Wallpaper and manufacturing method of wallpaper
The wallpaper structure with a base resin layer, pattern printing layer, and synchronized surface protective layer addresses the challenge of achieving a consistent three-dimensional design and gloss-matte appearance by ensuring a difference in gloss between its parts, enhancing both visual and tactile effects.
Patent Information
- Application Number
- JP2023085014
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for creating decorative sheets for wall decoration struggle with achieving a consistent three-dimensional design while maintaining a gloss-matte appearance, as the pattern printed on the pattern printing layer often differs from the surface protective layer, and embossing can disrupt the synchronized gloss-matte feeling.
A wallpaper structure is developed with a base resin layer, a pattern printing layer having first and second pattern forming parts on the same plane, and a surface protective layer that overlaps and synchronizes with one of these parts, creating a difference in gloss between them, achieved through specific lamination and heating processes.
The solution allows for a three-dimensional design with a gloss-matte effect without embossing, enhancing visual and tactile three-dimensional impressions while maintaining a synchronized gloss-matte appearance.
Smart Images

Figure 2024168395000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to wallpaper and a method for manufacturing wallpaper. [Background technology]
[0002] Conventionally, decorative sheets used for wall decoration of buildings and the like are preferred to have a low surface gloss. For this reason, for example, a gloss matte decorative sheet disclosed in Patent Document 1 is often used as a decorative sheet used for wall decoration of buildings and the like. The gloss matte decorative sheet disclosed in Patent Document 1 uses a chemical embossing method, and the surface protective layer is configured to include a matte resin layer that is a matte layer and a gloss resin layer that is a glossy layer. In addition, a gloss matte decorative sheet (see, for example, Patent Document 2) that can obtain a design in which the pattern printed on the pattern printing layer and the appearance of the surface protective layer are in harmony has also been proposed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5742972 [Patent Document 2] JP 2018-122574 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as described above, in the method of obtaining a surface protective layer including a matte resin layer and a gloss resin layer using a chemical embossing method, there is a problem that it is difficult to obtain a design in which the pattern printed on the pattern printing layer and the appearance of the surface protective layer are in harmony. In addition, in the method of obtaining a design in which the pattern printing layer and the surface protective layer are in harmony, the harmonious gloss matte feel of the surface protective layer may disappear if embossing is performed, and a three-dimensional design feel cannot be obtained if embossing is not performed.
[0005] The present invention has been made to solve such problems, and has an object to provide wallpaper that can achieve a three-dimensional design while maintaining a gloss-matt design. [Means for solving the problem]
[0006] According to one aspect of the present invention, there is provided wallpaper comprising a base resin layer, a pattern printing layer having a pattern printed thereon, and a surface protective layer laminated in that order on a paper substrate, wherein the pattern printing layer has a first pattern forming portion and a second pattern forming portion which form the same plane, the surface protective layer overlaps with only one of the first pattern forming portion and the second pattern forming portion when viewed from above and is positioned in sync with one of the pattern forming portions, and there is a gloss difference between the other of the first pattern forming portion and the second pattern forming portion and the surface protective layer.
[0007] According to another aspect of the present invention, there is provided a method for manufacturing wallpaper, comprising the steps of: forming a base resin layer containing at least one of vinyl chloride resin, polyolefin resin, and ethylene-vinyl acetate copolymer resin on one side of a paper base material; forming a pattern printed layer on the base resin layer, the pattern printed layer including a first pattern forming portion and a second pattern forming portion which are flush with each other; forming a surface protective layer on one of the pattern forming portions so as to overlap only one of the first pattern forming portion and the second pattern forming portion in a top view and to be in sync with the one of the pattern forming portions; heating a laminate comprising the paper base material, the base resin layer, the pattern printed layer, and the surface protective layer so that the surface temperature of the laminate is within the range of 130°C to 200°C; and cooling and drying the laminate after the heating step. Effect of the Invention
[0008] According to one aspect of the present invention, wallpaper can be obtained that can achieve a three-dimensional design while maintaining a gloss-matte design. [Brief description of the drawings]
[0009] [Figure 1]FIG. 1 is a cross-sectional view showing a schematic example of wallpaper according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a cross-sectional view showing a schematic example of wallpaper according to Reference Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Here, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of each thickness, etc. are different from the actual ones. In addition, the embodiments shown below are examples of configurations for embodying the technical idea of the present invention, and the technical idea of the present invention is not limited to the materials, shapes, etc. of the components described below. The technical idea of the present invention can be modified in various ways within the technical scope defined by the claims.
