Porous film, porous film production method, saccharified solution production method using porous film and filtration method using porous film

A porous membrane with a controlled pore size distribution and no defects is achieved by using a thermoplastic resin, solvents, and antioxidants, addressing turbidity leakage issues in existing membranes.

JP2024167047APending Publication Date: 2024-11-29ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024040134
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-03-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Porous hollow fiber membranes used for turbidity removal suffer from wide pore size distribution leading to turbidity leakage and defects, compromising their effectiveness.

Method used

A porous membrane is produced using a thermoplastic resin, a first solvent, a second solvent, and an antioxidant, with specific solvents and antioxidants selected to achieve a three-dimensional network structure, controlled pore size distribution, and defect-free composition.

Benefits of technology

The resulting membrane exhibits a sharp pore size distribution and no defects, enhancing mechanical strength and chemical resistance, effectively preventing turbidity leakage during filtration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167047000001_ABST
    Figure 2024167047000001_ABST
Patent Text Reader

Abstract

To provide a porous film having a three-dimensional network structure, pore size distribution equal to or below a certain fixed value and no defects, a porous film production method and a saccharified solution production method using the porous film.SOLUTION: In a porous film containing a thermoplastic resin a,: the porous film contains at least a first solvent, a second solvent and an antioxidant; the first solvent and the second solvent are at least one kind selected from among a sebacic acid ester, a citric acid ester, an acetyl citric acid ester, an adipic acid ester, a trimellitate ester, an oleate ester, a palmitate ester, stearate ester, a phosphate ester, a 6-30C fatty acid and an epoxidized vegetable oil; the second solvent is different from the first solvent; the antioxidant is contained by 0.05-0.5 mass%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a porous membrane, a method for producing a porous membrane, a method for producing a sugar solution using a porous membrane, and a filtration method using a porous membrane. [Background technology]

[0002] Membrane filtration using a porous membrane (also called a "porous hollow fiber membrane") for turbidity removal of a liquid to be treated, such as in the treatment of drinking water and sewage, is becoming widespread. A thermally induced phase separation method is known as a method for producing a porous membrane used in the membrane filtration method.

[0003] The thermally induced phase separation method uses a thermoplastic resin and an organic liquid. In particular, there are known methods of using a solvent that does not dissolve the thermoplastic resin at room temperature but dissolves it at high temperatures, i.e., a latent solvent (poor solvent), as the organic liquid, and a mixed solvent that uses a poor solvent and a non-solvent that does not dissolve the thermoplastic resin even at high temperatures. The latter method involves kneading a thermoplastic resin and an organic liquid at high temperature, dissolving the thermoplastic resin in the organic liquid, and then cooling to room temperature to induce phase separation. The organic liquid is then removed to produce a porous body, and has the following advantages: (a) It becomes possible to form films even with polymers such as polyethylene that do not have suitable solvents that can dissolve them at room temperature. (b) The film is formed by using a mixed solvent of a non-solvent and a poor solvent, dissolving the material at high temperatures, and then cooling and solidifying it, making it easy to obtain a film that has a three-dimensional mesh structure and has excellent chemical resistance and mechanical strength.

[0004] For example, Patent Document 1 discloses a porous hollow fiber membrane with a three-dimensional mesh structure that exhibits high chemical resistance and mechanical strength by mixing at least one non-solvent with a poor solvent, and a method for producing the same. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2017 / 155004 Summary of the Invention [Problem to be solved by the invention]

[0006] However, when the porous hollow fiber membrane described in Patent Document 1 is used for removing turbidity from a liquid to be treated, there are problems in that the wide pore size distribution causes leakage of suspended solids on the larger pore size side, or that defects cause leakage of suspended solids.

[0007] Therefore, the present invention has been made in consideration of the above circumstances, and an objective of the present invention is to provide a porous membrane having a three-dimensional mesh structure, a pore size distribution not exceeding a certain level, and being free of defects, a method for producing the porous membrane, a method for producing a sugar solution using the porous membrane, and a filtration method using the porous membrane. [Means for solving the problem]

[0008] In known techniques, a non-solvent and a poor solvent are used in a raw material containing a thermoplastic resin to produce a porous membrane having excellent chemical resistance and mechanical strength by using thermally induced phase separation. However, the present inventors have conducted extensive research and have come to invent a porous membrane having a pore size distribution below a certain level and free of defects by adding an antioxidant in addition to a non-solvent and a poor solvent (or a good solvent), a method for producing the same, a method for producing a sugar solution using the porous membrane, and a filtration method using the porous membrane.

[0009] That is, the present invention provides the following inventions.

[0010] [1] A porous membrane comprising a thermoplastic resin, the porous membrane comprises at least a first solvent, a second solvent, and an antioxidant; the first solvent is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; the second solvent is different from the first solvent and is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; A porous film, comprising the antioxidant in an amount of 0.05% by mass or more and 0.5% by mass or less.

[0011] [2] The porous membrane according to [1], wherein the antioxidant is a hindered phenol-based antioxidant.

[0012] [3] When the pore size distribution (P) of the porous membrane is expressed as pore size distribution (P) = (maximum pore size) / (average pore size), P≦2.4 (1) The porous membrane according to [1] or [2],

[0013] [4] The porous membrane according to any one of [1] to [3], wherein the average pore size of the porous membrane is 0.1 μm or more.

[0014] [5] The thickness of the porous membrane is 0.1 mm or more and 0.7 mm or less; The porous membrane according to any one of [1] to [4], characterized in that it has a burst strength of 0.5 MPa or more.

[0015] [6] The porous membrane according to any one of [1] to [5], wherein one surface of the porous membrane has a porosity of 20% or more.

[0016] [7] The porous membrane according to any one of [1] to [6], characterized in that the porous membrane is in the form of a hollow fiber, and the thermoplastic resin is a vinylidene fluoride resin.

[0017] [8] The porous membrane according to any one of [1] to [7], characterized in that it has a single layer structure.

[0018] [9] A method for producing a porous membrane comprising a thermoplastic resin, at least a first solvent, and a second solvent, comprising: the first solvent is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; the second solvent is different from the first solvent and is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; A method for producing a porous membrane, comprising mixing an antioxidant in addition to the thermoplastic resin, at least a first solvent, and a second solvent.

[0019]

[10] The method for producing a porous membrane according to [9], wherein the antioxidant is used for adjusting pore size and pore size distribution.

[0020]

[11] When the pore size distribution (Pa) of the porous membrane without using an antioxidant is expressed as Pa = (maximum pore size of the porous membrane without using an antioxidant) / (average pore size of the porous membrane without using an antioxidant), and the pore size distribution (Pb) of the porous membrane with using an antioxidant is expressed as Pb = (maximum pore size of the porous membrane with using an antioxidant) / (average pore size of the porous membrane with using an antioxidant), Pb / Pa≦0.95 (2) The method for producing a porous membrane according to [9] or

[10] ,

[0021]

[12] The antioxidant in the porous membrane is 0.01≦(remaining amount of antioxidant) / (mixed amount of antioxidant)≦0.5 The method for producing a porous membrane according to any one of [9] to

[11] , wherein the above satisfies the above condition.

[0022]

[13] The method for producing a porous membrane according to any one of [9] to

[12] , wherein the antioxidant is mixed in an amount of 0.5 mass % or more and 3.0 mass % or less.

[0023]

[14] The method for producing a porous membrane according to any one of [9] to

[13] , wherein the antioxidant is a hindered phenol-based antioxidant.

[0024]

[15] A method for producing a porous membrane according to any one of [9] to

[14] , characterized in that a mixture containing the thermoplastic resin, the first solvent, the second solvent, and the antioxidant, or a mixture containing the thermoplastic resin, the first solvent, the second solvent, the antioxidant, and an inorganic substance is melt-kneaded and extruded, and then the first solvent, the second solvent, the antioxidant, and, if contained, the inorganic substance are extracted from the porous membrane.

[0025]

[16] After extracting the first solvent, the second solvent, the antioxidant, and, if included, the inorganic matter from the porous membrane, The method for producing a porous membrane according to

[15] , characterized in that the mixture is dried or heat-treated at 160°C or less.

[0026]

[17] A method for producing a sugar solution, comprising: A liquefaction step in which an enzyme is added to the starch liquor to partially decompose the starch and obtain a sugar-containing liquefied product; a saccharification step of adding a saccharification enzyme to the obtained sugar-containing liquefied product to further decompose sugars and obtain a saccharified solution composition containing a saccharified solution and an insoluble component; a filtering step of passing the sugared solution composition through a porous membrane made of a resin having a three-dimensional network structure to separate the sugared solution from the insoluble components; and a washing step of passing or immersing the porous membrane in a washing solution to wash and remove insoluble matters adhering to the surface or inside of the porous membrane; wherein in the filtering step, filtering is performed using the porous membrane according to any one of [1] to [8].

[0027]

[18] A filtration method, comprising filtering using the porous membrane according to any one of [1] to [8]. Effect of the Invention

[0028] The present invention provides a defect-free porous membrane having a three-dimensional mesh structure and a pore size distribution (=maximum pore size / average pore size) not greater than a certain level, a method for producing the porous membrane, a method for producing a sugar solution using the porous membrane, and a filtration method using the porous membrane. [Brief description of the drawings]

[0029] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of the three-dimensional network structure of a porous membrane of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of an example of an apparatus for producing a porous membrane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] An embodiment of the present invention will be described in detail below. Note that the present invention is not limited to the following embodiment.

[0031] As used herein, the term "defect" refers to the presence of pores that deviate from the maximum pore size of the porous membrane.

