205.9 mg + Strain C 8.9 mg (4.1%)

[0088] Next, the decomposition of the biodegradable plastic was confirmed as follows. The natural seawater used was the same as that prepared in Test 5. 40 ml of this natural seawater was dispensed into each flask for the test. The natural seawater was not autoclaved. Using scissors sterilized with ethanol, the biodegradable plastic film was cut into pieces of approximately 10 to 20 mm square, and 2 to 4 pieces of the film were placed into each of the above flasks so that the amount of biodegradable plastic was approximately the same.

[0089] The biodegradable plastic was then exposed to a natural seawater environment for 96 days at 25°C and with shaking at 130 rpm. In addition, the weight loss rate of the biodegradable plastic and the rate of viable slices were calculated in the same manner as in Test 1. However, in this test, the growth of mycelium contained in the film was confirmed based on various numbers of slices, and the rate of viable slices was calculated.

[0090] FIG. 6 shows the weight loss rate of the biodegradable plastic for each strain obtained as described above, as well as the encapsulation concentration of mycelium and the rate of growing pieces in each biodegradable plastic. As shown in Figure 6, the weight loss rates of biodegradable plastics using strain A, strain B, strain C, and the blank were 17.1%, 19.8%, 6.1%, and 11.8%, respectively.

[0091] In addition, the encapsulation concentrations of strains A, B, and C in biodegradable plastics were 5.3%, 4.8%, and 4.1%, respectively, and the growth intercept rates were 100.0% (10 / 10), 20.0% (2 / 10), and 0.0% (0 / 22), respectively. As described above, according to the biodegradable plastic and the method for producing the biodegradable plastic of this embodiment, it was confirmed that when the plastic used is changed, strain A and strain B can promote the decomposition of the biodegradable plastic in a natural seawater environment.

[0092] [Test 7] The decomposition-promoting effect of the biodegradable plastic produced according to this embodiment in natural seawater was examined by changing the plastic used.

[0093] The fungal mycelium to be contained in the biodegradable plastic was the same as that prepared in Test 5. Moreover, a biodegradable plastic was prepared as follows. The following resin pellets were used: ·PBSA (Polybutylene succinate adipate): BioPBS TM FD92 (Mitsubishi Chemical Corporation)

[0094] As in Test 1, the resin (PBSA) was dissolved using chloroform, and a specified amount of mycelium powder was added to the stirred chloroform solution in which the resin had been completely dissolved. After stirring for approximately 40 seconds, the solution was immediately poured into a glass petri dish (diameter 50 mm x height 30 mm) and air-dried in a draft environment for approximately 2 hours until the chloroform had disappeared, creating a film containing the mycelium powder.

[0095] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A: PBSA 200.4 mg + Strain A 11.0 mg (mycelium concentration 5.2%) Strain B: PBSA 207.0 mg + Strain B 10.0 mg (4.6%) · Strain C: PBSA205.1mg + strain C9.2mg (4.3%)

[0096] Next, the decomposition of the biodegradable plastic was confirmed as follows. The natural seawater used was the same as that prepared in Test 5. 40 ml of this natural seawater was dispensed into each flask for the test. The natural seawater was not autoclaved. Using scissors sterilized with ethanol, the biodegradable plastic film was cut into pieces of approximately 10 to 20 mm square, and 2 to 4 pieces of the film were placed into each of the above flasks so that the amount of biodegradable plastic was approximately the same.

[0097] The biodegradable plastic was then exposed to a natural seawater environment for 96 days at 25°C and with shaking at 130 rpm. In addition, the weight loss rate of the biodegradable plastic and the rate of viable slices were calculated in the same manner as in Test 1. However, in this test, the growth of mycelium contained in the film was confirmed based on various numbers of slices, and the rate of viable slices was calculated.

[0098] FIG. 7 shows the weight loss rate of the biodegradable plastic for each strain obtained as described above, as well as the encapsulation concentration of mycelium and the rate of growing pieces in each biodegradable plastic. As shown in Figure 7, the weight loss rates of biodegradable plastics using strain A, strain B, strain C, and the blank were 72.9%, 23.8%, 8.0%, and 6.9%, respectively.