[0011] <Configuration> FIG. 1 is a cross-sectional view showing a schematic example of a wallpaper 10 according to an embodiment of the present invention. The wallpaper 10 comprises a paper base material 1, a base resin layer 2, a picture printed layer 3, and a surface protective layer 4, with the base resin layer 2, the picture printed layer 3, and the surface protective layer 4 laminated in this order on the paper base material 1. The thickness of the wallpaper 10 is, for example, within the range of 100 μm to 1000 μm.
[0012] (Paper base material 1) The paper base material 1 is formed using a material that is normally used as a paper base material, such as backing paper for wallpaper. The paper base material 1 has a basis weight of 50 [g / m 2 ] or more 100[g / m 2 ] or less, and the thickness is preferably within the range of 80 [μm] to 150 [μm]. By using, for example, plain paper as the material for the paper base material 1 as described above, it is possible to ensure that the wallpaper 10 has the rigidity required for a wall covering material.
[0013] (Base resin layer 2) The base resin layer 2 is laminated on the paper base material 1. Note that "on the paper base material 1" refers to the upper surface of the paper base material 1 in FIG. The base resin layer 2 is laminated on the paper substrate 1 using a coating method such as knife coating, nozzle coating, die coating, lip coating, comma coating, gravure coating, rotary screen coating, or reverse roll coating. The base resin layer 2 may be provided on the upper surface of the paper substrate 1 in the form of a sheet or in the form of a picture pattern.
[0014] The base resin layer 2 is mainly composed of an aqueous emulsion resin, such as a vinyl chloride resin, etc. The resin that becomes the base resin layer 2 contains an inorganic filler. The coating amount of the base resin layer 2 is 80 [g / m 2 ] or more 230[g / m 2 When the main component of the base resin layer 2 is vinyl chloride resin, the coating amount of the base resin layer 2 is limited by the degree of polymerization of the vinyl chloride resin.
[0015] In order to provide the wallpaper 10 with fire retardant properties, the total weight of the paper base material 1 and the base resin layer 2 is set to 200 [g / m 2 ] or less. A foaming agent is mixed into the base resin layer 2, which is a foamed resin layer, and foamed by heat treatment. Note that a foaming agent does not have to be mixed into the base resin layer 2. Here, a case where a foaming agent is mixed is described.
[0016] The expansion ratio of the base resin layer 2 is set within a range of 2 to 8 times. In this embodiment, as an example, a case where the expansion ratio of the base resin layer 2 is set within a range of 4 to 6 times will be described. The expansion ratio here is expressed as the value of (thickness of resin before foaming) / (thickness of resin after foaming). The thickness of the resin after foaming refers to the thickness at the point after foaming and before processing that changes the thickness of the base resin layer 2 is performed.
[0017] By setting the application amount and foaming ratio of the base resin layer 2 to the above values, it is possible to form a wallpaper 10 that has sufficient volume to obtain unevenness hiding properties and has excellent surface strength. Resins that can be used in the form of an aqueous emulsion, such as vinyl chloride resins and polyolefin resins, can be used as the material for the base resin layer 2. In addition, it is particularly preferable to use at least one type of ethylene copolymer (hereinafter sometimes referred to as "ethylene copolymer"), which contains ethylene and a component other than ethylene as monomers, as the material for the base resin layer 2.
[0018] Furthermore, ethylene-vinyl acetate copolymer (EVA) resin, ethylene-methyl methacrylate copolymer (EMMA), and ethylene-ethyl acrylate copolymer (EEA) are preferably used as the material for the base resin layer 2. In addition, ethylene-methyl acrylate copolymer (EMA), ethylene methacrylic acid copolymer (EMAA), and ethylene-α-olefin copolymer are preferably used as the material for the base resin layer 2.
[0019] When a vinyl chloride resin is used as the material for the base resin layer 2, the degree of polymerization of the vinyl chloride resin is preferably 600 or more. This is because, by using a vinyl chloride resin for the base resin layer 2 with a degree of polymerization of 600 or more, it is possible to increase the surface strength of the wallpaper 10. As described above, the base resin layer 2 is formed using a thermoplastic resin containing at least one of vinyl chloride resin, polyolefin resin, and ethylene-vinyl acetate copolymer resin.
[0020] Furthermore, a plasticizer, a foaming agent, a stabilizer (foaming stabilizer), a viscosity reducer, other organic additives, and inorganic powders are appropriately mixed into the base resin layer 2 depending on the application. Examples of inorganic powders include calcium carbonate, aluminum hydroxide, magnesium hydroxide, quartz sand, talc, silicas, magnesium silicate, zinc borate, titanium dioxide, and the like. The inorganic powder is added in an amount of, for example, 40 to 150 parts per 100 parts of resin. If the amount of inorganic powder added exceeds 150 parts per 100 parts of resin, the non-flammable performance will increase, but the sense of volume may decrease.
