Metal-semiconductor-metal photodetector
The asymmetrical Schottky junctions and gradient semiconductor heterostructures in MSM photodetectors address the challenge of high dark current densities, achieving a 28 times reduction in dark current density and improved sensitivity by independently controlling electron and hole current densities.
Patent Information
- Application Number
- JP2024070689
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-24
- Publication Date
- 2024-12-03
AI Technical Summary
Existing MSM photodetectors face challenges in achieving very low dark current densities, especially when using low bandgap semiconductor layers to absorb long wavelength light, due to limitations in modifying Schottky barrier heights and the difficulty in reproducing metal/III-V semiconductor interfaces.
The design of a metal-semiconductor-metal photodetector with asymmetrical Schottky junctions using different semiconductor materials for electron and hole Schottky junctions, along with gradient semiconductor heterostructures, to independently control the Schottky barrier heights and minimize dark current density.
The proposed design significantly reduces dark current density, enhancing sensitivity and performance by allowing independent optimization of electron and hole current densities, resulting in a 28 times lower dark current density compared to symmetric MSM photodetectors.
Smart Images

Figure 2024167162000001_ABST
Abstract
Description
[Technical field]
[0001] This disclosure relates to metal-semiconductor-metal photodetectors. Additionally, this disclosure relates to methods of making such photodetectors. [Background technology]
[0002] Metal-semiconductor-metal (MSM) photodetectors are commonly known as high speed photodetectors and have particularly beneficial applications in optical communication systems, such as optical fiber networks.
[0003] Generally speaking, the effectiveness of a photodetector is measured by its performance in many different parameters. These parameters include the spectral range of response, speed, responsivity (or sensitivity), and dark current density. The speed of a photodetector is the time required for the device to increase its photocurrent to a steady-state value when the incident light is switched on and decrease it when the light is switched off. The sensitivity is also called the responsivity or external quantum efficiency of the photodetector, which is a measure of how much incident light is collected on the photodetector and output as an external current density. It is defined by the ratio of the photocurrent divided by the total incident optical power. The dark current density is commonly defined as the current density flowing in the photodetector when no radiant flux (light source) is incident on the photodetector.
[0004] The ever-increasing speed of optical telecommunications requires faster and more sensitive photodetectors. The increased inherent speed of the photodetectors allows the information rate to be increased without changing either the communication protocol or the architecture of the network. On the other hand, the increased sensitivity of the photodetectors allows the power consumption to be reduced when the data flow increases. In addition, having very fast and sensitive photodetectors may allow the electrical connections currently used for very short range communication, for example between chips on the same printed circuit board, to be replaced by optical connections, reducing their power consumption.
[0005] A conventional prior art MSM photodetector is shown in FIGS. 1A and 1B and is described, for example, in Shi et al. [Non-Patent Document 1].
[0006] The MSM photodetector is a flat (planar) structure having several layers, including a semiconductor layer 10 and first and second metal electrodes 11 , 12 , disposed on a substrate 15 .
[0007] The semiconductor layer 10 has a band gap small enough to absorb incident light in the operating spectrum range, thereby exciting an electron from the valence band to the conduction band for each absorbed photon. Thus, a pair of free carriers is generated, i.e., an electron in the conduction band and a hole in the valence band. The free carriers are driven by the local electrostatic field towards the electrodes, where they are collected and contribute to the external current. For applications in optical communication systems with operating wavelengths, such as about 1.3 μm or about 1.5 μm, low band gap semiconductor materials, such as germanium, III-V compounds, or II-VI compounds, are suitable because their band gaps are smaller than the energy of the incident photons, i.e., 0.95 eV and 0.82 eV, respectively.
[0008] As shown in Figures 1A and 1B, first and second metal electrodes 11, 12 are deposited on either side of the semiconductor layer ("vertical arrangement", Figure 1A) or on top of the semiconductor layer ("horizontal arrangement", Figure 1B). The electrodes can be structured (as shown in Figures 1A and 1B) to improve optical coupling between the device and the incoming light. A bias voltage V is applied between the first electrode 11 (e.g., a cathode) and the second electrode 12 (e.g., an anode).
[0009] In an MSM photodetector, the metal electrode is configured with the semiconductor layer to form a Schottky junction. A Schottky junction, also referred to herein as a Schottky barrier or Schottky contact, is a potential barrier for electrons or holes formed at a metal-semiconductor interface. Schottky barriers have rectifying properties, making them suitable for use as diodes. Thus, in a Schottky junction, for a positive bias voltage, the current increases exponentially with voltage, while the Boltzmann constant k B If the temperature is T, the current for a negative bias voltage is several kΩ. B It is approximately constant with voltage when it is greater than T (thermal energy). In the lateral configuration shown in Figure 1B, both electrodes (anode and cathode) are on the same semiconductor layer. The electrodes are "interdigitated", so that a bias voltage V is applied between two adjacent Schottky junctions.
[0010] One of the main characteristics of a Schottky junction is the height of the potential barrier. B For an electronic Schottky junction in which the current flow under the potential T is dominated by a bunch of electrons crossing the junction, the potential barrier height is the height of the potential barrier seen by electrons injected into the semiconductor layer, and is defined herein as φ e This is called the "electron Schottky barrier height". BFor a hole Schottky junction in which the current flow under the potential T is dominated by a bunch of holes crossing the junction, the potential barrier height is the height of the potential barrier seen by holes injected into the semiconductor layer, and is defined herein as φ h This is called the "hole Schottky barrier height". The Schottky barrier height φ e and φ h The value of depends on the combination of metal and semiconductor at the interface.
[0011] 2A shows a theoretical band diagram of a prior art MSM photodetector using the same metal for both electrodes, as described, for example, in Ito et al. [Non-Patent Document 2]. For a graphical conversion of the band diagram, see, for example, Darling et al. [Non-Patent Document 3]. FIG. 2B shows a band diagram of a prior art MSM photodetector using different metals for both electrodes, as described, for example, in Fresser et al. [Non-Patent Document 4] and U.S. Patent Publication 2006 / 0133636.
[0012] This band diagram, in a 1D approximation, diagrammatically represents the energy levels (E axis) along an arbitrarily chosen line of constant static current density between two electrodes (x axis). Such an arbitrarily chosen line of constant static current density between two electrodes is indicated by dashed line 20 in Figures 1A and 1B. E F denotes the Fermi level in the metallic part, and E C denotes the minimum energy of the semiconductor conduction band, and E V denotes the maximum energy of the semiconductor valence band.
