Laminate and solar cell

JP2024167526APending Publication Date: 2024-12-04TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023083659
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

AI Technical Summary

Benefits of technology

【0008】 本発明によれば、ガスバリア層にマグネシウム、ケイ素、および酸素を含む積層体において、水存在環境下でもMgOの結晶化の進行が抑制された積層体と、それを用いた太陽電池を提供することができる。また、これにより、高いガスバリア性と高い耐久性を両立した積層体を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167526000001_ABST
    Figure 2024167526000001_ABST
Patent Text Reader

Abstract

To provide a laminate that contains magnesium, silicon, and oxygen in its gas barrier layer, which suppresses progression of crystallization of MgO even in environments with water, and a solar cell including the same.SOLUTION: A laminate includes a layer A and a layer B on at least one side of a substrate, where the layer A contains magnesium, silicon, and oxygen.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate that is required to have high gas barrier properties and durability. [Background technology]

[0002] In recent years, gas barrier films used as components for electronic devices such as solar cells, electronic paper, and organic electroluminescence displays have a water vapor transmission rate of 5.0×10 -2 g / m 2 / day or less, high gas barrier properties and flexibility are required. Gas barrier films, which are made by forming a vapor-deposited layer of inorganic substances or inorganic oxides on the surface of a polymer film substrate using physical vapor deposition (PVD) methods such as vacuum deposition and sputtering, achieve high flexibility and gas barrier properties due to the flexibility of the substrate and the high density of the vapor-deposited film.

[0003] One of the methods to achieve higher gas barrier properties and flexibility is to use ZnO and SiO 2 By sputtering using a target mainly composed of ZnO-SiO 2 A gas barrier film in which a SiO-based film is formed on a film substrate (Patent Document 1) and a MgO-SiO 2 By using a target mainly composed of MgO-SiO 2 A gas barrier film (Patent Document 2) has been proposed in which an amorphous single film of a composite oxide such as those based on the above-mentioned system is formed on a film substrate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-147710 A [Patent Document 2] Patent Publication No. 2021-169183 Summary of the Invention [Problem to be solved by the invention]

[0005] As shown in Patent Document 2, MgO-SiO 2 The high gas barrier properties of the laminate that forms the composite oxide are realized by the extremely high density due to the formation of an amorphous structure. Therefore, it has been found that depending on the method of use of the gas barrier film, for example, exposure to a high temperature environment with a large amount of water or water vapor for a long period of time, the gas permeation path may change due to structural changes in the laminate, such as fine cracks caused by changes in film quality due to MgO crystallization. However, with the above-mentioned configuration (Patent Document 2), depending on the method of use and the environment of use, the above-mentioned change in gas permeation path could not be completely controlled.

[0006] In view of the background of the conventional technology, the present invention aims to provide a laminate containing magnesium, silicon, and oxygen in a gas barrier layer, in which the progress of crystallization of MgO is suppressed even in an environment where water is present, and a solar cell using the same. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention employs the following means. That is, a preferred embodiment of the present invention is as follows. (1) A laminate having an A layer and a B layer on at least one side of a substrate, the A layer containing magnesium, silicon, and oxygen. (2) The laminate according to (1), wherein, with respect to the average composition in the thickness direction of the layer A, the ratio of atomic concentrations of magnesium atoms to silicon atoms, Mg / (Mg+Si), is 0.30 to 0.80 atm %. (3) The laminate according to (1) or (2), wherein the layer A has an average lifetime of 0.935 ns or less as measured by a positron beam method. (4) The laminate according to any one of (1) to (3), wherein the layer A has a half-width of an oxygen atom (O1s) peak measured by X-ray photoelectron spectroscopy of 3.25 eV or less. (5) The laminate according to any one of (1) to (4), wherein the layer B is a polymer film. (6) The laminate according to (5), wherein the layer B satisfies (i) and (ii). (i) Mass density 0.7g / cm 3 More than 1.75g / cm 3 below (ii) A thickness of 300 nm or more and 7,000 nm or less (7) The laminate according to any one of (1) to (6), wherein the layer B contains one or more compounds selected from a polyurethane compound, a polysilazane compound, a polysiloxane compound, an acrylate, a methacrylate, a mixture of an alkoxide and a water-soluble polymer, and a mixture of a polycondensate of an alkoxide and a water-soluble polymer. (8) The laminate according to any one of (1) to (4), wherein the layer B is an inorganic film. (9) The laminate according to (8), wherein the layer B is (iii) and (iV). (iii) Mass density 2.1g / cm 3 More than 7.5g / cm 3 below (iv) a thickness of 10 nm or more and 500 nm or less (10) The laminate according to any one of (1) to (9), wherein the layer B contains at least one element selected from the group consisting of tin, indium, zinc, aluminum, nickel, chromium, and titanium. (11) The laminate according to any one of (1) to (10), having a total light transmittance of 85% or more. (12) The laminate according to any one of (1) to (11), which has an average reflectance of 15% or less in the visible light region (380-780 nm). (13) A solar cell using the laminate according to any one of (1) to (12) as a protective member. Effect of the Invention

[0008] According to the present invention, it is possible to provide a laminate containing magnesium, silicon, and oxygen in a gas barrier layer, in which the progress of crystallization of MgO is suppressed even in a water-containing environment, and a solar cell using the same, and it is also possible to provide a laminate that has both high gas barrier properties and high durability. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a laminate of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing a winding type electron beam deposition apparatus for producing a laminate of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing, from above, the arrangement of materials for producing the laminate of the present invention. [Figure 4] FIG. 2 is a schematic diagram showing a side view of a material arrangement for producing a laminate of the present invention. [Diagram 5] FIG. 1 is a schematic diagram showing a roll-up sputtering apparatus for producing a laminate of the present invention. [Figure 6] FIG. 11 is a cross-sectional view showing an example of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below.

[0011] [Laminate] A preferred embodiment of the laminate of the present invention is a laminate having an A layer and a B layer on at least one side of a substrate, the A layer containing magnesium, silicon, and oxygen.

[0012] This embodiment makes it possible to obtain a laminate that has high gas barrier properties and is excellent in suppressing the progress of crystallization of MgO present in the gas barrier film even in a high-temperature environment in which there is a large amount of water or water vapor in the atmosphere. Details will be described later.

[0013] The magnesium and silicon contained in layer A are preferably in the form of an amorphous film, and from the viewpoint of gas barrier properties, are preferably contained as at least one compound selected from the group consisting of oxides, nitrides, oxynitrides, and carbides. Among these, it is more preferable that magnesium oxide and silicon oxide are contained.

[0014] The A layer contains oxygen when evaluated by X-ray photoelectron spectroscopy (XPS). 2 The term "layer A" refers to a thickness equivalent to a thickness where the oxygen atom content is 10.0 atm% or more at a location where argon ion etching is performed from the outermost surface of layer A to a position where the thickness of layer A is 1 / 2. From the viewpoints of transparency and denseness, the oxygen atom content is preferably 20.0 atm% or more, and more preferably 40.0 atm% or more. The outermost surface of layer A refers to the surface opposite to the surface of layer A closest to the substrate. Note that layer A contains magnesium means that the magnesium atom content is 5.0 atm% or more when evaluated by XPS as described above. Layer A contains silicon means that the silicon atom content is 2.0 atm% or more when evaluated by XPS as described above. The analysis method for each element in the evaluation by XPS is as described in the examples.

[0015] The A layer and B layer of the present invention are defined by the composition obtained by depth direction analysis of XPS. SiO 2The layers are removed by argon ion etching from the top surface of the laminate in 5 nm increments, in terms of thickness equivalent, and the composition is analyzed. The B layer is defined as the area between the measurement point where the magnesium content in the B layer is 1 atm% or less, where the layers are removed, and the measurement point where the magnesium content in the B layer is 1 atm% or more is the end point, and the argon ion etching and analysis are repeated. The A layer is defined as the area between the measurement point where the magnesium content in the A layer is 1 atm% or less, where the measurement point where the magnesium content in the B layer is 1 atm% or less is the end point, and the measurement point where the magnesium content in the B layer is 1 atm% or less is the end point, and the measurement point where the magnesium content in the B layer is 1 atm% or less is the end point, and the measurement point where the magnesium content in the B layer is 1 atm% or less is the end point. For example, if a layer containing magnesium, silicon, and oxygen is formed in a certain composition ratio, and then a layer containing magnesium, silicon, and oxygen is formed in a different composition ratio, the two layers may be combined to form one A layer. In addition, if a layer containing magnesium is formed on both sides of a layer not containing magnesium, the A layer is the layer containing magnesium that is closest to the substrate. Similarly, when a layer not containing magnesium with a certain composition ratio is formed and then a layer not containing magnesium with a different composition ratio is formed, the two layers together may become layer B.

[0016] In the present invention, it is preferable to have the substrate, the A layer, and the B layer in this order. The A layer contains magnesium, silicon, and oxygen to form a dense composite oxide, which can exhibit high gas barrier properties. It is preferable to form the B layer on the A layer, since this can inhibit the progress of crystallization of MgO present in the A layer. When the A layer and the B layer are interchanged, the desired gas barrier properties and the effect of inhibiting the progress of MgO crystallization may not be obtained.

[0017] As long as the A layer and the B layer are in this order from the substrate side, other layers may be present between the substrate and the A layer or on the B layer. For example, an anchor coat layer may be provided between the substrate and the A layer to smooth the substrate. In addition, a wet coat layer or a dry coat layer may be provided on the B layer to further suppress the progress of MgO crystallization and provide chemical resistance and scratch resistance, and the B layer may be formed together, or a substrate / A layer / B layer / A layer structure may be used.