[0032] <Porous membrane> The porous membrane of the present invention is described below. The porous membrane (preferably a porous hollow fiber membrane) preferably has a three-dimensional mesh structure. In this specification, the three-dimensional mesh structure refers to a structure as shown in FIG. 1. For example, thermoplastic resin a is bonded to form a mesh, and voids b are formed. In the three-dimensional mesh structure, so-called spherulite structure resin aggregates are hardly seen. It is preferable that the voids b of the three-dimensional mesh structure are surrounded by the thermoplastic resin a, and each part of the voids b is connected to each other. Since most of the thermoplastic resins used form a three-dimensional mesh structure that can contribute to the strength of the porous membrane (preferably a hollow fiber membrane), it is possible to form a support layer with high strength. In addition, chemical resistance is also improved. The reason for the improvement in chemical resistance is not clear, but it is thought that this is because there is a large amount of thermoplastic resin that forms a mesh that can contribute to strength, so even if a part of the mesh is corroded by a chemical, the strength of the layer as a whole is not significantly affected. In addition, it also becomes more resistant to alkalies (such as aqueous sodium hydroxide solutions) that are often used as cleaning agents for membranes.

[0033] The porous membrane contains a thermoplastic resin, and examples of the thermoplastic resin include polyolefin, copolymer of olefin and halogenated olefin, halogenated polyolefin, or a mixture thereof. Examples of the thermoplastic resin include polyethylene, polypropylene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, ethylene-tetrafluoroethylene copolymer, polyvinylidene fluoride (which may contain a domain of hexafluoropropylene), or a mixture thereof. These materials are excellent as membrane materials because they are thermoplastic and therefore easy to handle and strong. Among these, homopolymers and copolymers of vinylidene fluoride, ethylene, tetrafluoroethylene, and chlorotrifluoroethylene, as well as mixtures of the homopolymers and copolymers, are preferred because they have excellent mechanical strength, chemical strength (chemical resistance), and good moldability. More specifically, fluororesins such as polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer, and ethylene-chlorotrifluoroethylene copolymer can be mentioned. In this specification, the homopolymer and copolymer of vinylidene fluoride such as the polyvinylidene fluoride, and resins containing mixtures thereof are referred to as vinylidene fluoride resins. The thermoplastic resin of the present invention is particularly preferably a vinylidene fluoride resin.

[0034] The porous film may contain up to about 5% by mass of components (impurities, etc.) other than the thermoplastic resin. For example, the porous film contains a solvent and an antioxidant used during production. As described below, the porous film contains a first solvent (hereinafter also referred to as a non-solvent) used as a solvent during production, a second solvent (hereinafter also referred to as a good solvent or poor solvent), and / or an antioxidant. These components can be detected by pyrolysis GC-MS (gas chromatography-mass spectrometry) or LC-MS (liquid chromatography-mass spectrometry).

[0035] The porous membrane of the present invention will be described. The porous membrane contains a thermoplastic resin, a first solvent, a second solvent, and an antioxidant. That is, the porous membrane contains a thermoplastic resin, the porous membrane comprises at least a first solvent, a second solvent, and an antioxidant; the first solvent is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; the second solvent is different from the first solvent and is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; The porous film contains 0.05% by mass or more and 0.5% by mass or less of an antioxidant. The porous membrane contains a predetermined amount of an antioxidant, and thus has a three-dimensional network structure and a pore size distribution not exceeding a certain level, in addition to mechanical strength.

[0036] The porous membrane has a three-dimensional network structure, which increases the tensile elongation at break and enhances resistance to alkalis (such as aqueous sodium hydroxide solutions) that are often used as cleaning agents for membranes.

[0037] The porous membrane may further contain an inorganic substance, which is preferably at least one selected from the group consisting of silica, lithium chloride, and titanium oxide.

[0038] The porous membrane has a pore size distribution below a certain level. When the porous membrane has a pore size distribution below a certain level, leakage of suspended solids can be suppressed.

[0039] The porous membrane is a porous membrane having no significant defects from the outer and inner surface parts to the thick part. The absence of defects in the porous membrane makes it possible to suppress leakage of suspended solids.

[0040] Here, examples of the fatty acid having 6 to 30 carbon atoms include capric acid, lauric acid, oleic acid, etc. Examples of the epoxidized vegetable oil include epoxidized soybean oil, epoxidized linseed oil, etc.

[0041] It is preferable that the first solvent is a non-solvent in which the thermoplastic resin does not dissolve uniformly in the first solvent when the temperature of the first mixed liquid is raised to the boiling point of the first solvent in a first mixed liquid having a ratio of thermoplastic resin to first solvent of 20:80.

[0042] The second solvent is preferably a good solvent in which the thermoplastic resin dissolves uniformly in the second solvent when the temperature of the second mixed liquid is higher than 25°C and lower than the boiling point of the second solvent in a second mixed liquid having a ratio of thermoplastic resin to second solvent of 20:80. Here, "the thermoplastic resin is uniformly dissolved in the second solvent" means that the solution is not visually separated into two layers and is transparent.

[0043] It is more preferable that the second solvent is a poor solvent in which, in a second mixed liquid having a ratio of thermoplastic resin to second solvent of 20:80, the thermoplastic resin does not dissolve uniformly in the second solvent when the temperature of the second mixed liquid is 25°C, but the thermoplastic resin dissolves uniformly in the second solvent when the temperature of the second mixed liquid is any temperature higher than 100°C and lower than the boiling point of the second solvent.

[0044] The antioxidant is selected from Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1098, Irganox 1135, Irganox 1141, Irganox 1330, Irganox 1425WL, Irganox 1520L, Irganox 245, Irganox 259, Irganox 3114, Irganox 565, Irgafos 168, Irganox PS800FL, Irganox PS802FL, Irgastab FS042 and dibutylhydroxytoluene. Among the antioxidants, the hindered phenol-based antioxidant is preferred.

[0045] The antioxidant is contained in the porous film in an amount of 0.05% by mass to 0.5% by mass. When the antioxidant is contained in the porous film in an amount of 0.05% by mass to 0.5% by mass, the porous film has a pore size distribution below a certain level. From the same viewpoint, the antioxidant is preferably contained in the porous film in an amount of 0.1% by mass to 0.4% by mass, more preferably in an amount of 0.2% by mass to 0.3% by mass.

[0046] (Properties of porous membrane) The thickness (membrane thickness) of the porous membrane is preferably 0.1 mm to 1.0 mm, more preferably 0.1 mm to 0.7 mm, and even more preferably 0.2 mm to 0.7 mm. A thickness of 0.1 mm or more increases the strength, while a thickness of 1 mm or less reduces the pressure loss due to membrane resistance.

[0047] The pore size of the porous membrane is preferably 0.1 μm or more in average pore size. Also, it is suitable to be 0.1 μm or more and 5.0 μm or less. More preferably, the average pore size is 0.1 μm or more and 1.0 μm or less, and even more preferably, 0.1 μm or more and 0.7 μm or less. When the average pore size is 0.1 μm or more, the decrease in the filtration flow rate is small, which is preferable. When the average pore size is 5.0 μm or less, effective filtration separation of turbid matter is possible, and the turbid matter is less likely to clog the inside of the membrane, which is preferable because the decrease in the filtration amount over time is small. The average pore size of a porous membrane can be determined according to the method described in ASTM: F316-86 (also known as the half-dry method). The average pore size determined by this half-dry method is the average pore size of the smallest pore size layer of the membrane. The standard measurement conditions for measuring the average pore size by the half-dry method are ethanol as the liquid used, 25°C, and a pressure rise rate of 0.001 MPa / sec. The average pore size [μm] is calculated by the following formula. Average pore size [μm] = (2860 × surface tension [mN / m]) / half-dry air pressure [Pa]

[0048] The maximum pore size of the porous membrane is preferably 0.30 μm or more, since the decrease in the filtration flow rate is small, and more preferably 0.4 μm or more. The maximum pore size of the porous membrane is preferably 2.0 μm or less, and more preferably 1.5 μm or less, since effective filtration separation of turbid matters is possible, and the turbid matters are less likely to clog the inside of the membrane, and the decrease in the filtration rate over time is small. The maximum pore size of a porous membrane can be calculated from the pressure when air bubbles first emerge from the membrane in the half-dry method (bubble point method). In the case of the above-mentioned standard measurement conditions for the half-dry method, the pressure when air bubbles first emerge from the porous membrane (air pressure generating air pressure) is calculated as follows: Maximum pore size [μm] = 62834.2 / (air pressure at which air bubbles are generated [Pa]) More can be asked for.

[0049] The porosity of one surface of the porous membrane is preferably 20% or more. It is presumed that when the porosity of the porous membrane is high, the load of membrane fouling per hole is small and the number of holes completely blocked is small, so that high filtration performance can be exhibited. In addition, in the extraction removal process of the solvent, inorganic matter, and antioxidant in the manufacturing process of the porous membrane, a porous membrane with a high porosity can leave the antioxidant uniformly in the cross-sectional direction. Preferably, the porosity of one surface of the porous membrane is more preferably 25% or more, and even more preferably 30% or more. Here, the one surface of the porous membrane is preferably the surface on the side of the liquid to be filtered, and in the case of internal pressure filtration, it is preferably the surface on the inner surface side. In addition, the porosity of one surface of the porous membrane may be 60% or less from the viewpoint of the strength of the porous membrane. The porosity of one surface of the porous membrane can be determined by photographing the surface of the porous membrane using a Hitachi SU8000 series electron microscope, for example, by the method described in WO 2001 / 53213.

[0050] The porous membrane is preferably a single-layer structure. The single-layer structure means that the layer is composed of a single composition, and does not mean that the porous membrane of the substrate is laminated with a layer of a composition different from the substrate, or that the porous membrane is laminated with a plurality of layers by co-extrusion. The porous membrane can be judged to be a single-layer structure by visually observing the presence or absence of the interface between layers by observation means such as an electron microscope. When the porous membrane is a single-layer structure, the decomposition suppression effect of the antioxidant can be uniformly expressed on the cross section of the membrane, and the pore size distribution can be easily adjusted.