[0013] For both the embodiments of Figures 2A and 2B, band diagrams are shown for the case where the bias voltage applied between the electrodes is V=0 (left) and for the case where V≠0 (right).
[0014] In the example of FIG. 2A, the electrodes 11, 12 (in this example the cathode and anode, respectively) are formed by the same metal deposited on the semiconductor layer, and at V=0, the Fermi level of the metal (E F) is located at the same energy level (along the E axis) at both metal-semiconductor interfaces. As a result of having the same metal deposited on top of the semiconductor layer, for a given bias voltage V ≠ 0, the potential barrier seen by an electron injected into the semiconductor layer (electron Schottky barrier height φ e ) and the potential barrier seen by the holes injected into the semiconductor layer (hole Schottky barrier φ h ) is the same for both electrodes.
[0015] In an MSM photodetector, the dark current density I at a given bias voltage V ≠ 0 dark is the current density I of electrons injected into a semiconductor by a Schottky junction with a metal part at a negative potential e and the current density I of holes injected into the semiconductor by a Schottky junction with a metal part at a positive potential. h Each of these current densities is controlled by the Schottky barrier through different possible mechanisms: tunneling current, field-assisted tunneling current, and thermionic current. With a moderate reverse bias voltage (i.e., a few kΩ B At 100 kV, these current densities can be written as a good approximation: I e =I 0e exp[-φ e / k B T], where I 0e =A * e T 2 [exp(qV / k B T)-1] I h =I 0h exp[-φ h / k B T], where I 0h =A * h T 2 [exp(qV / k B T)-1] Here, A * e (resp.) A * h) is the effective Richardson constant for electron (resp. hole) emission [3].
[0016] k B T is about 25 meV at room temperature, so I e and I h is very sensitive to the barrier height. The aim is to reduce the dark current density I dark The aim is to make the
[0017] However, in such MSM photodetectors employing Schottky contacts with the same metal, the Schottky barrier height (holes and electrons) is limited by the band gap of the semiconductor. In fact, the sum of the two barrier heights, φ e +φ h is the band gap E of the semiconductor G Therefore, for example, the height of the potential barrier seen by an electron is φ e (e.g., by changing the properties of the metal) results in a change in the height of the potential barrier seen by the hole, φ h is changed to be equal to and opposite to I e is φ e is a decreasing function of I h is φ e Therefore, the sum of these two current densities has a minimum value that corresponds to the best optimization of the photodetector.
[0018] As an example, applicants have demonstrated that the dark current density of an MSM photodetector using Au / Ti / InP (gold / titanium / indium phosphide) as a Schottky contact is 129 fA.μm -2 It was determined that it cannot be less than this. In practice, it is difficult to define the conditions (nature of the metal, treatment of the semiconductor surface, etc.) for producing a Schottky contact that corresponds to such a minimum. At best, it is possible to approach such a minimum, which would result in an increased dark current density compared to the absolute minimum defined above.
[0019] In the example of FIG. 2B, a different metal is used for each electrode.
[0020] In such an embodiment, one metal electrode has a high electron Schottky barrier height (φ e ), and the other electrode may be selected to have a high hole Schottky barrier height (φ h ) The dark current may decay to reach a value lower than the minimum value mentioned above.
[0021] However, the Fermi level trapping at the metal / semiconductor interface observed in III-V semiconductors [5] does not provide access to a dynamic range for modifying the barrier height as large as that observed for silicon, for example. Indeed, the possibilities for modifying the Schottky barrier height in such semiconductors are rather limited due to the difficulties in producing metal / III-V semiconductor interfaces in a reproducible and industrial manner. [Prior art documents] [Patent documents]
[0022] [Patent Document 1] U.S. Patent No. 5,780,916 [Non-patent literature]
[0023] [Non-Patent Document 1] CX.Shi et al., IEEE Trans.Electron.Dev.39(5)1028(1992) [Non-Patent Document 2] MI Ito et al., Contacts, IEEE J.Quant. Elec.QE-22(7), 1073(1986) [Non-Patent Document 3] RBDarling et al.,J.App.Phys. 673152(1990) [Non-Patent Document 4] HSFresser et al., J.Vac.Sci. Technol.B13(6)2553(1995) [Non-Patent Document 5] N. Newman et al., J. Vac. Sci. Technol. B4(4)931(1986) Summary of the Invention [Problem to be solved by the invention]
[0024] Thus, there is a need for alternative designs of MSM photodetectors that exhibit very low dark current densities even when using low bandgap semiconductor layers to absorb long wavelength light. [Means for solving the problem]
[0025] In the following, the term "comprises" is synonymous with (has the same meaning as) "includes" and "contains", is inclusive and open, and does not exclude other undescribed components. Furthermore, the terms "about" and "substantially" when indicating a numerical value in this disclosure are synonymous with (has the same meaning as) a range that is included in 80% to 120%, preferably 90% to 110% of the numerical value.
[0026] According to a first aspect, the present disclosure provides a metal-semiconductor-metal photodetector configured to detect incident light of a given wavelength range, comprising: an absorbing semiconductor layer configured to absorb light within the given wavelength range; a first semiconductor layer in electrical contact with the absorbing semiconductor layer, the first semiconductor layer being made of a first semiconductor material having a first bandgap; a first metal electrode configured to be electrically connected to a negative pole of a voltage generator, the first metal electrode being in electrical contact with the first semiconductor layer, the first semiconductor layer being disposed between the first metal electrode and the absorbing semiconductor layer, the first metal electrode and the first semiconductor layer being configured to create an electronic Schottky junction under application of a bias voltage; a second semiconductor layer in electrical contact with the absorbing semiconductor layer, the second semiconductor layer being made of a second semiconductor material having a second bandgap different from the first semiconductor material; a second metal electrode configured to be electrically connected to a positive pole of the voltage generator, the second metal electrode being in electrical contact with the second semiconductor layer, the second semiconductor layer being disposed between the second metal electrode and the absorption, the second metal electrode and the second semiconductor layer being configured to generate a hole Schottky junction under application of a bias voltage.
[0027] In an electron Schottky junction, the bias voltage, e.g., several k B Under application of a bias voltage greater than T, i.e., greater than about 0.1 V at ambient temperature, current flow is dominated by a flux of electrons crossing the junction.
