Method for manufacturing porous silicon clathrate electrode active material and method for manufacturing lithium ion battery
The method of producing porous silicon clathrate particles with high type II silicon clathrate content and increased pores addresses the expansion issue in silicon electrodes, enhancing battery performance by selectively removing type I silicon clathrate using a hydrogen fluoride solution.
Patent Information
- Application Number
- JP2023085318
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-24
AI Technical Summary
Existing silicon electrode active materials, particularly type II silicon clathrates, face challenges with large expansion during battery charging due to limited pore content and structure, which affects battery performance.
A method to produce porous silicon clathrate particles with a high content of type II silicon clathrate and numerous pores by selectively removing type I silicon clathrate using a hydrogen fluoride solution, creating pores within the particles.
The method enhances the porosity of silicon clathrate particles, reducing expansion during charging and improving battery performance by increasing the proportion of type II silicon clathrate to 93.5% or more, with pore volume increase of 0.01 to 0.15 cc/g.
Smart Images

Figure 2024168549000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a porous silicon clathrate electrode active material and a method for producing a lithium ion battery. [Background technology]
[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is also known as an electrode active material for batteries, particularly lithium ion batteries.
[0003] Silicon electrode active materials have a large theoretical capacity and are effective in increasing the energy density of batteries. On the other hand, silicon electrode active materials have a problem of large expansion during charging. It is known that the expansion during charging can be suppressed by using a silicon clathrate electrode active material as the silicon electrode active material.
[0004] For example, Patent Document 1 discloses a silicon clathrate electrode active material having a silicon clathrate type II crystal phase, having voids inside the primary particles, and having a void volume of pores having a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2021-158004 Summary of the Invention [Problem to be solved by the invention]
[0006] There are two types of silicon clathrate crystals: type I silicon clathrate and type II silicon clathrate. In particular, type II silicon clathrate efficiently occludes lithium in the cage structure of the crystal, and therefore expands and contracts little during charging and discharging of the battery.
[0007] Furthermore, silicon clathrate particles having pores can absorb expansion caused by charging the battery by using the pores, thereby making it possible to reduce expansion during charging.
[0008] Under these circumstances, there is a need for the development of a method for producing silicon clathrate particles that have a high content of type II silicon clathrate and many pores.
[0009] The present disclosure aims to provide a method for producing a porous silicon clathrate electrode active material having a high content of type II silicon clathrate and many pores, and a method for producing a lithium ion battery that includes producing such a silicon clathrate electrode active material. [Means for solving the problem]
[0010] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A method for producing a porous silicon clathrate electrode active material, comprising the steps of: (a) providing a composition comprising silicon clathrate particles containing a type I silicon clathrate and a type II silicon clathrate; and (b) removing at least a portion of the type I silicon clathrate to form pores in the silicon clathrate particles or to increase the porosity of the silicon clathrate particles; <Aspect 2> 2. The method of claim 1, wherein the ratio of the mass of the type I silicon clathrate to the total mass of the composition including the silicon clathrate particles is 5.0 mass% or more. <Aspect 3> 2. The method of embodiment 1, wherein in step (b), the silicon clathrate particles are contacted with a hydrogen fluoride solution to remove at least a portion of the type I silicon clathrate. <Aspect 4> The method according to aspect 3, wherein the solvent of the hydrogen fluoride solution is a mixed solvent of water and an organic solvent. <Aspect 5> The method according to any one of aspects 1 to 4, wherein the silicon clathrate electrode active material is for use as a negative electrode active material in a lithium ion battery. <Aspect 6> Producing a silicon clathrate electrode active material by the method according to any one of aspects 1 to 5; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising: Effect of the Invention
[0011] According to the method of the present invention for producing a porous silicon clathrate electrode active material, it is possible to produce silicon clathrate particles having a high content of type II silicon clathrate and many pores. In addition, the present disclosure can provide a method for producing a lithium ion battery including producing such a silicon clathrate electrode active material. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a graph showing the relationship between the content of I-type silicon clathrate in a composition containing silicon clathrate particles and the increase in the amount of pores of 100 nm or less after removal of the I-type silicon clathrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0014] <<Method for producing porous silicon clathrate electrode active material>> The disclosed method of making a porous silicon clathrate electrode active material includes (a) providing a composition comprising silicon clathrate particles containing a silicon clathrate type I and a silicon clathrate type II, and (b) removing at least a portion of the silicon clathrate type I to form pores in the silicon clathrate particles or increase the porosity of the silicon clathrate particles.