[0018] From the viewpoint of transparency, the laminate of the present invention preferably has a total light transmittance of 85% or more. When used as a solar cell member, more efficient power generation is possible, so the total light transmittance is preferably 85% or more. In addition, from the viewpoint of visibility, the average reflectance in the visible light region (380-780 nm) is preferably 15% or less. When used as a solar cell member, more efficient power generation is possible, so the average reflectance in the visible light region (380-780 nm) is preferably 15% or less.

[0019] [A layer] The composition of Layer A of the present invention is preferably a laminate having a magnesium (Mg) atomic concentration of 5 to 50 (atm%), a silicon (Si) atomic concentration of 2 to 30 (atm%), and an oxygen (O) atomic concentration of 45 to 70 (atm%).

[0020] The composition ratio of layer A can be measured by X-ray photoelectron spectroscopy (XPS). After removing layer B by argon ion etching, layers are removed from the surface side by argon ion etching until the thickness of layer A is half, and the content ratio of each element is measured.

[0021] In order to prevent the A layer from becoming a crystalline layer and becoming susceptible to cracking, it is preferable that the magnesium atomic concentration is 50 atm % or less and / or the silicon atomic concentration is 2 atm % or more.

[0022] From the viewpoint of ensuring a sufficient ratio of silicate bonds in the A layer and improving the density to exhibit gas barrier properties, it is preferable that the magnesium atom concentration is 5 atm% or more and / or the silicon atom concentration is 30 atm% or less. The silicate bond is a bond between silicon (Si) and a metal (M) via oxygen (O), and can be written as Si-OM. The metal (M) may contain silicon.

[0023] From the viewpoint of preventing magnesium or silicon from being oxygen deficient and thus reducing light transmittance, the oxygen atomic concentration is preferably 45 atm% or more, and from the viewpoint of preventing excessive oxygen incorporation and thus increasing voids and defects, and thus exhibiting gas barrier properties, the oxygen atomic concentration is preferably 70 atm% or less.

[0024] From the above viewpoints, the composition of Layer A of the present invention is more preferably such that the magnesium atomic concentration is 8 to 35 (atm%), the silicon atomic concentration is 6 to 25 (atm%), and the oxygen atomic concentration is 50 to 65 (atm%), and even more preferably such that the magnesium atomic concentration is 15 to 30 (atm%), the silicon atomic concentration is 8 to 20 (atm%), and the oxygen atomic concentration is 50 to 65 (atm%).

[0025] In terms of the atomic concentration (atm %), O / (Mg+Si) is preferably 1.25 to 2.00. From the viewpoints of gas barrier properties and optical properties, O / (Mg+Si) is more preferably 1.40 to 1.75.

[0026] Regarding the composition of the A layer of the present invention, the atomic concentration (atm%) ratio Mg / (Mg+Si) of magnesium (Mg) atoms to silicon (Si) atoms is preferably 0.30 to 0.80. When the atomic concentration (atm%) ratio is Mg / (Mg+Si)≧0.30, the proportion of silicate bonds in the A layer is sufficient, and the denseness is improved to exhibit gas barrier properties. When the atomic concentration (atm%) ratio is Mg / (Mg+Si)≦0.80, the presence of crystal parts in the A layer is suppressed, and the tendency for cracks to occur can be suppressed. From the same viewpoint, the atomic concentration (atm%) ratio Mg / (Mg+Si) is more preferably 0.50 to 0.78, and even more preferably 0.55 to 0.76.

[0027] The thickness of the A layer in the present invention is determined from the distance from the starting point to the end point. 2The thickness is the equivalent thickness. The thickness of the A layer is preferably 5 nm or more, and preferably 500 nm or less. By having a thickness of 5 nm or more, it is possible to prevent the occurrence of regions that are not formed as a layer, which makes it impossible to ensure gas barrier properties. In addition, by having a thickness of 500 nm or less, it is possible to prevent the A layer from easily cracking, and it is also possible to improve bending resistance and stretchability. From the above viewpoint, it is more preferable that the thickness of the A layer is 10 nm or more and 300 nm or less.

[0028] Layer A of the laminate of the present invention preferably has an average lifetime of 0.935 ns or less as measured by the positron beam method (thin film compatible positron annihilation lifetime measurement method) (see Chapter I, Section 1 and Chapter V, Section 2 of "The Science of Positron Measurement" (Japan Radioisotope Association)). The positron beam method is one of the positron annihilation lifetime measurement methods, and is a technique for non-destructively evaluating information regarding the size, number concentration, and size distribution of vacancies of about 0.1 to 10 nm from the annihilation lifetime by measuring the time (on the order of several hundred ps to several tens of ns) from when a positron is incident on a sample to when it annihilates. A radioisotope ( 22 This method is significantly different from the usual positron annihilation method in that it uses a positron beam instead of Na), making it possible to measure thin films of several hundred nanometers thick formed on silicon or quartz substrates. The average pore radius and number concentration of pores can be calculated from the obtained measurements using the nonlinear least-squares program POSITRONFIT. The corresponding pores and basic skeletons on the sub-nm order can be obtained by analyzing the average lifetimes of the third and fourth components.

[0029] Here, the third component refers to the average life obtained by selecting an analysis for three components as the measurement conditions for the average life by the positron beam method, and the fourth component refers to the average life obtained by selecting an analysis for four components as the measurement conditions for the average life by the positron beam method. When performing an analysis using POSITRONFIT, the number of components in POSITRONFIT is determined from the number of peaks obtained in the pore radius distribution curve calculated using the distribution analysis program CONTIN based on the inverse Laplace transform method. The validity of the analysis is determined by the agreement between the average pore radius calculated by POSITRONFIT and the peak position of the pore radius distribution curve of CONTIN. The average life in this invention refers to the average life of the third component.

[0030] If the average life is greater than 0.935ns, the A layer will not be dense, and gas barrier properties may not be exhibited. From the viewpoint of gas barrier properties, the average life measured by the positron beam method is preferably 0.912ns or less, more preferably 0.863ns or less. The lower limit of the average life is not particularly limited, but is preferably 0.542ns or more. If the average life is less than 0.542ns, flexibility may decrease.

[0031] In order to set the average lifetime of layer A to 0.935 ns or less as measured by a positron beam method, as specified in the present invention, this can be achieved, for example, by forming a dense composite oxide film with an appropriate composition ratio on a substrate having an arithmetic mean roughness Ra of 10.0 nm or less. Here, "densely formed" refers to a state in which each oxide is mixed at the atomic level to form a dense network.

[0032] In the layer A of the present invention, the half-width of the peak of oxygen atoms (O1s) measured by X-ray photoelectron spectroscopy is preferably 3.25 eV or less. max If the peak intensity is F maxThe half-width of the O1s peak is the width of the peak when the half-width of the O1s peak is 1 / 2. The narrower the half-width of the O1s peak, the more uniform the bond network structure is formed, and the denser the film becomes. From the viewpoint of the uniformity of the bond and the barrier property, the half-width is more preferably 3.00 eV or less, and even more preferably 2.75 eV or less. The lower limit is not particularly limited, but is preferably 1.65 eV or more.

[0033] The layer A of the laminate of the present invention is preferably an amorphous film. Amorphous refers to an irregular structure in which atoms and molecules do not have a long-range regular order structure like crystals. In a crystalline structure, grain boundaries are generated, which become water vapor permeation paths, resulting in poor gas barrier properties and easy cracking, so it is preferable to be amorphous. Whether or not a film is amorphous can be confirmed by analytical methods such as cross-sectional TEM and thin film X-ray diffraction (XRD). In the case of cross-sectional TEM, the contrast is uniform in an amorphous film and grain boundaries are not observed, while in a crystalline film, grain boundaries corresponding to the crystal structure, such as a microcrystalline state or a columnar structure, are observed. In addition, in the case of thin film X-ray diffraction, no peaks are observed in an amorphous film, while diffraction peaks corresponding to the crystal structure are confirmed in a crystalline film. In particular, in MgO crystals, characteristic peaks are confirmed near 2θ=43° and 62°, and it is possible to detect 002 and 022 diffraction peaks from the positions of these diffraction peaks.

[0034] [Example of manufacturing method for layer A] The method for forming the A layer is not particularly limited, and may be a vacuum deposition method, a sputtering method, a reactive sputtering method, a molecular beam epitaxy method, a cluster ion beam method, an ion plating method, an atomic layer deposition method, a plasma polymerization method, an atmospheric pressure plasma polymerization method, a plasma CVD method, a laser CVD method, a thermal CVD method, a coating method, or the like. From the viewpoint of production cost, gas barrier properties, etc., it is preferable to use a vacuum deposition method. From the viewpoint of compound deposition, it is more preferable to use electron beam (EB) deposition or ion beam assisted deposition (IBAD) among the vacuum deposition methods.