[0099] In addition, the encapsulation concentrations of strains A, B, and C in biodegradable plastics were 5.2%, 4.6%, and 4.3%, respectively, and the growth intercept rates were 100.0% (10 / 10), 44.4% (4 / 9), and 15.0% (3 / 20), respectively. As described above, it has been found that the biodegradable plastic and the method for producing the biodegradable plastic of this embodiment can promote the decomposition of the biodegradable plastic in a natural seawater environment when the plastic used is changed.

[0100] [Test 8] Tests conducted to find a carbon source capable of improving the resistance of the fungal mycelium contained in the biodegradable plastic of this embodiment will be described below. In order for the biodegradable plastic of this embodiment to degrade favorably in a marine environment, it is desirable for the fungal mycelium in the biodegradable plastic to maintain its bioactivity for a long period of time. Therefore, this test was conducted to identify a carbon source to be used during liquid culture that is effective in improving the preservation of the fungal mycelium.

[0101] As in Test 1, fungal mycelium was prepared by inoculating frozen (-80°C) stock strains onto PDA medium (Potato Dextrose Agar) and culturing them in the dark at 25°C for approximately 1 to 2 weeks. The following two types of stock strains were used, with the experiment using strain B being experiment 3 and the experiment using strain C being experiment 4. Strain B: Fusarium oxysporum NBRC9971 Strain C: Glomerella cingulata NBRC107004 In addition, the same experiment was performed using strain A (Aspergillus flavus NBRC6343) and mycelial elongation was observed throughout all storage periods listed below. However, since strain A has particularly excellent drought resistance, the details are omitted here.

[0102] Next, each colony formed was cut into approximately 5 mm squares using a spatula, and the pieces were inoculated into Czapek liquid medium (0.3% NaNO3, 0.1% K2HPO4, 0.05% MgSO4·7H2O, 0.05% KCl, 0.001% FeSO4·7H2O) containing 3% (w / v) glucose or 3% (w / v) trehalose, and stored in the dark.

[0103] In experiment 3, the mycelium was stored at room temperature until the 17th day, and then at 4°C. The mycelium was powdered on the 91st day, and stored in this powdered state at 4°C until the 156th day. The survival of the mycelium was confirmed on the 45th, 91st, and 156th days. In experiment 4, the mycelium was stored at room temperature until day 203, then stored at 4°C from day 204, and powdered on day 206. The powdered mycelium was then stored at 4°C until day 384. The survival of the mycelium was confirmed on days 203, 322, and 384. The survival of the mycelium was confirmed by inoculating dried mycelium fragments or powder onto PDA medium and visually checking for growth. The results are shown in FIG.

[0104] As shown in FIG. 8, in Experiment 3, mycelial elongation was observed up to 91 days after inoculation and storage in Czapek liquid medium containing 3% (w / v) glucose, and mycelial elongation was observed up to 45 days after inoculation and storage in Czapek liquid medium containing 3% (w / v) trehalose. In addition, in experiment 4, when the culture was inoculated into Czapek liquid medium containing 3% (w / v) glucose and stored, hyphal elongation of the mycelium was observed up to 322 days, and when the culture was inoculated into Czapek liquid medium containing 3% (w / v) trehalose and stored, hyphal elongation of the mycelium was observed up to 203 days.

[0105] Thus, it was found that in the method for producing biodegradable plastics of this embodiment, the preservation quality of fungal mycelium can be improved by adding glucose and / or trehalose to the liquid medium in which the mycelium is cultured.

[0106] [Test 9] Tests conducted to find a carbon source capable of improving the resistance of the fungal mycelium contained in the biodegradable plastic of this embodiment will be described below. In the method for producing biodegradable plastics according to the present embodiment, it is desirable to maintain the bioactivity of the mycelium when the mycelium powder is kneaded into the heat-melted resin. Therefore, the present test was carried out to identify a carbon source that is effective in improving the heat resistance of fungal mycelium.

