Curable resin composition for film capacitors and film capacitors
The curable resin composition for film capacitors, using a high molecular weight maleimide resin and organic compounds with allyl groups and isocyanuric rings, addresses the limitations of thermoplastic resins by providing enhanced dielectric properties and mechanical strength, enabling reliable performance in high-temperature and high-voltage environments.
Patent Information
- Application Number
- JP2023085260
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing film capacitors face challenges with thermoplastic resins that have high moisture absorption, low dielectric breakdown voltage, and poor handling properties, making them unsuitable for high-temperature and high-voltage applications.
A curable resin composition comprising a maleimide resin with a number average molecular weight of 3,000 or more, an organic compound with allyl groups and isocyanuric rings, and a polymerization initiator, which results in a cured product with a dielectric constant of 2.7 or more, dielectric loss tangent less than 0.006, and a dielectric breakdown voltage of 220V/μm or more, even after 180° bending.
The composition provides a film capacitor with balanced dielectric properties, mechanical strength, and heat resistance, suitable for high-temperature and high-voltage applications.
Smart Images

Figure 2024168514000026 
Figure 2024168514000027 
Figure 2024168514000028
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin composition for a film capacitor and a film capacitor. [Background technology]
[0002] Film capacitors are capacitors that use plastic film as a dielectric, and have advantages such as excellent high-frequency characteristics, temperature characteristics, high-precision capacitance, and long life, and are used in many electrical devices and electronic circuits. In recent years, they have come to be used not only in power electronics, but also in automotive applications (Patent Documents 1 and 2).
[0003] The dielectric materials used in film capacitors are generally thermoplastic resins (Non-Patent Document 1). PET (polyethylene terephthalate) and PP (polypropylene) are lead wire type dielectric materials; in the past, PET was used for general purposes as it was small and low-cost, while PP, with its excellent high-frequency characteristics, was used for high frequencies / high currents, but now PP is widely used due to its advantages of high safety, high moisture resistance, and low cost. PPS (polyphenylene sulfide) and PEN (polyethylene naphthalate) are used in surface mount film capacitors due to their high heat resistance (for example, Patent Documents 3 and 4).
[0004] These various types of thermoplastic resin films are used, each with its own advantages and disadvantages. PET has a high moisture absorption rate and a relatively low dielectric breakdown voltage. PP has insulating properties and a low dielectric tangent, but its glass transition temperature is low, making it difficult to use stably for long periods in environments above 120°C, and it also has poor reflow resistance. PPS has high heat resistance, but a low dielectric breakdown voltage, and PEN has high moisture absorption and is highly environmentally dependent.
[0005] If heat resistance is the focus, the use of heat- or light-curable resin compositions can be considered; however, in general, there are almost no curable resin composition films that have well-balanced dielectric properties, low moisture absorption, and high dielectric breakdown voltage in thin films. In addition, they have been hardly considered due to their poor handling properties as films. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] : JP 2020-96073 A [Patent Document 2] : JP 2022-110539 A [Patent Document 3] : JP 2022-164735 A [Patent Document 4] : JP 2023-2364 A [Non-patent literature]
[0007] [Non-Patent Document 1] Rubycon Corporation technical document (https: / / www.rubycon.co.jp / wp-content / uploads / products-film / film-technical-note.pdf) DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a film capacitor using a curable resin composition for use in a dielectric film of a film capacitor and a film made of the cured product thereof. [Means for solving the problem]
[0009] The present invention has been made to solve the above-mentioned problems, and provides a film capacitor using the following curable resin composition and a film made of the cured product thereof.
[0010] That is, the present invention provides: (A) a maleimide resin having a number average molecular weight of 3,000 or more; (B) an organic compound having one or more allyl groups and one or more isocyanuric rings in one molecule; and (C) Polymerization initiator A curable resin composition for a film capacitor comprising: The present invention provides a curable resin composition for a film capacitor, the cured product of which satisfies the following properties: 1) Dielectric constant of 2.7 or more at 1 kHz and 25°C 2) Dielectric tangent at 1kHz and 25℃ is 0.006 or less 3) No damage occurs even when bent 180 degrees 10 times at a thickness of 5 μm 4) The dielectric breakdown voltage at 25℃ and 150℃ is 220V / μm or more.
[0011] When the maleimide resin, which is component (A), has a number average molecular weight of 3,000 or more, the glass transition temperature is high, and therefore the curable resin composition for film capacitors has excellent processability and formability into a film before and after curing, and the film itself also has good handleability.
[0012] Because the organic compound of component (B) has an isocyanuric ring, the mechanical properties and dielectric characteristics after curing are improved, and the cured product exhibits high voltage resistance.
[0013] By using such a curable resin composition for film capacitors, it is possible to obtain a cured product for film capacitors having 1) a relative dielectric constant of 2.7 or more at 1 kHz and 25°C, 2) a dielectric dissipation factor of 0.006 or less at 1 kHz and 25°C, 3) no damage even when bent 180° 10 times at a thickness of 5 μm, and 4) a dielectric breakdown voltage of 220 V / μm or more at 25°C and 150°C. From the cured product having the above properties, it is possible to obtain a film capacitor having a good balance of excellent properties such as relative dielectric constant, dielectric dissipation factor, physical strength, and heat resistance.
