Non-aqueous electrolyte secondary battery

The battery design addresses cycle characteristic deterioration by optimizing separator air permeability ratios and confining pressure to ensure even electrolyte distribution, enhancing long-term durability.

JP2024166906AActive Publication Date: 2024-11-29PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023083330
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

Non-aqueous electrolyte secondary batteries with positive and negative electrode tabs on the sealing plate side experience deterioration in cycle characteristics due to long-term use, leading to reduced long-term durability.

Method used

The battery design includes a separator with specific air permeability ratios and a confining pressure to ensure even electrolyte distribution, with the positive and negative electrode tabs facing the sealing plate, and a separator structure that satisfies the relationship 1.05≦T2/T1≦1.4, where T1 and T2 are air permeabilities of different regions, and applies a confining pressure of 0.05 MPa or more.

Benefits of technology

This design suppresses electrolyte shortage at the sealing plate side, maintaining excellent cycle characteristics and long-term durability by facilitating even electrolyte distribution within the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166906000001_ABST
    Figure 2024166906000001_ABST
Patent Text Reader

Abstract

To provide a non-aqueous electrolyte secondary battery having an excellent long period durability by suppressing deterioration of a cycle characteristic in accordance with a use of a long period.SOLUTION: A non-aqueous electrolyte secondary battery comprises: an electrode body having a positive electrode, a negative electrode, and a separator; an electrolyte; and a battery case. The battery case includes: an outer casing body; and a sealing plate. The positive electrode includes a positive electrode tub to an end part of the electrode body. The negative electrode includes a negative electrode tub to the end part of the electrode body. The electrode body is housed in the battery case so that the end part having the positive electrode tub and the negative electrode tub is opposite to the sealing plate. In a direction directed to a bottom part from the sealing plate of the battery case, when the length of the separator is L, both of an air permeability T1 in a first region from the end part of the sealing plate side of a separator toward the bottom part side up to a position of a length of 0.3L and an air permeability T2 in a second region from the end part of the bottom part side of the separator toward the sealing plate side up to the position of the length of 0.3L satisfy a relation of the following formula (I): 1.05≤T2 / T1≤1.4 (I).SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-aqueous electrolyte secondary battery. [Background technology]

[0002] Batteries such as non-aqueous electrolyte secondary batteries generally include an electrode assembly having a positive electrode and a negative electrode, and a battery case that houses the electrode assembly. The battery case includes an exterior body that houses the electrode assembly, and a sealing plate that seals the opening of the exterior body. As such a battery, a prismatic battery that uses a prismatic (box-shaped) exterior body is known. Patent Document 1 discloses a prismatic battery in which a positive electrode tab portion of a positive electrode and a negative electrode tab portion of a negative electrode are disposed on the sealing plate side of the battery case. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-189247 A Summary of the Invention [Problem to be solved by the invention]

[0004] It has been found that the cycle characteristics of a battery in which the positive electrode tab and the negative electrode tab are located on the sealing plate side are degraded when the battery is used for a long period of time.

[0005] An object of the present disclosure is to provide a non-aqueous electrolyte secondary battery that suppresses deterioration of cycle characteristics due to long-term use and has excellent long-term durability. [Means for solving the problem]

[0006] [1] An electrode assembly having a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; An electrolyte; a battery case that accommodates the electrode assembly and the electrolyte; the battery case includes an exterior body having an opening and a sealing plate that seals the opening, The positive electrode has a positive electrode tab at an end of the electrode body, from which a part of the positive electrode protrudes, The negative electrode has a negative electrode tab at an end of the electrode body, from which a part of the negative electrode protrudes, the electrode body is accommodated in the battery case such that the end portion having the positive electrode tab and the negative electrode tab faces the sealing plate, a first region of the separator extending from the sealing plate side to a position having a length of 0.3L toward the bottom side, and an air permeability T2 of a second region of the separator extending from the bottom side to a position having a length of 0.3L toward the sealing plate side, satisfying the relationship of formula (I). 1.05≦T2 / T1≦1.4 (I) [2] The nonaqueous electrolyte secondary battery according to [1], wherein the battery case is rectangular. [3] The nonaqueous electrolyte secondary battery according to [1] or [2], wherein the electrode body is a wound type electrode body. [4] The nonaqueous electrolyte secondary battery according to any one of [1] to [3], wherein the separator has a substrate and a functional layer formed on at least one surface of the substrate. [5] The nonaqueous electrolyte secondary battery according to [4], wherein the functional layer includes an adhesive layer. [6] The nonaqueous electrolyte secondary battery according to any one of [1] to [5], wherein a confining pressure of 0.05 MPa or more is applied to the nonaqueous electrolyte secondary battery in a stacking direction of the positive electrode, the negative electrode, and the separator. [7] The nonaqueous electrolyte secondary battery according to any one of [1] to [6], wherein the first region has a thickness greater than a thickness of the second region. [8] The nonaqueous electrolyte secondary battery according to [7], wherein in the positive electrode and the negative electrode, a thickness of a region facing the first region is smaller than a thickness of a region facing the second region. Effect of the Invention

