Golf ball
A golf ball with a polyether polycarbonate diol-based coating film ensures easy dirt removal without reducing spin performance, addressing contamination issues.
Patent Information
- Application Number
- JP2023084768
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Golf balls with improved spin performance are prone to contamination from dirt and grass juices, which can soak in and are difficult to remove without reducing spin performance.
A golf ball with a coating film containing polyurethane derived from a polyether polycarbonate diol, which allows for easy removal of dirt like mud or grass juice without significantly affecting spin performance.
The golf ball maintains high spin performance on approach shots while effectively wiping off dirt such as mud or grass juice.
Smart Images

Figure 2024168259000016 
Figure 2024168259000017 
Figure 2024168259000018
Abstract
Description
[Technical field]
[0001] The present invention relates to a golf ball having a coating. [Background technology]
[0002] Conventionally, a coating film is formed on the surface of a golf ball body, and efforts have been made to improve the coating film to improve the spin performance on approach shots.
[0003] For example, Patent Document 1 discloses a golf ball having a golf ball body and a coating film provided on the surface of the golf ball body, the coating film being formed from a curable coating composition consisting of a base agent containing polyrotaxane in which at least a portion of the hydroxyl groups of the cyclodextrin have been modified with a caprolactone chain via a -O-C3H6-O- group, and a curing agent containing polyisocyanate, the base agent being a polyrotaxane having cyclodextrin, linear molecules that encapsulate the cyclic structures of the cyclodextrin in a skewered shape, and blocking groups that are arranged at both ends of the linear molecules and prevent the cyclodextrin from being detached.
[0004] Patent Document 2 discloses a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, wherein at least one layer of the coating film contains, as a base resin, a polyurethane obtained by reacting a polyisocyanate composition with, as a polyol component, a polyol composition containing a polyrotaxane having at least two hydroxy groups and a urethane polyol, and wherein the content of the polyrotaxane having at least two hydroxy groups in the polyol component is greater than 0% by mass and less than 10% by mass. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-093386 A [Patent Document 2] JP 2021-137298 A Summary of the Invention [Problem to be solved by the invention]
[0006] A golf ball with excellent spin performance for approach shots has a problem of being easily soiled by mud, grass juice, etc. Therefore, improvements have been made to the stain resistance of the golf ball so that the ball is less susceptible to stains by mud, grass juice, etc. However, the stain resistance is not always sufficient, and the golf ball surface may be soiled. When the golf ball is soiled by mud, grass juice, etc., the dirt penetrates the golf ball and cannot be wiped off cleanly. To provide a golf ball which can be easily wiped clean even when soiled with mud, grass juice or the like, without substantially reducing the spin performance of approach shots. [Means for solving the problem]
[0007] The golf ball of the present invention, which is able to solve the above-mentioned problems, is a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, wherein at least one layer of the coating film contains polyurethane as a resin component, and the polyurethane has a structural unit derived from a polyether polycarbonate diol represented by formula (A).
[0008] [ka] [In formula (A), R 1 , R 2 are the same or different and are a linear or branched alkylene group having 1 to 30 carbon atoms, l and n are the same or different and are numbers from 2 to 15, and m is a number from 1 to 15.]
[0009] In the present invention, the polyurethane forming the coating film has structural units derived from polyether polycarbonate diol, making it easier to remove dirt from the golf ball without substantially reducing the spin performance on approach shots. Effect of the Invention
[0010] According to the present invention, a golf ball can be provided which can be easily wiped clean even when soiled with mud, grass juice or the like, without substantially reducing the spin performance of approach shots. [Brief description of the drawings]
[0011] [Figure 1] 1 is a partially cutaway cross-sectional view showing a golf ball according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic cross-sectional view illustrating measurement points of a coating film thickness. [Diagram 3] FIG. 4 is a schematic cross-sectional view illustrating measurement points of a coating film thickness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The golf ball of the present invention is a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, wherein at least one layer of the coating film contains polyurethane as a resin component, and the polyurethane has a structural unit derived from a polyether polycarbonate diol represented by formula (A).
[0013] [ka] [In formula (A), R 1 , R 2 are the same or different and are a linear or branched alkylene group having 1 to 30 carbon atoms, l and n are the same or different and are numbers from 2 to 15, and m is a number from 1 to 15.]
[0014] The polyurethane is a polymer having a plurality of urethane bonds in the main chain. The polyurethane used in the present invention is preferably obtained by reacting a polyisocyanate composition containing a polyisocyanate with a polyol composition containing a polyol. By the reaction between the polyisocyanate and the polyol, a plurality of urethane bonds are formed in the main chain of the polyurethane. The obtained polyurethane has a structural unit derived from the polyisocyanate and a structural unit derived from the polyol.
[0015] The structural unit derived from a polyisocyanate means a structural unit formed by the reaction of a polyisocyanate with a polyol. The structural unit derived from a polyol means a structural unit formed by the reaction of a polyol with a polyisocyanate.
[0016] In the present invention, the polyether polycarbonate diol represented by formula (A) may be simply referred to as "polyether polycarbonate diol (A)". The polyether polycarbonate diol (A) has a polyether structure of (-R 1 -O-) l are bonded by a carbonate group (-O-C(=O)-O-).
[0017] In the formula (A), when m=1, it is called a "polyether carbonate diol" rather than a "polyether polycarbonate diol", but in the present invention, the polyether carbonate diol represented by the formula (A) is also called "polyether polycarbonate diol (A)".
[0018] In formula (A), l and n are the same or different and are numbers from 2 to 15, preferably from 2 to 10, and more preferably from 2 to 6. m is preferably a number from 2 to 10, and more preferably a number from 3 to 10. l, m, and n are preferably integers.
[0019] In formula (A), R 1 and R2 The number of carbon atoms in the alkylene group represented by each of the following formulas is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more, and is preferably 30 or less, more preferably 15 or less, and even more preferably 8 or less.
[0020] The alkylene group may be a linear alkylene group or a branched alkylene group. 1 , R 2 is preferably a linear alkylene group having 1 to 10 carbon atoms.
[0021] R 1 and R 2 Examples of the alkylene group represented by the formula (C) include an ethylene group (C2), a propylene group (C3), a butylene group (C4), a pentylene group (C5), a hexylene group (C6), a heptylene group (C7), an octylene group (C8), a nonylene group (C9), a decylene group (C10), an undecylene group (C11), a dodecylene group (C12), a tridecylene group (C13), a tetradecylene group (C14), a pentadecylene group (C15), a hexadecylene group (C16), Examples of the alkoxysilene include a heptadecylene group (C17), an octadecylene group (C18), a nonadecylene group (C19), an icosilene group (C20), an icosilene group (C21), a docosilene group (C22), a tricosilene group (C23), a tetracosilene group (C24), a pentacosilene group (C25), a hexacosilene group (C26), a heptacosilene group (C27), an octacosilene group (C28), a nonacosilene group (C29), and a triacontylene group (C30). 1 and R 2 is particularly preferably an n-butylene group.
[0022] The polyether polycarbonate diol (A) is R 1 and R 2 are the same, and l and n are also preferably the same, R 1 and R 2It is more preferable that l is an n-butylene group, and l and n are the same. The polyether polycarbonate diol (A) used in the present invention is preferably a polytetramethyl ether polycarbonate diol.
[0023] The polyether polycarbonate diol (A) is preferably produced by polymerizing a polyoxyalkylene glycol with a carbonate compound in the presence of a catalyst according to a conventional method.
[0024] Examples of the polyoxyalkylene glycol used in the production of polyether polycarbonate diol (A) include polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, copolymerized polytetramethylene ether glycol of 3-methyltetrahydrofuran and tetrahydrofuran, copolymerized polyether polyol of neopentyl glycol and tetrahydrofuran, copolymerized polyether polyol of ethylene oxide and tetrahydrofuran, copolymerized polyether glycol of propylene oxide and tetrahydrofuran, etc. Among these, polytetramethylene ether glycol (PTMG) is more preferable. The polyoxyalkylene glycol may be used alone or in combination of two or more kinds.
[0025] The number average molecular weight (Mn) calculated from the hydroxyl value of the polyoxyalkylene glycol used in the production of the polyether polycarbonate diol (A) is preferably 150 or more, more preferably 200 or more, and even more preferably 250 or more, and is preferably 2000 or less, more preferably 1500 or less, and even more preferably 1200 or less. If the molecular weight is 250 or more, flexibility can be imparted to the resulting coating film, and if the molecular weight is 2000 or less, tackiness of the coating film can be suppressed.
[0026] Examples of carbonate compounds that can be used in the production of polyether polycarbonate diol (A) include dialkyl carbonates, diaryl carbonates, and alkylene carbonates. These may be used alone or in combination. Among these, dialkyl carbonates and alkylene carbonates are preferred from the viewpoint of reactivity.