[0014] The maleimide resin of the component (A) preferably contains an aromatic bismaleimide represented by the following general formula (1) and / or (2). [ka] (In the formula, X 1 are independently expressed by the following formula: [ka] and l is a number from 1 to 40. [ka] (In the formula, X 2 are independently X in the above formula 1 m is a number from 1 to 50, and n is a number from 1 to 50. 1 and A 2 are each independently a divalent group represented by the following general formula (3) or the following general formula (4). [ka] (In the formula, X 3 are independently represented by the above formula X 1 and X 2 R is a divalent group having the same structure as 1 are independently a hydrogen atom, a chlorine atom, or an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 6 carbon atoms. [ka] (In the formula, X 3 denotes the same thing as above.) The component (A) is preferably an aromatic bismaleimide represented by the above formula (1) and / or (2).
[0015] The aromatic bismaleimide compounds represented by the above general formulas (1) and / or (2) give films with good mechanical properties both before and after curing, and in particular with high mechanical strength, which makes them easy to handle. In addition, they have high compatibility with the above component (B), and can give cured products for film capacitors with uniform properties from location to location.
[0016] The component (B) is preferably an organic compound having two or more allyl groups in one molecule.
[0017] The organic compound of the component (B) has two or more allyl groups in one molecule, and thus has better crosslinking properties.
[0018] The blending amount of the component (B) is preferably 5 parts by mass to 40 parts by mass per 100 parts by mass of the component (A).
[0019] If the amount of the (B) component is 5 parts by mass or more per 100 parts by mass of the (A) component, the high dissolution viscosity of the (A) component prevents poor solvent removal during the drying process described below, and reduces the occurrence of poor appearance. If the amount of the (B) component is 40 parts by mass or less per 100 parts by mass of the (A) component, the film is easy to handle before and after curing, tack is unlikely to occur in the film before curing, and the strength of the film after curing does not decrease significantly.
[0020] The (C) polymerization initiator is preferably a thermal radical polymerization initiator and / or a photocuring initiator.
[0021] From the viewpoint of promoting crosslinking of the component (A) and the component (B), a thermal radical polymerization initiator and / or a photocuring initiator is preferred, and among these, an organic peroxide is more preferred.
[0022] The present invention provides a film-shaped cured resin for film capacitors having a thickness of 1 to 20 μm, obtained by curing the above-mentioned curable resin composition for film capacitors.
[0023] The capacitance can be increased by reducing the thickness of the film for a film capacitor. The thickness of the film is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less.
[0024] The present invention provides a film capacitor comprising the above-mentioned cured resin for a film capacitor.
[0025] By using the above-mentioned cured resin for film capacitors, it is possible to obtain a film capacitor that exhibits well-balanced properties in terms of dielectric constant, dielectric loss tangent, mechanical strength, and dielectric breakdown voltage. Effect of the Invention
[0026] The curable resin composition used in the dielectric film of the film capacitor of the present invention has excellent heat resistance and other properties required for a dielectric film of a film capacitor, and is therefore useful as a dielectric film for a film capacitor. [Brief description of the drawings]
[0027] [Figure 1] 1 is a schematic diagram of a film capacitor element used for an exterior cracking test, a withstand voltage test, and an insulation resistance test. [Diagram 2] FIG. 2 is a cross-sectional view of the film capacitor element of FIG. [Diagram 3] FIG. 2 is a schematic diagram of a current extraction electrode of a film capacitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The present invention will be described in detail below, but the present invention is not limited thereto. Means of the Invention The present inventors have conducted extensive research to solve the above problems and have found that the following resin composition can achieve the above object, thereby completing the present invention.
[0029] That is, the present invention provides: (A) a maleimide resin having a number average molecular weight of 3,000 or more; (B) an organic compound having one or more allyl groups and one or more isocyanuric rings in one molecule; and (C) Polymerization initiator A curable resin composition for a film capacitor comprising: The curable resin composition for a film capacitor is characterized in that a cured product of the curable resin composition satisfies the following properties: 1) Dielectric constant of 2.7 or more at 1 kHz and 25°C 2) Dielectric tangent at 1kHz and 25℃ is 0.006 or less 3) No damage occurs even when bent 180 degrees 10 times at a thickness of 5 μm 4) The dielectric breakdown voltage at 25℃ and 150℃ is 220V / μm or more.
[0030] Each component of the present invention will now be described in more detail.
[0031] (A) Maleimide resin with a number average molecular weight of 3,000 or more The component (A) used in the present invention is a maleimide resin having a number average molecular weight of 3,000 or more. In general, many maleimide compounds have a number average molecular weight of 2,000 or less. Many of these maleimide compounds having a number average molecular weight of 2,000 or less have a high glass transition temperature (Tg), but they are difficult to handle due to poor processability and formability into a film before and after curing, and poor handling of the film itself due to insufficient strength. For these reasons, the present invention uses a high molecular weight maleimide resin having a number average molecular weight of 3,000 or more.
[0032] The properties of the maleimide resin of component (A) at room temperature (25°C) are not particularly limited, but the number average molecular weight (Mn) calculated using polystyrene standards by gel permeation chromatography (GPC) measurement under the following measurement conditions is 3,000 or more, more preferably 3,500 to 50,000, and particularly preferably 4,000 to 40,000. If the number average molecular weight is 3,000 or more, the resulting composition is easily formed into a film after curing and has good handleability.
