Deposition of carbon doped silicon oxide
By employing silicon- and carbon-containing precursors with organic amino groups, the method addresses high dielectric constants and ashing resistance issues in silicon-containing films, achieving low dielectric constant and high-density carbon-doped silicon oxide films suitable for semiconductor applications.
Patent Information
- Application Number
- JP2024153385
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-02-05
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-02-04
AI Technical Summary
Conventional atomic layer deposition (ALD) and plasma-enhanced atomic layer deposition (PEALD) processes for silicon-containing films face challenges such as high dielectric constants due to water absorption and low ashing resistance, particularly in silicon oxide, silicon oxynitride, and silicon oxycarbonitride films, which are exacerbated by high carbon content and residual Si-OH groups.
The development of silicon- and carbon-containing precursors with organic amino groups that anchor to the substrate surface, allowing for the deposition of carbon-doped silicon oxide films at low temperatures using ALD or PEALD processes, which include stoichiometric or non-stoichiometric silicon and oxygen materials, and involve the use of oxygen and nitrogen-containing reactants to control film composition and properties.
The method results in films with reduced dielectric constants, improved wet etch resistance, and enhanced hydrophobicity, achieving densities of at least 1.4 g/cc with wet etch rates less than 2 Å/sec and dielectric constants of 5 or less, suitable for semiconductor applications.
Smart Images

Figure 2024167401000001 
Figure 2024167401000002 
Figure 2024167401000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Application No. 62 / 801,248, filed February 5, 2019, the entire contents of which are incorporated herein by reference for all possible purposes.
[0002] The present invention relates to organosilicon compounds that can be used to deposit silicon and oxygen containing films, including carbon doped silicon oxide films, methods for using the compounds to deposit silicon oxide containing films, and films resulting from the compounds and methods. [Background technology]
[0003] Atomic layer deposition (ALD) and plasma-enhanced atomic layer deposition (PEALD) are processes used to deposit silicon oxide conformal films, for example, at low temperatures (<500° C.). In both ALD and PEALD processes, precursors and reactive gases (e.g., oxygen or ozone) are pulsed separately for a specific number of cycles to repeatedly form a monolayer of silicon oxide in each cycle.
[0004] Organoaminosilane and chlorosilane precursors are known in the art and can be used to deposit silicon-containing films at relatively low temperatures (<300° C.) and relatively high growth rates per cycle (GPC>1.0 Å / cycle) by atomic layer deposition (ALD) and plasma enhanced atomic layer deposition (PEALD) processes. There is a need in the art to provide compositions and methods of using the compositions for depositing silicon-containing films with high carbon content (e.g., carbon content of about 10 at% or more as measured by X-ray photoelectron spectroscopy (XPS)) for certain applications in the electronics industry. Some important characteristics of carbon-doped silicon-containing films are wet etch resistance and hydrophobicity. Generally speaking, the introduction of carbon into silicon-containing films helps to reduce the wet etch rate and increase the hydrophobicity. Further benefits of the addition of carbon to silicon-containing films include reducing the dielectric constant and / or providing improvements to other electrical or physical characteristics of the film.
[0005] Examples of known precursors and methods are disclosed in the following publications, patents and patent applications: US Pat.
[0006] US Patent Application Publication No. 2015 / 087139 describes the use of amino-functionalized carbosilanes to deposit silicon-containing films by thermal ALD or PEALD processes.
[0007] US Pat. No. 9,337,018 describes the use of organoaminodisilanes to deposit silicon-containing films by thermal ALD or PEALD processes.
[0008] U.S. Patent Nos. 8,940,648, 9,005,719 and 8,912,353 describe the use of organoaminosilanes to deposit silicon-containing films by thermal ALD or PEALD processes.
[0009] US Patent Application Publication No. 2015 / 275355 describes the use of mono- and bis(organoamino)alkylsilanes to deposit silicon-containing films by thermal ALD or PEALD processes.
[0010] US 2015 / 376211 describes the use of mono(organoamino)-substituted, halide-substituted, and pseudohalide-substituted trisilylamines to deposit silicon-containing films by thermal ALD or PEALD processes.
[0011] WO 15 / 105350 describes the use of four-membered cyclodisilazanes having at least one Si—H bond to deposit silicon-containing films by thermal ALD or PEALD processes.
[0012] US Patent No. 8,575,033 describes a method for the deposition of silicon carbide films on a substrate surface, which includes the use of a gas-phase carbosilane precursor and may employ a plasma-enhanced atomic layer deposition process.
[0013] U.S. Patent Application Publication No. 2013 / 0224964 teaches a method of forming a dielectric film having Si-C bonds on a semiconductor substrate by atomic layer deposition (ALD), the method including: (i) adsorbing a precursor on a surface of the substrate; (ii) reacting the adsorbed precursor with a reactant gas on the substrate; and (iii) repeating steps (i) and (ii) to form a dielectric film having at least Si-C bonds on the substrate.
[0014] US 2014 / 302688 describes a method for forming a dielectric layer on a patterned substrate that may include combining a silicon- and carbon-containing precursor with a radical oxygen precursor in a plasma-free substrate processing region in a chemical vapor deposition chamber, where the silicon- and carbon-containing precursor reacts with the radical oxygen precursor to deposit a flowable silicon-carbon-oxygen layer on the patterned surface.
[0015] US 2014 / 302690 describes a method for forming a low-k dielectric material on a substrate. The method may include generating a radical precursor by flowing an unexcited precursor into a remote plasma region, and reacting the radical precursor with a gas-phase silicon precursor to deposit a flowable film on the substrate. The gas-phase silicon precursor may include at least one silicon and oxygen-containing compound and at least one silicon and carbon linker. The flowable film may be cured to form a low-k dielectric material.
[0016] US 2014 / 051264 describes a method for depositing an initially flowable dielectric film on a substrate. The method includes introducing a silicon-containing precursor into a deposition chamber containing the substrate. The method further includes generating at least one excited precursor, such as a radical nitrogen or oxygen precursor, using a remote plasma system located outside the deposition chamber. The excited precursor is also introduced into the deposition chamber, where it reacts with the silicon-containing precursor in a reaction zone to deposit an initially flowable film on the substrate. The flowable film may be treated, for example, in a steam environment, to form a silicon oxide film.
[0017] WO 14 / 134476 describes a method for the deposition of films containing SiCN and SiCON. A particular method includes exposing a substrate surface to a first precursor and a second precursor, the first precursor having the formula (X y H 3-y Si) z CH 4-z , (X y H 3-y Si)(CH2)(SiX p H 2-p )(CH2)(SiX y H 3-y ) or (X y H 3-y Si)(CH2) n (SiX y H3-y ), where X is a halogen, y has a value from 1 to 3, z has a value from 1 to 3, p has a value from 0 to 2, and n has a value from 2 to 5, and the second precursor comprises a reducible amine. Certain methods further include exposing the substrate surface to an oxygen source to provide a film comprising SiCON.
[0018] The reference entitled "Highly Stable Ultrathin Carbosiloxane Films by Molecular Layer Deposition", Han, Z. et al., Journal of Physical Chemistry C, 2013, 117, 19967, teaches the growth of carbosiloxane films using 1,2-bis[(dimethylamino)dimethylsilyl]ethane and ozone. Thermal stability shows that the films are stable below 40°C and show almost no thickness loss at 60°C. Summary of the Invention [Problem to be solved by the invention]
[0019] There is a demand for low dielectric constant silicon-containing films, such as, but not limited to, silicon oxide, silicon oxynitride, silicon oxycarbonitride, or carbon-doped silicon oxide, by thermal atomic layer deposition (ALD) or plasma-enhanced atomic layer deposition (PEALD) processes. As-deposited silicon-containing films, such as, but not limited to, silicon oxide, silicon oxynitride, silicon oxycarbonitride, or carbon-doped silicon oxide, by thermal atomic layer deposition (ALD) or plasma-enhanced atomic layer deposition (PEALD) processes, may have high k-values due to high moisture absorption, residual Si-OH groups contained in the film, or low ashing resistance due to low film density. There is also a demand for methods to reduce the dielectric constant (k-value) of silicon-containing films. [Means for solving the problem]
[0020] The present development solves problems associated with conventional precursors and processes by providing silicon- and carbon-containing precursors having at least one organic amino group that acts to anchor the precursor unit to the surface of a substrate as part of the process of depositing a silicon- and oxygen-containing film.
[0021] Described herein are processes for the deposition of stoichiometric or non-stoichiometric silicon and oxygen containing materials or films, such as, but not limited to, silicon oxide films, carbon doped silicon oxide films, silicon oxynitride films, or carbon doped silicon oxynitride films, at relatively low temperatures, such as at one or more temperatures below 600° C., in plasma enhanced ALD (PEALD), plasma enhanced cyclic chemical vapor deposition (PECCVD), plasma enhanced ALD-like processes, or ALD processes having an oxygen-containing reactant source, a nitrogen-containing reactant source, or a combination thereof.