[0021] The foaming agent and stabilizer to be mixed into the base resin layer 2 will be described below. (foaming agent) As the foaming agent, for example, a thermally expandable microcapsule foaming agent, azo-based, hydrazide-based, nitroso-based, ADCA (azodicarbonamide foaming agent), sodium bicarbonate, or other foaming agents commonly used in known foam cosmetic sheets can be used.
[0022] As the foaming agent, a thermally expandable microcapsule foaming agent is preferred from the viewpoint of performance (foaming ratio, strength). When ADCA and sodium bicarbonate are used as the foaming agent, for example, the ratio of ADCA to sodium bicarbonate is 3:1 to 1:3, and the total of the two types is within the range of 1 to 4 parts per 100 parts of the vinyl chloride resin. This makes it possible to ensure the foaming ratio and prevent the foam surface from becoming rough.
[0023] The amount of foaming agent added depends on the thickness and expansion ratio of the base resin layer 2, but is preferably in the range of 1 to 20 parts by weight, and more preferably 5 to 15 parts by weight, per 100 parts by weight of resin.
[0024] (Stabilizer) As the stabilizer, for example, two types of stabilizers (barium salt type and zinc salt type) are mixed in a ratio of 1:4 to 4:1, and the total of the two types is within the range of 1 to 4 parts per 100 parts of the vinyl chloride resin. This makes it possible to impart thermal stability and increase the foam thickness.
[0025] (Pattern printing layer 3) The picture-printed layer 3 is a layer having a first picture-forming portion 3a and a second picture-forming portion 3b formed between the first picture-forming portions 3a, and the first picture-forming portion 3a and the second picture-forming portion 3b form the same plane and are laminated on the base resin layer 2. A predetermined picture is formed by printing the first picture-forming portion 3a and the second picture-forming portion 3b. Note that "on the base resin layer 2" refers to the upper surface of the base resin layer 2 in FIG. 1. The first pattern forming portion 3a is formed using, for example, printing ink (non-foaming ink), foaming ink mainly composed of water-based emulsion resin, foaming ink mainly composed of vinyl chloride paste resin, or the like.
[0026] The first pattern forming portion 3a is formed by laminating on the base resin layer 2 using a method such as calendar molding, coating, gravure printing, screen printing, flexographic printing, or ink jet printing.
[0027] The first picture forming portion 3a is provided in the form of a sheet or a picture pattern. A pearl ink pattern layer may be printed on the base resin layer 2 on the same plane as the picture printed layer 3. The first picture forming portion 3a and the surface protective layer 4 are set to have a gloss difference, and the first picture forming portion 3a is set to have a glossiness higher than that of the surface protective layer 4. The glossiness of the first picture forming portion 3a here refers to the glossiness of the first picture forming portion 3a laminated on the base resin layer 2. In other words, the glossiness of the first picture forming portion 3a reflects the glossiness of the base resin layer 2 on which the first picture forming portion 3a is laminated, and in this embodiment, since the glossiness of the base resin layer 2 is adjusted by heating as described below, the gloss difference between the first picture forming portion 3a and the surface protective layer 4 is determined by the heating temperature, the glossiness of the base resin layer 2 obtained by this heating, the glossiness of the first picture forming portion 3a laminated on the base resin layer 2, and the glossiness of the surface protective layer 4. The magnitude of the gloss difference between the first picture forming portion 3a and the surface protective layer 4 may be such that a design sense can be obtained by the gloss difference and a three-dimensional design sense or the like can be obtained, and is set to, for example, about 2 to 30 in terms of the gloss value at 60° incidence measured by a specular gloss measurement method in accordance with JIS Z-8741.
[0028] The second picture forming portion 3b has a picture formed thereon and has a pattern with a different density from that of the first picture forming portion 3a. The first picture forming portion 3a and the second picture forming portion 3b, which have different densities, form the same plane, so that a predetermined picture is formed.
[0029] (Surface protective layer 4) The surface protective layer 4 is partially formed on the picture-printed layer 3. Note that "on the picture-printed layer 3" refers to the upper surface of the picture-printed layer 3 in FIG. 1. The surface protective layer 4 is made of a matte resin layer, which is a resin layer to which a matte coating agent for a matte finish is added. The surface protective layer 4 is formed only in a position that overlaps with the second picture-forming portion 3b when viewed from above. In the area where the surface protective layer 4 is not formed, the first picture-forming portion 3a is exposed, and the step between the first picture-forming portion 3a and the surface protective layer 4 forms an uneven surface on the surface of the wallpaper 10.
