Cathode electrode for solid electrolyte type electrochemical cell, and solid electrolyte type electrochemical cell including the same, and method of producing ammonia using solid electrolyte type electrochemical cell

The cathode electrode with a nitride layer of Nb and/or V and a metal layer of Ru, Fe, or Co in a solid electrolyte electrochemical cell enhances ammonia production efficiency by optimizing reaction cycles, addressing the low faradaic efficiency of conventional methods.

JP2024168559AInactive Publication Date: 2024-12-05HOKKAIDO UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023085349
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for producing ammonia using solid electrolyte electrochemical cells have low faradaic efficiency, necessitating improvements to enhance the production process.

Method used

A cathode electrode comprising a nitride layer of Nb and/or V with a metal layer of Ru, Fe, or Co is used in a solid electrolyte electrochemical cell, along with a method of alternating voltage application to facilitate ammonia production through specific reaction cycles.

Benefits of technology

The proposed cathode electrode achieves higher faradaic efficiency in ammonia production from water vapor and nitrogen, surpassing conventional methods by enabling efficient ammonia generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168559000001_ABST
    Figure 2024168559000001_ABST
Patent Text Reader

Abstract

To provide a cathode electrode for a solid electrolyte type electrochemical cell capable of producing ammonia from hydrogen and nitrogen with higher Faraday efficiency relative to a conventional technique.SOLUTION: The cathode electrode for a solid electrolyte type electrochemical cell, includes a nitride layer including a nitride of first metal, i.e., one or more species selected from the group consisting of Nb and V, and a metal layer including second metal, i.e., one or more species selected from the group consisting of Ru, Fe, and Co.SELECTED DRAWING: Figure 13
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a cathode electrode for a solid electrolyte electrochemical cell, a solid electrolyte electrochemical cell including the cathode electrode, and a method for producing ammonia using the solid electrolyte electrochemical cell. [Background technology]

[0002] Conventionally, a method for producing ammonia using an aqueous electrolyte has been used, but in this method, ammonia dissolves in the aqueous electrolyte and is difficult to separate, making it difficult to obtain pure ammonia.

[0003] In recent years, research has been conducted into the production of ammonia using electrochemical cells that use solid electrolytes, which makes it easier to obtain pure ammonia without the ammonia dissolving in the aqueous electrolyte. Additionally, a method of producing ammonia from water vapor and nitrogen has been attracting attention as a greener method of producing ammonia.

[0004] Non-Patent Document 1 uses Ni-BaCe as a cathode electrode. 0.9 Y 0.1 O 3-δ They disclose a solid electrolyte electrochemical cell that can produce ammonia from water vapor and nitrogen with a faradaic efficiency of 0.15% by using a cermet electrode or the like. Non-Patent Document 2 discloses an electrochemical cell using a solid electrolyte type electrochemical cell that can produce ammonia from water vapor and nitrogen with a faradic efficiency of 0.46% by using an Ag electrode as the cathode electrode, for example. In addition, Non-Patent Document 2 uses La as a cathode electrode. 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ A solid electrolyte electrochemical cell is also disclosed that can produce ammonia from water vapor and nitrogen with a faradaic efficiency of 0.33% by using electrodes or the like. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] N. Shimoda et al., Journal of the Ceramic Society of Japan, 125(4),252-256 (2017) [Non-Patent Document 2] DSYun et al., Journal of Power Sources, 284, 245-251 (2015) Summary of the Invention [Problem to be solved by the invention]

[0006] In the conventional techniques disclosed in Non-Patent Documents 1 and 2, the faradaic efficiency of ammonia production is low, and further improvement is required.

[0007] The present disclosure has been made in view of the above circumstances, and one of its objectives is to provide a cathode electrode for a solid electrolyte electrochemical cell capable of producing ammonia from water vapor and nitrogen with a higher faradaic efficiency than conventional techniques, a solid electrolyte electrochemical cell including the cathode electrode, and a method for producing ammonia using the solid electrolyte electrochemical cell. [Means for solving the problem]

[0008] Aspect 1 of the present invention is a nitride layer including a nitride of a first metal, which is at least one selected from the group consisting of Nb and V; and a metal layer on the nitride layer, the metal layer including a second metal, the second metal being at least one selected from the group consisting of Ru, Fe, and Co.