[0007] The nonaqueous electrolyte secondary battery of the present disclosure is inhibited from deteriorating in cycle characteristics due to long-term use, and can have excellent long-term durability. [Brief description of the drawings]

[0008] [Figure 1] 1 is a perspective view illustrating a nonaqueous electrolyte secondary battery according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II of FIG. [Diagram 3] FIG. 2 is a front view showing a schematic view of a separator that constitutes an electrode assembly. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] (Nonaqueous electrolyte secondary battery) Fig. 1 is a perspective view showing a non-aqueous electrolyte secondary battery according to an embodiment of the present invention, Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1, Fig. 3 is a front view showing a separator constituting an electrode assembly.

[0010] The nonaqueous electrolyte secondary battery (hereinafter also referred to as "the battery") 1 of this embodiment is, for example, a lithium ion secondary battery that performs charging and discharging by absorbing and releasing lithium ions. As shown in Fig. 1 and Fig. 2, the battery 1 includes an electrode assembly 200, an electrolyte, and a battery case 100 that contains the electrode assembly 200 and the electrolyte.

[0011] The battery case 100 has an exterior body 110 having an opening, and a sealing plate 120 that seals the opening of the exterior body 110. The present battery 1 is preferably a prismatic battery in which the battery case is prismatic (box-shaped). The exterior body 110 can have a space for accommodating the electrode assembly and the electrolyte, and can be prismatic (box-shaped). The exterior body 110 has a bottom 115 that faces the sealing plate 120. The sealing plate 120 can be attached to the exterior body 110 so as to close the opening of the exterior body 110 after the electrode assembly 200 is accommodated in the exterior body 110. The sealing plate 120 can be attached to the exterior body 110 by joining it to the periphery of the opening of the exterior body 110 by welding or the like. The sealing plate 120 may have a liquid injection hole 121 for injecting the electrolyte, a sealing member 122 for sealing the liquid injection hole 121, and a gas release valve 123 that breaks when the pressure inside the battery case 100 reaches or exceeds a predetermined value.

[0012] The electrode body 200 has a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode. In FIG. 2, the positive electrode, the negative electrode, and the separator 250 are stacked in a direction perpendicular to the paper surface. The electrode body 200 may be a wound type electrode body in which a laminate in which a positive electrode, a negative electrode, and a separator are stacked is wound, or may be a laminated type electrode body in which a positive electrode, a negative electrode, and a separator are stacked. The wound type electrode body may be flattened by pressing the laminate after rolling it. The laminated type electrode body may have a quadrangular shape in a plan view, preferably a square or rectangular shape, and more preferably a rectangular shape.

[0013] The positive electrode has a positive electrode tab 210A from which a part of the positive electrode protrudes at an end 201 of the electrode body 200 (FIG. 2). The positive electrode tab 210A can be a connection part that electrically connects the positive electrode to a positive electrode terminal 400, which is an external terminal of the battery 1. The positive electrode can have a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. In this case, the positive electrode tab 210A can be formed by the positive electrode current collector in an area where the positive electrode active material layer is not formed, and can be provided so as to protrude outward from an area of ​​the positive electrode current collector where the positive electrode active material layer is formed.

