Method for producing pet resin
The method of dissolving PET resin in a solvent and using activated carbon to adsorb impurities effectively reduces impurities and costs, enhancing PET resin quality and color tone.
Patent Information
- Application Number
- JP2023084737
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Chemical recycling of PET resin requires high energy and costs, while mechanical recycling struggles with insufficient impurity removal, leading to degraded color tone and increased costs.
A method involving dissolving PET resin in a good solvent, using activated carbon to adsorb impurities, and precipitating PET resin particles with a specific solvent mixture to achieve low impurity content.
Produces PET resin with low impurity content and improved color tone at reduced costs, without the need for depolymerization and repolymerization steps.
Smart Images

Figure 2024168242000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing PET resin. [Background technology]
[0002] There are two methods for regenerating PET resin from used PET bottles: chemical recycling and mechanical recycling. PET stands for polyethylene terephthalate. Chemical recycling involves depolymerizing used PET bottles into raw materials or intermediate raw materials for PET resin, purifying them, and repolymerizing them. Chemical recycling is disclosed in Patent Document 1.
[0003] In mechanical recycling, dirt and foreign matter are removed from the surface of used PET bottles, and contaminants accumulated inside the PET resin are diffused and removed by exposing them to high temperatures. Mechanical recycling is disclosed in Patent Documents 2 to 4. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 3715812 [Patent Document 2] Special Publication No. 2002-536203 [Patent Document 3] Special Publication No. 2005-532192 [Patent Document 4] Special Publication No. 2007-531642 Summary of the Invention [Problem to be solved by the invention]
[0005] Chemical recycling involves the process of depolymerizing used PET bottles into raw materials or intermediate raw materials for PET resin, refining them, and then repolymerizing them. Therefore, a large amount of energy is required to carry out chemical recycling, and the running costs are high. In addition, chemical recycling requires large-scale decomposition and polymerization equipment, so the initial costs are high. With mechanical recycling, it is difficult to sufficiently remove impurities contained in PET resin. If the impurities contained in PET resin cannot be sufficiently removed, the color tone of the PET resin will deteriorate.
[0006] In one aspect of the present disclosure, it is preferable to provide a method for producing a PET resin that can produce a PET resin with a low impurity content at low cost. [Means for solving the problem]
[0007] One aspect of the present disclosure is a method for producing a PET resin, comprising dissolving used PET resin in a good solvent to produce a PET solution, contacting the PET solution with activated carbon, separating substances having a size of 50 μm or more, including the activated carbon, from the PET solution, adding a poor solvent to the PET solution to precipitate PET resin particles, and recovering the precipitated PET resin particles.
[0008] b of the manufactured PET resin * The value is less than or equal to 1.5. * The value is CIE1976L * a * b * b in color space * The good solvents account for 25% by mass or more of the specific good solvents consisting of aprotic polar solvents, and the activated carbon has a total light transmittance of 80% or more for a test liquid measured by the following measurement method.
[0009] Measurement method of total light transmittance: 300 mg of the activated carbon and 30 mL of N-methyl-2-pyrrolidone (hereinafter referred to as NMP) are mixed to prepare a test liquid. Next, the test liquid is heated and stirred at 165°C for 15 minutes. Next, the activated carbon is removed from the test liquid by filtration. Next, the total light transmittance of the filtrate is measured using a glass cell with an optical path length of 10 mm.
[0010] According to a method for producing a PET resin that is one aspect of the present disclosure, a PET resin having a low impurity content can be produced at low cost. [Brief description of the drawings]
[0011] [Figure 1] 1 is a flowchart showing a method for producing a PET resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Exemplary embodiments of the present disclosure will now be described with reference to the drawings. First Embodiment 1. PET resin manufacturing method The method for producing PET resin is, for example, a method in which each step shown in Fig. 1 is carried out in sequence. In S1 of Fig. 1, used PET resin is converted into PET flakes by the following method.
[0013] First, used PET resin is prepared. The used PET resin may be, for example, a used PET bottle, a PET food tray, a PET blister pack, a PET food divider, or the like. Used PET resin is crushed into small pieces of about 8 mm square. Next, the small pieces are separated by gravity to remove foreign matter, dehydrated, dried, removed by an optical sorter, and colored flakes are removed. PET flakes are obtained through the above process.
[0014] The quality of PET flakes is determined according to the quality measurement and management items described in JIS K 7390-1:2015 "Plastics - Materials recycled from used polyethylene terephthalate (PET) bottles - Part 1: Designation system and fundamentals of specification notation" and JIS K 7390-2:2015 "Plastics - Materials recycled from used polyethylene terephthalate (PET) bottles - Part 2: Methods for preparing test pieces and determining characteristics."
[0015] The quality of the PET flakes preferably meets the "Quality Standard Values for PET Bottle Recycled Products (Example)" created by the Japan Container and Packaging Recycling Association. If the quality of the PET flakes is within the range of this standard value, the amount of impurities contained in the PET flakes will be reduced, and the amount of impurities contained in the PET resin produced by the production method of the present disclosure can be reduced.
[0016] The PET flakes may be either a homopolymer of polyethylene terephthalate or a copolyester in which a small proportion of a copolymerization component is copolymerized, such as isophthalic acid, diethylene glycol, 1,4-cyclohexanedimethanol, or 2,6-naphthalenedicarboxylic acid.
[0017] The moisture content of the PET flakes is preferably 1.0% or less, and more preferably 0.6% or less. When the moisture content of the PET flakes is 1.0% or less, hydrolysis of the PET resin can be suppressed when the PET flakes are dissolved in a good solvent.
[0018] In S2 of Figure 1, a process is performed in which PET flakes are dissolved in a good solvent to produce a PET solution (hereinafter referred to as the dissolving process). Note that PET flakes may contain impurities. These impurities include impurities other than PET resin dispersed or dissolved inside the PET flakes, coating materials and contaminants present on the surface of the PET flakes, impurities trapped between the PET flakes, etc. The purpose of steps S2 to S5 is to remove these impurities.
[0019] A good solvent is an organic solvent that dissolves PET resin. At least 25% by mass of the good solvents are specific good solvents. The specific good solvents are aprotic polar solvents. Examples of aprotic polar solvents include good solvents that are composed of molecules that do not have an alcoholic hydroxyl group or an ester bond.
[0020] When 25% by mass or more of the good solvents are the specific good solvents, the molecular weight of the PET resin is unlikely to decrease when the PET resin is dissolved in the good solvent. Of the good solvents, it is preferable that 50% by mass or more is the specific good solvent, more preferably 75% by mass or more is the specific good solvent, and particularly preferably that all of the good solvents are the specific good solvent. The more the amount of the specific good solvent contained in the good solvent, the less likely the molecular weight of the PET resin is to be reduced. In addition, theoretically, non-polar solvents are also less likely to reduce the molecular weight of the PET resin.
[0021] When PET resin is dissolved in a protic polar solvent, the molecular weight of the PET resin decreases due to an intermolecular reaction between the solvent and the PET resin. Examples of protic polar solvents include solvents made of molecules with alcoholic hydroxyl groups or amino groups containing hydrogen atoms. Non-polar solvents have difficulty dissolving PET by themselves.
[0022] The solubility of PET flakes in a good solvent is preferably 100 g / L or more. A PET flake solubility of 100 g / L or more means that when 100 g of PET flakes are put into 1 L of a good solvent and stirred at 165°C for 1 hour, the PET flakes are completely dissolved. When the PET flake solubility is 100 g / L or more, a smaller amount of good solvent can be used.
[0023] The specific good solvent is preferably at least one selected from the group consisting of N-alkyl-2-pyrrolidone, N-alkenyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. Examples of N-alkyl-2-pyrrolidone include NMP, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone, and Nn-octyl-2-pyrrolidone. Examples of N-alkenyl-2-pyrrolidone include N-vinyl-2-pyrrolidone. As the specific good solvent, NMP is particularly preferred.
[0024] The good solvent may include a good solvent that is not any of N-alkyl-2-pyrrolidone, N-alkenyl-2-pyrrolidone, and 2,5-dialkylimidazolidinone, so long as the solubility of the PET flakes is in the range of 100 g / L or more.
[0025] The concentration of the PET resin in the PET solution is preferably 40 g / L or more and 400 g / L or less, more preferably 40 g / L or more and 250 g / L or less, and particularly preferably 40 g / L or more and 150 g / L or less.