[0027] Specific examples of the carbonate compound include dimethyl carbonate, diethyl carbonate, dibutyl carbonate, diphenyl carbonate, ethylene carbonate, etc., with dimethyl carbonate and ethylene carbonate being preferred.
[0028] When producing the polyether polycarbonate diol (A), an ester exchange catalyst can be used as necessary to promote polymerization. As the ester exchange catalyst, any compound that is generally considered to have an ester exchange ability can be used without any restrictions.
[0029] Examples of the transesterification catalyst include compounds of Group 1 metals (excluding hydrogen) of the long period periodic table (hereinafter simply referred to as the "periodic table"), such as lithium, sodium, potassium, rubidium, and cesium; compounds of Group 2 metals of the periodic table, such as magnesium, calcium, strontium, and barium; compounds of Group 4 metals of the periodic table, such as titanium and zirconium; compounds of Group 5 metals of the periodic table, such as hafnium; compounds of Group 9 metals of the periodic table, such as cobalt; compounds of Group 12 metals of the periodic table, such as zinc; compounds of Group 13 metals of the periodic table, such as aluminum; compounds of Group 14 metals of the periodic table, such as germanium, tin, and lead; compounds of Group 15 metals of the periodic table, such as antimony and bismuth; and compounds of lanthanide metals, such as lanthanum, cerium, europium, and ytterbium.
[0030] The number average molecular weight of the polyether polycarbonate diol (A) is preferably 800 or more, more preferably 900 or more, and even more preferably 1000 or more, and is preferably 2500 or less, more preferably 2300 or less, and even more preferably 2100 or less. When the number average molecular weight of the polyether polycarbonate diol (A) is within the above range, a coating film that achieves both high approach spin and easy removal of dirt can be obtained.
[0031] The content of the polyether carbonate diol (A) component in the polyurethane is preferably 15% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, and is preferably 70% by mass or less, more preferably 63% by mass or less, and even more preferably 56% by mass or less. If the content of the polyether carbonate diol (A) component in the polyurethane is within the above range, a coating film that achieves both high approach spin and easy dirt removal is obtained.
[0032] The polyurethane forming the coating film of the golf ball of the present invention preferably has structural units derived from a polycarbonate diol (BC) different from the polyether polycarbonate diol (A). The polycarbonate diol (BC) is not particularly limited as long as it is different from the polyether polycarbonate diol (A).
[0033] The polycarbonate diol (BC) preferably has a repeating unit (B) represented by the following formula (B) and a repeating unit (C) represented by the following formula (C). The repeating unit (B) is represented by p=1 in formula (B). The repeating unit (C) is represented by q=1 in formula (C). When q is 0 in formula (C), no repeating unit (C) is present in the polycarbonate diol. In the present invention, a polycarbonate diol having a repeating unit (B) represented by the following formula (B) and a repeating unit (C) represented by the following formula (C) may be simply referred to as a "polycarbonate diol (BC)". Note that the "polycarbonate diol (BC)" also includes one that does not contain a repeating unit (C).
[0034] [ka] [ka]
[0035] (In the above formula (B), R 3 represents a divalent hydrocarbon group having 2 to 20 carbon atoms, p is a number from 3 to 50, and in the above formula (C), R 4 is R 3 and represents a divalent hydrocarbon group having 3 to 20 carbon atoms, or a divalent hydrocarbon group having 3 to 20 carbon atoms and containing an alicyclic structure or a heterocyclic structure, and q is a number from 0 to 50.
[0036] In formula (B), R 3 The number of carbon atoms in the divalent hydrocarbon group represented by the formula (I) is preferably 2 or more, more preferably 3 or more, and even more preferably 4 or more, and is preferably 20 or less, and more preferably 12 or less.
[0037] R in formula (B) 3 R is preferably a linear or branched alkylene group. 3 Examples of the alkylene group represented by the formula (C3), (C4), (C5), (C6), (C7), (C8), (C9), (C10), (C11), (C12), (C13), (C14), (C15), (C16), (C17), (C18), (C19), (C20), (C21), (C22), (C23), (C24), (C25), (C26), (C27), (C28), (C29), (C30), (C31), (C32), (C33), (C34), (C35), (C36), (C37), (C38), (C39 ...
[0038] In formula (B), R 3The divalent hydrocarbon group represented by the formula (I) is preferably derived from 1,4-butanediol, 1,5-pentanediol, or 1,6-hexanediol, and more preferably an n-butylene group or an n-hexylene group.
[0039] In formula (B), p is preferably 3 or more, more preferably 5 or more, and is preferably 50 or less, more preferably 40 or less, and even more preferably 30 or less. When p is 3 or more, the compatibility with other polyols is high, and when p is 50 or less, the abrasion resistance of the resulting polyurethane is high. p is preferably an integer.
[0040] In the repeating unit (C), R 4 The divalent hydrocarbon group represented by the following formula (I) preferably has 3 or more carbon atoms, more preferably 4 or more carbon atoms, and preferably has 20 or less carbon atoms, more preferably 12 or less carbon atoms.
[0041] In formula (C), R 4 R is preferably a linear or branched alkylene group. 4 Examples of the alkylene group represented by the formula (C3) include a propylene group (C4), a butylene group (C4), a pentylene group (C5), a hexylene group (C6), a heptylene group (C7), an octylene group (C8), a nonylene group (C9), a decylene group (C10), an undecylene group (C11), a dodecylene group (C12), a tridecylene group (C13), a tetradecylene group (C14), a pentadecylene group (C15), a hexadecylene group (C16), a heptadecylene group (C17), an octadecylene group (C18), a nonadecylene group (C19), and an icosylene group (C20).
[0042] R in formula (C) 4 Examples of the branched alkylene group represented by the formula (I) include those derived from one or more of neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, and 2-methyl-1,4-butanediol.
[0043] Furthermore, R in formula (C) 4 may be an aliphatic hydrocarbon group containing an alicyclic structure or a heterocyclic structure, and specific examples thereof include those derived from one or more of isosorbide, isomannide, isoidide, and 1,4-cyclohexanedimethanol.
[0044] In formula (C), q is preferably 1 or more, more preferably 2 or more, and is preferably 50 or less, more preferably 40 or less, and even more preferably 30 or less. q is preferably an integer. In formula (C), when q is 1 or more and the polycarbonate diol contains the repeating unit (C), compatibility with other polyols may be improved. When q is 50 or less, the durability and abrasion resistance of the resulting polyurethane are improved.
[0045] The polycarbonate diol (BC) may contain only one type of repeating unit (B) or may contain two or more types. The repeating unit (C) may also contain only one type or may contain two or more types. The repeating unit (B) and the repeating unit (C) may have the same structure.
[0046] The polycarbonate diol (BC) may contain repeating units other than the repeating units (B) and (C) in an amount of, for example, 5.0 mol % or less of all repeating units.
[0047] The polycarbonate diol (BC) can be produced in the same manner as in the production method of the polyether polycarbonate diol (A) described above, except that a dihydroxy compound for introducing the repeating unit (B) and a dihydroxy compound for introducing the repeating unit (C) are used instead of polyoxyalkylene glycol.
[0048] As the dihydroxy compound for introducing the repeating unit (B), a straight-chain aliphatic dihydroxy compound having 2 to 20 carbon atoms is preferred, and a straight-chain aliphatic dihydroxy compound having 3 to 6 carbon atoms is more preferred.
[0049] Examples of the linear aliphatic dihydroxy compound include one or more of 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,16-hexadecanediol, and 1,18-octadecanediol, and preferably 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,10-decanediol.
[0050] As the dihydroxy compound for introducing the repeating unit (C), a branched aliphatic dihydroxy compound having 3 to 20 carbon atoms is preferable, and a branched aliphatic dihydroxy compound having 4 to 12 carbon atoms is more preferable.
[0051] Examples of the branched aliphatic dihydroxy compound include neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, and 2-methyl-1,4-butanediol.
[0052] As a dihydroxy compound for introducing the repeating unit (C), an aliphatic dihydroxy compound containing an alicyclic structure or a heterocyclic structure can also be used. Examples of the aliphatic dihydroxy compound containing an alicyclic structure or a heterocyclic structure include isosorbide, isomannide, isoidide, and 1,4-cyclohexanedimethanol.
[0053] The polycarbonate diol can be produced, for example, by polymerizing a dihydroxy compound for introducing the repeating unit (B), and a dihydroxy compound and a carbonate compound for introducing the repeating unit (C) in the presence of a catalyst according to a conventional method.
[0054] The carbonate compound that can be used for producing the polycarbonate diol (BC) is not limited as long as it does not impair the effects of the present invention, and includes dialkyl carbonate, diaryl carbonate, and alkylene carbonate. These may be one type or multiple types. Among these, diaryl carbonate is preferred from the viewpoint of reactivity.
