Non-aqueous electrolyte lithium ion secondary battery
The non-aqueous electrolyte lithium ion secondary battery with a polymer and solid electrolyte protective layer addresses capacity deterioration by stabilizing Li metal layer growth and preventing electrolyte decomposition, enhancing battery performance.
Patent Information
- Application Number
- JP2023084734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Non-aqueous electrolyte lithium ion secondary batteries face capacity deterioration due to the inability of the solid electrolyte layer to follow volume fluctuations of the Li metal negative electrode during charging and discharging, leading to repeated capacity loss.
A non-aqueous electrolyte lithium ion secondary battery with a Li metal negative electrode, incorporating a negative electrode protective layer composed of 30-70% solid electrolyte and 20-40% LiFSI polymer, which stabilizes Li metal layer growth and suppresses electrolyte decomposition.
The battery design effectively suppresses capacity deterioration by maintaining Li ion conductivity and preventing local electrolyte decomposition, ensuring stable Li metal layer formation and capacity retention.
Smart Images

Figure 2024168239000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to non-aqueous electrolyte lithium-ion secondary batteries. [Background technology]
[0002] In recent years, lithium ion secondary batteries using non-aqueous electrolyte solutions have been developed. For example, Patent Document 1 discloses a hybrid solid-state battery in which an LLZ solid electrolyte sheet is attached to Li metal and the positive electrode side has a liquid structure. In the technology disclosed in Patent Document 1, the growth of dendrites is suppressed by providing a hard solid electrolyte layer. Therefore, short circuits between electrodes can be suppressed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2016-517157 Summary of the Invention [Problem to be solved by the invention]
[0004] The inventors have found the following problems with non-aqueous electrolyte lithium ion secondary batteries. When a secondary battery is charged and discharged, the volume of the Li metal anode changes. On the other hand, the solid electrolyte layer has a small breaking strain and it is difficult for it to follow the volume change of the Li metal anode. Therefore, repeated charging and discharging may cause capacity degradation.
[0005] The present disclosure has been made in consideration of such problems, and has an object to provide a non-aqueous electrolyte lithium ion secondary battery capable of suppressing capacity degradation. [Means for solving the problem]
[0006] One aspect of achieving the above object is to A non-aqueous electrolyte lithium ion secondary battery having a Li metal negative electrode, a negative electrode protection layer including a polymer and a solid electrolyte; the negative electrode protective layer contains the solid electrolyte in an amount of 30 parts by volume or more and 70 parts by volume or less relative to 100 parts by volume of the negative electrode protective layer, The polymer contains 20 parts by weight or more and 40 parts by weight or less of LiFSI based on 100 parts by weight of the polymer. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a nonaqueous electrolyte lithium ion secondary battery capable of suppressing capacity degradation. [Brief description of the drawings]
[0008] [Figure 1] 1 is a cross-sectional view of a secondary battery according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. However, the present disclosure is not limited to the following embodiments. In addition, the following description and drawings are appropriately simplified for clarity of explanation.
[0010] The configuration of a nonaqueous electrolyte lithium ion secondary battery according to an embodiment will be described with reference to FIG. 1. FIG. 1 is a cross-sectional view of a nonaqueous electrolyte lithium ion secondary battery (secondary battery 1) according to an embodiment. As shown in FIG. 1, the secondary battery 1 includes a separator 10, a negative electrode protective layer 20, a Li metal layer 30, and a current collecting foil 40. The secondary battery 1 is a secondary battery containing lithium (Li) in the negative electrode. In addition to the configuration shown in FIG. 1, the secondary battery 1 includes a positive electrode and an electrolyte solution (not shown). The electrolyte solution is a nonaqueous electrolyte solution in which an electrolyte is dissolved in a nonaqueous solvent. The positive electrode of the secondary battery 1 is separated from the Li metal layer 30 by the separator 10.
[0011] The secondary battery 1 has a structure in which a plurality of layers are stacked. Specifically, as shown in FIG. 1, the secondary battery 1 has a structure in which the separator 10, the negative electrode protective layer 20, the Li metal layer 30, and the current collecting foil 40 are stacked in this order. The method of forming the secondary battery 1 is not particularly limited. The secondary battery 1 may be formed, for example, by stacking the layers that have been previously formed. In addition, at least one of the layers constituting the secondary battery 1 may be formed by depositing it on an adjacent layer. Specifically, for example, the Li metal layer 30 may be formed when the secondary battery 1 is initially charged after the separator 10, the negative electrode protective layer 20, and the current collecting foil 40 are stacked.
[0012] The separator 10 separates the positive electrode and the negative electrode of the secondary battery 1. Hereinafter, the negative electrode protective layer 20, the Li metal layer 30, and the current collecting foil 40 may be referred to as the "negative electrode of the secondary battery 1". The negative electrode of the secondary battery 1 is a Li metal negative electrode containing Li metal. The separator 10 is a film-like member made of a porous material that is permeable to lithium ions and can prevent contact between the positive electrode and the negative electrode. The separator 10 is, for example, a polypropylene-based porous film. The negative electrode is provided on one surface of the separator 10, and the positive electrode is provided on the other surface.
