Fine porous separator for battery
A microporous separator for batteries, using a specific surfactant and polymerizable monomer, addresses the issues of hydrophilicity and dendrite formation, improving battery durability and performance.
Patent Information
- Application Number
- JP2023084286
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-23
AI Technical Summary
Existing alkaline battery separators suffer from poor long-term hydrophilicity and are prone to dendrite formation leading to short circuits.
A microporous separator for batteries is developed using a microporous base material combined with a poorly water-soluble surfactant having specific HLB values and solubility characteristics, and optionally with a radically polymerizable monomer to maintain hydrophilicity and suppress dendrite formation.
The microporous separator effectively maintains hydrophilicity over a long period, preventing dendrite formation and associated short circuits, enhancing the durability and performance of batteries.
Smart Images

Figure 2024167947000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a microporous separator for a battery. [Background technology]
[0002] In recent years, there has been a demand for improved performance of batteries, particularly secondary batteries, in view of the widespread use of portable devices, hybrid vehicles, and electric vehicles, the development of large stationary batteries for storing surplus power, etc. Various types of secondary batteries are known, including lithium-ion secondary batteries and zinc secondary batteries.
[0003] Incidentally, Patent Document 1 discloses a method for producing a separator for an alkaline battery, which comprises dissolving a polysulfone resin and a nonionic surfactant in a hydrophilic organic solvent to prepare a dope, and immersing this in a non-solvent such as water to regenerate a microporous membrane of polysulfone resin treated with the nonionic surfactant. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 2-276153 Summary of the Invention [Problem to be solved by the invention]
[0005] According to the investigations of the present inventors, the separator for an alkaline battery disclosed in Patent Document 1 required improvement from the viewpoint of long-term durability.
[0006] An object of the present disclosure is to provide a microporous battery separator that is capable of maintaining hydrophilicity for a long period of time and is capable of suppressing dendrites and the associated short circuits. [Means for solving the problem]
[0007] The present inventors conducted intensive research to solve the above problems and discovered that by using a microporous separator for a battery containing a specific surfactant, it is possible to maintain hydrophilicity for a long period of time and to suppress dendrites and the associated short circuits, which led to the present disclosure.
[0008] An example aspect of this embodiment is described as follows.
[0009] (1) A microporous separator for a battery, comprising a microporous substrate and a poorly water-soluble surfactant. (2) The microporous separator for a battery according to (1), wherein the surfactant has an HLB value of 3 to 13, a solubility of the surfactant in water at 25°C of less than 0.2 wt%, and a solubility of the surfactant in at least one polar solvent selected from isopropanol, methanol, ethanol, acetonitrile, acetone, ethylene glycol, xylene, and propylene glycol monomethyl ether acetate at 25°C of 10 wt% or more. (3) The microporous battery separator according to (1) or (2), wherein the surfactant has a hydrophobic portion containing at least one ethynylene group and two or more hydrophilic portions. (4) A microporous separator for a battery, which is obtained by reacting a microporous substrate with a poorly water-soluble surfactant and a radically polymerizable monomer. (5) The microporous separator for a battery according to (4), wherein the surfactant has an HLB value of 3 to 13, a solubility of the surfactant in water at 25° C. of less than 0.2 wt %, and a solubility of the surfactant in at least one polar solvent selected from isopropanol, methanol, ethanol, acetonitrile, acetone, ethylene glycol, xylene, and propylene glycol monomethyl ether acetate at 25° C. of 10 wt % or more. Effect of the Invention
[0010] The present disclosure makes it possible to provide a microporous battery separator that is capable of maintaining hydrophilicity for a long period of time and suppressing dendrites and the associated short circuits. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view showing an outline of a battery including a microporous battery separator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The microporous separator for a battery of this embodiment will be described in detail below. One aspect of this embodiment is a microporous separator for a battery that includes a microporous substrate and a poorly water-soluble surfactant. Another aspect of this embodiment is a microporous separator for a battery that is formed by reacting a microporous substrate, a poorly water-soluble surfactant, and a radical polymerizable monomer. In this disclosure, the microporous separator for a battery is also referred to as a microporous separator.