[0055] Specific examples of the carbonate compound include dimethyl carbonate, diethyl carbonate, dibutyl carbonate, diphenyl carbonate, ethylene carbonate, etc., with diphenyl carbonate being preferred.
[0056] The amount of catalyst remaining in the polycarbonate diol (BC) is preferably 100 ppm by weight or less, particularly 10 ppm by weight or less, calculated as metal, from the viewpoint of controlling the polyurethane reaction. On the other hand, the amount of catalyst required is preferably 0.01 ppm by weight or more, particularly 0.1 ppm by weight or more, and especially 5 ppm by weight or more, calculated as metal.
[0057] The polycarbonate diol (BC) is preferably a liquid polycarbonate diol. Here, liquid means that it is a viscous liquid at 25°C. By using a liquid polycarbonate diol, the coating film becomes softer and the spin performance is further improved. The viscosity of the liquid polycarbonate diol is preferably 50 mPa·s / 50°C to 100,000 mPa·s / 50°C, 30 mPa·s / 60°C to 50,000 mPa·s / 60°C, or 10 mPa·s / 70°C to 20,000 mPa·s / 70°C. The viscosity can be measured, for example, using a B-type viscometer with a rotor HM2.
[0058] The viscosity of the liquid polycarbonate diol is preferably 50 mPa·s or more / 50°C and 100,000 mPa·s or less / 50°C, more preferably 100 mPa·s or more / 50°C and 5,000 mPa·s or less / 50°C, and even more preferably 200 mPa·s or more / 50°C and 2,000 mPa·s or less / 50°C.
[0059] The number average molecular weight of the polycarbonate diol (BC) is preferably 400 or more, more preferably 450 or more, even more preferably 500 or more, and is preferably 1200 or less, more preferably 1,000 or less, and even more preferably 900 or less. If the number average molecular weight of the polycarbonate diol is 400 or more, the distance between the crosslinking points in the coating film is long, and the coating film becomes soft, so that the spin performance is improved. If the number average molecular weight is 1,200 or less, the distance between the crosslinking points in the coating film is not too long, and the coating film has good stain resistance. The number average molecular weight of the first polyol component may be measured, for example, by gel permeation chromatography (GPC) using polystyrene as a standard substance, tetrahydrofuran as an eluent, and an organic solvent-based GPC column (for example, "Shodex (registered trademark) KF series" manufactured by Showa Denko KK) as a column.
[0060] When the polyurethane forming the coating film of the golf ball of the present invention contains polyether polycarbonate diol (A) and polycarbonate diol (BC) as polyol components, the ratio of polyether polycarbonate diol (A) / polycarbonate diol (BC) is preferably 40 / 60 or more, more preferably 50 / 50 or more, even more preferably 60 / 40 or more, preferably 90 / 10 or less, more preferably 80 / 20 or less, and even more preferably 70 / 30 or less. If the ratio of polyether polycarbonate diol (A) / polycarbonate diol (BC) is within the above range, the coating film will have both high approach spin and ease of cleaning.
[0061] The polyurethane that forms the coating of the golf ball of the present invention has structural units derived from a polyisocyanate.
[0062] The polyisocyanate may be, for example, a compound having at least two isocyanate groups. Examples of the polyisocyanate include aromatic polyisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), 1,5-naphthylene diisocyanate (NDI), 3,3'-bitrylene-4,4'-diisocyanate (TODI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), and paraphenylene diisocyanate (PPDI); 4,4'-dicyclohexylmethane diisocyanate (H 12 Examples of the polyisocyanate include alicyclic polyisocyanates or aliphatic polyisocyanates such as cycloaliphatic polyisocyanate (MDI), hydrogenated xylylene diisocyanate (H6XDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and norbornene diisocyanate (NBDI); and derivatives of these polyisocyanates. In the present invention, two or more kinds of polyisocyanates may be used as the polyisocyanate.
[0063] The polyisocyanate derivatives include, for example, adduct modified products obtained by reacting diisocyanate with polyhydric alcohol, isocyanurate modified products of diisocyanate, biuret modified products, allophanate modified products, etc., and more preferably those from which free diisocyanate has been removed.The polyisocyanate composition preferably contains, as a polyisocyanate component, at least one selected from the group consisting of isocyanurate modified products of hexamethylene diisocyanate, adduct modified products of hexamethylene diisocyanate, biuret modified products of hexamethylene diisocyanate, and isocyanurate modified products of isophorone diisocyanate.
[0064] The biuret modified product may be, for example, a biuret modified product (the following formula (1)) in which a diisocyanate is trimerized. In formula (1), R represents a residue obtained by removing an isocyanate group from a diisocyanate. The biuret modified product is preferably a trimer of hexamethylene diisocyanate.
[0065] [ka]
[0066] The isocyanurate-modified product may be, for example, a trimer of diisocyanate represented by the following formula (2). In formula (2), R represents a residue obtained by removing an isocyanate group from a diisocyanate. The isocyanurate-modified product may be an isocyanurate-modified product of hexamethylene diisocyanate or an isocyanurate-modified product of isophorone diisocyanate, and a trimer of hexamethylene diisocyanate or an isocyanurate trimer of isophorone diisocyanate is preferred.
[0067] [ka]
[0068] The adduct modified product is a polyisocyanate obtained by reacting a diisocyanate with a polyhydric alcohol. The polyhydric alcohol is preferably a low molecular weight triol such as trimethylolpropane or glycerin. The adduct modified product is preferably, for example, a triisocyanate obtained by reacting a diisocyanate with trimethylolpropane (formula (3) below); or a triisocyanate obtained by reacting a diisocyanate with glycerin (formula (4) below). In formulas (3) and (4), R represents a residue obtained by removing an isocyanate group from a diisocyanate.
[0069] [ka] TIFF2024168259000008.tif57161
[0070] As the adduct modified product, for example, an adduct modified product of hexamethylene diisocyanate is preferable, and a triisocyanate obtained by reacting hexamethylene diisocyanate with trimethylolpropane; or a triisocyanate obtained by reacting hexamethylene diisocyanate with glycerin is preferable.
[0071] The allophanate is, for example, a triisocyanate obtained by reacting a diisocyanate with a low molecular weight diol to form a urethane bond, and then reacting the urethane bond with a diisocyanate.
[0072] (Adduct modification) In a preferred embodiment of the present invention, the polyisocyanate component is preferably an adduct modified product, and more preferably an adduct modified product of hexamethylene diisocyanate (preferably a trimer). When an adduct modified product of hexamethylene diisocyanate is used, the content of the adduct modified product of hexamethylene diisocyanate in the polyisocyanate component is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more. It is also preferable to use only the adduct modified product of hexamethylene diisocyanate as the polyisocyanate component.
[0073] (Isocyanurate modified) In another preferred embodiment of the present invention, the polyisocyanate component is preferably an isocyanurate modified product, more preferably an isocyanurate modified product of hexamethylene diisocyanate (preferably a trimer) or an isocyanurate modified product of isophorone diisocyanate (preferably a trimer). It is more preferable to use an isocyanurate modified product of hexamethylene diisocyanate (preferably a trimer) and an isocyanurate modified product of isophorone diisocyanate (preferably a trimer) in combination. When used in combination, the mass ratio of the isocyanurate modified product of hexamethylene diisocyanate to the isocyanurate modified product of isophorone diisocyanate (isocyanurate modified product of hexamethylene diisocyanate / isocyanurate modified product of isophorone diisocyanate) is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.3 or more, and is preferably 9 or less, more preferably 4 or less, even more preferably 3 or less. If the mass ratio is within the above range, the spin rate of an approach shot when the ball is biting into the grass is increased.
[0074] (Adduct modified + Isocyanurate modified) In another preferred embodiment of the present invention, the polyisocyanate component is preferably a combination of an adduct modified product and an isocyanurate modified product, and more preferably a combination of an adduct modified product (preferably a trimer) of hexamethylene diisocyanate and an isocyanurate modified product (preferably a trimer) of hexamethylene diisocyanate, or an adduct modified product (preferably a trimer) of hexamethylene diisocyanate and an isocyanurate modified product (preferably a trimer) of isophorone diisocyanate. In this case, the mass ratio of the adduct modified product to the isocyanurate modified product (adduct modified product / isocyanurate modified product) is preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.4 or more, and preferably 9 or less, more preferably 5 or less, and even more preferably 4 or less. If the mass ratio is within the above range, the spin performance is increased in approach shots from the rough.