[0026] When the concentration of the PET resin in the PET solution is within the above range, the viscosity of the PET solution can be suppressed, making it easier to filter out impurities from the PET solution. The temperature of the good solvent in the dissolving step (hereinafter referred to as the dissolving temperature) and the temperature of the PET solution in the dissolving step are not particularly limited. The dissolving temperature and the temperature of the PET solution in the dissolving step are preferably 100° C. or higher and 190° C. or lower, and more preferably 120° C. or higher and 170° C. or lower.
[0027] When the dissolving temperature and the temperature of the PET solution in the dissolving process are 100° C. or higher, the PET flakes can be dissolved in a short time with a good solvent. When the dissolving temperature and the temperature of the PET solution in the dissolving step are 190° C. or lower, thermal decomposition of the PET resin and the good solvent can be suppressed, and hydrolysis of the PET resin can be suppressed.
[0028] When the good solvent is NMP, the dissolving temperature and the temperature of the PET solution in the dissolving step are preferably 140°C or higher and 190°C or lower, and more preferably 160°C or higher and 180°C or lower.
[0029] The dissolving step can be carried out, for example, in a dissolving tank. The dissolving tank is equipped, for example, with an inlet for a good solvent and PET flakes, a stirrer, a temperature control device, and the like. In the dissolving step, for example, PET flakes are put into a preheated good solvent. In the dissolving step, for example, PET flakes are put into a good solvent before heating, and then the good solvent is heated.
[0030] In the steps after S2, the temperature of the PET solution in which all of the PET flakes have been dissolved (hereinafter referred to as the post-processing temperature) is preferably a temperature that is ΔT lower than the dissolution temperature and within a temperature range in which the PET resin does not precipitate.
[0031] ΔT is 20° C. or more and 30° C. or less. When the temperature during the post-processing is lower than the dissolving temperature by ΔT, the thermal decomposition of the PET resin and the good solvent and the hydrolysis of the PET resin can be suppressed in the steps after S2. When the good solvent is NMP, the temperature during the post-processing is preferably 110° C. or more and 170° C. or less, and more preferably 120° C. or more and 150° C. or less.
[0032] In S3 of Fig. 1, a first filtration is performed. The first filtration is a process for filtering out and removing coarse insoluble impurities contained in the PET solution. The PET solution contains soluble impurities that are dissolved in the good solvent, and insoluble impurities that are insoluble in the good solvent. Insoluble impurities include coarse insoluble impurities and minute insoluble impurities. Coarse insoluble impurities include solid foreign matter with a size of 50 μm or more. Examples of solid foreign matter include metal, glass, sand, and carbonized PET resin.
[0033] In the first filtration, large insoluble impurities are filtered out and removed from the PET solution. Small insoluble impurities are removed in the second filtration in S5, which will be described later. By removing the large insoluble impurities in the S3 step, clogging of the filter in the second filtration in S5 can be suppressed.
[0034] In the first filtration, the temperature of the PET solution is preferably low within a temperature range in which the PET resin does not precipitate. When the good solvent is NMP, the temperature of the PET solution in the first filtration is preferably 110° C. or higher and 170° C. or lower, more preferably 120° C. or higher and 150° C. or lower.
[0035] The mesh size of the filter used in the first filtration is preferably 5 μm or more and 100 μm or less, and more preferably 10 μm or more and 50 μm or less. When the filter aperture is within the above range, coarse insoluble impurities with a size of 100 μm or more can be removed without impairing the workability of the first filtration. When the filter aperture is 5 μm or more, clogging of the filter can be suppressed. In addition, when the filter aperture is 5 μm or more, high pressure is not required during the first filtration, and the time required for the first filtration can be shortened.
[0036] Before the first filtration, the PET solution may be filtered using a filter with larger mesh size, which can prevent clogging of the filter used in the first filtration. In S4 in Figure 1, the PET solution is brought into contact with activated carbon. At the end of step S3, the PET solution contains soluble impurities that are soluble in good solvents. The soluble impurities include yellowing substances generated during the PET bottle molding and recycling processes, colorants and additives intentionally added to PET bottles, and dirt adhering to the PET flakes. Examples of dirt adhering to the PET flakes include ink, glue, sugar, and pigments.
[0037] When the PET solution is brought into contact with the activated carbon, the soluble impurities in the PET solution are adsorbed by the activated carbon. The method of bringing the PET solution into contact with the activated carbon is not particularly limited. The method of bringing the PET solution into contact with the activated carbon may be a batch method or a continuous method. Examples of the method of bringing the PET solution into contact with the activated carbon include a method of putting the PET solution and the activated carbon in a container and stirring them, and a method of passing the PET solution through a column filled with activated carbon.
[0038] The amount of activated carbon used is preferably adjusted appropriately depending on the amount of soluble impurities contained in the PET solution. The amount (g) of activated carbon used per 1 L of PET solution is preferably 4 g / L or more and 40 g / L or less, more preferably 4 g / L or more and 25 g / L or less, and particularly preferably 4 g / L or more and 15 g / L or less.
[0039] When the amount of activated carbon used is 4g / L or more, the effect of activated carbon adsorbing soluble impurities in the PET solution is higher. Even if the amount of activated carbon used exceeds 40g / L, the effect of activated carbon adsorbing soluble impurities in the PET solution is not improved as much as when the amount of activated carbon used is 40g / L.
[0040] The temperature of the PET solution when it is brought into contact with the activated carbon is preferably low within a temperature range where the PET resin does not precipitate. When the good solvent contained in the PET solution is NMP, the temperature of the PET solution when it is brought into contact with the activated carbon is preferably 110°C or higher and 170°C or lower, more preferably 120°C or higher and 150°C or lower.
[0041] The time for contacting the PET solution with the activated carbon is preferably 5 minutes or more and 60 minutes or less, and more preferably 10 minutes or more and 30 minutes or less. When the time for contacting the PET solution with the activated carbon is within the above range, the thermal decomposition of the PET resin and the good solvent and the hydrolysis of the PET resin can be suppressed. When the time for contacting the PET solution with the activated carbon is 5 minutes or more, the activated carbon has a higher effect of adsorbing the soluble impurities in the PET solution.
[0042] After contacting the PET solution with the activated carbon, the PET solution and the activated carbon can be separated by a known solid-liquid separation method such as centrifugation or filter filtration, and the activated carbon can be removed from the PET solution. Hot filtration is preferable as the filter filtration. When the filter filtration is hot filtration, it is possible to suppress precipitation of the PET resin from the PET solution.
[0043] The filter has an opening of, for example, 50 μm or less. When the filter has an opening of 50 μm or less, substances having a size of 50 μm or more, including activated carbon, can be separated from the PET solution. Substances having a size of 50 μm or more are substances separated by a filter having an opening of 50 μm or less. Substances having a size of 50 μm or more include, for example, activated carbon and fine particles generated from activated carbon. The fine particles are generated when a part of the activated carbon breaks down. The objects separated from the PET solution may include substances having a size larger than the opening of the filter and smaller than 50 μm.
[0044] The temperature of the PET solution when separating the PET solution from the activated carbon is preferably low within a temperature range where the PET resin does not precipitate. When the good solvent contained in the PET solution is NMP, the temperature of the PET solution when separating the PET solution from the activated carbon is preferably 110° C. or higher and 170° C. or lower, more preferably 120° C. or higher and 150° C. or lower. The step of separating the PET solution from the activated carbon may be performed in S5.
[0045] The activated carbon used in step S4 is one that has a total light transmittance of 80% or more when measured by the following method using that activated carbon. The total light transmittance is a value measured before the activated carbon is used in step S4.
[0046] Measurement method: 300 mg of activated carbon and 30 mL of NMP are mixed to prepare a test solution. The test solution is then heated and stirred at 165°C for 15 minutes. The activated carbon is then removed from the test solution by filtration. The total light transmittance of the filtrate is then measured using a glass cell with an optical path length of 10 mm. The device used to measure the total light transmittance is a haze meter NDH8000 manufactured by Nippon Denshoku Industries Co., Ltd.
[0047] The total light transmittance measured by the above method using the activated carbon used in step S4 is preferably 85% or more, and more preferably 90% or more. Commercially available activated carbon contains tar components generated during the manufacturing process and minute activated carbon particles less than 50 μm in size. If a PET solution is brought into contact with commercially available activated carbon without removing the tar components, the tar components contained in the activated carbon will dissolve into the PET solution and contaminate the PET solution. The activated carbon used in the step S4 is preferably one that contains a small amount of tar components. The activated carbon used in the manufacturing method for PET resin of the present disclosure contains a small amount of tar components, so that dissolution of the tar components into the PET solution can be suppressed.