[0030] The surface protective layer 4 is formed at a position overlapping the second pattern forming portion 3b in top view, so that the second pattern forming portion 3b is synchronized with the surface protective layer 4. This allows the pattern of the second pattern forming portion 3b to be expressed both visually and tactilely. The surface protection layer 4 is formed by laminating on the picture-printed layer 3 using a method such as gravure printing, knife coating, nozzle coating, die coating, lip coating, or comma coating.
[0031] The surface protective layer 4 is formed of a transparent or semi-transparent material (resin) to such an extent that the pattern of the second pattern forming portion 3b can be seen through the surface protective layer 4. For example, a thermosetting resin is preferable as the material of the surface protective layer 4, i.e., the matte resin layer. For example, in consideration of the adhesiveness with the pattern printing layer 3, it is preferable to use a mixture of a thermosetting resin (binder) having a urethane bond such as a two-component curing urethane resin, a matte coating agent such as silica particles, and synthetic resin beads. The matte agent is added to reduce the gloss of the surface protective layer 4, so that a gloss difference occurs between the surface protective layer 4 and the first pattern forming portion 3a.
[0032] In this way, the surface protective layer 4 is formed of a thermosetting resin having a urethane bond, that is, a resin that is not affected by the gloss of the lower layer (the second pattern forming portion 3b), so that a difference in gloss occurs between the surface protective layer 4 and the first pattern forming portion 3a. This allows a visual three-dimensional effect to be appropriately expressed. In addition, the thermosetting resin having a urethane bond has a high hardness, which improves the scratch resistance of the wallpaper 10.
[0033] The silica particles are preferably contained in an amount of 5% by mass or more based on the total mass of the thermosetting resin. This allows the gloss of the surface protective layer 4 to be sufficiently reduced, and the gloss difference between the surface protective layer 4 and the first pattern forming portion 3a to be increased. The upper limit of the silica particles is set to 35% by mass or less based on the total mass of the thermosetting resin. As the synthetic resin beads, for example, acrylic resin beads with high transparency can be used. This improves the transparency of the surface protective layer 4, and allows the pattern of the pattern-printed layer 3 for imparting a design to be more clearly seen through. The average particle size of the synthetic resin beads is 30 μm or more. In addition, ethyl acetate and n-butyl acetate can be used as the solvent.
[0034] Furthermore, the surface of the surface protection layer 4 has a maximum height Rmax value of 30 μm or more as measured by a contact roughness meter, which allows a more appropriate three-dimensional feel to be obtained by touch. In this embodiment, a thermosetting resin is used as the binder of the surface protective layer 4, but other configurations can be adopted. For example, an ionizing radiation curable resin may be used. As the ionizing radiation curable resin, for example, an ultraviolet curable resin is preferable. As the ultraviolet curable resin, for example, (meth)acrylic resin, silicone resin, polyester resin, urethane resin, amide resin, and epoxy resin can be used. This can improve the hardness of the surface protective layer 4, that is, the outermost surface layer of the wallpaper 10, and can improve the surface physical properties of the wallpaper 10, such as abrasion resistance, scratch resistance, and solvent resistance. In addition, for example, a mixture of a thermosetting resin and an ionizing radiation curable resin may be used as the binder.
[0035] In addition, in this embodiment, an example has been shown in which synthetic resin beads are added to a thermosetting resin as the surface protection layer 4, but, for example, a configuration in which an inorganic compound filler is added instead of the synthetic resin beads, a configuration in which both synthetic resin beads and an inorganic compound filler are added, or a configuration in which at least one of synthetic resin beads and an inorganic compound filler is added may be used.
[0036] The shape of the surface protection layer 4 is not particularly limited, and may be a regularly arranged fixed shape such as a circle, a square, or a hexagon, or may be an irregular pattern shape. It may also be a shape that matches the pattern of the pattern-printed layer 3, which makes the pattern look more realistic. The amount of resin applied to form the surface protective layer 4 is 4 g / m 2 ] or more 6[g / m 2 It is preferable that the coating amount is within the range of 4 [g / m 2 If it is less than 6[g / m 2 If the thickness is more than 0.5 μm, it becomes difficult to satisfy the requirement for non-combustibility. The thickness of the surface protective layer 4 is preferably within the range of, for example, 0.5 μm to 30 μm.
[0037] <Wallpaper manufacturing method> A method for manufacturing the wallpaper 10 will now be described. First, a resin that will become the base resin layer 2 is applied to one surface of the paper substrate 1 by, for example, a coating method. 2 ] or more 230[g / m 2 ] is applied so as to have a thickness within the range below, thereby forming the base resin layer 2. Next, the first picture forming portion 3a and the second picture forming portion 3b are formed on the base resin layer 2 by gravure printing using water-based ink.