[0028] In a hole Schottky junction, the bias voltage, for example several kΩ B Under application of a bias voltage greater than T, i.e., greater than about 0.1 V at ambient temperature, current flow is dominated by a flux of holes across the junction.
[0029] Such an initial configuration allows for separately minimizing two components of the dark current density at a given bias voltage: one component is the current density of electrons injected into the absorbing semiconductor layer by the electron Schottky junction, and the other component is the current density of holes injected into the absorbing semiconductor layer by the hole Schottky junction. This is made possible by the asymmetry between the first semiconductor layer, also referred to herein as the "electron Schottky semiconductor layer," and the second semiconductor layer, also referred to herein as the "hole Schottky semiconductor layer," which are made of different semiconductor materials.
[0030] Additionally, the first semiconductor material and the first metal electrode have an electronic Schottky barrier φ such that the electronic Schottky junction is greater than half the first band gap of the first semiconductor layer. e and the second semiconductor material and the second metal electrode are selected to have a hole Schottky barrier φ such that the hole Schottky junction is greater than half the second band gap of the second semiconductor layer. h In comparison with the prior art photodetectors, the electron current density I e and the hole current density I h can be reduced, resulting in reduced dark current and better sensitivity.
[0031] According to one or more embodiments, the absorbing semiconductor layer comprises a semiconductor material selected from germanium, III-V compounds, or II-VI compounds. For example, the absorbing semiconductor layer comprises a semiconductor material selected from InGaAlAs alloys, such as InGaAs (band gap Eg=0.79 eV) for detection up to 1.6 μm, InAs / (In,Ga)Sb type II superlattices, or HgCdTe alloys for larger wavelengths (up to 14 μm).
[0032] According to one or more embodiments, the absorbing semiconductor layer comprises silicon.
[0033] According to one or more embodiments, at least one of the first and second semiconductor materials is selected from an InGaAlAs alloy, such as, for example, InAlAs; an InGaAs, such as, for example, InP; or an HgCdTe alloy, such as, for example, CdTe.
[0034] In all embodiments, the first and second semiconductor materials are different, and each of the first and second semiconductor materials is different from the semiconductor material of the absorbing semiconductor layer.
[0035] According to one or more embodiments, at least one of the first metal electrode and the second metal electrode includes one or more of the following materials: titanium, platinum, aluminum, chromium, tungsten, molybdenum, and tungsten silicide (WSi x ), molybdenum disilicide (MoSi x ) and other compounds.
[0036] According to one or more embodiments, at least one of the first metal electrode and the second metal electrode comprises a stack of different metals.
[0037] According to one or more embodiments, the photodetector further includes a first graded semiconductor heterostructure in contact with a surface of the absorbing semiconductor layer and a surface of the first semiconductor layer.
[0038] According to one or more embodiments, the photodetector further includes a second graded semiconductor heterostructure in contact with a surface of the absorbing semiconductor layer and a surface of the second semiconductor layer.
[0039] As used herein, a graded semiconductor heterostructure is a stack of several semiconductor layers that exhibit a gradient in bandgap ranging from a value close to that of the absorbing semiconductor layer at its interface with the absorbing semiconductor layer to a value close to that of the semiconductor layer at the opposite interface. Graded semiconductor heterostructures may be obtained by stacking several layers of semiconductors with different bandgaps or by varying the composition of a quaternary semiconductor alloy (e.g., InAlGaAs or InGaAsP) in a graded manner.
[0040] Graded semiconductor heterostructures can eliminate the conduction and valence band discontinuities that may exist between two different semiconductor layers. By reducing the parasitic potential barrier, better collection of the photogenerated carriers of charge (electrons and holes) is obtained, thus resulting in better quantum efficiency of the photodetector.
[0041] According to one or more embodiments, the photodetector further includes at least one of an interface layer in contact with a surface of the first semiconductor layer and a surface of the first metal electrode, and an interface layer in contact with a surface of the second semiconductor layer and a surface of the second metal electrode.
[0042] For example, the interface layer may include an oxide, such as silicon oxide, indium phosphide oxide, or InAlAs oxide, which may be used to control the Schottky barrier of the Schottky junction by adjusting its thickness.
[0043] According to one or more embodiments, the first metal electrode is disposed on a first side of the absorbing semiconductor layer and the second metal electrode is disposed on a second side of the absorbing semiconductor layer opposite the first side, which is referred to herein as a vertical arrangement of a photodetector.
[0044] In such a vertical arrangement, a first graded semiconductor heterostructure may be disposed in contact with a surface of the absorbing semiconductor layer and a surface of the first semiconductor layer, and / or a second graded semiconductor heterostructure may be disposed in contact with a surface of the absorbing semiconductor layer and a surface of the second semiconductor layer.
[0045] According to one or more embodiments, the first metal electrode and the second metal electrode are disposed on the same side of the absorbing semiconductor layer, which is referred to herein as a lateral arrangement of the photodetector.
[0046] In such a lateral arrangement, a first graded semiconductor heterostructure may be disposed in contact with a surface of the absorbing semiconductor layer and a surface of the first semiconductor layer, or a second graded semiconductor heterostructure may be disposed in contact with a surface of the absorbing semiconductor layer and a surface of the second semiconductor layer.
[0047] Additionally, a third graded semiconductor heterostructure may be disposed in contact with a surface of the first semiconductor layer and a surface of the second semiconductor layer.
[0048] According to a second aspect, the present disclosure provides a method for producing a method for a method of manufacturing a semiconductor device comprising: a photodetector according to a first aspect; and a voltage generator, wherein the first metal electrode is electrically connected to a negative terminal of the voltage generator and the second metal electrode is electrically connected to a positive terminal of the voltage generator.
[0049] According to a third aspect, the present specification refers to a method of manufacturing a photodetector according to the first aspect.
[0050] In some embodiments, the method according to the second aspect comprises: depositing a semiconductor stack on a substrate, the semiconductor stack including the absorbing semiconductor layer, the first semiconductor layer, and the second semiconductor layer; depositing a metal layer on the semiconductor stack to form the first metal electrode; flipping the substrate together with the semiconductor stack onto a host substrate; and etching the substrate and depositing a metal layer to form the second electrode.