[0009] Aspect 2 of the present invention is In the cathode electrode for a solid electrolyte electrochemical cell according to aspect 1, when the first metal is M and the nitride is MNx, x is 0.6 to 1.1.

[0010] Aspect 3 of the present invention is A solid electrolyte electrochemical cell comprising the cathode electrode for a solid electrolyte electrochemical cell according to embodiment 1 or 2, a solid electrolyte layer, and an anode electrode, in this order.

[0011] A fourth aspect of the present invention is A solid electrolyte electrochemical cell according to aspect 3, comprising: supplying water vapor to the anode electrode and supplying nitrogen to the cathode electrode; Repeating the process of increasing a voltage applied to the solid electrolyte electrochemical cell to generate ammonia and then decreasing the applied voltage; The method for producing ammonia includes the steps of: Effect of the Invention

[0012] According to an embodiment of the present invention, it is possible to provide a cathode electrode for a solid electrolyte electrochemical cell capable of producing ammonia from water vapor and nitrogen with a higher faradaic efficiency than conventional techniques, a solid electrolyte electrochemical cell including the cathode electrode, and a method for producing ammonia using the solid electrolyte electrochemical cell. [Brief description of the drawings]

[0013] [Figure 1A] FIG. 1A shows an optical microscope photograph of the upper surface of a solid electrolyte layer (a sintered body of BZCYYb4411) of an example. [Figure 1B] FIG. 1B shows an optical microscope photograph of the side surface of the solid electrolyte layer of the example. [Diagram 2] FIG. 2 shows a cross-sectional SEM image of the solid electrolyte layer of the example. [Diagram 3] FIG. 3 shows the X-ray diffraction pattern of the nitride layer of the example. [Figure 4] FIG. 4 shows the hydrogen permeability evaluation results of Test No. 1. [Diagram 5] FIG. 5 shows the hydrogen permeability evaluation results of Test No. 2. [Figure 6] FIG. 6 shows the hydrogen permeability evaluation results of Test No. 3. [Figure 7] FIG. 7 shows the hydrogen permeability evaluation results of Test No. 4. [Figure 8A] FIG. 8A shows a cross-sectional SEM image of Test No. 6. [Figure 8B] FIG. 8B shows a cross-sectional SEM image of Test No. 8. [Figure 9] FIG. 9 shows the IV curves for Tests No. 5 and No. 6. [Figure 10] FIG. 10 shows the IV curves for Tests No. 7 and No. 8. [Figure 11] FIG. 11 shows the IV curve for Test No. 9. [Figure 12] Figure 12 shows the cell voltage changes for Tests Nos. 6, 8 and 9 when D2O-N2 co-electrolysis was carried out for 10 min at 600 °C and a constant current density of -6 mA·cm-2. [Figure 13] Figure 13 shows the change in the signal intensity of D2 (m / z = 4) and ND3 (m / z = 20) in the MASS spectrum when D2O-N2 co-electrolysis was performed for 10 minutes at 600 °C and a constant current density of -6 mA·cm-2 for Tests No. 6, 8, and 9. [Figure 14A] Figure 14A shows the voltage-time curves for Test No. 6 when D2O-N2 co-electrolysis was performed at 600 °C and a constant current density of -8 mA·cm-2 for 10 h. [Figure 14B] Figure 14B shows the change in the signal intensity of D2 and ND3 in the MASS spectrum for Test No. 6 when D2O-N2 co-electrolysis was performed for 10 hours at 600 °C and a constant current density of -8 mA·cm-2. [Figure 15] Figure 15 shows the change in the signal intensity of D2 and ND3 in the MASS spectrum for Test No. 6 when the cycle of D2O-N2 co-electrolysis at 600 °C and a constant current density of -8 mA cm-2, followed by holding at an open circuit voltage to desorb ND3, was repeated 10 times. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present inventors have conducted research from various angles in order to realize a cathode electrode for a solid electrolyte electrochemical cell that is capable of producing ammonia from water vapor and nitrogen with a faradaic efficiency higher than that of conventional techniques.

