Prepreg for printed circuit board, metal laminate plate, and printed circuit board

The prepreg for printed circuit boards addresses noise suppression by controlling dielectric constants and loss tangents, and optimizing copper foil curing and microstrip line formation to enhance noise resistance and adhesiveness, effectively reducing impedance mismatch.

JP2024167001APending Publication Date: 2024-11-29SUMITOMO BAKELITE CO LTD

Patent Information

Application Number
JP2023083503
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing printed circuit boards face challenges in suppressing noise generation due to the deterioration of resistance to noise with faster and more highly integrated semiconductor components, which is not effectively addressed by current prepregs.

Method used

A prepreg for printed circuit boards is developed with a fiber base material and a thermosetting resin composition, where the dielectric constant difference is controlled to 2.5 or less at 10 GHz, dielectric loss tangent is between 0.0005 and 0.005, and the area without fiber base material is 30% or less, along with specific copper foil curing and microstrip line formation to achieve optimal impedance matching.

Benefits of technology

The prepreg effectively suppresses noise generation in printed circuit boards by ensuring minimal impedance mismatch and reduced dielectric loss, enhancing the resistance to noise and improving adhesiveness between prepreg and metal layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167001000001_ABST
    Figure 2024167001000001_ABST
Patent Text Reader

Abstract

To provide a prepreg for a printed circuit board which realizes an excellent resistance to noise of an electronic apparatus.SOLUTION: The prepreg for a printed circuit board of the present invention includes a fiber base material and a resin composition. The difference between the dielectric constant of the fiber base material at 10GHz and the dielectric constant of the resin composition at 10GHz in a cured body of the prepreg for a printed circuit board is 2.5 at largest. The dielectric tangent of the cured body of the prepreg for a printed circuit board at 10GHz is in the range from 0.0005 to 0.005, both inclusive. The ratio of the region which does not include the fiber base material of the prepreg for a printed circuit board is 30% at largest.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a prepreg for printed circuit boards, a metal-clad laminate, and a printed circuit board.

[0002] In recent years, advances in semiconductor technology have led to increased speed and power saving in semiconductor components, and the functionality of electronic devices has improved dramatically.

[0003] However, the use of semiconductor LC and LCI, which are becoming faster, more highly integrated, and consume less power, tends to deteriorate the resistance of electronic devices to noise, etc. For this reason, in recent years, there has been a demand for prepregs for printed circuit boards that realize excellent resistance to noise, etc. in electronic devices. For example, the technology described in Patent Document 1 is known. Patent Document 1 describes a polyphenylene ether resin composition containing a modified polyphenylene ether copolymer, a crosslinking curing agent, and an inorganic filler. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-113543 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a prepreg for a printed circuit board, which realizes a printed circuit board that suppresses the generation of noise. [Means for solving the problem]

[0006] The present inventors have conducted intensive research to solve the above problems. As a result, they have found that, in a prepreg for printed circuit boards including a fiber base material and a thermosetting resin composition, by controlling the difference between the relative dielectric constant of the fiber base material at 10 GHz and the relative dielectric constant of the thermosetting resin composition at 10 GHz to 2.5 or less, controlling the dielectric loss tangent of the cured body of the prepreg for printed circuit boards at 10 GHz to 0.0005 or more and 0.005 or less, and controlling the proportion of the region not including the fiber base material included in the prepreg for printed circuit boards measured by a specific method to 30% or less, excellent resistance to noise of electronic devices can be realized, and the present invention has been completed.

[0007] According to the present invention, there are provided the following prepreg for printed circuit boards, metal-clad laminate, and printed circuit board. [1] A prepreg for printed circuit boards comprising a fiber base material and a thermosetting resin composition, In a cured product of the prepreg for printed circuit boards, the difference between the relative dielectric constant of the fiber base material at 10 GHz and the relative dielectric constant of the thermosetting resin composition at 10 GHz is 2.5 or less, The dielectric loss tangent of the cured body of the prepreg for printed circuit boards at 10 GHz is 0.0005 or more and 0.005 or less, A prepreg for printed circuit boards, in which the proportion of areas not containing a fiber base material in the prepreg for printed circuit boards is 30% or less, as measured by the following procedure 1. (Step 1) (1) Using a microscope, an image of the prepreg from the out-of-plane direction is obtained. (2) The image obtained in (1) above is binarized. The threshold color is set to black and white, and anything below 30 out of 256 gradations is set to black. (3) The ratio of black areas after binarization is regarded as the ratio of areas that do not contain fiber base material. [2] Z, which is measured in step 2 below 0MD (t) satisfies the following condition 1: [1] A prepreg for printed circuit boards. (Step 2) 1. Place 18 μm copper foil on both sides of the prepreg, which has a thickness of 50 μm or more and 100 μm or less, and heat and harden it for 2 to 3 hours under conditions of a temperature of 200° C. to 250° C. and a load of 3 MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in any MD direction. 4. For each microstrip line formed in the MD direction, the characteristic impedance Z is measured using a network analyzer, and a microstrip line with a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines with a Z value in the range of 50Ω to 60Ω, the microstrip line with the smallest Z value is selected. The characteristic impedance of the selected microstrip line is then designated as Z1. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 0MD Measure (t). (Condition 1) In the time domain, which corresponds to the area where the microstrip line is formed, Z 0MD (t) is greater than or equal to (Z1-5)Ω and less than or equal to (Z1+5)Ω. [3] Z, which is measured in step 3 below 0TD (t) satisfies the following condition 2, [2] A prepreg for printed circuit boards. (Step 3) 1. Place 18 μm copper foil on both sides of the prepreg, which has a thickness of 50 μm or more and 100 μm or less, and heat and harden it for 2 to 3 hours under conditions of a temperature of 200° C. to 250° C. and a load of 3 MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in the TD direction perpendicular to the MD direction. 4. For each microstrip line formed in the TD direction, the characteristic impedance Z is measured using a network analyzer, and a microstrip line with a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines with a Z value in the range of 50Ω to 60Ω, the microstrip line with the smallest Z value is selected. The characteristic impedance of the selected microstrip line is designated as Z2. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 0TD Measure (t). (Condition 2) In the time domain, which corresponds to the area where the microstrip line is formed, Z 0TD (t) is greater than or equal to (Z2-5)Ω and less than or equal to (Z2+5)Ω. [4] Z, which is measured in step 4 below. 045° (t) satisfies condition 3 below, [3] A prepreg for printed circuit boards. (Step 4) 1. Place 18 μm copper foil on both sides of the prepreg, which has a thickness of 50 μm or more and 100 μm or less, and heat and harden it for 2 to 3 hours under conditions of a temperature of 200° C. to 250° C. and a load of 3 MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in a direction at 45° to the MD direction. 4. For each microstrip line formed at 45° to the MD direction, measure the characteristic impedance Z using a network analyzer, and select a microstrip line whose Z value is in the range of 50Ω to 60Ω. If there are multiple microstrip lines whose Z value is in the range of 50Ω to 60Ω, select the microstrip line whose Z value is the smallest. Then, the characteristic impedance of the selected microstrip line is designated as Z3. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 045° Measure (t). (Condition 3) In the time domain, which corresponds to the area where the microstrip line is formed, Z 045° (t) is greater than or equal to (Z3-5)Ω and less than or equal to (Z3+5)Ω. [5] The thermosetting resin composition contains silica particles. [1] to [4]. A prepreg for printed circuit boards. [6] The silica particles are present in an amount of 45% by mass or more and 65% by mass or less based on the total amount of the thermosetting resin composition. [5] A prepreg for printed circuit boards. [7] The thermosetting resin composition contains polyphenylene ether. [1] to [6], the prepreg for printed circuit boards. [8] The thermosetting resin composition contains a bismaleimide resin. [1] to [7], the prepreg for printed circuit boards. [9] The thermosetting resin composition contains styrene-butadiene rubber. [1] to [8]. A prepreg for printed circuit boards.