[0075] (HDI adduct modified + HDI isocyanurate modified) In another preferred embodiment of the present invention, when an adduct-modified product of hexamethylene diisocyanate and an isocyanurate-modified product of hexamethylene diisocyanate are used as the polyisocyanate component, the total content of the adduct-modified product of hexamethylene diisocyanate and the isocyanurate-modified product of hexamethylene diisocyanate in the polyisocyanate component is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. It is also preferable to use only the adduct-modified product of hexamethylene diisocyanate and the isocyanurate-modified product of hexamethylene diisocyanate as the polyisocyanate component.
[0076] (HDI isocyanurate modified + IPDI isocyanurate modified) In another preferred embodiment of the present invention, when an isocyanurate-modified product of hexamethylene diisocyanate and an isocyanurate-modified product of isophorone diisocyanate are used as the polyisocyanate component, the total content of the isocyanurate-modified product of hexamethylene diisocyanate and the isocyanurate-modified product of isophorone diisocyanate in the polyisocyanate component is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. It is also preferable to use only the isocyanurate-modified product of hexamethylene diisocyanate and the isocyanurate-modified product of isophorone diisocyanate as the polyisocyanate component.
[0077] (HDI adduct modified + IPDI isocyanurate modified) In another preferred embodiment of the present invention, when an adduct-modified hexamethylene diisocyanate and an isocyanurate-modified isophorone diisocyanate are used as the polyisocyanate component, the total content of the adduct-modified hexamethylene diisocyanate and the isocyanurate-modified isophorone diisocyanate in the polyisocyanate component is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. It is also preferable to use only the adduct-modified hexamethylene diisocyanate and the isocyanurate-modified isophorone diisocyanate as the polyisocyanate component.
[0078] The amount of isocyanate groups (NCO%) of the polyisocyanate component is preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and even more preferably 2.0% by mass or more, and is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. The amount of isocyanate groups (NCO%) of the polyisocyanate component can be expressed as 100 x [number of moles of isocyanate groups in polyisocyanate x 42 (molecular weight of NCO)] / total mass (g) of polyisocyanate.
[0079] Specific examples of the polyisocyanate component include Burnock (registered trademark) D-800, Burnock DN-950, and Burnock DN-955 manufactured by DIC Corporation, Desmodur (registered trademark) N75MPA / X, Desmodur N3300, Desmodur N3390, Desmodur L75(C), and Sumidur (registered trademark) E21-1 manufactured by Sumika Bayer Urethane Co., Ltd., Coronate (registered trademark) HX, Coronate HK, Coronate HL, and Coronate EH manufactured by Tosoh Corporation, Duranate (registered trademark) 24A-100, Duranate 21S-75E, Duranate TPA-100, Duranate TKA-100, and Duranate 24A-90CX manufactured by Asahi Kasei Chemicals Corporation, and VESTANAT (registered trademark) T1890 manufactured by Degussa.
[0080] The coating film of the golf ball of the present invention is preferably formed from a paint containing a polyol composition containing a polyol component and a polyisocyanate composition containing a polyisocyanate component. The paint may be a so-called curing paint in which the polyol composition is the main component and the polyisocyanate composition is the curing agent. The raw materials for forming the polyurethane used in the present invention will be described below.
[0081] (Polyol Composition) The polyol composition used in the present invention preferably contains a urethane polyol as a polyol component. The urethane polyol is a compound having a plurality of urethane bonds in a molecule and having two or more hydroxyl groups in one molecule. For example, the urethane polyol may be a urethane prepolymer obtained by reacting a first polyol component with a first polyisocyanate component under conditions in which the hydroxyl groups of the first polyol component are in excess of the isocyanate groups of the first polyisocyanate component.
[0082] The polyol composition used in the present invention preferably contains a urethane polyol as a polyol component, and the urethane polyol preferably has the polyether polycarbonate diol (A) as a first polyol component.
[0083] The urethane polyol preferably has, as a first polyol component, a structural unit derived from a low-molecular-weight polyol having a molecular weight of less than 400 or a high-molecular-weight polyol having a number-average molecular weight of 400 or more, in addition to the polyether polycarbonate diol (A).
[0084] Examples of the high molecular weight polyol include polyether polyol, polyester polyol, polycaprolactone polyol, polycarbonate polyol, and acrylic polyol. Examples of the polyether polyol include polyoxyethylene glycol (PEG), polyoxypropylene glycol (PPG), and polyoxytetramethylene glycol (PTMG). Examples of the polyester polyol include polyethylene adipate (PEA), polybutylene adipate (PBA), and polyhexamethylene adipate (PHMA). Examples of the polycaprolactone polyol include poly-ε-caprolactone (PCL). Examples of the polycarbonate polyol include polyhexamethylene carbonate. The high molecular weight polyol may be used alone or in a mixture of two or more kinds.
[0085] In the present invention, it is particularly preferable that the first polyol component constituting the urethane polyol contains the polycarbonate diol (BC) in addition to the polyether polycarbonate diol (A). By containing the polyether polycarbonate diol (A) and the polycarbonate diol (BC) in the first polyol component constituting the urethane polyol used in the present invention, the approach spin performance from the rough is further improved and dirt is easily removed.
[0086] When the first polyol component constituting the urethane polyol contains polyether polycarbonate diol (A) and polycarbonate diol (BC), the ratio of polyether polycarbonate diol (A) / polycarbonate diol (BC) is preferably 40 / 60 or more, more preferably 50 / 50 or more, even more preferably 60 / 40 or more, and preferably 90 / 10 or less, more preferably 80 / 20 or less, and even more preferably 70 / 30 or less. If the ratio of polyether polycarbonate diol (A) / polycarbonate diol (BC) is within the above range, a coating film that achieves both high approach spin and easy dirt removal is obtained.
[0087] The content of the polyether polycarbonate diol (A) in the urethane polyol is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% by mass or less. If the content of the polyether polycarbonate diol (A) is within the above range, a coating film that achieves both high approach spin and easy removal of dirt is obtained.
[0088] The first polyol component may contain a low molecular weight polyol having a molecular weight of less than 500. Examples of the low molecular weight polyol include diols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, and 1,6-hexanediol; and triols such as glycerin, trimethylolpropane, and hexanetriol. The low molecular weight polyols may be used alone or in combination of two or more.
[0089] The urethane polyol preferably contains a triol component and a diol component as a first polyol component. The triol component is preferably trimethylolpropane. The mixing ratio of the triol component and the diol component (triol component / diol component) is preferably 1.0 or more, more preferably 1.2 or more, and is preferably 2.6 or less, more preferably 2.4 or less, in terms of the molar ratio of OH groups.
[0090] The first polyisocyanate component capable of constituting the urethane polyol is not particularly limited as long as it has two or more isocyanate groups, and examples thereof include aromatic polyisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), 1,5-naphthylene diisocyanate (NDI), 3,3'-bitrylene-4,4'-diisocyanate (TODI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), and paraphenylene diisocyanate (PPDI); 4,4'-dicyclohexylmethane diisocyanate (H 12 Examples of the polyisocyanate include alicyclic polyisocyanates or aliphatic polyisocyanates such as cyclohexanediisocyanate (MDI), hydrogenated xylylene diisocyanate (H6XDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and norbornene diisocyanate (NBDI). These polyisocyanates may be used alone or in combination of two or more.
[0091] The urethane polyol preferably contains an alicyclic diisocyanate as a polyisocyanate component.
[0092] The weight average molecular weight of the urethane polyol is preferably 5,000 or more, more preferably 5,300 or more, even more preferably 5,500 or more, and is preferably 20,000 or less, more preferably 18,000 or less, even more preferably 16,000 or less. If the weight average molecular weight of the urethane polyol is 5,000 or more, the distance between crosslinking points in the coating film is long, and the coating film becomes soft, so that the spin performance is improved. If the weight average molecular weight is 20,000 or less, the distance between crosslinking points in the coating film is not too long, and the coating film has good stain resistance.
[0093] The hydroxyl value of the urethane polyol is preferably 10 mgKOH / g or more, more preferably 15 mgKOH / g or more, and even more preferably 20 mgKOH / g or more, and is preferably 200 mgKOH / g or less, more preferably 190 mgKOH / g or less, and even more preferably 180 mgKOH / g or less. The hydroxyl value can be measured, for example, by an acetylation method in accordance with JIS K 1557-1.
[0094] In another preferred embodiment, the polyol composition used in the present invention may further contain a second polyol as a polyol component in addition to the urethane polyol. Examples of the second polyol include a low molecular weight polyol having a molecular weight of less than 500 and a high molecular weight polyol having a number average molecular weight of 500 or more.
[0095] Examples of the low molecular weight polyols include diols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, and 1,6-hexanediol; and triols such as glycerin, trimethylolpropane, and hexanetriol. Examples of the high molecular weight polyols include polyether polyols, polyester polyols, polycaprolactone polyols, polycarbonate polyols, and acrylic polyols. Examples of the polyether polyols include polyoxyethylene glycol (PEG), polyoxypropylene glycol (PPG), and polyoxytetramethylene glycol (PTMG). Examples of the polyester polyols include polyethylene adipate (PEA), polybutylene adipate (PBA), and polyhexamethylene adipate (PHMA). Examples of the polycaprolactone polyols include poly-ε-caprolactone (PCL). The polycarbonate polyol may, for example, be polyhexamethylene carbonate.