[0015] In general, when ammonia is produced by supplying water vapor to the anode electrode of a solid electrolyte electrochemical cell, supplying nitrogen to the cathode electrode, and applying a voltage to the cell, it is believed that the reaction shown in formula (1) below occurs on the anode electrode side, and the reactions shown in formulas (2) and (3) below occur on the cathode electrode side. 2H2O→O2+4H + +4e - (1) N2+6H + +6e - →2NH3···(2) 2H + +2e - →H2···(3)

[0016] It is believed that the reaction of formula (2) above, which gives ammonia, occurs less easily than the reaction of formula (3) above, resulting in a lower faradaic efficiency of ammonia production.

[0017] As a result of intensive research, the present inventors have found that ammonia can be produced with a higher faradaic efficiency than the prior art by using a cathode electrode including a nitride layer containing a nitride of Nb and / or V (hereinafter also referred to as the "first metal"), which are group 5 elements, and a metal layer containing a predetermined metal (one or more selected from the group consisting of Ru, Fe, and Co, hereinafter also referred to as the "second metal"). In a solid electrolyte electrochemical cell including the cathode electrode, ammonia is believed to be produced by the following cycle. (i) The lattice nitrogen of the nitride in the nitride layer is hydrogenated. (ii) The nitrogen hydride is released to produce ammonia. (iii) Nitrogen is adsorbed onto the metal layer, and the nitrogen enters the lattice nitrogen site after desorption. The nitrides of Nb and / or V, which are group 5 elements, convert protons H generated on the anode electrode side and introduced through the solid electrolyte, which are necessary for ammonia production. + (or hydride ion H - It is believed that the embodiment of the present invention is able to produce ammonia with a higher faradaic efficiency than the conventional technology because the hydrogen ions are easily conducted through the electrolyte and the reactions (i) to (iii) are easily promoted.

[0018] Furthermore, the present inventors have newly discovered that the reaction of the above formula (3) occurs less easily when the nitride has more nitrogen vacancies, and have found that ammonia can be produced with higher faradaic efficiency.

[0019] Furthermore, the present inventors have found that in the above solid electrolyte electrochemical cell, even if ammonia is generated by applying a voltage and the voltage is maintained, the amount of ammonia generated gradually decreases over time. Regarding this, the present inventors have considered that, among the above reactions (i) to (iii), the desorption reaction (ii) is rate-limiting, and that nitrogen hydride before desorption covers the electrode surface, making it more difficult for the nitrogen hydride to desorb. Therefore, the present inventors have found a method for repeatedly applying a voltage sufficient for ammonia generation to the above solid electrolyte electrochemical cell, and then lowering the voltage (including, for example, bringing the voltage to an open circuit voltage (OCV) or stopping the voltage application) so that only the desorption reaction (ii) proceeds. It has been found that this allows ammonia to be generated efficiently.

[0020] The following provides details of each requirement stipulated by the embodiment of the present invention.

[0021] <1. Cathode electrode for solid electrolyte electrochemical cells> The cathode electrode for a solid electrolyte electrochemical cell according to an embodiment of the present invention comprises a nitride layer including a nitride (hereinafter, sometimes referred to as "MNx") of a first metal (hereinafter, sometimes referred to as "M") which is at least one selected from the group consisting of Nb and V; and a metal layer on the nitride layer, the metal layer including a second metal, the second metal being at least one selected from the group consisting of Ru, Fe, and Co. By using this cathode electrode, ammonia can be produced with a higher faradaic efficiency than in the prior art.

[0022] (Nitride layer) In an embodiment of the present invention, the nitride layer includes a nitride of a first metal, which is at least one selected from the group consisting of Nb and V, which are group 5 elements. The nitride may have a rock-salt crystal structure. As described above, the nitride is formed by ionizing protons H generated on the anode electrode side and introduced through the solid electrolyte. + (or hydride ion H - ) is easily transmitted (hereinafter referred to as H + and H - The nitride layer is also called "hydrogen permeability" because of its high conductivity and the above-mentioned reactions (i) to (iii). + and H - Either one of the two may be mainly conducted, and in either case, it is considered that it can contribute to the production of ammonia with high faradaic efficiency.

[0023] The ratio (molar ratio) of nitrogen in the first metal nitride MNx is not particularly limited, and may be, for example, x=0.5 to 1.5. Note that x is preferably 0.6 or more, and more preferably 0.7 or more. This can stabilize the crystal structure of MNx. Also, x is preferably 1.1 or less. This makes it easier for the above reactions (i) to (iii) to proceed. Furthermore, x is more preferably less than 1.0. This allows nitrogen defects to be introduced into the nitride layer, and a higher faradaic efficiency of ammonia production can be obtained.

