Increasing adhesion of metal-organic interface by silane vapor treatment

By depositing a silane monolayer on metal surfaces in electronic devices, the adhesion between metal and organic layers is strengthened, addressing adhesion issues and improving device reliability.

JP2024167161APending Publication Date: 2024-12-03YIELD ENGINEERING SYSTEMS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024066497
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-04-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Poor adhesion at metal-organic interfaces in electronic devices leads to defects, reduced yield, and reliability issues, particularly in miniaturized circuits where copper and dielectric layers are involved.

Method used

Roughening the metal surface to mechanically interlock with the dielectric layer is enhanced by depositing a monolayer of silane composition on the metal surface using vapor deposition, followed by coating with organic materials.

Benefits of technology

Improves adhesion strength without increasing surface roughness, reducing delamination and signal loss, and enhancing the reliability of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167161000001_ABST
    Figure 2024167161000001_ABST
Patent Text Reader

Abstract

To provide a method for improving the adhesion between copper and dielectric layers in order to produce very fine copper circuits with small line and space widths for next generation electronic devices.SOLUTION: A method of improving the adhesion of a metal-organic interface in an electronic device includes providing a substrate with a metal structure, depositing a mono-layer of a selected silane composition on a surface of the metal structure with a vapor of the selected silane composition, and coating the treated surface with an organic material.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to methods for improving the adhesion strength of metal-organic interfaces in electronic devices. [Background technology]

[0002] The fabrication process of electronic (or photonic) devices consists of many sequential steps to fabricate circuits on wafers or panels (collectively referred to herein as substrates) of materials (e.g., semiconductor wafers, glass panels, printed circuit boards, organic / ceramic substrates, etc.). Any source of defects introduced during the fabrication process reduces the yield of the resulting devices. One cause of defects is due to improper adhesion at the metal-organic interface of the device. Electronic devices (e.g., packaging substrates, integrated circuit chips, optoelectronic devices, etc.) contain numerous metal-organic interfaces. The adhesion between the metal components (e.g., interconnects, land pads, vias, etc.) and the organic components (e.g., dielectric materials, molding compounds, underfill materials, etc.) at the metal-organic interface can be compromised for many reasons. For example, the quality / structure of the materials at the interface, embedded particles / residues (debris, chemicals, etc.) on the interface, high thermo-mechanical interfacial tensions (e.g., CTE mismatch), etc. Poor adhesion between metal (e.g., copper pad) and organic (e.g., dielectric) at the interface may introduce defects (e.g., delamination, cracks, etc.) at the interface, leading to reduced device yield and / or reliability. A strong metal-organic interface ensures that downstream processes (e.g., chemicals and / or process conditions used during downstream processes) do not reduce the adhesive strength at the interface. Furthermore, miniaturization of electronic devices requires miniaturization of integrated circuit (IC) substrates (e.g., printed circuit boards (PCBs)) that consist of layers of organic materials (commonly referred to as build-up layers or dielectric layers, e.g., polymers, build-up layers, e.g., Ajinomoto Build-Up Film (ABF), etc.) and metal (e.g., copper) interconnect circuits (e.g., lines, planes, vias, etc.). To produce very fine copper circuits with small line-and-space widths for next generation electronic devices, there is a need to improve adhesion between copper and dielectric layers. Summary of the Invention [Means for solving the problem]

[0003] The adhesion improvement method relies on roughening the metal surface to allow the overlying dielectric layer to mechanically interlock with the metal surface and improve adhesion. For example, the surface of the metal interconnect is modified, for example, by etching, plasma ablation, etc., before depositing the dielectric layer to improve adhesion between the metal and the dielectric. However, such roughening may adversely affect the electrical performance of the electronic device and / or lead to reliability issues. For example, high frequency applications may require low surface roughness, and the etching / ablation may require additional cleaning steps and / or debris from the roughening process may be redeposited and embedded on the interface. The adhesion improvement method of the present disclosure may at least alleviate some of the above deficiencies. However, the scope of the present disclosure is defined by the claims and not by the ability to solve any problem.

[0004] Disclosed are embodiments of a method for improving the interfacial strength of a metal-organic interface in an electronic device. In some embodiments, the method for improving adhesion of a metal-organic interface in an electronic device includes providing a substrate with a metal structure. The method may also include depositing a monolayer of a selected silane composition on a surface of the metal structure with a vapor of the selected silane composition, and coating the treated surface with an organic material.

[0005] In one embodiment, a method for improving adhesion of a metal-organic interface in an electronic device is disclosed. The method may include providing a substrate with a copper interconnect structure and depositing a monolayer of a silane composition on the surface of the copper interconnect structure by vapor deposition. The silane composition may include (a) at least a primary or secondary amine group and at least one alkoxysilyl group, (b) the alkoxysilyl group may be one of ethoxy, methoxy, butoxy, propoxy, or isopropoxy, (c) the alkoxysilyl group may have 1-3 alkoxy groups attached, and (d) a boiling point less than about 250° C. at a pressure of about 0.1-10 Torr. The method may further include depositing ABF on the surface of the copper interconnect structure after depositing the monolayer of the silane composition.