[0013] (Microporous base material) The microporous substrate, together with a surfactant and an optional radical polymerizable monomer, constitutes a microporous separator. The microporous separator has a large number of minute pores.
[0014] The material of the microporous substrate is not particularly limited, but for example, a substrate containing polyolefin as a main component can be used. Specific examples of polyolefin include polyethylene and polypropylene.
[0015] The microporous substrate has an average pore size of, for example, 3.0 μm or less, preferably 0.5 μm or less, and more preferably 0.1 μm or less. There is no particular lower limit to the average pore size, but it is, for example, 0.01 μm or more. It is preferable that the average pore size is in the above range from the viewpoint of durability.
[0016] The microporous substrate preferably has a porosity of 30 to 60%, more preferably 40 to 50%. A porosity in this range is preferred from the viewpoint of a balance between ion conductivity and durability. The microporous substrate preferably has a thickness of 5 to 50 μm, more preferably 15 to 30 μm. A thickness in this range is preferred from the viewpoint of a balance between ion conductivity and durability.
[0017] (Poorly water-soluble surfactant) One of the features of the microporous separator of the present disclosure is the use of a poorly water-soluble surfactant, which prevents the microporous separator from dissolving in an electrolyte solution or the like when used in a battery, and allows the hydrophilicity of the microporous separator to be maintained for a long period of time.
[0018] In one preferred embodiment, the poorly water-soluble surfactant has an HLB value of 3 to 13, a solubility in water of less than 0.2 wt% at 25° C., and a solubility in at least one polar solvent selected from isopropanol, methanol, ethanol, acetonitrile, acetone, ethylene glycol, xylene, and propylene glycol monomethyl ether acetate of 10 wt% or more at 25° C. Such a surfactant is preferred from the viewpoint of uniform impregnation into the microporous separator.
[0019] The HLB of the surfactant is more preferably 5 to 12. The surfactant also more preferably has a solubility in water of less than 0.1 wt% at 25° C. There is no particular lower limit to the solubility in water, but it may be, for example, 0.01 wt% or more at 25° C.
[0020] The solubility of the surfactant in at least one polar solvent selected from isopropanol, methanol, ethanol, acetonitrile, acetone, ethylene glycol, xylene, and propylene glycol monomethyl ether acetate is more preferably 20 wt% or more. The upper limit of the solubility in polar solvents other than water is not particularly limited, but is preferably, for example, 30 wt% or less. In addition, the solubility of the surfactant in two or more polar solvents selected from isopropanol, methanol, ethanol, acetonitrile, acetone, ethylene glycol, xylene, and propylene glycol monomethyl ether acetate is preferably 10 wt% or more, more preferably 20 wt% or more.
[0021] The surfactant preferably contains at least one ethynylene group (-C≡C-), and more preferably contains an ethynylene group in the hydrophobic portion. The surfactant preferably has two or more hydrophilic portions. That is, the surfactant preferably has a hydrophobic portion containing at least one ethynylene group and two or more hydrophilic portions.
[0022] The molecular weight of the surfactant is usually 150 or more, and preferably 200 to 500. A molecular weight within the above range is preferable from the viewpoints of hydrophilic performance and durability.
[0023] As the surfactant, for example, one of the preferred embodiments is a surfactant represented by the following general formula (1): The surfactant represented by general formula (1) is preferred because the hydrophobic and hydrophilic structures are chemically stable against strong alkali and are poorly water-soluble.
[0024] [ka] (In general formula (1), m+n is 4 to 10, preferably 4 to 6.)
[0025] (Radical polymerizable monomer) In one embodiment of the microporous separator of the present disclosure, a radical polymerizable monomer is used. The radical polymerizable monomer is not particularly limited.
[0026] The radical polymerizable monomer is preferably a monomer having at least one unsaturated bond in the molecule and being soluble in a polar solvent. Examples of the radical polymerizable monomer include vinyl phosphonic acid, vinyl sulfonic acid, vinyl glycol monomer, vinyl ether monomer, and allyl ether monomer. Examples of the vinyl glycol monomer include ethylene glycol monovinyl ether.