[0096] The content of the urethane polyol in the polyol component contained in the polyol composition is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, and is preferably 99% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less. It is also preferable to use only the urethane polyol as the polyol component contained in the polyol composition.
[0097] The content of each component contained as a polyol is appropriately selected from the range of the content of each component so that the total content of these components is 100%.
[0098] (Polyisocyanate composition) As the polyisocyanate component of the polyisocyanate composition used in the present invention, those exemplified as polyisocyanates capable of forming polyurethane can be used. Examples of the polyisocyanate include aromatic polyisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), 1,5-naphthylene diisocyanate (NDI), 3,3'-bitrylene-4,4'-diisocyanate (TODI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), and paraphenylene diisocyanate (PPDI); 4,4'-dicyclohexylmethane diisocyanate (H 12 Examples of the polyisocyanate include alicyclic polyisocyanates or aliphatic polyisocyanates such as cycloaliphatic polyisocyanate (MDI), hydrogenated xylylene diisocyanate (H6XDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and norbornene diisocyanate (NBDI); and derivatives of these polyisocyanates. In the present invention, two or more kinds of polyisocyanates may be used as the polyisocyanate.
[0099] The polyisocyanate derivatives include, for example, adduct modified products obtained by reacting diisocyanate with polyhydric alcohol, isocyanurate modified products of diisocyanate, biuret modified products, allophanate modified products, etc., and more preferably those from which free diisocyanate has been removed.The polyisocyanate composition preferably contains, as a polyisocyanate component, at least one selected from the group consisting of isocyanurate modified products of hexamethylene diisocyanate, adduct modified products of hexamethylene diisocyanate, biuret modified products of hexamethylene diisocyanate, and isocyanurate modified products of isophorone diisocyanate.
[0100] In the curing reaction in the curable coating composition, the molar ratio (NCO group / OH group) of the hydroxy group (OH group) of the polyol composition and the isocyanate group (NCO group) of the polyisocyanate composition is preferably 0.6 or more, more preferably 0.75 or more, and even more preferably 0.9 or more. If the molar ratio (NCO group / OH group) is 0.6 or more, the curing reaction is good. The molar ratio (NCO group / OH group) is preferably 1.4 or less, more preferably 1.3 or less, and even more preferably 1.2 or less. If the molar ratio (NCO group / OH group) is 1.4 or less, the amount of isocyanate groups is not excessive, and the hardness of the resulting coating film is moderate and the appearance is good. Note that the reason why the appearance of the resulting coating film becomes poor when the amount of isocyanate groups in the coating is excessive is thought to be that when the amount of isocyanate groups is excessive, the reaction between the moisture in the air and the isocyanate groups increases, and a large amount of carbon dioxide gas is generated.
[0101] The coating material may be either a water-based coating material using water as a main dispersion medium or a solvent-based coating material using an organic solvent as a dispersion medium, but is preferably a solvent-based coating material. In the case of a solvent-based coating material, preferred solvents include toluene, isopropyl alcohol, xylene, methyl ethyl ketone, methyl ethyl isobutyl ketone, ethylene glycol monomethyl ether, ethylbenzene, propylene glycol monomethyl ether, isobutyl alcohol, and ethyl acetate. The solvent may be mixed into either the polyol composition or the polyisocyanate composition, but from the viewpoint of uniformly carrying out the curing reaction, it is preferable to mix the solvent into each of the polyol composition and the polyisocyanate composition.
[0102] The coating material preferably further contains modified silicone. By containing modified silicone as a leveling agent, unevenness of the coating surface can be reduced, and a smooth coating surface can be formed on the surface of the golf ball. The modified silicone may be one in which an organic group is introduced into the side chain or end of a polysiloxane skeleton, a polysiloxane block copolymer in which a polyether block and / or a polycaprolactone block is copolymerized with a polysiloxane block, or one in which an organic group is introduced into the side chain or end of the polysiloxane block copolymer. The polysiloxane skeleton or polysiloxane block is preferably linear, and examples of the polysiloxane skeleton or polysiloxane block include dimethylpolysiloxane, methylphenylpolysiloxane, and methylhydrogenpolysiloxane. Examples of the organic group include amino groups, epoxy groups, mercapto groups, and carbinol groups. In the present invention, it is preferable to use a polydimethylsiloxane-polycaprolactone block copolymer as the modified silicone oil, and it is more preferable to use a terminal carbinol modified polydimethylsiloxane-polycaprolactone block copolymer. Specific examples of the modified silicone used in the present invention include DBL-C31, DBE-224, and DCE-7521 manufactured by Gelest.
[0103] The modified silicone remains in the coating film formed from the coating composition. The content of the modified silicone in the coating film and the curable coating composition is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the resin component constituting the coating layer.
[0104] A known catalyst can be used for the curing reaction. Examples of the catalyst include monoamines such as triethylamine and N,N-dimethylcyclohexylamine; polyamines such as N,N,N',N'-tetramethylethylenediamine and N,N,N',N'',N''-pentamethyldiethylenetriamine; cyclic diamines such as 1,8-diazabicyclo[5.4.0]-7-undecene (DBU) and triethylenediamine; and tin-based catalysts such as dibutyltin dilaurate and dibutyltin diacetate. These catalysts may be used alone or in combination of two or more. Among these, tin-based catalysts such as dibutyltin dilaurate and dibutyltin diacetate are preferred, and dibutyltin dilaurate is particularly preferred.
[0105] The coating film may further contain, as necessary, additives that may be generally contained in paints for golf balls, such as an ultraviolet absorber, an antioxidant, a light stabilizer, a fluorescent brightening agent, an antiblocking agent, a leveling agent, a slip agent, and a viscosity modifier.
[0106] The golf ball of the present invention is a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, wherein at least one layer of the coating film contains polyurethane as a resin component, and the polyurethane has a structural unit derived from a polyether polycarbonate diol represented by formula (A).
[0107] When the coating film has a multi-layer structure, it is preferable that the outermost coating film contains polyurethane as a resin component, and the polyurethane has a structural unit derived from a polyether polycarbonate diol represented by formula (A).
[0108] When the coating film has a multi-layer structure, the coating film layer located at the outermost side is the outermost coating film layer. When the coating film is a single layer, the single layer coating film is the outermost coating film layer. The content of polyurethane in the resin component is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. It is also a preferred embodiment that the resin component of the coating film is substantially composed of only the polyurethane.
[0109] When the coating film has a multi-layer structure, examples of the base resin constituting the coating film layers other than the outermost layer include polyurethane, epoxy resin, acrylic resin, vinyl acetate resin, polyester resin, etc., among which polyurethane is preferred. In addition, the polyurethane that can be used for the outermost layer described above may be used as the resin constituting the coating film layers other than the outermost layer.
[0110] The thickness of the coating film containing the polyurethane is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 9 μm or more, and is preferably 40 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less. If the thickness of the coating film is within the above range, the appearance is good, the abrasion resistance of the golf ball is excellent, and the approach performance is good.
[0111] When the coating film of the golf ball of the present invention has a multi-layer structure, the total thickness of the coating film is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 9 μm or more, and is preferably 50 μm or less, more preferably 45 μm or less, and even more preferably 40 μm or less. If the thickness is 5 μm or more, the spin rate on approach shots increases, and if it is 50 μm or less, the spin rate on driver shots can be suppressed.
[0112] The tackiness and 10% modulus of the coating layer can be controlled by the resin components and amounts of the coating layer.
[0113] The 10% modulus of the coating film containing the polyurethane is 1 kgf / cm 2(0.10 MPa) or more is preferable, and 3 kgf / cm is more preferable. 2 (0.29MPa) or more, and more preferably 10kgf / cm 2 (0.98MPa) or more, 70kgf / cm 2 (6.9 MPa) or less is preferable, and 60 kgf / cm 2 (5.9MPa) or less, more preferably 50kgf / cm 2 (4.9MPa) or less. The 10% modulus of the coating film is 1kgf / cm 2 If it is more than 70kgf / cm, the coating film will have low adhesion and will be less likely to get dirty. 2 If the surface roughness is below this level, the static friction of the coating will increase, increasing the spin rate of approach shots from the rough (when the grass is biting).
[0114] (Golf ball) The golf ball of the present invention is not particularly limited as long as it is a golf ball having a golf ball body and at least one coating layer formed on the surface of the golf ball body. The structure of the golf ball body is not particularly limited, and it may be a one-piece golf ball, a two-piece golf ball, a multi-piece golf ball having three or more pieces, or a thread-wound golf ball. In any case, the present invention can be suitably applied.
