Nonaqueous electrolyte secondary battery
The non-aqueous electrolyte secondary battery design with a thick negative electrode and high lithium salt concentration addresses the capacity decrease issue by ensuring complete Li ion diffusion, maintaining charging capacity.
Patent Information
- Application Number
- JP2023084735
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Increasing the thickness of the negative electrode composite material in non-aqueous electrolyte secondary batteries leads to a decrease in cell capacity due to reduced contribution of the negative electrode material near the current collector during charging and discharging.
A non-aqueous electrolyte secondary battery design with a negative electrode composite material thickness of 135 μm or more and a non-aqueous electrolyte with a lithium salt concentration of 1.5 M or more, ensuring sufficient Li ion diffusion to the current collector.
This design suppresses the decrease in cell capacity by enabling all negative electrode active material to contribute to reactions, achieving charging capacity equivalent to the theoretical capacity.
Smart Images

Figure 2024168240000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery. [Background technology]
[0002] In recent years, secondary batteries using non-aqueous electrolytes have been developed. For example, Patent Document 1 discloses a nonaqueous electrolyte secondary battery in which the negative electrode active material is thickly packed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-027413 Summary of the Invention [Problem to be solved by the invention]
[0004] The inventors have found the following problems with non-aqueous electrolyte secondary batteries. It is expected that the energy density of a secondary battery can be increased by increasing the thickness of the negative electrode composite, i.e., by increasing the thickness of the negative electrode composite. However, when the negative electrode composite is increased in thickness, the negative electrode material near the negative electrode current collector is less likely to contribute to charging and discharging, and there is a risk that the cell capacity will be reduced compared to the theoretical capacity.
[0005] The present disclosure has been made in consideration of such problems, and has an object to provide a nonaqueous electrolyte secondary battery that is capable of suppressing a decrease in cell capacity even when the battery has a thick coating weight. [Means for solving the problem]
[0006] One embodiment for achieving the above object is a nonaqueous electrolyte secondary battery having a negative electrode mixture and a nonaqueous electrolyte, wherein the negative electrode mixture has a thickness of 135 μm or more and the nonaqueous electrolyte contains 1.5 M or more of a lithium salt. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery capable of suppressing a decrease in cell capacity even when the battery has a thick coating weight. [Brief description of the drawings]
[0008] [Figure 1] 2 is a partially enlarged cross-sectional view of a negative electrode of the nonaqueous electrolyte secondary battery according to the embodiment. FIG. [Diagram 2] FIG. 2 is a partially enlarged cross-sectional view of a negative electrode included in a nonaqueous electrolyte secondary battery having a low Li salt concentration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. However, the present disclosure is not limited to the following embodiments. In addition, the following description and drawings are appropriately simplified for clarity of explanation.
[0010] The configuration of the nonaqueous electrolyte secondary battery according to the embodiment will be described with reference to Fig. 1. Fig. 1 is a partially enlarged cross-sectional view of a negative electrode 1 included in the nonaqueous electrolyte secondary battery according to the embodiment. The nonaqueous electrolyte secondary battery according to the embodiment includes a positive electrode, a separator, a nonaqueous electrolyte, and the like (not shown) in addition to the negative electrode 1 shown in Fig. 1.
[0011] The positive electrode is a positive electrode sheet produced by applying a positive electrode paste onto a positive electrode current collector, followed by drying and rolling. The positive electrode current collector is, for example, an aluminum foil. The positive electrode paste is produced by kneading a positive electrode active material, an additive, and a solvent. The positive electrode active material is, for example, a lithium transition metal oxide or a lithium transition metal phosphate compound. The lithium transition metal oxide is, for example, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNiO2, LiCoO2, LiFeO2, LiMn2O4, LiNi 0.5 Mn 1.5The lithium transition metal phosphate compound is, for example, LiFePO4. The additive is, for example, a binder and a conductive assistant. The binder is, for example, polyvinylidene fluoride (PVdF). The conductive assistant is, for example, carbon black such as acetylene black and other carbon materials such as graphite.