[0035] An example of a method for forming the A layer using the winding type vapor deposition apparatus in FIG. 2 is shown. A compound thin film of materials B and C is provided as the A layer on the surface of the substrate 1 by electron beam vapor deposition. First, granular materials B and C having a size of about 2 to 5 mm are arranged as the vapor deposition materials as shown in FIG. 3 and FIG. 4. The vapor deposition material is not limited to granules, and molded bodies having different shapes such as square or tablet shapes may be used. In addition, the vapor deposition source materials are arranged in the width direction of the substrate in FIG. 3 and FIG. 4, but they may be arranged in other ways such as mixing two materials in one hearth liner or arranging them in the longitudinal direction. In addition, if the vapor deposition material absorbs moisture, the moisture in the material is taken into the A layer, and there is a possibility that the desired film composition and physical properties cannot be obtained. Therefore, it is preferable to perform a dehydration treatment by heating the material before use. In the winding chamber 5, the surface of the substrate 1 on which the A layer is to be provided is set on the unwinding roll 6 so that it faces the hearth liner 11, and the substrate 1 is unwound and passed through the main drum 10 via the guide rolls 7, 8, and 9. Next, the pressure inside the deposition device 4 was reduced by the vacuum pump to 5.0×10 -3 The ultimate vacuum level is 5.0×10 Pa or less. -3 The ultimate vacuum is preferably 5.0×10 Pa or less. -3 If the pressure is higher than Pa, residual gas may be taken into the A layer, and the desired film composition and physical properties may not be obtained. The temperature of the main drum 10 is set to -10°C, for example. From the viewpoint of preventing the substrate from being damaged by heat, it is preferably 20°C or less, and more preferably 0°C or less. Next, using one electron gun (hereinafter, EB gun) 13 as a heating source, the surfaces of materials B and C are heated to the desired film composition ratio. The EB gun has an acceleration voltage of 10 kV, and the acceleration current and film transport speed are adjusted so that the thickness of the A layer to be formed is about 150 nm, forming the A layer on the surface of the substrate 1. Thereafter, the substrate is wound up on the winding roll 18 via guide rolls 15, 16, and 17.

[0036] [B layer] Since the A layer has a high gas barrier property due to having a highly dense amorphous film, the gas barrier property may change due to fine cracks that occur when the film structure changes due to film crystallization, etc. Therefore, by forming the B layer, it is expected that the progress of MgO crystallization will be suppressed even in the presence of water or water vapor.

[0037] The layer B of the present invention may be an organic film from the viewpoint of suppressing contact with water vapor. When the layer B is a polymer film, (i) the mass density is 0.7 g / cm 3 More than 1.75g / cm 3 and (ii) the thickness is preferably 300 nm or more and 7,000 nm or less, more preferably 400 nm or more and 6,000 nm or less, and even more preferably 800 nm or more and 5,000 nm or less. 3 If the mass density is 1.0 g / cm or more, it is preferable because it is easy to form a highly dense B layer and the effect of suppressing the progress of crystallization of MgO is improved. 3 More preferably, 1.1 g / cm 3 More preferably, the mass density is 0.7 g / cm or more, and particularly preferably, 1.35 or more. 3 If the mass density is smaller than 1.75 g / cm, the density of the B layer will be low and sufficient suppression of the progress of crystallization may not be obtained. 3 If it is larger, the bond between molecules becomes stronger and cracks are more likely to occur, so that the crystallization progress may not be sufficiently suppressed. The mass density in the present invention can be measured by X-ray reflectometry (XRR). The polymer film refers to a film made of molecules with a molecular weight of 5,000 or more.

[0038] When the B layer is formed from a polymer film, the thickness of the B layer is preferably 300 nm or more and 7,000 nm or less. If the thickness of the B layer is thinner than 300 nm, the amount of water or water vapor in contact with the A layer increases, and the progress of crystallization of MgO in the A layer may not be sufficiently suppressed. If the thickness of the B layer is thicker than 7,000 nm, the total light transmittance of the laminate decreases, and when incorporated into a device, the conversion efficiency of a solar cell and the visibility of electronic paper and organic EL displays may deteriorate. Here, the thickness of the B layer is similarly determined from the above starting point to the end point. In addition, when the B layer in the present invention is a film made of molecules with a molecular weight of 5,000 or more and is an inorganic film described later, the mass density is 0.7 g / cm 3 More than 1.75g / cm 3 The thickness is preferably 300 nm or more and 7,000 nm or less.

[0039] From the viewpoints of denseness, transparency, adhesion, etc., the polymer film forming the B layer of the laminate of the present invention preferably contains one or more compounds selected from a polyurethane compound, a polysilazane compound, a polysiloxane compound, an acrylate, a methacrylate, a mixture of an alkoxide and a water-soluble polymer, and a mixture of a polycondensate of an alkoxide and a water-soluble polymer.

[0040] The polyurethane compound used in layer B has an acrylate or urethane bond in the main chain or side chain, and can be obtained, for example, by polymerizing an epoxy (meth)acrylate having a hydroxyl group and an aromatic ring in the molecule. The epoxy (meth)acrylate having a hydroxyl group and an aromatic ring in the molecule can be obtained by reacting a diepoxy compound of an aromatic glycol such as bisphenol A type, bisphenol F type, resorcin, or hydroquinone with a (meth)acrylic acid derivative. Examples of ethylenically unsaturated compounds include di(meth)acrylates such as 1,4-butanediol di(meth)acrylate and 1,6-hexanediol di(meth)acrylate, polyfunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate, and epoxy acrylates such as bisphenol A type epoxy di(meth)acrylate, bisphenol F type epoxy di(meth)acrylate, and bisphenol S type epoxy di(meth)acrylate. Among these, polyfunctional (meth)acrylates with excellent surface protection performance are preferred. In addition, these may be used in a single composition, or may be used by mixing two or more components.

[0041] Examples of polysilazane compounds and polysiloxane compounds include perhydropolysilazane, tetramethylsilane, trimethylmethoxysilane, dimethyldimethoxysilane, methyltrimethoxysilane, trimethylethoxysilane, dimethyldiethoxysilane, methyltriethoxysilane, tetramethoxysilane, tetramethoxysilane, hexamethyldisiloxane, hexamethyldisilazane, trimethylvinylsilane, methoxydimethylvinylsilane, trimethoxyvinylsilane, ethyltrimethoxysilane, dimethyldivinylsilane, Dimethylethoxyethynylsilane, diacetoxydimethylsilane, aryltrimethoxysilane, ethoxydimethylvinylsilane, methyltrivinylsilane, diacetoxymethylvinylsilane, methyltriacetoxysilane, aryloxydimethylvinylsilane, diethylvinylsilane, butyltrimethoxysilane, 3-aminopropyldimethylethoxysilane, tetravinylsilane, triacetoxyvinylsilane, tetraacetoxysilane, butyldimethoxyvinylsilane, phenyltrimethylsilane, dimethoxymethylphenylsilane silane, phenyltrimethoxysilane, hexyltrimethoxysilane, dimethylethoxyphenylsilane, benzoyloxytrimethylsilane, dimethylethoxy-3-glycidoxypropylsilane, dibutoxydimethylsilane, 3-butylaminopropyltrimethylsilane, 3-dimethylaminopropyldiethoxymethylsilane, divinylmethylphenylsilane, diacetoxymethylphenylsilane, benzyldimethylethoxysilane, diethoxymethylphenylsilane, diethoxy-3-glycidoxypropylmethylsilane, tetraaryl Examples of suitable silanes include oxysilane, diarylmethylphenylsilane, diphenylmethylvinylsilane, diphenylethoxymethylsilane, diacetoxydiphenylsilane, dibenzyldimethylsilane, diaryldiphenylsilane, 1,4-bis(dimethylvinylsilyl)benzene, 1,3-bis(3-acetoxypropyl)tetramethyldisiloxane, 1,3,5-trimethyl-1,3,5-trivinylcyclotrisiloxane, 1,3,5-tris(3,3,3-trifluoropropyl)-1,3,5-trimethylcyclotrisiloxane, etc. Among these, perhydropolysilazane, which has excellent denseness, is preferred.

[0042] Examples of the acrylate and methacrylate include hexanediol diacrylate, ethoxyethyl acrylate, phenoxyethyl acrylate, cyanoethyl (mono)acrylate, isobornyl acrylate, octadecyl acrylate, isodecyl acrylate, lauryl acrylate, β-carboxyethyl acrylate, tetrahydrofurfuryl acrylate, dinitrile acrylate, pentafluorophenyl acrylate, nitrophenyl acrylate, 2-phenoxyethyl acrylate, 2,2,2-trifluoromethyl acrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tripropylene glycol diacrylate, and tetraethylene glycol diacrylate. Examples of the vinyl compounds include aryl diacrylate, neopentyl glycol diacrylate, propoxylated neopentyl glycol diacrylate, polyethylene glycol diacrylate, tetraethylene glycol diacrylate, bisphenol A epoxy diacrylate, trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, propylated trimethylolpropane triacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, phenylthioethyl acrylate, naphthyloxyethyl acrylate, Ebecryl™ 130 cyclic diacrylate (CYTEC INDUSTRIES, INC., New Jersey, USA), epoxy acrylate CN120E50 (Sartomer Company, Exton, Pennsylvania, USA), the corresponding methacrylates of the above acrylates, and mixtures thereof. Representative vinyl compounds include vinyl ether, styrene, vinyl naphthylene, and acrylonitrile. Representative alcohols include hexanediol, naphthalenediol, 2-hydroxyacetophenone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, and hydroxyethyl methacrylate. Representative vinyl compounds include vinyl ether, styrene, vinyl naphthylene, and acrylonitrile.Representative carboxylic acids include phthalic acid, terephthalic acid, and (meth)acrylic acid. Representative acid anhydrides include phthalic anhydride and glutaric anhydride. Representative acyl halides include hexanedioyl dichloride and succinyl dichloride. Representative thiols include ethylene glycol-bisthioglycolate and phenylthioethyl acrylate. Representative amines include ethylenediamine and hexane 1,6-diamine.