[0051] According to one or more embodiments, the semiconductor stack further includes at least one of a first gradient semiconductor heterostructure in contact with a surface of the absorbing semiconductor layer and a surface of the first semiconductor layer, and a second gradient semiconductor heterostructure in contact with a surface of the absorbing semiconductor layer and a surface of the second semiconductor layer. [Brief description of the drawings]
[0052] Other advantages and features of the invention will become apparent from reading the following description illustrated by the drawings in which:
[0053] [Figure 1A] FIG. 1, as already described, is a cross-sectional view of a prior art MSM photodetector (vertical arrangement). [Figure 1B] FIG. 1, as already described, is a cross-sectional view of a prior art MSM photodetector (lateral arrangement). [Figure 2A] FIG. 1 is a theoretical energy band diagram for a prior art MSM photodetector that uses the same metal for both electrodes, as previously discussed. [Figure 2B] FIG. 1 is a theoretical energy band diagram for a prior art MSM photodetector using different metals for both electrodes, as previously described. [Figure 3A] FIG. 1 illustrates a photodetection circuit with a cross-sectional view of an MSM photodetector (vertical arrangement) according to an embodiment herein. [Figure 3B] FIG. 1 illustrates a photodetection circuit with a cross-sectional view of an MSM photodetector (horizontal arrangement) according to embodiments herein. [Figure 4A] FIG. 2 is a theoretical energy band diagram for an MSM photodetector using the same metal for both electrodes and a different semiconductor material at the metal-semiconductor interface according to embodiments herein. [Figure 4B]FIG. 2 is a theoretical energy band diagram for an MSM photodetector according to embodiments herein using different metals and different semiconductor materials at the metal-semiconductor interface. [Figure 5A] FIG. 1 illustrates a photodetection circuit with a cross-sectional view of an MSM photodetector (vertical arrangement) according to an embodiment herein. [Figure 5B] FIG. 5B is a theoretical energy band diagram for the MSM photodetector shown in FIG. 5A according to embodiments herein. [Figure 6A] FIG. 1 illustrates a photodetection circuit with a cross-sectional view of an MSM photodetector (horizontal arrangement) according to embodiments herein. [Figure 6B] FIG. 2 is a theoretical energy band diagram for a lateral geometry MSM photodetector according to an embodiment herein. [Figure 7A] FIG. 1 illustrates a photodetection circuit with a cross-sectional view of an MSM photodetector (horizontal arrangement) according to embodiments herein. [Figure 7B] FIG. 2 is a theoretical energy band diagram for a lateral geometry MSM photodetector according to an embodiment herein. [Figure 8] FIG. 2 shows a curve illustrating calculated dark current density as a function of electron barrier height for an embodiment of a photodetector according to the present disclosure. [Figure 9A] 1A-1C illustrate a first step of a method for fabricating an asymmetric MSM photodetector according to embodiments herein. [Figure 9B] FIG. 2 illustrates a second step of a method for fabricating an asymmetric MSM photodetector according to embodiments herein. [Figure 9C] FIG. 13 illustrates a third step of a method for fabricating an asymmetric MSM photodetector according to embodiments herein. [Figure 9D] FIG. 13 illustrates a fourth step of a method for fabricating an asymmetric MSM photodetector according to embodiments herein. [Figure 9E] FIG. 13 illustrates a fifth step of a method for fabricating an asymmetric MSM photodetector according to embodiments herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0054] 3A and 3B show photodetection circuits with two configurations of MSM photodetectors according to embodiments herein. In these embodiments, two metal electrodes 330, 340 are deposited on either side of the absorbing semiconductor layer 325 ("vertical configuration", FIG. 3A) or on the same side of the absorbing semiconductor layer 325 ("horizontal configuration", FIG. 3B). V is the bias voltage applied to the metal electrodes 330, 340, and line 20 shows an arbitrary line that follows the current density line between the two electrodes in a 1D approximation.
[0055] The MSM photodetector is configured to detect incident light in a given wavelength range, such as between about 1.3 μm and about 1.5 μm, for example about 1.3 μm or about 1.5 μm, for optical communications applications.
[0056] 3A and 3B, the MSM photodetector includes a support 310 and a semiconductor stack including an absorbing semiconductor layer 325, a first semiconductor layer 321 in electrical contact with the absorbing semiconductor layer, and a second semiconductor layer 322 in electrical contact with the absorbing semiconductor layer. The absorbing semiconductor layer 325 is configured to absorb light in the wavelength range.
[0057] In a vertical arrangement, such as shown in Figure 3A, the semiconductor stack is transferred onto a host substrate. Support 310 corresponds to the host substrate and can be any mechanical support, such as metal (e.g., Al or Cu), glass (e.g., SiO2), or semiconductor (e.g., silicon).
[0058] In a lateral arrangement, such as that shown in FIG. 3B , the support 310 may comprise, for example, an indium phosphide (InP) substrate for growth of InGaAlAs and / or InGaAsP alloys, or a gallium arsenide (GaAs) substrate for growth of AlGaAs alloys, or a CdZnTe substrate for growth of HgCdTe alloys, or a GaSb or InAs substrate for growth of a type-2 superlattice GaSb / InAs.
[0059] The first semiconductor layer 321 is made of a first semiconductor material and is in electrical contact with a first metal electrode 340 (the cathode in the examples of Figures 3A and 3B), thus forming a first semiconductor-metal interface in these embodiments. The first metal electrode 340, together with the first semiconductor layer 321, defines an electron Schottky barrier height φ e Thus, in this specification, the first semiconductor layer 321 is also referred to as an "electronic Schottky semiconductor layer."
[0060] The second semiconductor layer 322 is made of a second semiconductor material different from the first semiconductor material and is in electrical contact with a second metal electrode 330 (the anode in the examples of Figures 3A and 3B), thus forming a second semiconductor-metal interface in these embodiments. The second metal electrode 330 is formed of a metal that may or may not be the same as the metal of the first metal electrode 340. The second electrode 330 together with the second semiconductor layer 322 defines a Schottky barrier height φ seen by holes. h Thus, in this specification, the second semiconductor layer 322 is also referred to as a "hole Schottky semiconductor layer."
[0061] Figures 4A and 4B show energy band diagrams for the embodiment of the MSM photodetector shown in Figures 3A and 3B. The energy band diagrams are shown for V=0 (left) and V≠0 (right) with a bias voltage applied between the first and second metal electrodes 340, 330. In the embodiment of Figure 4A, the first and second electrodes 340, 330 are made of the same metal, while in the embodiment of Figure 4B, the first and second electrodes 340, 330 are made of different metals.