[10] The thermosetting resin composition includes a crosslinking agent. [1] to [9], a prepreg for printed circuit boards.

[11] The crosslinking agent contains a triallyl isocyanurate ring.

[10] A prepreg for printed circuit boards.

[12] A metal-clad laminate comprising a cured product of the prepreg for printed circuit boards according to any one of [1] to

[11] .

[13] A printed circuit board comprising the metal-clad laminate according to

[12] . Effect of the Invention

[0008] According to the present invention, there is provided a prepreg for a printed circuit board, which realizes a printed circuit board that suppresses the generation of noise. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram showing an example of an image of the prepreg according to the present embodiment from an out-of-plane direction. [Diagram 2] FIG. 1 is a diagram showing the measurement results of characteristic impedance of a prepreg in an example by a TDR method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference numerals and their explanations will be omitted as appropriate. Also, the drawings are schematic diagrams and do not correspond to the actual dimensional ratios.

[0011] [Definition and Overview of Prepreg] The prepreg according to the present embodiment is configured to include a fiber substrate in a thermosetting resin composition. The prepreg is obtained by impregnating a fiber substrate with the thermosetting resin composition. For example, the prepreg is obtained by impregnating a fiber substrate with a thermosetting resin composition and then semi-curing the fiber substrate. The prepreg is excellent in various properties such as dielectric properties and mechanical and electrical connection reliability under high temperature and humidity, and is suitable for manufacturing an insulating layer of a printed circuit board.

[0012] The prepreg according to this embodiment can be used, for example, to form an insulating layer or a build-up layer in a core layer of a printed wiring board.

[0013] 1 shows an example of an image of the prepreg according to this embodiment taken from the out-of-plane direction using a microscope (DSX-500 manufactured by Olympus Corporation). The fiber base material contained in the prepreg includes warp yarns 110 and weft yarns 120. The prepreg has a region 130 that does not include the fiber base material. The region 130 that does not include the fiber base material tends to have a smaller parasitic capacitance after thermal curing than other regions that include the fiber base material.

[0014] In the prepreg according to the present embodiment, the ratio of the region not containing the fiber base material is preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less, as measured by the following procedure 1. This allows a printed circuit board manufactured using the prepreg to have excellent resistance to noise and the like. (Step 1) (1) Using a microscope (Olympus: DSX-500), an image of the substrate prepreg from the out-of-plane direction is obtained. (2) The image obtained in (1) above is binarized. The threshold color is set to black and white, and anything below 30 out of 256 gradations is set to black. (3) The ratio of black areas after binarization is regarded as the ratio of areas that do not contain fiber base material.

[0015] In addition, in the cured product of the prepreg according to the present embodiment, the difference between the dielectric constant of the fiber base material and the dielectric constant of the thermosetting resin composition is preferably 2.5 or less, more preferably 2.0 or less, and even more preferably 1.7 or less. This allows the printed circuit board manufactured using the prepreg to have excellent resistance to noise and the like. In this specification, the dielectric constant is measured by a cavity resonator method at a frequency of 10 GHz.

[0016] In addition, the dielectric loss tangent of the cured body of the prepreg according to the present embodiment is preferably 0.005 or less, more preferably 0.004 or less. This allows the dielectric loss to be reduced in a printed circuit board manufactured using the prepreg. In addition, the dielectric loss tangent of the cured body of the prepreg is preferably 0.0005 or more, more preferably 0.001 or more. This allows the adhesion between the prepreg and the metal to be improved when a printed circuit board is manufactured using the prepreg. In this specification, the dielectric loss tangent refers to that measured by a cavity resonator method at a frequency of 10 GHz.

[0017] Furthermore, the characteristic impedance of the wiring on a printed circuit board is determined by a distributed constant consisting of parasitic inductance and parasitic capacitance. The characteristic impedance Z0 is expressed as √(L / C), where L is the parasitic inductance per unit length and C is the parasitic capacitance per unit length. In other words, if there is variation in the parasitic capacitance on a printed circuit board, this will cause mismatched parts of the characteristic impedance in the wiring on that printed circuit board. Signals will be reflected in the mismatched parts of the characteristic impedance, which will cause noise.

[0018] One method for evaluating the characteristic impedance is the TDR method, which measures the characteristic impedance of a sample by injecting a high-speed pulse signal into the sample and measuring the reflected voltage.

[0019] As mentioned above, the incident wave is reflected by the characteristic impedance mismatch. The reflection coefficient ρ is expressed as Z L , the known characteristic impedance is Z O Then, ρ=(Z L -Z O ) / (Z L +Z O Based on the reflection coefficient ρ, Z L The principle of the TDR method is to determine

[0020] The prepreg according to this embodiment has a Z 0MD (t) is preferably (Z1-5)Ω or more and (Z1+5)Ω or less, more preferably (Z1-4)Ω or more and (Z1+4)Ω or less, and even more preferably (Z1-3)Ω or more and (Z1+3)Ω or less. Note that the MD direction in the following step 2 is, for example, the longitudinal direction of the prepreg. (Step 2) 1. Place 18 μm copper foil on both sides of the prepreg, which has a thickness of 50 μm or more and 100 μm or less, and heat and harden it for 2 to 3 hours under conditions of a temperature of 200° C. to 250° C. and a load of 3 MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in any MD direction. 4. For each microstrip line formed in the MD direction, the characteristic impedance Z is measured using a network analyzer, and a microstrip line with a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines with a Z value in the range of 50Ω to 60Ω, the microstrip line with the smallest Z value is selected. The characteristic impedance of the selected microstrip line is then designated as Z1. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 0MD Measure (t).