[0043] From the viewpoints of reactivity, stability, and cost, for example, tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane can be suitably used as the alkoxide, and these may be used alone or in a mixture of two or more kinds. Examples of the water-soluble polymer include vinyl alcohol resins, polyvinylpyrrolidone, starch, and cellulose resins, and among them, vinyl alcohol resins with excellent gas barrier properties are preferred. Examples of vinyl alcohol resins include polyvinyl alcohol, ethylene-vinyl alcohol copolymers, and modified polyvinyl alcohol, and these resins may be used alone or in a mixture of two or more kinds. Vinyl alcohol resins are generally obtained by saponifying polyvinyl acetate or its copolymers, and may be partially saponified by saponifying a part of the acetate group, or may be completely saponified, but a higher degree of saponification is preferable.

[0044] The means for applying the coating liquid containing the resin that forms the B layer is not particularly limited, and it is preferable to adjust the solid content concentration of the coating material so that the thickness after drying will be the desired thickness, and apply the coating material by a wet coating method such as gravure coating, rod coating, bar coating, die coating, or spray coating, or a dry processing method such as vacuum deposition, plasma CVD, laser CVD, or thermal CVD.

[0045] When the material forming the B layer is an inorganic film, the mass density is set to 2.1 g / cm in order to suppress the progress of MgO crystallization even in the presence of water or water vapor. 3More than 7.5g / cm 3 The mass density is preferably 2.1 g / cm 3 If the mass density is 2.1 g / cm or more, a highly dense B layer is easily formed, and the effect of suppressing the progress of MgO crystallization is improved, which is preferable. 3 If the mass density is smaller than 2.1 g / cm, the density of the B layer is low and a coarse and dense film is formed, so that the crystallization progress may not be sufficiently suppressed. Therefore, in the present invention, the mass density of the inorganic film forming the B layer is 2.1 g / cm 3 More than 7.5g / cm 3 The following is preferred:

[0046] The inorganic film of the present invention refers to a film containing an inorganic substance. The inorganic substance may be a simple inorganic substance or an inorganic compound, such as tin, indium, zinc, aluminum, nickel, chromium, and titanium, and their oxides, nitrides, and carbides, and these may be used alone or in a mixture of two or more kinds. That is, it is preferable that the B layer contains one or more selected from tin, indium, zinc, aluminum, nickel, chromium, and titanium.

[0047] When the B layer is made of an inorganic film, the thickness is preferably 10 nm or more and 500 nm or less, more preferably 20 nm or more and 400 nm or less, and even more preferably 30 nm or more and 300 nm or less. If the thickness of the B layer is less than 10 nm, the amount of water or water vapor in contact with the A layer increases, so that the progress of MgO crystallization in the A layer may not be sufficiently suppressed. If the thickness of the B layer is more than 500 nm, the flexibility of the laminate decreases, cracks are easily generated, and water or water vapor penetrates to the A layer, so that the progress of MgO crystallization in the A layer may not be sufficiently suppressed. Here, the thickness of the B layer is determined from the definition in the same way.

[0048] The inorganic film forming the layer B of the laminate of the present invention is preferably an inorganic substance or an inorganic oxide, and from the viewpoints of denseness, transparency, etc., it is preferable that it contains one or more elements selected from tin, indium, zinc, aluminum, nickel, chromium, and titanium. From the viewpoint of transparency, it is more preferable that the layer B used in the present invention is formed mainly from the oxide of the inorganic substance. Note that, "mainly composed of an oxide of an inorganic substance" means that the oxide of an inorganic substance is contained in 80% by mass or more of the film 100% by mass.

[0049] Examples of inorganic oxides include tin-doped indium oxide (ITO), fluorine-doped tin oxide (FTO), tin oxide (SnO), indium zinc oxide (IZO), zinc oxide (ZnO), and aluminum oxide (Al 2 O 3 ), nickel oxide (NiO), chromium oxide (Cr 2 O 3 ), titanium dioxide (TiO 2 ) and the like. When oxides such as ITO, whose main component is indium oxide, are formed by sputtering or other methods, an amorphous film, which is a metastable phase, is formed. A typical method for reducing distortion and grain boundaries in the structure to be formed is to increase the crystallinity by annealing. Furthermore, it is even better if the inorganic oxide is a conductive film. If the inorganic oxide is insulating, friction during the film winding process can cause the B layer to become charged, and discharge can cause scratches or pinholes on the laminate surface. There is a concern that water or water vapor can pass through the scratches or pinholes, accelerating the crystallization of MgO. The surface resistance of inorganic oxides is 1×10 -4 It is preferable that the resistance is Ω / □ or less.

[0050] The mass density in the present invention can be measured by X-ray reflectometry (XRR).

[0051] The method for forming layer B made of an inorganic substance or an inorganic oxide is not particularly limited, and examples of methods that can be used include dry processing methods such as vacuum deposition, sputtering, reactive sputtering, molecular beam epitaxy, cluster ion beam, ion plating, atomic layer deposition, plasma polymerization, atmospheric pressure plasma polymerization, plasma CVD, laser CVD, thermal CVD, and coating, and wet coating methods such as gravure coating, rod coating, bar coating, die coating, and spray coating.

[0052] [Base material] The substrate used in the present invention is preferably in the form of a film in order to ensure flexibility. The film may be a single-layer film or a film having two or more layers, for example, a film formed by a co-extrusion method. The type of film may be a non-stretched film, a uniaxially stretched film, or a biaxially stretched film.

[0053] The material of the substrate used in the present invention is not particularly limited, but it is preferable that the substrate is mainly composed of an organic polymer. Examples of organic polymers that can be suitably used in the present invention include crystalline polyolefins such as polyethylene and polypropylene, amorphous cyclic polyolefins having a cyclic structure, polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyamides, polycarbonates, polystyrene, polyvinyl alcohol, saponified ethylene-vinyl acetate copolymers, polyacrylonitrile, polyacetal, and various other polymers. Among these, it is preferable to use amorphous cyclic polyolefins or polyethylene terephthalate, which have excellent transparency, versatility, and mechanical properties. In addition, the organic polymer may be either a homopolymer or a copolymer, and only one type of organic polymer may be used, or multiple types may be blended and used.

[0054] The surface of the substrate on which the layer A is formed may be pretreated to improve adhesion and smoothness by corona treatment, plasma treatment, ultraviolet treatment, ion bombardment treatment, solvent treatment, or treatment to form an anchor coat layer composed of an organic or inorganic substance or a mixture thereof. Also, on the side opposite to the side on which the layer A is formed, a coating layer of an organic or inorganic substance or a mixture thereof may be laminated for the purpose of improving the slipperiness during winding of the substrate and the scratch resistance of the substrate. The thickness of the substrate used in the present invention is not particularly limited, but is preferably 500 μm or less from the viewpoint of ensuring flexibility, and is preferably 5 μm or more from the viewpoint of ensuring strength against tension and impact. Furthermore, the thickness of the substrate is more preferably 10 μm or more and 150 μm or less from the viewpoint of ease of processing and handling of the film.

[0055] [Anchor coat layer] The laminate of the present invention has an anchor coat layer, and it is preferable that one side of the anchor coat layer is in contact with the substrate and the other side is in contact with the A layer. Furthermore, it is more preferable that the anchor coat layer contains a structure obtained by crosslinking a polyurethane compound having an aromatic ring structure. When defects such as protrusions or scratches exist on the substrate, pinholes or cracks may occur in the A layer laminated on the substrate starting from the defects, which may impair gas barrier properties and bending resistance, so it is preferable to provide an anchor coat layer. In addition, when the difference in thermal dimensional stability between the substrate and the A layer is large, gas barrier properties and bending resistance may also decrease, so it is preferable to provide an anchor coat layer. In addition, the anchor coat layer used in the present invention preferably contains a structure obtained by crosslinking a polyurethane compound having an aromatic ring structure from the viewpoint of thermal dimensional stability and bending resistance, and more preferably contains an ethylenically unsaturated compound, a photopolymerization initiator, an organic silicon compound and / or an inorganic silicon compound.

[0056] The polyurethane compound having an aromatic ring structure used in Layer A of the laminate of the present invention has an aromatic ring and a urethane bond in the main chain or side chain, and can be obtained, for example, by polymerizing an epoxy (meth)acrylate, a diol compound, or a diisocyanate compound having a hydroxyl group and an aromatic ring in the molecule.

[0057] An epoxy (meth)acrylate having a hydroxyl group and an aromatic ring in the molecule can be obtained by reacting a diepoxy compound of an aromatic glycol, such as bisphenol A type, hydrogenated bisphenol A type, bisphenol F type, hydrogenated bisphenol F type, resorcin, or hydroquinone, with a (meth)acrylic acid derivative.

[0058] Examples of the diol compound include ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2,4-dimethyl-2-ethylhexane-1,3-diol, neopentyl glycol, 2-ethyl-2-butyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 1,2-cyclohexadecane, and the like. Examples of the usable components include diphenylmethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 4,4'-thiodiphenol, bisphenol A, 4,4'-methylenediphenol, 4,4'-(2-norbornylidene)diphenol, 4,4'-dihydroxybiphenol, o-, m-, and p-dihydroxybenzene, 4,4'-isopropylidenephenol, 4,4'-isopropylidenebindiol, cyclopentane-1,2-diol, cyclohexane-1,2-diol, cyclohexane-1,4-diol, and bisphenol A. These may be used in a single composition or in a mixture of two or more components.