[0006] In another embodiment, a method for improving adhesion at a metal-organic interface in an electronic device is disclosed. The method may include providing a substrate having a metal structure formed thereon, and treating the surface of the metal structure with vapor of a silane composition. The silane composition may be any of the following: (i.) N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AE-APTMS), (ii.) N,N'-bis[(3-trimethoxysilyl)propyl]ethylenediamine (TMSP-ED), (iii.) bis(3-trimethoxysilylpropyl)amine, (TMSPA), (iv.) 3-mercaptopropyltrimethoxysilane (MPTMS), (v.) N-(2-aminoethyl)-3-aminopropylsilanetriol, 25% in water (AE-APSTMS), (vi.) N-(2-aminoethyl)-3-aminopropylsilanetriol, 25% in water (AE-APSTMS), (vi.) N-(2-aminoethyl)-3-aminopropyltrimethoxy ... ), (vi.) 3-thiocyanatopropyltriethoxysilane, 92% (TCPTES), (vii.) N-(6-aminohexyl)aminomethyltrimethoxysilane, (viii.) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, (ix.) bis[3-(triethoxysilyl)propyl]disulfide, 90% (TESPDS), (x.) cysteamine, (xi.) 3-aminopropanethiol, (xii.) aminoethylaminopropyl / methylsilsesquioxane in aqueous solution. San, (xiii.) aminopropylsilsesquioxane (APS) in aqueous solution, (xiv.) (2-diethylphosphatoethyltriethoxysilane), (xv.) (2-diethylphosphatoethyl)methyldiethoxysilane, (xvi.) N-(2-aminoethyl)-3-aminopropyltriethoxysilane, (xvii.) (3-(M-aminophenoxy)propyltrimethoxysilane, (xviii.) N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, (xix.) ) N-(2-aminoethyl)-3-aminoisobutylmethyldimethoxysilane, (xx.) N-(2-aminoethyl)-3-aminoisobutyldimethylmethoxysilane, (xxi.) 4-aminobutyltriethoxysilane, (xxii.) (aminoethylaminomethyl)phenethyltrimethoxysilane, (xxiii.) N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, (xxiv.) N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane, (xxv.)(xxvi.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvii.) m-aminophenyltrimethoxysilane, or (xxviii.) m-aminophenyltrimethoxysilane. The method may also include, after treating the surface, coating the treated surface with an organic material.

[0007] In yet another embodiment, a method for improving adhesion at a metal-organic interface in an electronic device is disclosed. The method may include providing a substrate having a copper interconnect structure and treating a surface of the copper interconnect structure with vapor of a silane composition. The silane composition may have a boiling point less than about 250° C. at a pressure of about 0.1 to 10 Torr, The following compounds are used: (i.) N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AE-APTMS), (ii.) N,N'-bis[(3-trimethoxysilyl)propyl]ethylenediamine (TMSP-ED), (iii.) bis(3-trimethoxysilylpropyl)amine, (TMSPA), (iv.) 3-mercaptopropyltrimethoxysilane (MPTMS), (v.) N-(2-aminoethyl)-3-aminopropylsilanetriol, 25% in water (AE-APST), (vi.) 3-thiocyanatopropyltriethoxysilane, 92% (TCPTES), (vii.) N-(6-aminohexyl)aminomethyltrimethoxysilane, (viii.) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, (ix.) bis[3-(triethoxysilyl)propyl]disulfide, 90% (TESPDS), (x.) cysteamine, (xi.) 3-aminopropanethiol, (xii.) aminoethylaminopropyl / methylsilsesquioxane in aqueous solution, (xiii.) aminopropylsilsesquioxane (APS) in aqueous solution, (xiv.) (2-diethylphosphatoethyl) (xv.) (2-diethylphosphatoethyl)methyldiethoxysilane, (xvi.) N-(2-aminoethyl)-3-aminopropyltriethoxysilane, (xvii.) (3-(M-aminophenoxy)propyltrimethoxysilane, (xviii.) N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, (xix.) N-(2-aminoethyl)-3-aminoisobutylmethyldimethoxysilane, (xx.) N-(2-aminoethyl)-3-aminoisobutyldimethylmethoxysilane, (xxi.) 4-aminobutyltriethoxysilane, (xxii.) (aminoethylaminomethyl)phenethyltrimethoxysilane, (xxiii.) N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, (xxiv.) N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane, (xxv.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvi.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvii.) m-aminophenyltrimethoxysilane, or (xxviii.)) m-aminophenyltrimethoxysilane. The method may also include, after treating the surface, coating the treated surface with ABF.

[0008] The accompanying drawings, which are incorporated herein and constitute a part of this disclosure, illustrate exemplary embodiments and, together with the description, serve to explain the disclosed principles. In the drawings, where appropriate, reference numerals are similarly labeled to indicate the same or similar structures, components, materials, and / or elements in different figures. It is understood that various combinations of structures, components, and / or elements other than those specifically shown are contemplated and are within the scope of the present disclosure.

[0009] For simplicity and clarity of description, the drawings show the general structure of the various described embodiments. Details of well-known components or features may be omitted to avoid obscuring other features, because these omitted features are well-known to those skilled in the art. Additionally, features in the figures are not necessarily drawn to scale. Dimensions of some features may be exaggerated relative to other features to improve understanding of the exemplary embodiments (see, for example, FIG. 3B). Those skilled in the art will appreciate that features in the figures are not necessarily drawn to scale, and should not be taken to represent dimensional or proportional relationships between different features in the figures, unless otherwise indicated. Additionally, aspects described with reference to one embodiment or figure may be applicable to and used in conjunction with other embodiments or figures, even if not specifically mentioned. [Brief description of the drawings]