[0021] In addition, the prepreg according to this embodiment has a Z 0TD (t) is preferably from (Z2-5)Ω to (Z2+5)Ω, more preferably from (Z2-4)Ω to (Z2+4)Ω, and even more preferably from (Z2-3)Ω to (Z2+3)Ω. (Step 3) 1. Place 18 μm copper foil on both sides of the prepreg, which has a thickness of 50 μm or more and 100 μm or less, and heat and harden it for 2 to 3 hours under conditions of a temperature of 200° C. to 250° C. and a load of 3 MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in the TD direction perpendicular to the MD direction. 4. For each microstrip line formed in the TD direction, the characteristic impedance Z is measured using a network analyzer, and a microstrip line with a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines with a Z value in the range of 50Ω to 60Ω, the microstrip line with the smallest Z value is selected. The characteristic impedance of the selected microstrip line is designated as Z2. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 0TD Measure (t).

[0022] In addition, the prepreg according to this embodiment has a Z 045° (t) is preferably from (Z3-5)Ω to (Z3+5)Ω, more preferably from (Z3-4)Ω to (Z3+4)Ω, and even more preferably from (Z3-3)Ω to (Z3+3)Ω. (Step 4) 1. Place 18 μm copper foil on both sides of the prepreg, which has a thickness of 50 μm or more and 100 μm or less, and heat and harden it for 2 to 3 hours under conditions of a temperature of 200° C. to 250° C. and a load of 3 MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in a direction at 45° to the MD direction. 4. For each microstrip line formed at 45° to the MD direction, measure the characteristic impedance Z using a network analyzer, and select a microstrip line whose Z value is in the range of 50Ω to 60Ω. If there are multiple microstrip lines whose Z value is in the range of 50Ω to 60Ω, select the microstrip line whose Z value is the smallest. Then, the characteristic impedance of the selected microstrip line is designated as Z3. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 045° Measure (t).

[0023] Hereinafter, each material constituting the prepreg according to this embodiment will be described in detail.

[0024] [Fiber base material] Examples of the fiber substrate include glass cloth, woven cloth containing an inorganic compound other than glass as a component, and woven cloth containing an organic compound such as aromatic polyamideimide resin, polyamide resin, aromatic polyester resin, polyester resin, polyimide resin, fluororesin, etc. Among these, glass cloth is particularly preferred from the viewpoint of the mechanical strength of the prepreg.

[0025] As the glass cloth, for example, a glass fiber substrate made of one or more types of glass selected from E glass, S glass, D glass, T glass, NE glass, NE-R glass, UT glass, L glass, HP glass, and quartz glass is preferably used. Among these, NE glass and NE-R glass are preferred because they have an excellent balance between the relative dielectric constant and strength and are relatively inexpensive.

[0026] From the viewpoint of reducing the range of variation in parasitic capacitance value for each portion of the printed circuit board, the material of the fiber base material preferably has a relative dielectric constant of 6.8 or less, more preferably 5.5 or less, and even more preferably 4.8 or less.

[0027] From the viewpoint of reducing dielectric loss in the printed circuit board, the fiber base material preferably has a dielectric loss tangent of 0.01 or less, more preferably 0.008 or less, and even more preferably 0.003 or less.

[0028] The thickness of the fiber substrate is not particularly limited, but is preferably 5 μm or more and 150 μm or less, more preferably 10 μm or more and 100 μm or less, and even more preferably 12 μm or more and 90 μm or less. By using a fiber substrate having such a thickness, the handling property during the production of the prepreg can be further improved. When the thickness of the fiber substrate is equal to or less than the upper limit, the impregnation property of the thermosetting resin composition in the fiber substrate is improved, and the occurrence of strand voids and a decrease in insulation reliability can be suppressed. In addition, the formation of through holes by a laser such as carbon dioxide gas, UV, or excimer can be facilitated. In addition, when the thickness of the fiber substrate is equal to or more than the lower limit, the strength of the fiber substrate and the prepreg can be improved. As a result, the handling property is improved, and the production of the prepreg becomes easier.

[0029] The content of the fiber base material is, for example, preferably 5% by volume to 45% by volume, more preferably 10% by volume to 40% by volume, and even more preferably 15% by volume to 30% by volume, when the entire prepreg is taken as 100% by volume, which makes it possible to achieve both the strength of the prepreg and a small variation range of the parasitic capacitance value for each part of the printed circuit board.

[0030] [Thermosetting resin composition] The relative dielectric constant of the thermosetting resin composition according to the present embodiment is preferably different from the relative dielectric constant of the fiber substrate by 2.5 or less. The relative dielectric constant of the thermosetting resin composition is, for example, preferably 2.0 or more and 5.0 or less, more preferably 2.5 or more and 4.5 or less, and most preferably 3.0 or more and 4.0 or less.

[0031] The thermosetting resin composition of the present embodiment is not particularly limited as long as it is curable by heat, and may be, for example, one or a combination of two or more selected from epoxy resins, phenolic resins, bismaleimide resins, coumarone resins, polyphenylene ethers, styrene-butadiene copolymers, and the like.

[0032] [Bismaleimide resin] The thermosetting resin composition preferably contains a bismaleimide resin. This can improve the strength of the cured prepreg. The bismaleimide resin is a (co)polymer of a compound having two or more maleimide groups. The compound having two or more maleimide groups includes, for example, a compound represented by the following general formula (1).

[0033] [ka]

[0034] In the above general formula (1), R 11 is a divalent organic group having 1 to 30 carbon atoms, which may contain at least one of an oxygen atom and a nitrogen atom. 11 More preferably, R is an organic group containing an aromatic ring. 11 Examples of such a copolymer include structures of the following general formula (2) or (3), with the structure (3) being more preferred from the viewpoint of improving the strength of the cured prepreg.

[0035] [ka]

[0036] In the above general formula (2), R 21 is a divalent organic group having 1 to 18 carbon atoms which may contain at least one of an oxygen atom and a nitrogen atom. 22 are each independently a hydrogen atom or a substituted or unsubstituted hydrocarbon group having 1 to 4 carbon atoms.

[0037] [ka]

[0038] In the above general formula (3), n is an average value and is a number from 1 to 5, preferably from 1 to 5, more preferably from 1 to 3, and even more preferably from 1 to 2.