[0107] First, fungal mycelium to be contained in the biodegradable plastic was prepared as follows. 1. Preculture Stock strains that had been frozen (-80°C) were inoculated into PDA medium (Potato Dextrose Agar) and cultured in the dark at 25°C for approximately 1 to 2 weeks. The following two types of stock strains were used: Strain A: Aspergillus flavus NBRC6343 Strain C: Glomerella cingulata NBRC107004

[0108] 2. Inoculation into liquid medium and preparation of mycelium mat The formed colonies were cut into pieces of about 5 mm square using a spatula, and the pieces were inoculated into Czapek liquid medium (0.3% NaNO3, 0.1% K2HPO4, 0.05% MgSO4·7H2O, 0.05% KCl, 0.001% FeSO4·7H2O) containing 3% (w / v) glucose, 3% (w / v) trehalose, or 3% (w / v) sucrose, and cultured in the dark at 25°C. This produced a mycelial mat consisting of filamentous fungi on the surface of the liquid medium. The static culture periods for each strain were as follows: Strain A: A mixture of strains cultured for 36 and 192 days was used. Strain C: 101 days

[0109] 3. Mycelium Mat Collection After a period of static cultivation, the mycelial mat that formed on the surface of the liquid medium was harvested.

[0110] 4. Drying the Mycelium Mat The mycelium mats were allowed to dry for a set period of time. The drying periods for each strain were as follows: Strain A: 321 days at room temperature (cultured for 36 days) At room temperature for 164 days (cultured for 192 days) Strain C: 17 days at room temperature, 84 days at 4°C, total 101 days

[0111] 5. Powderization of Mycelial Mat The dried mycelium mat and two zirconia balls (approximately 3.0 mm in diameter) were placed in a 2 ml screw-cap tube and shaken at 2500 rpm for 120 seconds using a mini bead beater BSP-3110BX to powderize the dried mycelium mat and obtain a powdered form of fungal mycelium (mycelium powder).

[0112] Next, a biodegradable plastic was prepared by the melt kneading method as follows. 6. Thermal melting of resin A given amount of resin pellets was added to a microtube (size: capacity 2 ml), placed in a block heater set to a given temperature, and heated for a given time until the pellets lost their shape and became candy-like. The following resin pellets were used: ·PCL (Polycaprolactone): PLACCEL H8C Lot.H8C-AJ-D01 (Daicel Corporation)

[0113] The predetermined temperatures were 70°C, 90°C, 110°C, and 130°C for strain A, and 70°C, 85°C, and 100°C for strain C. Each mycelium powder was added to the resin at each temperature in the following amounts.

[0114] 7.Completion of biodegradable plastic A predetermined amount of mycelium powder was added to the syrupy resin and manually kneaded with a spatula for 3 minutes to create resin pieces containing mycelium powder, thereby obtaining the biodegradable plastic of this embodiment.

[0115] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A Carbon source glucose: PCL 300.0 mg + strain A 9.8 mg (mycelium internal concentration 3.2%) Carbon source trehalose: PCL 314.9 mg + strain A 10.1 mg (same 3.1%) Carbon source sucrose: PCL 322.5 mg + strain A 10.3 mg (same 3.1%) ·Strain C Carbon source glucose: PCL 326.5 mg + strain A 11.1 mg (same 3.3%) Carbon source trehalose: PCL 316.9 mg + strain A 9.4 mg (same 2.9%) Carbon source sucrose: PCL 322.0 mg + strain A 9.5 mg (same 2.9%)

[0116] 8. Calculation of the percentage of viable sections Using scissors disinfected with ethanol, the resin pieces containing the mycelium powder were cut into appropriate sizes (approximately 5 x 5 mm square) on the day of preparation, immediately placed on PDA medium, and left in a dark place at 25°C. After 1 to 2 weeks, the percentage of the pieces in which mycelium contained in the film had grown was calculated. The results are shown in Figure 9.