[0033] [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-L TSKgel SuperHZ4000(4.6mmI.D.×15cm×1) TSKgel SuperHZ3000(4.6mmI.D.×15cm×1) TSKgel SuperHZ2000 (4.6mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 5 μL (0.2% by mass in THF solution)
[0034] Furthermore, the component (A) is preferably an aromatic bismaleimide compound represented by the following formula (1) and / or (2). By using a curable resin composition for a film capacitor containing this bismaleimide compound, not only can the mechanical properties of the resulting film be good both before and after curing, particularly the mechanical strength being high and easy to handle, but also a cured product of the curable resin composition can be obtained that has high compatibility with the component (B) described below and has uniform properties depending on the location.
[0035] [ka] (In the formula, X 1 are independently expressed by the following formula: [ka] and l is a number of 1 to 40, preferably 5 to 30. [ka] (In the formula, X 2 are independently represented by X in the above general formula (1). 1m is a number from 1 to 50, preferably from 1 to 40, and n is a number from 1 to 50, preferably from 1 to 40. 1 and A 2 are each independently represented by the following general formula (3) or the following general formula (4): [ka] (In the formula, X 3 are independently X in the above general formula (1). 1 And X in the above general formula (2) 2 R is a divalent group having the same structure as 1 are independently a hydrogen atom, a chlorine atom, or an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 6 carbon atoms. [ka] (In the formula, X 3 denotes the same thing as above.)
[0036] X in the above general formulas (1) to (3) 1 ~X 3 From the viewpoint of availability of raw materials, -CH2- and -C(CH3)2- are preferred. l is a number from 1 to 40, preferably 5 to 30, m is a number from 1 to 50, preferably 1 to 40, and n is a number from 1 to 50, preferably 1 to 40. When l, m, and n are within these ranges, a good balance is achieved between the solubility in a solution and film-forming ability of the aromatic bismaleimide compound when uncured, and the toughness and heat resistance of the obtained cured product. R 1 From the viewpoint of availability of raw materials, A is preferably a hydrogen atom or an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 3 carbon atoms. 1 and A 2 It is more preferable that they are different. The structure in the above formula (2) may be either a random type or a block type, but is preferably a block type from the viewpoint of the mechanical strength of the cured product.
[0037] The maleimide compound (A) may be used alone or in combination of two or more. The content of the component (A) in the composition of the present invention is preferably 50 to 95 mass %, more preferably 60 to 95 mass %.
[0038] (B) An organic compound having one or more allyl groups and one or more isocyanuric rings in one molecule. The component (B) used in the present invention is an organic compound having one or more allyl groups and one or more isocyanuric rings in one molecule, and is used as a crosslinking agent. Therefore, one or more, preferably two or more, allyl groups are contained in one molecule. In addition, the isocyanuric ring has high heat resistance, and not only acts to improve mechanical properties and dielectric properties after curing, but also contributes to maintaining a high voltage resistance.
[0039] Examples of the component (B) include those having an epoxy group, an acryloyl group or a carboxyl group, silicone-modified ones, and ether-modified ones. From the viewpoint of reactivity with the maleimide group and dielectric properties, alkyl diallyl isocyanurates such as triallyl isocyanurate and diallyl methyl isocyanurate are preferred.
[0040] The blend amount of the component (B) is preferably 5 parts by mass to 40 parts by mass, and more preferably 6 parts by mass to 35 parts by mass, per 100 parts by mass of the component (A). If the blending amount of component (B) is 5 parts by mass or more, the melt viscosity of component (A) does not impair the removal of the solvent during the drying step described below, and appearance defects are unlikely to occur. Also, if the blending amount of component (B) is 40 parts by mass or less, the handleability of the film before and after curing is not impaired, tack is unlikely to occur in the film before curing, and there is no risk of a significant decrease in the strength of the film after curing.
[0041] (C) Polymerization initiator The polymerization initiator of component (C) used in the present invention is added to promote the independent crosslinking reaction of the maleimide group of component (A) and the allyl group of component (B) and the crosslinking reaction between components (A) and (B). The (C) component is not particularly limited as long as it promotes the crosslinking reaction, and examples thereof include ion catalysts such as imidazoles, tertiary amines, quaternary ammonium salts, boron trifluoride amine complexes, organophosphines, and organophosphonium salts; radical polymerization initiators such as organic peroxides, hydroperoxides, and azoisobutyronitrile; and photocuring initiators such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-methyl-1-(4-(methylthio)phenyl)-2-morpholinopropanone-1, 2,4-diethylthioxanthone, and 2-ethylanthraquinone. Among these, thermal radical polymerization initiators and / or photocuring initiators are preferred from the viewpoint of promoting crosslinking between the (A) component and the (B) component, and among these, organic peroxides are more preferred. Examples of the organic peroxide include dicumyl peroxide, t-butyl peroxybenzoate, t-amyl peroxybenzoate, dibenzoyl peroxide, and dilauroyl peroxide. The polymerization initiator of the component (C) may use either a single type alone, or a combination of two or more types.
[0042] The amount of the polymerization initiator is preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the total of the components (A) and (B). If the amount of the polymerization initiator is within the range of 0.05 to 10 parts by mass, per 100 parts by mass of the total of the components (A) and (B), the balance between the heat resistance and moisture resistance of the cured product will not be impaired, and there is no risk of the curing speed during molding becoming extremely slow or fast. In addition, as is well known, the hardening speed during molding differs depending on the type of reaction initiator, and when using an organic peroxide, for example, check the half-life temperature of the organic peroxide. There is a strong correlation between the half-life temperature and the reaction initiation temperature.