[0027] (Polymerization initiator) The radical polymerizable monomer is usually used together with a polymerization initiator. The polymerization initiator is not particularly limited as long as it can initiate the polymerization of the radical polymerizable monomer, and examples thereof include a photoreactive polymerization initiator and a heat-reactive polymerization initiator. The polymerization initiator is not particularly limited, and may be a commercially available product.
[0028] (Microporous separator for batteries) One aspect of this embodiment is a microporous separator for a battery, which includes a microporous substrate and a poorly water-soluble surfactant, and is hereinafter also referred to as a first aspect. Another aspect of this embodiment is a microporous separator for a battery, which is obtained by reacting a microporous substrate, a poorly water-soluble surfactant, and a radical polymerizable monomer, and is hereinafter also referred to as a second aspect.
[0029] The microporous separator of the first embodiment includes the microporous substrate and a poorly water-soluble surfactant, and typically the poorly water-soluble surfactant is disposed in the pores of the microporous substrate.
[0030] The method for producing the first microporous separator is not particularly limited, but it can be obtained by preparing a solution containing the surfactant, for example, an alcohol solution such as an isopropanol solution, impregnating the microporous substrate with the solution, and drying. The impregnation and drying may be performed multiple times. The concentration of the surfactant in the solution is not particularly limited, but is, for example, 1 to 20 wt%, and preferably 3 to 10 wt%.
[0031] The microporous separator of the second embodiment is obtained by reacting a microporous substrate with a poorly water-soluble surfactant and a radically polymerizable monomer, and usually the radically polymerizable monomer is polymerized, and during the polymerization, the radically polymerizable monomer forms a bond with at least a part of the surfactant and with the microporous substrate. The microporous separator of the second embodiment is preferable because the surfactant forms a bond with the polymer derived from the radically polymerizable monomer, thereby allowing the microporous separator to maintain hydrophilicity for a long period of time.
[0032] The method for producing the second microporous separator is not particularly limited, but it can be obtained by preparing a solution containing the surfactant and the radical polymerizable monomer, for example, an alcohol solution such as an isopropanol solution, impregnating the microporous substrate with the solution, drying, and then polymerizing the radical polymerizable monomer. The impregnation and drying may be performed multiple times. The polymerization of the radical polymerizable monomer may be performed multiple times. The solution preferably contains a polymerization initiator, and the polymerization is preferably performed using light or heat depending on the type of polymerization initiator.
[0033] In the microporous separator of the second embodiment, the pore size of the microporous substrate can be reduced or some of the micropores can be blocked by polymerization of the radical polymerizable monomer, and the diffusion of ions such as zinc ions and dendrites can be effectively suppressed. The concentration of the surfactant in the solution is not particularly limited, but is, for example, 1 to 20 wt%, and preferably 3 to 10 wt%. The concentration of the radical polymerizable monomer in the solution is not particularly limited, but is, for example, 0.05 to 5 wt%, and preferably 0.1 to 3 wt%.
[0034] The microporous separator of the present embodiment is usually a component constituting a separator in a battery. The battery may further include a separator other than the microporous separator, for example, a separator made of a nonwoven fabric. The microporous separator may also be combined with another separator and used in a battery as a laminated separator. The microporous separator of the present embodiment can be used as a component of any battery, but is particularly suitable for use as a component of a battery that uses an alkaline solution, preferably a strong alkaline solution, as an electrolyte.
[0035] As an example, a schematic cross-sectional view of a battery including a microporous separator for a battery is shown in Fig. 1. In Fig. 1, a battery 100 includes a microporous separator for a battery 101, a nonwoven fabric (separator) 103, a negative electrode current collector 105, a negative electrode active material 107, a positive electrode current collector 109, a positive electrode active material 111, and an electrolyte 113. Note that a case is not shown in Fig. 1.