[0012] The separator separates the positive electrode from the negative electrode 1. The separator is a porous sheet containing a resin such as polyethylene, polypropylene, polyester, cellulose, polyamide, etc. The separator may have a single layer structure or a laminated structure of two or more layers. For example, the separator may have a three-layer structure in which polypropylene layers are laminated on both sides of a polyethylene layer.
[0013] The non-aqueous electrolyte is an electrolyte solution in which an electrolyte is dissolved in a non-aqueous solvent. The non-aqueous solvent is, for example, an organic solvent such as carbonates, ethers, esters, nitriles, sulfones, lactones, etc., and is preferably an organic solvent of carbonates. The organic solvent of carbonates is, for example, ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, etc. The non-aqueous solvent may be used alone or in combination of two or more. The electrolyte is, for example, a lithium salt such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethane)sulfonimide (LiTFSI), etc. The electrolyte may be used alone or in combination of two or more.
[0014] The negative electrode 1 is a negative electrode sheet produced by applying a negative electrode paste onto a negative electrode current collector, followed by drying and rolling. The negative electrode current collector is, for example, copper foil. The negative electrode paste is produced by kneading a negative electrode active material, an additive, and a solvent. The additive is, for example, a binder and a thickener. The binder is, for example, styrene-butadiene rubber (SBR) and its modified products, acrylonitrile-butadiene rubber and its modified products, acrylic rubber and its modified products, fluororubber, etc., and is preferably SBR. The thickener is, for example, a cellulose-based polymer such as carboxymethyl cellulose (CMC), methyl cellulose, cellulose acetate phthalate, hydroxypropyl methyl cellulose, polyvinyl alcohol, etc., and is preferably CMC.
[0015] As shown in FIG. 1, the negative electrode 1 has a negative electrode mixture layer (negative electrode mixture) 10 and a negative electrode current collector 30. The negative electrode mixture layer 10 is a layer formed using a negative electrode mixture containing a negative electrode active material 11 and a binder 12. The negative electrode active material 11 is, for example, a natural graphite-based material. In addition to the negative electrode 1, FIG. 1 illustrates Li ions 20. The nonaqueous electrolyte secondary battery according to the embodiment is a lithium ion secondary battery using the Li ions 20 as a carrier.
[0016] Ion conduction in the electrolyte of a lithium-ion secondary battery is mainly caused by the diffusion of the electrolyte. Generally, reducing the viscosity of the electrolyte is effective for improving ion conduction. Therefore, the Li salt concentration is generally set to about 1M from the viewpoint of the correlation between the increase in the number of Li carriers and the increase in viscosity.
[0017] FIG. 2 is a partially enlarged cross-sectional view of a negative electrode 100 of a nonaqueous electrolyte secondary battery having a low Li salt concentration. The nonaqueous electrolyte secondary battery shown in FIG. 2 has a nonaqueous electrolyte with a Li salt concentration of about 1M. Therefore, the nonaqueous electrolyte secondary battery shown in FIG. 2 has a lower Li salt concentration in the nonaqueous electrolyte than the nonaqueous electrolyte secondary battery shown in FIG. 1. When the Li salt concentration in the nonaqueous electrolyte is low and the negative electrode composite layer 10 is thick, as shown in FIG. 2, it is difficult for the Li ions 20 to sufficiently diffuse to the negative electrode current collector 30. Therefore, in the negative electrode 100 shown in FIG. 2, the negative electrode active material 11 near the negative electrode current collector 30 is unlikely to contribute to the reaction during charging and discharging. Therefore, a nonaqueous electrolyte secondary battery having a low Li salt concentration in the nonaqueous electrolyte and a thick negative electrode composite layer 10 may have a lower cell capacity than the theoretical capacity.