[0051] The tensile breaking strength of the porous membrane is preferably 2 MPa or more in order to ensure practical durability, and more preferably 4 MPa or more. The tensile breaking strength of the porous membrane is measured and calculated under the following conditions. Measuring equipment: Instron type tensile testing machine (Shimadzu Corporation, product name: AGS-5D) Chuck distance: 5cm Pulling speed: 20cm / min Measurement temperature: 25℃ Tensile breaking strength [Pa] = breaking load [N] / membrane cross-sectional area [m 2 ] (where, the membrane cross-sectional area [m 2 ]=π×[(Outer diameter [m] / 2) 2 -(Inner diameter [m] / 2) 2 ].)

[0052] The tensile breaking elongation of the porous membrane is preferably 60% or more in order to ensure practical durability, more preferably 80% or more, further preferably 100% or more, and particularly preferably 120% or more. The tensile elongation at break of the porous membrane is measured and calculated under the following conditions. Measuring equipment: Instron type tensile testing machine (Shimadzu Corporation, product name: AGS-5D) Chuck distance: 5cm Pulling speed: 20cm / min Measurement temperature: 25℃ Tensile elongation at break [%] = 100 × displacement at break [mm] / 50 [mm]

[0053] The rupture strength of the porous membrane is preferably 0.3 MPa or more, more preferably 0.5 MPa or more from the viewpoint of the resistance to rupture during internal pressure filtration and the membrane permeability, and is preferably 15 MPa or less, more preferably 10 MPa or less from the viewpoint of the membrane permeability. The burst strength of the porous membrane is measured using a pressure tester (manufactured by Hara Engineering Co., Ltd.).

[0054] The pure water permeability of the porous membrane is 500 L / (m 2 ·hr) or more 40000L / (m 2 ·hr), and more preferably 1000 L / (m 2 hr) or more.

[0055] The pore size distribution (P) of the porous membrane is the maximum pore size divided by the average pore size, and is expressed as pore size distribution (P) = (maximum pore size) / (average pore size). From the viewpoint of removing all turbidity from the liquid to be treated, the pore size distribution is preferably 2.4 or less, more preferably 2.1 or less. From the viewpoint of membrane permeability, the pore size distribution is preferably 1.0 or more, more preferably 1.3 or more.

[0056] In this specification, the pore size distribution of the porous membrane when no antioxidant is used is represented as Pa, and the pore size distribution of the porous membrane when an antioxidant is used is represented as Pb. Therefore, Pa and Pb are represented as Pa=(maximum pore size of the porous membrane when no antioxidant is used) / (average pore size of the porous membrane when no antioxidant is used), and the pore size distribution of the porous membrane when an antioxidant is used (Pb) is represented as Pb=(maximum pore size of the porous membrane when an antioxidant is used) / (average pore size of the porous membrane when an antioxidant is used). In addition, the ratio of the pore size distribution of the porous membrane when no antioxidant is used to the pore size distribution of the porous membrane when an antioxidant is used is represented as Pb / Pa. The pore size distribution becomes narrower when an antioxidant is used due to the effect of the antioxidant in suppressing the decomposition of the first and second solvents. Therefore, it is preferable that Pb / Pa≦1.0, and more preferably Pb / Pa≦0.95. From the viewpoint of membrane permeability, it is preferable that 0.3≦Pb / Pa, and more preferably 0.5≦Pb / Pa.

[0057] The ratio of the remaining amount of antioxidant to the mixed amount of antioxidant is the value obtained by dividing the concentration of antioxidant contained in the porous membrane by the concentration of antioxidant mixed, and is expressed as (remaining amount of antioxidant) / (mixed amount of antioxidant). In order to narrow the pore size distribution, the antioxidant in the porous membrane preferably satisfies 0.01≦(remaining amount of antioxidant) / (mixed amount of antioxidant)≦0.5, and more preferably satisfies 0.1≦(remaining amount of antioxidant) / (mixed amount of antioxidant)≦0.3.

[0058] (Liquid to be treated) The liquids to be treated by the porous membrane are suspended water and process liquids. The porous membrane is preferably used in a water purification method including a step of filtering suspended water.

[0059] The above-mentioned suspended water includes natural water, domestic wastewater, and treated water thereof. Examples of natural water include river water, lake water, groundwater, and seawater. Treated water of natural water that has been treated with sedimentation, sand filtration, coagulation-sedimentation sand filtration, ozone treatment, activated carbon treatment, and other treatments is also included in the suspended water to be treated. An example of domestic wastewater is sewage. Primary sewage treatment water that has been treated with screen filtration or sedimentation, secondary sewage treatment water that has been treated with biological treatment, and tertiary treatment (advanced treatment) water that has been treated with coagulation-sedimentation sand filtration, activated carbon treatment, and ozone treatment are also included in the suspended water to be treated. These suspended waters include turbid matter (humus colloids, organic colloids, clay, bacteria, etc.) consisting of fine organic matter, inorganic matter, and organic-inorganic mixtures on the order of μm or less.

[0060] The water quality of the above-mentioned suspended solids (such as the above-mentioned natural water, domestic wastewater, and treated water thereof) can generally be expressed by a single or a combination of turbidity and organic matter concentration, which are representative water quality indicators. When water quality is classified by turbidity (average turbidity, not instantaneous turbidity), it can be roughly classified into low turbidity water with a turbidity of less than 1, medium turbidity water with a turbidity of 1 to less than 10, high turbidity water with a turbidity of 10 to less than 50, and ultra-high turbidity water with a turbidity of 50 or more. When water quality is classified by organic matter concentration (total organic carbon concentration (TOC): mg / L) (also an average value, not an instantaneous value), it can be roughly classified into low TOC water with a turbidity of less than 1, medium TOC water with a turbidity of 1 to less than 4, high TOC water with a turbidity of 4 to less than 8, and ultra-high TOC water with a turbidity of 8 or more. Basically, the higher the turbidity or TOC of water, the more likely it is that the filtration membrane will be clogged, so the effect of using a porous membrane is greater for water with a higher turbidity or TOC.

[0061] The process liquid refers to a liquid to be separated when valuable and non-valuable materials are separated in food, pharmaceutical, and semiconductor manufacturing. In food manufacturing, for example, porous membranes are used when separating alcoholic beverages such as sake and wine from yeast. In pharmaceutical manufacturing, for example, porous membranes are used for sterilization during protein purification. In semiconductor manufacturing, for example, porous membranes are used for separating polishing agent and water from polishing wastewater.

[0062] <Method of manufacturing porous membrane> Next, a method for producing the porous membrane will be described.

[0063] The method for producing a porous membrane of the present invention is a method for producing a porous membrane comprising a thermoplastic resin, at least a first solvent, and a second solvent, the first solvent is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; the second solvent is different from the first solvent and is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; The method for producing a porous membrane is characterized in that an antioxidant is further mixed in addition to the thermoplastic resin, at least the first solvent, and the second solvent. The above production method makes it possible to produce a porous membrane having a three-dimensional network structure, a pore size distribution not exceeding a certain level, and no defects.

[0064] The method for producing a porous membrane includes the steps of (a) preparing a molten mixture, (b) supplying the molten mixture to a multi-layered spinning nozzle and extruding the molten mixture from the spinning nozzle to obtain a porous membrane, and (c) extracting the solvent and antioxidant (as well as additives) from the porous membrane.

[0065] The molten mixture is a mixture containing a thermoplastic resin such as polyvinylidene fluoride, a first solvent, a second solvent, and an antioxidant, or a mixture containing a thermoplastic resin such as polyvinylidene fluoride, a first solvent, a second solvent, an antioxidant, and an inorganic substance.

[0066] The mixture containing the thermoplastic resin such as polyvinylidene fluoride, a first solvent, a second solvent, and an antioxidant, or the mixture containing the thermoplastic resin such as polyvinylidene fluoride, a first solvent, a second solvent, an antioxidant, and an inorganic substance can be obtained by mixing using a Henschel mixer, a Banbury mixer, a Plosser mixer, or the like.

[0067] In terms of the order of mixing a thermoplastic resin such as polyvinylidene fluoride, a first solvent, a second solvent, an antioxidant, and an inorganic substance, it is more advantageous to mix the inorganic substance, the first solvent, and the second solvent first to allow the inorganic substance to fully adsorb the first solvent and the second solvent, and then mix the thermoplastic resin such as polyvinylidene fluoride, rather than mixing the five components simultaneously, in terms of improving the melt moldability and the porosity and mechanical strength of the resulting porous film. It is preferable to add the antioxidant after mixing the thermoplastic resin, the first solvent, and the second solvent, or after mixing the thermoplastic resin, the first solvent, the second solvent, and the inorganic substance, and further stir and mix. Although the reason is unclear, adding the antioxidant after mixing various raw materials increases the viscosity more than mixing only the first solvent and the second solvent, so that it is possible to suppress the formation of aggregates or lumps, and it is possible to mix more uniformly when adding it. Therefore, the effect of suppressing the decomposition of the organic liquid is increased. Furthermore, when the antioxidant is in powder form after mixing, it is mixed in a state close to the final particle size distribution, so that it can be mixed uniformly in the same manner, and the decomposition suppression effect is increased.

[0068] Alternatively, the thermoplastic resin such as polyvinylidene fluoride, the first solvent, the second solvent, and the antioxidant may be separately supplied directly to a melt kneading extrusion device such as a twin-screw extruder without pre-kneading with a Henschel mixer, etc. In order to improve kneading properties, the mixture may be melt-kneaded once after mixing to form pellets, and the pellets may be supplied to a melt kneading extrusion device, extruded into hollow fibers, and cooled and solidified to form hollow fibers.

[0069] The mixture can be melt-kneaded using a normal melt-kneading means, for example, an extruder. Although the case where an extruder is used will be described below, the melt-kneading means is not limited to an extruder. An example of a production apparatus used to carry out the production method of this embodiment is shown in FIG. 2.