[0039] The lower limit of the content of the bismaleimide resin is preferably 10% by mass or more, more preferably 12% by mass or more, and even more preferably 14% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. This can improve the strength of the cured prepreg. The upper limit of the content of the bismaleimide resin is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, when the entire thermosetting resin composition is taken as 100% by mass. This can reduce the dielectric constant of the cured prepreg.

[0040] [Cumarone resin] The thermosetting resin composition preferably contains a coumarone resin. This can reduce the dielectric constant and dielectric loss tangent of the cured prepreg. The coumarone resin is a (co)polymer having an average degree of polymerization of 4 to 8 and containing structural units derived from coumarone monomers.

[0041] The structural unit derived from the coumarone monomer is, for example, represented by the following general formula (4). [ka]

[0042] In general formula (4), R 41 is hydrogen or an organic group having 1 to 3 carbon atoms. 41 may be the same as each other or different from each other.

[0043] The coumarone resin is preferably a coumarone-indene resin, which is a copolymer with indene (C9H8). The coumarone-indene resin contains a structural unit derived from a coumarone monomer and a structural unit derived from an indene monomer. The coumarone-indene resin may further contain a structural unit derived from another monomer. The coumarone-indene resin may contain, for example, a structural unit derived from a styrene monomer.

[0044] The structural unit derived from the indene monomer is, for example, represented by the following general formula (5). [ka]

[0045] In general formula (5), R 51 From R 57 are each independently a hydrogen atom or an organic group having 1 to 3 carbon atoms.

[0046] The structural unit derived from the styrene-based monomer is, for example, represented by the following general formula (6).

[0047] [ka]

[0048] In general formula (6), R 61 is hydrogen or an organic group having 1 to 3 carbon atoms. 61 may be the same as each other or different from each other.

[0049] In the above general formulas (4) to (6), R 41 , R 51 From R 57 , and R C61 For example, the organic group structure may contain atoms other than hydrogen and carbon, specifically, one or more of oxygen atoms, nitrogen atoms, sulfur atoms, phosphorus atoms, silicon atoms, fluorine atoms, chlorine atoms, and the like.

[0050] In the above general formulas (4) to (6), R 41 , R 51 From R 57 , and R C61 The organic groups constituting each are, for example, independently hydrogen or an organic group having 1 to 3 carbon atoms, preferably hydrogen or an organic group having 1 carbon atom, and more preferably hydrogen.

[0051] In the above general formulas (4) to (6), R41 , R 51 From R 57 , and R 61 The organic groups constituting the formula (I) include alkyl groups such as methyl, ethyl, and n-propyl groups; alkenyl groups such as allyl and vinyl groups; alkynyl groups such as ethynyl groups; alkylidene groups such as methylidene and ethylidene groups; cycloalkyl groups such as cyclopropyl groups; and heterocyclic groups such as epoxy and oxetanyl groups.

[0052] The coumarone-indene resin may also contain a reactive group in the molecule that reacts with the epoxy group of the epoxy resin. This can further reduce the dielectric constant of the cured prepreg. Specifically, it may contain an OH group, a COOH group, etc. The coumarone-indene resin may also contain an aromatic structure having a phenolic hydroxyl group inside or at the end.

[0053] The upper limit of the weight average molecular weight Mw of the coumarone-indene resin is, for example, preferably 4000 or less, more preferably 2000 or less, even more preferably 1500 or less, and even more preferably 1200 or less. This improves the compatibility of the coumarone-indene resin, and allows the coumarone-indene resin to be appropriately dispersed. On the other hand, the lower limit of the weight average molecular weight Mw of the coumarone-indene resin is, for example, preferably 400 or more, more preferably 500 or more, even more preferably 550 or more, and even more preferably 600 or more. This allows the coumarone-indene resin to be appropriately dispersed.

[0054] The lower limit of the content of the coumarone-indene resin is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. This allows the dielectric constant and dielectric loss tangent of the cured prepreg to be small. Furthermore, the upper limit of the content of the coumarone-indene resin is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, when the entire thermosetting resin composition of this embodiment is taken as 100% by mass. This allows the heat resistance of the cured prepreg to be improved by setting the upper limit of the content of the coumarone-indene resin to the above-mentioned value or less.

[0055] [Polyphenylene ether] The thermosetting resin composition preferably contains polyphenylene ether, which can improve the heat resistance of the printed circuit board. The polyphenylene ether is not particularly limited as long as it contains one or more functional groups in the molecule that undergo a crosslinking reaction with a crosslinking agent.

[0056] Polyphenylene ether is, for example, a polymer having a structural unit represented by the following general formula (7).

[0057] [ka]

[0058] In the above general formula (7), R 71 , R 72 , R 73 , R 74 may be the same or different and are, for example, a hydrogen atom, a halogen atom, an optionally substituted alkyl group, an optionally substituted alkenyl group, an optionally substituted alkynyl group, an optionally substituted aryl group, an optionally substituted aralkyl group, and an optionally substituted alkoxy group.

[0059] The halogen atom is, for example, a fluorine atom, a chlorine atom, a bromine atom, etc. A chlorine atom or a bromine atom is preferable.

[0060] The "alkyl group" in the above-mentioned optionally substituted alkyl group is, for example, a linear or branched alkyl group having a carbon number of 1 or more and 6 or less, preferably a carbon number of 1 or more and 3 or less. More specifically, it is a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, etc., and a methyl group or an ethyl group is more preferable.

[0061] The "alkenyl group" of the above-mentioned optionally substituted alkenyl group is, for example, an ethenyl group, a 1-propenyl group, a 2-propenyl group, a 3-butenyl group, a pentenyl group, a hexenyl group, etc., and an ethenyl group or a 1-propenyl group is more preferable.

[0062] The "alkynyl group" in the above-mentioned optionally substituted alkynyl group is, for example, an ethynyl group, a 1-propynyl group, a 2-propynyl (propargyl) group, a 3-butynyl group, a pentynyl group, a hexynyl group, etc., and is more preferably an ethynyl group, a 1-propynyl group, or a 2-propynyl (propargyl) group.

[0063] The "aryl group" of the above-mentioned optionally substituted aryl group is, for example, a phenyl group, a naphthyl group, etc., and a phenyl group is more preferable.

[0064] The "aralkyl group" of the above-mentioned optionally substituted aralkyl group is, for example, a benzyl group, a phenethyl group, a 2-methylbenzyl group, a 4-methylbenzyl group, an α-methylbenzyl group, a 2-vinylphenethyl group, a 4-vinylphenethyl group, etc., and is more preferably a benzyl group.

[0065] The "alkoxy group" of the above-mentioned alkoxy group which may be substituted is, for example, a straight-chain or branched-chain alkoxy group having a carbon number of 1 to 6, preferably a carbon number of 1 to 3. Examples thereof include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, etc., and a methoxy group or an ethoxy group is more preferable.