[0015] The present inventors have found that there is a difference in solubility between type I silicon clathrate and type II silicon clathrate in a specific solution, particularly in a hydrogen fluoride (HF) solution, that is, type I silicon clathrate has a higher solubility in a HF solution. Therefore, the present inventors have found that it is possible to form pores in the silicon clathrate particles or increase the pores in the silicon clathrate particles by dissolving and removing type I silicon clathrate from silicon clathrate particles containing type I silicon clathrate and type II silicon clathrate using a HF solution or the like, thereby generating pores in the locations where type I silicon clathrate was present.
[0016] This makes it possible to obtain a porous silicon clathrate that expands little during charging.
[0017] In the present disclosure, the "electrode active material" can be used as either a "positive electrode active material" or a "negative electrode active material", and is particularly used as a "negative electrode active material".
[0018] <Providing a composition containing silicon clathrate particles> The method of the present disclosure includes providing a composition comprising silicon clathrate particles that contain a silicon clathrate type I and a silicon clathrate type II.
[0019] A composition including such silicon clathrate particles can be prepared by preparing a sodium silicon (NaSi) alloy and removing sodium from the NaSi alloy.
[0020] Specifically, a silicon source is reacted with a sodium source such as sodium hydride to prepare a NaSi alloy. The NaSi alloy thus prepared is then heated to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a composition containing silicon clathrate particles. Alternatively, the NaSi alloy thus prepared is reacted with aluminum fluoride as a sodium trapping agent to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a composition containing silicon clathrate particles.
[0021] In a composition containing silicon clathrate particles that can be used as a raw material in the method of the present disclosure, the ratio of the mass of the I-type silicon clathrate to the total mass of the composition containing the silicon clathrate particles may be 5.0 mass% or more, 6.0 mass% or more, 6.5 mass% or more, 6.8 mass% or more, or 7.0 mass% or more, and may be 12.0 mass% or less, 10.0 mass% or less, 9.0 mass% or less, 8.5 mass% or less, or 8.0 mass% or less.
[0022] The content ratio of the I-type silicon clathrate and the II-type silicon clathrate in the silicon clathrate particles can be calculated, for example, from the peak intensity ratio in the measurement results of X-ray diffraction (XRD).
[0023] <Removal of type I silicon clathrate> The method of the present disclosure includes removing at least a portion of the type I silicon clathrate to form pores in the silicon clathrate particles or to increase the porosity of the silicon clathrate particles.
[0024] The silicon clathrate particles may be contacted with a hydrogen fluoride solution to remove at least a portion of the type I silicon clathrate.
[0025] The solvent of the hydrogen fluoride solution may be water, an organic solvent, or a mixed solvent of water and an organic solvent. When the solvent contains water, that is, when the solvent is water or a mixed solvent of water and an organic solvent, particularly when the solvent is a mixed solvent of water and an organic solvent, sodium silicofluoride (Na 2 SiF 6 This is preferable in that the production of by-products such as
[0026] It is preferable that the solvent contains an organic solvent in that the amount of water remaining in the silicon clathrate electrode active material can be reduced. The proportion of the organic solvent in the solution may be 80% by mass or more, 90% by mass or more, or 95% by mass or more.
[0027] The organic solvent may be any organic solvent capable of dissolving hydrogen fluoride, and when the organic solvent is used in combination with water, any organic solvent capable of dissolving hydrogen fluoride and compatible with water may be used. The organic solvent is preferably an alcohol, more preferably a lower alcohol, and even more preferably ethanol.
[0028] In the method of the present disclosure, the ratio of the amount of hydrogen fluoride (mol) to the mass (g) of silicon clathrate (HF [mol] / Si [g]) may be 0.006 mol / g or more, 0.01 mol / g or more, 0.02 mol / g or more, 0.03 mol / g or more, 0.04 mol / g or more, or 0.05 mol / g or more, and may be 0.25 mol / g or less, 0.20 mol / g or less, 0.15 mol / g or less, 0.13 mol / g or less, or 0.11 mol / g or less. When this ratio is within the above range, the I-type silicon clathrate can be highly selectively removed from the silicon clathrate particles.
[0029] The contact method is, for example, a mixing operation such as stirring, but is not limited thereto.
[0030] The contact time may be 0.5 hours or more, 1 hour or more, or 2 hours or more, and may be 6 hours or less, 5 hours or less, or 4 hours or less.
[0031] In the silicon clathrate electrode active material produced by the method of the present disclosure, the ratio of the mass of the II-type silicon clathrate to the total mass of the I-type silicon clathrate and the II-type silicon clathrate may be 93.5% by mass or more, 94.0% by mass or more, 95.0% by mass or more, 96.0% by mass or more, 97.0% by mass or more, 98.0% by mass or more, or 99.0% by mass or more.
[0032] The silicon clathrate particles may contain pores with a diameter of 100 nm or less.
[0033] In the method of the present disclosure, the pores contained in the silicon clathrate particles, particularly pores with a diameter of 100 nm or less, can be increased by step (b). The increase in the amount of pores can be calculated as the difference between the amount of pores after step (b) and the amount of pores before step (b).
[0034] The increase in pores with a diameter of 100 nm or less may be 0.01 cc / g or more, 0.03 cc / g or more, 0.04 cc / g or more, 0.05 cc / g or more, or 0.06 cc / g or more, and may be 0.50 cc / g or less, 0.40 cc / g or less, 0.30 cc / g or less, 0.25 cc / g or less, 0.20 cc / g or less, 0.17 cc / g or less, or 0.15 cc / g or less.
[0035] <Application> The silicon clathrate electrode active material in the method of the present disclosure can be used as the negative electrode active material in a lithium ion battery.
[0036] <<How lithium-ion batteries are manufactured>> The disclosed method of making a lithium ion battery includes making a silicon clathrate electrode active material by the disclosed method and forming an electrode active material layer containing the silicon clathrate electrode active material.
[0037] For the method for producing the silicon clathrate electrode active material, reference can be made to the above description regarding the method for producing the silicon clathrate electrode active material of the present disclosure.
[0038] The method for forming the electrode active material layer is not particularly limited, and a known method can be adopted. For example, when the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure, the electrode active material layer formed on the negative electrode current collector layer, i.e., the negative electrode active material layer, can be obtained by applying a slurry containing the silicon clathrate electrode active material to the negative electrode current collector and drying it.
[0039] The method for forming the battery is not particularly limited, and any known method can be used. Hereinafter, a method for producing a battery in which the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure will be described.
[0040] The method for manufacturing a battery according to the present disclosure may include, in addition to manufacturing a silicon clathrate electrode active material and forming a negative electrode active material layer containing the silicon clathrate electrode active material, arranging, in this order, a negative electrode current collector layer, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.
[0041] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.
[0042] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0043] <Negative electrode active material layer> The negative electrode active material layer of the present disclosure is a layer containing a negative electrode active material, and optionally an electrolyte, a conductive assistant, and a binder.
[0044] (Negative electrode active material) The negative electrode active material comprises a silicon clathrate electrode active material of the present disclosure.
[0045] (electrolyte) The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.
[0046] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li 2 SP 2 S 5 System (Li 7 P 3 S 11 , Li 3 P.S. 4 , Li 8 P 2 S 9 etc.), Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2 S 5 , LiI-LiBr-Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -GeS 2 (Li 13 GeP 3 S 16 , Li 10 GeP 2 S 12 etc.), LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 , Li 7-x P.S.6-x Cl x etc.; or combinations thereof, but are not limited to these.
[0047] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).
[0048] When the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon clathrate electrode active material to the solid electrolyte in the negative electrode active material layer (mass of silicon clathrate electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.
[0049] The electrolyte preferably contains a supporting salt and a solvent.
[0050] As a supporting salt (lithium salt) of the electrolyte having lithium ion conductivity, for example, LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 Inorganic lithium salts such as LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiC(CF 3 SO 2 ) 3 Examples of organic lithium salts include:
[0051] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.
[0052] (Conductive assistant) The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.
[0053] (binder) The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.
[0054] The negative electrode active material layer may have a thickness of, for example, 0.1 to 1000 μm.
[0055] <Electrolyte layer> The electrolyte layer includes at least an electrolyte. The electrolyte layer may include a binder, etc., if necessary, in addition to the electrolyte. For the electrolyte and the binder, the above description regarding the negative electrode active material layer of the present disclosure can be referred to.
[0056] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.
[0057] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally an electrolyte, a conductive assistant, a binder, and the like.
[0058] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganate (LiMn 2 O 4 ), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O 2 , Li 1+x Mn 2-x-y MyO 4 Li-Mn spinel substituted with different elements having a composition represented by the formula (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO 4 , M may be one or more metals selected from Fe, Mn, Co, and Ni), but is not limited thereto.
[0059] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials that constitute the coating layer include LiNbO 3 In addition, Li 4 Ti 5 O 12 , Li 3 PO 4 These include, but are not limited to, the following.
[0060] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0061] For the electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode active material layer of the present disclosure.
[0062] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.
[0063] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.
[0064] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, the material may be, but is not limited to, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc.
[0065] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0066] The lithium ion battery produced by the method of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.
[0067] The lithium ion battery produced by the method of the present disclosure may be a primary battery or a secondary battery.
[0068] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type. EXAMPLES
[0069] 《Synthesis of Porous Silicon Clathrate Electrode Active Material》 <Alloying> (Synthesis Example 1) As a silicon (Si) source, Si powder (Kojundo Kagaku, SIEPB32) was prepared. This Si powder and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere and treated with hydrogen fluoride (HF) to obtain a Si powder having voids inside the primary particles, i.e., a Si powder having a porous structure.
[0070] A sodium silicon (NaSi) alloy was produced using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder having a porous structure were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.
[0071] <Clathrate formation> (Synthesis Example 1) The obtained NaSi alloy and aluminum fluoride (AlF 3 ) were weighed out so that the molar ratio was 1:0.34, and the weighed NaSi alloy and AlF 3 The powdered reaction raw material was mixed in a cutter mill to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction vessel and heated in a heating furnace under an argon atmosphere at 340°C for 60 hours to obtain a reaction product containing silicon clathrate particles. The obtained reaction product was dissolved in HNO3 and H 2 The reaction product was washed with an acid using a mixed solvent of 10:90 by volume of O and 10:10 to remove by-products from the reaction product. After washing, the mixture was filtered, and the filtered solid was dried at 120°C for 3 hours or more to obtain a composition containing silicon clathrate particles of Synthesis Example 1 containing silicon clathrate I and silicon clathrate II.
[0072] (Synthesis Examples 2 to 4) In the same manner as in Synthesis Example 1, compositions containing silicon clathrate particles of Synthesis Examples 2 to 4 were obtained.
[0073] <Removal of type I silicon clathrate> Example 1 100 ml of ethanol and 3.71 ml of 46 wt % HF aqueous solution were added to 2.2 g of the composition containing the silicon clathrate particles of Synthesis Example 1 and stirred. The solution was reacted by stirring for 3 hours to remove the I-type silicon clathrate. The resulting reaction solution was filtered, and the filtered solid was washed 8 times with 20 ml of ethanol. After washing, the silicon clathrate electrode active material of Example 1 was obtained by drying overnight at 60°C.
[0074] (Examples 2 and 3) Silicon clathrate electrode active materials of Examples 2 and 3 were obtained in the same manner as in Example 1, except that compositions containing silicon clathrate particles of Synthesis Examples 2 and 3 were used. In each Example, the Example number and the Synthesis Example number correspond to each other.
[0075] Example 4 20 ml of water, 75 ml of ethanol, and 4.5 ml of 46 wt% HF aqueous solution were added to 2.2 g of the composition containing the silicon clathrate particles of Synthesis Example 4 and stirred. The solution was reacted by stirring for 3 hours to remove the I-type silicon clathrate. The resulting reaction solution was filtered, and the filtered solid was washed three times with 50 ml of water and once with 20 ml of ethanol. After washing, the mixture was dried overnight at 120°C to obtain the silicon clathrate electrode active material of Example 4.
[0076] Comparative Example 1 The composition containing the silicon clathrate particles of Synthesis Example 1 was used as the silicon clathrate electrode active material of Comparative Example 1 without carrying out removal of the I-type silicon clathrate.
[0077] Evaluation Results The content ratio of each component in the composition containing silicon clathrate particles, and the ratio of the mass of the II-type silicon clathrate to the total mass of the I-type silicon clathrate and the II-type silicon clathrate are shown in Table 1 (in the table, "Before removing I-type"). The ratio of the contained components was calculated from the peak intensity ratio in the XRD measurement results. In Table 1, "II-type" indicates the II-type silicon clathrate, and "I-type" indicates the I-type silicon clathrate.
[0078] Table 1 shows the content ratio of each component in the silicon clathrate electrode active material, and the ratio of the mass of the II-type silicon clathrate to the total mass of the I-type silicon clathrate and the II-type silicon clathrate (in the table, "After I-type removal").
[0079] The amount of pores of 100 nm or less increased after removing the I-type silicon clathrate was calculated as the difference between the amount of pores before and after the I-type silicon clathrate removal step. The value of this amount of pores increased in Example 1 was 0.0661 cc / g (pores of 100 nm or less). The results of this amount of pores increased in Examples 1 to 4 are shown in Table 1. The values of the amount of pores increased in Examples 2 to 4 are shown as relative values when the value in Example 1 is set to 100.
[0080] [Table 1]
[0081] As shown in Table 1, the silicon clathrate electrode active material obtained by the method of the present disclosure had an increased content of type II silicon clathrate and an increased amount of pores of 100 nm or less.
[0082] In addition, a graph showing the relationship between the content ratio of I-type silicon clathrate in a composition containing silicon clathrate particles and the increase in the number of pores of 100 nm or less after removing the I-type silicon clathrate is shown in Figure 1. As shown in Figure 1, when this content ratio is within the range of the present disclosure, the increase in the number of pores of 100 nm or less after removing the I-type silicon clathrate was large. In Figure 1, "I-type" refers to the I-type silicon clathrate.
Claims
1. A method for producing a porous silicon clathrate electrode active material, comprising the steps of: (a) providing a composition comprising silicon clathrate particles containing a type I silicon clathrate and a type II silicon clathrate; and (b) removing at least a portion of the type I silicon clathrate to form pores in the silicon clathrate particles or to increase the porosity of the silicon clathrate particles;
2. 2. The method according to claim 1, wherein the ratio of the mass of the I-type silicon clathrate to the total mass of the composition containing the silicon clathrate particles is 5.0 mass% or more.
3. 2. The method of claim 1, wherein in step (b), the silicon clathrate particles are contacted with a hydrogen fluoride solution to remove at least a portion of the type I silicon clathrate.
4. The method according to claim 3 , wherein the solvent of the hydrogen fluoride solution is a mixed solvent of water and an organic solvent.
5. 10. The method of claim 1, wherein the silicon clathrate electrode active material is for use as an anode active material in a lithium ion battery.
6. Producing a silicon clathrate electrode active material by the method according to any one of claims 1 to 5; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising:
Citation Information
Patent Citations
Method for producing silicon clathrate electrode active material, and method for manufacturing lithium ion battery
JP2024165104A
Rapid reduction of sodium occupancy in type ii silicon clathrate by chemical etching
US20150376016A1
Active material, negative electrode layer, battery and these manufacturing methods
JP2021158004A