[0038] Next, for example, a matte resin containing synthetic resin beads is used to form a surface protective layer 4 only on the second pattern forming portion 3b by gravure printing. The laminate consisting of the paper substrate 1, base resin layer 2, picture printed layer 3 and surface protective layer 4 is then heated to a surface temperature in the range of 130° C. to 200° C., and then cooled and dried. In this way, wallpaper 10 is formed.
[0039] Here, when the laminate consisting of the paper base material 1, base resin layer 2, picture print layer 3, and surface protection layer 4 is heated to a surface temperature in the range of 130° C. to 200° C., the gloss (glossiness) of the base resin layer 2 increases. If the surface temperature is below 130° C., the gloss does not increase significantly, and conversely, if the surface temperature is 200° C. or higher, in the case where a foaming agent is mixed in the base resin layer 2, the foaming material becomes overfoamed, degrading the design properties.
[0040] The increase in gloss of the base resin layer 2 is equivalent to an increase in gloss of the first pattern forming portion 3a, and as a result, the difference in gloss between the first pattern forming portion 3a and the surface protective layer 4 increases, thereby enhancing the gloss matte design feel.
[0041] (effect) (1) In this embodiment, a picture-printed layer 3 including a first picture-forming portion 3a and a second picture-forming portion 3b that are flush with each other is formed, and a gloss difference is generated between the first picture-forming portion 3a and the surface protective layer 4. The surface protective layer 4 is arranged to overlap only with the second picture-forming portion 3b in a top view and to be in harmony with the second picture-forming portion 3b. Therefore, due to the gloss difference between the surface protective layer 4 and the first picture-forming portion 3a, a textured feel can be created on the surface side of the wallpaper 10, which is the surface of the surface protective layer 4 side of the wallpaper 10. Therefore, for example, a three-dimensional design can be obtained without using embossing, and the surface protective layer 4 and the second picture-forming portion 3b are in harmony with each other, so that a three-dimensional design having a gloss matte design can be easily obtained. (2) Furthermore, since the surface protective layer 4 is formed using a resin layer to which a matte coating agent such as silica particles has been added, the glossiness of the surface protective layer 4 is reduced, and the gloss difference between the surface protective layer 4 and the first pattern forming portion 3a can be made larger, thereby achieving an even more three-dimensional design feel. (3) When applying the resin that will become the surface protective layer 4 to the upper surface of the picture-printed layer 3, the amount of application is set to 4 [g / m 2 ] or more 6[g / m 2 ]Because the range is set as follows, a sufficient matte finish can be obtained. (4) Since at least one of synthetic resin beads and inorganic compound fillers is mixed into the surface protection layer 4, it is possible to give a three-dimensional design feeling not only visually but also tactilely. Therefore, it is possible to give a three-dimensional design feeling while maintaining the visual three-dimensional feeling by the gloss matte matching without applying embossing. (5) Since the second pattern forming portion 3b and the surface protective layer 4 are formed in harmony with each other, even if a foaming agent is added to the base resin layer 2, the synchronization between the second pattern forming portion 3b and the surface protective layer 4 and the loss of the gloss matte design are prevented, thereby realizing wallpaper 10 with a good gloss matte design. (6) Since the transparent or semi-transparent surface protection layer 4 is provided on the pattern-printed layer 3, the pattern of the pattern-printed layer 3 can be seen through. (7) The surface protective layer 4 contains a thermosetting resin having a urethane bond, and further contains a matte coating agent such as silica particles, which improves the adhesion of the surface protective layer 4 to the picture-printed layer 3, the deformation conformability of the wallpaper 10, and the scratch resistance. (8) After the surface protective layer 4 is formed on the pattern-printed layer 3, the surface is heated to a temperature in the range of 130° C. to 200° C. This improves the glossiness of the base resin layer 2, which in turn improves the glossiness of the first pattern-forming portion 3a and increases the gloss difference between the first pattern-forming portion 3a and the surface protective layer 4, thereby enhancing the matte gloss feel of the wallpaper 10.
[0042] In this way, by improving the gloss of the base resin layer 2, the gloss difference between the first picture forming portion 3a and the surface protective layer 4 is increased, so that in order to improve the gloss of the first picture forming portion 3a, it is not necessary to provide, for example, a separate gloss layer on the first picture forming portion 3a. Therefore, wallpaper with a matte gloss feeling can be produced by a simpler manufacturing process, and costs can be reduced accordingly. EXAMPLES
[0043] Examples and comparative examples of this embodiment are shown below, but this embodiment is not limited to the following.