[0010] [Figure 1A] FIG. 1 is a simplified schematic of a metal-organic interface in an electronic device. [Figure 1B] 1B is a schematic cross-sectional view of an exemplary electronic device including the interface of FIG. 1A. [Figure 2A] 1B is a flow chart of an exemplary method for treating a metal surface at the metal-oxide interface of FIG. 1A. [Figure 2B] 1B is a flow chart of another exemplary method for treating a metal surface at the metal-oxide interface of FIG. 1A. [Figure 3A] 1 shows the results of experiments performed on samples representing exemplary embodiments of the present disclosure. [Figure 3B] FIG. 3B is a schematic diagram of the structure of the sample in the test of FIG. 3A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Detailed Description All relative terms, such as "about," "substantially," and "approximately," indicate a possible variation of ±10% (unless otherwise indicated or another variant is specified). For example, a feature disclosed as being about "t" units thick (length, width, depth, etc.) may vary in thickness from (t-0.1t) units to (t+0.1t) units. In some cases, the specification also provides context to some of the relative terms used. For example, a structure (e.g., a coating edge) described as being substantially flat may deviate ±10% from being perfectly flat. Additionally, ranges described as varying from 5 to 10 or between 5 and 10 (5-10) include the endpoints (i.e., 5 and 10). Additionally, as used herein, a composition comprising at least one of A, B, or C is used to refer to a composition comprising one or more of A, B, or C. For example, a composition containing only A, a composition containing only B, a composition containing only C, a composition containing both A and B, a composition containing both A and C, a composition containing A, B, and C, etc.

[0012] Unless otherwise defined, all technical terms, notations, and other scientific or technical terms used herein have the same meaning as commonly understood by those skilled in the art to which this disclosure belongs. Some of the components, structures, and / or processes described or referenced herein are well understood and commonly used by those skilled in the art using conventional methodologies. Detailed descriptions of these components, structures, and processes are omitted. All patents, applications, published applications, and other publications mentioned as being incorporated herein by reference are incorporated by reference in their entirety. If any definitions or explanations set forth in this disclosure are contrary to or inconsistent with the definitions and / or explanations of these references, the definitions and / or explanations set forth in this disclosure shall take precedence over the definitions and / or explanations of the references incorporated by reference. None of the references described or referenced herein are admitted as prior art to this disclosure. It should be noted that the term "electronic device" is used in this disclosure to encompass all components and electronic / photonic assemblies (e.g., package substrates, printed circuit boards, interposers, integrated circuit chips, etc.).

[0013] The following discussion describes an exemplary method of improving the interfacial adhesion strength of a metal-organic interface in an electronic device. FIG. 1A is a simplified diagram of a metal-organic interface 30 of an exemplary electronic device illustrated in FIG. 1B. The interface 30 comprises a metal structure 10 (e.g., a line, a surface, a pad, a via wall, etc.) with an organic layer 20 formed on one of its surfaces. The organic layer 20 may be formed on the metal structure 10 by any known method (e.g., deposition, plating, growing, spraying, etc.) used in the fabrication of electronic devices. In an exemplary embodiment, the metal-organic interface 30 of FIG. 1A may be the interface of an exemplary package substrate 40 representing the electronic device of FIG. 1B. The package substrate 40 is an eight-layer high density interconnect (HDI) substrate (referred to as a 2+4+2 (2 build-up+4 core layers+2 build-up layers) stack) with two build-up layers 34 on either side of a core stack 32 having four circuit layers. The core stack 32 may be made of BT (bismaleimide triazine) epoxy with embedded glass fibers that separate the copper interconnect lines and plated through hole (PTH) vias of the core. The build-up layers 34 on one side of the core stack 32 may also include an organic dielectric material (such as ABF) that separates the copper interconnect structures (e.g., interconnect lines, interlayer vias, bond pads, etc.) in these layers. In some embodiments, the BT epoxy core stack 32 may be fabricated first, and then the build-up layers 34 may be formed successively on the top and bottom (e.g., by deposition, photolithographic patterning, etching, etc.). As illustrated by the dashed circle in Figures 1A and 1B, the metal-organic interface 30 in Figure 1A may be an interface located anywhere on the package substrate 40. As previously discussed, although the interface 30 is described as being part of the package substrate 40, the interface 30 can be part of any electronic device. For example, on a back-end structure such as an IC die.

[0014] In the embodiment illustrated in FIGS. 1A and 1B, the material of the metal structure 10 is a conductive interconnect material (e.g., copper, etc.). The material of the organic layer 20 depends on the location of the interface 30 in the package substrate 40. For example, if the interface 30 is an interface in the core stack 32, the organic layer 20 may be an organic material used in the core (e.g., BT epoxy, etc.). If the interface 30 is an interface in the build-up layer 34, the organic layer 20 may be an organic material used in the build-up layer (e.g., ABF, or any other build-up material, etc.). These materials are merely exemplary. In general, the organic layer 20 may comprise any material, such as a polymer, a dielectric, an epoxy (e.g., underfill epoxy, overmold epoxy, etc.), or a composite material made of two or more of the above materials. For example, a composite material of glass fiber, epoxy resin, and silica-filled material with a layer of copper thereon, commonly referred to as copper-clad laminate, etc. The metal structure 10 may comprise any metal or alloy, such as copper, gold, titanium, aluminum, etc. Additionally, metal structure 10 at interface 30 may be any portion of an interconnect structure (eg, interconnect lines, power planes, ground planes, interlayer vias, PTHs, bond pads, etc.) on package substrate 40 .