[0043] Furthermore, the cured product of the thermosetting resin composition for a film capacitor of the present invention satisfies the following properties, which are very important properties for a film for a film capacitor. 1) Dielectric constant of 2.7 or more at 1 kHz and 25°C 2) Dielectric tangent at 1kHz and 25℃ is 0.006 or less 3) No damage occurs even when bent 180 degrees 10 times at a thickness of 5 μm 4) The dielectric breakdown voltage at 25℃ and 150℃ is 220V / μm or more.
[0044] The dielectric constant described in 1) is a value related to the capacitance of a capacitor. Since the capacitance of a capacitor is proportional to the dielectric constant, it is preferable that the dielectric constant is high. PP is commonly used, with a low dielectric constant of 2.2, and although it is used due to its other excellent properties, its low dielectric constant is something that needs to be improved. The present invention surpasses this.
[0045] The dielectric dissipation factor described in 2) indicates the degree of electrical energy loss in the dielectric, and as a capacitor, a lower dielectric dissipation factor is preferable. Generally, thermosetting resins have a large dielectric dissipation factor, making them difficult to use as film materials for film capacitors. The present invention has a small dielectric dissipation factor and low electrical energy loss.
[0046] The fact that the film is not damaged even when bent 180 degrees 10 times at a thickness of 5 μm as described in 3) is important for the handleability of the film in both wound and laminated film capacitor structures, and the film cannot be used if it is damaged by the above-mentioned operations. In this respect, the present invention has sufficient strength and is easy to handle.
[0047] The dielectric breakdown voltage of 220 V / μm or more at 25° C. and 150° C. described in 4) means that the dielectric of the capacitor has high voltage resistance. Generally, thermoplastic resins such as PP become very soft at high temperatures and the dielectric breakdown voltage tends to decrease, but the resin composition of the present invention has a high dielectric breakdown voltage even at 150° C., and therefore can be used in applications requiring reliability at high temperatures, such as in-vehicle applications. In general, imide groups tend to have high withstand voltages. However, polyimides are prone to hygroscopicity and are susceptible to changes in the dielectric properties mentioned above. Meanwhile, maleimide compounds tend to be less prone to hygroscopicity than polyimides, and this tendency is particularly pronounced in polymeric maleimides.
[0048] <Other additives> The curable resin composition of the present invention may contain various additives as required. Examples of other additives are listed below.
[0049] A curable resin having a reactive group capable of reacting with a maleimide group In the present invention, in addition to the component (B), a curable resin having a reactive group capable of reacting with a maleimide group may be added. The type of the curable resin is not limited, and examples thereof include various resins other than component (A), such as epoxy resins, phenolic resins, melamine resins, silicone resins, cyclic imide resins, urea resins, thermosetting polyimide resins, modified polyphenylene ether resins, thermosetting acrylic resins, and epoxy-silicone hybrid resins. In addition, reactive groups that can react with maleimide groups include epoxy groups, maleimide groups, hydroxyl groups, acid anhydride groups, alkenyl groups such as allyl groups and vinyl groups, (meth)acrylic groups, and thiol groups. Compounds having allyl groups as other additives do not have an isocyanuric ring and are distinguished from component (B).
[0050] From the viewpoint of reactivity, the reactive group of the thermosetting resin is preferably selected from among an epoxy group, a maleimide group, a hydroxyl group, an acid anhydride group, and an alkenyl group, and from the viewpoint of dielectric properties, an alkenyl group or a (meth)acrylic group is more preferable. However, the amount of the thermosetting resin having a reactive group capable of reacting with a maleimide group is 0 to 80 parts by mass per 100 parts by mass of the component (A).
[0051] inorganic filler In the present invention, an inorganic filler may be further added. It can be blended for the purpose of increasing the strength or rigidity of the cured product of the curable resin composition of the present invention, or adjusting the thermal expansion coefficient or dimensional stability of the cured product. In addition, depending on the type of inorganic filler, it can be blended for the purpose of adjusting the relative dielectric constant or dielectric loss tangent. As the inorganic filler, those that are usually blended in epoxy resin compositions or silicone resin compositions can be used. For example, silicas such as spherical silica, fused silica, and crystalline silica, alumina, silicon nitride, aluminum nitride, boron nitride, barium sulfate, talc, clay, aluminum hydroxide, magnesium hydroxide, calcium carbonate, glass fiber, and glass particles can be mentioned. Furthermore, titanate-based materials such as barium titanate, strontium titanate, and calcium titanate can be used to improve dielectric properties. The inorganic filler may be used alone or in combination of two or more kinds.
[0052] The average particle size and shape of the inorganic filler are not particularly limited, but when forming a film, a spherical inorganic filler with an average particle size of 0.5 to 3 μm is preferably used. The average particle size is determined by measuring the median diameter (D 50 ) was calculated.
[0053] Furthermore, in order to improve the properties of the cured product of the curable resin composition, the inorganic filler is preferably surface-treated with a silane coupling agent having an organic group capable of reacting with a maleimide group. Examples of such silane coupling agents include epoxy group-containing alkoxysilane, amino group-containing alkoxysilane, (meth)acrylic group-containing alkoxysilane, and alkenyl group-containing alkoxysilane. As the silane coupling agent, an alkoxysilane containing a (meth)acrylic group and / or an amino group is preferably used, and specific examples thereof include 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, and 3-aminopropyltrimethoxysilane.
[0054] others In addition to the above, non-functional silicone oil, thermoplastic resin, thermoplastic elastomer, organic synthetic rubber, light stabilizer, polymerization inhibitor, flame retardant, pigment, dye, etc. may be blended, and an ion trapping agent, etc. may be blended to improve electrical properties.
[0055] The curable resin composition for the film for film capacitor of the present invention can be dissolved in an organic solvent and treated as a varnish when preparing a film. By making the composition into a varnish, it becomes easier to make a film. Regarding the organic solvent, any solvent that dissolves the thermosetting resin having a reactive group that can react with the maleimide group as the component (A), the component (B), and other additives can be used without limitation. For example, anisole, tetralin, mesitylene, xylene, toluene, tetrahydrofuran (THF), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), acetonitrile, etc. are listed, but aromatic organic solvents such as anisole, tetralin, mesitylene, xylene, and toluene are preferred. These may be used alone or in combination of two or more.
[0056] The curable resin composition for the film for film capacitors can be made into an uncured resin sheet or uncured resin film by applying the above-mentioned varnish to a substrate and volatilizing the organic solvent, and can be further cured to make a cured resin sheet or cured resin film, but the film for film capacitors is basically made of the cured material. The following are examples of manufacturing methods for sheets and films, but they are not limited to these. The only difference between sheets and films is the thickness, and generally, those thicker than 200 μm are called sheets, and those less than 200 μm are called films.
[0057] As mentioned above, thin films are used for film capacitors. The specific thickness is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. If it is 1 μm or more, there is no problem in terms of characteristics and strength.
[0058] The method for producing the film is, for example, to apply a curable resin composition (varnish) for film capacitors dissolved in an organic solvent to a substrate, then heat the substrate at a temperature of typically 80°C or higher, preferably 100°C or higher, for 0.5 to 20 minutes to remove the organic solvent, and further heat the substrate at a temperature of 130°C or higher, preferably 150°C or higher, for 0.1 to 10 hours to form a cured coating (film) with a flat surface. The temperature in the drying step for removing the organic solvent and the subsequent heat curing step may be constant, but it is preferable to increase the temperature stepwise. This allows the organic solvent to be efficiently removed from the composition and the curing reaction of the resin to proceed efficiently. When the curing reaction is a thermal radical polymerization reaction, it is preferable to cure in a nitrogen atmosphere because oxygen may inhibit the reaction.
[0059] In addition, when the curing reaction is a photopolymerization reaction, the curing is performed by irradiation with light under various conditions such as ordinary wavelength, illuminance, time, etc., for example, by irradiation with UV light of 365 nm, etc. Depending on the application, after photocuring under the above-mentioned conditions, thermal curing under conditions such as 180°C and 1 hour may be combined.
[0060] The method for applying the varnish includes, but is not limited to, a spin coater, a slit coater, a spray, a dip coater, a bar coater, and the like.
[0061] The substrate may be a general resin substrate, for example, polyolefin resin such as polyethylene (PE) resin, polypropylene (PP) resin, polystyrene (PS) resin, etc., polyester resin such as polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polycarbonate (PC) resin, etc. The surface of the substrate may be subjected to a release treatment. The thickness of the coating layer is not particularly limited, but is preferably within the above-mentioned thickness range. Furthermore, when an uncured film is produced, a cover film may be used on the coating layer.
[0062] Alternatively, each component may be premixed in advance using a Henschel mixer or the like, and extruded into a sheet or film using a melt kneader or extrusion molding machine and used as is. A resin composition may be produced by melt mixing using a hot two-roll mill, and then crushed into tablets or granules and heat cured using a hot press. This is a preferred method for producing systems containing a large amount of inorganic filler or sheet-shaped products.
[0063] A film capacitor can be produced by laminating an electrode layer on at least one surface of the film of the present invention.
[0064] Examples of the structure of a film capacitor include known structures such as a laminated type in which electrode layers and dielectric films are alternately laminated, and a wound type in which a tape-like highly dielectric film is wound around an electrode layer. In the case of a wound film capacitor in which an electrode layer is continuously laminated on a film, which has a simple structure and is relatively easy to manufacture, it is generally manufactured by winding two sheets of film with an electrode laminated on one side so that the electrodes do not come into contact with each other, and fixing the film after winding as necessary to prevent it from coming loose.
[0065] The electrode layer is not particularly limited, but may be a metal foil made of a conductive metal such as aluminum, zinc, or copper, or a vapor-deposited metal coating. In the present invention, either a metal foil or a vapor-deposited metal coating, or both, may be used. In particular, a vapor-deposited metal coating with small thickness variation is preferable. The vapor-deposited metal coating is not limited to a single layer, and may be multi-layered as necessary, for example, by forming an aluminum oxide layer of a semiconductor on an aluminum layer to provide moisture resistance (for example, JP-A-2-250306). The thickness of the vapor-deposited metal coating is not particularly limited, but is preferably in the range of 100 to 2,000 angstroms, more preferably 300 to 1,000 angstroms. If the thickness of the vapor-deposited metal coating is within this range, the capacitance of the capacitor and the strength of the metal coating are well balanced, which is preferable.
[0066] When a vapor-deposited metal film is used as the electrode layer, the method for forming the film is not particularly limited, and for example, a vacuum deposition method, a sputtering method, etc. can be used. Usually, a vacuum deposition method is used.