[0048] It is preferable to remove at least a part of the tar components contained in the activated carbon before contacting the PET solution with the activated carbon. The activated carbon used in the method for producing PET resin of the present disclosure can be produced, for example, by removing at least a part of the tar components contained in commercially available activated carbon. As a method for removing the tar components contained in the activated carbon, a method of extracting the tar components from the activated carbon using a tar extraction solvent (hereinafter referred to as a tar component extraction method) can be mentioned.
[0049] The tar extraction solvent is not particularly limited. The tar extraction solvent is preferably one that can extract a large amount of the tar components contained in the activated carbon. Examples of the tar extraction solvent that can extract a large amount of the tar components contained in the activated carbon include tar extraction solvents with a Hildebrand solubility parameter (SP value) in the range of 9 to 13.
[0050] Examples of tar extraction solvents having an SP value within the range of 9 to 13 include N,N-dimethylformamide (DMF) having an SP value of 12.1, N,N-dimethylacetamide (DMAc) having an SP value of 10.8, tetrahydrofuran (THF) having an SP value of 9.1, dimethylsulfoxide (DMSO) having an SP value of 12.1, and NMP having an SP value of 11.3. NMP is particularly preferred as the tar extraction solvent.
[0051] It is preferable that at least a part of the tar extraction solvent is a good solvent used in step S2, and it is more preferable that the entire tar extraction solvent is a good solvent used in step S2. When at least a part of the tar extraction solvent is a good solvent used in step S2, the same solvent can be used as both the good solvent in step S2 and the tar extraction solvent.
[0052] The tar component extraction method is not particularly limited. The tar component extraction method may be a batch type or a continuous type. Examples of the tar component extraction method include a method in which a tar extraction solvent and activated carbon are placed in a container and stirred, and a method in which a tar extraction solvent is passed through a column filled with activated carbon.
[0053] When the tar component extraction method is a batch type, it is preferable to perform the tar component extraction method multiple times. The total amount of the tar extraction solvent used is not particularly limited. The total amount of the tar extraction solvent used is preferably 5 parts by mass or more and 50 parts by mass or less, more preferably 10 parts by mass or more and 30 parts by mass or less, relative to 1 part by mass of activated carbon.
[0054] When the tar component extraction method is performed only once, the total amount of tar extraction solvent used is the amount used in one tar component extraction method. When the tar component extraction method is performed multiple times, the total amount of tar extraction solvent used is the sum of the amounts used in each tar component extraction method.
[0055] When the total amount of the tar extraction solvent used is 5 parts by mass or more per 1 part by mass of activated carbon, the effect of extracting the tar components contained in the activated carbon is higher. Even if the total amount of the tar extraction solvent used exceeds 50 parts by mass per 1 part by mass of activated carbon, it is difficult to improve the effect of extracting the tar components contained in the activated carbon compared to when the total amount of the tar extraction solvent used is 50 parts by mass per 1 part by mass of activated carbon.
[0056] The temperatures of the tar extraction solvent and activated carbon when carrying out the tar component extraction method are not particularly limited. The temperatures of the tar extraction solvent and activated carbon are preferably 60°C or higher and 180°C or lower. When the temperatures of the tar extraction solvent and activated carbon are 60°C or higher, the effect of extracting the tar components contained in the activated carbon is higher. When the temperatures of the tar extraction solvent and activated carbon are 180°C or lower, the boiling point of the tar extraction solvent only needs to be 180°C or lower, so there are more options for the tar extraction solvent. In addition, when the temperatures of the tar extraction solvent and activated carbon are 180°C or lower, thermal decomposition of the tar extraction solvent can be suppressed.
[0057] When the tar extraction solvent is NMP, the temperature of the tar extraction solvent when carrying out the tar component extraction method is preferably 140°C or higher and 170°C or lower. In the tar component extraction method, the contact time between the activated carbon and the tar extraction solvent is not particularly limited. The contact time between the activated carbon and the tar extraction solvent is preferably 0.5 hours or more and 5 hours or less, and more preferably 0.5 hours or more and 2 hours or less.
[0058] When the contact time between the activated carbon and the tar extraction solvent is 0.5 hours or more, the effect of extracting the tar components contained in the activated carbon is higher. Even if the contact time between the activated carbon and the tar extraction solvent exceeds 5 hours, the effect of extracting the tar components contained in the activated carbon is less likely to be improved compared to when the contact time between the activated carbon and the tar extraction solvent is 5 hours.
[0059] When the tar component extraction method is carried out, the activated carbon is usually miscible with the tar extraction solvent. After carrying out the tar component extraction method, it is preferable to sequentially carry out rinsing with a low-boiling point rinse solvent having a boiling point of less than 100° C. and drying.
[0060] When rinsing is performed, the tar extraction solvent is removed from the activated carbon, and the tar components adhering to the surface of the activated carbon are washed off. When rinsing is performed, the total light transmittance measured by the above method using activated carbon can be increased even if the amount of tar extraction solvent used or the number of times the tar component extraction method is performed is reduced.
[0061] Preferred low boiling point rinsing solvents include, for example, methanol, ethanol, 2-propanol, acetone, etc. When the tar extraction solvent and the good solvent used in step S2 are the same solvent, the rinsing step may be omitted.
[0062] The shape and size of the activated carbon before carrying out the tar component extraction method (hereinafter referred to as pre-extraction activated carbon) are not particularly limited. The diameter of the pre-extraction activated carbon is preferably 0.3 mm or more and 3 mm or less. When the diameter of the pre-extraction activated carbon is 0.3 mm or more and 3 mm or less, it is easy to separate the activated carbon from the PET solution after carrying out the tar component extraction method.
[0063] The specific surface area of the activated carbon before extraction is 500m 2 / g or more, 2500m 2 / g or less, and 2 / g or more, 2000m 2 When the specific surface area of the activated carbon before extraction is within the above range, the activated carbon can adsorb a larger amount of soluble impurities.
[0064] The activated carbon before extraction preferably contains many micropores with a pore diameter of 2 nm or less. When the activated carbon before extraction contains many micropores with a pore diameter of 2 nm or less, the activated carbon can efficiently adsorb soluble impurities with a smaller molecular weight than PET. Examples of soluble impurities with a smaller molecular weight include colorants and substances that cause yellowing. The definition of "containing many micropores with a pore diameter of 2 nm or less" is that the abundance ratio of micropores is the highest among micropores with a pore diameter of 2 nm or less, mesopores with a pore diameter of 2 nm to 50 nm, and macropores with a pore diameter of 50 nm or more.
[0065] The activated carbon is preferably one that is unlikely to generate dust when it comes into contact with a tar extraction solvent or a good solvent and in the steps after S4. In addition, the activated carbon is preferably one that allows tar components to be quickly removed by carrying out the tar component extraction method.
[0066] The main raw materials used for activated carbon include, for example, coconut shells, sawdust, and coal. Among these, coconut shells are preferred. Activated carbon made from coconut shells has many micropores among micropores, mesopores with a pore diameter of 2 to 50 μm, and macropores with a pore diameter of 50 μm or more, and is excellent at adsorbing small molecules. The activated carbon is preferably in the form of granules with a diameter of 0.3 mm or more, and more preferably in the form of granules with a diameter of 0.3 mm or more and 3 mm or less. Crushing is preferred as a method for producing activated carbon.
[0067] Compared with wood-based activated carbon, coconut shell-based granular activated carbon is less likely to lose its shape when in contact with a good solvent and is less likely to produce fine dust. Compared with coal-based activated carbon, coconut shell-based granular activated carbon allows tar components to be removed more quickly when subjected to a tar component extraction method. Compared with coal-based activated carbon, coconut shell-based granular activated carbon is less likely to produce fine dust. Coconut shell-based activated carbon is activated carbon made from coconut shells. Wood-based activated carbon is activated carbon made from wood materials. Coal-based activated carbon is activated carbon made from coal.
[0068] The activated carbon is preferably not in the form of powder. The definition of powder is that the diameter of the activated carbon is less than 0.3 mm. The difference between the powder and the above-mentioned granular form is the size of the activated carbon. The activated carbon is preferably not in the form of granules. The definition of granular is that the diameter of the activated carbon is increased by extrusion molding or compression molding of powdered or fibrous activated carbon. The difference between the granular form and the above-mentioned granular form is the presence or absence of extrusion molding or compression molding. The activated carbon is preferably not in the form of granulated carbon. The definition of granulated carbon is that powdered activated carbon or crushed activated carbon is molded by compression molding or the like.
[0069] Powdered activated carbon is not preferred because the particles are small and it is difficult to separate it from the PET solution by physical filtration or the like, and it is also difficult to recycle it. Granular activated carbon and granulated carbon are not preferred because the shape of the activated carbon is easily distorted when it comes into contact with a good solvent, and a lot of fine dust is easily generated.