[0015] With reference to FIG. 1A, in the method of the present disclosure, after the metal structure 10 is formed by any suitable method before forming the organic layer 20 on the surface of the metal structure 10 (e.g., by depositing a layer of organic material), a thin layer (e.g., monolayer) of a suitable silane is formed (e.g., deposited) on the surface of the metal structure 10 to improve the adhesion of the organic layer 20 on the metal structure 10. The metal structure 10 may be formed by any process (e.g., IC fabrication process) used to form a metal structure on an underlying substrate. For example, one exemplary process of forming the metal structure 10 on the underlying substrate (e.g., core stack 32 of FIG. 1B) may include depositing a layer of metal (e.g., copper) on the substrate (e.g., by chemical vapor deposition (CVD), etc.) and patterning the metal layer into a desired circuit pattern using a conventional photolithography process. The organic layer 20 may also be formed on the metal structure 10 by any known process (e.g., deposition, plating, spraying, etc.) used in the fabrication of package substrates 40. Prior to forming the organic layer 20, a silane monolayer is formed (deposited) on the surface of the metal structure, for example, by vapor phase silane deposition. Generally, the deposited silane monolayer may be about 1-30 Angstroms thick. In some embodiments, the silane monolayer may be about 1-10 Angstroms thick. It should be noted that the "thickness" of the monolayer may be the length of a silane molecule. The coverage of the monolayer on the substrate may not be 100% and when a measurement technique such as ellipsometry is used to measure the "thickness" of such a film, the derived thickness may be 0-100% of the length of the molecule, depending on the percentage coverage of the monolayer on the substrate.

[0016] Vapor phase silane deposition is a controlled process that provides a stable environment for the formation of a consistent self-assembled monolayer silane coating on the surface of the metal structure 10. The functional silane monolayer coating provides reactivity and functionality to the surface of the metal structure 10 by creating durable covalent bonds between the silane molecules and the underlying metal structure 10. As known to those skilled in the art, the physical and chemical properties of a solid surface are determined to a large extent by the outermost layer of atoms or chemical groups. As a result, coating the surface of the metal structure 10 with a suitable silane monolayer allows the metal structure 10 to form strong bonds with the molecules of the organic layer 20 onto which it is deposited (or otherwise formed). Silane surface modification of metal surfaces is known (see, for example, Sagiv; J. Am. Chem. Soc; Jan. 1, 1980; 102; pp. 92-98), but silane coupling agents for metals that could be achieved to form hydrolytically or mechanically unstable surface oxides have not been previously disclosed. Silane coupling agents suitable for adhesion between metal surfaces and organic layers have not been previously disclosed.

[0017] Suitable silane coupling agents for improving the adhesive strength of metal-organic interfaces may include a class of aminosilanes with at least one primary or secondary amine group and at least one alkoxysilyl group. The alkoxysilyl group may be one of ethoxy, methoxy, butoxy, propoxy, or isopropoxy. The alkoxysilyl group may have one to three alkoxy groups attached. Suitable silane coupling agents of the present disclosure may also include a class of thiol-containing silanes that include at least one thiol (SH) group and at least one alkoxysilyl group. Suitable silane coupling agents of the present disclosure may further include a class of thiocyanate-containing silanes that have at least one thiocyanate group (S≡N) and at least one alkoxysilyl group. In some embodiments, the selected silane composition may have a boiling point less than about 250° C. at a pressure of about 0.1 to 10 Torr.

[0018] Table 1 lists some of the silane compositions that may be used as effective coupling agents for metal-organic interfaces (interface 30 in FIG. 1A). These compositions may be particularly suitable for improving the adhesion of organic build-up materials (e.g., ABF, etc.) to the surfaces of metal structures 10 formed by different processes, such as, for example, electroless copper, physical vapor deposition (PVD) copper, electroplated copper, electroplated gold, PVD gold, etc. It should be noted that the list in Table 1 is not an exhaustive list, and suitable silane compositions of the present disclosure may include any composition from the aminosilane, thiol-containing silane, or thiocyanate-containing silane classes described above. Furthermore, in some embodiments, the selected silane composition may have a boiling point below about 250° C. at a pressure of about 0.1 to 10 Torr.

[0019] [Table 1] JPEG2024167161000003.jpg194158JPEG2024167161000004.jpg211158JPEG2024167161000005.jpg217159

[0020] It has been determined that treating the surface of the metal structure 10 with a vapor of at least one of the above silane chemistries (e.g., by depositing a monolayer of the silane composition by vapor phase silane deposition) prior to forming the organic layer 20 thereon improves the adhesive strength of the interface 30. In the vapor phase, the process works with individual molecules to form an ultra-thin monolayer coating on the metal structure 10. The above silane chemistries (including those listed in Table 1) were selected so that they do not react head with tail and therefore do not polymerize and form thick layers. With some chemistries, in the liquid phase, the chemicals may have a tendency to aggregate and form rough layers. Vapor phase deposition has the added benefit that device features can diffuse through small openings as they become smaller in size.