[0044] Example 1 Paper base material 1: 65 g / m 2 A plain paper with a thickness of 110 μm (for example, “WK665IHT” manufactured by KJ Specialty Paper Co., Ltd.) was used. For the base resin layer 2, for example, "PQLT" manufactured by Shin-Daiichi Vinyl Corporation is used as a vinyl chloride resin, to which 55 parts of a plasticizer and 150 parts of a filler are added, and the paste is applied in an amount of 200 [g / m 2 ] was applied to the paper base material 1 by a coating method. The picture printed layer 3 consisting of the first picture forming portion 3a and the second picture forming portion 3b was formed by gravure ink using a water-based ink.
[0045] The surface protective layer 4 is made of a matte resin (e.g., silica), and is formed by gravure printing so as to be in sync with the second pattern forming portion 3b. At this time, the coating amount was 4 g / m 2 In addition, synthetic resin beads (for example, acrylic beads) were added to the matte resin. After printing the matte resin that would become the surface protective layer 4, the surface was heated to a surface temperature of 170°C, and then cooled and dried to form the wallpaper 10. This caused a gloss difference to appear between the first pattern forming portion 3a and the surface protective layer 4.
[0046] Example 2 The amount of the matte resin applied to form the surface protective layer 4 is set to 3 [g / m 2 A wallpaper 10 was formed in the same manner as in Example 1, except that the first pattern forming portion 3a and the surface protective layer 4 were made to have a difference in gloss. Example 3 The amount of the matte resin applied to form the surface protective layer 4 is set to 7 [g / m 2A wallpaper 10 was formed in the same manner as in Example 1, except that the first pattern forming portion 3a and the surface protective layer 4 were made to have a difference in gloss.
[0047] Example 4 Wallpaper was formed in the same manner as in Example 1, except that after printing the matte resin layer that would become the surface protective layer 4, the surface was heated to a temperature of 120° C. This resulted in a difference in gloss between the first pattern forming portion 3a and the surface protective layer 4. Example 5 Wallpaper was formed in the same manner as in Example 1, except that after printing the matte resin layer that would become the surface protective layer 4, the surface was heated to a temperature of 210° C. This resulted in a difference in gloss between the first pattern forming portion 3a and the surface protective layer 4.
[0048] Example 6 A wallpaper was formed in the same manner as in Example 1, except that no synthetic resin beads were added to the matte resin that constitutes the surface protective layer. This resulted in a difference in gloss between the first pattern forming portion 3a and the surface protective layer 4. Example 7 The coating weight of the base resin layer is 60 [g / m 2 A wallpaper was formed in the same manner as in Example 1, except that the first pattern forming portion 3a and the surface protective layer 4 were made to have a difference in gloss. Example 8 The coating weight of the base resin layer is 250 [g / m 2 A wallpaper was formed in the same manner as in Example 1, except that the first pattern forming portion 3a and the surface protective layer 4 were made to have a difference in gloss.
[0049] Comparative Example 1 The coating weight of the base resin layer is 70 [g / m 2 ], and the coating amount of the surface protection layer was 3 [g / m 2 After printing the matte resin layer that would become the surface protective layer 4, the wallpaper was heated to a surface temperature of 110° C. in the same manner as in Example 1. In this case, no difference in gloss occurred between the first picture-forming portion 3a and the surface protective layer 4.
[0050] (Reference example 1) As Reference Example 1, wallpaper 10' having the configuration shown in Fig. 2 was formed. The wallpaper 10' shown in Fig. 2 is the same as the wallpaper 10 shown in Fig. 1 except that it has a first surface protective layer 4a and a second surface protective layer 4b as surface protective layers. The same parts are given the same reference numerals and detailed explanations thereof will be omitted.
[0051] The wallpaper 10' shown in Figure 2 is formed by laminating a paper base material 1, a base resin layer 2, a picture-printed layer 3, and a surface protective layer 4' in this order. The picture-printed layer 3 comprises a first picture-forming portion 3a and a second picture-printed portion 3b. The surface protective layer 4' comprises a first surface protective layer 4a and a second surface protective layer 4b. The first surface protective layer 4a is formed so as to cover the entire upper surface of the picture-printed layer 3. The second surface protective layer 4b is formed on the first surface protective layer 4a and is formed so as to overlap only with the second picture-forming portion 3b in a top view so as to be in harmony with the second picture-printed portion 3b in a top view.
[0052] The wallpaper 10' in the reference example 1 is formed in the following procedure. Paper base material 1: 65 g / m 2 A plain paper with a thickness of 110 μm (for example, “WK665IHT” manufactured by KJ Specialty Paper Co., Ltd.) was used. For the base resin layer 2, for example, "PQLT" manufactured by Shin-Daiichi Vinyl Corporation is used as a vinyl chloride resin, to which 55 parts of a plasticizer and 150 parts of a filler are added, and the paste is applied in an amount of 200 [g / m 2 ] was applied to the paper base material 1 by a coating method.
[0053] The picture printed layer 3 consisting of the first picture forming portion 3a and the second picture forming portion 3b was formed by gravure ink using a water-based ink. The first surface protective layer 4a is made of a matte resin, and after the pattern printed layer 3 is formed, it is coated with a coating amount of 3 [g / m2 by gravure printing. 2The second surface protective layer 4b is made of a gloss resin with synthetic resin beads (e.g., acrylic beads) added thereto, and after the first surface protective layer 4a is formed, it is printed on the second pattern forming portion 3b by gravure printing in synchronization with the second pattern forming portion 3b. The second surface protective layer 4b is formed with a coating amount of 3 [g / m 2 ] was molded into the shape. Thereafter, the surface was heated to a temperature of 170° C., and then cooled and dried to form wallpaper 10′. As a result, a gloss difference occurred between the surface protective layer 4 and the first pattern forming portion 3a.
[0054] (Evaluation method and criteria) The wallpapers of Examples 1 and 2, Comparative Examples 1 to 5, and Reference Example 1 were each evaluated by the following method. (1) Glossy matte design A sensory test was conducted on 10 panelists to evaluate the glossy and matte design of the wallpaper. The evaluation criteria are as follows: ◎: 9-10 people who thought it was good 〇: 7-8 people who thought it was good △: 1 to 6 people who thought it was good ×: 0 people thought it was good
[0055] (2) Three-dimensional design (touch) A sensory test was conducted on 10 examiners to evaluate the three-dimensional design (touch) of the wallpaper. The evaluation criteria are as follows: ◎: 9-10 people who thought it was good 〇: 7-8 people who thought it was good △: 1 to 6 people who thought it was good ×: 0 people thought it was good
[0056] (3) Concealment of unevenness A circular sticker with a thickness of 100 μm and a diameter of 20 mm was attached to a semi-fireproof gypsum board (thickness 9.5 mm), and the amount of glue applied when attaching it to the gypsum board was 20 g / m 2Wallpaper with glue applied so that the solid content was 100% was applied to the plaster board. Then, it was confirmed whether the circular sticker on the base could be clearly detected. The evaluation criteria are as follows: ○: Cannot be detected clearly △: Somewhat detectable. ×: Clearly detectable
[0057] (4) Non-flammable performance For each of the wallpapers obtained in the examples, comparative examples, and reference examples, a cone calorimeter C3 (a combustion tester manufactured by Toyo Seiki Seisakusho Co., Ltd.) was used to carry out a heat generation test for non-combustible materials (50 [kW / m 2 ] for 20 minutes). The evaluation criteria are as follows: ○: Calories burned are 6.0 [MJ] or less. △: Calories burned are greater than 6.0 [MJ] and less than 7.2 [MJ] ×: Calories burned are greater than 7.2 [MJ].
[0058] (Evaluation Results) The evaluation results are shown in Table 1 below. The overall "judgment" index based on the judgment results of each evaluation item is as follows: ⊚: The results of all evaluation items are '⊚' or '○'. ○: There are no “×” marks for any evaluation item, and there are two or more “◎” marks. △: There are no "x" marks for any evaluation item and only one "△" mark. ×: There is even one “×”.
[0059] [Table 1]
[0060] From Table 1, it was confirmed that if there is a gloss difference in the formed wallpaper, all evaluation items are satisfied, but if there is no gloss difference, the gloss matte design and three-dimensional design cannot be obtained, and the unevenness hiding ability and fire resistance are also reduced. In addition, the coating amount of the surface protective layer is 4 to 6 [g / m 2 ], a gloss difference is generated and a good gloss matte design can be obtained, but the coating amount of the surface protective layer is 4 to 6 [g / m 2 ] range, the gloss matte design impression is reduced.
[0061] Furthermore, after forming the surface protective layer, if the heating temperature is within the range of 130°C or more and 200°C or less, a gloss difference occurs and a good gloss matte design can be obtained, but if the heating temperature is outside the range of 130°C or more and 200°C or less, the gloss matte design is reduced. Furthermore, it is apparent that when synthetic resin beads are not added to the surface protective layer, the three-dimensional design feeling is reduced.
[0062] In addition, the coating amount of the base resin layer is 80 to 230 [g / m 2 ] range, 80 [g / m 2 If it is less than 230 [g / m 2 ], it can be seen that the non-flammable performance decreases. Furthermore, the wallpaper of Example 1 can exhibit the same properties as when a gloss resin is laminated, even though the gloss resin is not laminated as in Reference Example 1. In other words, the manufacturing process of the wallpaper can be simplified, and the cost can be reduced accordingly.