[0070] The porous hollow fiber membrane (porous membrane) manufacturing apparatus shown in Fig. 2 includes an extruder 10, a hollow fiber forming nozzle 20, a coagulation bath 30 in which a solution for coagulating the membrane-forming stock solution is stored, and a plurality of rollers 50 for transporting and winding up the porous hollow fiber membrane 40. The space S shown in Fig. 2 is an empty run section through which the membrane-forming stock solution discharged from the hollow fiber forming nozzle 20 passes before reaching the solution in the coagulation bath 30.

[0071] The molten mixture is extruded by the extruder 10 through a hollow fiber nozzle 20, which is attached to the tip of the extruder 10 and discharged from the hollow fiber nozzle 20. The hollow fiber-shaped molten mixture discharged from the discharge port is solidified by passing through a coolant such as air or water, and then passes through the above-mentioned free run section S consisting of an air layer due to the intended porous hollow fiber membrane, and then passes through the coagulation bath 30 containing water or the like. In other words, the free run section S is the portion from the discharge port of the hollow fiber nozzle 20 to the water surface of the coagulation bath 30. A container such as a cylinder may be used for the free run section S from the discharge port as necessary. After passing through the coagulation bath 30, the hollow fiber is wound into a skein or the like as necessary.

[0072] The first and second solvents are extracted and removed using a liquid suitable for extraction that dissolves the thermoplastic resin used or is miscible with the first and second solvents without denaturing the thermoplastic resin. Specifically, the liquid can be contacted by a technique such as immersion. The liquid is preferably volatile so that it can be easily removed from the porous membrane after extraction. Examples of the liquid include alcohols and methylene chloride. If the first and second solvents are water-soluble, water can also be used as the extraction liquid.

[0073] The antioxidant is preferably extracted and removed from the porous membrane using a volatile liquid, such that it can be easily removed from the membrane after extraction. Examples of such liquids include alcohols and methylene chloride. If the antioxidant is water-soluble, water can also be used as the extraction liquid.

[0074] The extraction and removal of the inorganic substance is usually carried out using an aqueous liquid. For example, when the inorganic substance is silica, the silica is first converted to a silicate by contacting with an alkaline solution, and then the silicate is extracted and removed by contacting with water.

[0075] The first and second solvents may be extracted and removed first, and the inorganic matter may be extracted and removed first. When the first and second solvents are immiscible with water, it is preferable to extract and remove the first and second solvents first, and then extract and remove the inorganic matter. Usually, the first and second solvents and the inorganic matter are mixed and coexist in the concentrated partial phase of the first and second solvents, so that the inorganic matter can be extracted and removed smoothly, which is advantageous.

[0076] Furthermore, the extraction and removal of the first and second solvents and the extraction and removal of the inorganic substances can be carried out simultaneously if they can be extracted and removed with the same solvent. Usually, they are extracted and removed separately.

[0077] In the above extraction removal, the first solvent, the second solvent, and the antioxidant (and additives, if included) are not completely extracted from the film, but a certain amount remains in the film. When the first solvent, the second solvent, and the antioxidant are extracted and removed in the presence of inorganic matter, it is considered that the antioxidant is partially inhibited from being extracted and can remain in the film. To determine residual solvent, one porous membrane cut to approximately 74 mg is placed in a 50 mL vial, to which 15.5 mL of 50% aqueous ethanol solution is added (bath ratio: 0.211 mL / mg), and heated to 40°C. After 24 hours, all of this extract is removed and subjected to GC / MS measurement under the following conditions. The detection limit is estimated by defining S / N=3 from the peak of a standard solution of known concentration, and results obtained from this measurement above the detection limit are evaluated as "residual," and results below the detection limit are evaluated as "no residual." GC device: Agilent7890 Column: DB-5MS (30 m, 0.25 mm diameter, film thickness 1.0 μm) Column temperature: 40°C (5 min) - 20°C / min heating - 320°C (11 min) Flow rate: 1mL / min Inlet temperature: 320℃ Split:Splitless Injection volume: 1μL MS instrument: Agilent MSD5977B HES Interface: 300℃ Ionization: EI 70eV Measurement method: SCAN method Ion source temperature: 230℃

[0078] The concentration of the thermoplastic resin in the melt-kneaded product is preferably 20 to 60% by mass, more preferably 25 to 45% by mass, and even more preferably 30 to 45% by mass. When this value is 20% by mass or more, the mechanical strength can be increased, while when it is 60% by mass or less, the water permeability can be increased. The melt-kneaded product may contain an additive.

[0079] As described above, the melt-kneaded product may contain four components, namely, a thermoplastic resin, a first solvent, a second solvent, and an antioxidant, or may contain five components, namely, a thermoplastic resin, a first solvent, a second solvent, an antioxidant, and an additive. The solvent includes at least a non-solvent, as described later.

[0080] As the extractant used in the step (c), it is preferable to use a liquid such as methylene chloride or various alcohols which does not dissolve the thermoplastic resin but has high affinity with the solvent and the antioxidant.

[0081] When a melt-kneaded product containing no additives is used, the hollow fiber membrane obtained through step (c) may be used as the porous membrane. When a melt-kneaded product containing additives is used to produce a porous membrane, the production method according to this embodiment preferably further comprises, after step (c), a step (d) of extracting and removing the additives from the hollow fiber membrane to obtain a porous membrane. As the extractant in step (d), it is preferable to use a liquid such as an inorganic acid, such as hydrochloric acid or sulfuric acid, or an inorganic alkali, such as caustic soda, which can dissolve the additives used but not the thermoplastic resin.

[0082] As described above, an inorganic substance may be used as the additive. The inorganic substance is preferably an inorganic fine powder. Examples of the inorganic fine powder include silica, alumina, titanium oxide, zirconium oxide, calcium carbonate, etc., and among these, silica is preferred.

[0083] The inorganic fine powder preferably has an average primary particle size of 3 nm to 500 nm, more preferably 5 nm to 100 nm, and particularly preferably fine silica having an average primary particle size of 3 nm to 500 nm.

[0084] The finely powdered silica is preferably a hydrophobic finely powdered silica that is less likely to aggregate and has good dispersibility, and more preferably a hydrophobic finely powdered silica having a MW (methanol wettability) value of 30% by volume or more. The MW value here refers to the volume % of methanol that completely wets the powder. Specifically, silica is placed in pure water, and methanol is added below the liquid surface while stirring. The MW value is determined by calculating the volume % of methanol in the aqueous solution when 50% by mass of the silica has settled.

[0085] The above-mentioned "primary particle size of inorganic fine powder" means a value obtained by analyzing an electron microscope photograph. That is, a group of inorganic fine powders is first pretreated by the method of ASTM D3849. Then, the particle diameters of 3,000 to 5,000 particles captured in a transmission electron microscope photograph are measured, and the primary particle size of the inorganic powder is calculated by arithmetically averaging these values.

[0086] The inorganic fine powder in the porous film can be analyzed by identifying the elements present using fluorescent X-rays or other methods to determine the materials present.

[0087] When using organic substances as additives, hydrophilic polymers such as polyvinylpyrrolidone and polyethylene glycol can be used to impart hydrophilicity to the porous membrane. Also, the viscosity of the molten mixture can be controlled by using highly viscous additives such as glycerin and ethylene glycol.

[0088] In the method for producing the porous membrane, the speed (spinning speed) and temperature (discharge temperature) when the molten mixture is extruded from the spinning nozzle are not particularly limited, and any speed (spinning speed) and temperature (discharge temperature) can be used.

[0089] Next, the step (a) of preparing a molten mixture in the method for producing a porous membrane of the present invention will be described in detail. In the method for producing a porous membrane of the present invention, a non-solvent for a thermoplastic resin is mixed with a good solvent or a poor solvent. When a non-solvent is used as a raw material for the membrane in this way, a porous membrane with a three-dimensional network structure is obtained. Although the mechanism of action is not necessarily clear, it is considered that the crystallization of the polymer is appropriately inhibited and a three-dimensional network structure is easily formed by mixing a non-solvent and using a solvent with a lower solubility. For example, the non-solvent and the poor solvent or the good solvent are selected from various esters such as sebacic acid esters, citric acid esters, acetyl citrate esters, adipic acid esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids with 6 to 30 carbon atoms, and epoxidized vegetable oils.

[0090] Specific examples of the above esters and their boiling points are as follows: the boiling points of acetyl tributyl citrate are 343°C, dibutyl sebacate are 345°C, dibutyl adipate are 305°C, diisobutyl adipate are 293°C, bis 2-ethylhexyl adipate are 335°C, diisononyl adipate is 250°C or higher, diethyl adipate is 251°C, triethyl citrate is 294°C, and triphenyl phosphite is 360°C.

[0091] A solvent that can dissolve a thermoplastic resin at room temperature is called a good solvent. A solvent that cannot dissolve a thermoplastic resin at room temperature but can dissolve the resin at a high temperature is called a poor solvent for the thermoplastic resin. A solvent that cannot dissolve the resin even at a high temperature is called a non-solvent. In the present invention, a good solvent, a poor solvent, and a non-solvent can be determined as follows.

[0092] To determine whether a solvent is a good solvent, poor solvent, or non-solvent, specifically, put about 2g of thermoplastic resin and about 8g of solvent into a test tube, heat it to the boiling point of the solvent in 10°C increments using a test tube block heater, mix the contents of the test tube with a spatula, etc., and judge the solubility in the above temperature range. In other words, if the thermoplastic resin dissolves in the solvent, it is a good solvent or poor solvent, and if it does not dissolve in the solvent, it is a non-solvent.

[0093] For example, if polyvinylidene fluoride (PVDF) is used as the thermoplastic resin and acetyl tributyl citrate, dibutyl sebacate, or dibutyl adipate is used as the solvent, PVDF does not dissolve uniformly in these solvents at 25°C, but when the temperature of the mixture is raised, PVDF mixes uniformly and dissolves in these solvents at any temperature above 100°C and below the boiling point. On the other hand, if bis 2-ethylhexyl adipate, diisononyl adipate, bis 2-ethylhexyl sebacate, or oleic acid is used as the solvent, PVDF does not dissolve in these solvents even when the temperature is raised to the boiling point.