[0070] Wood-based activated carbon is generally produced from sawdust generated during lumber processing, and is therefore often in powder or granular form. Granular activated carbon is not preferred because it is prone to losing its shape when in contact with a good solvent, and is prone to generating a lot of fine dust. Powdered activated carbon is not preferred because the particles are small and it is difficult to separate from the PET solution by physical filtration or the like. Coal-based activated carbon is not preferred because it is prone to losing its shape and is prone to generating a lot of fine dust. In addition, coal-based activated carbon is not preferred because the tar components continue to dissolve even when the tar component extraction method is repeated, making it difficult to obtain a high degree of cleaning.
[0071] In S5 of FIG. 1, a second filtration is performed. In the step S3, coarse insoluble impurities are removed from the PET solution. In the step S4, soluble impurities are removed from the PET solution. At the end of the step S4, the PET solution contains minute insoluble impurities and soluble impurities that were not adsorbed by the activated carbon.
[0072] Examples of minute insoluble impurities include carbonized PET resin, additives intentionally added to PET bottles, coating materials applied to the surfaces of PET bottles, etc. Also, examples of minute insoluble impurities include fine particles generated from the activated carbon in the step S4. The second filtration is a step in which minute insoluble impurities contained in the PET solution and soluble impurities not adsorbed by the activated carbon are filtered out and removed from the PET solution.
[0073] The second filtration is, for example, hot filtration. The mesh size of the filter used in the second filtration is preferably 0.5 μm or more and 50 μm or less, and more preferably 1 μm or more and 45 μm or less.
[0074] When the filter aperture is within the above range, insoluble impurities whose size is larger than the filter aperture and is 50 μm or less can be removed. Insoluble impurities whose size is 50 μm or less were difficult to remove using conventional mechanical recycling methods. When the filter aperture is 50 μm or less, substances whose size is 50 μm or more can be separated and removed from the PET solution.
[0075] If the filter has an opening of 0.5 μm or more, high pressure is not required during the second filtration, and the time required for the second filtration can be shortened. Before the second filtration, the PET solution may be filtered using a filter with a larger opening. In this case, clogging of the filter used in the second filtration can be suppressed.
[0076] In the second filtration, the temperature of the PET solution is preferably low within a temperature range in which the PET resin does not precipitate. When the good solvent is NMP, the temperature of the PET solution in the second filtration is preferably 110°C or higher and 170°C or lower, more preferably 120°C or higher and 150°C or lower.
[0077] During the period from the end of the second filtration to the end of step S6, the temperature of the PET solution is preferably low within a temperature range in which the PET resin does not precipitate. When the good solvent is NMP, during the period from the end of the second filtration to the end of step S6, the temperature of the PET solution is preferably 110°C or higher and 170°C or lower, more preferably 120°C or higher and 150°C or lower. In S6 of Figure 1, a poor solvent is added to the PET solution to precipitate PET resin particles (hereinafter referred to as PET particles). A poor solvent is a solvent that has low solubility for PET resin. The solubility of a poor solvent for PET resin is lower than that of a good solvent for PET resin.
[0078] By adding a poor solvent to a PET solution, the PET solution becomes a mixed solvent of a good solvent and a poor solvent. A mixed solvent of a good solvent and a poor solvent has a lower solubility for PET resin than a good solvent. Therefore, when a poor solvent is added to a PET solution, PET particles precipitate from the PET solution.
[0079] The poor solvent is preferably miscible with the good solvent at a temperature of 100°C or higher. The boiling point of the poor solvent is preferably T1°C or higher and T2°C or lower. T1 is a temperature 10°C lower than the temperature of the PET solution immediately before the poor solvent is added. T2 is a temperature 20°C higher than the temperature of the PET solution immediately before the poor solvent is added. When the good solvent contained in the PET solution is NMP, the boiling point of the poor solvent is preferably 110°C or higher and 150°C or lower.
[0080] When the boiling point of the poor solvent is T1°C or higher, the poor solvent added to the PET solution can be prevented from boiling violently, and the good solvent and the poor solvent can be easily mixed. When the boiling point of the poor solvent is T2°C or lower, the poor solvent can be easily removed from the precipitated PET particles by heating.
[0081] The poor solvent is preferably a non-polar solvent. When the poor solvent is a non-polar solvent, it is easy to precipitate fine PET particles from the PET solution. In addition, when the poor solvent is a non-polar solvent, it is possible to prevent the precipitated PET particles from fusing together or aggregating to form large lumps.
[0082] When the specific good solvent is NMP, the poor solvent is preferably a saturated hydrocarbon, more preferably at least one saturated hydrocarbon selected from the group consisting of n-octane, n-nonane, n-decane, n-undecane, and n-dodecane having a carbon number of 8 to 12, and particularly preferably n-octane. Since n-octane has a low boiling point, it can be easily removed by reducing pressure, heating, etc.
[0083] The temperature of the PET solution immediately before the addition of the poor solvent is preferably low within a temperature range in which the PET resin does not precipitate, and is preferably equal to or lower than the boiling point of the poor solvent immediately before the addition of the poor solvent.
[0084] When the good solvent is NMP, the temperature of the PET solution immediately before the addition of the poor solvent is preferably 110° C. or more and 170° C. or less, and more preferably 120° C. or more and 150° C. or less.
[0085] When the good solvent is NMP and the poor solvent is n-octane, the temperature of the PET solution immediately before the addition of the poor solvent is preferably 110°C or higher and 170°C or lower, and more preferably 120°C or higher and 140°C or lower.
[0086] A method of adding a poor solvent is preferably a method of adding the poor solvent little by little over time while stirring the PET solution. A method of adding a poor solvent is preferably a method of adding the same volume of the poor solvent as the good solvent in the PET solution over a period of 1 minute or more and 30 minutes or less, more preferably a method of adding the poor solvent over a period of 5 minutes or more and 30 minutes or less. An example of a method of adding a poor solvent is a method of dropping the poor solvent.
[0087] When the poor solvent is added in small amounts, only the PET resin tends to selectively precipitate in particulate form within a limited range of the mixing ratio of the good solvent and the poor solvent. When only the PET resin selectively precipitates in particulate form, PET particles with few impurities can be recovered.
[0088] The amount of the poor solvent added is preferably an amount sufficient to precipitate almost the entire amount of the PET resin in the PET solution, and is usually 1 to 3 times the volume of the good solvent contained in the PET solution.
[0089] After the entire amount of the poor solvent is added, the solid-liquid mixture consisting of the PET particles, the good solvent, and the poor solvent is cooled to a temperature suitable for filtering and recovering the PET particles. The temperature of the solid-liquid mixture after cooling is preferably 50° C. or more and 110° C. or less, more preferably 80° C. or more and 100° C. or less.
[0090] When the temperature of the solid-liquid mixture after cooling is 50°C or higher, the mixed solvent of the good solvent and the poor solvent is unlikely to separate into two layers, making it easy to filter and recover the PET particles from the solid-liquid mixture. Also, when the temperature of the solid-liquid mixture after cooling is 50°C or higher, soluble impurities are unlikely to precipitate in the mixed solvent. When the temperature of the solid-liquid mixture after cooling is 110°C or lower, adhesion between the PET particles recovered by filtering can be suppressed.
[0091] The particle size of the PET particles precipitated from the PET solution is preferably 100 μm or more and 1500 μm or less, and more preferably 100 μm or more and 1000 μm or less. When the particle size of the PET particles is 100 μm or more, it is easy to filter and collect only the PET particles, and insoluble impurities can be prevented from being mixed into the PET particles. When the particle size of the PET particles is 1500 μm or less, insoluble impurities are unlikely to be incorporated into the PET particles, and good and poor solvents in the PET particles can be easily removed. The particle size of the PET particles is measured using the 2D measurement function of a Hirox digital microscope KH-8700.
[0092] In S7 of FIG. 1, the PET particles are recovered by filtering the solid-liquid mixture consisting of the precipitated PET particles, the good solvent, and the poor solvent through a filter. The filtration method is not particularly limited. The filtration method may be any of gravity filtration, pressure filtration, and vacuum filtration. The mesh size of the filter used for filtration is preferably 5 μm or more and 100 μm or less, more preferably 10 μm or more and 50 μm or less.
[0093] When the filter aperture is within the above range, it is easy to separate and remove minute insoluble impurities and the mixed solvent present in the mixed solvent of the good solvent and the poor solvent from the PET particles. When the filter aperture is 5 μm or more, it is possible to prevent the insoluble impurities from being filtered out together with the PET particles. In addition, when the filter aperture is 5 μm or more, it is not necessary to apply high pressure when filtering the solid-liquid mixture, and the time required for filtering can be shortened. When the filter aperture is 100 μm or less, it is possible to prevent the PET particles from passing through the filter.