[0066] When the above alkyl group, aryl group, alkenyl group, alkynyl group, aralkyl group, and alkoxy group are substituted, they may have one or more substituents. Such substituents are, for example, halogen atoms (e.g., fluorine atom, chlorine atom, bromine atom), alkyl groups having 1 to 6 carbon atoms (e.g., methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group), aryl groups (e.g., phenyl group, naphthyl group), alkenyl groups (e.g., ethenyl group, 1-propenyl group, 2-propenyl group), alkynyl groups (e.g., ethynyl group, 1-propynyl group, 2-propynyl group), aralkyl groups (e.g., benzyl group, phenethyl group), alkoxy groups (e.g., methoxy group, ethoxy group), etc. The polyphenylene ether may have a structural unit represented by the following general formula (8).

[0067] [ka]

[0068] In the above general formula (8), R 81 ,R 82 ,R 83 ,R 84 ,R 85 ,R 86 ,R 87 ,R 88 may be the same or different and are a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group. -A- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.

[0069] The polyphenylene ether may include modified polyphenylene ethers which are functionalized in part or in whole with ethylenically unsaturated groups such as vinylbenzyl groups, epoxy groups, amino groups, hydroxyl groups, mercapto groups, carboxyl groups, silyl groups, and the like.

[0070] In addition, it is preferable that the polyphenylene ether has a hydroxy group, an epoxy group, or an ethylenically unsaturated group at both ends. The ethylenically unsaturated group is, for example, an alkenyl group such as a methacrylate group, an ethenyl group, an allyl group, a methacrylic group, a propenyl group, a butenyl group, a hexenyl group, and an octenyl group, a cycloalkenyl group such as a cyclopentenyl group and a cyclohexenyl group, and an alkenylaryl group such as a vinylbenzyl group and a vinylnaphthyl group. In addition, both ends may be the same functional group or different functional groups.

[0071] The weight average molecular weight of the polyphenylene ether is preferably 500 to 5000, more preferably 1000 to 4000. By making the weight average molecular weight of the polyphenylene ether equal to or greater than the lower limit, the flexibility of the prepreg can be improved. On the other hand, by making the weight average molecular weight of the polyphenylene ether equal to or less than the upper limit, the solubility of the polyphenylene ether can be improved.

[0072] The lower limit of the polyphenylene ether content is preferably 5% by mass or more, more preferably 6% by mass or more, and even more preferably 7% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. This can improve the heat resistance of the cured body of the prepreg. Furthermore, the upper limit of the polyphenylene ether content is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, when the entire thermosetting resin composition of this embodiment is taken as 100% by mass. This can improve the compatibility of the polyphenylene ether.

[0073] [Styrene-butadiene copolymer] The thermosetting resin composition preferably contains a styrene-butadiene copolymer. This can improve the strength of the cured prepreg. The styrene-butadiene copolymer is a copolymer containing a structural unit derived from a styrene-based monomer and a structural unit derived from a diene-based monomer. The styrene-butadiene copolymer is more preferably an elastomer such as styrene-butadiene rubber.

[0074] The structural unit derived from a styrene-based monomer includes, for example, a structural unit represented by the following general formula (9).

[0075] [ka]

[0076] In the general formula (9), R 91 is a hydrogen atom or an alkyl group, and R 92 is an alkyl group, and n is an integer of 0 to 5.

[0077] In the styrene-butadiene copolymer, the content of structural units derived from styrene-based monomers in all structural units in the styrene-butadiene copolymer is preferably 10 mol% or more and 90 mol% or less, more preferably 15 mol% or more and 85 mol% or less, even more preferably 20 mol% or more and 80 mol% or less, particularly more preferably 30 mol% or more and 80 mol% or less, and most preferably 40 mol% or more and 80 mol% or less.

[0078] The structural unit derived from a diene monomer includes, for example, a structural unit represented by the following general formula (10).

[0079] [ka]

[0080] In the general formula (10), R a1 is a hydrogen atom or an alkyl group.

[0081] In the styrene-butadiene copolymer, the content of structural units derived from diene monomers in all structural units in the styrene-butadiene copolymer is preferably 10 mol% or more and 90 mol% or less, more preferably 15 mol% or more and 85 mol% or less, even more preferably 20 mol% or more and 80 mol% or less, particularly more preferably 30 mol% or more and 80 mol% or less, and most preferably 40 mol% or more and 80 mol% or less.

[0082] The lower limit of the content of the styrene-butadiene copolymer is preferably 2% by mass or more, more preferably 3% by mass or more, and even more preferably 4% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. This can improve the heat resistance of the prepreg. The upper limit of the content of the polyphenylene ether is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, when the entire thermosetting resin of this embodiment is taken as 100% by mass. This can suppress a decrease in the oxidation resistance of the prepreg.

[0083] [Filling material] The thermosetting resin composition according to the present embodiment may contain a filler. This allows the cured body of the prepreg to have a low linear expansion coefficient while suppressing water absorption. As the filler, for example, one or a combination of two or more selected from the following can be used: silicates such as talc, calcined clay, uncalcined clay, mica, and glass; oxides such as titanium oxide, alumina, boehmite, silica, and fused silica; carbonates such as calcium carbonate, magnesium carbonate, and hydrotalcite; hydroxides such as aluminum hydroxide, magnesium hydroxide, and calcium hydroxide; sulfates or sulfites such as barium sulfate, calcium sulfate, and calcium sulfite; borates such as zinc borate, barium metaborate, aluminum borate, calcium borate, and sodium borate; nitrides such as aluminum nitride, boron nitride, silicon nitride, and carbon nitride; and titanates such as strontium titanate and barium titanate. Among these, silica is preferred.

[0084] The lower limit of the average particle size of the filler is not particularly limited, but may be, for example, 0.01 μm or more, or 0.05 μm or more. From the viewpoint of stably obtaining a low linear expansion coefficient, it is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1.0 μm or more. This can suppress the viscosity of the varnish using the thermosetting resin composition of this embodiment from increasing, and can improve workability. In addition, the upper limit of the average particle size of the filler is not particularly limited, but is, for example, preferably 5.0 μm or less, more preferably 2.0 μm or less, and even more preferably 1.5 μm or less. This can suppress phenomena such as the sedimentation of the filler in the varnish of the thermosetting resin.

[0085] In this embodiment, the average particle size of the filler can be determined by measuring the particle size distribution of the particles on a volume basis using, for example, a laser diffraction particle size distribution measuring device (LA-500, manufactured by HORIBA Corporation), and taking the median size (D50) thereof.