[0036] The microporous separator of this embodiment can maintain hydrophilicity for a long period of time, and can suppress dendrites and the associated short circuit. For this reason, the microporous separator of this embodiment is preferably used as a component of a secondary battery. The microporous separator of this embodiment is preferably used as a component of, for example, a lithium ion secondary battery or a zinc secondary battery using a zinc negative electrode. Specific examples of zinc secondary batteries include nickel-zinc secondary batteries, air-zinc secondary batteries, and silver-zinc secondary batteries. Among them, nickel-zinc secondary batteries have the advantages of excellent discharge performance and being usable at low temperatures, and have the advantage of being highly safe because they use a non-flammable alkaline electrolyte. One aspect of this embodiment is a battery having the microporous separator, preferably a secondary battery, and more preferably a zinc secondary battery. When a battery is constructed using the microporous separator of this embodiment, there is no particular limitation on other components. EXAMPLES
[0037] The present embodiment will be described below with reference to examples, but the present disclosure is not limited to these examples.
[0038] [Example 1] The negative electrode current collector used was a punched metal of oxygen-free copper (C1020) with a 3 μm-thick Sn plating layered on top.
[0039] Zinc oxide powder, metallic zinc powder, carboxymethyl cellulose, and SBR (styrene-butadiene rubber) dispersion solution were mixed by hand in a weight ratio of 95 / 5 / 1 / 3 to obtain a mixed powder. The mixed powder and pure water were mixed in a weight ratio of 1:1, placed in a container, and mixed in a Thinky revolution-rotation mixer for 15 minutes to produce a white slurry ink (negative electrode mixture).
[0040] The slurry ink was applied to the negative electrode current collector in an amount of 100 mg / cm 2 The negative electrode current collector after coating was dried at 80°C for 2 hours, and then pressed with a linear pressure of 1 ton using a roll press manufactured by Tester Giken to obtain a negative electrode having a zinc composite layer and a negative electrode current collector. A pure copper foil with a thickness of 120 μm was joined to the upper end of the negative electrode using a resistance welder to obtain a negative electrode for a zinc secondary battery.
[0041] Acetylenol E40 manufactured by Kawaken Fine Chemicals, a commercially available surfactant, was used as a stock solution, which was added dropwise to an isopropanol solvent so that the concentration of Acetylenol E40 (HLB=6, solubility in water 0.12 wt%) became 7 wt%, and the solution was stirred to dissolve the solution, yielding an isopropanol solution with a concentration of Acetylenol E40 of 7 wt%.
[0042] A suitable amount of this solution was placed in a tray, and a PP (polypropylene) porous membrane with a thickness of 20 μm, a porosity of 50%, and an average pore size of 0.03 μm was impregnated with the solution and allowed to stand for a certain period of time. The porous membrane was then removed and dried at 60° C. The PP porous membrane containing the surfactant obtained by drying was used as a hydrophilized PP microporous separator.
[0043] The negative electrode was enclosed in the hydrophilized PP microporous separator by welding the ends. The positive electrode was manufactured by welding a positive electrode terminal to an electrode made of a composite of nickel Celmet (nickel foam metal) and nickel hydroxide. The entire positive electrode was welded and wrapped in a hydrophilic nonwoven fabric 120 μm thick. The wrapped negative and positive electrodes were placed in a battery case so that one positive electrode was sandwiched between two negative electrodes, and an appropriate amount of 6M KOH solution in which zinc oxide was saturated and dissolved at room temperature was dropped as an electrolyte, after which the case was sealed and left to stand for a certain period of time to produce a single cell.
[0044] [Example 2] A hydrophilized PP microporous separator and a single cell were produced in the same manner as in Example 1, except that Acetylenol E40 was changed to Acetylenol E60 (HLB=11, solubility in water less than 0.1 wt%) manufactured by Kawaken Fine Chemicals, and the number of times the PP porous membrane was immersed in a vat containing an isopropanol solution with a concentration of Acetylenol E60 of 7 wt% was changed from once to twice.
[0045] [Example 3] A hydrophilized PP microporous separator and a unit cell were produced in the same manner as in Example 1, except that Acetylenol E40 was changed to Acetylenol E40 and Acetylenol E60 (mass ratio 1:1).
[0046] [Comparative Example 1] A hydrophilized PP microporous separator and a single cell were produced in the same manner as in Example 1, except that Acetylenol E40 was replaced with sodium lauryl sulfonate (HLB ≈ 18, solubility in water 5 wt % or more).