[0117] As shown in Fig. 9, when glucose was used as the carbon source, the growth rate of strain A was 100% at 70°C and 90°C, 80% at 110°C, and 30% at 130°C. When trehalose was used as the carbon source, the growth rate of strain A was 70% at 70°C, 50% at 90°C, and 28.6% at 110°C. When sucrose was used as the carbon source, the growth rate of strain A was 100% at 70°C and 90°C, and 40% at 110°C.

[0118] For strain C, when glucose was used as the carbon source, 77.8% growth was observed at 70°C and 9.1% growth was observed at 85°C. When trehalose was used as the carbon source, 40% growth was observed at 70°C. Furthermore, when sucrose was used as the carbon source, 100% growth was observed at 70°C.

[0119] Thus, in the method for producing biodegradable plastics according to the present embodiment, it was found that the heat resistance of fungal mycelium can be improved by adding glucose, trehalose, and / or trehalose to the liquid medium in which the mycelium is cultured. In particular, it was found that the heat resistance of fungal mycelium can be more suitably improved by adding glucose and / or sucrose.

[0120] [Test 10] In this embodiment, a test was conducted on the decomposition promoting effect of a biodegradable plastic produced by kneading a heat-melted resin with a powdered mycelium on an artificial seawater agar medium. First, fungal mycelium to be contained in the biodegradable plastic was prepared as follows. 1. Preculture Stock strains that had been frozen (-80°C) were inoculated into PDA medium (Potato Dextrose Agar) and cultured in the dark at 25°C for approximately 1 to 2 weeks. The following two types of stock strains were used: Strain A: Aspergillus flavus NBRC6343 Strain C: Glomerella cingulata NBRC107004

[0121] 2. Inoculation into liquid medium and preparation of mycelium mat The formed colonies were cut into pieces of approximately 5 mm square using a spatula, and the pieces were inoculated into Czapek liquid medium (0.3% NaNO3, 0.1% K2HPO4, 0.05% MgSO4·7H2O, 0.05% KCl, 0.001% FeSO4·7H2O) containing 3% (w / v) glucose and cultured statically in the dark at 25°C. The static culture periods for each strain were as follows: Strain A: A mixture of strains cultured for 36 and 192 days was used. Strain C: 101 days

[0122] 3. Mycelium Mat Collection After a period of static cultivation, the mycelial mat that formed on the surface of the liquid medium was harvested.

[0123] 4. Drying the Mycelium Mat The mycelium mats were allowed to dry for a set period of time. The drying periods for each strain were as follows: Strain A: 322 days (cultured for 36 days) at room temperature 166 days at room temperature (cultured for 192 days) Strain C: 17 days at room temperature, 36 days at 4°C, total 53 days

[0124] 5. Powderization of Mycelial Mat The dried mycelium mat and two zirconia balls (approximately 3.0 mm in diameter) were placed in a 2 ml screw-cap tube and shaken at 2500 rpm for 120 seconds using a mini bead beater BSP-3110BX to powderize the dried mycelium mat and obtain a powdered form of fungal mycelium (mycelium powder).

[0125] Next, a biodegradable plastic was prepared as follows. 6. Thermal melting of resin A given amount of resin pellets was added to a microtube (size: 2 ml capacity), placed in a block heater set at 100°C, and heated for a certain period of time until the pellets lost their shape and became candy-like. The temperature was then lowered to 70°C and the molten resin was used for the subsequent tests. The following resin pellets were used: ·PCL (Polycaprolactone): PLACCEL H8C Lot.H8C-AJ-D01 (Daicel Corporation)

[0126] 7.Completion of biodegradable plastic A predetermined amount of mycelium powder was added to the syrupy resin and manually kneaded with a spatula for 3 minutes to create resin pieces containing mycelium powder, thereby obtaining the biodegradable plastic of this embodiment.