[0086] The lower limit of the content of the inorganic filler is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 45% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. This allows the printed circuit board to have a low thermal expansion. The upper limit of the content of the inorganic filler is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 55% by mass or less, when the entire thermosetting resin composition is taken as 100% by mass. This improves handling properties and makes it easier to form a prepreg.

[0087] [Crosslinking agent] The thermosetting resin composition may include a crosslinking agent. The crosslinking agent may include at least one of an addition polymerization type and a radical polymerization type.

[0088] The crosslinking agent is, for example, one or a combination of two or more selected from maleimide compounds, cyanate ester resins, phenolic resins, epoxy resins, and compounds having two or more carbon-carbon unsaturated double bonds in one molecule.

[0089] As the compound having two or more carbon-carbon unsaturated double bonds in one molecule, a trialkenyl isocyanurate compound such as triallyl isocyanurate (TAIC) represented by chemical formula (11) is particularly preferred.

[0090] [ka]

[0091] The lower limit of the content of the crosslinking agent is preferably 10% by mass or more, more preferably 12% by mass or more, and even more preferably 14% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. This can improve the curability of the prepreg. The upper limit of the content of the crosslinking agent is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less, when the entire thermosetting resin composition is taken as 100% by mass. This can prevent the dielectric constant of the printed circuit board from becoming high.

[0092] [Coupling agent] The thermosetting resin composition may contain a coupling agent. As the coupling agent, an allyl isocyanurate-based silane coupling agent represented by chemical formula (12) is particularly preferable.

[0093] [ka]

[0094] The lower limit of the content of the coupling agent is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.8% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. The upper limit of the content of the coupling agent is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, when the entire thermosetting resin composition is taken as 100% by mass.

[0095] [Leveling agent] The thermosetting resin composition may contain a leveling agent, such as an acrylic copolymer, such as a polyacrylate compound.

[0096] The lower limit of the content of the leveling agent is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.3% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. This allows the coating surface uniformity of the thermosetting resin composition to be improved. The upper limit of the content of the leveling agent is preferably 1% by mass or less, more preferably 0.7% by mass or less, and even more preferably 0.5% by mass or less, when the entire thermosetting resin composition is taken as 100% by mass. This allows the coating surface uniformity of the thermosetting resin composition to be compatible with other performances.

[0097] [Radical initiator] The thermosetting resin composition may contain a radical initiator. The radical initiator is not particularly limited as long as it can promote the reaction between the thermosetting resin and the crosslinking agent. The radical initiator can promote the polymerization reaction of the radical polymerization type crosslinking agent.

[0098] The radical initiator is, for example, one or a combination of two or more organic peroxides such as α,α'-di(t-butylperoxy)diisopropylbenzene, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, benzoyl peroxide, 3,3',5,5'-tetramethyl-1,4-diphenoquinone, chloranil, 2,4,6-tri-t-butylphenoxyl, t-butylperoxyisopropyl monocarbonate, azobisisobutyronitrile, etc. Among these, it is particularly preferable to include α,α'-di(t-butylperoxy)diisopropylbenzene.

[0099] The lower limit of the content of the radical initiator is preferably 0.5% by mass or more, more preferably 0.7% by mass or more, and even more preferably 0.9% by mass or more, when the entire thermosetting resin composition is taken as 100% by mass. This can improve the curability of the prepreg. The upper limit of the content of the radical initiator is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, when the entire thermosetting resin composition is taken as 100% by mass. This can reduce the dielectric constant of the cured prepreg.

[0100] [Method of manufacturing varnish resin] In the present embodiment, the varnish-like thermosetting resin composition may contain a solvent, which may be one or a combination of two or more selected from, for example, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, ethyl acetate, cyclohexane, heptane, cyclohexane, cyclohexanone, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene glycol, cellosolve-based solvents, carbitol-based solvents, anisole, and N-methylpyrrolidone.

[0101] When the thermosetting resin composition is in the form of a varnish, the solid content of the thermosetting resin composition is, for example, preferably 30% by mass or more and 80% by mass or less, and more preferably 40% by mass or more and 70% by mass or less, when the entire thermosetting resin composition is taken as 100% by mass. This allows a thermosetting resin composition with excellent workability and film-forming properties to be obtained.

[0102] The varnish-like thermosetting resin composition can be prepared by dissolving, mixing, and stirring the above-mentioned components in a solvent using various mixers such as those used in an ultrasonic dispersion system, a high-pressure collision dispersion system, a high-speed rotation dispersion system, a bead mill system, a high-speed shear dispersion system, and a rotation-revolution dispersion system.

[0103] [Prepreg manufacturing method] The prepreg according to the present embodiment can be formed, for example, by impregnating a fiber substrate with a thermosetting resin composition and then semi-curing the composition. The method of impregnating a fiber substrate with a thermosetting resin composition is not particularly limited, but includes, for example, a method of dissolving the thermosetting resin composition in a solvent to prepare a varnish and immersing the fiber substrate in the varnish, a method of applying the varnish to the fiber substrate with various coaters, a method of spraying the varnish to the fiber substrate with a spray, and a method of laminating both sides of the fiber substrate with a resin film made of a thermosetting resin composition.

[0104] When the prepreg is used to form an insulating layer in a core layer of a printed wiring board, for example, two or more prepregs can be stacked and the resulting laminate can be heat-cured to form an insulating layer for the core layer.

[0105] [Metal-clad laminate manufacturing method] The metal-clad laminate of this embodiment has a structure in which a metal layer is disposed on at least one surface of the prepreg.

[0106] The method for producing the metal-clad laminate is, for example, as follows. A metal foil is placed on both the upper and lower sides or one side of the outer side of a prepreg or a laminate of two or more prepregs, and these are bonded under high vacuum conditions using a laminator or Becquerel device, or a metal foil is placed on both the upper and lower sides or one side of the outer side of the prepreg as is. When two or more prepregs are laminated, a metal foil is placed on both the upper and lower sides or one side of the outermost side of the laminated prepregs. Next, the laminate of the prepreg and the metal foil is heated and pressurized to obtain a metal-clad laminate. Here, it is preferable to continue pressing until the end of cooling during the heating and pressurizing.

[0107] Examples of the metal constituting the metal foil include copper, copper-based alloys, aluminum, aluminum-based alloys, silver, silver-based alloys, gold, gold-based alloys, zinc, zinc-based alloys, nickel, nickel-based alloys, tin, tin-based alloys, iron, iron-based alloys, Fe-Ni-based alloys such as Kovar (trade name), 42 alloy, Invar, and Super Invar, W, and Mo. Among these, the metal constituting the metal foil is preferably copper or a copper alloy because it has excellent conductivity, is easy to form a circuit by etching, and is inexpensive. That is, the metal foil is preferably copper foil. In addition, the metal foil may be a metal foil with a carrier. The thickness of the metal foil is preferably 0.5 μm or more and 20 μm or less, more preferably 1.5 μm or more and 18 μm or less.