[0059] Examples of the diisocyanate compound include aromatic diisocyanates such as 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,4-diphenylmethane diisocyanate, and 4,4-diphenylmethane diisocyanate, ethylene diisocyanate, hexamethylene diisocyanate, and 2,2,4-trimethylhexamethylene diisocyanate, Examples of the isocyanate include aliphatic diisocyanate compounds such as 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, and lysine triisocyanate, alicyclic isocyanate compounds such as isophorone diisocyanate, dicyclohexylmethane-4,4-diisocyanate, and methylcyclohexylene diisocyanate, and aromatic aliphatic isocyanate compounds such as xylylene diisocyanate and tetramethylxylylene diisocyanate, etc. These may be used as a single composition or as a mixture of two or more components.

[0060] The component ratio of the epoxy (meth)acrylate having a hydroxyl group and an aromatic ring in the molecule, the diol compound, and the diisocyanate compound is not particularly limited as long as it is within a range that results in a desired weight average molecular weight. The weight average molecular weight (Mw) of the polyurethane compound having an aromatic ring structure in the present invention is preferably 5,000 to 100,000. If the weight average molecular weight (Mw) is 5,000 to 100,000, the resulting cured film has excellent thermal dimensional stability and bending resistance, which is preferable. The weight average molecular weight (Mw) in the present invention is a value measured using gel permeation chromatography and converted into standard polystyrene.

[0061] Examples of ethylenically unsaturated compounds include di(meth)acrylates such as 1,4-butanediol di(meth)acrylate and 1,6-hexanediol di(meth)acrylate, polyfunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate, and epoxy acrylates such as bisphenol A type epoxy di(meth)acrylate, bisphenol F type epoxy di(meth)acrylate, and bisphenol S type epoxy di(meth)acrylate. Among these, polyfunctional (meth)acrylates that are excellent in thermal dimensional stability and surface protection performance are preferred. In addition, these may be used in a single composition, or two or more components may be mixed and used.

[0062] The content of the ethylenically unsaturated compound is not particularly limited, but from the viewpoint of thermal dimensional stability and surface protection performance, it is preferably in the range of 5 to 90 mass%, and more preferably in the range of 10 to 80 mass%, of the total amount (100 mass%) of the ethylenically unsaturated compound and the polyurethane compound having an aromatic ring structure.

[0063] The photopolymerization initiator is not particularly limited as long as it can maintain the gas barrier properties and flex resistance of the laminate of the present invention. Examples of photopolymerization initiators that can be suitably used in the present invention include 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, phenyl glyoxylic acid methyl ester, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-2-methyl- ... )-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone and other alkylphenone-based photopolymerization initiators; 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, acylphosphine oxide-based photopolymerization initiators such as bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and other titanocene-based photopolymerization initiators such as bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium; and photopolymerization initiators having an oxime ester structure such as 1,2-octanedione,1-[4-(phenylthio)-,2-(0-benzoyloxime)].

[0064] Among these, from the viewpoint of curability and surface protection performance, photopolymerization initiators selected from 1-hydroxy-cyclohexylphenyl-ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide are preferred. These may be used in a single composition or in a mixture of two or more components.

[0065] The content of the photopolymerization initiator is not particularly limited, but from the viewpoint of curability and surface protection performance, it is preferably in the range of 0.01 to 10 mass %, and more preferably in the range of 0.1 to 5 mass %, of the total amount of polymerizable components.

[0066] Examples of the organosilicon compound include vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-isocyanatepropyltriethoxysilane.

[0067] Among these, from the viewpoint of curability and polymerization activity by irradiation with active energy rays, at least one organosilicon compound selected from the group consisting of 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, vinyltrimethoxysilane, and vinyltriethoxysilane is preferred. These may be used in a single composition or in a mixture of two or more components.

[0068] The content of the organosilicon compound is not particularly limited, but from the viewpoint of curability and surface protection performance, it is preferably in the range of 0.01 to 10 mass %, and more preferably in the range of 0.1 to 5 mass %, of the total amount of polymerizable components.

[0069] As the inorganic silicon compound, silica particles are preferred from the viewpoints of surface protection performance and transparency, and the primary particle size of the silica particles is preferably in the range of 1 to 300 nm, more preferably in the range of 5 to 80 nm. Note that the primary particle size here refers to the particle diameter d calculated by applying the specific surface area s calculated by the gas adsorption method to the following formula (1): d=6 / ρs (1) ρ: Density.

[0070] The thickness of the anchor coat layer is preferably 200 nm or more and 4,000 nm or less, more preferably 300 nm or more and 2,000 nm or less, and even more preferably 500 nm or more and 1,000 nm or less. If the thickness of the anchor coat layer is thinner than 200 nm, the adverse effects of defects such as protrusions and scratches present on the substrate may not be suppressed. If the thickness of the anchor coat layer is thicker than 4,000 nm, the smoothness of the anchor coat layer decreases and the uneven shape of the surface of the A layer laminated on the anchor coat layer also becomes large, making it difficult for the laminated vapor deposition film to become dense, and the effect of improving the gas barrier property may be difficult to obtain. Here, the thickness of the anchor coat layer can be measured from a cross-sectional observation image by a transmission electron microscope (TEM).

[0071] The arithmetic mean roughness Ra of the anchor coat layer is preferably 10 nm or less. When Ra is 10 nm or less, it is preferable because it is easy to form a homogeneous A layer on the anchor coat layer, and the repeatability reproducibility of the gas barrier property is improved. When the surface Ra of the anchor coat layer is greater than 10 nm, the uneven shape of the A layer surface on the anchor coat layer also becomes large, the evaporated film is difficult to be dense, and the effect of improving the gas barrier property may be difficult to obtain. In addition, cracks due to stress concentration are likely to occur in the part with many unevenness, which may cause a decrease in the repeatability reproducibility of the gas barrier property. Therefore, in the present invention, it is preferable to set the Ra of the anchor coat layer to 10 nm or less, more preferably 5 nm or less. The Ra of the anchor coat layer in the present invention can be measured by a cross-sectional TEM.

[0072] When applying an anchor coat layer to the laminate of the present invention, as an example of a coating means for a coating liquid containing a resin that forms an anchor coat layer containing a polyurethane compound having an aromatic ring structure, it is preferable to first adjust the solid content concentration of a coating material containing a polyurethane compound having an aromatic ring structure on a substrate so that the thickness after drying is a desired thickness, and then apply the coating material by, for example, a reverse coating method, a gravure coating method, a rod coating method, a bar coating method, a die coating method, a spray coating method, a spin coating method, etc. Also, in the present invention, it is preferable to dilute the coating material containing a polyurethane compound having an aromatic ring structure using an organic solvent from the viewpoint of coating suitability.

[0073] Specifically, it is preferable to dilute the coating material to a solid content concentration of 10% by mass or less using a hydrocarbon solvent such as xylene, toluene, methylcyclohexane, pentane, or hexane, or an ether solvent such as dibutyl ether, ethyl butyl ether, or tetrahydrofuran. These solvents may be used alone or in combination of two or more. In addition, various additives may be added to the coating material for forming the anchor coat layer as necessary. For example, catalysts, antioxidants, light stabilizers, stabilizers such as ultraviolet absorbers, surfactants, leveling agents, antistatic agents, etc. may be used.

[0074] Next, it is preferable to dry the coating film after application to remove the dilution solvent. Here, the heat source used for drying is not particularly limited, and any heat source such as a steam heater, an electric heater, or an infrared heater can be used. In order to improve gas barrier properties, the heating temperature is preferably 50 to 150°C. In addition, the heat treatment time is preferably several seconds to 1 hour. Furthermore, the temperature may be constant during the heat treatment, or the temperature may be gradually changed. In addition, the heat treatment may be performed while adjusting the humidity in the range of 20 to 90% RH in terms of relative humidity during the drying treatment. The heat treatment may be performed in the air or while an inert gas is enclosed.

[0075] Next, it is preferable to subject the dried coating film containing a polyurethane compound having an aromatic ring structure to an active energy ray irradiation treatment to crosslink the coating film, thereby forming an anchor coat layer.

[0076] The active energy rays to be applied in such a case are not particularly limited as long as they can cure the anchor coat layer, but it is preferable to use ultraviolet treatment from the viewpoint of versatility and efficiency. As the ultraviolet source, known ones such as high pressure mercury lamps, metal halide lamps, microwave type electrodeless lamps, low pressure mercury lamps, xenon lamps, etc. can be used. In addition, it is preferable to use the active energy rays under an inert gas atmosphere such as nitrogen or argon from the viewpoint of curing efficiency. The ultraviolet treatment may be performed either under atmospheric pressure or under reduced pressure, but in the present invention, it is preferable to perform the ultraviolet treatment under atmospheric pressure from the viewpoint of versatility and production efficiency. Regarding the oxygen concentration during the ultraviolet treatment, the oxygen gas partial pressure is preferably 1.0% or less, more preferably 0.5% or less, from the viewpoint of controlling the crosslinking degree of the anchor coat layer. The relative humidity may be arbitrary.

[0077] As the ultraviolet ray generating source, known sources such as a high pressure mercury lamp, a metal halide lamp, a microwave type electrodeless lamp, a low pressure mercury lamp, a xenon lamp, etc. can be used.