[0024] In one embodiment of the present invention, the nitride layer may contain the nitride of the first metal in a cross-sectional view parallel to the stacking direction at 50% by area or more, 75% by area or more, or 90% by area or more. The nitride layer may have a portion where the nitride of the first metal is continuous from one surface to the other surface in the stacking direction.

[0025] In the embodiment of the present invention, the thickness of the nitride layer is not particularly limited and may be, for example, the thickness of a typical cathode electrode in a solid electrolyte electrochemical cell. In the embodiment of the present invention, the nitride layer may be formed by a known method such as a sputtering method or a deposition method.

[0026] (metal layer) In an embodiment of the present invention, the metal layer is formed on the nitride layer and contains a second metal which is at least one selected from the group consisting of Ru, Fe and Co. The second metal is a catalyst that can be generally used in the Haber-Bosch process for synthesizing ammonia from nitrogen and hydrogen, and is considered to be likely to cause the nitrogen adsorption reaction of (iii) above.

[0027] In one embodiment of the present invention, the metal layer may contain the second metal in an amount of 50% or more, 75% or more, or 90% or more by area in a cross-sectional view parallel to the stacking direction. The metal layer may have a portion in which the second metal is continuous from one surface to the other surface in the stacking direction.

[0028] In the embodiment of the present invention, the thickness of the metal layer is not particularly limited and may be, for example, 1 nm to 100 nm, or 50 nm or less. In the embodiment of the present invention, the metal layer may be formed by a known method such as a sputtering method or a vapor deposition method.

[0029] <2. Solid electrolyte electrochemical cell> The solid electrolyte electrochemical cell according to the embodiment of the present invention includes the above-mentioned cathode electrode for solid electrolyte electrochemical cells (i.e., a metal layer and a nitride layer), a solid electrolyte layer, and an anode electrode, in this order, which allows ammonia to be produced with a higher faradaic efficiency than the conventional technology.

[0030] (Solid electrolyte layer) In the embodiment of the present invention, the solid electrolyte layer is not particularly limited, and may be, for example, a known ceramic material that conducts protons, such as a perovskite-type metal oxide, a ceramic material that conducts hydride ions, or a combination of these. In the embodiment of the present invention, the solid electrolyte layer may be formed by a known method.

[0031] (anode electrode) In the embodiment of the present invention, the anode electrode is not particularly limited, and may be made of a known material and may be formed by a known method. For example, a conductive material, a semiconducting material, or a dual conductive material that conducts oxide ions and electrons (holes) (La 1-x Sr x Chief of Staff 3-δ (LSC), LaSrCoO 4+δ (LSC4), LaNiO 3-δ (LNO), La 1-x Sr x Co 1-y Fe y O 3-δ (LSCF), La 1-x Sr x MnO 3-δ (LSM), Sm x Sr 1-x Chief of Staff 3-δ (SSC), or triple conducting materials that conduct protons, oxide ions and electrons (holes) (BaCo 1-x-y-z Fe x Zr y Y z O 3-δ (BCFZY), BaPr 1-x Y x O 3-δ (BPY), PrNi 1-x Co x O 3-δ (PNC), PrBa 1-x Sr x Co 2-y Fe y O 5+δ (PBSCF), NdBa 1-x Sr x Co2-y Fe y O 5+δ (NBSCF), PrBa 1-x Ca x Co2O 5+δ (PBCC), Ba 1-x Gd 0.8 La 0.2+x Co2O 6-δ In order to obtain a protonic ceramic reversible cell with better characteristics, the anode electrode preferably contains one or more of the dual conductive materials and / or one or more of the triple conductive materials, and more preferably contains one or more of the triple conductive materials.

[0032] The solid electrolyte electrochemical cell may include other layers without departing from the scope of the embodiments of the present invention. For example, the anode electrode and the solid electrolyte layer may be in direct contact with each other, or may not be in direct contact with each other, i.e., another layer may be present between the anode electrode and the solid electrolyte layer. The solid electrolyte layer and the nitride layer of the cathode electrode may be in direct contact with each other, or may not be in direct contact with each other, or may be in direct contact with each other, i.e., another layer may be present between the solid electrolyte layer and the nitride layer.