[0115] (core) The one-piece golf ball body, as well as the cores used in thread-wound golf balls, two-piece golf balls and multi-piece golf balls will now be described.
[0116] A known rubber composition (hereinafter, sometimes simply referred to as a "rubber composition for the core") can be used for the one-piece golf ball body and core. For example, a rubber composition containing a base rubber, a co-crosslinking agent, and a crosslinking initiator can be molded by hot pressing.
[0117] As the base rubber, it is preferable to use high-cis polybutadiene having cis bonds of 40% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, which is advantageous in terms of resilience. As the co-crosslinking agent, α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms or a metal salt thereof is preferable, and a metal salt of acrylic acid or a metal salt of methacrylic acid is more preferable. As the metal of the metal salt, zinc, magnesium, calcium, aluminum, and sodium are preferable, and zinc is more preferable. The amount of the co-crosslinking agent used is preferably 20 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the base rubber. When an α,β-unsaturated carboxylic acid having 3 to 8 carbon atoms is used as the co-crosslinking agent, it is preferable to compound a metal compound (for example, magnesium oxide). As the crosslinking initiator, an organic peroxide is preferably used. Specifically, organic peroxides such as dicumyl peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, di-t-butyl peroxide, etc., can be mentioned, and among these, dicumyl peroxide is preferably used. The amount of the crosslinking initiator is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 3 parts by mass or less, more preferably 2 parts by mass or less, based on 100 parts by mass of the base rubber.
[0118] The core rubber composition may further contain an organic sulfur compound. As the organic sulfur compound, compounds belonging to diphenyl disulfides (e.g., diphenyl disulfide, bis(pentabromophenyl) disulfide), thiophenols, and thionaphthols (e.g., 2-thionaphthol) can be suitably used. The amount of the organic sulfur compound is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, per 100 parts by mass of the base rubber. The core rubber composition may further contain a carboxylic acid and / or a salt thereof. As the carboxylic acid and / or a salt thereof, a carboxylic acid having 1 to 30 carbon atoms and / or a salt thereof is preferred. As the carboxylic acid, either an aliphatic carboxylic acid or an aromatic carboxylic acid (e.g., benzoic acid) can be used. The amount of the carboxylic acid and / or a salt thereof is 1 part by mass or more and 40 parts by mass or less, per 100 parts by mass of the base rubber.
[0119] The core rubber composition may further contain, in addition to the base rubber, co-crosslinking agent, crosslinking initiator, and organic sulfur compound, a weight adjuster such as zinc oxide or barium sulfate, an antiaging agent, color powder, etc. The hot press molding conditions for the core rubber composition may be appropriately set according to the rubber composition, but it is usually preferable to heat the core rubber composition at 130°C to 200°C for 10 to 60 minutes, or to heat the core rubber composition at 130°C to 150°C for 20 to 40 minutes, and then heat the core rubber composition at 160°C to 180°C for 5 to 15 minutes in two stages.
[0120] (cover) The golf ball body preferably has a core and a cover that encases the core. In this case, the hardness of the cover is preferably 80 or less, more preferably 60 or less, even more preferably 50 or less, and particularly preferably 45 or less, in Shore D hardness. If the cover has a hardness of 60 or less, the spin rate will be higher. The cover hardness is not particularly limited, but is preferably 10 or more, more preferably 15 or more, and even more preferably 20 or more, in Shore D hardness. The cover hardness is a slab hardness measured by molding the cover composition that forms the cover into a sheet.
[0121] The thickness of the cover is preferably 0.1 mm or more, more preferably 0.2 mm or more, and even more preferably 0.3 mm or more, and is preferably 1.0 mm or less, more preferably 0.9 mm or less, and even more preferably 0.8 mm or less. If the thickness of the cover is 0.1 mm or more, the shot feeling of the golf ball becomes better, and if it is 1.0 mm or less, the resilience of the golf ball can be maintained.
[0122] The resin component constituting the cover is not particularly limited, and examples thereof include various resins such as ionomer resin, polyester resin, urethane resin, polyamide resin, thermoplastic polyamide elastomer commercially available under the trade name "Pebax (registered trademark)" (e.g., "Pebax 2533") from Arkema Co., Ltd., thermoplastic polyester elastomer commercially available under the trade name "Hytrel (registered trademark)" (e.g., "Hytrel 3548", "Hytrel 4047") from Toray DuPont Co., Ltd., thermoplastic polyurethane elastomer commercially available under the trade name "Elastollan (registered trademark)" (e.g., "Elastollan XNY82A", "Elastollan XNY97A") from BASF Japan Ltd., thermoplastic styrene elastomer and thermoplastic polyester elastomer commercially available under the trade name "Tefabloc" from Mitsubishi Chemical Corporation, etc. The cover materials may be used alone or in combination of two or more kinds.
[0123] Among these, polyurethane and ionomer resin are preferred as the resin component constituting the cover, and polyurethane is particularly preferred. When polyurethane is used as the resin component constituting the cover, the content of polyurethane in the resin component is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. When ionomer resin is used as the resin component constituting the cover, the content of ionomer resin in the resin component is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more.
[0124] The polyurethane may be in the form of either so-called thermoplastic polyurethane or thermosetting polyurethane. Thermoplastic polyurethane is a polyurethane that exhibits plasticity when heated, and generally means a polyurethane having a linear structure that has been molecular weighted to a certain degree. On the other hand, thermosetting polyurethane (two-component curing polyurethane) is a polyurethane obtained by reacting a low molecular weight urethane prepolymer with a curing agent (chain length extender) to increase the molecular weight when molding the cover. Thermosetting polyurethane includes polyurethane having a linear structure and polyurethane having a three-dimensional crosslinked structure by controlling the number of functional groups of the prepolymer and curing agent (chain length extender) used. As the polyurethane, a thermoplastic elastomer is preferable.
[0125] In addition to the resin components described above, the cover may contain pigment components such as white pigments (e.g., titanium oxide), blue pigments, and red pigments, weight adjusters such as calcium carbonate and barium sulfate, dispersants, antioxidants, ultraviolet absorbing agents, light stabilizers, fluorescent materials, or fluorescent brighteners, to the extent that the performance of the cover is not impaired.
[0126] The manner in which the cover is molded using the cover composition is not particularly limited, but examples thereof include a manner in which the cover composition is directly injection molded onto the core, or a manner in which a hollow shell is molded from the cover composition, the core is covered with a plurality of shells, and compression molded (preferably, a method in which a hollow half shell is molded from the cover composition, the core is covered with two half shells, and compression molded). The golf ball body with the molded cover is removed from the mold, and is preferably subjected to surface treatment such as deburring, cleaning, and sandblasting as necessary. Also, a mark can be formed as desired.
[0127] The total number of dimples formed on the cover is preferably 200 to 500 inclusive. If the total number of dimples is less than 200, the effect of the dimples is difficult to obtain. If the total number of dimples is more than 500, the size of each dimple becomes small, making it difficult to obtain the effect of the dimples. The shape (shape in plan view) of the dimples formed is not particularly limited, and may be a circle; a polygon such as an approximately triangular, approximately rectangular, approximately pentagonal, or approximately hexagonal; or other irregular shape; or may be used alone or in combination of two or more types.
[0128] In the case where the golf ball is a three-piece golf ball, a four-piece golf ball, a five-piece golf ball or more, the material of the intermediate layer provided between the core and the outermost cover layer may be, for example, a thermoplastic resin such as polyurethane, ionomer resin, polyamide, or polyethylene; a thermoplastic elastomer such as a styrene elastomer, a polyolefin elastomer, a polyurethane elastomer, or a polyester elastomer; or a cured product of a rubber composition. Here, examples of the ionomer resin include a copolymer of ethylene and α,β-unsaturated carboxylic acid in which at least a part of the carboxyl groups is neutralized with a metal ion, or a ternary copolymer of ethylene, α,β-unsaturated carboxylic acid, and α,β-unsaturated carboxylic acid ester in which at least a part of the carboxyl groups is neutralized with a metal ion. The intermediate layer may further contain a weight adjuster such as barium sulfate or tungsten, an antioxidant, a pigment, or the like. The intermediate layer may be called an inner cover layer or an outer core layer depending on the configuration of the golf ball.
[0129] (Formation of coating film) The coating film of the golf ball of the present invention can be formed by applying a paint to the surface of the golf ball body. The method for applying the paint is not particularly limited, and any known method can be used, such as spray coating or electrostatic coating.
[0130] In the case of spray coating using an air gun, the polyisocyanate composition and the polyol composition may be supplied by respective pumps and continuously mixed in a line mixer arranged just before the air gun, and the resulting mixture may be spray coated, or the polyol composition and the polyisocyanate composition may be spray coated separately using an air spray system equipped with a mixing ratio control mechanism. The coating may be spray coated in one go, or may be overcoated multiple times.
[0131] The paint applied to the golf ball body can be dried at a temperature of 30° C. to 70° C. for 1 hour to 24 hours to form a coating.
[0132] The diameter of the golf ball of the present invention is preferably 40 mm to 45 mm. From the viewpoint of satisfying the standards of the United States Golf Association (USGA), the diameter is preferably 42.67 mm or more. From the viewpoint of air resistance, the diameter is preferably 44 mm or less, and more preferably 42.80 mm or less. The mass of the golf ball is preferably 40 g or more and 50 g or less. From the viewpoint of obtaining large inertia, the mass is preferably 44.00 g or more, and more preferably 45.00 g or more. From the viewpoint of satisfying the standards of the USGA, the mass is preferably 45.93 g or less.
[0133] In the golf ball of the present invention, when the diameter is 40 mm to 45 mm, the compressive deformation amount (amount of shrinkage in the compressive direction) when a final load of 1275 N is applied from an initial load of 98 N is preferably 2.0 mm or more, more preferably 2.2 mm or more, and preferably 4.0 mm or less, more preferably 3.5 mm or less. A golf ball having a compressive deformation amount of 2.0 mm or more is not too hard and has a good shot feeling. On the other hand, by making the compressive deformation amount 4.0 mm or less, the resilience is increased.
[0134] 1 is a partially cutaway cross-sectional view showing a golf ball 1 according to one embodiment of the present invention. Golf ball 1 has a spherical core 2, a cover 3 that encases the spherical core 2, and a coating 4 provided on the surface of the cover 3. A large number of dimples 31 are formed on the surface of the cover 3. The portions of the surface of the cover 3 other than the dimples 31 are lands 32. EXAMPLES
[0135] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present invention are included within the scope of the present invention.
[0136] [Evaluation method] (1) Slab hardness (Shore D hardness) The intermediate layer composition and the cover composition were used to prepare a sheet having a thickness of about 2 mm by injection molding, and the sheet was stored at 23° C. for two weeks. The sheet was stacked in three or more sheets so as not to be affected by the measurement substrate, and the hardness was measured using an automatic hardness tester (Digitest II, manufactured by H. Burleith Co., Ltd.). The detector used was "Shore D."
[0137] (2) Coating thickness (μm) The golf ball was cut into a hemisphere, and the cross section of the coating on the hemisphere was observed using a microscope (Keyence Corporation, VHX-1000) to determine the coating thickness. The film thickness measurement points will be explained with reference to Figures 2 and 3. Figure 2 is a schematic diagram of a cross section of a golf ball. As shown in Figure 2, in the cross section of the golf ball, a line A passing through the center of the ball and the bottom of one of the dimples, a line B perpendicular to line A, and a line C at a 45° angle with line A are drawn, and the intersections of these lines with the coating surface are designated as pole P, equator E, and shoulder S, respectively.
[0138] FIG. 3 is a schematic diagram of a cross section passing through the bottom De of a dimple 31 and the center of a golf ball 1. The bottom De of a dimple is the deepest part of the dimple 31. The edge Ed is the point of contact between the dimple 31 and the tangent T when a common tangent T is drawn on both sides of the dimple 31. The measurement point Y on the slope is the point where a perpendicular line is drawn from the midpoint of the line connecting the bottom De and the edge Ed of the dimple to the dimple 31 and the slope of the dimple intersects with the perpendicular line. The measurement point X on the land is the midpoint between the edges of adjacent dimples. Note that in cases where there is no land portion, such as when adjacent dimples are in contact with each other, or when the land portion is extremely narrow and it is difficult to measure the film thickness, the bottom, edge, and slope of the dimple are used as the measurement points.
[0139] For the measurements, first test specimens were prepared from three locations on six balls: the dimple where the pole P is located, and the dimples near the equator E and shoulder S. Next, for each test specimen (dimple), the thickness of the paint film was measured at the dimple's bottom De, edge Ed, slope Y, and land X. Finally, the measurements for the six balls were averaged, and this average was used as the paint film thickness.
[0140] (3) 10% modulus of coating The tensile properties of the coating film were measured according to JIS K7161 (2014). Specifically, a coating material containing a polyisocyanate composition and a polyol composition was dried and cured at 40°C for 4 hours to produce a coating film (thickness 0.05 mm). This coating film was punched out into a test piece type 2 (parallel part width 10 mm, gauge length 50 mm) specified in JIS K7127 (1999) to produce a test piece. A tensile test was performed on this test piece using a precision universal testing machine (Shimadzu Corporation, Autograph (registered trademark)). The test conditions were a gripper distance of 100 mm, a tensile speed of 50 mm / min, and a test temperature of 23°C. The tensile stress at 10% strain (10% modulus) was then recorded.
[0141] (4) Approach spin speed A sand wedge (manufactured by Cleveland Golf, product name "CG15 Ford Wedge", loft angle: 58°) was attached to a Golf Laboratory swing machine, and a golf ball was hit at a head speed of 16 m / s, and the hit golf ball was photographed continuously to measure the dry spin speed (rpm). When measuring the approach spin speed from the rough (under conditions of biting into the grass), two grass leaves (approximately 3 cm long) were attached to the golf ball to be measured, and the ball was hit so that the grass was positioned between the club face and the golf ball when hit. The measurement was performed 10 times for each golf ball, and the average value was taken as the spin speed. A spin retention rate of 70% or more was considered to pass. <Spin retention rate = 100 x rough spin / dry spin>
[0142] (5) Ease of cleaning dirt from golf balls The ease of removing dirt from a golf ball was measured as follows. The balls were set on the grass in the rough and hit with a wedge 10 times per ball, three balls at each level, then wiped with a damp towel to check if the dirt on the grass could be removed. <Evaluation criteria> 〇: If you wipe the stain with a damp towel, the stain will come off completely. △: The dirt can be almost completely removed by wiping with a damp towel, but if you look closely you can see that some dirt remains. ×: When the stain is wiped off with a damp towel, some of it comes off, but it is clear at a glance that some stain remains.
[0143] 1. Preparation of Spherical Cores The rubber composition shown in Table 1 was kneaded and then hot-pressed at 150°C for 19 minutes in upper and lower molds having hemispherical cavities to obtain a spherical core with a diameter of 39.7 mm. The amount of barium sulfate was adjusted so that the ball mass was 45.6 g.
[0144] [Table 1] Polybutadiene rubber: JSR Corporation, "BR730 (high cis polybutadiene)" Zinc acrylate: Nisshoku Techno Fine Chemical Co., Ltd., "ZN-DA90S" Zinc oxide: "Ginrei R" manufactured by Toho Zinc Co., Ltd. Barium sulfate: Sakai Chemical Industry Co., Ltd., "Barium Sulfate BD" Diphenyl disulfide: Sumitomo Seika Chemicals Dicumyl peroxide: NOF Corporation, "Percumyl (registered trademark) D"
[0145] 2. Preparation of intermediate layer composition and cover composition The materials shown in Tables 2 and 3 were mixed in a twin-screw extruder to prepare pellets of an intermediate layer composition and a cover composition. The extrusion conditions were a screw diameter of 45 mm, a screw rotation speed of 200 rpm, and a screw L / D of 35, and the mixture was heated to 160 to 230°C at the die of the extruder.
[0146] [Table 2] Himilan (registered trademark) AM7329: Zinc ion neutralized ethylene-methacrylic acid copolymer ionomer resin manufactured by Mitsui Dow Polychemicals Surlyn 8945: Sodium ion neutralized ethylene-methacrylic acid copolymer ionomer resin manufactured by DuPont
[0147] [Table 3] Elastollan XNY82A: BASF Japan, thermoplastic polyurethane elastomer Tinuvin 770: Hindered amine light stabilizer manufactured by BASF Japan
[0148] 3. Forming the middle layer The intermediate layer composition obtained above was directly injection molded onto the spherical core obtained as described above to form an intermediate layer (thickness: 1.0 mm) covering the spherical core.
[0149] 4. Preparation of the Reinforcement Layer A reinforcing layer composition (manufactured by Shinto Paint Co., Ltd., product name "Porin (registered trademark) 750LE") was prepared using a two-component curing type epoxy resin as the base resin. The base material contained 30 parts by mass of bisphenol A type solid epoxy resin and 70 parts by mass of solvent. The curing agent contained 40 parts by mass of modified polyamidoamine, 5 parts by mass of titanium dioxide, and 55 parts by mass of solvent. The mass ratio of the base material to the curing agent was 1 / 1. This reinforcing layer composition was applied to the surface of the intermediate layer with an air gun and held in an atmosphere of 23°C for 12 hours to form a reinforcing layer. The thickness of the reinforcing layer was 7 μm.