[0108] [Printed circuit board manufacturing method] In this embodiment, a printed wiring board is produced using the above-mentioned prepreg or metal-clad laminate. The printed wiring board of this embodiment includes a cured product of the above-mentioned prepreg and a wiring pattern provided on both sides or one side of the cured product. Other configurations of the printed wiring board of this embodiment are not particularly limited, and may include various conventionally known parts, or may be subjected to various processing. The printed wiring board of this embodiment can be used as a part for fixing semiconductor elements (electronic components) such as LSIs, resistor elements, capacitors, and inductors, and connecting the semiconductor elements (electronic components) with wiring. The printed wiring board of the present invention can be produced by forming a wiring pattern on one side or both sides of the above-mentioned cured product of the prepreg or the above-mentioned metal-clad laminate using a known method such as a subtractive method, an additive method, or a semi-additive method. EXAMPLES

[0109] The present invention will be described in detail below using examples, but the present invention is not limited to the descriptions of these examples.

[0110] (Preparation of Varnish) Table 1 shows the mass % value of each component of the solid content of the thermosetting resin composition when the solid content in the examples is 100 mass %. A solvent was adjusted so that the solid content of each component shown in Table 1 was 70 mass % relative to the entire thermosetting resin composition, and a varnish was prepared using a high-speed stirrer.

[0111] [Table 1]

[0112] The information on the raw material ingredients in Table 1 is shown below. (resin) Resin 1: Biphenyl aralkyl maleimide resin (Nippon Kayaku Co., Ltd., MIR-3000-70MT) Resin 2: Polyphenylene ether resin with methacrylate groups at both ends (SABIC Japan, SA9000) Resin 3: Coumarone-indene resin (manufactured by Nippon Paint Chemical Co., Ltd., Escutron V120S) Resin 4: Styrene butadiene rubber (Gray Valley, Ricon 100) (Crosslinking agent) Crosslinking agent 1: Triallyl isocyanurate (Mitsubishi Chemical Corporation, TAIC) (Coupling Agent) Coupling agent 1: Allyl isocyanurate-based silane coupling agent (Shin-Etsu Chemical Co., Ltd., X-12-1290) (Leveling agent) Leveling agent 1: Polyacrylate compound (BYK-Chemie, BYK-361N) (Radical initiator) Radical initiator 1: α,α'-di(t-butylperoxy)diisopropylbenzene (Perbutyl P, manufactured by NOF Corporation) (Inorganic filler) Filler 1: Silica particles (Admatechs, SC4050-KNT, average particle size: 1 μm)

[0113] (Preparation of prepregs) A prepreg was obtained by impregnating a fiber substrate with the above-mentioned varnish and drying for 2 minutes at 150° C. As the fiber substrate in each example, a glass cloth shown in Table 2 was used.

[0114] [Table 2]

[0115] (measurement) The prepreg in each example was subjected to the following measurements. The measurement results are shown in Table 3.

[0116] (Difference in relative dielectric constant / dielectric tangent) The prepregs obtained in each example were heated and cured at 225°C for 2 hours. The resin compositions were then subjected to measurement of their dielectric constants at 10 GHz and dielectric loss tangents at 10 GHz using a cylindrical cavity resonator method. The difference between the dielectric constant of the glass cloth and that of the resin compositions was calculated.

[0117] (Percentage of area not containing glass cloth) For the prepregs obtained in each of the Examples, the proportion of the area not containing the glass cloth was measured by the following procedure 1. (Step 1) (1) Using a microscope (Olympus: DSX-500), an image of the prepreg from the out-of-plane direction is obtained. (2) The image obtained in (1) above is binarized. The threshold color is set to black and white, and anything below 30 out of 256 gradations is set to black. (3) The ratio of the black areas after binarization is the ratio of the area that does not contain glass cloth.

[0118] (Z 0MD (t), Z 0TD (t), Z 045° (t) Step 2 below to 0MD (t), Z1, Z in step 3 0TD (t), Z2, Z in step 4 045° (t), Z3 was measured.0MD (t), Z 0TD (t), and Z 045° Table 3 shows the maximum and minimum values ​​in the time domain corresponding to the region where the microstrip line is formed (t), as well as the values ​​of Z1, Z2, and Z3. (Step 2) 1. 18μm copper foil is placed on both sides of the 70μm thick prepreg, and then heated and cured for 2 hours at a temperature of 225℃ and a load of 3MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in any MD direction. 4. For each microstrip line formed in the MD direction, the characteristic impedance Z is measured using a network analyzer, and a microstrip line with a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines with a Z value in the range of 50Ω to 60Ω, the microstrip line with the smallest Z value is selected. The characteristic impedance of the selected microstrip line is then designated as Z1. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 0MD Measure (t). (Step 3) 1. 18μm copper foil is placed on both sides of the 70μm thick prepreg, and then heated and cured for 2 hours at a temperature of 225℃ and a load of 3MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in the TD direction perpendicular to the MD direction. 4. For each microstrip line formed in the TD direction, the characteristic impedance Z is measured using a network analyzer, and a microstrip line with a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines with a Z value in the range of 50Ω to 60Ω, the microstrip line with the smallest Z value is selected. The characteristic impedance of the selected microstrip line is designated as Z2. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 0TD Measure (t). (Step 4) 1. 18μm copper foil is placed on both sides of the 70μm thick prepreg, and then heated and cured for 2 hours at a temperature of 225℃ and a load of 3MPa to obtain a copper-clad laminate. 2. A circuit is formed on the copper-clad laminate by etching. 3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in a direction at 45° to the MD direction. 4. For each microstrip line formed at 45° to the MD direction, measure the characteristic impedance Z using a network analyzer, and select a microstrip line whose Z value is in the range of 50Ω to 60Ω. If there are multiple microstrip lines whose Z value is in the range of 50Ω to 60Ω, select the microstrip line whose Z value is the smallest. Then, the characteristic impedance of the selected microstrip line is designated as Z3. 5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line over time. Z 045° Measure (t).