[0078] The cumulative amount of UV light is 0.1 to 1.0 J / cm 2 is preferably 0.2 to 0.6 J / cm 2 It is more preferable that the integrated light amount is 0.1 J / cm 2 If the integrated light amount is 1.0 J / cm or more, a desired degree of crosslinking of the anchor coat layer can be obtained, which is preferable. 2 If the thickness is less than this, damage to the substrate can be reduced, which is preferable.

[0079] [Other layers] The laminate of the present invention may be formed with an overcoat layer or a sealing resin layer for the purpose of improving scratch resistance, chemical resistance, printability, etc., within a range in which the gas barrier property and water vapor transmission rate are not reduced, or may have a laminated structure in which an adhesive layer or film made of an organic polymer compound is laminated for bonding to an element, etc. Also, a low refractive index layer may be formed to improve optical properties. In particular, from the viewpoint of transparency and conductivity, a transparent electrode layer can also be used as an electrode for a solar cell or an organic light-emitting element.

[0080] As long as Layer B fulfills the above functions, it may also serve as an overcoat layer, a sealing resin layer, an adhesive layer, and a low refractive index layer. The overcoat layer and the sealing resin layer may be formed on either side of the laminate.

[0081] [Applications of laminates] Since the laminate of the present invention has both high light transmittance and gas barrier properties, it can be suitably used for optical elements such as electronic paper and organic electroluminescence (EL) displays. In addition, it can be suitably used for solar cells and flexible displays, which will be described later.

[0082] [Solar cell] A preferred embodiment of the solar cell of the present invention is a solar cell including the laminate. This embodiment allows the solar cell to have high durability and energy conversion efficiency, and also has excellent appearance quality. In particular, organic solar cells, dye-sensitized solar cells, and perovskite solar cells have low corrosion resistance to water, so it is expected that the use of the laminate of the present invention will provide a higher effect.

[0083] [Flexible display] A preferred embodiment of the flexible display of the present invention is a flexible display using the laminate or optical laminate described above. By using this embodiment, the flexible display can have high durability and excellent appearance quality and color characteristics. EXAMPLES

[0084] The present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.

[0085] [Evaluation method] (1) Thickness of each layer The thickness of each layer of the laminate was analyzed by X-ray photoelectron spectroscopy (XPS). 2 Etching and composition analysis were repeated at 5 nm equivalent thickness intervals. The thickness of layer B was measured by removing layers from the top surface of the laminate, starting from the measurement point where the magnesium content was 1 atm% or less, and repeating argon ion etching and analysis. The measurement was terminated at the measurement point where the magnesium content in layer B was 1 atm% or more. The thickness of layer A was measured from the measurement point defined as the end point of layer B, starting from the measurement point defined as the end point of layer B, and repeating argon ion etching and analysis. The measurement was terminated at the measurement point where the magnesium content in layer A was 1 atm% or less.

[0086] The peaks used in the analysis were 2s for magnesium and 1s for oxygen.

[0087] The XPS measurement conditions were as follows. Equipment: PHI5000VersaProbeII (ULVAC-PHI) Excitation X-ray: monochromatic AlKα Analysis range: φ100μm Photoelectron escape angle: 45° Ar ion etching: 2.0kV, raster size 2×2.

[0088] (2) Composition of Layer A The composition of the A layer of the laminate was analyzed by X-ray photoelectron spectroscopy (XPS). The SiO 2 The content ratio of each element was measured at the location where etching was performed based on the converted thickness. The peaks used in the analysis were 2s for magnesium, 2p for silicon, and 1s for oxygen.

[0089] The O1s half-width is the maximum value of the peak. max If the peak intensity is F max The peak width at 1 / 2 was calculated.

[0090] The XPS measurement conditions were as follows. Equipment: PHI5000VersaProbeII (ULVAC-PHI) Excitation X-ray: monochromatic AlKα Analysis range: φ100μm Photoelectron escape angle: 45° Ar ion etching: 3.0kV, raster size 2×2.

[0091] (3) Water vapor permeability The water vapor permeability of the laminate was measured at a temperature of 40°C, humidity of 90% RH, and an area of ​​50 cm 2 The measurements were performed under the following conditions using a water vapor transmission rate measuring device (model name: DELTAPERM (registered trademark)) manufactured by Technolox, UK. Two samples were measured per level. The data obtained from the measurements of the two samples were averaged and rounded off to the first decimal place, and the resulting value was calculated as the water vapor transmission rate (g / m 2 / day).

[0092] (4)Light transmittance The total light transmittance was measured using a haze meter NDH4000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with the JIS K7361 (1997) standard.

[0093] (5) Spectral characteristics (spectral reflectance) Using a spectrophotometer V-670 (manufactured by JASCO Corporation) and an absolute reflectance measurement unit ARSN-733, the spectral reflectance in the wavelength range of 300 to 800 nm was measured under the following conditions.

[0094] Of the obtained data, the average spectral reflectance at wavelengths of 380 nm to 780 nm was evaluated. Incident angle: 5° (vertical direction to the sample plane is 0°) ·Measurement wavelength: 300nm~800nm Bandwidth: 5.0nm Data capture interval: 0.5 nm Scanning speed: 1,000nm / min

[0095] (6) Mass density The mass density of layer B was calculated using XRR (X-ray reflectivity measurement). The laminate was sampled to 30 mm x 40 mm, fixed to a sample holder, and X-ray reflectivity measurement was performed under the following measurement conditions. In the measurement data, the density value was estimated from the critical angle, and the film thickness value was estimated from the vibration period. Curve fitting was performed using these as initial values, and analysis was performed by optimizing each parameter of film thickness and density, and the thickness, density, and structural density index of each region were measured under the following conditions. Equipment: Rigaku SmartLab Analysis software: Rigaku GlobalFit Sample size: 30mm x 40mm ·Incoming X-ray wavelength: 0.1541nm (Cu Kα1 ray) Output: 45kV, 30mA Entrance slit size: 0.05mm x 5.0mm Receiving slit size: 0.05mm x 20.0mm Measurement range (θ): 0~4.0° Step(θ): 0.002°

[0096] (7) Positron lifetime and pore radius distribution The positron lifetime and pore radius distribution were measured by the positron beam method (thin film positron annihilation lifetime measurement method). The sample to be measured was attached to a 15 mm x 15 mm square Si wafer, degassed in vacuum at room temperature, and then measured. The measurement conditions were as follows: Equipment: Fuji Invac small positron beam generator PALS200A ·Positron source: 22 Na-based positron beam Gamma ray detector: BaF 2 Scintillator + photomultiplier tube ·Device constants: 255~278ps, 24.55ps / ch Beam intensity: 1keV Measurement depth: 0 to 100 nm (estimated) ·Measurement temperature: room temperature Measurement atmosphere: Vacuum Measurement count: Approx. 5,000,000 counts The measurement results were subjected to three-component analysis using the nonlinear least squares program POSITRONFIT.

[0097] (8) Constant temperature and humidity test The test was conducted in accordance with the standard JIS C 60068-2-78 (2015). The test conditions are as follows: Test temperature: 85±2℃ Relative humidity: 85±5%RH Test time: 250 hours

[0098] After the test, the water vapor transmission rate of the samples was measured in the same manner as above, and the change in water vapor transmission rate was evaluated as follows. ◎: Change in water vapor transmission rate is 1.0×10 -3 g / m 2 Less than / day 〇: Change in water vapor transmission rate is 1.0×10 -3 Above 5.0×10 ―3 g / m 2 Less than / day △: Change in water vapor transmission rate is 5.0×10 -3 More than 7.5 x 10 ―3 g / m 2 Less than / day ×: Change in water vapor transmission rate is 7.5×10 ―3 g / m 2 / day or more

[0099] The change in water vapor transmission rate was calculated using the following formula. Change in water vapor transmission = (water vapor transmission rate after constant temperature and humidity test) - (water vapor transmission rate before constant temperature and humidity test).

[0100] (9) Evaluation of crystallization progress The progress of MgO crystallization was measured by XRD (X-ray diffraction). The sample to be measured was attached to a 10mm x 10mm square silicon non-reversible plate, and measurements were performed at room temperature and normal pressure. The diffraction peak used in the analysis was the diffraction peak on the 002 plane of the MgO crystal, and the progress of crystallization was evaluated based on the presence or absence of this peak. The diffraction peak was evaluated by regarding the signal that could be detected from the signal (S) to noise (N) ratio (S / N) as one peak. The measurement conditions were as follows: Equipment: Rigaku SmartLab (rotating anode type) ·X-ray source: CuKα ray Output: 45kV, 200mA Slit system: 2 / 3°×10mm-sample-0.3mm-0.8mm Incident vertical divergence prevention solar slit 5° Vertical solar slit for preventing divergence of light receiving 5° Scan method: 2θ / θ continuous scan Measurement range (2θ): 5~60° Scan step: 0.02° Scan speed: 0.5° / min The S / N ratio was evaluated as follows. ◎: S / N less than 2.5 〇: S / N is 2.5 or more and less than 5.0 ×: S / N is 5.0 or more

[0101] Example 1 (Synthesis of polyurethane compounds having aromatic ring structures) In a 5-liter four-neck flask, 300 parts by mass of bisphenol A diglycidyl ether acrylic acid adduct (manufactured by Kyoeisha Chemical Co., Ltd., product name: Epoxy Ester 3000A) and 710 parts by mass of ethyl acetate were placed and heated to an internal temperature of 60°C. 0.2 parts by mass of di-n-butyltin dilaurate was added as a synthesis catalyst, and 200 parts by mass of dicyclohexylmethane 4,4'-diisocyanate (manufactured by Tokyo Chemical Industry Co., Ltd.) were added dropwise over 1 hour while stirring. After the end of the dropwise addition, the reaction was continued for 2 hours, and then 25 parts by mass of diethylene glycol (manufactured by Wako Pure Chemical Industries, Ltd.) were added dropwise over 1 hour. After the dropwise addition, the reaction was continued for 5 hours to obtain a polyurethane compound having an aromatic ring structure with a weight average molecular weight of 20,000.