[0014] The negative electrode has a negative electrode tab 210B from which a part of the negative electrode protrudes at an end 201 of the electrode body 200 (FIG. 2). The negative electrode tab 210B can be a connection part that electrically connects the negative electrode to a negative electrode terminal 500, which is an external terminal of the battery 1. The negative electrode can have a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. In this case, the negative electrode tab 210B can be formed by the negative electrode current collector in a region where the negative electrode active material layer is not formed, and can be provided so as to protrude outward from a region of the negative electrode current collector where the negative electrode active material layer is formed.

[0015] The end 201 of the electrode body 200 on which the positive electrode tab 210A and the negative electrode tab 210B are provided is usually the same end (FIG. 2). When the electrode body 200 is a wound electrode body, it is preferable that the positive electrode tab 210A and the negative electrode tab 210B are provided at one of the ends of the electrode body 200 in a direction parallel to the winding axis. When the electrode body 200 is a laminated electrode body and the laminated electrode body is quadrangular in plan view, it is preferable that the positive electrode tab 210A and the negative electrode tab 210B are provided at the same side of the rectangle. When the laminated electrode body is rectangular in plan view, the positive electrode tab 210A and the negative electrode tab 210B may be provided at one long side of the rectangle.

[0016] As shown in FIG. 2, the electrode body 200 is accommodated in the battery case 100 so that the end 201 having the positive electrode tab 210A and the negative electrode tab 210B faces the sealing plate 120. At this time, the end 201 is disposed closer to the sealing plate 120 than the end 202 of the electrode body 200, which is located at a position facing the end 201. When the electrode body 200 is accommodated in the battery case 100, the direction in which the positive electrode tab 210A and the negative electrode tab 210B protrude (the up-down direction in FIG. 2) may be a direction perpendicular to the surface of the sealing plate 120. For example, when the electrode body 200 is a wound type electrode body, the positive electrode tab 210A and the negative electrode tab 210B are provided at one of the ends in a direction parallel to the winding axis of the wound type electrode body, and the electrode body 200 may be accommodated in the battery case 100 so that this end faces the sealing plate 120 and the winding axis of the wound type electrode body is perpendicular to the sealing plate 120.

[0017] The separator 250 of the electrode body may have a substrate and a functional layer on at least one side of the substrate. The functional layer may be formed on both sides of the substrate. The functional layer may be an adhesive layer, a heat-resistant layer, etc. The functional layer may include one or both of an adhesive layer and a heat-resistant layer. The separator 250 preferably includes a substrate and an adhesive layer as a functional layer.

[0018] 3, the separator 250 has a length of L in the direction from the sealing plate 120 toward the bottom 115 opposite the sealing plate 120 in the battery case 100. The separator 250 has a first region 251 that extends from the end on the sealing plate 120 side toward the bottom 115 side to a position 0.3L long, and has a second region 252 that extends from the end on the bottom 115 side toward the sealing plate 120 side to a position 0.3L long. The air permeability T1 of the first region 251 and the air permeability T2 of the second region 252 satisfy the relationship of the following formula (I). 1.05≦T2 / T1≦1.4 (I)

[0019] 3 shows the shape of the separator 250 included in the electrode assembly 200 housed in the battery case 100 when viewed from the front of the battery case 100 (as viewed in FIG. 2). Therefore, the length L of the separator 250 is the length of the separator 250 when the electrode assembly 200 housed in the battery case 100 is viewed from the direction in which the positive electrode, negative electrode, and separator 250 are stacked (the length in the vertical direction in FIG. 2).

[0020] The air permeability T1 and the air permeability T2 represent the time required for a certain amount of gas to permeate, and the larger the value, the more difficult the gas is to permeate. The air permeability T1 and the air permeability T2 in the first region 251 and the second region 252 are measured for the flat portion of the separator 250 between the positive electrode and the negative electrode, which is disposed on the outermost side in the stacking direction of the positive electrode, the negative electrode, and the separator of the electrode assembly 200, and can be measured by the method described in the examples below.