[0094] The PET particles collected in step S7 contain a good solvent and a poor solvent. If the good solvent is a high-boiling point solvent with high polarity, it is difficult to remove all of the good solvent from the PET particles even if the PET particles are heated and dried under reduced pressure or in a clean gas stream. It is not preferable for the good solvent to remain in the produced PET resin.
[0095] Therefore, in S8 of FIG. 1, a step of extracting the good solvent and the poor solvent from the recovered PET particles using an extraction solvent (hereinafter referred to as a solvent extraction step) is carried out. The extraction solvent is an organic solvent that is miscible with both good and poor solvents and does not easily dissolve the PET resin. The extraction solvent is preferably a solvent that can swell the PET particles when contacted with the PET particles at a temperature equal to or lower than the boiling point of the extraction solvent.
[0096] Examples of extraction solvents capable of swelling PET particles when contacted with the PET particles at a temperature below the boiling point of the extraction solvent include solvents having an SP value, which is preferably 8.5 or more and 13.0 or less, more preferably 9.0 or more and 9.8 or less.
[0097] When the SP value of the extraction solvent is within the above range, the PET particles tend to swell when brought into contact with the extraction solvent, and the effect of extracting the good solvent and the poor solvent from the PET particles is further enhanced. The boiling point of the extraction solvent is preferably 50° C. or higher and 100° C. or lower. When the boiling point of the extraction solvent is 50° C. or higher, the PET particles tend to swell when the extraction solvent is brought into contact with the PET particles at the boiling point of the extraction solvent, and the effect of extracting the good solvent and the poor solvent from the PET particles is further enhanced. When the boiling point of the extraction solvent is 100° C. or lower, the extraction solvent can be easily removed from the PET particles by heating and drying.
[0098] As the extraction solvent having an SP value and a boiling point within the above ranges, at least one selected from the group consisting of tetrahydrofuran having an SP value of 9.2 and a boiling point of 66°C, methyl acetate having an SP value of 9.6 and a boiling point of 57°C, ethyl acetate having an SP value of 9.1 and a boiling point of 77°C, and acetone having an SP value of 9.9 and a boiling point of 57°C is preferred, with tetrahydrofuran being particularly preferred.
[0099] The temperature of the extraction solvent and the PET particles in the solvent extraction process is not particularly limited. The temperature of the extraction solvent and the PET particles in the solvent extraction process is preferably close to the boiling point of the extraction solvent. When the temperature of the extraction solvent and the PET particles in the solvent extraction process is close to the boiling point of the extraction solvent, the effect of extracting the good solvent and the poor solvent from the PET particles is higher.
[0100] The solvent extraction step is preferably a step of performing extraction while refluxing the extraction solvent at the boiling point of the extraction solvent. When the extraction solvent is tetrahydrofuran, the solvent extraction step is preferably a step of performing extraction while refluxing tetrahydrofuran at 66°C, which is the boiling point of tetrahydrofuran.
[0101] The solvent extraction process may be a batch process or a continuous process, and examples of the solvent extraction process include a process in which PET particles and an extraction solvent are placed in a container and stirred, and a process in which an extraction solvent is passed through a column packed with PET particles.
[0102] When the solvent extraction process is a batch type, it is preferable to perform extraction multiple times. The number of extractions is preferably 2 to 3 times. The amount of extraction solvent used is not particularly limited. The amount of extraction solvent used is preferably 2.5 parts by mass or more and 25 parts by mass or less, and more preferably 5 parts by mass or more and 15 parts by mass or less, per 1 part by mass of PET particles. When the amount of extraction solvent used is 2.5 parts by mass or more, the effect of extracting the good solvent and the poor solvent is even higher. Even if the amount of extraction solvent used exceeds 25 parts by mass, it is difficult to improve the effect of extracting the good solvent and the poor solvent compared to when the amount of extraction solvent used is 25 parts by mass. The extraction solvent contains, for example, about 0.4% by mass of a stabilizer. In this embodiment, since the amount of the stabilizer is small, the step of removing the stabilizer is omitted, but when scaling up, it is preferable to remove the stabilizer. An example of an extraction solvent containing a stabilizer is THF. An example of a stabilizer is BHT. BHT is poorly soluble in water and easily soluble in alcohol and oils and fats. The boiling point of BHT is 265°C. The solvent used may contain a stabilizer. The solvent used is defined as a good solvent, a poor solvent, or an extraction solvent used in the manufacturing method of the PET resin of the present disclosure. When the stabilizer cannot be removed from the solvent used by reducing pressure or heating, it is preferable to carry out a step of removing the stabilizer from the solvent used as appropriate. For example, when THF containing BHT as an antioxidant is used in the solvent removal step (S8), it can be washed with alcohol or hexane, which is a low-boiling point solvent that is miscible with THF and has a boiling point of less than 100°C.
[0103] After the solvent extraction step, the PET particles are washed with a solvent that is easier to remove than the extraction solvent, and the PET particles are dried. As a solvent that is easier to remove than the extraction solvent, a low-boiling point solvent that is miscible with the extraction solvent and has a boiling point of less than 100°C is preferable, and ethanol and acetone are more preferable. When the extraction solvent is a low-boiling point solvent, the step of washing with a solvent that is easier to remove than the extraction solvent may be omitted.
[0104] At the end of the step S8, there may still be a trace amount of volatile impurities remaining inside the PET particles. The volatile impurities include good solvents, poor solvents, and extraction solvents. In S9 of FIG. 1, the volatile impurities are removed from the PET particles by the following method.
[0105] PET particles are put into a decontamination device. When the PET particles are exposed to a reduced pressure and high temperature environment in the decontamination device, the volatile impurities accumulated inside the PET particles are diffused and removed. The pressure inside the decontamination device is preferably 10 kPa or less, more preferably 5 kPa or less, and particularly preferably 1 kPa or less. When the pressure inside the decontamination device is 10 kPa or less, the effect of removing volatile impurities is even higher.
[0106] The temperature inside the decontamination equipment is preferably 110°C or higher and 190°C or lower, and more preferably 130°C or higher and 170°C or lower. When the temperature inside the decontamination equipment is 110°C or higher, the effect of removing volatile impurities is higher. When the temperature inside the decontamination equipment is 190°C or lower, the solvent inside the PET particles is less likely to undergo thermal decomposition, and the PET particles are less likely to discolor.
[0107] The time for which the PET particles are exposed to a reduced pressure, high temperature environment in the decontamination equipment is preferably 6 hours or more and 36 hours or less, and more preferably 12 hours or more and 36 hours or less. When the time is 6 hours or more, the effect of removing volatile impurities is higher. When the time is more than 36 hours, the removal of volatile impurities is less advanced than when the time is 36 hours.
[0108] In S10 in Fig. 1, a pelletizing process is performed. The pelletizing process is a process in which PET particles are made into pellets of PET resin (hereinafter referred to as PET pellets) by extrusion molding. The pellets have a shape suitable for molding.
[0109] The pelletizing process can remove trace amounts of volatile impurities remaining inside the PET particles. Volatile impurities include good solvents, poor solvents, and extraction solvents. In the pelletizing process, an extruder is used. The extruder is, for example, an extruder that is widely used in the manufacturing process of virgin PET resin pellets or recycled PET resin pellets. The extruder is equipped with one or more vacuum passages. Acetaldehyde, cyclic oligomers, and solvents used in the previous steps that are generated during melting of the PET resin are sucked into the vacuum passage and removed.
[0110] The extruder preferably has at least two screws to efficiently remove contaminants, gases derived from impurities, or solvent vapor. The overall length of the extruder screw is preferably short to prevent thermal degradation due to retention of PET resin. It is preferable to perform a crystallization treatment on the PET pellets after extrusion molding. When crystallization treatment is performed, it is possible to prevent the PET pellets from fusing due to heat during drying of moisture before molding processing.
[0111] In S11 in Figure 1, the PET pellets after the crystallization process are subjected to a solid-state polymerization process. In the solid-state polymerization process, the molecular weight of the PET resin is restored to a level suitable for PET bottle use. In addition, the solid-state polymerization process can remove acetaldehyde and cyclic oligomers generated during the extrusion molding of the PET pellets, the solvents used in the previous processes, and other volatile impurities.