[0022] In one embodiment, described herein is a method for depositing a film comprising silicon and oxygen on a substrate, the method comprising: (a) providing the substrate in a reactor; (b) reacting a silicon-containing compound represented by Formulas A, B, and C: [ka] wherein R 1 But linear C1~C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C3-C 10 Alkenyl groups, C3-C 10 Alkynyl groups and C4-C 10 aryl groups; R 2 But hydrogen, C1-C 10 Straight chain alkyl group, branched chain C3~C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C2-C 10 Alkenyl groups, C2-C10 Alkynyl groups and C4-C 10 R in formula A, B or C is selected from the group consisting of aryl groups. 1 and R 2 and are either linked to form a cyclic ring structure or are not linked to form a cyclic ring structure; R 3-9 But hydrogen, straight chain C1-C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C2-C 10 Alkenyl groups, C2-C 10 Alkynyl groups and C4-C 10 R is independently selected from the group consisting of aryl groups; 10 But linear C1~C 10 Alkyl groups, C2-C 10 Alkenyl groups and C2-C 10 (c) purging the reactor with a purge gas; (d) introducing at least one of an oxygen-containing source and a nitrogen-containing source into the reactor; (e) purging the reactor with a purge gas (steps b through e are repeated until a resulting silicon-containing film of the desired thickness is deposited); (f) R 3 x Si(NR 1 R 2 ) 4-x treating the resulting silicon-containing film with 1-3 is the same as previously described, preferably methyl or ethyl, and x=1, 2 or 3, and the process is carried out at one or more temperatures in the range of about 20° C. to 300° C.
[0023] Methods for making the above compounds are also disclosed herein.
[0024] Additionally, disclosed herein are methods for treating as-deposited films or capping film deposits by chemical treatment.
[0025] The embodiments of the present invention may be used alone or in combination with each other. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] In the context of describing the invention (particularly in the context of the claims below), the use of the terms "a," "an," and "the" and similar referents are to be construed to cover both the singular and the plural, unless otherwise indicated herein or clearly contradicted by context. The terms "comprising," "having," "including," and "containing" are to be construed as open-ended terms (i.e., meaning "including, but not limited to"), unless otherwise indicated. The recitation of ranges of values herein is merely intended to serve as a shorthand method of individually referring to each individual value falling within that range, unless otherwise indicated herein, and each individual value is incorporated herein as if it were individually recited herein. All methods described herein can be performed in any suitable order, unless otherwise indicated herein or clearly contradicted by context. The use of any and all examples or exemplary language (e.g., "such as") provided herein, unless otherwise claimed, is intended merely to better illuminate the invention and does not pose a limitation on the scope of the invention. No language in the specification should be construed as indicating any non-claimed element as essential to the practice of the invention.
[0027] Described herein are compositions and methods relating to the formation of stoichiometric or non-stoichiometric silicon and oxygen-containing films or materials, such as, but not limited to, silicon oxide films, carbon-doped silicon oxide films, silicon oxynitride films, carbon-doped silicon oxynitride films, or combinations thereof, at one or more temperatures below about 300° C. or from about 25° C. to about 300° C., and in some embodiments, from 25° C. to about 300° C. The films described herein are deposited in a deposition process such as atomic layer deposition (ALD) or in a process similar to ALD, such as, but not limited to, a plasma-enhanced ALD (PEALD) process or a plasma-enhanced cyclic chemical vapor deposition process (PECCVD). The low temperature (e.g., deposition temperature or temperatures ranging from about ambient to 600° C.) deposition methods described herein provide films or materials that exhibit at least one or more of the following advantages: low chemical impurities, high conformality in thermal atomic layer deposition, plasma-enhanced atomic layer deposition (ALD) processes or processes similar to plasma-enhanced ALD, ability to control carbon content in the resulting film; and / or the film has an etch rate of 5 angstroms / second (Å / sec) or less when measured in 0.5 wt% dilute HF. For carbon-doped silicon oxide films, more than 1% carbon is desired to control the etch rate to less than 2Å / sec in 0.5 wt% dilute HF, in addition to other characteristics such as, but not limited to, a density of about 1.4 g / cc or more, about 1.8 g / cc or more, or about 2.0 g / cc or more.
[0028] The methods disclosed herein can be carried out using equipment known in the art, for example, the methods can use reactors that are conventional in the semiconductor manufacturing art.
[0029] Without wishing to be bound by any theory or explanation, it is believed that the effectiveness of the precursor compositions disclosed herein can vary depending on the number of silicon atoms and, in particular, the number of silicon atom bonds.Typically, the precursors disclosed herein have 3-5 silicon atoms and 5-8 silicon-oxygen bonds.
[0030] The precursors disclosed herein have a different structure than those known in the art and can work better than conventional silicon-containing precursors to provide a relatively large GPC, resulting in higher quality films, having a more favorable wet etch rate, or having less elemental contamination.
[0031] 1. A method for depositing a carbon doped silicon oxide film using a vapor deposition process, comprising: [ka] wherein R 1 But linear C1~C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C3-C 10 Alkenyl groups, C3-C 10 Alkynyl groups and C4-C 10 aryl groups; R 2 But hydrogen, C1-C 10 Straight chain alkyl group, branched chain C3~C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C2-C 10 Alkenyl groups, C2-C 10 Alkynyl groups and C4-C 10 R in formula A or B is selected from the group consisting of aryl groups. 1 and R 2 are either linked to form a cyclic ring structure or are not linked to form a cyclic ring structure; R 3-9But hydrogen, straight chain C1-C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C2-C 10 Alkenyl groups, C2-C 10 Alkynyl groups and C4-C 10 R is independently selected from the group consisting of aryl groups; 10 But linear C1~C 10 Alkyl groups, C2-C 10 Alkenyl groups and C2-C 10 Disclosed herein are methods that include compounds selected from the alkynyl group.
[0032] In a preferred embodiment, subject to the above proviso, for formulae A and B, a preferred embodiment is 1-9 and for formula C, preferred embodiments include compounds in which each of R 1-2 each of R is C3-C4 alkyl; 10 Includes compounds where is methyl.
[0033] In the formula above, and throughout this specification, the term "oligosiloxane" means a compound that contains at least three repeating -Si-O-siloxane units in a cyclic structure.
[0034] In the above formula and throughout this specification, the term "alkyl" refers to a straight or branched chain functional group having 1 to 10 carbon atoms. Exemplary straight chain alkyl groups include, but are not limited to, methyl, ethyl, propyl, butyl, pentyl, and hexyl groups. Exemplary branched chain alkyl groups include, but are not limited to, iso-propyl, iso-butyl, sec-butyl, tert-butyl, iso-pentyl, tert-pentyl, iso-hexyl, and neo-hexyl. In certain embodiments, the alkyl group may have one or more functional groups attached to the alkyl group, such as, but not limited to, an alkoxy group, a dialkylamino group, or combinations thereof attached to the alkyl group. In other embodiments, the alkyl group does not have one or more functional groups attached to the alkyl group. The alkyl group may be saturated or alternatively unsaturated.
[0035] In the formula above and throughout this specification, the term "cyclic alkyl" refers to a cyclic functional group having 3 to 10 carbon atoms. Exemplary cyclic alkyl groups include, but are not limited to, cyclobutyl, cyclopentyl, cyclohexyl, and cyclooctyl groups.
[0036] In the above formula and throughout this specification, the term "alkenyl group" refers to a group having one or more carbon-carbon double bonds and having 2 to 10 or 2 to 6 carbon atoms.
[0037] In the formulas described herein and throughout this specification, the term "dialkylamino", "alkylamino" or "organoamino" refers to a group having two alkyl groups attached to a nitrogen atom or one alkyl attached to a nitrogen atom and having 1-10, 2-6, or 2-4 carbon atoms. Examples include HNMe, HNBu. t , NMe2, NMeEt, NEt2 and NPr i Including, but not limited to, 2.
[0038] In the above formula and throughout this specification, the term "aryl" refers to an aromatic cyclic functional group having 4 to 10 carbon atoms, 5 to 10 carbon atoms, or 6 to 10 carbon atoms. Exemplary aryl groups include, but are not limited to, phenyl, benzyl, chlorobenzyl, tolyl, o-xylyl, 1,2,3-triazolyl, pyrrolyl, and furanyl.
[0039] Throughout this specification, the term "alkyl hydrocarbon" refers to straight or branched chain C1-C 20 Hydrocarbons, cyclic C6-C 20 "hydrocarbon" refers to a hydrocarbon. Exemplary hydrocarbons include, but are not limited to, heptane, octane, nonane, decane, dodecane, cyclooctane, cyclononane, and cyclodecane.
[0040] Throughout this specification, the term "alkoxy" refers to a C1-C 10 -OR 1 The base is R 1 is defined above. Exemplary alkoxy groups include, but are not limited to, methoxy, ethoxy, iso-propoxy, n-propoxy, n-butoxy, sec-butoxy, tert-butoxy, and phenoxy.
[0041] Throughout this specification, the term "ashing" refers to the process of removing photoresist or carbon hardmasks in semiconductor manufacturing processes using a plasma containing an oxygen source, such as an O2 / inert gas plasma, an O2 plasma, a CO2 plasma, a CO plasma, an H2 / O2 plasma, or combinations thereof.
[0042] In the formula above and throughout this specification, the term "heterocycle" refers to a non-aromatic saturated monocyclic or polycyclic ring system of about 3 to about 10 ring atoms, preferably about 5 to about 10 ring atoms, in which one or more of the atoms is an element other than carbon, such as nitrogen, oxygen, or sulfur. Preferred heterocycles contain about 5 to about 6 ring atoms. The prefix aza, oxo, or thio before a heterocycle means that at least one nitrogen, oxygen, or sulfur atom, respectively, is present as a ring atom. Heterocycle groups are optionally substituted.