[0033] <3. Ammonia manufacturing method> A method for producing ammonia according to an embodiment of the present invention includes the steps of: supplying water vapor to the anode electrode and supplying nitrogen to the cathode electrode of the solid electrolyte electrochemical cell; and repeatedly increasing a voltage applied to the solid electrolyte electrochemical cell to generate ammonia and then decreasing the applied voltage, thereby enabling efficient generation of ammonia.

[0034] There are no particular limitations on the method of supplying the water vapor and nitrogen, such as the amount of supply, and they may be supplied to each electrode by a known method.

[0035] The applied voltage may be a voltage sufficient to generate ammonia (this may vary depending on the temperature, but for example, 1 V or more at 500°C). When the applied voltage is reduced after the generation of ammonia, the voltage may be reduced to, for example, less than the above voltage (such as the open circuit voltage), or the application of the voltage may be stopped. After the applied voltage is increased, it may be held for a certain period of time, or it may not be held. Even if held, the amount of ammonia generated may decrease over time, so the applied voltage may be reduced immediately. There is no particular limit to the time from the start of the reduction (or halt) until the applied voltage is increased again, and it may be appropriately adjusted so that the elimination reaction of (ii) above proceeds to a certain degree. EXAMPLES

[0036] The following examples are provided to more specifically describe the embodiments of the present invention. The embodiments of the present invention are not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all of these are included in the technical scope of the embodiments of the present invention.

[0037] <Preparation of solid electrolyte layer> The solid electrolyte layer is made of BaZr, a perovskite oxide and proton-conducting ceramic material. 0.4 Ce 0.4 Y 0.1 Yb 0.1 O 3-δ (hereinafter also referred to as "BZCYYb4411") was produced by the solid phase method as follows. BaCO3 (Kojundo Chemical, purity 99.95%), ZrO2 (Kojundo Chemical, purity 98%), CeO2 (Kojundo Chemical, purity 99.99%), Y2O3 (Kojundo Chemical, purity 99.99%), and Yb2O3 (Kojundo Chemical, purity 99.9%) were weighed out according to the stoichiometric ratio and wet mixed in a planetary ball mill. The mixture was calcined at 1100°C, mixed again in a ball mill, and finally heated at 1600°C for 12 hours to obtain a sintered body of BZCYYb4411.

[0038] The sintered body was analyzed by X-ray diffraction and found to have a cubic perovskite structure with a lattice constant a of 4.326 Å and a theoretical density of 6.237 g cm for BZCYYb4411. -3 The relative density to the total was 97%. Fig. 1A shows an optical microscope photograph of the top surface of the sintered body, Fig. 1B shows an optical microscope photograph of the side surface of the sintered body (part of the sintered body is held with tweezers), and Fig. 2 shows a cross-sectional SEM image of the sintered body. From Fig. 2, the particle size of BZCYYb4411 was about 3 to 5 μm.

[0039] <Preparation of nitride layer for cathode electrode> As the nitride layer of the cathode electrode, a V nitride (VNx) layer (1 μm) was formed on the solid electrolyte layer by reactive RF-sputtering using a magnetron sputtering device (ULVAC, MPS-3000) as follows. The metal target used was a V target with a purity of 99.9% and a diameter of 2 inches. First, the pressure in the chamber was set at about 1.0×10 -5 After exhausting the gas until the pressure was below 1 Pa, the substrate temperature was heated to 100°C. Then, a mixed gas of high purity argon gas (99.999%) and ultra-high purity nitrogen gas (99.9995%) was supplied into the chamber at a total supply rate of 20 sccm, of which the nitrogen supply rate was 50% (10 sccm). At this time, the chamber pressure was about 0.4 Pa. Next, using a high frequency power supply, the target output was adjusted to 150 W and the helicon coil output to 50 W, and sputtering was performed for a specified time while rotating the substrate so that the thickness was 1 μm, obtaining a VNx layer. The nitrogen supply rate was changed from the above conditions to 5% (1 sccm) and 2.5% (0.5 sccm) of the total gas supply rate to fabricate different VNx layers. These VNx layers were also fabricated on Si wafers under the same conditions for analysis.