[0112] In the solid-state polymerization step, a solid-state polymerization apparatus generally used in the manufacturing process of virgin PET resin pellets or recycled PET resin can be used. A specific method of solid-state polymerization is, for example, a method in which the PET pellets after the crystallization treatment are heated to a temperature of 130°C or higher and 190°C or lower under an inert gas atmosphere or under vacuum from which oxygen has been removed. The time of solid-state polymerization can be adjusted according to the target intrinsic viscosity IV of the PET resin.
[0113] When the PET resin is used for PET bottles, the intrinsic viscosity IV is 0.70 to 0.85. The intrinsic viscosity IV varies depending on the use of the PET bottle. The solid-state polymerization time is preferably 12 hours or more and 36 hours or less. When the solid-state polymerization time is 36 hours or less, the productivity of the PET resin is high.
[0114] The produced PET resin can be used to produce PET bottles, fibers, films, sheets, etc. When the raw material used PET resin is used PET bottles and the produced PET resin is used to produce PET bottles, recycling from PET bottles to PET bottles can be carried out.
[0115] b of the manufactured PET resin * The value is less than 1.5. CIE1976L * a * b * The method for measuring the color tone in the color space is the method described in the Examples below. In the PET resin purification process, the heating temperature is set so that PET does not precipitate, and the heating time is shortened, so that the color tone in the color space can be measured. * In addition, if the activated carbon used is not coal-based activated carbon, the increase in the value of b * In addition, if the activated carbon used is coconut shell activated carbon, b * The value tends to be small.
[0116] 2. Benefits of PET resin manufacturing method (1A) In the method for producing a PET resin according to the present disclosure, a PET solution is brought into contact with activated carbon. The activated carbon adsorbs soluble impurities contained in the PET solution. Therefore, according to the method for producing a PET resin according to the present disclosure, a PET resin having a low content of impurities can be produced. In particular, according to the method for producing a PET resin according to the present disclosure, a PET resin having a low content of soluble impurities can be produced. A PET resin having a low content of impurities has a good color tone.
[0117] In addition, the method for producing a PET resin according to the present disclosure does not require depolymerization and repolymerization steps, unlike chemical recycling, and therefore can produce a PET resin with a low impurity content at low cost.
[0118] (1B) The activated carbon used in the manufacturing method of the PET resin of the present disclosure has a low content of tar components. Therefore, when activated carbon is used, it is possible to suppress the elution of tar components into the PET solution. As a result, it is possible to manufacture a PET resin with a lower content of impurities. (1C) In the method for producing a PET resin according to the present disclosure, for example, the tar components contained in the activated carbon can be removed before the PET solution is brought into contact with the activated carbon. In this case, the tar components can be further prevented from dissolving into the PET solution. As a result, a PET resin with a lower impurity content can be produced.
[0119] <Example> 1. Preparation of model specimen (1-1) Preparation of triple extrusion PET A commercially available virgin resin for PET bottles (CB-602A_K manufactured by Far East New Century) was melted at 280°C and extruded to produce pellets. A twin-screw extruder PCM-30 manufactured by Ikegai was used for extrusion. Next, the pellets were cut using a pelletizer to obtain multiple small pieces. The width of each small piece was 3 mm, and the mass of each small piece was about 15 mg. Next, the small pieces were placed in a solid-state polymerization device and dried at 120°C for 4 hours. Next, the temperature was raised to 170°C and crystallized for 2 hours. Next, solid-state polymerization was carried out at 205°C for 14 hours. By the above process, a single-extruded PET was obtained. The process for obtaining the single-extruded PET was repeated a total of three times to obtain a triple-extruded PET. The triple-extruded PET was pulverized using a frozen pulverizer to obtain fine particles with a particle size of about 600 μm or less.
[0120] (1-2) Creation of green PET A commercially available carbonated bottle was prepared. This carbonated bottle was Perrier 500mL. The carbonated bottle consisted of three layers. The outermost layer of the three layers was cut to a width of about 5 mm. The cut outermost layer was crushed using a freezing crusher to obtain green PET.
[0121] (1-3) Creation of simulated burnt wood Virgin PET resin (CB-602A_K) was placed on a metal plate and heated from below with a burner. Heating was continued until the PET resin stopped generating bubbles due to decomposition and the PET resin was completely blackened. Next, the blackened PET resin was crushed at room temperature until it became fine particles with a particle size of about 100 μm, obtaining simulated burnt material.
[0122] (1-4) Preparation of model samples A model sample was obtained by mixing 95 parts by weight of triple-extruded PET, 4.8 parts by weight of green PET, and 0.2 parts by weight of simulated burnt material. The model sample corresponds to used PET resin.
[0123] 2. Example 1 (2-1) Preparation of washed activated carbon (a) 30 mL of special grade NMP was added to 3.0 g of activated carbon to prepare a solid-liquid mixture. NMP corresponds to the tar extraction solvent. The activated carbon was coconut shell-based granular activated carbon CW830A manufactured by Futamura Chemical. The average pore diameter of the coconut shell-based granular activated carbon CW830A was 1.67 nm. The particle diameter of the coconut shell-based granular activated carbon CW830A was 0.50 to 2.36 mm. The average particle diameter of the coconut shell-based granular activated carbon CW830A was 1.35 mm. The coconut shell-based granular activated carbon CW830A was crushed carbon.
[0124] Next, the solid-liquid mixture was heated to 165°C and stirred with a stirrer for 60 minutes. At this time, the tar components were removed from the activated carbon. Next, the solid-liquid mixture was suction filtered to recover the activated carbon. (b) The recovered activated carbon was subjected to the above-mentioned operation (a) once again. Note that the treatments (a) and (b) correspond to the tar component extraction method, respectively. In Example 1, the tar component extraction method was performed twice.
[0125] (c) After (a) and (b), the activated carbon was washed with 10 mL of industrial alcohol having the following composition: Ethanol: 86.90% i-Propanol: 4.90% n-Propanol: 8.20% The activated carbon was then air-dried at room temperature for 15 hours. Through the above steps, washed activated carbon was obtained.
[0126] (2-2) PET resin production (i) A solid-liquid mixture was prepared by adding 3.0 g of the model sample, 30 mL of NMP, and 300 mg of washed activated carbon to a 50 mL Erlenmeyer flask. The solid-liquid mixture contained a PET solution in which PET resin was dissolved in NMP, and washed activated carbon. NMP corresponds to a specific good solvent consisting of an aprotic polar solvent. In the solid-liquid mixture, the PET solution and the washed activated carbon were in contact with each other.
[0127] (ii) The solid-liquid mixture was then heated and stirred at a temperature of 165° C. for 15 minutes. (iii) Next, the solid-liquid mixture was subjected to hot filtration using a filtering device and a screen mesh. Prior to hot filtration, the filtering device was preheated to 130° C. The mesh size of the screen mesh was 1.0 μm.
[0128] The washed activated carbon-containing material was separated and removed from the solid-liquid mixture by hot filtration. The washed activated carbon-containing material had a size of 1.0 μm or more. The washed activated carbon-containing material also contained material with a size of 50 μm or more. The washed activated carbon-containing material contained NMP insoluble matter in addition to the washed activated carbon. NMP insoluble matter is a material that does not dissolve in NMP. The NMP insoluble matter included fine particles generated by the disintegration of part of the washed activated carbon.
[0129] As a result of hot filtration, the PET solution and the washed activated carbon were separated. The PET solution after hot filtration gelled when left to cool. The gel was transformed into a solution by heating to 165°C. (iv) Next, the PET solution was kept at 130°C and 60 mL of n-octane was added dropwise to the PET solution over a period of 5 minutes while stirring. n-octane corresponds to a poor solvent. At this time, PET particles slowly precipitated from the PET solution. As a result, a solid-liquid mixture containing PET particles, NMP, and n-octane was obtained. Next, the solid-liquid mixture was cooled to about 80°C while continuing to stir the solid-liquid mixture.
[0130] (v) Next, the PET particles were collected from the solid-liquid mixture using a screen mesh with an opening of 10 μm. (vi) Next, a process was carried out to extract NMP and n-octane from the collected PET particles using an extraction solvent. Specifically, PET particles and 100 mL of THF were placed in a 100 mL Erlenmeyer flask and heated to reflux. THF corresponds to the extraction solvent. At this time, the NMP and n-octane contained in the PET particles were replaced with THF. Next, the solid-liquid mixture was filtered through a screen mesh with an opening of 10 μm.
[0131] (vii) Next, the above process (vi) was repeated once more. (viii) Next, the PET particles were vacuum dried at 63°C for 15 hours. Through the above steps, PET particles made of PET resin were produced. When the produced PET particles were visually observed, the particle size of the PET particles was uniform. The production conditions of Example 1, and Examples 2 to 6 and Comparative Examples 1 to 8 described later are shown in Table 1.