[0018] On the other hand, when the Li salt concentration is 1.5M or more and the negative electrode composite layer 10 is thickly applied, the number of Li carriers increases compared to the case shown in FIG. 2, so that the Li ions 20 are sufficiently diffused to the negative electrode current collector 30 as shown in FIG. 1. Therefore, in the negative electrode 1 shown in FIG. 1, the negative electrode active material 11 contained in the negative electrode composite layer 10 is likely to contribute to the reaction during charging and discharging. Therefore, in a nonaqueous electrolyte secondary battery in which the Li salt concentration in the nonaqueous electrolyte is high and the negative electrode composite layer 10 is thickly applied, the decrease in cell capacity compared to the theoretical capacity is suppressed. In this way, the nonaqueous electrolyte secondary battery according to the embodiment can suppress the decrease in cell capacity even when the layer is thickly applied.
[0019] The present disclosure is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit and scope of the present disclosure. EXAMPLES
[0020] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these examples.
[0021] <Preparation of positive electrode> LiNi as the positive electrode active material 1 / 3 Co 1 / 3 Mn 1 / 3O2 was used. A slurry was prepared by mixing the positive electrode active material, conductive additive, and PVdF in a weight ratio of 87:10:3. The slurry was applied to an Al foil to obtain a positive electrode.
[0022] <Preparation of negative electrode> A natural graphite material with an average particle size of 20 μm was used as the negative electrode active material (carbon material). A styrene-butadiene copolymer (SBR) was used as the binder. Carboxymethylcellulose (CMC) was used as the thickener. The carbon material, SBR, and CMC were mixed in a weight ratio of 98:1:1 with water as a dispersion medium, and applied to a copper foil to obtain a negative electrode. The weight of the negative electrode mix was adjusted so that the capacity ratio to the capacity of the positive electrode was about 1.1.
[0023] <Checking the electrode weight, thickness and density> Each electrode was punched out using a φ12 punch. The weight and film thickness (diffusion length, thickness of composite material) of the punched φ12 electrode were measured, and the weight and thickness of the conductive foil used were subtracted to calculate the basis weight and density.
[0024] <Preparation of electrolyte> Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were used as the non-aqueous solvent. 1.0M (mol / L) LiPF6 was used as the electrolyte. 1.0wt% vinylene carbonate (VC) was used as the additive. A non-aqueous electrolyte solution was obtained by adjusting the volume ratio and molar concentration to a predetermined value.
[0025] <Measurement of electrolyte viscosity> The viscosity of the electrolyte was measured using a rotational viscometer as specified in JIS 8803. The representative value was the value at 25°C.
[0026] <Preparation of laminated battery> The above-mentioned positive electrode and negative electrode are opposed to each other via a separator to form an electrode assembly, and then the electrode assembly is charged with an electrolyte. The laminate was sealed to obtain a battery for evaluation (laminated battery). A polypropylene / polyethylene / polypropylene three-layer porous membrane with an air permeability of 300 seconds measured by the Gurley test method was used as the separator.
[0027] <Activation of laminated batteries> In the initial charge, the battery was charged in a 25° C. thermostatic chamber at a constant current of 0.1 C up to 4.10 V. Then, the battery was discharged at a constant current of 0.3 C down to 3.00 V. This was repeated three times.
[0028] <Initial characteristic evaluation> The battery was charged to 4.10 V at a current value of 0.1 C using a constant current-constant voltage method, and then charged at a constant voltage until the current value during constant voltage charging became 1 / 50 C, at which point the battery was fully charged. The battery was then discharged to 3.00 V at a current value of 0.2 C using a constant current method, and the capacity at that point was taken as the initial capacity.
[0029] The compositions and measurement results for each of the examples and comparative examples are shown in Tables 1 to 3.
[0030] [Table 1]
[0031] [Table 2]
[0032] [Table 3]
[0033] In each Example and Comparative Example, the negative electrode basis weight / density and the electrolyte viscosity were changed. As shown in Tables 1 to 3, above a certain film thickness, charging equivalent to the theoretical capacity could not be performed at a standard Li salt concentration of 1.0 M even when measured under the same conditions, and the charging capacity tended to increase with increasing Li salt concentration.