[0021] The present battery 1 is usually used by being installed so that the sealing plate 120 side is the upper surface and the bottom 115 side is the lower surface, as shown in FIG. 1. Therefore, the liquid level of the electrolyte when the present battery 1 is fully charged is usually at a position lower than the end of the electrode body 200 on the sealing plate 120 side. In this state, if a secondary battery in which the separator 250 does not satisfy the relationship of the above formula (I) is used for a long period of time, the electrolyte tends to accumulate on the bottom 115 side of the battery case 100 and the electrolyte tends to be insufficient on the sealing plate 120 side. Since the cycle characteristics are reduced on the sealing plate 120 side where the electrolyte is insufficient, it is considered that the long-term durability of the secondary battery is reduced. In contrast, the separator 250 of the present battery 1 satisfies the relationship of the above formula (I). Therefore, the electrolyte pushed out from the negative electrode due to the expansion and contraction of the negative electrode accompanying the charge and discharge of the battery is relatively difficult to pass through the separator 250 in the second region 252. On the other hand, since the air permeability T1 of the first region 251 is smaller than the air permeability T2 of the second region 252, the electrolyte can easily move from the second region 252 side to the first region 251 side within the separator 250. This makes it easier for the electrolyte to be supplied from the bottom 115 side of the battery case 100 to the sealing plate 120 side, thereby preventing a shortage of electrolyte on the sealing plate 120 side. As a result, even when the battery 1 is used for a long period of time, deterioration of the cycle characteristics can be prevented, and excellent long-term durability can be obtained.

[0022] The ratio (T2 / T1) of the air permeability T1 to the air permeability T2 may be 1.1 or more and 1.3 or less, or 1.1 or more and 1.2 or less. If the ratio (T2 / T1) is small, the electrolyte shortage occurs on the sealing plate 120 side, and the cycle characteristics tend to deteriorate. If the ratio (T2 / T1) is large, the electrolyte shortage occurs on the bottom 115 side, and the cycle characteristics tend to deteriorate.

[0023] The air permeability T1 of the first region 251 is not particularly limited as long as it is smaller than the air permeability T2 of the second region 252, but may be 50 seconds or more and 400 seconds or less, 80 seconds or more and 300 seconds or less, or 120 seconds or more and 250 seconds or less. The air permeability T2 of the second region 252 is not particularly limited as long as it is larger than the air permeability T1 of the first region 251, but may be 80 seconds or more and 500 seconds or less, 100 seconds or more and 400 seconds or less, or 150 seconds or more and 350 seconds or less.

[0024] The air permeability of the intermediate region between the first region 251 and the second region 252 of the separator 250 is preferably greater than T1 and less than T2.

[0025] The air permeabilities T1 and T2 in the first region 251 and the second region 252 of the separator 250 can be adjusted by the degree of porosity, density, and thickness of the substrate and functional layer constituting the separator 250, the presence or absence of a functional layer, the type of the functional layer, and combinations thereof. Examples of methods for forming the first region 251 and the second region 252 with different air permeabilities include the following methods. [a] A method in which a substrate having partially compressed and non-compressed portions is used as the separator 250 to vary the thickness and density. [b] Heating the substrate to vary the degree of porosity of the substrate. [c] A method for adjusting at least one of the presence or absence, the type, and the amount of application of a functional layer formed on the surface of the substrate of separator 250. [d] A combination of two or more of the above [a] to [c].

[0026] Alternatively, the first region 251 and the second region 252 having different air permeabilities may be formed in the separator 250 during the manufacture of the electrode body 200 as follows. The electrode body 200 may be manufactured by pressing a laminate in which a positive electrode, a negative electrode, and a separator 250 are laminated. A positive electrode and a negative electrode having regions with different thicknesses are prepared so that the thickness of the region facing the first region 251 of the separator 250 is small and the thickness of the region facing the second region 252 is large when the electrode body 200 is made. When a laminate in which such positive electrodes and negative electrodes with different thicknesses and a separator are laminated is pressed, the separator 250 has regions with different thicknesses formed to correspond to the thicknesses of the positive electrode and the negative electrode, and the thickness of the first region 251 can be made larger than the thickness of the second region 252. As a result, the thickness and density of the first region 251 and the second region 252 of the separator 250 can be made different, and the first region 251 and the second region 252 having different air permeabilities can be formed.