[0132] [Table 1]
[0133] The "tar component extraction method" in Table 1 refers to the processes (a) and (b) in the "(2-1) Preparation of washed activated carbon" above. The "tar extraction solvent" in Table 1 refers to the solvent used in the processes (a) and (b) in the "(2-1) Preparation of washed activated carbon" above. The "number of extractions" in Table 1 refers to the total number of times that the process (a) was performed and the number of times that the process (b) was performed in the "(2-1) Preparation of washed activated carbon" above.
[0134] The "good solvent" in Table 1 is the solvent added to the model sample in (i) above. The "filter opening" in Table 1 is the opening of the screen mesh used in (iii) above. The "poor solvent" in Table 1 is the solvent added dropwise to the PET solution in (iv) above. The "extraction solvent" in Table 1 is the extraction solvent used in (vi) and (vii) above.
[0135] 3. Examples 2 to 6 and Comparative Examples 1 to 8 PET resins of Examples 2 to 6 and Comparative Examples 1 to 8 were produced basically in the same manner as in Example 1. However, in Example 2, ethanol was used as the extraction solvent, and in Example 3, acetone was used as the extraction solvent.
[0136] In Example 4, the opening of the screen mesh used in (iii) was 10 μm. In Example 4, substances having a size of 10 μm or more, including activated carbon, were separated from the PET solution in (iii). The substances having a size of 10 μm or more also contained substances having a size of 50 μm or more.
[0137] In Example 5, the opening of the screen mesh used in (iii) was 25 μm. In Example 5, substances having a size of 25 μm or more, including activated carbon, were separated from the PET solution in (iii). The substances having a size of 25 μm or more also contained substances having a size of 50 μm or more.
[0138] In Example 6, the opening of the screen mesh used in (iii) was 45 μm. In Example 6, substances having a size of 45 μm or more, including activated carbon, were separated from the PET solution in (iii). The substances having a size of 45 μm or more also contained substances having a size of 50 μm or more.
[0139] In Comparative Example 1, no activated carbon was used. In Comparative Example 2, the activated carbon used was SG840, a granular wood-based activated carbon manufactured by Futamura Chemical. In Comparative Example 3, the activated carbon used was GM830A, a granular coal-based activated carbon manufactured by Futamura Chemical.
[0140] In Comparative Example 4, the activated carbon used was GL830A, a coal-based granular activated carbon manufactured by Futamura Chemical Co., Ltd. In Comparative Example 5, the good solvent used was benzyl alcohol. In Comparative Example 6, the good solvent used was DMP. In Comparative Example 7, the activated carbon was not subjected to the tar component extraction method. In Comparative Example 8, the opening of the screen mesh used in the above step (iii) was 100 μm. In Comparative Example 8, after the above step (iii), substances having a size of 50 μm or more remained in the solid-liquid mixture.
[0141] 4. Evaluation Method for Each Example and Comparative Example The PET resins produced in each Example and Comparative Example were evaluated in the following items (4-1) to (4-4). In addition, the activated carbons used in the production of the PET resins, except for Comparative Example 1, were evaluated in the following item (4-5). The evaluation results are shown in Table 1 or Table 2 below.
[0142] [Table 2]
[0143] (4-1) PET resin recovery rate X The PET resin recovery rate X (%) was calculated by the following formula (1). Formula (1) X = (A / B) x 100 In formula (1), A is the mass of the produced PET resin. B is the mass of the triple-extruded PET contained in the model sample. The PET resin recovery rate X is shown in Table 2.
[0144] (4-2) Intrinsic viscosity IV 0.25 g of the produced PET resin was heated and dissolved in a mixed solution at 130°C to prepare a resin-containing solution. The mixed solution was a solution in which phenol and 1,1,2,2-tetrachloroethane were mixed in a volume ratio of 6:4. Next, the resin-containing solution was cooled to room temperature and kept at 30°C in a thermostatic water bath. The flow time of the resin-containing solution was measured using an automatic viscosity measuring device (SS-500-L1) manufactured by Shibata Scientific Instruments Manufacturing Co., Ltd. The intrinsic viscosity IV was calculated based on the measured flow time. The intrinsic viscosity IV of the produced PET resin is shown in Table 2.
[0145] The intrinsic viscosity IV of the triple-extruded PET contained in the model sample was also calculated in the same manner. The intrinsic viscosity IV of the triple-extruded PET contained in the model sample was 0.704 in each of the Examples and Comparative Examples. The IV retention was also calculated. The IV retention is the ratio (%) of the intrinsic viscosity IV of the produced PET resin to the intrinsic viscosity IV of the triple-extruded PET contained in the model sample. The IV retention is shown in Table 2.
[0146] (4-3) Color tone of PET resin 0.7 g of the produced PET resin was placed in a PVC ring with an inner diameter of 35 mm and a thickness of 3.5 mm. The PET resin was then pressed under a pressure of 200 kg / cm. 2 The plate was pressed at 100° C. to create a plate with a thickness of about 2.3 mm. * a * b * The color tone in the color space was measured using a HunterLab ColorQuestXE. The color tone of the manufactured PET resin is shown in Table 2.
[0147] The color tone of the triple-extruded PET contained in the model sample was also calculated in the same manner. * / a * / b * ) was (89.92 / -3.50 / 4.39) in each of the Examples and Comparative Examples.
[0148] (4-4) Number of black foreign objects A light board was used to confirm that there was no foreign matter or dust on the two PTFE sheets. Next, 100 mg of the produced PET resin was sandwiched between the two PTFE sheets. Next, the two PTFE sheets were pressed at 280°C for 5 seconds using a manual hydraulic heating press, and then quenched. At this time, a PET sheet was formed between the two PTFE sheets. The thickness of the PET sheet was about 100 μm.
[0149] Next, the PET sheet was observed with a Hirox microscope KH-8700, and counted automatically at 7 mm 2 The number of black foreign bodies per sample and the diameter of each of the black foreign bodies were measured. The magnification during observation was 100 times. The settings of the automatic counting function were as follows:
[0150] Filter settings: None Binarization settings: Target is brightness, gradation density is 106~255 Conditions: Smoothness is 9, Maximum area is 100%, Minimum area is 6, Total area 7mm of black foreign matter in the manufactured PET resin2 The number of black foreign matter particles per unit area is shown in Table 2. In Table 2, the number of black foreign matter particles with a diameter of 1.0 μm or more and less than 10 μm is shown separately from the number of black foreign matter particles with a diameter of 10 μm or more and 50 μm or less.
[0151] The number of black foreign objects was also calculated for the triple-extruded PET contained in the model sample. The number of black foreign objects having a diameter of 1.0 μm or more and less than 10 μm for the triple-extruded PET contained in the model sample was 70 for each of the examples and comparative examples. The number of black foreign objects having a diameter of 10 μm or more and less than 50 μm for the triple-extruded PET contained in the model sample was 17 for each of the examples and comparative examples.
[0152] (4-5) Total light transmittance Activated carbon to be measured for total light transmittance was prepared. The activated carbon to be measured for total light transmittance was in a state immediately before being used for the production of PET resin. That is, in each of the Examples and Comparative Examples 2 to 6 and 8, the activated carbon to be measured for total light transmittance was activated carbon to which the tar component extraction method had been applied and which had not yet been used for the production of PET resin. In Comparative Example 7, the activated carbon to be measured for total light transmittance was activated carbon to which the tar component extraction method had not been applied and which had not yet been used for the production of PET resin.
[0153] A test solution was prepared by mixing 300 mg of activated carbon to be measured for total light transmittance with 30 mL of NMP. The test solution was then heated and stirred at 165°C for 15 minutes. The activated carbon was then removed from the test solution by filtration. PTFE filter paper with a retention particle size of 1.0 mm was used for filtration. The filtrate was then transferred to a glass cell with an optical path length of 10 mm, and the total light transmittance was measured using a haze meter NDH8000 manufactured by Nippon Denshoku Industries Co., Ltd. The total light transmittance is shown in Table 1.
[0154] 5. Evaluation Results of Each Example and Comparative Example The PET resin produced in each Example had a good color tone. The reason for the good color tone is that the content of impurities in the PET resin is low. In each Example, the PET resin recovery rate X was high. In each Example, the intrinsic viscosity IV and IV retention rate of the produced PET resin were high. The reason for the high intrinsic viscosity IV and IV retention rate is that the molecular weight of the PET resin is difficult to decrease. In each Example, the number of black foreign matter contained in the produced PET resin was small. In Examples 1 to 3, the number of black foreign matter contained in the produced PET resin was particularly small.
[0155] The PET resins produced in each Comparative Example had poor color tone. In Comparative Examples 5 and 6, the molecular weight of the PET resin was reduced, and most of the PET particles were precipitated in a bulk state. Therefore, in Comparative Examples 5 and 6, it was not possible to measure the color tone of the produced PET particles. In Comparative Examples 5 and 6, the intrinsic viscosity IV and IV retention of the produced PET resins were low. In Comparative Examples 2, 3, and 8, the number of black foreign matters contained in the produced PET resin was large. In Comparative Example 4, b * The value was 2.47. That is, the color tone of the PET resin produced in Comparative Example 4 was poor.
[0156] <Other embodiments> Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments and can be implemented in various modified forms. (1) Some of the steps shown in Fig. 1 may be omitted. For example, some or all of steps S3 and S8 to S11 may be omitted. Furthermore, steps other than S1 to S11 may be added. (2) Steps S2 to S4 in FIG. 1 may be as follows. PET flakes and activated carbon are simultaneously put into a good solvent. The PET flakes are then dissolved in the good solvent to produce a PET solution. When the PET solution is produced, activated carbon is already present in the PET solution. After the PET solution is produced, the PET solution comes into contact with the activated carbon.
[0157] (3) Steps S2 to S4 in FIG. 1 may be as follows: Activated carbon is put into a good solvent. Next, PET flakes are put into the good solvent. After that, the PET flakes are dissolved in the good solvent to produce a PET solution. When the PET solution is produced, activated carbon is already present in the PET solution. After the PET solution is produced, the PET solution comes into contact with the activated carbon.
[0158] (4) The function of one component in each of the above embodiments may be shared by multiple components, or the functions of multiple components may be performed by one component. Also, part of the configuration of each of the above embodiments may be omitted. Also, at least part of the configuration of each of the above embodiments may be added to or substituted for the configuration of another of the above embodiments.
[0159] (5) In addition to the above-described method for producing PET resin, the present disclosure can be realized in various forms, such as a method for recycling PET resin and a method for removing impurities from PET resin.
[0160] [Technical idea disclosed in this specification] [Item 1] Used PET resin is dissolved in a good solvent to produce a PET solution. contacting the PET solution with activated carbon; Separating materials having a size of 50 μm or more, including the activated carbon, from the PET solution; A poor solvent is added to the PET solution to precipitate PET resin particles; The precipitated PET resin particles are collected, 25% by mass or more of the good solvents are specific good solvents consisting of aprotic polar solvents, The activated carbon has a total light transmittance of 80% or more as measured by the following measurement method for a test liquid; b of the manufactured PET resin * The value is less than or equal to 1.5, How PET resin is manufactured. Measurement method of total light transmittance: 300 mg of the activated carbon and 30 mL of N-methyl-2-pyrrolidone are mixed to prepare a test liquid. Next, the test liquid is heated and stirred at 165°C for 15 minutes. Next, the activated carbon is removed from the test liquid by filtration. Next, the total light transmittance of the filtrate is measured using a glass cell with an optical path length of 10 mm. [Item 2] A method for producing the PET resin according to item 1, Prior to contacting the PET solution with the activated carbon, removing at least a portion of the tar components contained in the activated carbon; How PET resin is manufactured. [Item 3] Item 1 or 2, a method for producing a PET resin, The specific good solvent is at least one selected from the group consisting of N-alkyl-2-pyrrolidone, N-alkenyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. How PET resin is manufactured. [Item 4] Item 3. A method for producing a PET resin according to item 3, The specific good solvent is N-methyl-2-pyrrolidone. How PET resin is manufactured. [Item 5] A method for producing a PET resin according to any one of items 1 to 4, After contacting the PET solution with the activated carbon, the PET solution is filtered through a filter having an opening of 0.5 μm or more and 50 μm or less. How PET resin is manufactured. [Item 6] A method for producing a PET resin according to any one of items 1 to 5, Extracting the good solvent and the poor solvent from the recovered PET resin particles using an extraction solvent. How PET resin is manufactured. [Item 7] Item 6. A method for producing a PET resin according to item 6, The extraction solvent is at least one selected from the group consisting of tetrahydrofuran, acetone, and ethanol; How PET resin is manufactured. [Item 8] A method for producing a PET resin according to any one of items 1 to 7, The activated carbon mainly has micropores with a pore diameter of 2 nm or less. How PET resin is manufactured. [Item 9] A method for producing a PET resin according to any one of items 1 to 8, The activated carbon is a granular activated carbon having a diameter of 0.3 mm or more and 3 mm or less. How PET resin is manufactured. [Item 10] A method for producing a PET resin according to any one of items 1 to 9, The activated carbon is crushed carbon. How PET resin is manufactured. [Item 11] A method for producing a PET resin according to any one of items 1 to 10, The particle diameter of the precipitated PET resin particles is 100 μm or more and 1000 μm or less, The precipitated PET resin particles are collected by filtration using a filter having an opening of 5 μm or more and 100 μm or less. How PET resin is manufactured. [Item 12] A method for producing a PET resin according to any one of items 1 to 11, The method of adding the poor solvent to the PET solution is dropwise. How PET resin is manufactured.
Claims
1. Dissolving used PET resin in a good solvent to produce a PET solution; contacting the PET solution with activated carbon; Separating materials having a size of 50 μm or more, including the activated carbon, from the PET solution; A poor solvent is added to the PET solution to precipitate PET resin particles; Collecting the precipitated PET resin particles; 25% by mass or more of the good solvent is a specific good solvent composed of an aprotic polar solvent, The activated carbon has a total light transmittance of 80% or more for a test liquid measured by the following measurement method, The produced PET resin b * The value is 1.5 or less. Manufacturing method of PET resin. Measurement method of total light transmittance: 300 mg of the activated carbon and 30 mL of N-methyl-2-pyrrolidone are mixed to prepare a test liquid. Next, the test liquid is heated and stirred at 165° C. for 15 minutes. Next, the activated carbon is removed from the test liquid by filtration. Next, the total light transmittance of the filtrate is measured using a glass cell having an optical path length of 10 mm.
2. A method for producing the PET resin according to claim 1, Prior to contacting the PET solution with the activated carbon, removing at least a portion of the tar components contained in the activated carbon; Manufacturing method of PET resin.
3. A method for producing the PET resin according to claim 1 or 2, The specific good solvent is at least one selected from the group consisting of N-alkyl-2-pyrrolidone, N-alkenyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. Manufacturing method of PET resin.
4. A method for producing the PET resin according to claim 3, The specific good solvent is N-methyl-2-pyrrolidone. Manufacturing method of PET resin.
5. A method for producing the PET resin according to claim 1 or 2, After contacting the PET solution with the activated carbon, the PET solution is filtered through a filter having an opening of 0.5 μm or more and 50 μm or less. Manufacturing method of PET resin.
6. A method for producing the PET resin according to claim 1 or 2, Extracting the good solvent and the poor solvent from the recovered PET resin particles using an extraction solvent. Manufacturing method of PET resin.
7. A method for producing the PET resin according to claim 6, The extraction solvent is at least one selected from the group consisting of tetrahydrofuran, acetone, and ethanol; Manufacturing method of PET resin.
8. A method for producing the PET resin according to claim 1 or 2, The activated carbon mainly has micropores with a pore diameter of 2 nm or less. Manufacturing method of PET resin.
9. A method for producing the PET resin according to claim 1 or 2, The activated carbon is a granular activated carbon having a diameter of 0.3 mm or more and 3 mm or less. Manufacturing method of PET resin.
10. A method for producing the PET resin according to claim 1 or 2, The activated carbon is crushed carbon. Manufacturing method of PET resin.
11. A method for producing the PET resin according to claim 1 or 2, The particle diameter of the precipitated PET resin particles is 100 μm or more and 1000 μm or less, The precipitated PET resin particles are collected by filtration using a filter having an opening of 5 μm or more and 100 μm or less. Manufacturing method of PET resin.
12. A method for producing the PET resin according to claim 1 or 2, The method of adding the poor solvent to the PET solution is dropwise. Manufacturing method of PET resin.
Citation Information
Patent Citations
Process for recovering waste polyethylene glycol terephthalate (PET) material
CN102911396A
PET waste recovery and regeneration method and polyester material prepared by PET waste recovery and regeneration method
CN114015112A
Recycling of polyester-containing polymer waste and apparatus therefor
JP1999060795A
Titanium oxide / Carbon composite particle and its manufacturing method
JP2001321677A
Method for producing fluorine-containing ether compound and method for producing article
JP2020128559A