[0067] When forming a metal thin film layer on a film, the film surface may be previously subjected to treatment for improving adhesion, such as corona treatment, plasma treatment, etc. When a metal foil is used as the electrode layer, the thickness of the metal foil is not particularly limited, but is usually in the range of 0.1 to 100 μm, preferably 0.5 to 50 μm, and more preferably 2 to 15 μm.
[0068] The method of sealing and fixing the capacitor is not particularly limited, and for example, the capacitor may be sealed with resin or enclosed in an insulating case, etc., so that the capacitor can be fixed and the structure can be protected at the same time. The method of connecting the lead wires is also not limited, and examples of the method include welding, ultrasonic welding, thermo-welding, and fixing with adhesive tape. The lead wires may be connected to the electrodes before winding. When enclosing the capacitor in an insulating case, the openings may be sealed with a thermosetting resin such as an acrylic resin or an epoxy resin, if necessary.
[0069] The curable resin composition for a film for a film capacitor of the present invention is used for a film capacitor, but can be used for other purposes if it is suitable. For example, it can be used in a wide range of applications, such as semiconductor encapsulation materials, impregnated into glass cloth such as quartz cloth to form prepregs, and further in substrates, interlayer insulating films, and build-up films using prepregs. EXAMPLES
[0070] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0071] The components used in the examples and comparative examples are shown below. In the following, the number average molecular weight (Mn) was measured under the following measurement conditions using polystyrene as the standard. Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-L TSKgel SuperHZ4000(4.6mmI.D.×15cm×1) TSKgel SuperHZ3000(4.6mmI.D.×15cm×1) TSKgel SuperHZ2000 (4.6mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 5 μL (0.2% by mass in THF solution)
[0072] (A) Maleimide resin (A-1) A maleimide compound represented by the following formula (5) (BMI-6100, manufactured by Designer Molecules Inc., Mn: 24000) [ka] (A-2) A maleimide compound represented by the following formula (6) (SLK-6200, manufactured by Shin-Etsu Chemical Co., Ltd., Mn: 23000) [ka] (A-3): A linear alkylene group-containing bismaleimide compound represented by the following formula (SLK-3000, manufactured by Shin-Etsu Chemical Co., Ltd., Mn: 7500) [ka] (A-4): 4,4'-diphenylmethane bismaleimide (BMI-1000: manufactured by Daiwa Chemical Industry Co., Ltd., Mn: 358, for comparison) (A-5): Crystalline bisphenol A type epoxy resin (YL-6810: trade name manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 170, melting point 45°C, for comparison) (A-6): Trisphenolmethane type epoxy resin (EPPN-502H: manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 168, softening point 60°C, for comparison) (A-7): Phenol resin (DL-92: manufactured by Meiwa Kasei Co., Ltd., hydroxyl equivalent 107, for comparison)
[0073] (B) An organic compound having one or more allyl groups and one or more isocyanuric rings in one molecule. (B-1): Triallyl isocyanurate (TAIC, manufactured by Mitsubishi Chemical Corporation) (B-2): Alkyl diallyl isocyanurate (L-DAIC, manufactured by Shikoku Kasei Co., Ltd.) (B-3): Diallyl isophthalate (Daiso DAP 100 monomer, manufactured by Osaka Soda Co., Ltd., for comparison) (B-4): Bifunctional acrylic monomer (KAYARADR-684, manufactured by Nippon Kayaku Co., Ltd., for comparative example)
[0074] (C) Polymerization initiator (C-1) Dicumyl peroxide (Percumyl D, NOF Corp.) (C-2): 2-phenyl-4-ethylimidazole (2P4MZ, manufactured by Shikoku Kasei Co., Ltd.)
[0075] Comparative PP film PP film with a thickness of 18 μm (PP18R, manufactured by Shin-Etsu Film Co., Ltd.; the film was used as is for the test)
[0076] <Film Preparation> A varnish was prepared with the formulation shown in Tables 1 and 2, and this varnish-like curable resin composition was applied to the release surface of a 38 μm-thick PET film (TN-200, manufactured by Toyobo STC) using a roller coater so that the thickness after drying would be 5 μm. The uncured resin film was then dried at 100°C for 10 minutes to obtain an uncured resin film. The uncured resin film was then sandwiched between the release surfaces of PET films (TN-010, manufactured by Toyobo STC) and cured at 180°C for 1 hour at 2 MPa using a vacuum press (manufactured by Nikko Materials) to obtain a cured resin film. At this time, the appearance of the film was checked, and a mark of ◯ was given for films that were smooth and flat, and a mark of X was given for films that were not smooth and had blistering or the like.
[0077] <Handleability of cured film> The cured films obtained above were subjected to a 180° folding test 10 times in succession. Handling properties were evaluated as follows: ◯ if the film could be folded 180° 10 times in succession, △ if it broke in the middle of 2 to 10 times, and X if it broke or could not be folded in half 180° on the first try.
[0078] <1kHz relative dielectric constant, dielectric loss tangent> Using the above-mentioned cured film, the dielectric constant and dielectric loss tangent at 1 kHz at 25°C were measured according to the method specified in JIS C 2138. The tester used was an "LCR Meter IM3536" (manufactured by Hioki E.E. Corporation), and the measurements were performed in silicone oil.