[0027] When the electrode body 200 is a wound type electrode body, the electrolyte will enter the electrode body 200 from both ends in the direction parallel to the winding axis of the wound type electrode body. On the other hand, in a laminated type electrode body, the electrolyte will enter the electrode body 200 from the position of each side in a plan view. Therefore, in a wound type electrode body, the electrolyte is less likely to enter the electrode body 200 compared to a laminated type electrode body, and therefore a decrease in cycle characteristics due to a shortage of electrolyte is likely to occur. However, by making the separator 250 satisfy the relationship of the above formula (I) as in the present battery 1, even when the battery is provided with a wound type electrode body, the decrease in cycle characteristics due to a shortage of electrolyte on the sealing plate 120 side can be suppressed, and excellent long-term durability can be obtained.

[0028] The separator 250 is disposed between the positive electrode and the negative electrode. When the separator 250 includes an adhesive layer, the adhesive layer allows the separator 250 to be disposed close to the positive electrode and the negative electrode, and the distance between the negative electrode and the positive electrode (the distance between the plates) can be reduced. In a battery having an electrode assembly with such a small distance between the plates, the electrolyte can be easily moved from the second region 252 side of the separator 250 to the first region 251 side, compared to a battery having an electrode assembly with a relatively large distance between the plates, and therefore the long-term durability can be further improved.

[0029] The battery 1 may be applied with a confining pressure of 0.05 MPa or more in the stacking direction of the positive electrode, the negative electrode, and the separator 250. The confining pressure may be 0.1 MPa or more, 0.5 MPa or more, 0.5 MPa or more and 5 MPa or less, 0.5 MPa or more and 4 MPa or less, or 0.5 MPa or more and 3 MPa or less. The confining pressure can be measured by a tactile sensor. In the battery 1 to which the confining pressure is applied, the inter-electrode distance can be reduced, so that the electrolyte can be easily moved from the second region 252 side of the separator 250 to the first region 251 side. Therefore, the battery 1 to which the above confining pressure is applied can further improve long-term durability.

[0030] The length L of the separator 250 is, for example, 50 mm or more, may be 80 mm or more, or may be 100 mm or more, and is usually 120 mm or less. If the length L of the separator 250 is large, a decrease in cycle characteristics due to a shortage of electrolyte on the sealing plate 120 side is likely to occur. When the separator 250 satisfies the relationship of formula (I) as in the present battery 1, the present battery 1 has excellent long-term durability even when the length L is large.

[0031] As described above, the positive electrode plate can have a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode current collector is, for example, a metal foil made of an aluminum material such as aluminum or an aluminum alloy. The positive electrode active material layer contains a positive electrode active material. Examples of the positive electrode active material include lithium transition metal oxides such as layered or spinel-based oxides (e.g., LiNiCoMnO2, LiNiO2, LiCoO2, LiFeO2, LiMn2O4, LiNi 0.5 Mn 1.5 O4, LiCrMnO4, LiFePO4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2). The lithium transition metal oxide is preferably a lithium nickel cobalt manganese composite oxide (NCM).

[0032] The positive electrode active material layer may contain one or both of a binder and a conductive assistant in addition to the positive electrode active material. Examples of the binder include styrene butadiene rubber (SBR), polyvinylidene fluoride (PVdF), and polytetrafluoroethylene (PTFE). Examples of the conductive assistant include carbon materials such as fibrous carbon, carbon black (acetylene black, ketjen black, etc.), coke, and activated carbon. Examples of the fibrous carbon include carbon nanotubes (hereinafter also referred to as "CNTs"). The CNTs may be single-walled carbon nanotubes (SWCNTs) or multi-walled carbon nanotubes such as double-walled carbon tubes (DWCNTs).

[0033] As described above, the negative electrode current collector and the negative electrode active material layer formed on the negative electrode current collector can be included. The negative electrode current collector is, for example, a metal foil made of a copper material such as copper and a copper alloy. The negative electrode active material layer includes a negative electrode active material. Examples of the negative electrode active material include carbon-based active materials containing carbon (C) atoms such as graphite; and metal-based active materials containing metal elements such as metal simple substances or metal oxides containing elements selected from the group consisting of silicon (Si), tin (Sn), antimony (Sb), bismuth (Bi), titanium (Ti), and germanium (Ge). The negative electrode active material layer may include a Si-based active material containing silicon elements as a metal-based active material. Examples of the Si-based active material include silicon simple substance, SiC (a composite material of silicon and carbon, for example, a composite material in which silicon nanoparticles are dispersed in porous carbon particles), SiOx, LixSiyOz, and the like.

[0034] The negative electrode active material layer may contain one or both of a binder and a conductive assistant in addition to the negative electrode active material. Examples of the binder include cellulose-based binders such as carboxymethyl cellulose (CMC), methyl cellulose (MC), and hydroxypropyl cellulose; styrene butadiene rubber (SBR), polyacrylic acid (PAA), acrylonitrile butadiene rubber (NBR), polyvinylidene fluoride (PVdF), and polytetrafluoroethylene (PTFE). Examples of the conductive assistant include those mentioned above.

[0035] The substrate of the separator may be a film made of a resin such as polyethylene, polypropylene, polyester, cellulose, or polyamide, or a porous sheet such as a nonwoven fabric. The substrate may have a single-layer structure or a multilayer structure. The adhesive layer of the separator may be formed by an adhesive. A separator having a substrate and an adhesive layer may be formed, for example, by applying an adhesive to the substrate, or by applying an adhesive to a release sheet or the like to form an adhesive layer, laminating the adhesive layer on the substrate, and then peeling off the release sheet. Examples of the adhesive include hot melt adhesives, ultraviolet curing adhesives, and thermosetting adhesives. Examples of the base resin of the adhesive include one or more resins selected from the group consisting of acrylic resins, urethane resins, ethylene vinyl acetate resins, epoxy resins, and fluororesins. The heat-resistant layer of the separator includes a filler and may further include a binder. Examples of the filler include ceramic particles that are one or more types selected from the group consisting of alumina, boehmite, aluminum hydroxide, silica, magnesia, titania, silicon nitride, and titanium nitride. Examples of the binder include one or more types selected from the group consisting of acrylic binders such as acrylic resins, fluoropolymer binders such as polyvinylidene fluoride, and styrene-butadiene rubber (SBR).

[0036] The electrolyte is usually a non-aqueous electrolyte, preferably a non-aqueous solvent such as an organic solvent containing a supporting salt. Examples of the supporting salt include LiPF6, LiBF4, LiClO4, LiFSO3, and LiBOB (lithium bis(oxalato)borate). The electrolyte may contain one or more of these supporting salts. Examples of the non-aqueous solvent include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), and diethyl carbonate (DEC). The electrolyte may contain one or more of these non-aqueous solvents. The electrolyte may contain additives other than the above-mentioned supporting salts and non-aqueous solvents.

[0037] The exterior body 110 and the sealing plate 120 constituting the battery case 100 are preferably made of metal and can be formed using aluminum, an aluminum alloy, iron, an iron alloy, or the like, and can be formed using, for example, an aluminum laminate film. EXAMPLES

[0038] The present disclosure will be described more specifically below with reference to examples and comparative examples. Example 1 (Preparation of positive electrode) Lithium nickel cobalt manganese composite oxide (NCM) as a positive electrode active material, acetylene black (AB) as a conductive assistant, and polyvinylidene fluoride (PVdF) as a binder were used in a ratio of NCM:AB:PVdF=97:2:1 (mass ratio), which was mixed with N-methylpyrrolidone (NMP) to obtain a positive electrode mixture slurry. The positive electrode mixture slurry was applied to an aluminum foil having a thickness of 15 μm as a positive electrode current collector so that an exposed portion (1) was formed in which the end (side edge) in the width direction of the positive electrode current collector was exposed, and then dried. Next, the positive electrode mixture slurry applied to the positive electrode current collector was compressed using a pair of rollers to form a positive electrode active material layer on the positive electrode current collector, thereby obtaining a positive electrode raw material. The positive electrode raw material has a region where a positive electrode active material layer is formed on the positive electrode current collector, and an exposed portion (1) in which the positive electrode active material layer is not formed and the positive electrode current collector is exposed. The amount of the positive electrode mixture slurry applied to the region on the exposed portion (1) side of the positive electrode active material layer was made smaller than the amount of the positive electrode mixture slurry applied to other regions other than the exposed portion (1), and the gap between the pair of rollers was adjusted to compress the layer, thereby making the thickness of the positive electrode active material on the exposed portion (1) side relatively small. The positive electrode raw sheet was then cut so that positive electrode tabs were repeatedly formed at regular intervals to obtain a positive electrode. The positive electrode tabs were formed from the region of the exposed portion (1).

[0039] (Preparation of negative electrode) Graphite as the negative electrode active material, carboxymethylcellulose (CMC) as the binder, and styrene butadiene rubber (SBR) were used in a ratio of graphite:CMC:SBR=100:1:1 (mass ratio), which was mixed with water and kneaded using a stirring granulator to obtain a negative electrode mixture slurry. The negative electrode mixture slurry was applied to a copper foil having a thickness of 10 μm as a negative electrode current collector so that an exposed portion (2) was formed in which the end (side edge) in the width direction of the negative electrode current collector was exposed, and then dried. Next, a pair of rollers was used to compress the negative electrode mixture slurry applied to the negative electrode current collector, thereby forming a negative electrode active material layer on the negative electrode current collector to obtain a negative electrode raw material. The negative electrode raw material has a region where the negative electrode active material layer is formed on the negative electrode current collector, and an exposed portion (2) in which the negative electrode active material layer is not formed and the negative electrode current collector is exposed. The amount of the negative electrode mixture slurry applied to the region on the exposed portion (2) side of the negative electrode active material layer was made smaller than the amount of the negative electrode mixture slurry applied to other regions other than the exposed portion (2), and the gap between the pair of rollers was adjusted to compress the layer, thereby making the thickness of the negative electrode active material on the exposed portion (2) side relatively small. The negative electrode raw sheet was then cut so that negative electrode tabs were repeatedly formed at regular intervals to obtain a negative electrode. The negative electrode tabs were formed from the region of the exposed portion (2).

[0040] (Preparation of electrode body) A separator (1) having a substrate but no adhesive layer was prepared. A positive electrode and a negative electrode were laminated with the separator (1) interposed therebetween to obtain a laminate. At this time, the positive electrode and the negative electrode were laminated so that the positive electrode tab and the negative electrode tab did not overlap each other in the lamination direction of the laminate. The laminate was wound and pressed to obtain a flat wound electrode body. By pressing the wound laminate, the separator (1) was compressed according to the thicknesses of the positive electrode (positive electrode active material layer) and the negative electrode (negative electrode active material layer), and regions of different thicknesses were formed in the separator (1).

[0041] (Preparation of non-aqueous electrolyte secondary battery) LiPF6 was used as the supporting salt, and a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) (EC:EMC:DMC=30:40:40 (volume ratio)) was used as the non-aqueous solvent. LiPF6 and the mixed solvent were mixed so that the concentration of LiPF6 was 1 mol / L to prepare an electrolyte. A battery was obtained by housing the electrode body and electrolyte in a square battery case having an exterior body and a sealing plate, so that the ends having the positive and negative electrode tabs of the electrode body faced the sealing plate side, as shown in FIG. 2. In the electrode body housed in the battery case, the separator was thicker on the sealing plate side and thinner on the bottom side, and the positive and negative electrodes were thinner on the sealing plate side and thicker on the bottom side. A constraining plate was placed on each of the two surfaces of the battery that were parallel to the winding axis of the electrode body (i.e., the two surfaces that were perpendicular to the stacking direction of the positive electrode, negative electrode, and separator of the electrode body), and a constraining pressure of 0.05 MPa or more was applied to the battery by sandwiching it between the two constraining plates. The constraining pressure was measured by a tactile sensor.

[0042] [Examples 2 to 4, Comparative Examples 1 to 3] An electrode body was produced by adjusting the coating amounts of the positive electrode mixture slurry and the negative electrode mixture slurry, the compressed amount of the positive electrode mixture slurry coated on the positive electrode current collector, and the compressed amount of the negative electrode mixture slurry coated on the negative electrode current collector so that the air permeabilities of the first region and the second region of the separator were adjusted to satisfy the relationship in Table 1. A battery to which a confining pressure was applied was obtained in the same manner as in Example 1, except that this electrode body was used.