[0094] The good solvent (second solvent) is at least one selected from various esters such as sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitate esters, oleate esters, palmitate esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils, and in a mixed liquid (second mixed liquid) in which the ratio of thermoplastic resin to second solvent is 20:80, the thermoplastic resin dissolves uniformly in the solvent when the temperature of the second mixed liquid is any temperature higher than 25°C and lower than the boiling point of the solvent.

[0095] The poor solvent (second solvent) is such that, in the second mixed liquid, the thermoplastic resin does not dissolve uniformly in the poor solvent when the temperature of the second mixed liquid is 25°C, but the thermoplastic resin dissolves uniformly in the poor solvent when the temperature of the second mixed liquid is any temperature higher than 100°C and lower than the boiling point of the poor solvent.

[0096] The non-solvent (first solvent) is at least one selected from various esters such as sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitate esters, oleate esters, palmitate esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils, and in a mixed liquid (first mixed liquid) in which the ratio of thermoplastic resin to non-solvent (first solvent) is 20:80, even if the temperature of the first mixed liquid is raised to the boiling point of the non-solvent (first solvent), the thermoplastic resin does not dissolve uniformly in the non-solvent (first solvent).

[0097] In the method for producing the porous membrane, an antioxidant is mixed. Although not limited, the order of mixing is preferably such that a series of raw materials are added, followed by adding and mixing the antioxidant. When the amount of the antioxidant is 0.5% by mass or more, the decomposition of the first and second solvents is suppressed, and when it is 3.0% by mass or less, a porous membrane with few defects can be produced, which is preferable. In this case, when the pore size distribution of the porous membrane is expressed as P=(maximum pore size) / (average pore size), when the pore size distribution when no antioxidant is used is Pa, and the pore size distribution when the antioxidant is used is Pb, the pore size distribution becomes narrower due to the effect of the antioxidant in suppressing the decomposition of the first and second solvents, and it is preferable that Pb / Pa≦0.95.

[0098] In the method for producing the porous membrane, the antioxidant is used to suppress the decomposition of the first solvent or the second solvent, and is used for a solvent that decomposes quickly. That is, in the present invention, it is preferable to use the antioxidant for a solvent that decomposes more easily and has a maximum decomposition temperature of 280° C. or less in TG-DTA measurement.

[0099] In the method for producing the porous membrane, when the ratio of the remaining amount of antioxidant to the mixed amount of antioxidant in the porous membrane (remaining amount of antioxidant / mixed amount of antioxidant) is taken, in order to narrow the pore size distribution, it is preferable to satisfy 0.01≦(remaining amount of antioxidant) / (mixed amount of antioxidant)≦0.5, and more preferably 0.1≦(remaining amount of antioxidant) / (mixed amount of antioxidant)≦0.3.

[0100] In the method for producing a porous membrane of the present invention, an inorganic substance may be further added. The inorganic substance is preferably at least one selected from the group consisting of silica, lithium chloride, and titanium oxide.

[0101] In addition, the porous membrane after solidification can be stretched in the longitudinal direction at a stretching ratio of 3 times or less at any of the following stages: (i) before the extraction and removal of the first and second solvents and inorganic substances; (ii) after the extraction and removal of the first and second solvents and before the extraction and removal of inorganic substances; (iii) after the extraction and removal of inorganic substances and before the extraction and removal of the first and second solvents; (iv) after the extraction and removal of the first and second solvents and inorganic substances. Generally, when a porous membrane is stretched in the longitudinal direction, the water permeability is improved, but the pressure resistance (e.g., burst strength and compressive strength) is reduced, so that the membrane does not have a practical strength after stretching in many cases. However, the porous membrane (e.g., porous hollow fiber membrane) obtained by the manufacturing method of the present invention has high mechanical strength. Therefore, stretching at a stretching ratio of 1.1 times or more and 3.0 times or less is possible. The water permeability of the porous membrane (e.g., porous hollow fiber membrane) is improved by stretching. The stretch ratio here refers to the value obtained by dividing the length of the hollow fiber after stretching by the length of the hollow fiber before stretching. For example, when a porous hollow fiber membrane with a hollow fiber length of 10 cm is stretched to a length of 20 cm, the stretch ratio is 2 times according to the following formula. 20cm÷10cm=2

[0102] The stretching of the porous membrane is preferably carried out at a space temperature of 0° C. or more and 160° C. or less. If the temperature is higher than 160° C., the stretching unevenness is large and the elongation at break and the water permeability are reduced, which is not preferable, while if the temperature is lower than 0° C., the possibility of breakage during stretching is high and it is not practical. The space temperature during stretching is more preferably 10° C. or more and 140° C. or less, and even more preferably 20° C. or more and 100° C. or less.

[0103] In the present invention, it is preferable to stretch the porous membrane in a state containing the first solvent and the second solvent. The porous membrane containing the first solvent and the second solvent is less likely to break during stretching than the porous membrane not containing the first solvent and the second solvent. Furthermore, the porous membrane containing the first solvent and the second solvent can shrink the porous membrane more after stretching, so the degree of freedom in setting the shrinkage ratio after stretching is increased.

[0104] In addition, it is preferable to stretch the porous membrane in a state containing inorganic matter. The porous membrane containing inorganic matter is harder to be flattened during stretching due to the hardness of the porous membrane caused by the presence of inorganic matter contained in the porous membrane. In addition, it can prevent the pore size of the finally obtained porous membrane from being too small or the thread diameter from being too thin.

[0105] Furthermore, in the present invention, it is more preferable to stretch a porous film containing both the first solvent, the second solvent, and an inorganic substance.

[0106] For the reasons mentioned above, it is preferable to stretch the porous membrane before the extraction of the first solvent and the second solvent, or the inorganic substance, rather than stretching the porous membrane after the extraction of the first solvent and the second solvent, and it is even more preferable to stretch the porous membrane before the extraction of the first solvent and the second solvent, and the inorganic substance, rather than stretching the porous membrane before the extraction of the first solvent and the second solvent, or the inorganic substance.

[0107] In addition, the method of extracting the stretched porous membrane has the advantage that the voids on the surface and inside of the porous membrane are increased by stretching, so that the extraction solvent can easily penetrate into the inside of the porous membrane.In addition, the method of extracting after the process of stretching and then shrinking has the advantage that, as described later, the porous membrane has low tensile modulus and is easy to bend, so when extraction is performed in liquid flow, the porous membrane is easily shaken by the liquid flow, and the stirring effect is increased, so that extraction can be performed efficiently in a short time.

[0108] In the present invention, when the porous membrane is stretched and then shrunk (i.e., when the method has a step of stretching the porous membrane and then shrinking it), a porous membrane with a low tensile modulus can be finally obtained. Here, "low tensile modulus" means that the threads are easily stretched with a small force and return to their original shape when the force is removed. If the tensile modulus is low, the porous membrane is not flattened and is easily bent, and is easily swayed by the water flow during filtration. The bending of the threads is not constant and swayed according to the water flow, so that the layer of contaminants that adhere to and accumulate on the membrane surface is easily peeled off without growing, and the amount of filtrate can be maintained high. Furthermore, when the threads are forcibly swayed by flushing or air scrubbing, the shaking is large and the cleaning recovery effect is high.

[0109] Regarding the degree of yarn length shrinkage when shrinking after drawing, it is desirable to set the yarn length shrinkage ratio relative to the yarn length increment by drawing to be in the range of 0.3 to 0.9. For example, when a 10 cm yarn is drawn to 20 cm and then drawn to 14 cm, the yarn length shrinkage ratio is 0.6 according to the following formula. Yarn length shrinkage ratio = {(maximum yarn length when stretched) - (yarn length after shrinkage)} / [(maximum yarn length when stretched) - (original yarn length)] = (20 - 14) / (20 - 10) = 0.6 If the fiber length shrinkage ratio is more than 0.9, the water permeability tends to be low, and if it is less than 0.3, the tensile modulus tends to be high, which are not preferable. In the present invention, the fiber length shrinkage ratio is more preferably in the range of 0.50 to 0.85.

[0110] In addition, by adopting a process of stretching the porous membrane to the maximum thread length when stretched and then shrinking it, the finally obtained porous membrane will not break even when stretched to the maximum thread length during use. Here, when the stretching ratio is X and the yarn length shrinkage ratio relative to the yarn length increment due to stretching is Y, the ratio Z, which represents the degree of guarantee of breaking elongation, can be defined by the following formula. Z = (Maximum yarn length during stretching - yarn length after shrinkage) / yarn length after shrinkage = (XY-Y) / (X+Y-XY)

[0111] The ratio Z, which indicates the degree of the guarantee of the breaking elongation, is preferably 0.2 to 1.5, more preferably 0.3 to 1.0. If Z is too small, the guarantee of the breaking elongation is low, and if Z is too large, the possibility of breakage during stretching increases, but the water permeability decreases.

[0112] Furthermore, in the production method of the present invention, when the process includes a step of stretching and then shrinking, the tensile breaking elongation is such that breaks at low elongation are extremely rare, and the distribution of tensile breaking elongation can be narrowed.

[0113] The space temperature in the process of stretching and then shrinking is preferably in the range of 0° C. to 160° C. in terms of shrinkage time and physical properties. If it is lower than 0° C., shrinkage takes too long and is not practical, while if it exceeds 160° C., it is not preferable because the breaking elongation and water permeability are reduced.

[0114] In the present invention, it is preferred to crimp the porous membrane during the shrinking step, which allows a highly crimped porous membrane to be obtained without being crushed or damaged.