[0127] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A: PCL 300.0 mg + Strain A 9.8 mg (mycelium concentration 3.2%) · Strain C: PCL326.5mg + strain C11.1mg (3.3%)

[0128] Next, the decomposition of the biodegradable plastic was confirmed as follows. 8. Preparation of Artificial Seawater Agar Medium NaNO3 was added to 0.3% (w / v) and K2HPO4 was added to 0.1% (w / v) of Daigo Artificial Seawater SP for Marine Microalgae Cultivation, which had the same composition as Test 1, prepared at a ratio of 36g / L. Then, 1.5% (w / v) agar was added and the mixture was autoclaved. After that, an appropriate amount was dispensed into a plastic disposable dish and cooled and solidified at room temperature.

[0129] 9. Exposure of biodegradable plastics to an artificial seawater agar medium environment Using scissors disinfected with ethanol, biodegradable plastic resin pieces were cut to an appropriate size (approximately 5 mm square) and placed on the agar medium. The biodegradable plastics were then exposed to an artificial seawater agar medium environment at 25°C for 173 days.

[0130] 10. Calculation of weight loss rate of biodegradable plastics After exposure to the above artificial seawater agar medium environment, only those pieces that were visually confirmed to be resin pieces were collected and weighed, and the weight loss rate was calculated using the following formula. Weight reduction rate (%) = (weight of resin piece before placing agar medium - weight of resin piece at time of recovery) / weight of resin piece before placing agar medium x 100

[0131] 11. Calculation of growth section rate Using scissors disinfected with ethanol, the resin pieces containing mycelium powder were cut into appropriate sizes (approximately 5 x 5 mm square) on the day of preparation, immediately placed on artificial seawater agar medium, etc., and left in a dark place at 25°C. After 1 to 2 weeks, the percentage of the pieces in which mycelium growth was observed in the resin pieces was calculated. In this test, the growth of mycelium contained in the film was confirmed for all 16 pieces. The results are shown in Figure 10.

[0132] FIG. 10 shows the weight loss rate of the biodegradable plastic for each strain obtained as described above, as well as the encapsulation concentration of mycelium and the rate of growing pieces in each biodegradable plastic. As shown in FIG. 10, the weight loss rates of biodegradable plastics using strain A and strain C were 32.1% and 54.1%, respectively.

[0133] The encapsulation concentrations of strain A and strain C in biodegradable plastics were 3.2% and 3.3%, respectively, and the growth intercept rates were 100.0% (16 / 16) and 81.3% (13 / 16), respectively. As described above, it has been found that the biodegradable plastic and the method for producing a biodegradable plastic of this embodiment can promote the decomposition of a biodegradable plastic produced by kneading mycelium powder with heat-melted resin in an artificial seawater environment.

[0134] [Test 11] In this embodiment, a test was conducted on the decomposition promoting effect of a biodegradable plastic produced by kneading a heat-melted resin with a powdered mycelium on a natural seawater agar medium. First, fungal mycelium to be contained in the biodegradable plastic was prepared as follows. 1. Preculture Stock strains that had been frozen (-80°C) were inoculated into PDA medium (Potato Dextrose Agar) and cultured in the dark at 25°C for approximately 1 to 2 weeks. The following three types of stock strains were used: Strain A: Aspergillus flavus NBRC6343 Strain B: Fusarium oxysporum NBRC9971 Strain C: Glomerella cingulata NBRC107004

[0135] 2. Inoculation into liquid medium and preparation of mycelium mat The formed colonies were cut into pieces of about 5 mm square using a spatula, and the pieces were inoculated into Czapek liquid medium (0.3% NaNO3, 0.1% K2HPO4, 0.05% MgSO4·7H2O, 0.05% KCl, 0.001% FeSO4·7H2O) containing 3% (w / v) glucose, and cultured statically in the dark at 25°C. This produced a mycelium mat consisting of filamentous fungi on the surface of the liquid medium. The static culture periods for each strain were as follows: Strain A: A mixture of strains cultured for 36 and 192 days was used. Strain B: 101 days Strain C: 101 days

[0136] 3. Mycelium Mat Collection After a period of static cultivation, the mycelial mat that formed on the surface of the liquid medium was harvested.

[0137] 4. Drying the Mycelium Mat The mycelium mats were allowed to dry for a set period of time. The drying periods for each strain were as follows: Strain A: 322 days (cultured for 36 days) at room temperature 166 days at room temperature (cultured for 192 days) Strain B: 17 days at room temperature, 36 days at 4°C, total 53 days Strain C: 17 days at room temperature, 36 days at 4°C, total 53 days

[0138] 5. Powderization of Mycelial Mat The dried mycelium mat and two zirconia balls (approximately 3.0 mm in diameter) were placed in a 2 ml screw-cap tube and shaken at 2500 rpm for 120 seconds using a mini bead beater BSP-3110BX to powderize the dried mycelium mat and obtain a powdered form of fungal mycelium (mycelium powder).

[0139] Next, a biodegradable plastic was prepared as follows. 6. Thermal melting of resin A given amount of resin pellets was added to a microtube (size: 2 ml capacity), placed in a block heater set at 100°C, and heated for a certain period of time until the pellets lost their shape and became candy-like. The temperature was then lowered to 70°C and the molten resin was used for the subsequent tests. The following resin pellets were used: ·PCL (Polycaprolactone): PLACCEL H8C Lot.H8C-AJ-D01 (Daicel Corporation)

[0140] 7.Completion of biodegradable plastic A predetermined amount of mycelium powder was added to the syrupy resin and manually kneaded with a spatula for 3 minutes to create a film containing mycelium powder, thereby obtaining the biodegradable plastic of this embodiment.

[0141] The mixing ratio of mycelium powder and resin in biodegradable plastic is as follows: Strain A: PCL 300.0 mg + Strain A 9.8 mg (mycelium concentration 3.2%) ·Strain B: PCL315.5mg + Strain B10.1mg (3.1%) · Strain C: PCL326.5mg + strain C11.1mg (3.3%)

[0142] Next, the decomposition of the biodegradable plastic was confirmed as follows. 8.Collecting natural seawater The natural seawater used was seawater collected from the beach in front of Enoshima Aquarium on the morning of June 29, 2022. The pH of the collected seawater was 8.1. The number of microorganisms contained was not measured. Then, 1.5% (w / v) agar was added and autoclaved. After that, an appropriate amount was dispensed into a plastic disposable dish and cooled and solidified at room temperature.

[0143] 9. Exposure of biodegradable plastics to a natural seawater agar medium environment Using scissors disinfected with ethanol, biodegradable plastic resin pieces were cut to an appropriate size (approximately 5 mm square) and placed on the agar medium. The biodegradable plastics were then exposed to a natural seawater agar medium environment at 25°C for 173 days. In addition, the weight loss rate of the biodegradable plastic and the growth slice rate were calculated in the same manner as in Test 10. The results are shown in FIG.

[0144] FIG. 11 shows the weight loss rate of the biodegradable plastic for each strain obtained as described above, as well as the encapsulation concentration of mycelium and the rate of growing pieces in each biodegradable plastic. As shown in FIG. 11, the weight loss rates of biodegradable plastics using strain A, strain B, and strain C were 19.6%, 37.1%, and 16.6%, respectively.

[0145] In addition, the encapsulation concentrations of strains A, B, and C in biodegradable plastics were 3.2%, 3.1%, and 3.3%, respectively, and the growth intercept rates were 100.0% (16 / 16), 18.8% (3 / 16), and 81.3% (13 / 16), respectively. As described above, it has been found that the biodegradable plastic and the method for producing a biodegradable plastic of this embodiment can promote the decomposition of a biodegradable plastic produced by kneading mycelium powder with heat-melted resin in a natural seawater environment.

[0146] The present invention is not limited to the above-mentioned embodiments and examples, and various modifications are possible within the scope of the present invention. For example, the sugars are not limited to the above-mentioned types, and other types can be used as long as they can improve the resistance of biodegradable plastics. [Industrial Applicability]

[0147] INDUSTRIAL APPLICABILITY The present invention can be suitably used for providing biodegradable plastics that can be decomposed in a marine environment.

Claims

1. A biodegradable plastic comprising mycelium of a fungus capable of decomposing biodegradable plastics.

2. 2. The biodegradable plastic according to claim 1, wherein the mycelium of the fungus is in a powdered form.

3. The biodegradable plastic according to claim 1 or 2, characterized in that the biodegradable plastic is at least one synthetic polymer selected from the group consisting of aliphatic polyesters, aromatic polyesters, and derivatives thereof, and mixtures thereof.

4. 4. The biodegradable plastic according to claim 3, characterized in that the synthetic polymer is selected from the group consisting of polycaprolactone (PCL), polybutylene adipate terephthalate (PBAT), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polylactic acid (PLA), polyhydroxyalkanoate (PHA), polyglycolic acid (PGA), polyethylene terephthalate succinate (PETS), starch polyester, and polybutylene succinate terephthalate (PBST).

5. 3. The biodegradable plastic according to claim 1, wherein the fungus is a filamentous fungus.

6. 6. The biodegradable plastic according to claim 5, wherein the filamentous fungus is a fungus imperfecti or an ascomycete fungus.

7. 6. The biodegradable plastic according to claim 5, wherein the filamentous fungus is a fungus belonging to the genus Aspergillus, Fusarium, or Glomerella.

8. 3. The biodegradable plastic according to claim 2, characterized in that the fungal mycelium powder is contained in an amount of 0.001% to 10% by mass.

9. A method for producing a biodegradable plastic, comprising adding to a biodegradable plastic mycelium of a fungus capable of decomposing said biodegradable plastic.

10. 10. The method for producing biodegradable plastics according to claim 9, wherein the mycelium of the fungus is powdered and added to the biodegradable plastics.

11. inoculating a liquid medium with the filamentous fungus; a step of culturing the filamentous fungus for a predetermined period of time under static or agitated conditions to prepare a mycelium mat of the filamentous fungus; harvesting the mycelium mat; drying the mycelium mat for a predetermined period of time; and The dried mycelium mat is powdered. The method for producing a biodegradable plastic according to claim 10.

12. 12. The method for producing biodegradable plastics according to claim 11, characterized in that the resistance of the mycelium of the fungus is improved by adding glucose, trehalose, and / or sucrose to the liquid medium.

13. The method for producing biodegradable plastics according to claim 12, characterized in that the resistance is storage resistance or heat resistance.

14. The method for producing biodegradable plastics according to claim 11, characterized in that the filamentous fungus is selected from the group consisting of Fungi Imperfecti and Ascomycota.

15. The method for producing biodegradable plastics according to claim 11, characterized in that the filamentous fungus is selected from the genus Aspergillus, the genus Fusarium, or the genus Glomerella.

16. 11. The method for producing biodegradable plastics according to claim 10, characterized in that the powder of said mycelium is dispersed in a biodegradable plastic dissolved in an organic solvent and molded by a solution casting method.

17. 11. The method for producing biodegradable plastics according to claim 10, wherein the powder of mycelium is dispersed in a heat-melted biodegradable plastic and molded by a melt-kneading method.

18. 18. The method for producing biodegradable plastics according to claim 16 or 17, characterized in that in the molding, the powder of mycelium is molded into a film, thin film or lump.

Citation Information

Patent Citations

  • Error pulse generation circuit

    JP1988010843A

  • Biodegradable film and its production

    JP1991179036A

  • Biodegradable resin containing microorganism

    JP2002356623A

  • Masterbatch compositions containing high concentrations of biological entities

    JP6985154B2

Cited By

  • Method for decomposing plastic

    JP2022139662A

  • Method for decomposing plastic

    JP7683250B2

  • Mushroom mycelium powder manufacturing method using PLA powder and mushroom mycelium powder manufactured thereby

    KR102873089B1