[0150] 5.Cover molding The pellet-like cover composition was poured into each recess of the lower mold of the half-shell molding die, and pressed to form the half shells. The sphere on which the reinforcing layer was formed was concentrically covered with two half shells. This sphere and half shells were poured into a final mold having a number of pimples on the cavity surface. A cover (thickness: 0.5 mm) was molded by compression molding to obtain a golf ball body. Many dimples with the inverted shape of the pimples were formed on the cover.
[0151] 6. Paint Preparation Preparation of urethane polyols No. 1 to No. 7 As the first polyol component, polytetramethylene ether glycol (PTMG), polycarbonate diol (PCD), polyether polycarbonate diol, and trimethylolpropane (TMP) were dissolved in a solvent (toluene, methyl ethyl ketone) so as to have the compounding ratio shown in Table 4. Dibutyltin dilaurate was added as a catalyst to the mixture so as to be 0.1% by mass relative to 100% by mass of the polyol component. While maintaining this polyol solution at 80°C, isophorone diisocyanate (IPDI) as the first polyisocyanate component was added dropwise and mixed. After the addition, stirring was continued until the isocyanate was consumed, and then the mixture was cooled to room temperature to prepare a urethane polyol (solid content: 60% by mass). The composition of the obtained urethane polyol is shown in Table 4.
[0152] [Table 4]
[0153] The materials used in Table 4 are as follows: PCD500: Polycarbonate diol manufactured by Daicel Corporation (viscosity 1400 mPa·s / 25°C) PEPCD1002: Polytetramethylene ether polycarbonate diol manufactured by Mitsubishi Chemical Corporation (number average molecular weight: 1000, polytetramethylene ether glycol with a number average molecular weight of 250 linked by carbonate bonds) PEPCD2002: Polytetramethylene ether polycarbonate diol manufactured by Mitsubishi Chemical Corporation (number average molecular weight: 2000, polytetramethylene ether glycol with a number average molecular weight of 250 linked by carbonate bonds) PTMG1000: Polytetramethylene ether glycol manufactured by Mitsubishi Chemical Corporation TMP: Trimethylolpropane manufactured by Tokyo Chemical Industry Co., Ltd. IPDI: Isophorone diisocyanate manufactured by Sumika Covestro Urethane Co., Ltd.
[0154] Preparation of Polyol Compositions No. 1 to 7 100 parts by mass of the urethane polyol component was mixed with 100 parts by mass of a solvent (a mixed solvent of xylene / methyl ethyl ketone=70 / 30 (mass ratio)) to prepare polyol compositions No. 1 to No. 7. Dibutyltin dilaurate was added as a catalyst in an amount of 0.1% by mass relative to 100% by mass of the resin component of the polyol composition.
[0155] Preparation of Polyisocyanate Compositions Polyisocyanates were mixed in the mixing ratios shown in Table 5 to prepare polyisocyanate compositions.
[0156] The following polyisocyanates were used: HDI isocyanurate modified product: Isocyanurate modified product of hexamethylene diisocyanate (Asahi Kasei Chemicals Corporation, Duranate TKA-100 (NCO content: 21.7%)) HDI adduct modified product: Adduct modified product of hexamethylene diisocyanate (Asahi Kasei Chemicals Corporation, Duranate E402-80B (NCO content: 7.3%) HDI biuret modified product: biuret modified product of hexamethylene diisocyanate (manufactured by Asahi Kasei Chemicals Corporation, Duranate (registered trademark) 21S-75E (NCO content: 15.5%)) IPDI isocyanurate modified product: isocyanurate modified product of isophorone diisocyanate (Degussa, VESTANAT (registered trademark) T1890 (NCO content: 12.0%))
[0157] [Table 5]
[0158] 7. Formation of coating film A curable coating composition was prepared by blending the polyol composition and the polyisocyanate composition as shown in Table 5. The surface of the golf ball body obtained above was sandblasted and marked, and then a coating was applied with a spray gun and the coating was dried in an oven at 40°C for 24 hours to obtain a golf ball having a diameter of 42.7 mm and a mass of 45.6 g. The coating thickness was 10±2 μm.
[0159] The coating was performed by placing the golf ball body on a rotor equipped with prongs, rotating the rotor at 300 rpm, and moving the air gun vertically at a spray distance (7 cm) from the golf ball body. The interval between each recoat was 1.0 second. The spraying conditions for the air gun were as follows: recoat; 2 times, spray air pressure; 0.15 MPa, pressure tank air pressure; 0.10 MPa, application time per coat; 1 second, ambient temperature; 20°C to 27°C, ambient humidity; 65% or less. The evaluation results of the obtained golf balls are shown in Table 5.
[0160] As is clear from Table 5, a golf ball having a golf ball body and at least one layer of coating film formed on the surface of the golf ball body, at least one layer of the coating film containing polyurethane as a resin component, and the polyurethane having a structural unit derived from polyether polycarbonate diol (A), could have the dirt easily wiped off without substantially reducing the spin performance on approach shots. [Explanation of symbols]
[0161] 1: Golf ball, 2: Spherical core, 3: Cover, 4: Coating, 31: Dimples, 32: Land
[0162] A preferred embodiment (1) of the present invention is a golf ball having a golf ball body and at least one layer of coating film provided on the surface of the golf ball body, wherein at least one layer of the coating film contains polyurethane as a resin component, and the polyurethane has a structural unit derived from a polyether polycarbonate diol represented by formula (A).
[0163] [ka] [In formula (A), R 1 , R 2 are the same or different and are a linear or branched alkylene group having 1 to 30 carbon atoms, l and n are the same or different and are numbers from 2 to 15, and m is a number from 1 to 15.
[0164] A preferred embodiment (2) of the present invention is the golf ball according to the embodiment (1), wherein the polyether polycarbonate diol has a number average molecular weight of 800 to 2,500.
[0165] A preferred embodiment (3) of the present invention is the golf ball according to embodiment (1) or (2), in which the content of the polyether polycarbonate diol component in the polyurethane is 15% by mass to 70% by mass.
[0166] A preferred embodiment (4) of the present invention is a compound represented by the formula (1), 1 , R 2 and (3) are each a linear alkylene group having 1 to 10 carbon atoms.
[0167] A preferred embodiment (5) of the present invention is a golf ball according to any one of the embodiments (1) to (4), in which the polyurethane has a structural unit derived from a polycarbonate diol different from the polyether polycarbonate diol.
[0168] A preferred embodiment (6) of the present invention is a golf ball according to any one of the embodiments (1) to (5), in which the polyurethane has a structural unit derived from a polyisocyanate.
[0169] A preferred embodiment (7) of the present invention is the golf ball according to embodiment (6), in which the polyisocyanate is at least one selected from the group consisting of an isocyanurate-modified product of hexamethylene diisocyanate, an adduct-modified product of hexamethylene diisocyanate, a biuret-modified product of hexamethylene diisocyanate, and an isocyanurate-modified product of isophorone diisocyanate.
[0170] A preferred embodiment (8) of the present invention is a golf ball according to any one of the embodiments (1) to (7), in which the outermost layer of the coating contains the polyurethane.
Claims
1. A golf ball having a golf ball body and at least one layer of coating film provided on a surface of the golf ball body, At least one layer of the coating film contains polyurethane as a resin component, and the polyurethane has a structural unit derived from a polyether polycarbonate diol represented by formula (A). 【Chemistry 1】 [In formula (A), R 1 , R 2 are the same or different and are linear or branched alkylene groups having 1 to 30 carbon atoms, l and n are the same or different and are numbers from 2 to 15, and m is a number from 1 to 15.
2. 2. The golf ball according to claim 1, wherein the polyether polycarbonate diol has a number average molecular weight of 800 to 2,500.
3. 2. The golf ball according to claim 1, wherein the polyurethane contains 15% by mass to 70% by mass of the polyether polycarbonate diol component.
4. In formula (1), R 1 , R 2 and each are a linear alkylene group having 1 to 10 carbon atoms.
5. 2. The golf ball according to claim 1, wherein the polyurethane has structural units derived from a polycarbonate diol different from the polyether polycarbonate diol.
6. The golf ball according to claim 1 , wherein the polyurethane has structural units derived from a polyisocyanate.
7. The polyisocyanate is Isocyanurate modified hexamethylene diisocyanate, Adduct modified product of hexamethylene diisocyanate, A biuret-modified product of hexamethylene diisocyanate, and 7. The golf ball according to claim 6, wherein the resin is at least one selected from the group consisting of isocyanurate modified products of isophorone diisocyanate.
8. 2. The golf ball according to claim 1, wherein the outermost layer of the coating contains the polyurethane.
Citation Information
Patent Citations
Golf ball
JP2016093386A
Golf ball
JP2021137298A