[0115] Generally, hollow fiber membranes are straight and unbent, so that when they are bundled together to form a filtration module, there is a high possibility that the hollow fiber bundle will have a low porosity because there will be no gap between the hollow fibers. In contrast, when hollow fiber membranes with a high degree of crimping are used, the individual fibers will bend and the hollow fiber membrane intervals will be wider on average, resulting in a fiber bundle with a high porosity. In addition, a filtration module made of hollow fiber membranes with a low degree of crimping will have fewer porosity in the fiber bundle, particularly when used under external pressure, and the flow resistance will increase, so that the filtration pressure will not be effectively transmitted to the center of the fiber bundle. Furthermore, the cleaning effect of the inside of the fiber bundle will be reduced when filtration deposits are peeled off from the hollow fiber membranes by backwashing or flushing. A fiber bundle made of hollow fiber membranes with a high degree of crimping has a large porosity, so the hollow fiber membrane gaps are maintained even during external pressure filtration, and drift is less likely to occur.

[0116] The porous membrane (preferably a hollow fiber membrane) obtained by the production method of the present invention preferably has a crimp degree in the range of 1.5 to 2.5. A crimp degree of 1.5 or more is preferable for the reasons described above, and a crimp degree of 2.5 or less can suppress a decrease in the filtration area per volume.

[0117] Methods for crimping a porous membrane include a method in which the porous membrane is stretched and then shrunk during the process, and the membrane is taken up while being sandwiched between, for example, a pair of gear rolls having periodic irregularities or a pair of sponge belts having periodic irregularities.

[0118] In the manufacturing method of the present invention, it is preferable to use a take-up machine consisting of a pair of opposing caterpillar belts for drawing. In this case, take-up machines are used on the upstream and downstream sides of drawing, and in each take-up machine, a porous membrane is sandwiched between opposing belts, and the two belts are moved in the same direction at the same speed to feed the yarn. In this case, it is preferable to perform drawing by setting the yarn feed speed on the downstream side faster than that on the upstream side. By performing drawing in this way, it is possible to draw the yarn without slipping due to the drawing tension during drawing, and to prevent the yarn from being crushed flat.

[0119] Here, the endless track belt is preferably such that the inside in contact with the driving roll is made of a highly elastic belt such as a fiber-reinforced belt, and the outside surface in contact with the porous membrane is made of an elastic body. It is more preferable that the compressive elastic modulus in the thickness direction of the elastic body is 0.1 MPa or more and 2 MPa or less, and the thickness of the elastic body is 2 mm or more and 20 mm or less. In particular, it is preferable that the elastic body on the outside surface is made of silicone rubber in terms of chemical resistance and heat resistance.

[0120] In the production of the porous membrane, drying or heat treatment may be performed regardless of whether or not the membrane is stretched. Regardless of whether or not the membrane is stretched, drying or heat treatment can increase the compressive strength. The drying or heat treatment is preferably performed at 160°C or less, and more preferably at 40°C or more and 160°C or less. If the temperature is 160°C or less, the decrease in breaking elongation and the decrease in water permeability can be suppressed, and further decomposition of the antioxidant remaining in the membrane can be suppressed, so that the antioxidant can remain in the membrane. If the temperature is 40°C or more, the pressure resistance can be increased. In addition, it is preferable to perform the drying or heat treatment on the porous membrane after extracting the first solvent, the second solvent, the antioxidant, and inorganic substances if contained, in order to reduce changes in the fiber diameter, porosity, pore size, and water permeability.

[0121] <Method of producing sugar solution> The method for producing a saccharified solution of the present invention comprises the steps of: A liquefaction step in which an enzyme is added to the starch liquor to partially decompose the starch and obtain a sugar-containing liquefied product; a saccharification step of adding a saccharification enzyme to the obtained sugar-containing liquefied product to further decompose sugars and obtain a saccharified solution composition containing a saccharified solution and an insoluble component; a filtering step of passing the sugared solution composition through a porous membrane made of a resin having a three-dimensional network structure to separate the sugared solution from the insoluble components; and a washing step of passing or immersing the porous membrane in a washing solution to wash and remove insoluble matters adhering to the surface or inside of the porous membrane; In the filtering step, the sugared solution composition is filtered using the porous membrane of the present embodiment.

[0122] The filtration step in the method for producing a saccharified solution of the present invention may be, for example, a so-called internal pressure filtration step in which a saccharified solution composition is supplied to the hollow part (inner surface) of a porous membrane, passed through the membrane thickness (thick part) of the porous membrane, and the liquid that seeps out from the outer surface of the porous membrane is extracted as a saccharified solution (filtrate), or it may be a so-called external pressure filtration step in which a saccharified solution composition is supplied from the outer surface of the porous membrane, and the saccharified solution (filtrate) that seeps out from the inner surface of the porous membrane is extracted via the hollow part.

[0123] In the filtration step in the method for producing a sugar solution of the present invention, the sugar solution composition is filtered using the porous membrane of the present invention.

[0124] In this specification, the term "inside the porous membrane" refers to the membrane thickness (thick wall) portion where numerous pores are formed.

[0125] In addition, in the present specification, the type and amount of sugar contained in the "saccharified solution" are not particularly limited, but examples of sugar include glucose and the like.

[0126] In addition, in the present specification, the type and amount of the "insoluble components" contained in the sugared solution composition and removed by filtration are not particularly limited, and examples thereof include undecomposed proteins and starches.

[0127] Conventionally, glucose refined solution has generally been produced by liquefying a raw material containing starch to obtain a saccharified solution composition, which is then clarified with diatomaceous earth, and further desalted, decolorized, and concentrated. In the present invention, a specific porous membrane is used instead of such diatomaceous earth.

[0128] The washing step in the method for producing a saccharified solution of the present invention includes a washing step in which an aqueous solution containing 0.1% by weight to 4% by weight of sodium hydroxide and 0.01% by weight to 0.5% by weight of sodium hypochlorite is passed through or immersed in the porous membrane as a washing solution (chemical solution) to wash the surface and inside of the porous membrane. The washing step may include a washing solution step in which washing is performed with the washing solution, and then a rinsing step in which rinsing is performed with rinsing water to remove remaining washing solution components. Examples of the washing step include back pressure water washing in which a washing solution is passed in the opposite direction to the flow direction of the saccharified solution composition in the filtration step, i.e., from the saccharified solution side to the saccharified solution composition water side, thereby detaching and removing adherent matter (insoluble components) from the filtration surface (saccharified solution composition supply side surface) of the porous membrane, and air scrubbing in which the porous membrane is shaken by air to shake off the insoluble components adhered to the porous membrane. The amount of rinsing water used in the rinsing step is preferably 100 L / m per unit area of ​​the porous membrane.2 Less than or equal to 50 L / m 2 It is also preferable that the chlorine concentration in the filtrate at the end of the rinsing step is 0.1 ppm or less, and the pH of the filtrate is 8.6 or less.

[0129] <Filtration method> The filtration method of the present invention is characterized in that filtration is carried out using the porous membrane of the present invention. By using the porous membrane of the present invention, filtration can be carried out with high efficiency. EXAMPLES

[0130] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The physical properties in the examples and comparative examples were determined by the following methods.

[0131] (1) Outer and inner diameters of the membrane The porous membrane was thinly sliced ​​with a razor and the outer and inner diameters were measured with a 100x magnifying glass. For one sample, measurements were taken at 60 points at 30mm intervals. The standard deviation and average value were calculated, and the standard deviation / average value was used as the coefficient of variation.

[0132] (2) Film thickness The thickness of the porous membrane was determined as follows. (film thickness) = [(outer diameter) - (inner diameter)] / 2

[0133] (3) Average pore diameter The average pore size of the porous membrane was determined according to the method described in ASTM: F316-86 (also known as the half-dry method). The half-dry method determines the average pore size of the smallest pore size layer of the porous membrane. The standard measurement conditions for measuring the average pore size using the half-dry method were ethanol as the liquid used, 25°C, and a pressure rise rate of 0.001 MPa / sec. The average pore size [μm] was calculated from the following formula. Average pore size [μm] = (2860 × surface tension [mN / m]) / half-dry air pressure [Pa]

[0134] The surface tension of ethanol at 25° C. is 21.97 mN / m (Chemical Handbook, Basic Edition, 3rd Revised Edition, edited by the Chemical Society of Japan, page II-82, Maruzen Co., Ltd., 1984). Therefore, in the case of the standard measurement conditions of the present invention, Average pore size [μm] = 62834.2 / (half dry air pressure [Pa]) It can be found by:

[0135] (4) Maximum pore diameter The maximum pore size of the porous membrane was determined from the pressure (air pressure generating bubbles) when bubbles first appeared from the membrane in the half-dry method (bubble point method). In the case of the above-mentioned standard measurement conditions for the half-dry method, the pressure when bubbles first appeared from the porous membrane was calculated as follows: Maximum pore size [μm] = 62834.2 / (air pressure at which air bubbles are generated [Pa]) More can be asked for.

[0136] (5) Pore size distribution The pore size distribution of the porous membrane was determined by dividing the maximum pore size by the average pore size, i.e., pore size distribution = (maximum pore size) / (average pore size).

[0137] (6) Pure water permeability One end of a wet porous membrane about 10 cm long that had been immersed in ethanol and then repeatedly immersed in pure water was sealed, and a syringe needle was inserted into the hollow part of the other end. Pure water at 25°C was injected into the hollow part through the syringe needle at a pressure of 0.1 MPa in an environment of 25°C, and the amount of pure water permeating from the outer surface was measured. The pure water flux was calculated using the following formula to evaluate the water permeability. Pure water permeability [L / m 2 ·hr]=60×(permeation rate [L]) / {π×(membrane outer diameter [m])×(membrane effective length [m])×(measurement time [hr])}

[0138] The effective membrane length here refers to the net membrane length excluding the portion where the injection needle is inserted.