[0013] The negative electrode protective layer 20 includes a polymer 21 and a solid electrolyte 22. The negative electrode protective layer 20 suppresses excessive contact between the Li metal layer 30 and the electrolyte. The polymer 21 includes lithium bis(fluorosulfonyl)imide (hereinafter referred to as LiFSI). The polymer 21 includes LiFSI at a weight ratio of 20% to 40% relative to the polymer 21. When the weight ratio of LiFSI is 20% or more relative to the polymer 21, the conductivity of Li ions in the negative electrode protective layer 20 can be sufficiently maintained. Therefore, when the weight ratio of LiFSI is 20% or more relative to the polymer 21, the occurrence of reaction unevenness due to an increase in overvoltage can be suppressed, and local decomposition of the electrolyte can be suppressed. Furthermore, when the weight ratio of LiFSI is 40% or less relative to the polymer 21, the brittleness of the polymer 21 can be sufficiently reduced. Therefore, when the weight ratio of LiFSI is 40% or less relative to the polymer 21, the breakage of the negative electrode protective layer 20 due to repeated charging and discharging can be suppressed.
[0014] The negative electrode protective layer 20 contains a solid electrolyte 22 in a volume ratio of 30% to 70% with respect to the volume of the negative electrode protective layer 20. The solid electrolyte 22 is, for example, Li7La 3 ZrO 12 The solid electrolyte is an oxide-based solid electrolyte such as lithium lanthanum zirconate (LLZ). Since the negative electrode protective layer 20 contains the solid electrolyte 22, the negative electrode protective layer 20 is harder and has a higher Li concentration at the interface between the negative electrode protective layer 20 and the Li metal layer 30 than a negative electrode protective layer that does not contain the solid electrolyte 22. Therefore, in the secondary battery 1, the Li metal layer 30 is smoothly formed during the initial charge, the surface area of the Li metal layer 30 is reduced, and decomposition of the electrolyte is suppressed. LLZ is suitable for the solid electrolyte 22 from the viewpoints that it is a hard solid electrolyte that is stable in reduction and contains Li ions.
[0015] When the solid electrolyte 22 is 30% or more in volume ratio to the anode protective layer 20, the strength of the anode protective layer 20 can be sufficiently maintained, and smooth growth of the Li metal layer 30 can be promoted. The conduction of Li ions in the anode protective layer 20 is considered to be mainly performed by the polymer 21. Therefore, when the solid electrolyte 22 is 70% or less in volume ratio to the anode protective layer 20, the conductivity of the anode protective layer 20 can be sufficiently maintained. Therefore, when the solid electrolyte 22 is 70% or less in volume ratio to the anode protective layer 20, the occurrence of reaction unevenness due to an increase in overvoltage can be suppressed, and local decomposition of the electrolyte can be suppressed.
[0016] The Li metal layer 30 is a layer containing lithium metal. The Li metal layer 30 functions as a negative electrode active material of the secondary battery 1. The Li metal layer 30 may be formed, for example, when the secondary battery 1 is initially charged after the separator 10, the negative electrode protective layer 20, the current collecting foil 40, etc. are laminated. The current collecting foil 40 is a metal member that exchanges electrons with the Li metal layer 30 during charging and discharging. The current collecting foil 40 is, for example, a copper foil.
[0017] Since the secondary battery 1 has the above-mentioned configuration, the dissolution and precipitation of Li becomes stable when the secondary battery 1 is repeatedly charged and discharged, and therefore the secondary battery 1 can suppress the deterioration of the capacity.
[0018] The present disclosure is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit and scope of the present disclosure. EXAMPLES
[0019] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these examples.
[0020] <Preparation of negative electrode protective film> A predetermined amount of PVdF-HFP copolymer, LiFSI and LLZ were added to butyl butyrate and dispersed for 1 minute using an ultrasonic homogenizer. The dispersion was applied to copper foil and dried to obtain a negative electrode. The compositions of each example and each comparative example are shown in Table 1.
[0021] <Cell Preparation> LiNi x Co y Mn (1-x-y) A positive electrode was prepared by mixing O2 (x=0.5, y=0.2), a conductive additive, and a binder, applying the mixture to an aluminum foil, and pressing the mixture. Next, the negative electrode was placed opposite the positive electrode via a separator, and an electrolyte was injected to prepare a coin cell. A PP film was used as the separator. A 4MLiFSI-dissolved DME (dimethoxyethane) solution was used as the electrolyte. Next, a current of 0.4mA / cm was applied to the negative electrode. 2 The cell was activated at a current density of 0.01 and a voltage range of 3.0-4.3 V.
[0022] <Cycle test> 1mA / cm 2 A cycle test was performed for 20 cycles at a current density of 1000 V and a voltage range of 3.0-4.3 V. The discharge capacity retention rate was calculated by dividing the discharge capacity at the 20th cycle of the cycle test by the discharge capacity at the 1st cycle of the cycle test. The discharge capacity retention rate ratio was calculated by dividing the discharge capacity retention rate of each Example and Comparative Example by the discharge capacity retention rate of Comparative Example 4. The calculation results are shown in Table 1.
[0023] [Table 1]
[0024] As shown in Table 1, the coin cells of Examples 1 to 5 maintained their capacity compared to the coin cells of Comparative Examples 1 to 4. [Explanation of symbols]
[0025] 1 Secondary battery 10 Separator 20 Negative electrode protective layer 21 Polymer 22 Solid electrolyte 30 Li metal layer 40 Current collecting foil
Claims
[Claim 1] A non-aqueous electrolyte lithium ion secondary battery having a Li metal negative electrode, a negative electrode protection layer including a polymer and a solid electrolyte; the negative electrode protective layer contains the solid electrolyte in an amount of 30 parts by volume or more and 70 parts by volume or less relative to 100 parts by volume of the negative electrode protective layer, The polymer contains 20 parts by weight or more and 40 parts by weight or less of LiFSI based on 100 parts by weight of the polymer; Non-aqueous electrolyte lithium-ion secondary battery.
Citation Information
Patent Citations
Electrochemical cell with solid and liquid electrolytes
JP2016517157A