[0063] The present invention can have the following configurations, for example. (1) This wallpaper has a base resin layer, a picture printing layer having a picture printed thereon, and a surface protective layer laminated in that order on a paper base material, the picture printing layer having a first picture forming portion and a second picture forming portion which are flush with each other, the surface protective layer overlapping only one of the first picture forming portion and the second picture forming portion in a top view and being positioned in sync with the one picture forming portion, and there is a gloss difference between the other of the first picture forming portion and the second picture forming portion and the surface protective layer. (2) The wallpaper according to (1) above, wherein the surface protective layer is a resin layer to which a matte coating agent has been added. (3) The coating amount of the surface protective layer is 4 [g / m 2 ] or more 6[g / m 2 ] The wallpaper according to (1) or (2) above, characterized in that the thickness is within the range below. (4) The wallpaper according to any one of the above (1) to (3), wherein the base resin layer is a layer containing at least one of polyvinyl chloride resin, polyolefin resin, and ethylene-vinyl acetate copolymer resin. (5) The wallpaper according to any one of (1) to (4) above, wherein the surface protective layer contains at least one of synthetic resin beads and an inorganic compound filler. (6) The paper base material has a basis weight of 50 [g / m 2 ] or more 100[g / m 2 ] or less and a thickness in the range of 80 [μm] to 150 [μm]. (7) forming a base resin layer containing at least one of vinyl chloride resin, polyolefin resin, and ethylene-vinyl acetate copolymer resin on one surface of a paper substrate; forming a picture-printed layer including a first picture-forming portion and a second picture-forming portion that are flush with each other on the base resin layer; forming the surface protective layer on one of the first and second picture forming portions so as to overlap and be in phase with only the one of the first and second picture forming portions when viewed from above; a step of heating the laminate in which the paper base material, the base resin layer, the picture print layer, and the surface protective layer are formed, so that the surface temperature of the laminate is within a range of 130 [°C] to 200 [°C]; A method for manufacturing wallpaper, comprising the steps of: cooling and drying the laminate after the heating step. [Explanation of symbols]
[0064] 1 Paper base material 2 Base resin layer 3. Pattern printing layer 3a First pattern forming section 3b Second pattern forming part 4 Surface protective layer 4a First surface protective layer 4b Second surface protection layer 10, 10′ wallpaper
Claims
1. A wallpaper in which a base resin layer, a pattern printed layer having a pattern printed thereon, and a surface protective layer are laminated in this order on a paper substrate, The pattern-printed layer has a first pattern-forming portion and a second pattern-forming portion that are flush with each other, the surface protection layer is arranged to overlap only one of the first picture forming portion and the second picture forming portion in a top view and to be synchronized with the one picture forming portion; A wallpaper characterized in that there is a gloss difference between the other of the first picture forming portion and the second picture forming portion and the surface protective layer.
2. 2. The wallpaper according to claim 1, wherein the surface protective layer is a resin layer to which a matte coating agent has been added.
3. The coating amount of the surface protective layer is 4 [g / m 2 ] or more 6 [g / m 2 2. The wallpaper according to claim 1, wherein the thickness of the wallpaper is within a range of 0.1 to 1.0 mm.
4. 2. The wallpaper according to claim 1, wherein the base resin layer is a layer containing at least one of a polyvinyl chloride resin, a polyolefin resin, and an ethylene-vinyl acetate copolymer resin.
5. 2. The wallpaper according to claim 1, wherein the surface protective layer contains at least one of synthetic resin beads and an inorganic compound filler.
6. The paper base material has a basis weight of 50 [g / m 2 ] or more 100 [g / m 2 2. The wallpaper according to claim 1, wherein the thickness of the wallpaper is within a range of 80 μm to 150 μm.
7. forming a base resin layer containing at least one of vinyl chloride resin, polyolefin resin, and ethylene-vinyl acetate copolymer resin on one surface of a paper substrate; forming a picture-printed layer including a first picture-forming portion and a second picture-forming portion that are flush with each other on the base resin layer; forming a surface protective layer on one of the first and second picture forming portions so as to overlap and be in phase with only the one of the first and second picture forming portions when viewed from above; a step of heating the laminate obtained by laminating the paper base material, the base resin layer, the picture print layer, and the surface protection layer so that the surface temperature of the laminate is within a range of 130 [°C] to 200 [°C]; A method for manufacturing wallpaper, comprising the steps of: cooling and drying the laminate after the heating step.
Citation Information
Patent Citations
Electroconductive fiber
JP1982042972A
Gloss mat decorative sheet
JP2018122574A