[0043] Exemplary silicon compounds having formulas A-C are set forth in Tables 1a and 1b. Table 1a. Exemplary silicon compounds having formula A or B [Table 1-1] [Table 1-2] [Table 1-3] [Table 1-4] [Table 1-5] [Table 1-6] Table 1b. Exemplary silicon compounds having formula C [Table 2] Preferably, the silicon precursor compounds having formula A, B or C according to the present invention and compositions comprising silicon precursor compounds having formula A or B according to the present invention are substantially free of halide ions. As used herein, the term "substantially free" means less than 5 ppm (by weight) as measured by ICP-MS, preferably less than 3 ppm as measured by ICP-MS, more preferably less than 1 ppm as measured by ICP-MS, and most preferably 0 ppm as measured by ICP-MS, when referring to halide ions (or halides), such as chloride (i.e. chloride-containing species, such as HCl, or silicon compounds having at least one Si-Cl bond), fluoride, bromide and iodide. Chloride is known to act as a decomposition catalyst for silicon precursor compounds having formula A-C. Significant levels of chloride in the final product can decompose silicon precursor compounds. Slow decomposition of silicon precursor compounds can directly affect the film deposition process making it difficult for semiconductor manufacturers to meet film specifications. In addition, shelf life or stability is negatively affected by the greater decomposition rate of the silicon precursor compounds, thereby making it difficult to guarantee a shelf life of 1-2 years. Accelerated decomposition of silicon precursor compounds thus leads to safety and performance concerns related to the formation of these flammable and / or pyrophoric gaseous by-products. Preferably, the silicon precursor compounds having formula A or B are free of metal ions, such as Li + , Mg 2+ , Al 3+ , Fe 2+ , Fe 2+ , Fe 3+ , Ni 2+ , Cr 3+Substantially free of. As used herein, the term "substantially free of" means less than 5 ppm (by weight), preferably less than 3 ppm, more preferably less than 1 ppm, and most preferably less than 0.1 ppm, when measured by ICP-MS, with respect to Li, Al, Fe, Ni, Cr. In some embodiments, the silicon precursor compound having formula A is free of metal ions, such as Li + , Mg 2+ , Al 3+ , Fe 2+ , Fe 3+ , Ni 2+ , Cr 3+ As used herein, the term "free" of metal impurities, when referring to Li, Mg, Al, Fe, Ni, Cr, precious metals, such as volatile Ru or Pt complexes derived from ruthenium or platinum catalysts used in the synthesis, means less than 1 ppm (by weight), preferably less than 0.1 ppm, as measured by ICP-MS or other analytical methods for measuring metals.
[0044] In one embodiment of the present invention, there is provided a method for depositing a carbon-doped silicon and oxygen-containing film on at least one surface of a substrate at a temperature between 20° C. and 300° C., comprising: a. providing a substrate in a reactor; b. introducing at least one silicon precursor having formulae A-C described herein into a reactor; c. purging the reactor with a purge gas to remove at least a portion of the unabsorbed precursor; d. introducing an oxygen-containing source into the reactor; e. purging the reactor with a purge gas to remove at least a portion of the unreacted oxygen-containing source; f. repeating steps b through e until a silicon-containing film of a desired thickness is deposited; gR 3 x Si(NR 1 R 2 )4-x wherein R 1-3 But hydrogen, straight chain C1-C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C3-C 10 Alkenyl groups, C3-C 10 treating the resulting silicon-containing film with a silicon precursor, each independently selected from an alkynyl group, preferably methyl or ethyl, where x=1, 2 or 3; h. Purge the reactor with a purge gas to remove surface hydroxyls and R 3 x Si(NR 1 R 2 ) 4-x removing at least a portion of any by-products from the reaction with the silicon precursor having the formula: A method is described herein that includes:
[0045] In certain embodiments, during the deposition process, the as-deposited film by steps bf can be treated using steps g through h, which can be performed, for example, by one ALD cycle, two ALD cycles, five ALD cycles, or ten or more ALD cycles until all reactive hydroxyls are consumed, to reduce the dielectric constant to 5 or less, preferably 4 or less, and most preferably 3 or less. 3 x Si(NR 1 R 2 ) 4-xExemplary silicon precursors having the formula include, but are not limited to, diethylaminotriethylsilane, dimethylaminotriethylsilane, ethylmethylaminotriethylsilane, t-butylaminotriethylsilane, iso-propylaminotriethylsilane, di-isopropylaminotriethylsilane, pyrrolidinotriethylsilane, diethylaminotrimethylsilane, dimethylaminotrimethylsilane, ethylmethylaminotrimethylsilane, t-butylaminotrimethylsilane, iso-propylaminotrimethylsilane, di-isopropylaminotrimethylsilane, pyrrolidinotrimethylsilane, diethylaminodimethylsilane, dimethylaminodimethylsilane, ethylmethylaminodimethylsilane, t-butylaminodimethylsilane, iso-propylaminodimethylsilane, di-isopropylaminodimethylsilane, pyrrolidinodimethylsilane, diethylaminodiethylsilane, dimethylaminodiethylsilane, ethylmethylaminodiethylsilane, t-butylaminodiethylsilane, iso-propylaminodiethylsilane, di-isopropylaminodiethylsilane, pyrrolidinodimethylsilane, diethylaminodiethylsilane, dimethylaminodiethylsilane, ethylmethylaminodiethylsilane, t-butylaminodiethylsilane, iso-propylaminodiethylsilane, di-isopropylaminodiethylsilane, pyrrolidinodimethylsilane, diethylaminosilane, bis(diethylamino)dimethylsilane, bis(dimethylamino)dimethylsilane, bis(ethylmethylamino)dimethylsilane, bis(di-isopropylamino)dimethylsilane, bis(isopropylamino)dimethylsilane, bis(tert-butylamino)dimethylsilane, dipyrrolidinodimethylsilane, bis(diethylamino)diethylsilane, bis(dimethylamino)diethylsilane, bis(ethylmethylamino)diethylsilane, bis(di-isopropylamino)diethylsilane, bis(isopropylamino)dimethylsilane, )diethylsilane, bis(tert-butylamino)diethylsilane, dipyrrolidinodiethylsilane, bis(diethylamino)methylvinylsilane, bis(dimethylamino)methylvinylsilane, bis(ethylmethylamino)methylvinylsilane, bis(di-isopropylamino)methylvinylsilane, bis(iso-propylamino)methylvinylsilane, bis(tert-butylamino)methylvinylsilane, dipyrrolidinomethylvinylsilane, 2,6-dimethylpiperidinomethylsilane, 2,6-dimethylpiperidinodimethylsilane, 2,Examples of suitable silanes include 6-dimethylpiperidinotrimethylsilane, tris(dimethylamino)phenylsilane, tris(dimethylamino)methylsilane, tris(dimethylamino)ethylsilane, and mixtures thereof. In some embodiments, steps g-h can be performed at a temperature between 300° C. and 550° C. after steps b-f have been performed to the desired thickness.
[0046] In another particular embodiment, the method described herein deposits a silicon- and oxygen-containing film, including two silicon-containing films, on a substrate at a temperature between 20° C. and 300° C. The method includes: a. providing a substrate in a reactor; b. introducing at least one silicon precursor having formulae A-C described herein into a reactor; c. purging the reactor with a purge gas to remove at least a portion of the unabsorbed precursor; d. introducing an oxygen-containing source into the reactor; e. purging the reactor with a purge gas to remove at least a portion of the unreacted oxygen-containing source; f. repeating steps b through e until a first silicon-containing film of a desired thickness is deposited; g.Formula R 3 x Si(NR 1 R 2 ) 4-x wherein R 1-3 But hydrogen, straight chain C1-C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C3-C 10 Alkenyl groups and C3-C 10 introducing at least one silicon precursor, each independently selected from an alkynyl group, preferably methyl or ethyl, where x=1, 2, 3, into a reactor; h. purging the reactor with a purge gas to remove at least a portion of the unabsorbed precursor; i. introducing an oxygen-containing source into a reactor; j. purging the reactor with a purge gas to remove at least a portion of the unreacted oxygen-containing source; and k. repeating steps g through j until a second silicon-containing film of a desired thickness is deposited; Includes.
[0047] In one particular embodiment, during the deposition process, the desired thickness of the first silicon-containing film according to steps bf is 10 Å to 500 Å, 10 Å to 100 Å, or 10 Å to 50 Å. The desired thickness of the second silicon-containing film according to steps gk is 1 Å to 50 Å, 2 Å to 40 Å, 2 Å to 30 Å, 2 Å to 20 Å, or 2 Å to 10 Å. The second silicon-containing film has a higher density and lower carbon content relative to the first silicon-containing film, thus providing oxygen ashing resistance during the semiconductor manufacturing process and resulting in less damage to the first silicon-containing film. Formula R 3 x Si(NR 1 R 2 ) 4-x (In the formula, R 3 is hydrogen, and R 2-3 are independently selected from hydrogen, linear C1-C5 alkyl groups, branched C3-C5 alkyl groups, and x=1, 2), exemplary silicon precursors in this embodiment include, but are not limited to, di-iso-propylaminosilane, di-sec-butylaminosilane, bis(diethylamino)silane, bis(tert-butylamino)silane, and mixtures thereof. In some embodiments, steps b-f are performed at a lower temperature of 20° C.-150° C. to maximize the carbon content remaining in the carbon-doped silicon oxide, while steps g-k are performed at a higher temperature of 200° C.-300° C. to provide a denser silicon oxide with less carbon content, making the second silicon-containing film better ash-resistant. In certain embodiments, the oxygen-containing sources in steps d and i are the same. In alternative embodiments, the oxygen-containing sources in steps d and i are different. In some embodiments, steps g through h can be performed at a temperature between 300° C. and 550° C. after steps b through f have been performed to the desired thickness.
[0048] The methods disclosed herein provide a method for producing a crystalline silicon thin film having the following characteristics: a density of at least about 1.4 g / cc or greater, about 1.8 g / cc or greater, or about 2.1 g / cc or greater; a wet etch rate of less than about 2.5 Å / s as measured in a solution of dilute HF (0.5 wt % dHF) acid in 1:100 HF:water; and a surface roughness of less than about 5×10 as measured by secondary ion mass spectrometry (SIMS). 20 and a hydrogen impurity concentration less than at / cc.
[0049] In certain embodiments of the methods and compositions described herein, a layer of silicon-containing dielectric material is deposited on at least a portion of a substrate, for example, by chemical vapor deposition (CVD) process using a reaction chamber.Suitable substrates include, but are not limited to, semiconductor materials, such as gallium arsenide (GaAs), silicon, and silicon-containing compositions, such as crystalline silicon, polysilicon, amorphous silicon, epitaxial silicon, silicon dioxide (SiO2), silicon glass, silicon nitride, fused silica, glass, quartz, borosilicate glass, and combinations thereof.Other suitable materials include chromium, molybdenum, and other metals commonly used in semiconductor, integrated circuit, flat panel display, and flexible display applications. The substrate may have further layers, such as silicon, SiO2, organosilicate glass (OSG), fluorinated silicate glass (FSG), boron carbonitride, silicon carbide, hydrogenated silicon carbide, silicon nitride, hydrogenated silicon nitride, silicon carbonitride, hydrogenated silicon carbonitride, boron nitride, organic-inorganic composites, photoresists, organic polymers, porous organic and inorganic materials and composites, metal oxides, such as aluminum oxide and germanium oxide. Further layers may be germanosilicates, aluminosilicates, copper and aluminum, and diffusion barrier materials, such as, but not limited to, TiN, Ti(C)N, TaN, Ta(C)N, Ta, W, or WN.
[0050] The deposition methods disclosed herein may include one or more purge gases. The purge gases used to purge unconsumed reactants and / or reaction by-products are inert gases that do not react with the precursors. Exemplary purge gases include, but are not limited to, argon (Ar), nitrogen (N2), helium (He), neon, hydrogen (H2), and mixtures thereof. In certain embodiments, a purge gas, such as Ar, is fed into the reactor at a flow rate of about 10 to about 2000 sccm for about 0.1 to 1000 seconds, thereby purging unreacted materials and any by-products that may remain in the reactor.
[0051] A purge gas, such as argon, purges the unabsorbed excess complex from the process chamber. After sufficient purging, an oxygen source can be introduced into the reaction chamber to react with the absorbed surface, followed by another gas purge to remove reaction by-products from the chamber. The process cycle can be repeated to achieve the desired film thickness. In some cases, pumping can be replaced by purging with an inert gas, or both can be used to remove unreacted silicon precursor.
[0052] Throughout this specification, the term "ALD or ALD-like" refers to processes including, but not limited to, the following processes: a) processes in which the respective reactants, including the silicon precursor and the reactive gas, are introduced sequentially into a reactor, such as a single-wafer ALD reactor, a semi-batch ALD reactor, or a batch furnace ALD reactor; b) processes in which the respective reactants, including the silicon precursor and the reactive gas, are exposed to the substrate by moving or rotating the substrate into different compartments of the reactor, each compartment being separated by an inert gas curtain, i.e., a spatial ALD reactor or a roll-to-roll ALD reactor.
[0053] The method of the present invention is carried out by an ALD process using an oxygen-containing source, such as ozone, hydrogen peroxide, or a plasma, the plasma can further include an inert gas, such as one or more of the following: oxygen plasma with or without an inert gas, water vapor plasma with or without an inert gas, nitrogen oxide (e.g., N2O, NO, NO2, or combinations thereof) plasma with or without an inert gas, carbon oxide (e.g., CO2, CO, or combinations thereof) plasma with or without an inert gas, and combinations thereof. In certain embodiments, the oxygen-containing plasma source further includes an inert gas. In these embodiments, the inert gas is selected from the group consisting of argon, helium, nitrogen, hydrogen, or combinations thereof. In alternative embodiments, the oxygen-containing plasma source does not include an inert gas.
[0054] The oxygen-containing plasma source can be generated in situ or alternatively remotely. In one particular embodiment, the oxygen-containing source comprises oxygen and is flowed or introduced during steps b to d of the method together with other reagents, such as, but not limited to, at least one silicon precursor and optionally with an inert gas.
[0055] In certain embodiments, the composition described herein--and used in the disclosed method--can further comprise a solvent.Exemplary solvents can include, but are not limited to, ethers, tertiary amines, alkyl hydrocarbons, aromatic hydrocarbons, tertiary amino ethers, and combinations thereof.In certain embodiments, the difference between the boiling point of the silicon precursor and the boiling point of the solvent is 40° C. or less.In some embodiments, the composition can be delivered into the reactor chamber for silicon-containing film by direct liquid injection.
[0056] For embodiments in which at least one silicon precursor having formulas A-C is used in a composition containing a solvent, the solvent or mixture thereof selected does not react with the silicon precursor. The amount of solvent in the composition is, by weight, 0.5 wt% to 99.5 wt% or 10 wt% to 75 wt%. In this or other embodiments, the solvent has a boiling point (bp) close to the bp of the silicon precursor of formulas A-C, or the difference between the bp of the solvent and the bp of the silicon precursor of formulas A-C is 40°C or less, 30°C or less, 20°C or less, or 10°C. Alternatively, the boiling point difference is a range that includes any one or more of the following endpoints: 0, 10, 20, 30, or 40°C. Examples of suitable ranges of bp difference include, but are not limited to, 0°C to 40°C, 20°C to 30°C, or 10°C to 30°C. Examples of suitable solvents in the composition include, but are not limited to, ethers (e.g., 1,4-dioxane, dibutyl ether), tertiary amines (e.g., pyridine, 1-methylpiperidine, 1-ethylpiperidine, N,N'-dimethylpiperazine, N,N,N',N'-tetramethylethylenediamine), nitriles (e.g., benzonitrile), alkyl hydrocarbons (e.g., octane, nonane, dodecane, ethylcyclohexane), aromatic hydrocarbons (e.g., toluene, mesitylene), tertiary amino ethers (e.g., bis(2-dimethylaminoethyl) ether), or mixtures thereof.
[0057] In certain embodiments, the silicon oxide film or carbon-doped silicon oxide film deposited using the methods described herein is formed in the presence of an oxygen-containing source, including ozone, water (H2O) (e.g., deionized water, purified water, and / or distilled water), oxygen (O2), oxygen plasma, NO, NO2O, NO2, carbon monoxide (CO), carbon dioxide (CO2), and combinations thereof. The oxygen-containing source is passed, for example, through a plasma generator, either in situ or remote, to provide an oxygen-containing plasma source, including oxygen, for example, oxygen plasma, plasma including oxygen and argon, plasma including oxygen and helium, ozone plasma, water plasma, nitrous oxide plasma, or carbon dioxide plasma. In certain embodiments, the oxygen-containing plasma source includes an oxygen source gas introduced into the reactor at a flow rate of about 1 to about 2000 standard cubic centimeters (sccm) or about 1 to about 1000 sccm. The oxygen-containing plasma source can be introduced for a time period ranging from about 0.1 to about 100 seconds. In one particular embodiment, the oxygen-containing plasma source comprises water having a temperature of 10° C. or greater. In an embodiment in which a film is deposited by a PEALD process or a plasma-enhanced cyclic CVD process, depending on the volume of the ALD reactor, the precursor pulse may have a pulse duration longer than 0.01 seconds (e.g., about 0.01 to about 0.1 seconds, about 0.1 to about 0.5 seconds, about 0.5 to about 10 seconds, about 0.5 to about 20 seconds, about 1 to about 100 seconds) and the oxygen-containing plasma source may have a pulse duration shorter than 0.01 seconds (e.g., about 0.001 to about 0.01 seconds).
[0058] Each step of supplying the precursor, oxygen source and / or other precursors, source gases, and / or reagents can be performed with varying times for supplying them to vary the stoichiometric composition of the resulting dielectric film.
[0059] Energy is applied to at least one of the silicon precursors of formulas A-C, oxygen-containing sources, or combinations thereof to induce a reaction and form a dielectric film or coating on the substrate. Such energy can be provided by, but is not limited to, thermal, plasma, pulsed plasma, helicon plasma, high-density plasma, inductively coupled plasma, X-ray, electron beam, photon, remote plasma methods, and combinations thereof. In certain embodiments, a secondary RF frequency source can be used to modify the plasma characteristics at the substrate surface. In embodiments where deposition involves plasma, the plasma generation process can include a direct plasma generation process in which the plasma is generated directly in the reactor, or alternatively, a remote plasma generation process in which the plasma is generated outside the reactor and fed into the reactor.
[0060] At least one silicon precursor can be transported to the reaction chamber, for example, to a plasma-enhanced cyclic CVD reactor, a PEALD reactor, or a batch furnace type reactor, by various means. In one embodiment, a liquid transport system is utilized. In an alternative embodiment, a device that combines liquid transport and flash vaporization processes, such as a turbo vaporizer manufactured by MSP Corporation of Shoreview, MN, can be used to allow low volatility materials to be transported volumetrically, which results in reproducible transport and deposition without thermal decomposition of the precursor. In liquid transport formulations, the precursors described herein may be transported in a substantially liquid form, or alternatively, may be used in a solvent formulation or composition that includes the precursor. Thus, in certain embodiments, the precursor formulation can include at least one solvent component of suitable characteristics to be desirable and advantageous in a given end-use application for forming a film on a substrate.
[0061] As described above, the purity level of at least one silicon precursor is high enough to be acceptable for reliable semiconductor manufacturing.In certain embodiments, at least one silicon precursor described herein comprises less than 2wt%, less than 1wt%, or less than 0.5wt% of one or more of the following impurities: free amine, free halide, or halogen ion, and higher molecular weight species.The higher purity level of the silicon precursor described herein can be obtained through one or more of the following processes: purification, adsorption, and / or distillation.
[0062] In one embodiment of the method described herein, a plasma-enhanced cyclic deposition process can be used, for example a PEALD-like process or a PEALD process, in which deposition is carried out using at least one silicon precursor and an oxygen plasma source. A PEALD-like process is defined as a plasma-enhanced cyclic CVD process, but provides a highly conformal silicon and oxygen-containing film.
[0063] having the formula A-B, wherein R 3-9 Organoamino-functionalized cyclic oligosiloxane precursors, in which some of R are methyl rather than hydrogen, are believed to be preferred for this method, because they either do not contain any Si-H groups or have a limited number of Si-H groups, which may decompose at temperatures above 600° C., potentially resulting in undesired chemical vapor deposition. However, under certain conditions, such as using short precursor pulses or low reactor pressures, the method can be used with organoamino-functionalized cyclic oligosiloxane precursors having the formula A-B, where R 3-9 Using organoamino-functionalized cyclic oligosiloxane precursors, some of which are hydrogen, it can also be carried out at temperatures above 600° C. without significant undesirable chemical vapor deposition.
[0064] A variety of commercial ALD reactors, such as single-wafer reactors, semi-batch reactors, batch furnace reactors, or roll-to-roll reactors, can be used to deposit solid silicon oxide, silicon oxynitride, carbon-doped silicon oxynitride, or carbon-doped silicon oxide.
[0065] Process temperatures for the methods described herein use one or more of the following temperatures as endpoints: 0° C., 25° C., 50° C., 75° C., 100° C., 125° C., 150° C., 175° C., 200° C., 225° C., 250° C., 275° C., 300° C. Exemplary temperature ranges include, but are not limited to, the following: from about 0° C. to about 300° C.; from about 25° C. to about 300° C.; from about 50° C. to about 290° C.; from about 25° C. to about 250° C.; or from about 25° C. to about 200° C.
[0066] In certain embodiments, the oxygen source is selected from the group consisting of water vapor, water plasma, ozone, oxygen, oxygen plasma, oxygen / helium plasma, oxygen / argon plasma, nitrogen oxide plasma, carbon dioxide plasma, hydrogen peroxide, organic peroxides, and mixtures thereof.
[0067] In further embodiments of the methods described herein, the film deposited from ALD, ALD-like, PEALD or PEALD-like or as-deposited film is subjected to a treatment step (post-deposition treatment). The treatment step can be performed during at least a portion of the deposition step, after the deposition step and combinations thereof. Exemplary treatment steps include, but are not limited to, treatment with high temperature thermal annealing at temperatures ranging from 500°C to 1200°C, 600°C to 800°C, 550°C to 750°C, 600°C to 750°C or 600°C to 700°C; plasma treatment, e.g., helium plasma, argon plasma, etc.; ultraviolet (UV) light treatment; laser; electron beam treatment and combinations thereof to affect one or more properties of the film.
[0068] In another embodiment, the vessel or container for depositing silicon-containing film comprises one or more silicon precursor compounds as described herein.In one particular embodiment, the vessel comprises at least one pressurizable vessel (preferably made of stainless steel, for example, with the design disclosed in U.S. Patent Nos. 7,334,595; 6,077,356; 5,069,244; and 5,465,766), the disclosures of which are incorporated herein by reference.The vessel can comprise either glass (borosilicate or quartz glass) or 316, 316L, 304 or 304L series stainless steel alloy (UNS designation S31600, S31603, S30400, S30403), and is equipped with suitable valves and fittings to allow the transport of one or more precursors to the reactor for CVD or ALD process. In this or other embodiments, the silicon precursor is provided in a pressurizable vessel constructed of stainless steel, the purity of the precursor being 98 wt% or greater, or 99.5 wt% or greater, which is suitable for many semiconductor applications, and the headspace of the vessel or container is filled with an inert gas selected from helium, argon, nitrogen, and combinations thereof.
[0069] In certain embodiments, the gas line connecting the precursor canister to the reaction chamber is heated to one or more temperatures according to the process requirements, and the container of at least one silicon precursor is kept at one or more temperatures for bubbling.In other embodiments, the solution containing at least one silicon precursor is injected into a vaporizer kept at one or more temperatures for direct liquid injection.
[0070] A flow of argon and / or other gases can be used as a carrier gas to facilitate transport of at least one silicon precursor vapor into the reaction chamber during the precursor pulse. In certain embodiments, the process pressure of the reaction chamber is about 50 mTorr to 10 Torr. In other embodiments, the process pressure of the reaction chamber can be 760 Torr or less (e.g., about 50 mTorr to about 100 Torr).
[0071] In a typical PEALD process or a process similar to PEALD, such as a PECCVD process, a substrate, such as a silicon oxide substrate, is heated in a heater stage in a reaction chamber where it is exposed to a silicon precursor to initially chemisorb a complex onto the surface of the substrate.
[0072] Films deposited using silicon precursors having formulas A-C described herein have improved properties when compared to films deposited under the same conditions using silicon precursors disclosed above, such as, but not limited to, a wet etch rate lower than the wet etch rate of the film before the treatment step, or a density higher than the density before the treatment step. In one particular embodiment, during the deposition process, the as-deposited film is treated intermittently. These intermittent or intermediate treatments can be performed, for example, after each ALD cycle, after every certain number of ALD cycles, such as, but not limited to, after every 1 ALD cycle, every 2 ALD cycles, every 5 ALD cycles, or every 10 or more ALD cycles.
[0073] Precursors of formulas A-C exhibit growth rates of 1.0 Å / cycle or greater, preferably 1.5 Å / cycle or greater, and most preferably 2.0 Å / cycle or greater.
[0074] In embodiments in which the film is treated with a high temperature annealing step, the annealing temperature is at least 100° C. higher than the deposition temperature. In this or other embodiments, the annealing temperature is from about 400° C. to about 1000° C. In this or other embodiments, the annealing process can be performed in a vacuum (<760 Torr), in an inert environment, or in an oxygen-containing environment (e.g., H2O, N2O, NO2, or O2).
[0075] In embodiments in which the film is treated by UV treatment, the film is exposed to broadband UV, or alternatively, a UV source having a wavelength of about 150 nanometers (nm) to about 400 nm. In one particular embodiment, the as-deposited film is exposed to UV in a chamber separate from the deposition chamber after reaching a desired film thickness.
[0076] In embodiments where the film is treated with plasma, a passivation layer, such as SiO2 or carbon-doped SiO2, is deposited to prevent chlorine and nitrogen contaminants from penetrating the film during subsequent plasma treatment. The passivation layer can be deposited using atomic layer deposition or cyclic chemical vapor deposition.
[0077] In embodiments in which the film is treated with a plasma, the plasma source is selected from the group consisting of a hydrogen plasma, a hydrogen and helium containing plasma, and a hydrogen and argon containing plasma. The hydrogen plasma lowers the dielectric constant of the film and increases its resistance to damage from plasma ashing processes, while keeping the carbon content in the bulk approximately unchanged.
[0078] Without intending to be bound by any particular theory, it is believed that silicon precursor compounds having chemical structures represented by Formulas A-C defined above can immobilize organic amino groups by reacting with hydroxyls on the substrate surface to provide multiple Si-O-Si fragments per precursor molecule, thus increasing the growth rate of silicon oxide or carbon-doped silicon oxide compared to conventional silicon precursors, such as bis(tert-butylamino)silane or bis(diethylamino)silane, which have only one silicon atom.
[0079] In certain embodiments, the silicon-containing films described herein have a dielectric constant of 6 or less, 5 or less, 4 or less, and 3 or less. In these or other embodiments, the films can have a dielectric constant of about 5 or less, about 4 or less, or about 3.5 or less. However, it is believed that films having other dielectric constants (e.g., higher or lower dielectric constants) can also be formed depending on the desired end use of the film. Examples of silicon-containing films formed using the silicon precursors and processes having formulas A-C described herein include those having the formulas Si x O y C z N v H w where, in atomic percent wt%, as measured, for example, by XPS or other means, Si is about 10% to about 40%; O is about 0% to about 65%; C is about 0% to about 75% or about 0% to about 50%; N is about 0% to about 75% or about 0% to about 50%; and H is about 0% to about 50%, with x+y+z+v+w=100 atomic wt%. Another example of a silicon-containing film formed using the silicon precursors and processes of formulas A-C described herein is silicon carbonate nitride, with a carbon content of 1 at% to 80 at%, as measured by XPS. Yet another example of a silicon-containing film formed using the silicon precursors and processes having formulas A-C described herein is amorphous silicon, with the sum of both the nitrogen content and the carbon content being less than 10 at%, preferably less than 5 at%, and most preferably less than 1 at%, as measured by XPS.
[0080] As mentioned above, the method described herein can be used to deposit a silicon-containing film on at least a portion of a substrate. Examples of suitable substrates include, but are not limited to, silicon, SiO2, Si3N4, OSG, FSG, silicon carbide, hydrogenated silicon oxycarbide, hydrogenated silicon oxynitride, silicon carbonate nitride, hydrogenated silicon carbonate nitride, anti-reflective coating, photoresist, germanium, germanium-containing, boron-containing, Ga / As, flexible substrates, organic polymers, porous organic and inorganic materials, metals such as copper and aluminum, and diffusion barrier layers such as, but not limited to, TiN, Ti(C)N, TaN, Ta(C)N, Ta, W or WN. The film is compatible with various subsequent processing steps, such as chemical mechanical planarization (CMP) and anisotropic etching processes.
[0081] The deposited films have applications including, but not limited to, computer chips, optical devices, magnetic information storage devices, coatings on supporting materials or substrates, microelectrochemical systems (MEMS), nanoelectrochemical systems, thin film transistors (TFTs), light emitting diodes (LEDs), organic light emitting diodes (OLEDs), IGZO, and liquid crystal displays (LCDs). Potential applications of the resulting solid silicon oxide or carbon doped silicon oxide include, but are not limited to, shallow trench insulators, interlayer dielectrics, passivation layers, etch stop layers, part of a dual spacer, and sacrificial layers for patterning.
[0082] In certain embodiments, one or more silicon precursors having formulas A-C described herein can be used to form silicon and oxygen-containing films that are solid and non-porous or substantially free of pores.
[0083] The following examples are provided to illustrate certain aspects of the invention and are not intended to limit the scope of the appended claims. EXAMPLES
[0084] Thermal atomic layer deposition of silicon oxide films was performed in a laboratory-scale ALD processing tool. The silicon precursor was delivered to the chamber by vapor extraction. All gases (e.g., purge and reactant gases or precursor and oxygen source) were preheated to 100° C. before entering the deposition region. The gas and precursor flow rates were controlled by ALD diaphragm valves with fast action. The substrate used in the deposition was a 12-inch long silicon strip. Thermocouples were attached to the sample holder to check the substrate temperature. The deposition was performed using ozone as the oxygen source gas. The typical deposition process and parameters are shown in Table 2.
[0085] Table 2. Process for thermal atomic layer deposition of silicon oxide films using ozone as the oxygen source in a laboratory-scale ALD processing tool. [Table 3]
[0086] After deposition, the samples were subjected to precursor processing in the same lab-scale ALD processing tool. The silicon precursor was delivered to the chamber by vapor draw. The precursor vapor was preheated to 100° C. before entering the deposition region. The ALD diaphragm valves controlled the gas and precursor flow rates with rapid operation.
[0087] Wet etch rate (WER) measurements were performed by using a 1:99 diluted hydrofluoric (HF) acid solution. For each set of experiments, a thermal oxide wafer was used as a standard to confirm the performance of the etching solution. Before starting to collect the WER of the bulk film, the samples were all etched for 15 seconds to remove any surface layer. Following this procedure, the typical wet etch rate of the thermal oxide wafer for the 1:99 diluted HF aqueous solution was 0.5 Å / s. All density measurements were performed by X-ray reflectivity (XRR) technique. Compositional analysis was performed using secondary ion mass spectrometry (D-SIMS) or X-ray photoelectron spectroscopy (XPS). Dielectric constant (k) measurements were performed using a Materials Development Corporation (MDC) mercury probe (Model 802B) calibrated by a thermal oxide standard.
[0088] Example 1: A compound having the formula B, wherein R 1 =R 2 =R 3 =R 4 =R 6 =R 8 = methyl, R 5 =R 7 =R 9 Chemical treatments during thermal atomic layer deposition of silicon-containing films deposited from 2-dimethylamino-2,4,6,8-tetramethylcyclotetrasiloxane where = hydrogen
[0089] Atomic layer deposition of silicon and oxygen containing films was performed using the following precursor: 2-dimethylamino-2,4,6,8-tetramethylcyclotetrasiloxane. The deposition was performed in a laboratory scale ALD processing tool. The silicon precursor was transported to the chamber by vapor extraction. The deposition process and parameters are provided in Table 2. Steps 1-6 are repeated until the desired thickness is reached. The temperature, ozone concentration and GPC of the deposition process are provided in Table 3a and the film properties are provided in 3b. Carbon doped silicon oxide films were obtained at different ozone concentrations at low temperature (100°C).
[0090] Table 3a. Thermal ALD deposition temperature, ozone concentration, and GPC of 2-dimethylamino-2,4,6,8-tetramethylcyclotetrasiloxane in an ozone process. [Table 4]
[0091] Table 3b. Thermal ALD deposition temperature, ozone concentration, and film properties of 2-dimethylamino-2,4,6,8-tetramethylcyclotetrasiloxane in an ozone process. [Table 5]
[0092] Films deposited at 100° C. (Samples A-C) were treated with either the silicon precursor N,N-dimethyltrimethylsilylamine (DMATMS) at 300° C. for 5 min at a precursor chamber pressure of 0.3 Torr, or with the silicon precursor N,N-diethylaminotrimethylsilylamine (DEATMS) at 450° C. for 5 min at 0.3 Torr. The k values of the films before and after treatment and the WER after treatment are shown in Table 4.
[0093] Table 4. k values and WER of SiOC films before and after chemical treatment with DMATMS at 300°C or DEATMS at 450°C. [Table 6]
[0094] Example 2: A compound having the formula C, wherein R 1 and R 2 is ethyl, and R 10 Chemical processing for thermal atomic layer deposition of carbon-doped silicon oxide films using diethylaminomethylsilane (=methyl)
[0095] Atomic layer deposition of silicon oxide films was performed using the following precursor: diethylaminomethylsilane. The deposition was performed in a laboratory-scale ALD processing tool. The silicon precursor was transported into the chamber by vapor extraction. The deposition process and parameters are provided in Table 2. Steps 1-6 were repeated until the desired thickness was reached. The substrate temperature was 100° C. The deposition temperature, ozone concentration, GPC and film properties are provided in Table 5.
[0096] Table 5. Thermal ALD deposition temperature of diethylaminomethylsilane in ozone process, GPC [Table 7]
[0097] Films deposited at 100° C. were treated with the silicon precursor N,N-diethylaminotrimethylsilylamine (DEATMS) at 300° C. for 5 and 25 min, with the silicon precursor di-iso-propylaminosilane (DIPAS) at 300° C. for 5 and 10 min, or annealed at 300° C. without any chemical treatment. The k values of the films before and after the different treatments are shown in Table 6.
[0098] Table 6. k values of carbon-doped silicon oxide films before and after chemical treatment with DEATMS at 300°C or with DIPAS at 300°C. [Table 8]
[0099] Although the present disclosure has been described with reference to certain preferred embodiments, it will be understood by those skilled in the art that various changes can be made and equivalents substituted for those elements without departing from the scope of the invention. In addition, many modifications can be made to adapt a particular situation or material to the teachings of the invention without departing from the essential scope thereof. Therefore, it is not intended that the invention be limited to the particular embodiments, but rather that the invention will include all embodiments falling within the scope of the appended claims. The present invention can be embodied in the following manner. (Appendix 1) 1. A method for depositing a carbon-doped silicon oxide film on a substrate, comprising: a) providing a substrate in a reactor; b) Formulas A~C: [ka] wherein R 1 But linear C1~C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C3-C 10 Alkenyl groups, C3-C 10 Alkynyl groups and C4-C 10 aryl groups; R 2 But hydrogen, C1-C 10 Straight chain alkyl group, branched chain C3~C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C2-C 10 Alkenyl groups, C2-C 10 Alkynyl groups and C4-C 10 R in formula A or B is selected from the group consisting of aryl groups. 1 and R 2 and are either linked to form a cyclic ring structure or are not linked to form a cyclic ring structure; R 3-9 But hydrogen, straight chain C1-C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C2-C 10 Alkenyl groups, C2-C 10 Alkynyl groups and C4-C 10 R is independently selected from the group consisting of aryl groups; 10 But linear C1~C 10 Alkyl groups, C2-C 10 Alkenyl groups and C2-C 10introducing at least one first silicon precursor selected from an alkynyl group into a reactor; c) purging the reactor using a purge gas to remove at least a portion of any of the at least one first silicon precursor that is not absorbed on the substrate; d) introducing an oxygen-containing source into the reactor to react with the at least one first silicon precursor to form a silicon oxide film; e) purging the reactor with a purge gas to remove at least a portion of any unreacted oxygen-containing source; f) repeating steps b) through e) until a silicon oxide film of a desired thickness is deposited; g)R 3 x Si(NR 1 R 2 ) 4-x wherein R 1-3 treating the silicon oxide film with a second silicon precursor, wherein x=1, 2 or 3, as defined above, to form a carbon doped silicon oxide film; h) purging the reactor using a purge gas to remove at least a portion of any by-products from the process of treating the silicon oxide film with the second silicon precursor; and carried out at one or more temperatures in the range of about 20° C. to 300° C. (Appendix 2) R 1-2 Each of the following is a C1 to C4 alkyl group: (Appendix 3) R 1-3 is independently selected from the group consisting of methyl and ethyl. (Appendix 4) The at least one first silicon precursor compound is selected from the group consisting of 2-dimethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-diethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-ethylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-isopropylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-dimethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-diethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-ethylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-iso-propylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-dimethylamino-2,4,6-trimethylcyclotrisiloxane, 2-diethylamino-2,4,6-trimethylcyclotrisiloxane, 2-ethylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-iso-propylamino-2,4,6-trimethylcyclotrisiloxane, 2-dimethylamino-2,4,6,8- Tetramethylcyclotetrasiloxane, 2-diethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-ethylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-isopropylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-pyrrolidino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-pyrrolyl-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-piperidino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-2,5-dimethylpiperidino -2,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclohexylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-phenylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclohexylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclopentylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-pyrrolidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-pyrrolyl-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-phenylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclopentylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-pyrrolidino-2 ,4,6-trimethylcyclotrisiloxane, 2-pyrrolyl-2,4,6-trimethylcyclotrisiloxane, 2-cyclohexylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-phenylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-cyclohexylamino-2,4,6-trimethylcyclotrisiloxane, 2-cyclopentylamino-2,4,6-trimethylcyclotrisiloxane, 2-pyrrolidino-2,4,6,8-tetramethylcyclotrisiloxane Methylcyclotetrasiloxane, 2-pyrrolyl-2,4,6,8-tetramethylcyclotetrasiloxane, 2-piperidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-2,5-dimethylpiperidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-phenylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane The method according to claim 1, wherein the silane is selected from the group consisting of silane, 2-cyclohexylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-cyclopentylamino-2,4,6,8-tetramethylcyclotetrasiloxane, dimethylaminomethylsilane, diethylaminomethylsilane, di-iso-propylaminomethylsilane, di-sec-butylaminomethylsilane, cyclohexylmethylaminomethylsilane, and 2,6-dimethylpiperidinomethylsilane. (Appendix 5) The at least one second silicon precursor compound is selected from the group consisting of diethylaminotriethylsilane, dimethylaminotriethylsilane, ethylmethylaminotriethylsilane, t-butylaminotriethylsilane, iso-propylaminotriethylsilane, di-isopropylaminotriethylsilane, pyrrolidinotriethylsilane, diethylaminotrimethylsilane, dimethylaminotrimethylsilane, ethylmethylaminotrimethylsilane, t-butylaminotrimethylsilane, iso-propylaminotrimethylsilane, di-isopropylaminotrimethylsilane, pyrrolidinotrimethylsilane, diethylaminodimethylsilane, dimethylaminodimethylsilane, ethylmethylaminodimethylsilane, t-butylaminodimethylsilane, iso-propylaminodimethylsilane, di-isopropylaminodimethylsilane, pyrrolidinodimethylsilane, diethylaminodiethylsilane, dimethylaminodiethylsilane, ethylmethylaminodiethylsilane, t-butylaminodiethylsilane, iso-propylaminodiethylsilane, di-isopropylaminodiethylsilane, pyrrolidinodiethyl Silane, bis(diethylamino)dimethylsilane, bis(dimethylamino)dimethylsilane, bis(ethylmethylamino)dimethylsilane, bis(di-isopropylamino)dimethylsilane, bis(iso-propylamino)dimethylsilane, bis(tert-butylamino)dimethylsilane, dipyrrolidinodimethylsilane, bis(diethylamino)diethylsilane, bis(dimethylamino)diethylsilane, bis(ethylmethylamino)diethylsilane, bis(di-isopropylamino)diethylsilane, bis(iso-propylamino)di Ethylsilane, bis(tert-butylamino)diethylsilane, dipyrrolidinodiethylsilane, bis(diethylamino)methylvinylsilane, bis(dimethylamino)methylvinylsilane, bis(ethylmethylamino)methylvinylsilane, bis(di-isopropylamino)methylvinylsilane, bis(iso-propylamino)methylvinylsilane, bis(tert-butylamino)methylvinylsilane, dipyrrolidinomethylvinylsilane, 2,6-dimethylpiperidinomethylsilane, 2,6-dimethylpiperidinodimethylsilane, 2,The method according to claim 1, wherein the silane is selected from the group consisting of 6-dimethylpiperidinotrimethylsilane, tris(dimethylamino)phenylsilane, tris(dimethylamino)methylsilane and tris(dimethylamino)ethylsilane. (Appendix 6) a wet etch rate of less than about 2.5 Å / s, as measured in a solution of dilute HF (0.5 wt % dHF) acid in 1:99 HF:water; and a wet etch rate of less than about 5×10, as measured by secondary ion mass spectrometry (SIMS). 20 A carbon-doped silicon oxide film deposited by the method described in Appendix 1, having at least one characteristic selected from the group consisting of: hydrogen impurities less than at / cc; and a dielectric constant of 5.0 or less. (Appendix 7) 1. A method for depositing a carbon-doped silicon oxide film on a substrate, comprising: a) providing a substrate in a reactor; b) Formulas A~C: [ka] wherein R 1 But linear C1~C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C3-C 10 Alkenyl groups, C3-C 10 Alkynyl groups and C4-C 10 aryl groups; R 2 But hydrogen, C1-C 10 Straight chain alkyl group, branched chain C3~C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C3-C 10 Heterocyclic groups, C2-C 10 Alkenyl groups, C2-C 10 Alkynyl groups and C4-C 10 R in formula A or B is selected from the group consisting of aryl groups. 1 and R 2and are either linked to form a cyclic ring structure or are not linked to form a cyclic ring structure; R 3-9 But hydrogen, straight chain C1-C 10 Alkyl group, branched chain C3-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups, C2-C 10 Alkenyl groups, C2-C 10 Alkynyl groups and C4-C 10 R is independently selected from the group consisting of aryl groups; 10 But linear C1~C 10 Alkyl groups, C2-C 10 Alkenyl groups and C2-C 10 introducing at least one first organoaminopolysiloxane precursor selected from an alkynyl group into a reactor; c) purging the reactor with a purge gas to remove at least a portion of any of the at least one first silicon precursor that is not absorbed on the substrate; d) introducing an oxygen-containing plasma source into the reactor to react with the at least one first silicon precursor to form a first silicon-containing film; e) purging the reactor using a purge gas to remove at least a portion of any unreacted oxygen-containing plasma source; f) repeating steps b) through e) until a first silicon-containing film of a desired thickness is deposited; g)R 3 x Si(NR 1 R 2 ) 4-x wherein R 1-3 introducing at least one second silicon precursor into the reactor, wherein x=1, 2 or 3; h) purging the reactor using a purge gas to remove at least a portion of any of the at least one second silicon precursor that is not absorbed into the first silicon-containing film; i) introducing an oxygen-containing source into a reactor to form a second silicon-containing film; j) purging the reactor with a purge gas to remove at least a portion of any unreacted oxygen-containing source; k) repeating steps g) through j) until a second silicon-containing film of a desired thickness is deposited. and carried out at one or more temperatures in the range of about 20° C. to 300° C. (Appendix 8) R 1-2 and each of is a C1 to C4 alkyl group. (Appendix 9) R 1-3 and each is independently selected from the group consisting of methyl and ethyl. (Appendix 10) The first silicon precursor compound is 2-dimethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-diethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-ethylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-isopropylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-dimethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-diethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-ethylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-iso-propylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-dimethylamino-2,4,6-trimethylcyclotrisiloxane, 2-diethylamino-2,4,6-trimethylcyclotrisiloxane, 2-ethylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-iso-propylamino-2,4,6-trimethylcyclotrisiloxane, 2-dimethylamino-2,4,6,8-tetramethyl ethylcyclotetrasiloxane, 2-diethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-ethylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-isopropylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-pyrrolidino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-pyrrolyl-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-piperidino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-2,5-dimethylpiperidino-2 ,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclohexylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-phenylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclohexylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclopentylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-pyrrolidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-pyrrolyl-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-phenylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclopentylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-pyrrolidino-2 ,4,6-trimethylcyclotrisiloxane, 2-pyrrolyl-2,4,6-trimethylcyclotrisiloxane, 2-cyclohexylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-phenylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-cyclohexylamino-2,4,6-trimethylcyclotrisiloxane, 2-cyclopentylamino-2,4,6-trimethylcyclotrisiloxane, 2-pyrrolidino-2,4,6,8-tetramethylcyclotrisiloxane Methylcyclotetrasiloxane, 2-pyrrolyl-2,4,6,8-tetramethylcyclotetrasiloxane, 2-piperidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-2,5-dimethylpiperidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-phenylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane 8. The method according to claim 7, wherein the silane is selected from the group consisting of silane, 2-cyclohexylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-cyclopentylamino-2,4,6,8-tetramethylcyclotetrasiloxane, dimethylaminomethylsilane, diethylaminomethylsilane, di-iso-propylaminomethylsilane, di-sec-butylaminomethylsilane, cyclohexylmethylaminomethylsilane, and 2,6-dimethylpiperidinomethylsilane. (Appendix 11) 8. The method of claim 7, wherein the at least one second silicon precursor compound is selected from the group consisting of di-iso-propylaminosilane, di-sec-butylaminosilane, bis(diethylamino)silane, and bis(tert-butylamino)silane. (Appendix 12) a density of at least about 2.1 g / cc; a wet etch rate of less than about 2.5 Å / s as measured in a solution of dilute HF (0.5 wt % dHF) acid in 1:99 HF:water; and a wet etch rate of less than about 5×10 as measured by secondary ion mass spectrometry (SIMS). 20 8. A carbon-doped silicon oxide film deposited by the method of claim 7, having at least one characteristic selected from the group consisting of: hydrogen impurities less than at / cc; and a dielectric constant of 5.0 or less.
Claims
1. 1. A method for depositing a carbon-doped silicon oxide film on a substrate, comprising: a) providing a substrate in a reactor; b) Formulas A to C: [Formula 1] wherein R 1 But linear C 1 ~C 10 Alkyl group, branched chain C 3 ~C 10 Alkyl group, C 3 ~C 10 Cyclic alkyl group, C 3 ~C 10 Heterocyclic group, C 3 ~C 10 Alkenyl group, C 3 ~C 10 Alkynyl group and C 4 ~C 10 aryl groups; R 2 is hydrogen, C 1 ~C 10 Straight chain alkyl group, branched chain C 3 ~C 10 Alkyl group, C 3 ~C 10 Cyclic alkyl group, C 3 ~C 10 Heterocyclic group, C 2 ~C 10 Alkenyl group, C 2 ~C 10 Alkynyl group and C 4 ~C 10 aryl groups; R in formula A or B is selected from the group consisting of 1 and R 2 and are either linked to form a cyclic ring structure or are not linked to form a cyclic ring structure; R 3-9 is hydrogen, linear C 1 ~C 10 Alkyl group, branched chain C 3 ~C 10 Alkyl group, C 3 ~C 10 Cyclic alkyl group, C 2 ~C 10 Alkenyl group, C 2 ~C 10 Alkynyl group and C 4 ~C 10 aryl groups; R 10 But linear C 1 ~C 10 Alkyl group, C 2 ~C 10 Alkenyl group and C 2 ~C 10 introducing at least one first silicon precursor selected from an alkynyl group into a reactor; c) purging the reactor using a purge gas to remove at least a portion of any of the at least one first silicon precursor that is not absorbed on the substrate; d) introducing an oxygen-containing source into the reactor to react with the at least one first silicon precursor to form a silicon oxide film; e) purging the reactor with a purge gas to remove at least a portion of any unreacted oxygen-containing source; f) repeating steps b) through e) until a silicon oxide film of a desired thickness is deposited; g) R 3 x Si(NR 1 R 2 ) 4-x wherein R 1-3 treating the silicon oxide film with a second silicon precursor, wherein x=1, 2, or 3, as defined above, to form a carbon-doped silicon oxide film, wherein the second silicon precursor does not react with the oxygen-containing source by introducing the oxygen-containing source into the reactor; h) purging the reactor using a purge gas to remove at least a portion of any by-products from the process step of treating the silicon oxide film with the second silicon precursor; wherein the process is carried out at one or more temperatures in the range of 20°C to 300°C.
2. R 1-2 Each of these is C 1 ~C 4The method of claim 1 , wherein the group is an alkyl group.
3. R 1-3 2. The method of claim 1 , wherein each is independently selected from the group consisting of methyl and ethyl.
4. The at least one first silicon precursor compound is selected from the group consisting of 2-dimethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-diethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-ethylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-isopropylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-dimethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-diethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-ethylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-iso-propylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-dimethylamino-2,4,6-trimethylcyclotrisiloxane, 2-diethylamino-2,4,6-trimethylcyclotrisiloxane, 2-ethylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-iso-propylamino-2,4,6-trimethylcyclotrisiloxane, 2-dimethylamino-2,4,6,8- Tetramethylcyclotetrasiloxane, 2-diethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-ethylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-isopropylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-pyrrolidino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-pyrrolyl-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-piperidino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-2,5-dimethylpiperidino -2,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclohexylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-phenylmethylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclohexylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-cyclopentylamino-2,4,4,6,6-pentamethylcyclotrisiloxane, 2-pyrrolidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-pyrrolyl-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-phenylmethylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclopentylamino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-pyrrolidino-2 ,4,6-trimethylcyclotrisiloxane, 2-pyrrolyl-2,4,6-trimethylcyclotrisiloxane, 2-cyclohexylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-phenylmethylamino-2,4,6-trimethylcyclotrisiloxane, 2-cyclohexylamino-2,4,6-trimethylcyclotrisiloxane, 2-cyclopentylamino-2,4,6-trimethylcyclotrisiloxane, 2-pyrrolidino-2,4,6,8-tetramethylcyclotrisiloxane Methylcyclotetrasiloxane, 2-pyrrolyl-2,4,6,8-tetramethylcyclotetrasiloxane, 2-piperidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-2,5-dimethylpiperidino-2,4,4,6,6,8,8-heptamethylcyclotetrasiloxane, 2-cyclohexylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-phenylmethylamino-2,4,6,8-tetramethylcyclotetrasiloxane The method according to claim 1, wherein the silane is selected from the group consisting of silane, 2-cyclohexylamino-2,4,6,8-tetramethylcyclotetrasiloxane, 2-cyclopentylamino-2,4,6,8-tetramethylcyclotetrasiloxane, dimethylaminomethylsilane, diethylaminomethylsilane, di-iso-propylaminomethylsilane, di-sec-butylaminomethylsilane, cyclohexylmethylaminomethylsilane and 2,6-dimethylpiperidinomethylsilane.
5. The at least one second silicon precursor compound is selected from the group consisting of diethylaminotriethylsilane, dimethylaminotriethylsilane, ethylmethylaminotriethylsilane, t-butylaminotriethylsilane, iso-propylaminotriethylsilane, di-isopropylaminotriethylsilane, pyrrolidinotriethylsilane, diethylaminotrimethylsilane, dimethylaminotrimethylsilane, ethylmethylaminotrimethylsilane, t-butylaminotrimethylsilane, iso-propylaminotrimethylsilane, di-isopropylaminotrimethylsilane, pyrrolidinotrimethylsilane, diethylaminodimethylsilane, dimethylaminodimethylsilane, ethylmethylaminodimethylsilane, t-butylaminodimethylsilane, iso-propylaminodimethylsilane, di-isopropylaminodimethylsilane, pyrrolidinodimethylsilane, diethylaminodiethylsilane, dimethylaminodiethylsilane, ethylmethylaminodiethylsilane, t-butylaminodiethylsilane, iso-propylaminodiethylsilane, di-isopropylaminodiethylsilane, pyrrolidinodiethyl Silane, bis(diethylamino)dimethylsilane, bis(dimethylamino)dimethylsilane, bis(ethylmethylamino)dimethylsilane, bis(di-isopropylamino)dimethylsilane, bis(iso-propylamino)dimethylsilane, bis(tert-butylamino)dimethylsilane, dipyrrolidinodimethylsilane, bis(diethylamino)diethylsilane, bis(dimethylamino)diethylsilane, bis(ethylmethylamino)diethylsilane, bis(di-isopropylamino)diethylsilane, bis(iso-propylamino)di Ethylsilane, bis(tert-butylamino)diethylsilane, dipyrrolidinodiethylsilane, bis(diethylamino)methylvinylsilane, bis(dimethylamino)methylvinylsilane, bis(ethylmethylamino)methylvinylsilane, bis(di-isopropylamino)methylvinylsilane, bis(iso-propylamino)methylvinylsilane, bis(tert-butylamino)methylvinylsilane, dipyrrolidinomethylvinylsilane, 2,6-dimethylpiperidinomethylsilane, 2,6-dimethylpiperidinodimethylsilane, 2,The method according to claim 1, wherein the silane is selected from the group consisting of 6-dimethylpiperidinotrimethylsilane, tris(dimethylamino)phenylsilane, tris(dimethylamino)methylsilane and tris(dimethylamino)ethylsilane.
6. a wet etch rate of less than 2.5 Å / s as measured in a solution of dilute HF (0.5 wt % dHF) acid in 1:99 HF:water; and a wet etch rate of less than 5×10 as measured by secondary ion mass spectrometry (SIMS). 20 13. A carbon doped silicon oxide film deposited by the method of claim 1, comprising at least one of the characteristics selected from the group consisting of: less than at / cc hydrogen impurity; and a dielectric constant of 5.0 or less.
Citation Information
Patent Citations
Compositions and methods for depositing carbon-doped silicon-containing films
JP2014523638A
Compositions and methods for deposition of silicon oxide films
JP2015188087A
Organoamino-functionalized linear and cyclic oligosiloxanes for deposition of silicon-containing films
JP2018154615A