[0139] (7) Remaining amount of antioxidant After crushing the porous membrane into approximately 5 mm squares, the antioxidant remaining in the membrane was extracted with chloroform, and the concentration of the supernatant was measured using LC-MS (Shimadzu Corporation, product name: Nexera X2) under the following conditions to calculate the concentration. Note that in this specification, the remaining amount of antioxidant is the amount of antioxidant remaining relative to the amount of polyvinylidene fluoride (PVDF). LC device: SHIMADZU, Nexera X2 Column: Waters, ACQUITY UPLC BEH-C18 1.7 μm (2.1 mm I.D. × 50 mm) Column temperature: 40℃ Detection: PDA 200~800nm Flow rate: 0.3mL / min Mobile phase: A = 10 mM ammonium acetate aqueous solution, B = acetonitrile Gradient: as shown in Table 1 below. Injection volume: 1μL MS equipment:Bruker,amaZon SL Ionization: ESI+ Scan range: m / z 500-1500

[0140] [Table 1]

[0141] (8) Bursting strength (MPa) One end of a dry hollow fiber membrane about 5 cm long was sealed, the other end was connected to the device, and pure water at 40°C was applied to the inner surface. The applied pressure was increased from 0 MPa in increments of 0.02 MPa, and the pressure at which the hollow fiber membrane was visually confirmed to have burst was taken as the burst strength. This test was performed using a pressure test device (manufactured by Hara Engineering Co., Ltd.).

[0142] (9) Defects The bubble point in the porous membrane was measured 20 times (n=20), and the average value and standard deviation (σ) were calculated. If any data significantly deviated from the average value + 3σ, the porous membrane was determined to be defective. A: No large pores that deviate from the average maximum pore size + 3σ B: Large pores exceeding the average maximum pore size + 3σ

[0143] (10) Solvent Residuals One piece of porous membrane cut to approximately 74 mg was placed in a 50 mL vial, to which 15.5 mL of 50% aqueous ethanol solution was added (bath ratio: 0.211 mL / mg) and heated to 40°C. After 24 hours, the entire amount of the extract was taken out and subjected to GC / MS measurement under the following conditions. The detection limit was estimated by defining S / N=3 from the peak of a standard solution with a known concentration, and results obtained from this measurement were evaluated as "residues present" when the detection limit was above the detection limit, and "no residues" when the detection limit was below the detection limit. GC device: Agilent7890 Column: DB-5MS (30 m, 0.25 mm diameter, film thickness 1.0 μm) Column temperature: 40°C (5 min) - 20°C / min heating) - 320°C (11 min) Flow rate: 1mL / min Inlet temperature: 320℃ Split:Splitless Injection volume: 1μL MS instrument: Agilent MSD5977B HES Interface: 300℃ Ionization: EI 70eV Measurement method: SCAN method Ion source temperature: 230℃

[0144] (11) Open area ratio The inner surface of the hollow fiber membrane was photographed using a Hitachi SU8000 series electron microscope at an accelerating voltage of 3 kV. The images were taken at a magnification that allowed the shapes of 20 or more pores to be confirmed, and in this example and comparative example, the images were taken at a magnification of 3000 to 5000. Using the photographed image, for example, as described in International Publication No. 2001 / 53213, a transparent sheet was placed on top of the copy of the image, and the holes were filled in black with a black pen or the like, and the transparent sheet was then copied onto a blank sheet of paper, so that the holes were clearly distinguished as black and the non-holes as white. Then, using commercially available image analysis software Winroof 6.1.3, binarization was performed by discriminant analysis. The opening rate was calculated by determining the area occupied by the binarized image thus obtained.

[0145] [Example 1] The molten mixture was extruded using a spinning nozzle with a double-tube structure to obtain a porous membrane of Example 1. A molten mixture of 40% polyvinylidene fluoride (PVDF) resin (Solef6010, manufactured by Solvay) as a thermoplastic resin, 22.8% fine silica (primary particle size: 16 nm) as an inorganic powder, 2.0% Irganox 1010 as an antioxidant, 21.1% bis-2-ethylhexyl adipate (DOA, boiling point 335°C) as a first solvent, and 14.1% dibutyl sebacate (DBS, boiling point 345°C) as a second solvent was extruded into a hollow fiber-shaped molded product at a discharge temperature of 235°C using air as a hollow portion forming fluid. The extruded hollow fiber-shaped molded product was passed through an idle running distance of 290 mm, and then solidified in water at 30°C, and a hollow fiber membrane was produced by a thermally induced phase separation method. It was taken up at a speed of 6.5 m / min and wound into a skein. The obtained hollow fiber-shaped extrudate was immersed in isopropanol to extract and remove bis(2-ethylhexyl) adipate and dibutyl sebacate. It was then immersed in water for 30 minutes to replace the hollow fiber membrane with water. It was then immersed in a 20% by mass NaOH aqueous solution at 70°C for 1 hour, and further repeatedly washed with water to extract and remove fine silica. The obtained hollow fiber membrane was subjected to a heat treatment at 60°C.

[0146] Table 2 shows the composition and production conditions, as well as various properties, of the obtained porous membrane of Example 1. The membrane structure exhibited a three-dimensional network structure as shown in FIG.

[0147] [Example 2] A porous film was produced in the same manner as in Example 1, except that the molten mixture was prepared using 23.2 mass% fine silica (primary particle size: 16 nm) as inorganic powder, 1.0 mass% Irganox 1010 as antioxidant, 21.5 mass% bis-2-ethylhexyl adipate (DOA, boiling point 335°C) as first solvent, and 14.3 mass% dibutyl sebacate (DBS, boiling point 345°C) as second solvent.

[0148] Table 2 shows the composition and production conditions, as well as various properties, of the resulting porous membrane of Example 2. The membrane had a three-dimensional network structure as shown in FIG.

[0149] [Example 3] A porous film was produced in the same manner as in Example 1, except that the molten mixture was prepared using 23.2 mass% fine silica (primary particle size: 16 nm) as inorganic powder, 1.0 mass% Irganox 1010 as antioxidant, 23.8 mass% bis-2-ethylhexyl adipate (DOA, boiling point 335°C) as first solvent, and 11.9 mass% dibutyl sebacate (DBS, boiling point 345°C) as second solvent.

[0150] Table 2 shows the composition and production conditions, as well as various properties, of the resulting porous membrane of Example 3. The membrane had a three-dimensional network structure as shown in FIG.

[0151] [Example 4] A molten mixture was prepared using 23.2% by mass of fine silica (primary particle size: 16 nm) as inorganic powder, 1.0% by mass of Irganox 1010 as antioxidant, 17.9% by mass of bis 2-ethylhexyl adipate (DOA, boiling point 335°C) as first solvent, and 17.9% by mass of dibutyl sebacate (DBS, boiling point 345°C) as second solvent, and the discharge temperature was set to 220°C. A porous film was prepared in the same manner as in Example 1, except for the following conditions.

[0152] The extruded hollow fiber-shaped molding was passed through an idle running distance of 270 mm, and then solidified in water at 30°C, and a hollow fiber membrane (hollow fiber extrudate) was produced by a thermally induced phase separation method. It was taken up at a speed of 2.0 m / min and wound into a skein. The obtained hollow fiber extrudate was immersed in methylene chloride to extract and remove bis(2-ethylhexyl) adipate and dibutyl sebacate. It was then immersed in water for 30 minutes to replace the hollow fiber membrane with water. It was then immersed in a 20% by mass NaOH aqueous solution at 70°C for 1 hour, and further washed with water repeatedly to extract and remove the fine silica.

[0153] Table 2 shows the composition and production conditions, as well as various properties, of the resulting porous membrane of Example 4. The membrane had a three-dimensional network structure as shown in FIG.

[0154] [Example 5] A molten mixture was prepared using 23.2% by mass of fine silica (primary particle size: 16 nm) as inorganic powder, 1.0% by mass of Irganox 1010 as antioxidant, 24.2% by mass of bis 2-ethylhexyl adipate (DOA, boiling point 335°C) as first solvent, and 11.5% by mass of dibutyl sebacate (DBS, boiling point 345°C) as second solvent, and the discharge temperature was set to 230°C. A porous film was prepared in the same manner as in Example 1, except for the following conditions.

[0155] The extruded hollow fiber-shaped molding was passed through an idle running distance of 300 mm, and then solidified in water at 30°C, and a hollow fiber membrane (hollow fiber extrudate) was produced by a thermally induced phase separation method. It was taken up at a speed of 6.5 m / min and wound into a skein. The obtained hollow fiber extrudate was immersed in methylene chloride to extract and remove bis(2-ethylhexyl) adipate and dibutyl sebacate. It was then immersed in water for 30 minutes to replace the hollow fiber membrane with water. It was then immersed in a 20% by mass NaOH aqueous solution at 70°C for 1 hour, and further washed with water repeatedly to extract and remove fine silica.

[0156] Table 2 shows the composition and production conditions, as well as various properties, of the obtained porous membrane of Example 5. The membrane structure exhibited a three-dimensional network structure as shown in FIG.

[0157] [Example 6] A porous membrane was produced in the same manner as in Example 1 except that a molten mixture was prepared using 23.4 mass% fine silica (primary particle size: 16 nm) as inorganic powder, 0.5 mass% Irganox 1010 as antioxidant, 24.0 mass% bis 2-ethylhexyl adipate (DOA, boiling point 335°C) as first solvent, and 12.0 mass% dibutyl sebacate (DBS, boiling point 345°C) as second solvent, and the discharge temperature was set to 245°C.

[0158] Table 2 shows the composition and production conditions, as well as various properties, of the resulting porous membrane of Example 6. The membrane had a three-dimensional network structure as shown in FIG.

[0159] [Example 7] A porous membrane was produced in the same manner as in Example 1 except that a molten mixture was prepared using 23.4 mass% fine silica (primary particle size: 16 nm) as inorganic powder, 0.5 mass% Irganox 1010 as antioxidant, 25.8 mass% bis 2-ethylhexyl adipate (DOA, boiling point 335°C) as first solvent, and 10.3 mass% dibutyl sebacate (DBS, boiling point 345°C) as second solvent, and the discharge temperature was set to 245°C.

[0160] Table 2 shows the composition and production conditions, as well as various properties, of the obtained porous membrane of Example 7. The membrane structure exhibited a three-dimensional network structure as shown in FIG.