[0040] X-ray diffraction patterns (X-ray source: CuKα) were obtained for the VNx layers. The results are shown in Figure 3. Figure 3 shows, from the top, the XRD patterns of VNx layers fabricated with nitrogen supply amounts of 50% (Ar / N2: 10 / 10), 5% (Ar / N2: 19 / 1), and 2.5% (Ar / N2: 19.5 / 0.5), as well as the XRD pattern of a general rock-salt VNx layer for reference. As can be seen from Figure 3, all of the VNx layers had a rock-salt crystal structure. The composition of the VNx layers was analyzed by EPMA, including the amount of oxygen impurities, and the results are shown in Table 1.

[0041] [Table 1]

[0042] As shown in Table 1, the VNx layer fabricated with the nitrogen supply amount during sputtering set to 50% of the total gas supply amount had an excess of nitrogen, while the VNx layer fabricated with the nitrogen supply amount during sputtering set to 2.5% of the total gas supply amount had a nitrogen deficiency. Hereinafter, the VNx layer fabricated with the nitrogen supply amount during sputtering set to 50% of the total gas supply amount is referred to as "VN 1.1 " and the VNx layer prepared with the nitrogen supply amount set to 2.5% of the total gas supply amount was described as "VN 0.9 " should be written.

[0043] <Preparation of metal layer for cathode electrode> As the metal layer of the cathode electrode, a Ru layer (50 nm) or an Fe layer (50 nm) was formed on the nitride layer by DC sputtering. For comparison, a cathode electrode without the Ru layer or the Fe layer was also prepared.

[0044] <Evaluation of hydrogen permeability of cathode electrode> On the cathode side and the opposite side surface of the solid electrolyte (BZCYYb4411) layer, Pt paste was screen-printed as an anode electrode, and the cathode electrodes were different in Test No. 1 (cathode electrode: VN 0.9 ), No.2 (cathode electrode: VN 0.9 / Ru), No.3 (cathode electrode: VN 1.1) and No. 4 (cathode electrode: VN 1.1 A solid electrolyte electrochemical cell using ZnO (ZnO / Ru) was fabricated.

[0045] The hydrogen permeability was evaluated for the cells of test Nos. 1 to 4. Specifically, for each cell, Ar was supplied to the cathode electrode side, and a mixed gas of 3% H2O / 20% H2 / Ar was supplied to the anode electrode side, and an open circuit voltage (OCV) was applied to the cathode electrode for 1 hour, followed by -1.5 V for 1 hour, and the current density was measured when this was repeated. At the same time, a gas chromatograph (GC) was placed on the cathode electrode side, and the hydrogen permeation flux (J H2 ) was measured.

[0046] 4 to 7 show the hydrogen permeability evaluation results of Test Nos. 1 to 4. In FIG. 4 to FIG. 7, the plots of "x" indicate the hydrogen permeation flux (J H2 ) and the solid line indicates the current density. As shown in FIG. 4, in Test No. 1 (cathode electrode: VN 0.9 ) are the absolute value of the current density and the hydrogen permeation flux (J H2 ) was low. As shown in FIG. 5, in Test No. 2 (cathode electrode: VN 0.9 / Ru) shows the absolute current density and hydrogen permeation flux (J H2 ) was clearly increased. As shown in FIG. 6, in Test No. 3 (cathode: VN 1.1 ) shows that the absolute value of the current density and the hydrogen permeation flux (J H2 ) was clearly increased. As shown in FIG. 7, in Test No. 4 (cathode electrode: VN 1.1 / Ru) showed a larger absolute value of current density and hydrogen permeation flux (J H2 ) was increasing. Table 2 shows the current density and hydrogen flux increase (ΔJ H2 ) are summarized here. Here, ΔJH2 is the average of J at OCV H2 and the difference from J when a steady state is reached with an applied voltage of -1.5 V H2 was determined as such.

[0047]

Table 2

[0048] It can be seen from Table 2 that in both Test No. 2 and Test No. 4, since the absolute value of the current density and the increase in hydrogen flux (ΔJ H2 ) are large when a voltage of -1.5 V is applied, it was found that each cell including the nitride layer has sufficient hydrogen permeability (proton or hydride ion conductivity). Also, when comparing Test No. 1 and Test No. 3, it is considered that the VN 0.9 layer has low activity for the hydrogen generation reaction, while the VN 1.1 layer has high activity for the hydrogen generation reaction. Also, when comparing Test No. 1 and No. 2, since the addition of a Ru catalyst layer to the VN 0.9 surface significantly improves the activity of the hydrogen generation reaction, it is considered that in Test No. 2, hydrogen generation occurs at the VN 0.9 / Ru / gas phase triple-phase interface. Although cross-sectional SEM images of each cell were obtained before and after the hydrogen permeability evaluation, no particular changes were observed in each layer of each cell before and after the evaluation.