[0047] [Comparative Example 2] A hydrophilized PP microporous separator and a single cell were produced in the same manner as in Example 1, except that Acetylenol E40 was changed to polyoxyethylene alkyl ether (C12) (HLB=10, solubility in water of 1.0 wt% or more).
[0048] [Example 4] The negative electrode current collector used was a punched metal of oxygen-free copper (C1020) with a 3 μm-thick Sn plating layered on top.
[0049] Zinc oxide powder, metallic zinc powder, carboxymethyl cellulose, and SBR dispersion solution were mixed by hand in a weight ratio of 95 / 5 / 1 / 3 to obtain a mixed powder. The mixed powder and pure water were mixed in a weight ratio of 1:1, placed in a container, and mixed in a Thinky revolution-rotation mixer for 15 minutes to produce a white slurry ink (negative electrode mixture).
[0050] The slurry ink was applied to the negative electrode current collector in an amount of 100 mg / cm 2 The negative electrode current collector after coating was dried at 80°C for 2 hours, and then pressed with a linear pressure of 1 ton using a roll press manufactured by Tester Giken to obtain a negative electrode having a zinc composite layer and a negative electrode current collector. A pure copper foil with a thickness of 120 μm was joined to the upper end of the negative electrode using a resistance welder to obtain a negative electrode for a zinc secondary battery.
[0051] Acetylenol E40 was used as a stock solution, and was added dropwise to an isopropanol solvent so that the final concentration of Acetylenol E40 was 7 wt%, and dissolved by stirring to obtain an isopropanol solution containing Acetylenol E40. This solution was further mixed with ethylene glycol monovinyl ether (TCI), vinylphosphonic acid, and photopolymerization initiator Omnirad 1173 (IGM) to obtain concentrations of 2 wt%, 0.05 wt%, and 0.025 wt%, respectively, to obtain an isopropanol solution containing a surfactant and a monomer.
[0052] A suitable amount of this solution was placed in a resin tub, and a PP porous membrane with a thickness of 20 μm, a porosity of 50%, and an average pore size of 0.03 μm was impregnated with the solution and left to stand in the dark for a certain period of time.Then, in the dark, the porous membrane was pulled up and dried at 60°C, and then the porous membrane was left to stand on a flat glass and irradiated with UV light at room temperature for 5 minutes each side to perform a curing treatment.Then, it was washed with pure water and dried, and used as a hydrophilized PP microporous separator.
[0053] The negative electrode was enclosed in the hydrophilized PP microporous separator by welding the ends. The positive electrode was manufactured by welding a positive electrode terminal to an electrode made of a composite of nickel Celmet (nickel foam metal) and nickel hydroxide. The entire positive electrode was welded and wrapped in a hydrophilic nonwoven fabric 120 μm thick. The wrapped negative and positive electrodes were placed in a battery case so that one positive electrode was sandwiched between two negative electrodes, and an appropriate amount of 6M KOH solution in which zinc oxide was saturated and dissolved at room temperature was dropped as an electrolyte, after which the case was sealed and left to stand for a certain period of time to produce a single cell.
[0054] [Example 5] A hydrophilized PP microporous separator and a single cell were produced in the same manner as in Example 4, except that Acetylenol E40 was changed to Acetylenol E60.
[0055] [Example 6] A hydrophilized PP microporous separator and a unit cell were produced in the same manner as in Example 4, except that vinylphosphonic acid was changed to ethylene glycol monovinyl ether.
[0056] [Example 7] A hydrophilized PP microporous separator and a unit cell were produced in the same manner as in Example 4, except that vinyl sulfonic acid manufactured by TCI was used instead of vinyl phosphonic acid.
[0057] Table 1 shows the results of a contact angle (wettability) test and a permeability test for pure water and highly concentrated alkaline water (6M KOH) conducted on the hydrophilized PP microporous separators produced in the examples and comparative examples.
[0058] <Contact angle test> The contact angle was determined using a droplet contact angle camera by dropping a droplet of pure water or highly concentrated alkaline water (6M KOH) onto a hydrophilized PP microporous separator and measuring the contact angle of the droplet after 30 seconds.