[0034] <Comparative Examples 1 to 12> When the film thickness was less than 135 μm, charging equivalent to the theoretical capacity was possible regardless of the Li salt concentration. In other words, the electrode thickness did not have a large effect on the charge capacity during the initial charge.
[0035] <Comparative Examples 13 to 18 and Examples 1 to 6> When the film thickness was greater than 135 μm, the charge capacity tended to decrease as the Li salt concentration decreased. The tendency became more pronounced as the film thickness increased, and charging equivalent to the theoretical capacity could not be performed at a Li salt concentration of 1.0 M. The charge capacity increased at a Li salt concentration of 1.5 M, preferably 2.0 M.
[0036] <Regarding Comparative Examples 13 to 14, 19 to 26, and Examples 1 to 2, and 7 to 14> When a negative electrode with a film thickness of 135 μm or more was used, the electrolyte viscosity was changed, and as a general trend, the charge capacity tended to decrease as the electrolyte viscosity increased. In Comparative Examples 21 to 26 and Examples 9 to 14, charging equivalent to the theoretical capacity was possible even with a Li salt concentration of 1.0 M only when the electrolyte viscosity was less than 2.5 mPa s (Comparative Example 26). On the other hand, when the electrolyte viscosity was 2.5 mPa s or more, the charge capacity tended to improve by increasing the Li salt concentration above 1.0 M.
[0037] <Regarding Comparative Examples 13 to 14, 27 to 32, and Examples 1 to 2, and 15 to 20> When a negative electrode having a thickness of 135 μm or more was used, the result of changing the composite density of the negative electrode showed an overall tendency that the charge capacity decreased as the composite density increased. In Comparative Examples 27 to 32 and Examples 15 to 20, 3 In the following cases, charging was possible at almost the theoretical capacity even at a Li salt concentration of 1.0M. 3 In the above cases, there was a tendency for the charge capacity to improve by increasing the Li salt concentration above 1.0M.
[0038] From the above results, it was found that when the combination of negative electrode film thickness, composite density, and electrolyte viscosity is more severe than a certain set of conditions, the charge capacity at the first charge increases with increasing Li salt concentration, and the preferred Li salt concentration is 1.5M or 2.0M.
[0039] The tendency of the conditions in the above examples is considered to affect the diffusion of Li ions as an internal reaction of the electrolyte, and the charge capacity is considered to change due to the change in the diffusion speed mp of Li ions or the change in the required diffusion distance. These factors affect the diffusion resistance of the electrolyte. On the other hand, in a battery system, when charging and discharging are performed by constant current, constant voltage (CCCV), the capacity can be input and output without depending on the internal resistance. The fact that the charge capacity changes despite the charging by CCCV in the above examples suggests that a phenomenon different from a simple increase or decrease in resistance is occurring. The assumed mechanism is that the initial SEI (Solid Electrolyte Interphase) formation is uneven locally due to insufficient Li ion diffusion in the electrolyte, and the active material part becomes isolated in the diffusion of Li ions, which is considered to reduce the charge capacity. In this state, Li ions are not supplied from the outside to the isolated part, so the reaction needs to be completed by the nearby Li ions, and if the Li salt concentration is low, there is a lack of Li ions and sufficient charging cannot be performed. On the other hand, in a system with a high Li-ion concentration as shown in this disclosure, it is believed that charging equivalent to the theoretical capacity can be performed because the necessary amount of charge can be secured even without an external supply of Li ions. [Explanation of symbols]
[0040] 1,100 negative electrode, 10 negative electrode composite layer (negative electrode composite), 11 negative electrode active material, 12 binder, 20 Li ion, 30 negative electrode current collector
Claims
[Claim 1] A non-aqueous electrolyte secondary battery having a negative electrode mixture and a non-aqueous electrolyte, The thickness of the negative electrode mixture is 135 μm or more, The non-aqueous electrolyte contains 1.5M or more of a lithium salt. Nonaqueous electrolyte secondary battery.
Citation Information
Patent Citations
Power storage device
JP2022027413A