[0079] <Breakdown voltage> The dielectric breakdown voltage of the cured film described above was measured at 25°C and 150°C according to the method specified in JIS C 2110-1. The tester used was a dielectric breakdown voltage tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.), and measurements were taken in silicone oil using the short-time breakdown method.
[0080] [Table 1]
[0081] [Table 2]
[0082] All of the cured resin films produced in Examples 1 to 6 shown in Table 1 had a relative dielectric constant of 2.7 or more, a dielectric loss tangent of 0.006 or less, good cured film handleability, and a dielectric breakdown voltage of 220 V / μm or more at 25° C. and 150° C. The films also had a smooth appearance. Moreover, the cured resin films of Examples 1 to 6 exhibited superior properties in terms of the relative dielectric constant and the dielectric breakdown voltage at 150° C., as compared with the PP film shown in Comparative Example 11 (Table 2). On the other hand, the curable resin compositions shown in Table 2 that did not contain the (B) component (Comparative Example 1), did not contain an isocyanuric ring (Comparative Example 2), and did not contain an allyl group or an isocyanuric ring (Comparative Example 3) all had a dielectric tangent exceeding 0.006, and were inferior in terms of the appearance of the film and the dielectric breakdown voltage properties compared to Examples 1 to 6, and were unsuitable as curable resin compositions for film capacitors. Furthermore, in the case of a curable resin composition containing a linear alkylene group-containing bismaleimide compound (Mn: 7,500), whether it contained no allyl group or an isocyanuric ring (Comparative Example 4) or contained an allyl group and an isocyanuric ring (Comparative Example 5), the relative dielectric constant was less than 2.7 and the dielectric breakdown voltage at 150°C was less than 220 V / μm, and these were unsuitable as curable resin compositions for film capacitors. In the case of a curable resin composition containing 4,4'-diphenylmethane bismaleimide ((Mn: 358)) as the component (A), the handleability of the cured film was poor (Comparative Examples 6 and 7), and the composition was unsuitable as a curable resin composition for a film capacitor. In the case of a curable resin composition containing a crystalline bisphenol A type epoxy resin, a trisphenolmethane type epoxy resin, and a phenolic resin having no maleimide group as the component (A), the handleability of the cured film was insufficient, the dielectric tangent was the highest, and the breakdown voltage at 25°C and 150°C was the lowest (Comparative Example 8). In the case of a curable resin composition containing a trisphenolmethane type epoxy resin and a phenolic resin, the handleability of the cured film was poor (Comparative Example 9). In the case of a curable resin composition using a maleimide compound and a crystalline bisphenol A type epoxy resin, the dielectric tangent was high (Comparative Example 10). Thus, the curable resin compositions shown in Comparative Examples 8 to 10 were unsuitable as curable resin compositions for film capacitors. From the above, the usefulness of the invention was confirmed.
[0083] [Example 7] Two sheets of aluminum foil (conductor: thickness 6 μm, width 5 mm) and the film produced in Example 1 (film: thickness 5 μm, width 7 mm) were stacked and wound as shown in Fig. 1 to produce a film capacitor element. Fig. 2 shows a cross-sectional view of the film capacitor element in Fig. 1. The current extraction electrode was obtained by inserting copper foil (tab-type lead: 0.1 mm) into the center of the element length. Figure 3 shows a schematic diagram of the current extraction electrode of the film capacitor. The produced element was covered with an epoxy resin to produce a film capacitor, which was designated Example 7. The film capacitor of Example 7 had a capacitance of 1500 pF and a rated voltage of 630 VDC.
[0084] Exterior crack test, voltage resistance test, insulation resistance test In each of the exterior cracking test, the voltage resistance test, and the insulation resistance test, 20 pieces of the film capacitor of Example 7 were used. In the exterior cracking test, the film capacitor of Example 7 was placed in a high-temperature bath at 150° C. and left there for 15 minutes. After that, those that had exterior cracks visually were judged to have failed. In the voltage resistance test, 1300VDC was applied to the film capacitor for 1 minute, and any that caused dielectric breakdown were deemed to have failed. The insulation resistance test was conducted based on the insulation resistance measurement method specified in JIS C 5101-1, and any value below 50,000 MΩ was deemed to have failed. As a result of the exterior cracking test, voltage withstand test, and insulation resistance test, no failures were found in the exterior cracking, voltage withstand test, or insulation resistance test.
[0085] [Example 8] A film having a thickness of 1 μm produced using the compounding ratio used in Example 1 was subjected to the same procedure as in Example 7 to produce a film capacitor element. This was designated Example 8. The film capacitor of Example 8 had a capacitance of 6500 pF and a rated voltage of 650 VDC.
[0086] Exterior crack test, voltage resistance test, insulation resistance test Similarly, 20 pieces of the film capacitor of Example 8 were used for each of the exterior cracking test, the withstand voltage test, and the insulation resistance test. The evaluation criteria were the same as those of Example 7. As a result of the exterior cracking test, voltage withstand test, and insulation resistance test, no failures were found in the exterior cracking, voltage withstand test, or insulation resistance test.
[0087] [Example 9] A film having a thickness of 20 μm produced using the compounding ratio used in Example 1 was treated in the same manner as in Example 7 to produce a film capacitor element. This was designated Example 9. The film capacitor of Example 9 had a capacitance of 600 pF and a rated voltage of 590 VDC.
[0088] Exterior crack test, voltage resistance test, insulation resistance test Similarly, 20 pieces of the film capacitor of Example 9 were used for each of the exterior cracking test, the withstand voltage test, and the insulation resistance test. The evaluation criteria were the same as those of Example 7. As a result of the exterior cracking test, voltage withstand test, and insulation resistance test, no failures were found in the exterior cracking, voltage withstand test, or insulation resistance test.
[0089] From the above, it was confirmed that the present invention is also useful as a film capacitor.
[0090] The present specification includes the following aspects. [1]: (A) a maleimide resin having a number average molecular weight of 3,000 or more; (B) an organic compound having one or more allyl groups and one or more isocyanuric rings in one molecule; and (C) Polymerization initiator A curable resin composition for a film capacitor comprising: A curable resin composition for a film capacitor, characterized in that a cured product of the curable resin composition satisfies the following properties: 1) Dielectric constant of 2.7 or more at 1 kHz and 25°C 2) Dielectric tangent at 1kHz and 25℃ is 0.006 or less 3) No damage occurs even when bent 180 degrees 10 times at a thickness of 5 μm 4) The dielectric breakdown voltage at 25℃ and 150℃ is 220V / μm or more. [2]: The curable resin composition for a film capacitor according to [1], characterized in that the maleimide resin of the component (A) contains an aromatic bismaleimide represented by the following general formula (1) and / or (2): [ka] (In the formula, X 1 are independently expressed by the following formula: [ka] and l is a number from 1 to 40. [ka] (In the formula, X 2 are independently X in the above formula 1 m is a number from 1 to 50, and n is a number from 1 to 50. 1 and A 2 are each independently a divalent group represented by the following general formula (3) or the following general formula (4). [ka] (In the formula, X 3 are independently represented by the above formula X 1 and X 2 R is a divalent group having the same structure as 1 are independently a hydrogen atom, a chlorine atom, or an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 6 carbon atoms. [ka] (In the formula, X 3 denotes the same thing as above.) [3]: The curable resin composition for a film capacitor according to [1] or [2], wherein the component (B) is an organic compound having two or more allyl groups in one molecule. [4]: The curable resin composition for a film capacitor according to any one of [1] to [3], characterized in that the blending amount of the (B) component is 5 parts by mass to 40 parts by mass per 100 parts by mass of the (A) component. [5]: The curable resin composition for a film capacitor according to any one of [1] to [4], wherein the polymerization initiator (C) is a thermal radical polymerization initiator and / or a photocuring initiator. [6]: A cured resin material for a film capacitor, which is obtained by curing the curable resin composition for a film capacitor according to any one of [1] to [5], and is in the form of a film having a thickness of 1 to 20 μm. [7]: A film capacitor comprising the cured resin material according to [6].
[0091] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. (A) a maleimide resin having a number average molecular weight of 3,000 or more; (B) an organic compound having one or more allyl groups and one or more isocyanuric rings in one molecule; and (C) Polymerization initiator A curable resin composition for a film capacitor comprising: A curable resin composition for a film capacitor, characterized in that a cured product of the curable resin composition satisfies the following properties: 1) Dielectric constant of 2.7 or more at 1 kHz and 25°C 2) Dielectric tangent at 1 kHz and 25°C is 0.006 or less 3) No damage occurs even when bending 180 degrees 10 times at a thickness of 5 μm 4) The dielectric breakdown voltage at 25°C and 150°C is 220V / μm or more.
2. 2. The curable resin composition for a film capacitor according to claim 1, wherein the maleimide resin of the component (A) contains an aromatic bismaleimide represented by the following general formula (1) and / or (2): 【Chemistry 1】 (In the formula, X 1 are independently expressed by the following formula: 【Chemistry 2】 and l is a number from 1 to 40. 【Chemistry 3】 (In the formula, X 2 is independently selected from X 1 m is a number from 1 to 50, and n is a number from 1 to 50. 1 and A 2 are each independently a divalent group represented by the following general formula (3) or the following general formula (4): 【Chemistry 4】 (In the formula, X 3 are independently selected from the formula X 1 and X 2 is a divalent group having the same structure as 1 are independently a hydrogen atom, a chlorine atom, or an unsubstituted or substituted aliphatic hydrocarbon group having 1 to 6 carbon atoms. 【Chemistry 5】 (In the formula, X 3 indicates the same as above.)
3. 2. The curable resin composition for a film capacitor according to claim 1, wherein the component (B) is an organic compound having two or more allyl groups in one molecule.
4. The curable resin composition for a film capacitor according to claim 1, characterized in that the blending amount of the component (B) is 5 parts by mass to 40 parts by mass per 100 parts by mass of the component (A).
5. The curable resin composition for a film capacitor according to claim 1, wherein the polymerization initiator (C) is a thermal radical polymerization initiator and / or a photocuring initiator.
6. A cured resin material for a film capacitor, which is obtained by curing the curable resin composition for a film capacitor according to any one of claims 1 to 5, and has a film shape having a thickness of 1 to 20 μm.
7. A film capacitor comprising the cured resin according to claim 6.
Citation Information
Patent Citations
Laminated film capacitor
JP1989200609A
Heat-curable maleimide resin composition
JP2022097398A
JP164735A
Polyacrylonitrile film and its production
JP1999000539A
Biaxially oriented polypropylene film for capacitor, polypropylene film for metal layer integrated capacitor, film capacitor and film roll
JP2023002364A