[0062] As shown in FIG. 4A, at V=0, the Fermi level E F is located at the same energy level (along the E axis) at both metal-semiconductor interfaces, but E C and E Vare not parallel, indicating the existence of a quasi-electric field within the semiconductor stack. In the energy band diagrams, the dashed lines are merely guides to the eye, and no semiconductor stack is defined between the two interfaces in these schemes. In operation, a bias voltage V is applied to establish a collection field for the collection of photocarriers. As shown in Figure 4A, due to the different semiconductor materials at the metal-semiconductor interface, the potential barrier seen by electrons injected into the first semiconductor layer (electron Schottky barrier height φ e ) and the potential barrier seen by the holes injected into the second semiconductor layer (hole Schottky barrier height φ h ) can be controlled independently. Thus, in this case, the sum of the two barrier heights is no longer fixed at a value equal to the semiconductor bandgap as in the prior art. Conversely, the present disclosure allows each of these barrier heights to be greater than half the bandgap of the corresponding semiconductor layer in contact with each of these electrodes.
[0063] 4B shows an energy band diagram of an MSM photodetector, such as that shown in FIG. 3A and FIG. 3B, using different metals for both electrodes (330 and 340) and different semiconductor materials for the electron Schottky semiconductor layer 321 and the hole Schottky semiconductor layer 322 at the metal-semiconductor interface. In this case, one metal-semiconductor interface is selected to have a high electron Schottky barrier height and the other metal-semiconductor interface is selected to have a high hole Schottky barrier height. Thus, the two potential barriers can be maximized independently, so that both the electrons and holes injected from the electrodes into the semiconductor layers 321, 322, respectively, have a higher barrier height to overcome compared to FIG. 2B.
[0064] Therefore, the current at the two Schottky junctions is drastically reduced, as is the dark current density of the MSM photodetector.
[0065] 3A and 3B, an asymmetry is thus obtained between the metal electrode 340-electron Schottky semiconductor layer 321 interface and the metal electrode 330-hole Schottky semiconductor layer 322 interface. This asymmetry makes it possible to separately minimize the current density of electrons injected into the electron Schottky semiconductor layer 321 by the electron Schottky junction and the hole current injected into the hole Schottky semiconductor layer 322 by the hole Schottky junction.
[0066] A person skilled in the art can then determine, among the available materials, the semiconductor material / metal pair that forms a Schottky junction with the weakest current density (electrons and holes) under reverse bias. For example, for each of the two junctions (electrons and holes), a specific structure for testing can be made. Such a structure may, for example, include a metal layer to be tested and a Schottky semiconductor layer, the latter epitaxially grown on a doped semiconductor and having an N-type to test the electron Schottky semiconductor-metal interface, or a P-type to test the hole Schottky semiconductor-metal interface.
[0067] As an example, the test procedure described above made it possible to determine the barrier heights of Schottky junctions created by Ti / Au contacts on InAlAs for electrons and on InP for holes.
[0068] The inventors have determined that the barrier height seen from the electron in a Schottky InAlAs / Ti / Au junction is φ e = 735 meV, i.e., dark current density I e = 4fA.μm -2 It was decided that:
[0069] The inventors further defined the barrier height as seen from the hole in the Schottky InP / Ti / Au junction as φ h = 786 meV, i.e., dark current density I h =0.5fA.μm -2 It was decided that:
[0070] Therefore, the dark current density for the MSM photodetector (the sum of the electron current injected at the InAlAs / Ti / Au junction and the hole current injected at the InP / Ti / Au junction) is 4.5 fA.μm -2 i.e., 1 / 28th of the absolute minimum current density of a symmetric detector described for a symmetric MSM photodetector using Au / Ti / InP (gold / titanium / indium phosphide) as the Schottky contact.
[0071] 5A, 6A, and 7A show another embodiment of an MSM photodetector according to embodiments of the present specification, and 5B, 6B, and 7B show band diagrams of the MSM photodetector according to embodiments of the present specification. In 5B, 6B, and 7B, the electric field in each layer is zero for simplicity.
[0072] FIG. 5A illustrates another embodiment of an MSM photodetector according to embodiments herein in a vertical arrangement.
[0073] 5A includes a semiconductor stack 320 having an absorbing semiconductor layer 325, an electron Schottky semiconductor layer 321, and a hole Schottky semiconductor layer 322. The semiconductor stack further includes a first graded semiconductor heterostructure 326 in contact with a surface of the absorbing semiconductor layer 325 and in contact with a surface of the electron Schottky semiconductor layer 321, and a second graded semiconductor heterostructure 327 in contact with a surface of the absorbing semiconductor layer 325 and a surface of the hole Schottky semiconductor layer 322. In such a vertical arrangement, metal electrodes 330, 340 are disposed on either side of the semiconductor stack and are in electrical contact with the hole Schottky semiconductor layer 322 and the electron Schottky semiconductor layer 321, respectively.
[0074] For example, if absorbing semiconductor layer 325 is made of InGaAs and electron Schottky semiconductor layer 321 is made of InAlAs, first graded semiconductor heterostructure 326 may include an alloy of InGaAlAs and thus may have a bandgap that ranges from the bandgap of InAlAs to the bandgap of InGaAs.
[0075] The first graded semiconductor heterostructure 326 allows for smoothing of the conduction and valence band discontinuities that exist between the absorbing semiconductor layer 325 and the electron Schottky semiconductor layer 321. By limiting the resulting parasitic potential barrier, better collection of photogenerated charge carriers may occur.
[0076] On the other hand, if the absorbing semiconductor layer 325 is made of InGaAs and the hole Schottky semiconductor layer 322 is made of InP, the second graded semiconductor heterostructure 327 may comprise an alloy of InGaAsP and thus may have a bandgap that ranges from the bandgap of InP to the bandgap of InGaAs.
[0077] It is noted that in some embodiments, the MSM photodetector may include only one of the first graded semiconductor heterostructure or the second graded semiconductor heterostructure, although better performance is expected with both graded semiconductor heterostructures.
[0078] FIG. 5B shows the band diagram of the MSM photodetector shown in FIG. 5A. The semiconductor stack has a band gap E g and an absorbing semiconductor layer 325 having a band gap E g1 and an electron Schottky semiconductor layer 321 having a band gap E g2 a first graded semiconductor heterostructure 326 disposed between the electron Schottky semiconductor layer 321 and the absorbing semiconductor layer 325; and a second graded semiconductor heterostructure 327 disposed between the hole Schottky semiconductor layer 322 and the absorbing semiconductor layer 325.
[0079] For example, electrodes 330, 340 include a stack of two metal layers: a titanium layer and a gold layer. The titanium layer in the first metal electrode 340 creates an electron Schottky barrier with the first semiconductor layer 321, and the titanium layer in the second metal electrode 330 creates a hole Schottky barrier with the second semiconductor layer 322. The gold layer is used as an inert metal to protect the titanium and is also a very good conductor.
[0080] The absorbing semiconductor layer 325 has a band gap E g The electron Schottky semiconductor layer 321 is made of InGaAs having a band gap E g1 = 1.45 eV, so that at the titanium-InAlAs interface, there is a high potential barrier φ against electrons injected from titanium into InAlAs. e = 0.73 eV. g2 = 1.35 eV, so there is a high potential barrier φ for holes injected from titanium into InP at the titanium-InP interface. h = 0.79 eV.
[0081] In FIG. 5B, ΔE C1 and ΔE C2 are the energy difference between the conduction bands of the electron Schottky semiconductor layer 321 and the absorbing semiconductor layer 325, and the energy difference between the conduction bands of the hole Schottky semiconductor layer 322 and the absorbing semiconductor layer 325, respectively. For example, in the above example, ΔE C1 = 0.52 eV, ΔE C2 =0.25 eV.
[0082] Furthermore, ΔE V1 and ΔE V2 are the energy difference between the valence bands of the absorbing semiconductor layer 320 and the electron Schottky semiconductor layer 321, and the energy difference between the valence bands of the absorbing semiconductor layer 325 and the hole Schottky semiconductor layer 322, respectively. For example, in the above example, ΔE V1 = 0.19 eV, ΔE V2 =0.35 eV.
[0083] In this example too, the dark current is significantly reduced compared to the prior art symmetric MSM photodetectors (28 times lower compared to the Au / Ti / InP junctions of the symmetric MSM photodetectors), and fabrication is simplified since the same metal can be used for both electrodes.
[0084] FIG. 6A illustrates another embodiment of an MSM photodetector according to embodiments herein in a lateral arrangement.
[0085] The MSM photodetector shown in Figure 6A includes a semiconductor stack 320 and two electrodes 330, 340 disposed on the semiconductor stack. The semiconductor stack 320 includes an absorbing semiconductor layer 325, an electron Schottky semiconductor layer 321 in electrical contact with the first electrode 340, and a hole Schottky semiconductor layer 322 in electrical contact with the second electrode 330. In the example of Figure 6A, the hole Schottky semiconductor layer 322 is disposed between the electron Schottky semiconductor layer 321 and the absorbing semiconductor layer 325. Furthermore, the electron Schottky semiconductor layer 321 is configured such that the second electrode 330 can be disposed in contact with the hole Schottky semiconductor layer 322. Advantageously, in the example of Figure 6A, the semiconductor stack further includes a graded semiconductor heterostructure 327 in contact with a surface of the absorbing semiconductor layer 325 and also in contact with a surface of the hole Schottky semiconductor layer 322. It should be noted that the semiconductor stack may further include a graded semiconductor heterostructure (not shown in FIG. 6A) in contact with a surface of the electron Schottky semiconductor layer 321 and also in contact with a surface of the hole Schottky semiconductor layer 322.
[0086] 6B depicts a band diagram for the MSM photodetector shown in FIG. 6A, further comprising a graded semiconductor heterostructure in contact with the surface of the electron Schottky semiconductor layer 321 and in contact with the surface of the hole Schottky semiconductor layer 322. As detailed above, the semiconductor stack has a bandgap E g and an absorbing semiconductor layer 325 having a band gap E g1 and an electron Schottky semiconductor layer 321 having a band gap E g2and a hole Schottky semiconductor layer 322 having an absorbing semiconductor layer 325. In such an embodiment, the electron Schottky semiconductor 321 is grown on the hole Schottky semiconductor 322. Further, a graded semiconductor heterostructure 327 is disposed between the hole Schottky semiconductor layer 322 and the absorbing semiconductor layer 325, and a graded semiconductor heterostructure (not shown in FIG. 6A ) is disposed between the electron Schottky semiconductor layer 321 and the hole Schottky semiconductor layer 322.
[0087] For example, the electrodes 330, 340 are made of titanium / gold. The absorbing semiconductor layer 325 has a band gap E g The electron Schottky semiconductor layer 321 is made of InGaAs having a band gap E g1 = 1.45 eV, so that at the titanium-InAlAs interface, there is a high potential barrier φ against electrons injected from titanium into InAlAs. e = 0.73 eV. g2 = 1.35 eV, so that at the titanium-InP interface, there is a high potential barrier φ for holes injected from titanium into InP. h = 0.79 eV.
[0088] In FIG. 6B, ΔE C2 is the energy difference between the conduction bands of the hole Schottky semiconductor layer 322 and the absorbing semiconductor layer 325. ΔE C3 is the energy difference between the conduction bands of the electron Schottky semiconductor layer 321 and the hole Schottky semiconductor layer 322. For example, in the above example, ΔE C2 =0.25eV, ΔE C3 =0.34 eV.
[0089] Furthermore, ΔE V2 is the energy difference between the valence bands of the absorbing semiconductor layer 325 and the hole Schottky semiconductor layer 322. ΔE V3is the energy difference between the valence bands of the electron Schottky semiconductor layer 321 and the hole Schottky semiconductor layer 322. For example, in the above example, ΔE V2 = 0.35 eV and ΔE V3 =0.19 eV.
[0090] A similar reduction in dark current is observed compared to the prior art symmetric MSM photodetector.
[0091] FIG. 7A illustrates another embodiment of an MSM photodetector according to embodiments herein in a lateral arrangement.
[0092] The MSM photodetector shown in Figure 7A includes a semiconductor stack 320 and two electrodes 330, 340 arranged on top of the semiconductor stack. The semiconductor stack includes an absorbing semiconductor layer 325, an electron Schottky semiconductor layer 321 in electrical contact with a first electrode 340, and a hole Schottky semiconductor layer 322 in electrical contact with a second electrode 330. In the example of Figure 7A, the electron Schottky semiconductor layer 321 is arranged between the hole Schottky semiconductor layer 322 and the absorbing semiconductor layer 325. Furthermore, the hole Schottky semiconductor layer 322 is structured such that the first electrode 340 can be arranged in contact with the electron Schottky semiconductor layer 321. Advantageously, in the example of Figure 7A, the semiconductor stack further includes a graded semiconductor heterostructure 326 in contact with a surface of the absorbing semiconductor layer 325 and also in contact with a surface of the electron Schottky semiconductor layer 321. The semiconductor stack may further include a graded semiconductor heterostructure (not shown in FIG. 7A) in contact with a surface of the electron Schottky semiconductor layer 321 and also in contact with a surface of the hole Schottky semiconductor layer 322.
[0093] 7B depicts a band diagram for the MSM photodetector shown in FIG. 7A, where a graded semiconductor heterostructure is further disposed in contact with a surface of the electron Schottky semiconductor layer 321 and in contact with a surface of the hole Schottky semiconductor layer 322. As detailed above, the semiconductor stack has a bandgap E g and an absorbing semiconductor layer 325 having a band gap E g1and an electron Schottky semiconductor layer 321 having a band gap E g2 and hole Schottky semiconductor layer 322 having a . In this embodiment, hole Schottky semiconductor 322 is grown on electron Schottky semiconductor 321. Additionally, a graded semiconductor heterostructure 326 is disposed between electron Schottky semiconductor 321 and absorbing semiconductor layer 325, and a graded semiconductor heterostructure (not shown in FIG. 7A ) is disposed between electron Schottky semiconductor layer 321 and hole Schottky semiconductor layer 322.
[0094] For example, the electrodes 330, 340 are made of titanium / gold. The absorbing semiconductor layer 325 has a band gap E g The electron Schottky semiconductor layer 321 is made of InGaAs having a band gap E g1 = 1.45 eV, so that at the titanium-InAlAs interface, there is a high potential barrier φ against electrons injected from titanium into InAlAs. e = 0.73 eV. g2 = 1.35 eV, so that at the titanium-InP interface, there is a high potential barrier φ for holes injected from titanium into InP. h = 0.79 eV.
[0095] In FIG. 7B, ΔE C1 is the energy difference between the conduction bands of the electron Schottky semiconductor layer 321 and the absorbing semiconductor layer 325. ΔE C3 is the energy difference between the conduction bands of the electron Schottky semiconductor layer 321 and the hole Schottky semiconductor layer 322. For example, ΔE C1 = 0.52 eV and ΔE C3 =0.34 eV.
[0096] Furthermore, ΔE V1 is the energy difference between the valence bands of the absorbing semiconductor layer 325 and the electron Schottky semiconductor layer 321. ΔE V3is the energy difference between the valence bands of the electron Schottky semiconductor layer 321 and the hole Schottky semiconductor layer 322. For example, ΔE V1 = 0.19 eV and ΔE V3 =0.19 eV.
[0097] The advantages of this arrangement are the same as those described for Figures 6A and 6B. Furthermore, because hole transport is slower than electron transport, the arrangement of Figure 7A may be advantageous because it shortens the average path that holes take to the collecting electrode.
[0098] FIG. 8 presents curves showing calculated dark current density as a function of electron barrier height in an embodiment of a photodetector according to the present disclosure compared to the calculated dark current in a prior art photodetector.
[0099] In FIG. 8, curve 801 represents the minimum energy E of the conduction band, which is equal to the Schottky barrier height seen by electrons injected from the titanium layer into the InP layer as a good approximation. c and the Fermi level E F 8. Curve 802 shows the calculated electron dark current density for a Ti / InP Schottky junction as a function of the difference between the current density and the electron dark current density. Curve 803 shows the calculated hole dark current density for the same Schottky junction. The sum of the two current densities 802 corresponds to the dark current density in a symmetric MSM photodetector according to the prior art. It has a minimum value that corresponds to the best optimization of the photodetector. Such a minimum value is an absolute minimum and depends on the nature of the materials (semiconductor and metal) used for the Schottky junction.
[0100] 8 also shows the calculated dark current density 804 for an asymmetric MSM photodetector according to the present specification. In this example, the electron Schottky semiconductor is InP as before, and the hole Schottky semiconductor is InAlAs. The metal electrodes are made of titanium. Curve 801 is the calculated electron dark current density, and curve 805 is the calculated hole dark current density. As shown in FIG. 8, the total current density 804 of the asymmetric MSM shows an absolute minimum that is lower than the absolute minimum of the symmetric MSM.
[0101] 9A, 9B, 9C, 9D, and 9E show steps of a method for fabricating an asymmetric MSM photodetector according to an embodiment herein.
[0102] In a first step (FIG. 9A), a semiconductor stack 320 is deposited on a substrate 901, for example made of InP, including an absorbing semiconductor layer, an electron Schottky semiconductor layer, a hole Schottky semiconductor layer, and an (optional) graded semiconductor layer(s). The semiconductor stack 320 has a thickness, for example comprised between about 500 nm and about 1000 nm. A metal layer 340, having a thickness comprised between about 150 nm and about 250 nm, deposited on the semiconductor stack 320 to create the first electrode of the MSM photodetector, may comprise one metal, for example titanium, or a stack of metal layers, for example titanium / gold. Titanium is used as a diffusion barrier for gold to prevent gold atoms from diffusing into the semiconductor stack. Gold is an inert material, which has the properties of a low risk of oxidation over time and a very low resistivity.
[0103] In a second step (FIG. 9B), the substrate 901 with the semiconductor stack 320 and metal layer 340 is flipped over and attached onto a host substrate 905 using an adhesive layer 906. The host substrate may be made of, for example, glass or silicon. The adhesive layer may comprise a polymer that provides glass-like properties after UV curing for attaching the semiconductor stack onto a substrate such as glass, or another type of polymer such as Benzocyclobutene BCB for attaching the semiconductor stack onto an opaque substrate such as silicon.
[0104] In a third step (FIG. 9C), the substrate 901 is etched and a metal layer 330 is deposited to form the second electrode. The metal layer 330 is, for example, about 150 nm and may be structured, for example by photolithography. The metal layer 330 may comprise one metal, for example titanium, or a stack of metal layers, for example Ti / Au.
[0105] In a fourth step (FIG. 9D), the semiconductor stack 320 is etched to produce mesas that electrically isolate the photodetectors. This step may be done using wet etching techniques, e.g., chemical solutions, or dry etching techniques, e.g., induced current plasma recipes.
[0106] As shown in FIG. 9E, a vertical MSM photodetector is obtained and a bias voltage V may be applied between electrodes 330, 340.
[0107] Although the above method has been described for a vertical arrangement of MSM photodetectors, e.g., as shown in FIG. 3A or FIG. 5A, one skilled in the art would adapt the method for a horizontal arrangement of MSM photodetectors, e.g., as shown in FIG. 3B, FIG. 6A, FIG. 7A, etc.
[0108] Since the electrodes of the horizontal arrangement are located on the same side of the semiconductor stack, the transfer of the stack onto a host substrate (Figure 9B) is optional. Subsequent fabrication steps may be identical to those previously described, i.e. metal deposition to form the electrodes (Figure 9C), isolation mesas (Figure 9D). The connection to the external circuit (Figure 9E) differs from the vertical arrangement, since it is based on the "interdigitated" circuit shown in Figure 1B.
[0109] While the present invention has been described with respect to a limited number of embodiments, those skilled in the art having the benefit of this disclosure will recognize that other embodiments may be devised which do not depart from the spirit of the invention disclosed herein. Accordingly, the scope of the present invention should be limited only by the appended claims.
Claims
1. 1. A metal-semiconductor-metal photodetector configured to detect incident light of a given wavelength range, comprising: an absorbing semiconductor layer (325) configured to absorb light within said given wavelength range; a first semiconductor layer (321) made of a first semiconductor material having a first bandgap and in electrical contact with the absorbing semiconductor layer; A first metal electrode (340) configured to be electrically connected to a negative pole of a voltage generator, the first metal electrode (340) is in electrical contact with the first semiconductor layer (321); the first semiconductor layer (321) is disposed between the first metal electrode (340) and the absorbing semiconductor layer (325); The first metal electrode (340) and the first semiconductor layer (321) are configured to create an electronic Schottky junction under application of a bias voltage, the electronic Schottky junction having an electronic Schottky barrier (φ) seen by the electrons that is greater than half of the first band gap of the first semiconductor material. e the first metal electrode (340) having a a second semiconductor layer (322) in electrical contact with the absorbing semiconductor layer, the second semiconductor layer (322) being made of a second semiconductor material having a second bandgap and different from the first semiconductor material; a second metal electrode (330) configured to be electrically connected to the positive pole of the voltage generator, the second metal electrode (330) is in electrical contact with the second semiconductor layer; the second semiconductor layer (322) is disposed between the second metal electrode (330) and the absorbing semiconductor layer (325); The second metal electrode (330) and the second semiconductor layer (322) are configured to produce a hole Schottky junction under application of a bias voltage, the hole Schottky junction having a hole Schottky barrier (φ) seen by the hole that is greater than half of the second band gap of the second semiconductor material. h and the second metal electrode (330) having a first metal layer (332).
2. 2. The metal-semiconductor-metal photodetector of claim 1, wherein the absorbing semiconductor layer (325) comprises a semiconductor material selected from germanium, a III-V compound, or a II-VI compound.
3. The metal-semiconductor-metal photodetector of claim 1, wherein the absorbing semiconductor layer (325) comprises silicon.
4. 4. The metal-semiconductor-metal photodetector of claim 1, wherein the first metal electrode (340) is disposed on a first side of the absorbing semiconductor layer (325) and the second metal electrode (330) is disposed on a second side of the absorbing semiconductor layer opposite the first side.
5. 5. The metal-semiconductor-metal photodetector of claim 4, further comprising a first graded semiconductor heterostructure (326) in contact with a surface of the absorbing semiconductor layer (325) and a surface of the first semiconductor layer (321).
6. 6. The metal-semiconductor-metal photodetector of claim 4 or 5, further comprising a second graded semiconductor heterostructure (327) in contact with a surface of the absorbing semiconductor layer and a surface of the second semiconductor layer (322).
7. 4. The metal-semiconductor-metal photodetector of claim 1, wherein the first metal electrode (340) and the second metal electrode (330) are disposed on the same side of the absorbing semiconductor layer (325).
8. 8. The metal-semiconductor-metal photodetector of claim 7, further comprising a first gradient semiconductor heterostructure (326) in contact with a surface of the absorbing semiconductor layer (325) and a surface of the first semiconductor layer (321) or a second gradient semiconductor heterostructure (327) in contact with a surface of the absorbing semiconductor layer and a surface of the second semiconductor layer (322).
9. 9. The metal-semiconductor-metal photodetector of claim 7 or 8, further comprising a third graded semiconductor heterostructure in contact with a surface of the first semiconductor layer (321) and a surface of the second semiconductor layer (322).
10. 10. The metal-semiconductor-metal photodetector of claim 1, further comprising at least one of an interface layer in contact with a surface of the first semiconductor layer (321) and a surface of the first metal electrode (340) and an interface layer in contact with a surface of the second semiconductor layer (322) and a surface of the second metal electrode (330).
11. A photodetection circuit, comprising: A metal-semiconductor-metal photodetector according to any one of claims 1 to 10; a voltage generator, wherein the first metal electrode (340) is electrically connected to a negative terminal of the voltage generator and the second metal electrode (330) is electrically connected to a positive terminal of the voltage generator.
12. A method for making the metal-semiconductor-metal photodetector of claim 1, comprising the steps of: depositing a semiconductor stack (320) on a substrate (901) comprising the absorbing semiconductor layer (325), the first semiconductor layer (321) and the second semiconductor layer (322); depositing a metal layer on the semiconductor stack (320) to form the first metal electrode; inverting the substrate (901) together with the semiconductor stack (320) and attaching it onto a host substrate (905); and etching the substrate (901) and depositing a metal layer to form the second electrode (330).
13. 13. The method of claim 12, wherein the semiconductor stack (320) further comprises at least one of a first gradient semiconductor heterostructure (326) in contact with a surface of the absorbing semiconductor layer (325) and a surface of the first semiconductor layer (321) and a second gradient semiconductor heterostructure (327) in contact with a surface of the absorbing semiconductor layer and a surface of the second semiconductor layer.
Citation Information
Patent Citations
Asymmetric contacted metal-semiconductor-metal photodetectors
US5780916A