[0043] Example 5 A separator (2) having an adhesive layer on both sides of a substrate was prepared. An electrode assembly was obtained in the same manner as in Example 1, except that the separator (2) was used, and a battery to which a confining pressure was applied was obtained.

[0044] [Air permeability measurement] Among the separators in the electrode body, the separator between the positive electrode and the negative electrode, which is arranged on the outermost side (outer circumference side) of the wound electrode body, was defined as the first region from the end of the sealing plate side toward the bottom side of the battery case to a position with a length of 0.3L, and the second region was defined as the position with a length of 0.3L from the end of the bottom side toward the sealing plate side. In each of the first region and the second region, three or more positions were set at different positions so that the air permeability in each region of the flat part of the wound electrode body was measured evenly. The set positions were fixed so as to be located directly under the measurement head of the Oken type testing machine, and the air permeability was measured and the arithmetic average was calculated. This was defined as the air permeability T1 of the first region and the air permeability T2 of the second region, and the ratio (T2 / T1) was calculated. The results are shown in Table 1.

[0045] [Cycle test] In an environment of 25°C, the battery was repeatedly charged to 4.1Vcccv (constant current / constant voltage) at a current value of 0.33C (cutoff current: 0.05C) and discharged to a potential of 3V at a current value of 0.33C, with this being one charge / discharge cycle. The capacity retention rate [%] was calculated as the retention rate of the discharge capacity W200 at the 200th cycle relative to the discharge capacity W1 at the 1st cycle according to the following formula. The results are shown in Table 1. Capacity maintenance rate [%]=(W200 / W1)×100

[0046] [Table 1] [Explanation of symbols]

[0047] 1 nonaqueous electrolyte secondary battery, 100 battery case, 110 exterior body, 115 bottom, 120 sealing plate, 121 liquid inlet, 122 sealing member, 123 gas exhaust valve, 200 electrode body, 201, 202 end, 210A positive electrode tab, 250 separator, 251 first region, 252 second region, 400 positive electrode terminal, 500 negative electrode terminal.

Claims

1. An electrode assembly having a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; An electrolyte; a battery case that accommodates the electrode assembly and the electrolyte; the battery case includes an exterior body having an opening and a sealing plate that seals the opening, The positive electrode has a positive electrode tab at an end of the electrode body, from which a part of the positive electrode protrudes, The negative electrode has a negative electrode tab at an end of the electrode body, from which a part of the negative electrode protrudes, the electrode body is accommodated in the battery case such that the end portion having the positive electrode tab and the negative electrode tab faces the sealing plate, a first region of the separator extending from the sealing plate side to a position having a length of 0.3 L toward the bottom side, and an air permeability T2 of a second region of the separator extending from the bottom side to a position having a length of 0.3 L toward the sealing plate side, satisfying the relationship of formula (I). 1.05≦T2 / T1≦1.4 (I)

2. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the battery case is rectangular.

3. 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrode assembly is a wound electrode assembly.

4. 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the separator comprises a substrate and a functional layer formed on at least one surface of the substrate.

5. The nonaqueous electrolyte secondary battery according to claim 4 , wherein the functional layer includes an adhesive layer.

6. 3 . The nonaqueous electrolyte secondary battery according to claim 1 , wherein a confining pressure of 0.05 MPa or more is applied to the nonaqueous electrolyte secondary battery in a stacking direction of the positive electrode, the negative electrode, and the separator.

7. The nonaqueous electrolyte secondary battery according to claim 1 , wherein a thickness of the first region is greater than a thickness of the second region.

8. 8 . The nonaqueous electrolyte secondary battery according to claim 7 , wherein a thickness of a region of the positive electrode and the negative electrode facing the first region is smaller than a thickness of a region of the positive electrode facing the second region.

Citation Information

Patent Citations

  • Alkaline storage battery

    JP1998284116A

  • Alkaline storage battery

    JP1998284117A

  • Nonaqueous electrolyte battery, electrode for nonaqueous electrolyte battery, and manufacturing method of this electrode for nonaqueous electrolyte battery

    JP2007123237A

  • Nonaqueous electrolyte secondary battery

    JP2013218898A

  • Electrochemical device

    JP2014116237A