[0161] [Example 8] The molten mixture was extruded using a spinning nozzle with a double-tube structure to obtain a porous membrane of Example 8. A melt-kneaded mixture was prepared using 40% polyvinylidene fluoride (PVDF) resin (Solvay, Solef6010) as a thermoplastic resin, 23.2% fine silica (primary particle size: 16 nm) as an inorganic powder, 1.0% Irganox1010 as an antioxidant, 24.2% bis-2-ethylhexyl adipate (DOA, boiling point 335°C) as a first solvent, and 11.5% dibutyl sebacate (DBS, boiling point 345°C) as a second solvent, and air was used as a fluid for forming the hollow portion, and a hollow fiber-shaped molded product was extruded at a discharge temperature of 230°C. The extruded hollow fiber-shaped molded product was passed through an empty running distance of 300 mm, then solidified in water at 30°C, and a hollow fiber membrane (hollow fiber-shaped extrudate) was produced by a thermally induced phase separation method. The extrudate was taken up at a speed of 6.5 m / min, sandwiched between belts and stretched at a speed of 15 m / min, then relaxed at a speed of 12 m / min while being exposed to hot air at 120°C, and wound up. The obtained hollow fiber extrudate was immersed in isopropanol to extract and remove bis(2-ethylhexyl) adipate and dibutyl sebacate. The hollow fiber membrane was then immersed in water for 30 minutes to replace the water. The hollow fiber membrane was then immersed in a 20% by mass NaOH aqueous solution at 70°C for 1 hour, and further repeatedly washed with water to extract and remove the fine silica. The obtained hollow fiber membrane was subjected to a heat treatment at 100°C.

[0162] Table 2 shows the composition and production conditions, as well as various properties, of the obtained porous membrane of Example 8. The membrane structure exhibited a three-dimensional network structure as shown in FIG.

[0163] [Comparative Example 1] A molten mixture was prepared using 23.5% by mass of fine silica (primary particle size: 16 nm) as inorganic powder, 0.3% by mass of Irganox 1010 as antioxidant, 24.1% by mass of bis-2-ethylhexyl adipate (DOA, boiling point 335°C) as first solvent, and 12.1% by mass of dibutyl sebacate (DBS, boiling point 345°C) as second solvent, and air was used as hollow portion forming fluid, except that the extrusion was performed at a discharge temperature of 245°C, a porous film was produced in the same manner as in Example 1.

[0164] Table 3 shows the composition and production conditions of the obtained porous membrane of Comparative Example 1, as well as various properties.

[0165] [Comparative Example 2] A porous film was produced in the same manner as in Comparative Example 1, except that the molten mixture was prepared using 23.6 mass% fine silica (primary particle size: 16 nm) as the inorganic powder, 24.3 mass% bis(2-ethylhexyl) adipate (DOA, boiling point 335°C) as the first solvent, and 12.1 mass% dibutyl sebacate (DBS, boiling point 345°C) as the second solvent without using an antioxidant.

[0166] Table 3 shows the composition and production conditions of the obtained porous membrane of Comparative Example 2, as well as various properties.

[0167] [Comparative Example 3] A porous film was produced in the same manner as in Comparative Example 1, except that the molten mixture was prepared using 22.1 mass% fine silica (primary particle size: 16 nm) as the inorganic powder, 3.9 mass% Irganox 1010 as the antioxidant, 20.4 mass% bis-2-ethylhexyl adipate (DOA, boiling point 335°C) as the first solvent, and 13.6 mass% dibutyl sebacate (DBS, boiling point 345°C) as the second solvent.

[0168] Table 3 shows the composition and production conditions of the obtained porous membrane of Comparative Example 3, as well as various properties.

[0169] The obtained porous membranes of Examples 1 to 8 and Comparative Examples 1 to 3 had a single layer structure.

[0170] [Table 2]

[0171] [Table 3]

[0172] *1: Polyvinylidene fluoride resin (manufactured by Solvay, product name "Solef6010") *2: Bis 2-ethylhexyl adipate (manufactured by New Japan Chemical Co., Ltd., DOA, boiling point 335°C) *3: Dibutyl sebacate (Toyokuni Oil Mills, DBS, boiling point 345℃) *4: Fine silica (manufactured by Nippon Aerosil Co., Ltd., primary particle size: 16 nm) *5: Irganox 1010, manufactured by BASF

[0173] As shown in Tables 2 and 3, in Examples 1 to 8, by mixing a certain amount or more of an antioxidant into the film-forming solution in the film formation by thermally induced phase separation, it is possible to obtain a porous film with a sharp pore size distribution and no defects. On the other hand, in Comparative Examples 1 to 3 in which the amount of antioxidant is outside a certain range, the pore size distribution is broad, or even if the pore size distribution is sharp, there are defects, and therefore it is understood that there is a risk of leakage of suspended solids. [Industrial Applicability]

[0174] According to the present invention, since the porous film is formed by containing an antioxidant, a porous film having a sharp pore size distribution and free of defects is provided. [Explanation of symbols]

[0175] A: Thermoplastic resin b: void area 10: Extruder 20: Hollow fiber forming nozzle 30: Coagulation bath 40: Porous hollow fiber membrane 50: Lola S: Air running club

Claims

1. A porous membrane comprising a thermoplastic resin, the porous membrane comprises at least a first solvent, a second solvent, and an antioxidant; the first solvent is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; the second solvent is different from the first solvent and is at least one selected from the group consisting of sebacic acid esters, citric acid esters, acetyl citrate esters, adipic acid esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; A porous film, comprising the antioxidant in an amount of 0.05% by mass or more and 0.5% by mass or less.

2. The porous membrane according to claim 1 , wherein the antioxidant is a hindered phenol-based antioxidant.

3. When the pore size distribution (P) of the porous membrane is expressed as pore size distribution (P)=(maximum pore size) / (average pore size), P≦2.4 (1) The porous membrane according to claim 1, characterized in that

4. The porous membrane according to claim 1, characterized in that the average pore size of the porous membrane is 0.1 μm or more.

5. The thickness of the porous membrane is 0.1 mm or more and 0.7 mm or less, The porous membrane according to claim 1, characterized in that the burst strength is 0.5 MPa or more.

6. The porous membrane according to claim 1 , wherein the porosity of one surface of the porous membrane is 20% or more.

7. The porous membrane according to claim 1, characterized in that the porous membrane is in the form of a hollow fiber and the thermoplastic resin is a vinylidene fluoride-based resin.

8. 2. The porous membrane according to claim 1, characterized in that it has a single layer structure.

9. 1. A method for producing a porous membrane comprising a thermoplastic resin, at least a first solvent, and a second solvent, comprising: the first solvent is at least one selected from the group consisting of sebacic acid esters, citrate esters, acetyl citrate esters, adipate esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; the second solvent is different from the first solvent and is at least one selected from the group consisting of sebacic acid esters, citric acid esters, acetyl citrate esters, adipic acid esters, trimellitic acid esters, oleic acid esters, palmitic acid esters, stearic acid esters, phosphate esters, fatty acids having 6 to 30 carbon atoms, and epoxidized vegetable oils; A method for producing a porous membrane, comprising mixing an antioxidant in addition to the thermoplastic resin, at least a first solvent, and a second solvent.

10. The method for producing a porous membrane according to claim 9, wherein the antioxidant is used for adjusting pore size and pore size distribution.

11. When the pore size distribution (Pa) of the porous membrane when no antioxidant is used is expressed as Pa=(maximum pore size of the porous membrane when no antioxidant is used) / (average pore size of the porous membrane when no antioxidant is used), and the pore size distribution (Pb) of the porous membrane when an antioxidant is used is expressed as Pb=(maximum pore size of the porous membrane when an antioxidant is used) / (average pore size of the porous membrane when an antioxidant is used), Pb / Pa≦0.95... (2) The method for producing a porous membrane according to claim 9,

12. The antioxidant in the porous membrane is 0.01≦(remaining amount of antioxidant) / (mixed amount of antioxidant)≦0.5 (3) The method for producing a porous membrane according to claim 9, wherein the above formula is satisfied.

13. The method for producing a porous membrane according to claim 9 , wherein the antioxidant is mixed in an amount of 0.5% by mass to 3.0% by mass.

14. The method for producing a porous film according to claim 9, wherein the antioxidant is a hindered phenol-based antioxidant.

15. 10. The method for producing a porous membrane according to claim 9, characterized in that a mixture containing the thermoplastic resin, the first solvent, the second solvent, and the antioxidant, or a mixture containing the thermoplastic resin, the first solvent, the second solvent, the antioxidant, and an inorganic substance is melt-kneaded and extruded, and then the first solvent, the second solvent, the antioxidant, and, if contained, the inorganic substance are extracted from the porous membrane.

16. After extracting the first solvent, the second solvent, the antioxidant, and, if present, the inorganic matter from the porous membrane, The method for producing a porous membrane according to claim 15, characterized in that the porous membrane is dried or heat-treated at 160° C. or less.

17. A method for producing a sugar solution, comprising the steps of: a liquefaction step in which an enzyme is added to the starch liquid to partially decompose the starch and obtain a sugar-containing liquefied product; a saccharification step in which a saccharification enzyme is added to the obtained sugar-containing liquefied product to further decompose sugars, thereby obtaining a saccharified solution composition containing a saccharified solution and an insoluble component; a filtering step of passing the sugared solution composition through a porous membrane made of a resin having a three-dimensional network structure to separate the sugared solution from the insoluble components; and a washing step of passing a washing solution through or immersing the porous membrane in a washing solution to wash and remove insoluble matters adhering to the surface or inside of the porous membrane; 2. A method for producing a sugared solution, comprising: filtering the sugared solution composition using the porous membrane according to claim 1 in the filtering step.

18. A filtration method, comprising filtering using the porous membrane according to claim 1.

Citation Information

Patent Citations

  • Porous hollow fiber membrane, production method therefor, and filtration method

    WO2017155004A1