[0059] <Penetration test> The permeability test was carried out using a sample cut into a 50 mm square from a hydrophilized PP microporous separator. The samples were gently placed in a tray containing pure water or highly concentrated alkaline water (6M KOH) and visually observed to see how many seconds it took for the sample to sink and how uniformly the sample became transparent. The samples that took the shortest time to sink and became uniformly transparent were evaluated as having higher permeability. The permeability of each sample was compared and qualitatively evaluated.
[0060] [Table 1]
[0061] <Cycle characteristic evaluation> Using the single cells prepared in the examples and comparative examples, the single cells were activated by a 0.2C charge / discharge cycle, assuming a state of charge / charging rate (SOC) of 100% and an initial capacity of 160mAh, and then a cycle test was performed by charging and discharging the cells under the conditions of "Cycle Test Charge / Discharge Pattern" in Table 2 until the cycle in which the discharge capacity began to decrease from the initial discharge capacity. During the cycle test, the number of cycles until a short circuit occurred (the number of cycles until the capacity began to decrease) was counted. The results are shown in Table 3.
[0062] [Table 2]
[0063] <Initial internal resistance ratio (%)> The initial internal resistance was measured for each of the single cells produced in the Examples and Comparative Examples. Specifically, the initial internal resistance was calculated from the amount of change in voltage during a certain period of discharge from a state of charge / charging rate (SOC) of 60% under a condition of a temperature of 25° C. From these results, the initial internal resistance of Example 1 was set to 100%, and the initial internal resistance ratios of the other Examples and Comparative Examples were calculated as ratios (%) to the initial internal resistance of Example 1. The results are shown in Table 3.
[0064] [Table 3]
[0065] As can be seen from Table 3, the batteries corresponding to the Examples using the microporous separator of this embodiment had low internal resistance and a higher number of cycles at which a short circuit occurred than the batteries corresponding to the Comparative Examples, and were clearly superior in battery performance.
[0066] The upper limit and / or lower limit of the numerical ranges described in this specification can be arbitrarily combined to define a preferred range. For example, the upper limit and lower limit of the numerical range can be arbitrarily combined to define a preferred range, the upper limit of the numerical range can be arbitrarily combined to define a preferred range, and the lower limit of the numerical range can be arbitrarily combined to define a preferred range.
[0067] Although the present embodiment has been described in detail above, the specific configuration is not limited to this embodiment, and even if there are design changes within the scope that does not deviate from the gist of this disclosure, they are included in this disclosure.
Claims
1. A microporous separator for a battery, comprising a microporous substrate and a poorly water-soluble surfactant.
2. 2. The microporous battery separator according to claim 1, wherein the surfactant has an HLB value of 3 to 13, a solubility of the surfactant in water at 25° C. of less than 0.2 wt %, and a solubility of the surfactant in at least one polar solvent selected from isopropanol, methanol, ethanol, acetonitrile, acetone, ethylene glycol, xylene, and propylene glycol monomethyl ether acetate at 25° C. of 10 wt % or more.
3. The microporous battery separator according to claim 1 , wherein the surfactant has a hydrophobic portion containing at least one ethynylene group and two or more hydrophilic portions.
4. A microporous separator for a battery, which is obtained by reacting a microporous substrate with a poorly water-soluble surfactant and a radically polymerizable monomer.
5. 5. The microporous battery separator according to claim 4, wherein the surfactant has an HLB value of 3 to 13, a solubility of the surfactant in water at 25° C. of less than 0.2 wt %, and a solubility of the surfactant in at least one polar solvent selected from isopropanol, methanol, ethanol, acetonitrile, acetone, ethylene glycol, xylene, and propylene glycol monomethyl ether acetate at 25° C. of 10 wt % or more.
Citation Information
Patent Citations
Aqueous resin composition for binder for heat-resistant layer of lithium ion secondary battery separator
CN115428248A
Separator for battery and battery
JP2000164193A
Separator for battery and manufacturing method of battery using same
JP2007035541A
CERAMIC BINDER COMPOSITION FOR CERAMIC-COATED SEPARATOR FOR LITHIUM-ION BATTERY, PRODUCTION METHOD AND USE THEREOF
JP2018509493A
Slurry for pattern coating
JP2019008884A