[0102] (Formation of anchor coat layer) A polyethylene terephthalate film having a thickness of 50 μm ("Lumirror" (registered trademark) U48 manufactured by Toray Industries, Inc.) was used as the substrate.

[0103] As a coating liquid for forming an anchor coat layer, 150 parts by mass of the polyurethane compound, 20 parts by mass of dipentaerythritol hexaacrylate (manufactured by Kyoeisha Chemical Co., Ltd., trade name: Light Acrylate DPE-6A), 5 parts by mass of 1-hydroxy-cyclohexylphenyl ketone (manufactured by BASF Japan Ltd., trade name: "IRGACURE" (registered trademark) 184), 3 parts by mass of 3-methacryloxypropylmethyldiethoxysilane (manufactured by Shin-Etsu Silicone Co., Ltd., trade name: KBM-503), 170 parts by mass of ethyl acetate, 350 parts by mass of toluene, and 170 parts by mass of cyclohexanone were mixed to prepare a coating liquid. Next, the coating liquid was applied to the substrate with a microgravure coater (gravure line number 150UR, gravure rotation ratio 100%), dried at 100 ° C. for 1 minute, and after drying, ultraviolet treatment was performed under the following conditions to provide an anchor coat layer with a thickness of 1 μm. UV treatment equipment: LH10-10Q-G (manufactured by Fusion UV Systems Japan) Inlet gas: N 2 (Nitrogen inert box) UV source: Microwave electrodeless lamp Accumulated light output: 400mJ / cm 2 Sample temperature control: room temperature.

[0104] (Formation of Layer A) Using the winding type deposition device shown in Figure 2, MgO+SiO was deposited as layer A on the surface of the anchor coat layer of the substrate by electron beam (EB) deposition. 2 The layer was formed to a target thickness of 200 nm.

[0105] The specific procedure is as follows. First, as the deposition material, granular magnesium oxide (MgO) (purity 99.9%) and silicon dioxide (SiO) with a size of about 2 to 5 mm were used. 2 (99.99% purity) were preheated at 100°C for 8 hours. Then, each material was set in a carbon hearth liner 11 as shown in Figure 3. The area ratio of the materials was MgO:SiO 2 =1:1. In the winding chamber 5, the substrate 1 was set on the unwinding roll 6 so that the surface on which the A layer was to be formed faced the hearth liner 11, and was unwound and passed through the main drum 10 via guide rolls 7, 8, and 9. At this time, the temperature of the main drum was controlled to -10°C. Next, the pressure inside the deposition device 4 was reduced by the vacuum pump, and the pressure was reduced to 5.0 x 10 -3 Next, an electron gun (hereinafter, EB gun) 13 was used as a heating source, and MgO and SiO were heated to a film composition ratio of about Mg:Si=2:1 in atomic concentration (atm%). 2 The heating ratio was controlled. The EB gun had an acceleration voltage of 10 kV, and the acceleration current and film transport speed were adjusted so that the thickness of the A layer formed was about 200 nm, and the A layer was formed on the surface of the substrate 1. Thereafter, the film was taken up on a take-up roll 18 via guide rolls 15, 16, and 17.

[0106] (Formation of layer B containing organic matter) Following the formation of the A layer, the coating liquid for forming the B layer was prepared by blending 150 parts by mass of the polyurethane compound, 20 parts by mass of dipentaerythritol hexaacrylate (manufactured by Kyoeisha Chemical Co., Ltd., trade name: "Light Acrylate" (registered trademark) DPE-6A), 5 parts by mass of 1-hydroxy-cyclohexylphenyl-ketone (manufactured by BASF Japan Ltd., trade name: "IRGACURE" (registered trademark) 184), 3 parts by mass of 3-methacryloxypropylmethyldiethoxysilane (manufactured by Shin-Etsu Silicone Co., Ltd., trade name: KBM-503), 170 parts by mass of ethyl acetate, 350 parts by mass of toluene, and 170 parts by mass of cyclohexanone. The coating liquid was then applied to the substrate with a microgravure coater (gravure line number 150UR, gravure rotation ratio 100%), dried at 100 ° C. for 1 minute, and after drying, ultraviolet treatment was performed under the following conditions to provide a B layer having a thickness of 1,500 nm on the A layer. UV treatment equipment: LH10-10Q-G (manufactured by Fusion UV Systems Japan) Inlet gas: N 2 (Nitrogen inert box) UV source: Microwave electrodeless lamp Accumulated light output: 400mJ / cm 2 Sample temperature control: Room temperature

[0107] Example 2 A laminate was obtained in the same manner as in Example 1, except that in forming the B layer, the target thickness was set to 4,500 nm.

[0108] Example 3 A laminate was obtained in the same manner as in Example 1, except that in forming the B layer, the target thickness was set to 700 nm.

[0109] Example 4 On the A layer formed by the above method, a 10% by mass solution of perhydropolysilazane (PHPS, AQUAMICA NN120-10, catalyst-free type, manufactured by AZ Electronic Materials Co., Ltd.) in dibutyl ether was applied with a wireless bar as the B layer, dried for 1 minute in an atmosphere of 65°C temperature and 55% RH humidity, and further held for 10 minutes in an atmosphere of 25°C temperature and 10% RH (dew point temperature -8°C) temperature and dehumidified. After dehumidification, a modification treatment was performed under the following conditions, and a laminate was obtained in the same manner as in Example 1, except that a 750 nm thick B layer was provided on the A layer. Modification treatment equipment: Excimer irradiation equipment MODEL: MECL-M-1-200 (manufactured by M.D.COM) Wavelength: 172nm Lamp filling gas: Xe Excimer light intensity: 130mW / cm 2 (172 nm) Stage heating temperature: 70℃ Oxygen concentration in the irradiation device: 1.0% Excimer irradiation time: 5sec

[0110] Example 5 The B layer was coated to a thickness of 1,500 nm using a coating solution prepared by the following procedure. Polyvinyl alcohol (hereinafter sometimes abbreviated as PVA, molecular weight 1,700, saponification degree 98.5%) was added to a solvent with a mass ratio of water / isopropyl alcohol = 97 / 3, and heated and stirred at 90 ° C to obtain a polyvinyl alcohol solution with a solid content of 10 mass %. A tetraethoxysilane solution was also obtained by adding dropwise 13.3 g of 0.02N hydrochloric acid aqueous solution while stirring to a solution mixed with 8.4 g of tetraethoxysilane and 3.3 g of methanol. Furthermore, an ethyl silicate solution was obtained by adding dropwise 5.0 g of 0.06N hydrochloric acid aqueous solution while stirring to a solution mixed with 8.0 g of Ethyl Silicate 48 manufactured by Colcoat Co., Ltd. and 12.0 g of methanol. The tetraethoxysilane solution and the ethyl silicate solution were mixed with SiO 2 The inorganic component solution was obtained by mixing the PVA solids and the SiO 2A polyvinyl alcohol solution and an inorganic component solution were mixed and stirred so that the converted solid content mass ratio was 65 / 35, and then diluted with water to obtain a coating solution with a solid content of 12 mass %. A laminate was obtained in the same manner as in Example 1, except that the obtained coating solution was applied onto Layer A and dried at 110°C to provide Layer B.

[0111] Example 6 Except for forming a B layer containing an inorganic film as the B layer, a laminate was obtained in the same manner as in Example 1. The method for forming the B layer on the A layer is as follows.

[0112] (Formation of layer B containing inorganic substances or inorganic oxides) Following the formation of the A layer, a B layer was provided on the A layer of the base material 34 using a sputtering device having a structure shown in Fig. 5. A sputtering target made of ITO was connected to a sputtering power supply 28, and sputtering was carried out using argon gas and oxygen gas, to provide an ITO layer as the B layer on the A layer of the base material 34 with a target thickness of 500 nm.

[0113] The specific operation is as follows. First, in the winding chamber 22 of the sputtering device 28 in which an ITO sputtering target is placed on the sputtering electrode 28, the side of the base material 34 on which the B layer is to be provided (the side on which the A layer is formed) is set on the unwinding roll 23 so that it faces the sputtering electrode 28, and the base material 34 is unwound and passed through the guide rolls 24, 25, and 26 onto the main drum 27 whose temperature is controlled at 100° C. Next, the pressure inside the sputtering device 21 is reduced by a vacuum pump, and the pressure is reduced to 2.0×10 -3 Next, the vacuum level was 5.0×10 Pa or less. -1 Argon gas and oxygen gas were introduced at an oxygen gas partial pressure of 10% so that the oxygen gas pressure was 10 Pa, and an input power of 1,500 W was applied to the sputtering electrode 28 by a DC pulse power supply to generate argon-oxygen gas plasma, and an ITO layer was formed on the surface of layer A of the substrate 34 by sputtering. The thickness of the ITO layer formed was adjusted by the film transport speed. Thereafter, the film was taken up on a take-up roll 32 via guide rolls 29, 30, and 31 to obtain a laminate.