[0119] The measurement results of step 2-4 above will be described with reference to FIG. 2. 0MD (t), Z 0TD (t), and Z 045° FIG. 2(a) is a graph showing the measurement results of Z 0MD (t), and Fig. 2(b) shows the measurement results for Z 0TD (t), and Fig. 2(c) shows the measurement results for Z 045° The measurement results for (t) are shown in Table 3. In each graph, the area enclosed by the dashed line is the time domain corresponding to the area where the microstrip line is formed. In other words, the characteristic impedance in this time domain is the characteristic impedance in the microstrip line plane. This time domain can be calculated by performing an inverse Fourier transform on the measurement results of the network analyzer. 0MD (t), Z 0TD (t), and Z 045° The maximum and minimum values ​​of (t) are the maximum and minimum values ​​within the regions enclosed by dashed lines in each graph shown in FIG.

[0120] [Table 3]

[0121] (evaluation) The prepregs of each Example were evaluated for signal noise when used as printed circuit boards, and it was confirmed that signal noise was suppressed in all Examples. [Explanation of symbols]

[0122] 110 Warp 120 Weft 130 Area without fiber substrate

Claims

1. A prepreg for printed circuit boards comprising a fiber base material and a thermosetting resin composition, In a cured product of the prepreg for printed circuit boards, a difference between a relative dielectric constant of the fiber base material at 10 GHz and a relative dielectric constant of the thermosetting resin composition at 10 GHz is 2.5 or less, The dielectric loss tangent of the cured body of the prepreg for printed circuit boards at 10 GHz is 0.0005 or more and 0.005 or less, A prepreg for printed circuit boards, in which the proportion of an area not containing a fiber base material in the prepreg for printed circuit boards is 30% or less, as measured by the following procedure 1. (Step 1) (1) Using a microscope, an image of the prepreg from an out-of-plane direction is obtained. (2) The image obtained in (1) above is binarized. The threshold color is set to black and white, and 30 out of 256 gradations is set as the threshold, and anything below that is set to black. (3) The proportion of black areas after binarization is regarded as the proportion of areas that do not contain a fiber base material.

2. Z, which is measured in the following procedure 2 0MD (t) satisfies the following condition 1: The prepreg for printed circuit boards according to claim 1 . (Step 2) 1. 18 μm copper foil is placed on both sides of the prepreg having a thickness of 50 μm to 100 μm, and cured by heating at a temperature of 200° C. to 250° C. and a load of 3 MPa for a period of 2 to 3 hours to obtain a copper-clad laminate.

2. A circuit is formed on the copper-clad laminate by etching.

3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in any MD direction.

4. The characteristic impedance Z of each microstrip line formed in the MD direction is measured by a network analyzer, and a microstrip line having a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines having a Z value in the range of 50Ω to 60Ω, the microstrip line with the smallest Z value is selected. Then, the characteristic impedance Z of the selected microstrip line is calculated. 1 Let us assume that.

5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line per time. Z 0MD (t) is measured. (Condition 1) In the time domain corresponding to the region where the microstrip line is formed, Z 0MD (t) is (Z 1 -5) Ω or more (Z 1 +5) Ω or less.

3. Z, which is measured in the following procedure 3. 0TD (t) satisfies the following condition 2: The prepreg for printed circuit boards according to claim 2 . (Step 3) 1. 18 μm copper foil is placed on both sides of the prepreg having a thickness of 50 μm to 100 μm, and cured by heating at a temperature of 200° C. to 250° C. and a load of 3 MPa for a period of 2 to 3 hours to obtain a copper-clad laminate.

2. A circuit is formed on the copper-clad laminate by etching.

3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in the TD direction perpendicular to the MD direction.

4. The characteristic impedance Z of each microstrip line formed in the TD direction is measured by a network analyzer, and a microstrip line having a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines having a Z value in the range of 50Ω to 60Ω, the microstrip line having the smallest Z value is selected. Then, the characteristic impedance Z of the selected microstrip line is calculated. 2 Let us assume that.

5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line per time. Z 0TD (t) is measured. (Condition 2) In the time domain corresponding to the region where the microstrip line is formed, Z 0TD (t) is (Z 2 -5) Ω or more (Z 2 +5) Ω or less.

4. Z, which is measured in the following procedure 4. 045° (t) satisfies the following condition 3: The prepreg for printed circuit boards according to claim 3. (Step 4) 1. 18 μm copper foil is placed on both sides of the prepreg having a thickness of 50 μm to 100 μm, and cured by heating at a temperature of 200° C. to 250° C. and a load of 3 MPa for a period of 2 to 3 hours to obtain a copper-clad laminate.

2. A circuit is formed on the copper-clad laminate by etching.

3. On the copper-clad laminate, microstrip lines with line widths of 120 / 140 / 160 / 180 / 200 μm, heights of 18 μm and lengths of 40 mm are formed in a direction at 45° to the MD direction.

4. For each microstrip line formed at 45° to the MD direction, the characteristic impedance Z is measured by a network analyzer, and a microstrip line with a Z value in the range of 50Ω to 60Ω is selected. If there are multiple microstrip lines with a Z value in the range of 50Ω to 60Ω, the microstrip line with the smallest Z value is selected. Then, the characteristic impedance Z of the selected microstrip line is calculated. 3 Let us assume that.

5. A pulse signal with a voltage amplitude of 125 mV and a rise time of 20 ps is applied to the selected microstrip line with the internal impedance of the signal source set to 50 Ω, and a TDR analysis is performed on the reflected voltage from the microstrip line per time. Z 045° (t) is measured. (Condition 3) In the time domain corresponding to the region where the microstrip line is formed, Z 045° (t) is (Z 3 -5) Ω or more (Z 3 +5) Ω or less.

5. The thermosetting resin composition contains silica particles. The prepreg for printed circuit boards according to claim 1 or 2.

6. The silica particles are present in an amount of 45% by mass or more and 65% by mass or less based on the entire thermosetting resin composition. The prepreg for printed circuit boards according to claim 5 .

7. The thermosetting resin composition contains polyphenylene ether. The prepreg for printed circuit boards according to claim 1 or 2.

8. The thermosetting resin composition contains a bismaleimide resin. The prepreg for printed circuit boards according to claim 1 or 2.

9. The thermosetting resin composition contains styrene-butadiene rubber. The prepreg for printed circuit boards according to claim 1 or 2.

10. The thermosetting resin composition includes a crosslinking agent. The prepreg for printed circuit boards according to claim 1 or 2.

11. The crosslinking agent contains a triallyl isocyanurate ring. The prepreg for printed circuit boards according to claim 10.

12. A metal-clad laminate comprising the cured prepreg for printed circuit boards according to claim 1 or 2.

13. A printed circuit board comprising the metal-clad laminate according to claim 12.

Citation Information

Patent Citations

  • Polyphenylene ether resin composition, prepreg, metal-clad laminate and printed wiring board

    JP2016113543A

Cited By

  • Resin composition, prepreg, laminate, metal-clad laminated plate, and wiring board

    WO2025258485A1