[0021] The silane composition chemistry selected for any particular application will depend on the materials forming the interface, the process conditions, etc., e.g., the materials constituting the metal structure 10 and the organic layer 20, the process conditions, etc. It has been determined that these silane chemistries are effective in improving adhesion on both smooth and rough surfaces and providing good post-deposition film stability. While it is expected that the disclosed silane chemistries or compositions will be suitable for a wide variety of materials used as the metal structure 10 and the organic layer 20 in electronic devices, they have been determined to be particularly effective in improving adhesion between organic layers 20 including ABF and silicon nitride and metal structures 10 including copper. It is also expected that these silane chemistries will be effective in improving the adhesion strength between any metal with a labile oxide and polyamide. It is believed that the functionalization and reactive groups of the disclosed silane chemistries allow for a variety of bonding mechanisms between the metal structure 10 and the organic layer 20. The bonds formed are expected to provide anchoring between the silane groups and the metal surface, as well as planar cross-linking bonds that improve the stability of the monolayer. While all of the above disclosed silane chemistries are effective in improving adhesion between metal structure 10 and organic layer 20, for metal structures 10 containing copper, preferred amines may include silane composition numbers 1, 2, 3, 5, 7, 8, 9, 11 and 12 (Table 1), and preferred compositions containing sulfur may include those numbered 4, 6, 11 and 12 in Table 1.

[0022] In some embodiments, the surface of metal structure 10 may be treated with one or more of the above silane chemicals using a vapor phase silane deposition process. In some embodiments of an exemplary vapor phase silane deposition process, vapor of a desired silane chemical is introduced into a process chamber that supports therein a substrate (e.g., packaging substrate 40 of FIG. 1B) with exposed metal structure 10. The process chamber of any suitable semiconductor processing equipment may be used for the vapor phase silane deposition process. For example, the process chamber of the process apparatus described in any of U.S. Patent Nos. 7,727,588; 8,252,375; 8,361,548; 10,147,617; 10,319,612; 10,490,431; 11,367,640; 11,444,053; 11,335,662; 11,296,049; 11,456,274; and 11,465,225 may be used. Each of these references is incorporated herein in its entirety. In some embodiments, the temperature and pressure of the vapor in the process chamber may be adjusted to maintain the silane chemistry applied in its gas phase. The exact value (or range) of the temperature and pressure that maintains the silane in its gas phase depends on the silane chemistry applied and the application (e.g., the materials involved, etc.). Generally, the metal structure 10 may be exposed to the silane vapor for any desired time (e.g., about 3 minutes to 2 hours). In some embodiments, the metal structure 10 may be exposed to the silane vapor for a period or time of about 10 to 30 minutes or about 15 to 20 minutes. In some embodiments, longer times may be used. A silane monolayer may be formed during the initial stages of exposure (e.g., the first 10 to 20 minutes). Increasing the exposure time may increase the density of the formed monolayer.

[0023] FIG. 2A is a flow chart of an exemplary process 100A that may be used to process a substrate having a metal structure 10 formed thereon. One or more substrates with metal structures 10 may be placed in a process chamber. The surface of the metal structure 10 and / or the substrate may be prepared for silanization (step 110). In some embodiments, the surface preparation may include a wet process, such as, for example, a dilute acid bath or exposing the surface to a dry active plasma to remove contaminants and native oxides from the surface. The process chamber may then be purged to remove oxygen and moisture (step 120). In some embodiments, the process chamber may be exposed to one or more successive vacuum and nitrogen purge cycles to generate a relatively oxygen- and moisture-free environment in the process chamber, as described in more detail in, for example, U.S. Pat. Nos. 7,727,588 and 8,252,375. In some embodiments, heated nitrogen gas may be used. For example, in some embodiments, the process chamber may be exposed to a vacuum (e.g., about 10 Torr for 2 minutes, etc.) and then room temperature or heated nitrogen gas (e.g., 150° C.) one or more times to remove moisture and oxygen from the chamber. If heated nitrogen gas is used, the pre-heated nitrogen gas may warm the surface of the substrate. In embodiments where it is desired not to heat the substrate before the oxygen level is reduced below an acceptable level (e.g., <100 ppm), room temperature (or cooled) nitrogen gas may be used. Vapor of the desired silane composition (e.g., a composition listed in Table 1) may then be admitted to the process chamber (step 130). The chemical vapor injected into the chamber may be evaporated from the silane solution and then admitted to the process chamber or may be delivered by an inert carrier gas (e.g., nitrogen, etc.). For example, heated nitrogen gas may be bubbled through liquid silane of the desired chemical and then admitted to the process chamber. In some embodiments, the silane vapor in step 130 may be evaporated from a pure liquid chemical, or may be evaporated from a solid or semi-solid chemical.As previously described, the exposure time of the silane vapor to the substrate may be varied depending on the reaction rate of the substrate to obtain a dense monolayer film. The temperature and pressure of the chamber may also be adjusted to maintain the silane chemical in the gas phase. After the metal structure 10 has been exposed to the silane vapor for a sufficient time, the chamber may be evacuated to remove excess chemical vapor from the chamber (step 140). In some embodiments, similar to step 120, the process chamber may be alternately exposed to vacuum and nitrogen gas one or more times to completely remove chemical vapor from the chamber. In some embodiments, the chamber may then be vented to the atmosphere (step 150). After the metal structure 10 has been treated with the silane vapor, an organic layer 20 may be formed on the treated metal structure 10 by any suitable process (e.g., deposition, etc.) known in the art. In some embodiments, a conformal coating of the organic layer 20 may be deposited on the substrate surface with the metal structure 10.

[0024] In some embodiments, the process of FIG. 2A may be used in a process apparatus having a pre-heated chamber. In other embodiments of the process apparatus, the process chamber and / or substrate may be heated from room temperature to a process temperature prior to silane treatment (step 130) and then cooled to a temperature safe for exposure to atmospheric oxygen (typically <100C). Such a process may be used to treat oxygen-sensitive metals (e.g., copper). FIG. 2B is a flow chart of another exemplary process that may be used. Process steps in FIG. 2B similar to those described with reference to FIG. 2A are numbered similarly and are not described in detail. In the process 100B of FIG. 2B, after purging the chamber as described with reference to FIG. 2A (step 120), the process chamber and / or substrate may be heated to a process temperature (step 125). The process temperature (e.g., 150° C., 175° C., 200° C., etc.) may depend on the process apparatus used. The metal surface is then treated with vapors of the selected silane (step 130). The substrate is then cooled (step 135) to a safe unloading temperature, for example, below about 100° C. The chamber may then be evacuated (step 140) and vented (step 150). It should be noted that the process described in FIGS. 2A and 2B is merely exemplary, and many variations are possible. For example, the steps described may be performed in a different order, or some steps may be removed. For example, in process 100B of FIG. 2B, steps 135 and 140 may be swapped (e.g., step 140 may be performed before step 135). In some embodiments, processes 100A and 100B may be part of a larger process. For example, in some embodiments, process 100A or 100B may be incorporated into a process used to deposit organic materials on metal structures.

[0025] When metal structure 10 is exposed to silane vapor in step 130, the silane chemical may bond to the surface of metal structure 10. The silane may bond to the metal structure using any mechanism, but in some embodiments in which metal structure 10 comprises copper, the silane chemical may bond to metal structure 10 using one or more of the mechanisms listed in Table 2 below.

[0026] [Table 2]

[0027] The surface of the copper metal structure 10 may be filled with Cu atoms or CuO molecules resulting in different bonding mechanisms as outlined above. The unique feature of the selected silane chemistries is that they can form covalent bonds in areas where the native oxide has been removed and only copper remains, either oxidative or chelate bonds. This "dual functionality" supports whether the selected chemistries are amine or thiol functional. The orientation of the molecules may change from one point on the surface to another, but the molecules will still bond. In some embodiments, each of these selected molecules will use all of the bonding mechanisms at various locations on the surface.

[0028] Adhesion tests (peel tests) were conducted to evaluate the effect of treating exemplary metal structures with the exemplary disclosed silane chemistries of Table 1. Tests were conducted using a TMI peel test apparatus at a 90° peel angle and a peel rate of 50 mm / min. Table 3 below lists details of some of the samples tested.

[0029] [Table 3]

[0030] With reference to Table 3, in the samples designated "AEAPTMS 175C," the process chamber (or substrate) was heated to approximately 175°C in a N2 atmosphere, and after a period of stabilization (typically 2-30 minutes), the chamber was depressurized to base pressure, AE-APTMS silane vapor (silane chemical 1 in Table 1) was introduced into the process chamber, and the substrate was exposed to the vapor for approximately 90 minutes. Similarly, for the samples designated "TMSP-ED 175C," the process chamber / substrate was heated to 175°C and the substrate was treated with vapor of silane chemical 2 in Table 1. For the samples designated "Thermal 175C" and "Thermal 200C," the substrate was heated to 175°C and 200°C, respectively, held at that temperature, and cooled without silane treatment. These samples served as control samples to separate the effects of heating the substrate on surface properties (e.g., by dehydration) from the effects of silane reaction with the substrate surface. The "baseline" samples were not subjected to thermal processing or silane treatment and served as control samples. Tests included samples in which the copper layer was formed by CCL (copper clad laminates) and samples in which the copper layer was formed by PVD (physical vapor deposition) to determine the effect of the silane composition on the surface of copper layers formed by different methods (e.g., CCL Cu and PVD Cu).

[0031] FIG. 3A summarizes the peel test results, and FIG. 3B illustrates the cross-sectional structure of the test samples. In these samples, the interface tested was a copper ABF interface. As can be seen in FIG. 3A, the peel test data shows the achievable adhesion promotion of ABF to both CCL Cu and PVD Cu surfaces. For example, comparison of test results of silane test samples (e.g., AEAPTMS 175C and TMSP-ED 175C samples) with unprocessed samples (e.g., Baseline samples) and thermally processed samples (e.g., Thermal 175C and Thermal 200C samples) shows that silane treatment results in increased adhesion strength at the metal-organic interface. Fracture analysis of the post-test samples confirmed the prediction, showing that samples that did not receive silane treatment suffered adhesive failure at the copper ABF interface, while silane treated samples failed due to cohesive failure in the ABF layer, thereby confirming the effectiveness of the disclosed silane treatment to improve adhesion. Although only the results of samples treated using silane chemistries 1 and 2 (of Table 1) on the copper surface at the Cu-ABF interface are described herein, predictions (e.g., based on the structure and chemical properties of the listed silane compositions, metallic, organic, etc.) indicate that all of the above silane chemistries are expected to be effective in improving adhesion of copper structures to other organic materials (build-up layers, dielectric layers, etc.) used in electronic devices.

[0032] Treating the surface of the metal structure 10 using the disclosed process may improve adhesion between the metal structure 10 and the organic layer 20 in an electronic device. This improved adhesion may result in reduced (or elimination) post-etch delamination from the top and sidewalls of the metal-organic interface that causes interfacial failure and reliability issues in electronic devices. Because improved adhesion is achieved without increasing the roughness of the surface of the metal structure 10, signal loss may also be eliminated.

[0033] Although the disclosed process is described with reference to electronic devices, this is merely exemplary. As will be appreciated by those skilled in the art, the disclosed method embodiments may also be used in other applications. For example, the disclosed method embodiments may also be used for adhesion promotion of metal-organic interfaces in devices used in drug delivery, drug absorption, gas separation, lithium ion batteries, CO2 capture, medical sensors, biological markers, wearable devices, and the like. The disclosed silane treatment method may be incorporated into any suitable process equipment (e.g., process ovens, deposition systems, coating machines, and the like). Furthermore, although several process steps have been disclosed in the above description with reference to specific embodiments, those skilled in the art will recognize that this is merely exemplary and that these steps are applicable to all disclosed embodiments. Other embodiments of the disclosed method will be apparent to those skilled in the art from consideration of the disclosure herein.

Claims

1. 1. A method for improving adhesion at a metal-organic interface in an electronic device, comprising: Providing a substrate having a metal structure formed thereon; treating the surface of the metal structure with vapors of a silane composition comprising: (i.) N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AE-APTMS); (ii.) N,N'-bis[(3-trimethoxysilyl)propyl]ethylenediamine (TMSP-ED); (iii.) Bis(3-trimethoxysilylpropyl)amine, (TMSPA); (iv.) 3-mercaptopropyltrimethoxysilane (MPTMS); (v.) N-(2-aminoethyl)-3-aminopropyl silanetriol, 25% in water (AE-APST); (vi.) 3-Thiocyanatopropyltriethoxysilane, 92% (TCPTES); (vii.) N-(6-aminohexyl)aminomethyltrimethoxysilane; (viii.) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, (ix.) Bis[3-(triethoxysilyl)propyl]disulfide, 90% (TESPDS); (x.) cysteamine, (xi.) 3-aminopropanethiol, (xii.) aminoethylaminopropyl / methylsilsesquioxane in aqueous solution; (xiii.) aminopropylsilsesquioxane (APS) in aqueous solution; (xiv.) (2-diethylphosphatoethyltriethoxysilane), (xv.) (2-diethylphosphatoethyl)methyldiethoxysilane, (xvi.) N-(2-aminoethyl)-3-aminopropyltriethoxysilane, (xvii.) (3-(M-aminophenoxy)propyltrimethoxysilane, (xviii.) N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, (xix.) N-(2-aminoethyl)-3-aminoisobutylmethyldimethoxysilane, (xx.) N-(2-aminoethyl)-3-aminoisobutyldimethylmethoxysilane, (xxi.) 4-aminobutyltriethoxysilane, (xxii.) (aminoethylaminomethyl)phenethyltrimethoxysilane, (xxiii.) N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, (xxiv.) N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane, (xxv.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvi.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvii.) m-aminophenyltrimethoxysilane, or (xxviii.) m-aminophenyltrimethoxysilane; and After treating the surface, coating the treated surface with an organic material. A method comprising:

2. The silane composition comprises: (i.) N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AE-APTMS); (ii.) N,N'-bis[(3-trimethoxysilyl)propyl]ethylenediamine (TMSP-ED); (iii.) Bis(3-trimethoxysilylpropyl)amine, (TMSPA); (v.) N-(2-aminoethyl)-3-aminopropyl silanetriol, 25% in water (AE-APST); (vii.) N-(6-aminohexyl)aminomethyltrimethoxysilane; (viii.) N-(6-aminohexyl)aminopropyltrimethoxysilane; (ix.) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, (xi.) cysteamine, or (xii.) 3-aminopropanethiol The method of claim 1 , comprising at least one of:

3. The method of claim 1 , wherein treating the surface of the metal structure comprises depositing a monolayer of the silane composition on the treated surface.

4. The method of claim 3, wherein the monolayer is about 1 to 10 Angstroms thick.

5. The method of claim 1, wherein the silane composition has a boiling point below about 250° C. at a pressure of about 0.1 to 10 Torr.

6. 10. The method of claim 1, wherein preparing the substrate comprises providing a substrate in a process chamber, the method further comprising purging oxygen or moisture from the process chamber prior to treating the surface with vapor of the silane composition.

7. 7. The method of claim 6, further comprising purging the silane composition vapor from the process chamber after treating the surface with the silane composition vapor.

8. The method of claim 1 , wherein the metal structure comprises copper.

9. The method of claim 8 , wherein the organic material comprises ABF.

10. The method of claim 1 , wherein the substrate is part of a package substrate.

11. The method of claim 1 , wherein the metal structure is an interconnect structure of the electronic device.

12. The method of claim 11 , wherein the interconnect structure is one of an interconnect line, a power plane, a ground plane, a via, or a plated-through hole.

13. 1. A method for improving adhesion at a metal-organic interface in an electronic device, comprising: Providing a substrate having a copper interconnect structure; treating the surface of the copper interconnect structure with vapor of a silane composition having a boiling point below about 250° C. at a pressure of about 0.1 to 10 Torr, the silane composition comprising: the below described (i.) N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AE-APTMS); (ii.) N,N'-bis[(3-trimethoxysilyl)propyl]ethylenediamine (TMSP-ED); (iii.) Bis(3-trimethoxysilylpropyl)amine, (TMSPA); (iv.) 3-mercaptopropyltrimethoxysilane (MPTMS); (v.) N-(2-aminoethyl)-3-aminopropyl silanetriol, 25% in water (AE-APST); (vi.) 3-Thiocyanatopropyltriethoxysilane, 92% (TCPTES); (vii.) N-(6-aminohexyl)aminomethyltrimethoxysilane; (viii.) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, (ix.) Bis[3-(triethoxysilyl)propyl]disulfide, 90% (TESPDS); (x.) cysteamine, (xi.) 3-aminopropanethiol, (xii.) aminoethylaminopropyl / methylsilsesquioxane in aqueous solution; (xiii.) aminopropylsilsesquioxane (APS) in aqueous solution; (xiv.) (2-diethylphosphatoethyltriethoxysilane), (xv.) (2-diethylphosphatoethyl)methyldiethoxysilane, (xvi.) N-(2-aminoethyl)-3-aminopropyltriethoxysilane, (xvii.) (3-(M-aminophenoxy)propyltrimethoxysilane, (xviii.) N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, (xix.) N-(2-aminoethyl)-3-aminoisobutylmethyldimethoxysilane, (xx.) N-(2-aminoethyl)-3-aminoisobutyldimethylmethoxysilane, (xxi.) 4-aminobutyltriethoxysilane, (xxii.) (aminoethylaminomethyl)phenethyltrimethoxysilane, (xxiii.) N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, (xxiv.) N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane, (xxv.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvi.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvii.) m-aminophenyltrimethoxysilane, or (xxviii.) m-aminophenyltrimethoxysilane; and After treating the surface, coating the treated surface with ABF. A method comprising:

14. The method of claim 13 , wherein treating the surface comprises forming a monolayer of the silane composition on the treated surface.

15. The method of claim 13 , wherein coating the engineered surface with an ABF comprises depositing an ABF on the coated surface.

16. 14. The method of claim 13, wherein the substrate is part of a package substrate and the copper interconnect structure is one of an interconnect line, a power plane, a ground plane, a via, or a plated-through hole.

17. The silane composition comprises: (i.) N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AE-APTMS); (ii.) N,N'-bis[(3-trimethoxysilyl)propyl]ethylenediamine (TMSP-ED); (iii.) Bis(3-trimethoxysilylpropyl)amine, (TMSPA); (v.) N-(2-aminoethyl)-3-aminopropyl silanetriol, 25% in water (AE-APST); (vii.) N-(6-aminohexyl)aminomethyltrimethoxysilane; (viii.) N-(6-aminohexyl)aminopropyltrimethoxysilane; (ix.) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, (xi.) cysteamine, or (xii.) 3-aminopropanethiol The method of claim 13, comprising at least one of the following:

18. 1. A method for improving adhesion at a metal-organic interface in an electronic device, comprising: Providing a substrate having a copper interconnect structure, depositing by vapor deposition a monolayer of a silane composition on a surface of the copper interconnect structure, the silane composition (a) comprising at least a primary or secondary amine group and at least one alkoxysilyl group, (b) the alkoxysilyl group may be one of ethoxy, methoxy, butoxy, propoxy, or isopropoxy, (c) the alkoxysilyl group may be one of 1 to 3 alkoxy groups linked together, and (d) having a boiling point less than about 250° C. at a pressure of about 0.1 to 10 Torr; and depositing an ABF on a surface of the copper interconnect structure after depositing the monolayer of the silane composition.

19. The silane composition comprises: (i.) N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AE-APTMS); (ii.) N,N'-bis[(3-trimethoxysilyl)propyl]ethylenediamine (TMSP-ED); (iii.) Bis(3-trimethoxysilylpropyl)amine, (TMSPA); (iv.) 3-mercaptopropyltrimethoxysilane (MPTMS); (v.) N-(2-aminoethyl)-3-aminopropyl silanetriol, 25% in water (AE-APST); (vi.) 3-Thiocyanatopropyltriethoxysilane, 92% (TCPTES); (vii.) N-(6-aminohexyl)aminomethyltrimethoxysilane; (viii.) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, (ix.) Bis[3-(triethoxysilyl)propyl]disulfide, 90% (TESPDS); (x.) cysteamine, (xi.) 3-aminopropanethiol, (xii.) aminoethylaminopropyl / methylsilsesquioxane in aqueous solution; (xiii.) aminopropylsilsesquioxane (APS) in aqueous solution; (xiv.) (2-diethylphosphatoethyltriethoxysilane), (xv.) (2-diethylphosphatoethyl)methyldiethoxysilane, (xvi.) N-(2-aminoethyl)-3-aminopropyltriethoxysilane, (xvii.) (3-(M-aminophenoxy)propyltrimethoxysilane, (xviii.) N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, (xix.) N-(2-aminoethyl)-3-aminoisobutylmethyldimethoxysilane, (xx.) N-(2-aminoethyl)-3-aminoisobutyldimethylmethoxysilane, (xxi.) 4-aminobutyltriethoxysilane, (xxii.) (aminoethylaminomethyl)phenethyltrimethoxysilane, (xxiii.) N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, (xxiv.) N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane, (xxv.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvi.) N-(6-aminohexyl)aminopropyltrimethoxysilane, (xxvii.) m-aminophenyltrimethoxysilane, or (xxviii.) m-aminophenyltrimethoxysilane The method of claim 18, comprising at least one of the following:

20. The silane composition comprises: (i.) N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AE-APTMS); (ii.) N,N'-bis[(3-trimethoxysilyl)propyl]ethylenediamine (TMSP-ED); (iii.) Bis(3-trimethoxysilylpropyl)amine, (TMSPA); (v.) N-(2-aminoethyl)-3-aminopropyl silanetriol, 25% in water (AE-APST); (vii.) N-(6-aminohexyl)aminomethyltrimethoxysilane; (viii.) N-(6-aminohexyl)aminopropyltrimethoxysilane; (ix.) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, (xi.) cysteamine, or (xii.) 3-aminopropanethiol 20. The method of claim 19, comprising at least one of: