Negative electrode of secondary battery, method for fabricating the negative electrode, and secondary battery using the negative electrode
The use of high and low aspect ratio Si-containing particles with graphite in a specific mass ratio stabilizes the electrode structure, addressing capacity deterioration and maintaining high cycle characteristics in secondary batteries.
Patent Information
- Application Number
- JP2023083565
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2043-05-22
AI Technical Summary
Si-containing particles in negative electrodes of secondary batteries experience significant volume changes during charging and discharging, leading to decreased filling properties and conductive path breakage, resulting in capacity deterioration and poor cycle characteristics.
A negative electrode configuration using a combination of graphite particles, first Si-containing particles with a high aspect ratio, and second Si-containing particles with a lower aspect ratio, where the first Si-containing particles have an aspect ratio of 4.0 to 10.0 and the second Si-containing particles have an aspect ratio of 1.0 to 3.0, with a mass ratio of 10:90 to 50:50, to stabilize the structure and prevent capacity deterioration.
The proposed electrode design effectively suppresses capacity deterioration during repeated charging and discharging, maintaining high cycle characteristics and capacity retention.
Smart Images

Figure 2024167467000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative electrode for a secondary battery and a method for producing the same, and also to a secondary battery using the negative electrode. [Background technology]
[0002] 2. Description of the Related Art In recent years, secondary batteries have been suitably used as portable power sources for personal computers, mobile terminals, and the like, and as power sources for driving vehicles such as electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), and the like.
[0003] In applications as a power source for driving vehicles, particularly BEVs, secondary batteries are desired to have a higher capacity from the viewpoint of extending the driving range of the vehicle. Si-containing particles are known as a high-capacity negative electrode active material, and it is known that the Si-containing particles can increase the capacity of secondary batteries (see, for example, Patent Document 1). Patent Document 1 discloses a technology in which Si-containing particles and graphite particles such as natural graphite are used in combination as a negative electrode active material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-38862 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, while the Si-containing particles have a high capacity, they undergo a large volume change due to expansion / contraction when the secondary battery is charged and discharged. Therefore, when the Si-containing particles and the graphite particles are used in combination, particularly when the ratio of the Si-containing particles is large, the packing property of these particles decreases when the secondary battery is repeatedly charged and discharged, which may cause the conductive path to be broken, internal stress, etc. Therefore, when the Si-containing particles and the graphite particles are used in combination, there is a problem that the cycle characteristics of the secondary battery are reduced, specifically, there is a problem that the capacity deterioration is large when the secondary battery is repeatedly charged and discharged.
[0006] In view of the above circumstances, an object of the present invention is to provide a negative electrode containing Si-containing particles and graphite particles, which is capable of suppressing capacity degradation when a secondary battery is repeatedly charged and discharged. [Means for solving the problem]
[0007] The negative electrode disclosed herein includes a negative electrode current collector and a negative electrode active material layer supported by the negative electrode current collector. The negative electrode active material layer contains graphite particles, first Si-containing particles, and second Si-containing particles. The first Si-containing particles have a larger aspect ratio than the second Si-containing particles. The aspect ratio of the first Si-containing particles is 4.0 to 10.0, and the aspect ratio of the second Si-containing particles is 1.0 to 3.0. The mass ratio of the first Si-containing particles to the second Si-containing particles is 10:90 to 50:50.
[0008] According to this configuration, it is possible to provide a negative electrode that contains Si-containing particles and graphite particles and that can suppress capacity degradation when the secondary battery is repeatedly charged and discharged.
[0009] From another aspect, a method for manufacturing a negative electrode of a secondary battery disclosed herein includes the steps of preparing a negative electrode paste containing graphite particles, first Si-containing particles, second Si-containing particles, and a dispersion medium, applying the negative electrode paste to a negative electrode current collector, drying the applied negative electrode paste to form a negative electrode active material layer, and pressing the negative electrode active material layer. The first Si-containing particles have a larger aspect ratio than the second Si-containing particles. The aspect ratio of the first Si-containing particles is 4.0 to 10.0, and the aspect ratio of the second Si-containing particles is 1.0 to 3.0. The mass ratio of the first Si-containing particles to the second Si-containing particles is 10:90 to 50:50.
[0010] The negative electrode obtained by such a configuration can impart excellent resistance to capacity degradation to the secondary battery when repeatedly charged and discharged.
[0011] From another aspect, the present disclosure provides a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, the negative electrode being the above-described negative electrode.
[0012] According to this configuration, it is possible to provide a secondary battery that has excellent resistance to capacity degradation when repeatedly charged and discharged. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a cross-sectional view illustrating a schematic configuration of a negative electrode of a secondary battery according to one embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view that illustrates a schematic configuration of particles contained in a negative electrode active material layer of the negative electrode of FIG. 1. [Diagram 3] FIG. 1 is a cross-sectional view showing a schematic configuration of a lithium ion secondary battery constructed using a negative electrode of a secondary battery according to one embodiment of the present invention. [Figure 4] 4 is a schematic exploded view showing the configuration of a wound electrode body of the lithium ion secondary battery of FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Matters not mentioned in this specification but necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field. In addition, in the following drawings, members and parts having the same function are described with the same reference numerals. Furthermore, the dimensional relationships (length, width, thickness, etc.) in each drawing do not reflect the actual dimensional relationships. In addition, the numerical range expressed as "A to B" in this specification includes A and B.
[0015] In this specification, the term "secondary battery" refers to an electricity storage device that can be repeatedly charged and discharged. In addition, in this specification, the term "lithium ion secondary battery" refers to a secondary battery that uses lithium ions as a charge carrier and realizes charging and discharging by the transfer of charge associated with the lithium ions between the positive and negative electrodes.
[0016] The negative electrode disclosed herein is used in a secondary battery, and is preferably used in a lithium ion secondary battery. One embodiment of the negative electrode disclosed herein will be specifically described with reference to FIG. 1. FIG. 1 is a cross-sectional view that typically illustrates an example of a negative electrode 60 according to this embodiment, and is a cross-sectional view along the thickness direction and the width direction. The negative electrode 60 according to this embodiment shown in FIG. 1 is a negative electrode for a lithium ion secondary battery.
[0017] As shown in the figure, the negative electrode 60 includes a negative electrode current collector 62 and a negative electrode active material layer 64 supported by the negative electrode current collector 62. In other words, the negative electrode 60 includes the negative electrode current collector 62 and the negative electrode active material layer 64 provided on the negative electrode current collector 62. The negative electrode active material layer 64 may be provided on only one side of the negative electrode current collector 62, or may be provided on both sides of the negative electrode current collector 62 as in the illustrated example. The negative electrode active material layer 64 is preferably provided on both sides of the negative electrode current collector 62.
[0018] As shown in the illustrated example, a negative electrode active material layer non-forming portion 62a where no negative electrode active material layer 64 is provided may be provided at one end in the width direction of the negative electrode 60. In the negative electrode active material layer non-forming portion 62a, the negative electrode current collector 62 is exposed, and the negative electrode active material layer non-forming portion 62a can function as a current collector. However, the configuration for collecting current from the negative electrode 60 is not limited to this.
[0019] In the illustrated example, the shape of the negative electrode collector 62 is a foil (or sheet), but is not limited thereto. The negative electrode collector 62 may have various forms such as a rod, a plate, a mesh, etc. As with conventional lithium ion secondary batteries, the material of the negative electrode collector 62 may be a metal with good electrical conductivity (e.g., copper, nickel, titanium, stainless steel, etc.), and among these, copper is preferable. Copper foil is particularly preferable as the negative electrode collector 62.
[0020] The dimensions of the negative electrode current collector 62 are not particularly limited and may be appropriately determined depending on the battery design. When a copper foil is used as the negative electrode current collector 62, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 6 μm or more and 20 μm or less.
[0021] The negative electrode active material layer 64 contains a negative electrode active material. At least graphite particles, first Si-containing particles with a high aspect ratio, and second Si-containing particles with a low aspect ratio are used as the negative electrode active material. This will be described in detail with reference to FIG. 2. FIG. 2 is a schematic cross-sectional view showing particles contained in the negative electrode active material layer 64 shown in FIG. 1. As shown in FIG. 2, the negative electrode active material layer 64 contains graphite particles 12, first Si-containing particles 14 with a high aspect ratio, and second Si-containing particles 16 with a low aspect ratio.
[0022] The graphite constituting the graphite particles 12 may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.
[0023] The shape of the graphite particles 12 is not particularly limited and may be flaky, spherical, etc. The graphite particles 12 are preferably spheroidized graphite particles. When the graphite particles 12 are spherical, the circularity of the graphite particles 12 is preferably 0.85 to 1, more preferably 0.88 to 1, and further preferably 0.90 to 1.
[0024] In this specification, "circularity" refers to the ratio of the perimeter of a perfect circle having the same area as the projected area of the particle to the perimeter of the projected image of the particle (i.e., circularity = perimeter of a perfect circle having the same area as the projected area of the particle / perimeter of the projected image of the particle). Therefore, the closer the circularity is to 1, the closer the projected image of the particle is to a perfect circle, and the closer the particle is to a perfect sphere. The circularity can be determined, for example, by using a commercially available static automatic image analyzer to determine the circularity of 100 or more particles and calculating the average value.
[0025] There is no particular limitation on the average particle diameter (D50) of the graphite particles 12. The average particle diameter (D50) of the graphite particles 12 is, for example, 1 μm to 30 μm, preferably 5 μm to 25 μm, more preferably 10 μm to 23 μm, and further preferably 12 μm to 20 μm.
[0026] In this specification, the term "average particle size (D50)" refers to the median size (D50), which is the particle size corresponding to a cumulative frequency of 50 volume % from the fine particle side with a small particle size in the volume-based particle size distribution based on the laser diffraction / scattering method. The average particle size (D50) can be determined using a commercially available laser diffraction / scattering type particle size distribution measuring device, etc.
[0027] The content ratio of the graphite particles to the total of the graphite particles 12, the first Si-containing particles 14, and the second Si-containing particles 16 is preferably 40 mass% to 90 mass%, more preferably 45 mass% to 85 mass%, and even more preferably 50 mass% to 80 mass%.
[0028] The first Si-containing particle 14 and the second Si-containing particle 16 may be, for example, particles of a Si-C composite material. The Si-C composite material typically includes a carbon domain and a Si-containing domain. The first Si-containing particle 14 and the second Si-containing particle 16 may not be a Si-C composite material, and may be Si particles, Si oxide particles, or the like.
[0029] The carbon domains are, for example, carbonized products of carbon precursors (e.g., petroleum pitch, coal pitch, phenolic resin, etc.); graphite, etc. The carbon domains preferably constitute a carbon matrix. Thus, the Si-C composite material is preferably a material in which a plurality of Si-containing domains are dispersed in a carbon matrix. In this case, it is advantageous because the carbon matrix can mitigate the volume change caused by the expansion / contraction of the Si-containing domains.
[0030] The Si-containing domain contains Si, for example, Si, Si oxide (SiO x ), Si nitrides (SiNx), Si carbides (SiCx), etc. The Si-containing domain is preferably composed of Si and Si oxides (SiO x The Si-containing domain may be a fine particle.
[0031] The average particle diameter of the Si-containing domain is, for example, 50 nm or less, and may be 5 nm to 50 nm. The "average particle diameter of the Si-containing domain" can be obtained as follows. First, the negative electrode active material layer 64 is processed with FIB (focused ion beam) to prepare a sample for observation with a scanning transmission electron microscope (STEM). Then, the sample is subjected to elemental analysis by EDX element mapping, and then a BF image (bright field image) and a HAADF image (high angle scattering annular dark field image) are obtained. The diameter of the Si-containing domain can be obtained from the contrast and shape obtained from the BF image and the HAADF image. The diameters of 10 or more arbitrarily selected Si-containing domains are obtained, and the average value is defined as the "average particle diameter of the Si-containing domain" here.
[0032] The Si-C composite material is, for example, a material in which fine particles containing Si are dispersed inside a carbon material; or a material in which fine particles containing Si are embedded in the pores of granulated porous graphite; etc.
[0033] The Si content in the first Si-containing particle 14 and the Si content in the second Si-containing particle 16 are not particularly limited. The Si content in the first Si-containing particle 14 and the Si content in the second Si-containing particle 16 are each preferably 20 mass% to 80 mass%, more preferably 30 mass% to 70 mass%, and further preferably 40 mass% to 60 mass%. The ratio of the Si content in the first Si-containing particle 14 to the Si content in the second Si-containing particle 16 is preferably 1.0 or less.
[0034] In order to obtain a suitable filling state between the first Si-containing particles 14 and the second Si-containing particles 16, the mass ratio of the first Si-containing particles 14 to the second Si-containing particles 16 is 10:90 to 50:50, preferably 15:85 to 40:60, more preferably 18:82 to 35:65, and even more preferably 20:80 to 30:70.
[0035] The total content of the first Si-containing particles 14 and the second Si-containing particles 16 with respect to the total of the graphite particles 12, the first Si-containing particles 14, and the second Si-containing particles 16 is preferably 10 mass% to 60 mass%, more preferably 15 mass% to 55 mass%, and even more preferably 20 mass% to 50 mass%.
[0036] The aspect ratio of the first Si-containing particle 14 is larger than that of the second Si-containing particle 16. The aspect ratio of the first Si-containing particle 14 is 4.0 to 10.0. The aspect ratio of the second Si-containing particle 16 is 1.0 to 3.0. Therefore, the second Si-containing particle 16 has a spherical or nearly spherical shape.
[0037] By using such first Si-containing particles 14 and second Si-containing particles 16 together with graphite particles at a predetermined mass ratio, it is possible to suppress the capacity degradation during repeated charging and discharging of the secondary battery. The reason for this is considered to be as follows.
[0038] When such first Si-containing particles 14 and second Si-containing particles 16 are contained in the negative electrode active material layer 64, the first Si-containing particles 14 having a high aspect ratio are filled like wedges into the gaps between the second Si-containing particles 16 having a low aspect ratio (in other words, substantially spherical). As a result, the Si-containing particles are less likely to deform when the secondary battery is charged and discharged, and the internal stress during expansion / contraction can be alleviated, thereby suppressing the displacement of the Si-containing particles. In addition, the conductive path can be suppressed. This makes it possible to suppress the capacity degradation when the secondary battery is repeatedly charged and discharged.
[0039] Therefore, if the aspect ratio of the first Si-containing particle 14 is too small, the first Si-containing particle 14 is difficult to enter into the gap between the second Si-containing particles 16. On the other hand, if the aspect ratio of the first Si-containing particle 14 is too large, the filling property decreases. For this reason, the aspect ratio of the first Si-containing particle 14 is 4.0 to 10.0, preferably 4.5 to 9.0, more preferably 5.0 to 9.0, and further preferably 5.0 to 7.0. The first Si-containing particle 14 is preferably a Si-C composite particle in which a Si-containing domain is introduced into flake graphite or flake graphite granules.
[0040] If the second Si-containing particles 16 are too non-spherical, their packing properties decrease. Therefore, the aspect ratio of the second Si-containing particles 16 is 1.0 to 3.0, preferably 1.0 to 2.0, more preferably 1.0 to 1.5, and further preferably 1.0 to 1.3. The second Si-containing particles 16 are preferably Si-C composite particles in which Si-containing domains are introduced into spherical graphite granules.
[0041] In this specification, the aspect ratio of a particle refers to the ratio of the long axis diameter of the particle to the short axis diameter of the particle (long axis diameter / short axis diameter). The aspect ratios of the first Si-containing particle 14 and the second Si-containing particle 16 can be obtained by acquiring images of the first Si-containing particle 14 and the second Si-containing particle 16, respectively, determining the ratio of the long axis diameter to the short axis diameter (long axis diameter / short axis diameter) for 100 or more arbitrarily selected particles, and calculating the average value. The aspect ratio can be easily measured using an image-type particle size distribution analyzer.
[0042] 2 is a schematic diagram conceptually illustrating the packed state of the first Si-containing particles 14 and the second Si-containing particles 16, the arrangement of the graphite particles 12, the first Si-containing particles 14, and the second Si-containing particles 16 in the negative electrode active material layer 64 is not limited to the illustrated example. All the first Si-containing particles 14 do not have to be inserted between the second Si-containing particles 16 like wedges.
[0043] There is no particular limitation on the sizes of the first Si-containing particle 14 and the second Si-containing particle 16. The major axis diameter (D1) of the first Si-containing particle 14 is, for example, 2 μm to 15 μm, and preferably 4 μm to 12 μm. The major axis diameter (D2) of the second Si-containing particle 16 is, for example, 2 μm to 10 μm, and preferably 4 μm to 8 μm.
[0044] Here, the cycle characteristics of the secondary battery can be improved if the ratio (D1 / D2) of the major axis diameter (D1) of the first Si-containing particle 14 with a high aspect ratio to the major axis diameter (D2) of the second Si-containing particle 16 with a low aspect ratio is not too long. This is considered to be because the number of first Si-containing particles that fill the gaps between the second Si-containing particles 16 like wedges increases. Therefore, the ratio (D1 / D2) of the major axis diameter (D1) of the first Si-containing particle 14 to the major axis diameter (D2) of the second Si-containing particle 16 is preferably 2 or less, more preferably 1.5 or less, and even more preferably 1.0 or less. The ratio (D1 / D2) may be 0.5 or more, 0.7 or more, or 0.8 or more.
[0045] The major axis diameter (D1) of the first Si-containing particle 14 and the major axis diameter (D2) of the second Si-containing particle 16 can be determined by obtaining images of the first Si-containing particle 14 and the second Si-containing particle 16, respectively, determining the major axis diameters of 100 or more arbitrarily selected particles, and calculating the average value. The major axis diameter (D1) and the major axis diameter (D2) can be easily measured using an image particle size distribution analyzer.
[0046] The first Si-containing particle 14 and the second Si-containing particle 16 can be produced according to a known method. Various methods for producing particles of Si-C composite materials are known (see, for example, JP 2015-38862 A, WO 2014 / 046144 A, and prior art documents cited in the WOs).
[0047] The negative electrode active material layer 64 may contain components other than the negative electrode active material, examples of which include a binder and a conductive material. Examples of the binder include styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), and the like. CMC also functions as a thickener. Examples of the conductive material include carbon black such as acetylene black, carbon fiber, and carbon nanotubes (CNT). Among these, CNT is preferred. When CNT is used as the conductive material, the negative electrode active material layer 64 may contain a dispersant for CNT.
[0048] The content of the negative electrode active material in the negative electrode active material layer 64 (i.e., relative to the total mass of the negative electrode active material layer 64) is preferably 90 mass% or more, and more preferably 95 mass% or more. The content of the binder in the negative electrode active material layer is preferably 0.1 mass% to 8 mass% or less, and more preferably 0.5 mass% to 5 mass% or less. The content of the conductive material in the negative electrode active material layer 64 is preferably 0.01 mass% to 3 mass% or less, and more preferably 0.05 mass% to 1 mass% or less.
[0049] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, not less than 10 μm and not more than 400 μm, and preferably not less than 20 μm and not more than 300 μm.
[0050] The density of the negative electrode active material layer 64 is not particularly limited, but is, for example, 0.7 g / cm 3 or more, preferably 1.0 g / cm 3 More preferably, it is 1.2 g / cm 3 On the other hand, the density of the negative electrode active material layer 64 is, for example, 2.3 g / cm 3 Less than or equal to 2.0 g / cm 3 It may be the following:
[0051] The negative electrode 60 may include members other than the negative electrode current collector 62 and the negative electrode active material layer 64. For example, an insulating layer (not shown) adjacent to the negative electrode active material layer 64 may be provided on the negative electrode active material layer non-forming portion 62a. The insulating layer contains, for example, an insulating inorganic filler or the like.
[0052] The negative electrode 60 can be suitably manufactured by a manufacturing method including a step of preparing a negative electrode paste containing graphite particles 12, first Si-containing particles 14, second Si-containing particles 16, and a dispersion medium (hereinafter also referred to as a "paste preparation step"); a step of applying the prepared negative electrode paste to a negative electrode current collector 62 (hereinafter also referred to as a "coating step"); a step of drying the applied negative electrode paste to form a negative electrode active material layer 64 (hereinafter also referred to as a "drying step"); and a step of pressing the negative electrode active material layer 64 (hereinafter also referred to as a pressing step). Here, the first Si-containing particles 14 have a larger aspect ratio than the second Si-containing particles 16, and the aspect ratio of the first Si-containing particles 14 is 4.0 to 10.0, and the aspect ratio of the second Si-containing particles 16 is 1.0 to 3.0. The mass ratio of the first Si-containing particles to the second Si-containing particles is 10:90 to 50:50.
[0053] In this specification, the term "paste" refers to a mixture in which a part or all of the solid content is dispersed in a dispersion medium, and includes so-called "slurry", "ink", and the like.
[0054] In the paste preparation step, first, the first Si-containing particles 14 having an aspect ratio of 4.0 to 10.0 and the second Si-containing particles 16 having an aspect ratio of 1.0 to 3.0 are prepared. At this time, these are measured so that the mass ratio of the first Si-containing particles to the second Si-containing particles is 10:90 to 50:50.
[0055] The paste can be prepared by mixing the graphite particles 12, the first Si-containing particles 14, the second Si-containing particles 16, and optional components (e.g., binder, conductive material, etc.) with a dispersion medium (e.g., water) using a known mixing device, stirring device, etc. Here, it is preferable to premix the first Si-containing particles 14 and the second Si-containing particles 16 by dry blending, and use the obtained premix to prepare the negative electrode paste. By premixing the first Si-containing particles 14 and the second Si-containing particles 16, the filling state of the first Si-containing particles 14 and the second Si-containing particles 16 in the negative electrode active material layer 64 becomes better, and the cycle characteristics can be further improved. It is preferable to premix the first Si-containing particles 14 and the second Si-containing particles 16 so that they are uniformly mixed.
[0056] The first Si-containing particles 14 and the second Si-containing particles 16 can be premixed by dry blending according to a known method. For example, the first Si-containing particles 14 and the second Si-containing particles 16 can be mixed uniformly using a mixer equipped with a stirring blade (e.g., a disperser, a tumbler mixer, a Henschel mixer, a ribbon mixer, etc.), a Nauta mixer, etc. The obtained premix, graphite particles, and optional components (e.g., a binder, a conductive material, etc.) can be mixed with a dispersion medium (e.g., water) to obtain a negative electrode paste.
[0057] The coating step can be performed according to a known method. Specifically, for example, the coating step can be performed by applying the obtained negative electrode paste onto the negative electrode current collector 62 using a coating device such as a gravure coater, a comma coater, a slit coater, or a die coater.
[0058] The drying step can be carried out according to a known method. Specifically, for example, the dispersion medium is removed from the negative electrode current collector 62 on which the negative electrode paste is applied, using a drying device such as a drying oven, to form the negative electrode active material layer 64. This allows the drying step to be carried out. The drying temperature and drying time may be appropriately determined according to the solid content concentration of the negative electrode paste, and are not particularly limited. The drying temperature is, for example, 60°C or higher and 200°C or lower, and preferably 70°C or higher and 150°C or lower. The drying time is, for example, 10 seconds or higher and 30 minutes or lower, and preferably 30 seconds or higher and 10 minutes or lower.
[0059] The pressing step can be carried out according to a known method. Specifically, the pressing step can be carried out by applying pressure to the negative electrode active material layer 64 formed above using a roller press or the like. The pressing step allows the graphite particles 12, the first Si-containing particles 14, and the second Si-containing particles 16 to be densely packed, and the number of the first Si-containing particles packed like wedges into the gaps between the second Si-containing particles 16 can be increased. In this way, the negative electrode 60 is obtained.
[0060] The negative electrode 60 according to this embodiment can provide the secondary battery with excellent resistance to capacity degradation during repeated charging and discharging. In addition, the negative electrode 60 according to this embodiment uses a negative electrode active material containing Si, so that the capacity of the secondary battery can be increased. Therefore, the secondary battery using the negative electrode 60 according to this embodiment has a high capacity and excellent cycle characteristics.
[0061] From another perspective, the secondary battery disclosed herein includes a positive electrode, a negative electrode, and an electrolyte. The negative electrode is the negative electrode 60 according to the above-described embodiment. Hereinafter, an embodiment of the secondary battery disclosed herein will be described with reference to Figs. 3 and 4, taking a lithium ion secondary battery as an example. The following configuration example is a flat prismatic lithium ion secondary battery having a flat wound electrode body and a flat battery case.
[0062] The lithium ion secondary battery 100 shown in FIG. 3 is a sealed lithium ion secondary battery 100 constructed by housing a flat wound electrode body 20 and a nonaqueous electrolyte (not shown) in a flat rectangular battery case (i.e., an outer container) 30. The battery case 30 is provided with a positive electrode terminal 42 and a negative electrode terminal 44 for external connection, and a thin-walled safety valve 36 that is set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher. The battery case 30 is also provided with an injection port (not shown) for injecting the nonaqueous electrolyte. The positive electrode terminal 42 is electrically connected to a positive electrode current collector plate 42a. The negative electrode terminal 44 is electrically connected to a negative electrode current collector plate 44a. The material of the battery case 30 is, for example, a lightweight metal material with good thermal conductivity, such as aluminum.
[0063] As shown in Fig. 3 and Fig. 4, the wound electrode body 20 has a configuration in which a positive electrode sheet 50 and a negative electrode sheet 60 are overlapped with two long separator sheets 70 interposed therebetween and wound in the longitudinal direction. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed along the longitudinal direction on one or both sides (both sides here) of a long positive electrode current collector 52. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed along the longitudinal direction on one or both sides (both sides here) of a long negative electrode current collector 62. The positive electrode active material layer-free portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode active material layer-free portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends in the winding axis direction (i.e., the sheet width direction perpendicular to the longitudinal direction) of the wound electrode body 20. The positive electrode active material layer-free portion 52a and the negative electrode active material layer-free portion 62a are joined to the positive electrode current collector 42a and the negative electrode current collector 44a, respectively.
[0064] The positive electrode current collector 52 constituting the positive electrode sheet 50 may be a known positive electrode current collector used in lithium ion secondary batteries, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). The positive electrode current collector 52 is preferably aluminum foil.
[0065] The dimensions of the positive electrode current collector 52 are not particularly limited and may be appropriately determined depending on the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0066] The positive electrode active material layer 54 contains a positive electrode active material. As the positive electrode active material, a positive electrode active material having a known composition used in a lithium ion secondary battery may be used. Specifically, for example, as the positive electrode active material, a lithium composite oxide, a lithium transition metal phosphate compound, or the like may be used. The crystal structure of the positive electrode active material is not particularly limited, and may be a layered structure, a spinel structure, an olivine structure, or the like.
[0067] The lithium composite oxide is preferably a lithium transition metal composite oxide containing at least one of Ni, Co, and Mn as a transition metal element, and specific examples thereof include lithium nickel-based composite oxides, lithium cobalt-based composite oxides, lithium manganese-based composite oxides, lithium nickel manganese-based composite oxides, lithium nickel cobalt manganese-based composite oxides, lithium nickel cobalt aluminum-based composite oxides, and lithium iron nickel manganese-based composite oxides.
[0068] In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than those. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may be a semimetal element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I. This also applies to the above-mentioned lithium nickel composite oxide, lithium cobalt composite oxide, lithium manganese composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.
[0069] Examples of the lithium transition metal phosphate compound include lithium iron phosphate (LiFePO 4 ), lithium manganese phosphate (LiMnPO 4 ), lithium manganese iron phosphate, etc.
[0070] These positive electrode active materials may be used alone or in combination of two or more. As the positive electrode active material, lithium nickel cobalt manganese based composite oxide is particularly preferable because of its excellent properties such as initial resistance characteristics.
[0071] The average particle diameter (D50) of the positive electrode active material is not particularly limited, but is, for example, 0.05 μm or more and 25 μm or less, preferably 1 μm or more and 20 μm or less, and more preferably 3 μm or more and 15 μm or less.
[0072] The positive electrode active material layer 54 may contain components other than the positive electrode active material, such as trilithium phosphate, a conductive material, a binder, etc. As the conductive material, for example, carbon black such as acetylene black (AB), carbon fibers such as vapor grown carbon fiber (VGCF) and carbon nanotubes (CNT), and other carbon materials (e.g., graphite, etc.) can be suitably used. As the binder, for example, polyvinylidene fluoride (PVdF) can be used.
[0073] The content of the positive electrode active material in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 85 mass% or more and 99 mass% or less. The content of the trilithium phosphate in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.1 mass% or more and 15 mass% or less, and more preferably 0.2 mass% or more and 10 mass% or less. The content of the conductive material in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.1 mass% or more and 20 mass% or less, and more preferably 0.3 mass% or more and 15 mass% or less. The content of the binder in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.4 mass% or more and 15 mass% or less, and more preferably 0.5 mass% or more and 10 mass% or less.
[0074] The thickness of the positive electrode active material layer 54 per side is not particularly limited, but is usually 10 μm or more, and preferably 20 μm or more. On the other hand, the thickness is usually 400 μm or less, and preferably 300 μm or less.
[0075] As the negative electrode sheet 60, the above-mentioned negative electrode 60 is used.
[0076] The separator 70 may be a porous sheet (film) made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, or polyamide. Such a porous sheet may have a single-layer structure or a laminated structure of two or more layers (for example, a three-layer structure in which a PP layer is laminated on both sides of a PE layer). A heat-resistant layer (HRL) may be provided on the surface of the separator 70.
[0077] The thickness of the separator 70 is not particularly limited, but is, for example, 5 μm to 50 μm, and preferably 10 μm to 30 μm. The air permeability of the separator 70 obtained by the Gurley test method is not particularly limited, but is preferably 350 sec / 100 cc or less.
[0078] The non-aqueous electrolyte typically contains a non-aqueous solvent and a supporting salt (electrolyte salt). As the non-aqueous solvent, organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones, which are used in electrolytes of general lithium ion secondary batteries, can be used without any particular limitation. Among them, carbonates are preferable, and specific examples thereof include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC). Such non-aqueous solvents can be used alone or in appropriate combination of two or more. As an example, the non-aqueous solvent is composed of only carbonates. As another example, non-aqueous solvents include carbonates and esters, such as methyl acetate.
[0079] The supporting salt is, for example, LiPF 6 , LiBF 4 , lithium salts such as lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF 6 The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.
[0080] The nonaqueous electrolyte may contain various additives other than the above-mentioned components, such as film-forming agents such as vinylene carbonate (VC) and oxalate complexes; gas generating agents such as biphenyl (BP) and cyclohexylbenzene (CHB); and thickeners, as long as the effects of the present invention are not significantly impaired.
[0081] The lithium ion secondary battery 100 is suppressed from deteriorating in capacity when repeatedly charged and discharged, and has a high capacity. The lithium ion secondary battery 100 can be used for various applications. Suitable applications include a driving power source mounted on vehicles such as electric vehicles (BEVs), hybrid vehicles (HEVs), and plug-in hybrid vehicles (PHEVs). The lithium ion secondary battery 100 can also be used as a storage battery for small power storage devices and the like. The lithium ion secondary battery 100 can also be used in the form of a battery pack in which a plurality of lithium ion secondary batteries 100 are typically connected in series and / or parallel.
[0082] The above describes, as an example, a rectangular lithium ion secondary battery 100 equipped with a flat wound electrode assembly 20. However, the lithium ion secondary battery can also be configured as a lithium ion secondary battery equipped with a laminated electrode assembly (i.e., an electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately laminated). The lithium ion secondary battery can also be configured as a cylindrical lithium ion secondary battery, a laminated case type lithium ion secondary battery, etc.
[0083] Furthermore, the lithium ion secondary battery 100 can also be constructed as an all-solid-state lithium ion secondary battery using a solid electrolyte instead of a non-aqueous electrolyte according to known methods.
[0084] Furthermore, although the negative electrode 60 according to this embodiment is suitable as a negative electrode for a lithium ion secondary battery, it can be constructed and used as a negative electrode for other secondary batteries, and the other secondary batteries can be constructed according to known methods.
[0085] Examples of the present invention will be described in detail below, but it is not intended that the present invention be limited to those shown in these examples.
[0086] <Preparation of negative electrode> Example 1 The following negative electrode active materials were prepared. The major axis length and aspect ratio of the first Si-containing particle and the second Si-containing particle were measured using an image particle size distribution analyzer. The Si content of the first Si-containing particle and the second Si-containing particle was measured using a commercially available ICP analyzer. First Si-containing particle: Si-C composite material, aspect ratio = 7, major axis length = 6 μm, Si content = 48 mass% Second Si-containing particle: Si-C composite material, aspect ratio = 1.2, major axis length = 6 μm, Si content = 53 mass% Graphite particles: average particle size (D50) = 13 μm
[0087] Carboxymethyl cellulose (CMC), polyacrylic acid (PAA), and styrene butadiene rubber (SBR) were prepared as binders, and a dispersion of single-walled carbon nanotubes (SWCNT) was prepared as a conductive material.
[0088] A negative electrode paste containing graphite particles, first Si-containing particles, second Si-containing particles, CMC, PAA, SBR, and SWCNTs in a mass ratio of 60:8:32:1:1:2:0.1 was prepared by the following procedure: First, the first Si-containing particles and the second Si-containing particles were premixed uniformly by dry blending them using a disper at a rotation speed of 3000 rpm.
[0089] The obtained preliminary mixture, graphite particles, CMC, and PAA were dry-blended using a planetary mixer at a rotation speed of 60 rpm. The obtained mixture, SWCNT dispersion, and dispersion medium were kneaded using a planetary mixer. SBR and further the dispersion medium were added to this and mixed uniformly to prepare a negative electrode paste.
[0090] The negative electrode paste thus prepared was applied to the surface of a copper foil having a thickness of 10 μm and dried to form a negative electrode active material layer. After the negative electrode active material layer was roll-pressed, the obtained sheet was processed to a predetermined size to obtain a negative electrode sheet.
[0091] Example 2 The negative electrode sheet of Example 2 was obtained in the same manner as in Example 1, except that Si-C composite particles having an aspect ratio of 5, a major axis length of 5 μm, and a Si content of 50 mass% were used as the first Si-containing particles, and the mass ratio of the solid contents of the negative electrode paste was changed to graphite particles:first Si-containing particles:second Si-containing particles:CMC:PAA:SBR:SWCNT=60:12:28:1:1:2:0.1.
[0092] Example 3 A negative electrode sheet of Example 3 was obtained in the same manner as in Example 1, except that Si-C composite particles having an aspect ratio of 7, a major axis length of 10 μm, and a Si content of 52 mass% were used as the first Si-containing particles.
[0093] Example 4 The negative electrode sheet of Example 4 was obtained in the same manner as in Example 1, except that when preparing the negative electrode paste, the first Si-containing particles and the second Si-containing particles were not premixed, and the graphite particles, the first Si-containing particles, the second Si-containing particles, CMC, and PAA were dry-blended using a planetary mixer at a rotation speed of 60 rpm.
[0094] Comparative Example 1 A negative electrode sheet of Comparative Example 1 was obtained in the same manner as in Example 1, except that Si-C composite particles having an aspect ratio of 2, a major axis length of 7 μm, and a Si content of 51 mass % were used as the first Si-containing particles.
[0095] Comparative Example 2 A negative electrode sheet of Comparative Example 2 was obtained in the same manner as in Example 1, except that Si-C composite particles having an aspect ratio of 5, a major axis length of 5 μm, and a Si content of 50 mass% were used as the first Si-containing particles, and the mass ratio of the solid contents of the negative electrode paste was changed to graphite particles:first Si-containing particles:second Si-containing particles:CMC:PAA:SBR:SWCNT=60:2:38:1:1:2:0.1.
[0096] Comparative Example 3 A negative electrode sheet of Comparative Example 3 was obtained in the same manner as in Example 1, except that Si-C composite particles having an aspect ratio of 5, a major axis length of 5 μm, and a Si content of 50 mass% were used as the first Si-containing particles, and the mass ratio of the solid contents of the negative electrode paste was changed to graphite particles:first Si-containing particles:second Si-containing particles:CMC:PAA:SBR:SWCNT=60:24:16:1:1:2:0.1.
[0097] Comparative Example 4 A negative electrode sheet of Comparative Example 4 was obtained in the same manner as in Example 1, except that the mass ratio of the solid contents of the negative electrode paste was changed to graphite particles:first Si-containing particles:second Si-containing particles:CMC:PAA:SBR:SWCNT=60:40:0:1:1:2:0.1.
[0098] Comparative Example 5 A negative electrode sheet of Comparative Example 5 was obtained in the same manner as in Example 1, except that the mass ratio of the solid contents of the negative electrode paste was changed to graphite particles:first Si-containing particles:second Si-containing particles:CMC:PAA:SBR:SWCNT=60:0:40:1:1:2:0.1.
[0099] <Preparation of lithium-ion secondary battery for evaluation> LiNi as a positive electrode active material powder 1 / 3 Co 1 / 3 Mn 1 / 3 O 2A positive electrode paste was prepared by mixing polyvinylidene fluoride (PVdF) as a binder with N-methylpyrrolidone (NMP) in a mass ratio of NCM:AB:PVdF=100:1:1. The paste was applied to the surface of an aluminum foil with a thickness of 15 μm and dried to form a positive electrode active material layer. After the positive electrode active material layer was roll-pressed, the sheet obtained was processed to a predetermined size to obtain a positive electrode sheet.
[0100] A separator made of porous polyolefin was prepared. Leads were attached to each of the negative electrode sheet and positive electrode sheet prepared above, and the sheets were laminated with a separator interposed therebetween to prepare an electrode body. This was housed in a case made of aluminum laminate film together with a non-aqueous electrolyte. The non-aqueous electrolyte was a mixed solvent containing ethylene carbonate (EC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 15:5:40:40, and LiPF as a supporting electrolyte. 6 was dissolved at a concentration of 1.0 mol / L. The case was then sealed to obtain a lithium ion secondary battery for evaluation.
[0101] <Cycle characteristic evaluation> Each of the lithium ion secondary batteries for evaluation prepared above was placed in an environment of 25° C. Each of the lithium ion secondary batteries for evaluation was charged at a constant current of 0.4 C to 4.2 V, and then charged at a constant voltage until the current value reached 0.1 C. Next, each of the lithium ion secondary batteries for evaluation was discharged at a constant current of 0.4 C to 2.5 V. The discharge capacity at this time was measured to obtain the initial capacity.
[0102] The above charge / discharge cycle was repeated 200 times. The discharge capacity after 200 cycles was determined in the same manner as the initial capacity. As an index of cycle characteristics, the capacity retention rate (%) was calculated by (discharge capacity after 200 charge / discharge cycles / initial capacity)×100. The results are shown in Table 1.
[0103] [Table 1]
[0104] The results in Table 1 show that when the aspect ratio of the first Si-containing particle is 4.0 to 10.0, the aspect ratio of the second Si-containing particle is 1.0 to 3.0, and the mass ratio of the first Si-containing particle to the second Si-containing particle is 10:90 to 50:50, the capacity retention rate after 200 charge / discharge cycles is significantly high. Therefore, it is found that the negative electrode disclosed herein can suppress capacity degradation when the secondary battery is repeatedly charged and discharged.
[0105] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.
[0106] That is, the negative electrode of the secondary battery, the manufacturing method thereof, and the secondary battery disclosed herein are the following items [1] to [9]. [1] A negative electrode comprising a negative electrode current collector and a negative electrode active material layer supported on the negative electrode current collector, the negative electrode active material layer contains graphite particles, first Si-containing particles, and second Si-containing particles; the first Si-containing particle has a larger aspect ratio than the second Si-containing particle; the first Si-containing particle has an aspect ratio of 4.0 to 10.0; the aspect ratio of the second Si-containing particle is 1.0 to 3.0; a mass ratio of the first Si-containing particles to the second Si-containing particles is 10:90 to 50:50; Negative electrode. [2] The negative electrode according to item [1], wherein a ratio of a major axis diameter of the first Si-containing particle to a major axis diameter of the second Si-containing particle is 1.5 or less. [3] The negative electrode according to item [1], wherein a ratio of a major axis diameter of the first Si-containing particle to a major axis diameter of the second Si-containing particle is 1.0 or less. [4] The negative electrode according to any one of items [1] to [3], wherein the first Si-containing particle has a major axis length of 4 μm to 12 μm, and the second Si-containing particle has a major axis length of 2 μm to 10 μm. [5] The negative electrode according to any one of items [1] to [4], wherein the aspect ratio of the first Si-containing particle is 5.0 to 9.0, and the aspect ratio of the second Si-containing particle is 1.0 to 2.0. [6] The negative electrode according to any one of items [1] to [5], wherein a content ratio of the graphite particles to a total of the graphite particles, the first Si-containing particles, and the second Si-containing particles is 40% by mass to 90% by mass. [7] preparing a negative electrode paste containing graphite particles, first Si-containing particles, second Si-containing particles, and a dispersion medium; applying the negative electrode paste to a negative electrode current collector; A step of drying the applied negative electrode paste to form a negative electrode active material layer; and a step of pressing the negative electrode active material layer; Equipped with the first Si-containing particle has a larger aspect ratio than the second Si-containing particle; the first Si-containing particle has an aspect ratio of 4.0 to 10.0; the aspect ratio of the second Si-containing particle is 1.0 to 3.0; a mass ratio of the first Si-containing particles to the second Si-containing particles is 10:90 to 50:50; A method for manufacturing a negative electrode of a secondary battery. [8] The manufacturing method according to item [7], wherein in the step of preparing the negative electrode paste, the first Si-containing particles and the second Si-containing particles are premixed by dry blending, and the obtained premix is used for preparing the negative electrode paste. [9] A positive electrode, a negative electrode, and an electrolyte; A secondary battery comprising: A secondary battery, wherein the negative electrode is the negative electrode according to any one of items [1] to [6]. [Explanation of symbols]
[0107] 12 Graphite particles 14 1st Si-containing particles 16 2nd Si-containing particles 20 Wound electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode sheet (positive electrode) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 60 Negative electrode sheet (negative electrode) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64 Negative electrode active material layer 70 Separator sheet (separator) 100 Lithium-ion secondary battery
Claims
1. A negative electrode comprising a negative electrode current collector and a negative electrode active material layer supported on the negative electrode current collector, the negative electrode active material layer contains graphite particles, first Si-containing particles, and second Si-containing particles, the first Si-containing particle has a larger aspect ratio than the second Si-containing particle; the aspect ratio of the first Si-containing particle is 4.0 to 10.0; the aspect ratio of the second Si-containing particles is 1.0 to 3.0; The mass ratio of the first Si-containing particles to the second Si-containing particles is 10:90 to 50:
50. Negative electrode.
2. 2. The negative electrode according to claim 1, wherein a ratio of a major axis diameter of the first Si-containing particle to a major axis diameter of the second Si-containing particle is 1.5 or less.
3. 2. The negative electrode according to claim 1, wherein a ratio of a major axis diameter of the first Si-containing particle to a major axis diameter of the second Si-containing particle is 1.0 or less.
4. 2. The negative electrode according to claim 1, wherein the first Si-containing particles have a major axis length of 4 μm to 12 μm, and the second Si-containing particles have a major axis length of 2 μm to 10 μm.
5. 2. The negative electrode according to claim 1, wherein the aspect ratio of the first Si-containing particles is 5.0 to 9.0, and the aspect ratio of the second Si-containing particles is 1.0 to 2.
0.
6. 2. The negative electrode according to claim 1, wherein a content ratio of the graphite particles to a total of the graphite particles, the first Si-containing particles, and the second Si-containing particles is 40% by mass to 90% by mass.
7. preparing a negative electrode paste containing graphite particles, first Si-containing particles, second Si-containing particles, and a dispersion medium; applying the negative electrode paste to a negative electrode current collector; A step of drying the applied negative electrode paste to form a negative electrode active material layer; and a step of pressing the negative electrode active material layer; Equipped with the first Si-containing particle has a larger aspect ratio than the second Si-containing particle; the aspect ratio of the first Si-containing particle is 4.0 to 10.0; the aspect ratio of the second Si-containing particles is 1.0 to 3.0; The mass ratio of the first Si-containing particles to the second Si-containing particles is 10:90 to 50:
50. A method for manufacturing a negative electrode of a secondary battery.
8. 8. The manufacturing method according to claim 7, wherein in the step of preparing the negative electrode paste, the first Si-containing particles and the second Si-containing particles are premixed by dry blending, and the obtained premix is used for preparing the negative electrode paste.
9. A positive electrode, a negative electrode, an electrolyte, A secondary battery comprising: A secondary battery, wherein the negative electrode is the negative electrode according to claim 1.
Citation Information
Patent Citations
Negative material for lithium secondary battery, composition for negative active material layer for lithium secondary battery, negative electrode for lithium secondary battery and method of manufacturing lithium secondary battery
JP2016154114A
Porous silicon-containing composite, carbon composite using the same, electrode, lithium battery, and electronic element including the same
JP2020066574A
Core-shell composite negative electrode material, its preparation method and application
JP2021535581A
Anode and secondary battery including said anode
JP2023534856A
Negative electrode for nonaqueous secondary batteries; nonaqueous secondary battery; negative electrode active material; method for producing negative electrode active material; composite body comprising nano-silicon, carbon layer and cationic polymer layer; and method for producing composite body composed of nano-silicon and carbon layer
WO2015114692A1