[0114] Then, test pieces were cut out from the obtained laminate and various evaluations were carried out.

[0115] Example 7 A laminate was obtained in the same manner as in Example 6, except that in forming the B layer, it was provided to have a target thickness of 250 nm.

[0116] Example 8 A laminate was obtained in the same manner as in Example 6, except that in forming layer B, it was provided with a target thickness of 10 nm.

[0117] Example 9 A laminate was obtained in the same manner as in Example 6, except that SnO was used as the sputtering target, sputtering was performed with argon gas and oxygen gas, and an SnO layer was provided as layer B with a target thickness of about 250 nm.

[0118] Example 10 A laminate was obtained in the same manner as in Example 6, except that ZnO was used as the sputtering target, sputtering was performed with argon gas and oxygen gas, and a ZnO layer was provided as layer B with a target thickness of about 250 nm.

[0119] Example 11 Al as a sputtering target 2 O 3 The sputtering was performed using argon gas and oxygen gas, and Al was used as the B layer. 2 O 3 A laminate was obtained in the same manner as in Example 6, except that the layer was provided to a target thickness of about 250 nm.

[0120] Example 12 Cr as a sputtering target 2 O 3 The sputtering was performed using argon gas and oxygen gas, and Cr was used as the B layer. 2 O 3 A laminate was obtained in the same manner as in Example 6, except that the layer was provided to a target thickness of about 250 nm.

[0121] Example 13 TiO as a sputtering target 2 The sputtering was performed with argon gas and oxygen gas, and TiO was used as the B layer. 2 A laminate was obtained in the same manner as in Example 6, except that the layer was provided to a target thickness of about 250 nm.

[0122] Example 14 A laminate was obtained in the same manner as in Example 6, except that NiO was used as the sputtering target, sputtering was performed with argon gas and oxygen gas, and a NiO layer was provided as layer B with a target thickness of about 250 nm.

[0123] Comparative Example 1 A laminate was obtained in the same manner as in Example 1, except that the layer B was not formed.

[0124] Comparative Example 2 Using the above-mentioned polyurethane compound as the coating material, the coating liquid was applied to the surface of the anchor coat layer of the substrate using a microgravure coater to provide a polyurethane compound layer as layer B with a target thickness of 2,000 nm on the surface of the anchor coat layer of the substrate shown in Figure 6.

[0125] Comparative Example 3 Using ITO as a sputtering target, an ITO layer was formed as layer B to a target thickness of 200 nm on the surface of the anchor coat layer of the substrate shown in FIG. 6 by a sputtering method using argon gas and oxygen gas.

[0126] [Table 1]

[0127] [Table 2]

[0128] [Table 3]

[0129] In Example 1, the B layer is a polyurethane resin film, and the total light transmittance is 89.0% or more, the average spectral reflectance is 14.0% or less, and the water vapor transmission rate is 1.0×10 -3 g / m 2 / day, which is favorable. Furthermore, the S / N ratio of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was favorable at less than 2.5. In Example 2, the total light transmittance was 86.0% or more because the film thickness was as thick as 1500 nm, but the average spectral reflectance was favorable at 14.0% or less, and the change in water vapor transmission rate was also 1.0×10 -3 g / m 2 / day, which is favorable. Furthermore, the S / N ratio of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was favorable at less than 2.5. Furthermore, in Example 3, the total light transmittance was 90.0% or more and the average spectral reflectance was 14.0% or less, which is favorable, but since the thickness of layer B was a thin film at 735 nm, the S / N ratio of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was 2.5 or more and less than 5.0. The change in water vapor transmission rate was 1.0×10 -3 Above 5.0×10 ―3 g / m 2 In Example 4, the total light transmittance was 89.0% or more and the average spectral reflectance was 14.0% or less, which was favorable. However, since the thickness of the B layer was a thin film of 750 nm, the S / N ratio of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was 2.5 or more and less than 5.0, but the change in water vapor transmission rate was 1.0×10 -3 Above 5.0×10 ―3 g / m 2 In Example 5, the total light transmittance is 90.0% or more, the average spectral reflectance is 14.0% or less, and the water vapor transmission rate change is 1.0×10 -3 g / m 2 / day, which is favorable. Furthermore, the S / N ratio of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was favorable at less than 2.5. In Examples 6 to 7, even when the B layer formed an ITO film and had different thicknesses, the total light transmittance was favorable at 86.0% or more, and the change in water vapor transmission rate was also favorable at less than 1.0×10 -3g / m 2 / day, which is favorable. Furthermore, the S / N of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was favorable at less than 2.5. In Example 8, the total light transmittance was 90.0% or more and the average spectral reflectance was 14.0% or less, which is favorable. However, since the thickness of the B layer was a thin film of 20 nm, the S / N of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was 2.5 or more and less than 5.0, but the change in water vapor transmission rate was 1.0×10 -3 Above 5.0×10 ―3 g / m 2 / day. Examples 9 to 10 have a good average spectral reflectance of 14.0% or less, and a mass density of 5.5 g / cm 3 Because the water vapor permeability rate is high, the change is 1.0×10 -3 g / m 2 / day, which is favorable. Furthermore, the S / N ratio of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was favorable at less than 2.5. In Examples 11 and 12, the B layer formed an oxide film with excellent corrosion resistance, and the change in water vapor transmission rate was 1.0×10 -3 g / m 2 In Example 13, the total light transmittance is 90.0% or more, the average spectral reflectance is 14.0% or less, and the water vapor transmission rate change is 1.0×10 -3 g / m 2 / day, which is favorable. Furthermore, the S / N ratio of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, was favorable at less than 2.5. In Example 14, the B layer forms a NiO film having an oxide film with excellent corrosion resistance, and the decrease in water vapor transmission rate is favorable at 10% or less. Furthermore, the S / N ratio of the peak of the 002 plane derived from MgO crystals, which is an evaluation of the progress of crystallization, is less than 2.5, and the change in water vapor transmission rate is also favorable at 1.0×10 -3 g / m 2 / day, which is good.

[0130] Comparative Example 1 has good total light transmittance and average spectral reflectance, but does not have layer B, so the peak S / N of the 002 plane derived from MgO crystals is 5.0 or more, and the crystallization growth suppression effect is inferior to Examples 1 to 14. Comparative Examples 2 and 3 have good total light transmittance and average spectral reflectance, but does not have layer A, which is a highly dense amorphous film, so the water vapor permeability is inferior to Examples 1 to 14. [Industrial Applicability]

[0131] Since the laminate of the present invention has both high light transmittance and gas barrier properties, it can be suitably used in optical elements such as electronic paper and organic electroluminescence (EL) displays. In addition, it can be suitably used in solar cells and flexible displays, but the applications are not limited thereto. [Explanation of symbols]

[0132] 1 Base material 2 A layer 3 Anchor coat layer 4. Winding-type electron beam (EB) deposition equipment 5,22 Winding room 6,23 Unwinding roll 7,8,9,24,25,26 Unwinding side guide roll 10,27 Main drum 11 Haasliner 12 Evaporation materials 13 Electron gun 14 Electron beam 15,16,17,29,30,31 Winding side guide roll 18,32 Winding roll 19 Evaporation material B 20 Evaporation material C 21. Winding sputtering equipment 28 Sputtering Electrode 33 B layer 34 Substrate with layer A formed on the surface

Claims

1. A laminate having an A layer and a B layer on at least one side of a substrate, the A layer containing magnesium, silicon, and oxygen.

2. 2. The laminate according to claim 1, wherein the ratio Mg / (Mg+Si) of atomic concentrations of magnesium atoms to silicon atoms in an average composition in the thickness direction of the A layer is 0.30 to 0.80 atm %.

3. The laminate according to claim 1 or 2, wherein the A layer has an average lifetime of 0.935 ns or less as measured by a positron beam method.

4. 3. The laminate according to claim 1, wherein the A layer has a half-width of an oxygen atom (O1s) peak of 3.25 eV or less as measured by X-ray photoelectron spectroscopy.

5. The laminate of claim 1 , wherein the B layer is a polymeric film.

6. The laminate according to claim 5 , wherein the layer B satisfies both (i) and (ii). (i) Mass density 0.7 g / cm 3 Above 1.75g / cm 3 the following (ii) a thickness of 300 nm or more and 7,000 nm or less

7. 7. The laminate according to claim 5 or 6, wherein the layer B contains at least one selected from a polyurethane compound, a polysilazane compound, a polysiloxane compound, an acrylate, a methacrylate, a mixture of an alkoxide and a water-soluble polymer, and a mixture of a polycondensate of an alkoxide and a water-soluble polymer.

8. The laminate according to claim 1 , wherein the layer B is an inorganic film.

9. The laminate according to claim 8, wherein the B layer is (iii) and (iv). (iii) Mass density 2.1 g / cm 3 Above 7.5g / cm 3 the following (iv) a thickness of 10 nm or more and 500 nm or less

10. 10. The laminate according to claim 8, wherein the layer B contains at least one element selected from the group consisting of tin, indium, zinc, aluminum, nickel, chromium, and titanium.

11. The laminate according to claim 1 or 2, having a total light transmittance of 85% or more.

12. 3. The laminate according to claim 1, having an average reflectance of 15% or less in the visible light region (380-780 nm).

13. A solar cell comprising the laminate according to claim 1 or 2 as a protective member.

Citation Information

Patent Citations

  • Transparent film and method for producing the same, and sputtering target for transparent film formation