[0049] <H2O-N2 Co-electrolysis Test ~ I-V Curve Evaluation ~> The anode electrodes of Test No. 1 to 4 were changed from Pt to those screen-printed with PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+σ (PBSCF) to fabricate solid oxide electrochemical cells for Test No. 5 to 8. For comparison, a solid oxide electrochemical cell for Test No. 9 with only a Ru layer (50 nm) as the cathode electrode was also fabricated. Cross-sectional SEM images of each cell were obtained. As an example, Fig. 8A shows a cross-sectional SEM image of Test No. 6, and Fig. 8B shows a cross-sectional SEM image of Test No. 8. From Figs. 8A and 8B, it can be seen that VN 0.9 Layer 1a, VN 1.1 Both layer 1b and BZCYYb4411 layer 2 were confirmed to be dense layers.

[0050] For the cells of Test Nos. 5 to 9, a H2O-N2 co-electrolysis test was carried out by supplying nitrogen to the cathode electrode side and a mixed gas of 3% H2O / Ar to the anode electrode side and applying a voltage. Figure 9 shows the results of Test No. 5 (cathode: VN 0.9 ) and No.6 (cathode electrode: VN 0.9 10 shows the IV curves of Test No. 7 (cathode electrode: VN / Ru) at 500 °C and 600 °C. 1.1 ) and No.8 (cathode electrode: VN 1.1 10 shows the IV curves of Test No. 1 (cathode electrode: Ru) at 500°C and 600°C, and FIG. 11 shows the IV curves of Test No. 9 (cathode electrode: Ru) at 500°C and 600°C. In both cases, a higher current density was observed at 600°C than at 500°C. Table 3 shows the current density values ​​at 600°C and -1.8V for the cells of Test Nos. 5 to 9.

[0051] [Table 3]

[0052] The following can be seen from Table 3. Test No. 5 has an absolute value of the current density at -1.8 V that is smaller by more than one order of magnitude than Test No. 9. This is because, as mentioned above, VN 0.9 This is consistent with the low activity of the Ru cathode for the hydrogen evolution reaction. In Test No. 6, the absolute value of the current density was about 20 times that of Test No. 5, and the current density was almost the same as that of the Ru cathode. Test No. 7 showed a current density at -1.8 V that was approximately 1.8 times that of Test No. 9. 1.1suggests that it is more active than Ru for the hydrogen generation reaction on the solid electrolyte. Furthermore, in Test No. 8, the absolute value of the current density increased by about 1.3 times compared to Test No. 7. From the above, VN 0.9 / Ru and VN 1.1 / Ru, it is considered that the hydrogen generation reaction proceeds at the triple-phase interface of the VN layer / Ru layer / gas phase.

[0053] <D2O-N2 Coelectrolysis Test ~ Evaluation of Hydrogen and Ammonia Generation Amounts ~> To facilitate the detection of ammonia, from the above H2O-N2 coelectrolysis test, H2O (water vapor) was changed to D2O (water vapor of heavy water), and a D2O-N2 coelectrolysis test was conducted for the cells of Test Nos. 5 to 9. As a result of evaluating the I-V curves of Test Nos. 6, 8, and 9, a tendency similar to that of the above H2O-N2 coelectrolysis test was obtained.

[0054] Figure 12 shows the cell voltage change when electrolysis was performed for 10 minutes at 600 °C and a constant current density of -6 mA·cm -2 for each cell of Test Nos. 6, 8, and 9. In each case, when held at a constant current density of -6 mA·cm -2 for 10 minutes, Test Nos. 6 and 8 maintained a substantially constant cell voltage at -1.5 V, and Test No. 9 maintained a substantially constant cell voltage at -1.3 V.

[0055] Figure 13 shows the signal intensities of D2 (the upper three solid lines in the figure, m / z = 4) and ND3 (the lower three solid lines in the figure, m / z = 20) in the MASS spectrum when electrolysis was performed for 600 seconds at 600 °C and a constant current density of -6 mA·cm -2 100 seconds after the start for each cell of Test Nos. 6, 8, and 9. As shown by the upper three solid lines in Figure 13, deuterium D2 decreased rapidly when the current was interrupted, but as shown by the lower three solid lines in Figure 13, heavy ammonia ND3 was observed to continue for some time after the current interruption and decreased over about 10 minutes. This is considered to show that, as described above, the desorption reaction (ii) during ammonia generation is rate-determining and the gradually desorbed ND3 is being detected. For D2 and ND3, the amount (mol) of the product was calculated from the total peak area in Figure 13, and the ammonia yield and Faraday efficiency were calculated by comparing with the total amount of electricity that flowed. The results are shown in Table 4.

[0056] [Table 4]

[0057] The following can be seen from Table 4: Test Nos. 6 and 8 are examples that satisfy the requirements of the embodiment of the present invention, and a higher Faraday efficiency (for example, more than 1%) than the conventional one was obtained. Furthermore, Test No. 6 is an example that satisfies a more preferable requirement of the embodiment of the present invention (x of the VNx layer is less than 1.0), and an even higher Faraday efficiency was obtained. Furthermore, the metal layer of Test No. 6 was changed from a Ru layer to an Fe layer (50 nm) to prepare a solid electrolyte electrochemical cell of Test No. 10, and the production efficiency and Faraday efficiency of each gas were calculated in the same manner. The results are shown in Table 5.

[0058] [Table 5]

[0059] The following can be seen from Table 5: Test No. 10 is an example that satisfies the requirements of the embodiment of the present invention, and a higher Faraday efficiency (for example, more than 1%) than the conventional one was obtained. Furthermore, Test No. 10 is an example that satisfies a more preferable requirement of the embodiment of the present invention (x of the VNx layer is less than 1.0), and an even higher Faraday efficiency was obtained.

[0060] Figure 14A shows the results for Test No. 6 at 600°C and -8mA cm -2 FIG. 14B shows the voltage-time curves when D2O-N2 co-electrolysis was performed for 10 hours at a constant current density of 1000 mA, and FIG. 14B shows the signal intensities of D2 and ND3 in the MASS spectrum. As shown in FIG. 14B, D2 generation occurs at a constant rate, whereas ND3 generation does not occur after about 2 hours. This is because VN0.9 This indicates that the surface is covered with an ammonia chemisorption layer, inhibiting the ammonia production reaction.

[0061] Figure 15 shows the results for Test No. 6 at 600℃ and -6mA cm -2 15 shows the signal intensities of D2 and ND3 in the MASS spectrum when a cycle of D2O-N2 co-electrolysis at a constant current density of 1000 s, followed by holding at an open circuit potential (OCV) to desorb ND3, was repeated 10 times. As shown in FIG. 15, it can be seen that when ammonia desorption is promoted by holding at an open circuit potential, ND3 production is reactivated in the next cycle. Thus, in the embodiment of the present invention, although catalyst deactivation may occur due to ammonia chemisorption, it is believed that activity can be restored and ammonia can be efficiently produced by desorbing the adsorption layer (specifically, by increasing and then decreasing the voltage applied to the solid electrolyte electrochemical cell). [Explanation of symbols]

[0062] 1a VN 0.9 layer 1b VN 1.1 layer 2 BZCYYb4411 layer

Claims

1. a nitride layer including a nitride of a first metal, which is at least one selected from the group consisting of Nb and V; a metal layer formed on the nitride layer and containing a second metal, the second metal being at least one selected from the group consisting of Ru, Fe and Co.

2. 2. The cathode electrode for a solid electrolyte electrochemical cell according to claim 1, wherein, when said first metal is M and said nitride is MNx, x is 0.6 to 1.

1.

3. 3. A solid electrolyte electrochemical cell comprising the cathode electrode for a solid electrolyte electrochemical cell according to claim 1, a solid electrolyte layer, and an anode electrode, in this order.

4. 4. The solid electrolyte electrochemical cell according to claim 3, further comprising: supplying water vapor to the anode electrode and supplying nitrogen to the cathode electrode; Repeating the process of increasing a voltage applied to the solid electrolyte electrochemical cell to generate ammonia and then decreasing the applied voltage; A method for producing ammonia, comprising: