Polymer coagulant and method for producing the same, and sludge dewatering method
A water-in-oil emulsion polymer flocculant with (meth)allyl sulfonate and nonionic or cationic monomers forms a comb-shaped structure to enhance charge neutralization and flocculation, addressing the inefficiencies of conventional flocculants by achieving low moisture content and high filtration rates in difficult-to-dewater sludge.
Patent Information
- Application Number
- JP2023085834
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional polymer flocculants struggle with low solid content and high water content in difficult-to-dewater sludge, lacking effective charge neutralization and flocculation properties, leading to inefficient dewatering and high moisture content in the dehydrated cake.
A polymer flocculant in the form of a water-in-oil emulsion containing (meth)allyl sulfonate and a nonionic or cationic monomer, without crosslinkable monomers, forming a comb-shaped structure with a trunk and branch polymer configuration, enhancing charge neutralization and flocculation performance.
The polymer flocculant achieves excellent flocculation properties, large floc diameter, and low moisture content in the dehydrated cake with a low additive amount, improving filtration rate and filtrate appearance.
Smart Images

Figure 2024168838000001 
Figure 2024168838000002 
Figure 2024168838000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer flocculant and a method for producing the same, and more particularly to a polymer flocculant in the form of a water-in-oil emulsion having excellent dehydration and flocculation performance, and a method for producing the same. [Background technology]
[0002] Polymer flocculants are used for the purpose of flocculating, settling and separating suspended solids contained in domestic and industrial wastewater, etc., and as retention aids in the paper industry, and as admixtures and muddying agents in civil engineering and construction. Of these, cationic polymer flocculants are mainly used for the dehydration treatment of domestic and industrial wastewater sludge, but for organic sludge that is difficult to dehydrate because of low solids, low fibrous content in the organic components, decayed organic components, or high salt concentration, water-in-oil emulsion polymer flocculants containing cross-linked polymers using small amounts of known bifunctional or higher cross-linking monomers such as methylenebisacrylamide are used.
[0003] Patent Document 1 describes a papermaking additive and its manufacturing method. This papermaking additive is a graft polymer containing a monomer unit consisting of sodium methallylsulfonate in the main chain. However, the use of sodium methallylsulfonate in the side chain is not disclosed. In addition, the additive is manufactured by aqueous solution polymerization, and there is no disclosure of its manufacture by emulsion polymerization. Patent Document 2 describes an aqueous solution of an acrylamide polymer. However, the solution is produced by aqueous solution polymerization, and there is no disclosure of production by emulsion polymerization. Furthermore, in order to obtain the molecular weight required for a polymer flocculant, the viscosity of the reaction solution increases extremely in these aqueous solution polymerizations, causing the reaction solution to turn into a gel immediately after the start of polymerization, making it impossible to control the molecular structure.
[0004] These are structurally not significantly different from conventional polymer flocculants, and have not been able to significantly improve the tendency for the amount added to increase. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 3125409 [Patent Document 2] Patent No. 3803670 Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a polymer flocculant consisting of a high-performance water-in-oil emulsion which has excellent flocculation properties for difficult-to-dewater sludge by improving its charge neutralization ability with sludge particles while maintaining the three-dimensional structure of the polymer, has a large floc diameter, is excellent in filtration rate and appearance of filtrate, can be effectively dewatered, and can produce a dehydrated cake with a low moisture content with a small amount of addition, and a method for producing the same. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have discovered that a polymer segment (s) containing at least a (meth)allyl sulfonate and a nonionic monomer or a cationic monomer as constituent units and not containing a monomer unit derived from a crosslinkable monomer, a polymer segment (m) having at least a nonionic monomer or a cationic monomer as a constituent unit and not containing a monomer unit derived from a crosslinkable monomer; The molecule has both of the following: The inventors have found that a polymer flocculant comprising a water-in-oil emulsion containing a polymer in which two or more of the polymer moieties (s) are bonded to a polymer moiety (m) can solve the above problems, and have completed the present invention.
[0008] The present invention which solves the above problems is described below.
[0009] [1] A polymer segment (s) having at least a (meth)allyl sulfonate salt and a nonionic monomer or a cationic monomer as constituent units and not containing a monomer unit derived from a crosslinkable monomer; a polymer segment (m) having at least a nonionic monomer or a cationic monomer as a constituent unit and not containing a monomer unit derived from a crosslinkable monomer; The molecule has both of the following: A polymer flocculant comprising a water-in-oil emulsion containing a comb polymer in which two or more of the polymer portions (s) are bonded to the polymer portion (m), the polymer portion (m) serves as a trunk polymer, and the polymer portion (s) serves as a branch polymer.
[0010] [2] The polymer flocculant according to [1], wherein a ratio of the monomer units constituting the polymer portion (s) to the monomer units constituting the polymer portion (m) is 25 / 75 to 70 / 30 in mass ratio.
[0011] [3] The polymer flocculant according to any one of [1] to [2], wherein the content of the monomer units derived from the (meth)allylsulfonate is 300 to 5000 ppm relative to the monomer units constituting the polymer portion (s).
[0012] [4] The cationic monomer is represented by the following general formula (1): CH 2 =CR 1 -CO-XQN + R 2 R 3 R 4 Z - ···(1) (In the general formula (1), R 1 is a hydrogen atom or a methyl group, R 2 and R 3 each independently represents an alkyl group having 1 to 3 carbon atoms or a benzyl group; R 4 represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different; X represents an oxygen atom or NH; Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms; Z -indicates the counter anion.) The polymer flocculant according to any one of [1] to [3], comprising one or more cationic monomers represented by the following formula:
[0013] [5] The polymer flocculant according to [4], wherein the cationic monomer is at least one of a quaternary salt of methyl chloride of dimethylaminoethyl acrylate and a quaternary salt of methyl chloride of dimethylaminoethyl methacrylate.
[0014] [6] The polymer flocculant according to any one of [1] to [5], wherein the content of the monomer units derived from the cationic monomer in the polymer portion (s) is 35 mol % or more relative to the monomer units constituting the polymer portion (s).
[0015] [7] The polymer flocculant according to any one of [1] to [6], wherein the content of the monomer units derived from the cationic monomer in the polymer portion (m) is 30 mol % or more relative to the monomer units constituting the polymer portion (m).
[0016] [8] The polymer flocculant according to any one of [1] to [7], wherein the content of the monomer units derived from the cationic monomer in the polymer is 31 mol % or more based on the total amount of the monomer units constituting the polymer portion (s) and the polymer portion (m).
[0017] [9] In a frequency dependency measurement (25°C) using a rheometer, the angular frequency (A) at which the storage modulus and loss modulus of a 0.5% by mass aqueous solution of the polymer are equal to each other is divided by the angular frequency (B) at which the storage modulus and loss modulus of a 0.1% by mass aqueous solution of the polymer are equal to each other, and the value (A / B) satisfies the following formula (1): 0.005 ≦ (A / B) ≦ 0.1 Formula (1) and a value (C / D) obtained by dividing a storage modulus (C) of a 0.5% by mass aqueous solution of the polymer at the angular frequency (A) by a storage modulus (D) of a 0.1% by mass aqueous solution of the polymer at the angular frequency (B) satisfies the following formula (2): 0.5 ≦ (C / D) ≦ 3.0 Formula (2) The polymer flocculant according to any one of [1] to [8], which satisfies the above.
[0018]
[10] A polymeric flocculant comprising a water-in-oil emulsion containing a polymer having at least a (meth)allyl sulfonate salt and a nonionic monomer or a cationic monomer as structural units, In a frequency dependency measurement (25° C.) using a rheometer, the angular frequency (A) at which the storage modulus and loss modulus of a 0.5% by mass aqueous solution of the polymer are equal to each other is divided by the angular frequency (B) at which the storage modulus and loss modulus of a 0.1% by mass aqueous solution of the polymer are equal to each other, and the value (A / B) is expressed by the following formula (1): 0.005 ≦ (A / B) ≦ 0.1 Formula (1) and a value (C / D) obtained by dividing a storage modulus (C) of a 0.5% by mass aqueous solution of the polymer at the angular frequency (A) by a storage modulus (D) of a 0.1% by mass aqueous solution of the polymer at the angular frequency (B) satisfies the following formula (2): 0.5 ≦ (C / D) ≦ 3.0 Formula (2) A polymer flocculant characterized by satisfying the above.
[0019]
[11] The polymer flocculant according to
[10] , wherein the polymer does not contain a monomer unit derived from a crosslinkable monomer.
[0020]
[12] The polymer flocculant according to
[10] or
[11] , wherein the polymer is a comb polymer having a trunk polymer and a branch polymer.
[0021]
[13] The cationic monomer is represented by the following general formula (1): CH 2 =CR 1 -CO-XQN + R 2 R 3 R 4 Z - ···(1) (In the general formula (1), R 1 is a hydrogen atom or a methyl group, R2 and R 3 each independently represents an alkyl group having 1 to 3 carbon atoms or a benzyl group; R 4 represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different; X represents an oxygen atom or NH; Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms; Z - indicates the counter anion.) The polymer flocculant according to any one of
[10] to
[12] , comprising one or more cationic monomers represented by the following formula:
[0022]
[14] The polymer flocculant according to
[13] , wherein the cationic monomer is at least one of a quaternary salt of methyl chloride of dimethylaminoethyl acrylate and a quaternary salt of methyl chloride of dimethylaminoethyl methacrylate.
[0023]
[15] The polymer flocculant according to any one of
[10] to
[14] , wherein the content of the monomer units derived from the cationic monomer in the polymer is 31 mol % or more based on the total amount of the monomer units constituting the polymer.
[0024]
[16] A method for producing the polymer flocculant according to any one of [1] to
[15] , a first polymerization step of subjecting a first monomer composition containing at least a (meth)allylsulfonate salt and a nonionic monomer or a cationic monomer to water-in-oil emulsion polymerization in the presence of an oil and a first surfactant to obtain a water-in-oil emulsion containing a first polymer; a second polymerization step of mixing the water-in-oil emulsion containing the first polymer with a second surfactant and a second monomer composition containing at least a nonionic monomer or a cationic monomer to carry out polymerization; A method for producing a polymer flocculant, comprising the steps of:
[0025]
[17] The method for producing a polymer flocculant according to
[16] , wherein the surfactant present in the second polymerization step is a nonionic surfactant having an HLB value of 7 to 10.
[0026]
[18] The method for producing a polymer flocculant according to
[16] or
[17] , wherein the second surfactant is a combination of sorbitan sesquioleate and polyoxyethylene sorbitol tetraoleate.
[0027]
[19] A method for dewatering sludge, comprising adding the polymer flocculant according to any one of [1] to
[15] to sludge. Effect of the Invention
[0028] The polymer flocculant of the present invention improves the charge neutralization ability with sludge particles while maintaining the three-dimensional structure of the polymer, and therefore has excellent flocculation properties for difficult-to-dewater sludge, large floc diameters, excellent filtration speed and filtrate appearance, and can effectively dewater sludge, producing a dewatered cake with a low moisture content with a small amount of addition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The present invention will be described in detail below. In this specification, acrylate and / or methacrylate are referred to as (meth)acrylate, acrylamide and / or methacrylamide are referred to as (meth)acrylamide, acrylic acid and / or methacrylic acid are referred to as (meth)acrylic acid, allylsulfonic acid and / or methallylsulfonic acid are referred to as (meth)allylsulfonic acid, and an acid and its salt are referred to as an acid (salt).
[0030] The first polymer flocculant of the present invention comprises a polymer portion (s) having at least a (meth)allyl sulfonate and a nonionic monomer or a cationic monomer as constituent units and not including a monomer unit derived from a crosslinkable monomer; a polymer segment (m) having at least a nonionic monomer or a cationic monomer as a constituent unit and not containing a monomer unit derived from a crosslinkable monomer; The molecule has both of the following: The emulsion is characterized by being made of a water-in-oil type emulsion containing a polymer in which two or more polymer portions (s) are bonded to a polymer portion (m), i.e., it contains a graft copolymer consisting of a polymer portion (m) and a polymer portion (s).
[0031] The graft copolymer constituting this polymer flocculant is a comb polymer with the polymer portion (m) as the trunk polymer and the polymer portion (s) as the branch polymer. By forming such a comb polymer, the branch polymer portion reacts with sludge, improving the performance of the polymer flocculant. In addition, even if the molecular weight is increased, the dispersibility in sludge and the like is high, and the reactivity with sludge is likely to be high. Because of the comb structure, when dissolved in water and reacted with sludge, it forms a three-dimensional structure in the aqueous solution compared to linear polymers, and the structure is not as hard as that of cross-linked polymers, so the side chains react easily with sludge and are effectively neutralized, so it is believed that a dehydrated cake with a low water content can be obtained even with a small amount added.
[0032] (Meth)allyl sulfonate is believed to have a chain transfer function and a function of forming a terminal double bond after polymerization, and is therefore useful for forming a comb polymer. As the (meth)allyl sulfonate, it is preferable to use sodium methallyl sulfonate or sodium allyl sulfonate, and it is particularly preferable to use sodium methallyl sulfonate.
[0033] The content of the monomer units derived from the (meth)allylsulfonate salt in the polymer is not particularly limited, but is preferably 300 to 5000 ppm, more preferably 500 to 4000 ppm, relative to the monomer units constituting the polymer portion (s). If it is less than 300 ppm, the amount of the branch polymer of the comb polymer is insufficient, and if it exceeds 5000 ppm, the molecular weight of the branch polymer becomes small, and in either case, the function as a flocculant is likely to decrease.
[0034] The nonionic monomer is not particularly limited, but examples thereof include (meth)acrylamide-based compounds represented by the following chemical formula (2), as well as alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and hydroxyethyl (meth)acrylate, styrene, acrylonitrile, and vinyl acetate. Among these nonionic monomers, the (meth)acrylamide-based compounds represented by the following chemical formula (2) are preferred because they have excellent copolymerizability with cationic monomers, are easily polymerized to a high molecular weight, which is necessary for a polymer flocculant, and have excellent performance as a polymer flocculant.
[0035] CH 2 =CR 1 -CO-NR 2 R 3 ···(2)
[0036] In the above chemical formula (2), R 1 is a hydrogen atom or a methyl group, R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms.
[0037] Among these (meth)acrylamide compounds, acrylamide is most preferred because it is water-soluble and has particularly excellent performance as a polymer flocculant. These nonionic monomers may be used alone or in combination of two or more kinds.
[0038] The content of monomer units derived from nonionic monomers in the polymer is not particularly limited, but is preferably from 0 to 69 mol %, and more preferably from 2 to 65 mol %. The content ratio of monomer units derived from nonionic monomers in the polymer portion (s) of the polymer is preferably 0 to 65 mol %, more preferably 2 to 60 mol %, and particularly preferably 5 to 50 mol %, relative to the monomer units constituting the polymer portion (s). The content of monomer units derived from nonionic monomers in the polymer portion (m) of the polymer is preferably 0 to 70 mol %, more preferably 2 to 65 mol %, and particularly preferably 5 to 50 mol %, based on the monomer units constituting the polymer portion (m).
[0039] The cationic monomer is a monomer having a radically polymerizable double bond and a cationic group that can be radically polymerized, and includes a compound represented by the following general formula (1) as well as a diallyldialkylammonium halide such as diallyldimethylammonium chloride. Among these cationic monomers, the compound represented by the following general formula (1) is preferred because it has excellent radical polymerization reactivity, is easy to increase the molecular weight required for a polymer flocculant, and the resulting water-soluble polymer has excellent performance as a polymer flocculant.
[0040] CH 2 =CR 1 -CO-XQN + R 2 R 3 R 4 Z - (1)
[0041] In the general formula (1), R 1 is a hydrogen atom or a methyl group, R 2 and R 3 each independently represents an alkyl group having 1 to 3 carbon atoms or a benzyl group; R 4 represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different; X represents an oxygen atom or NH; Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms; Z - indicates the counter anion. Z - Examples of the ions include halide ions such as chloride ions and sulfate ions.
[0042] Specific examples of the cationic monomer represented by the general formula (1) include hydrochlorides and sulfates of dialkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylamino-2-hydroxypropyl (meth)acrylate, and dialkylaminoalkyl (meth)acrylamides such as dimethylaminopropyl (meth)acrylamide, etc. In addition, quaternary salts of dialkylaminoalkyl (meth)acrylates and dialkylaminoalkyl (meth)acrylamides with alkyl halides such as methyl chloride, benzyl halide adducts such as benzyl chloride, and dialkyl sulfate adducts such as dimethyl sulfate, etc., are exemplified.
[0043] Among these preferred cationic monomers, the most preferred are the quaternary salts of methyl chloride adducts of dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate, which are easily polymerized to a high molecular weight, as required for polymer flocculants. These cationic monomers may be used alone or in combination of two or more.
[0044] The content of the monomer units derived from the cationic monomer in the polymer is preferably 31 mol% or more, more preferably 35 to 95 mol%, and most preferably 40 to 85 mol%, based on the total amount of the monomer units constituting the polymer. If it is less than 31 mol%, the charge of the sludge particles cannot be sufficiently neutralized, the flocs are not tightly packed, and the moisture content increases. The content of the monomer units derived from the cationic monomer in the polymer portion (s) of the polymer is preferably 35 mol % or more, and more preferably 40 to 95 mol %, based on the monomer units constituting the polymer portion (s). The content of the monomer units derived from the cationic monomer in the polymer portion (m) of the polymer is preferably 30 mol % or more, and more preferably 35 to 95 mol %, based on the monomer units constituting the polymer portion (m).
[0045] The above polymer does not contain any monomer unit derived from a crosslinkable monomer. Here, "not containing" includes not only the case where it does not contain any monomer unit at all, but also the case where it does not contain substantially any monomer unit. "Substantially not containing" refers to the case where the content of the monomer unit derived from the crosslinkable monomer is less than 1 ppm.
[0046] The polymer flocculant of the present invention has the above-mentioned graft copolymer as its main component, but may also contain other polymers in addition to the graft copolymer, and the other polymers may contain monomer units derived from crosslinkable monomers.
[0047] Of the polymers contained in the polymer flocculant of the present invention, it is preferable that 90% by mass or more is the above-mentioned graft copolymer, more preferably 95% by mass or more, and even more preferably 99% by mass or more, and of course it may be 100% by mass.
[0048] In the present invention, among the monomers copolymerizable with the above-mentioned monomers, any monomer can be used without particular limitation, so long as it is a monomer excluding a crosslinkable monomer having two or more functionalities. As the copolymerizable monomer, the anionic monomers exemplified below can be used.
[0049] Examples of the anionic monomer include (meth)acrylic acid and salts thereof, as well as vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, maleic acid, and salts thereof. Among these anionic monomers, (meth)acrylic acid and salts thereof are preferred because they are easy to increase in molecular weight, which is necessary for a polymer flocculant, and have excellent performance as a polymer flocculant. As salts, ammonium salts and alkali metal salts such as sodium salts and potassium salts are preferred. These anionic monomers may be used alone or in combination of two or more.
[0050] In the present invention, the ratio of the monomer units contained in the polymer portion (s) to the monomer units contained in the polymer portion (m) is preferably 25 / 75 to 70 / 30 by mass. If the ratio of the polymer portion (s) is less than 25% by mass, the moisture content of the dehydrated cake does not decrease, and if it exceeds 70% by mass, flocs may not be formed. A more preferred ratio is 35 / 65 to 65 / 35.
[0051] The content of the graft copolymer in the water-in-oil emulsion is preferably 25 to 55% by mass, and more preferably 30 to 50% by mass, based on the emulsion.
[0052] The water-in-oil emulsion polymer flocculant of the present invention preferably has a viscoelasticity of its aqueous solution that satisfies the following condition: In frequency-dependent measurement (25° C.) using a rheometer, the angular frequency (A) at which the storage modulus and loss modulus of a 0.5% by mass aqueous solution of the polymer are equal is divided by the angular frequency (B) at which the storage modulus and loss modulus of a 0.1% by mass aqueous solution of the polymer are equal is expressed as A / B by the following formula (1): 0.005 ≦ (A / B) ≦ 0.1 Formula (1) and a value (C / D) obtained by dividing a storage modulus (C) of a 0.5% by mass aqueous solution of the polymer at the angular frequency (A) by a storage modulus (D) of a 0.1% by mass aqueous solution of the polymer at the angular frequency (B) satisfies the following formula (2): 0.5 ≦ (C / D) ≦ 3.0 Formula (2) It is preferable that the following is satisfied. When (A / B) and (C / D) are within this range, the reaction with sludge is high and firm flocs are formed, and a dehydrated cake with a low moisture content can be obtained even with a small amount of addition. If (A / B) is greater than 0.1, the number of polymer segments (s) that are branch polymers relative to the polymer segments (m) that are trunk polymers decreases, and the flocs do not compact, tending to have a high moisture content. If (A / B) is less than 0.005, the polymer segments (s) that are branch polymers become too short and numerous, resulting in insufficient floc formation. A more preferable range for (A / B) is 0.01≦(A / B)≦0.09. If (C / D) is less than 0.5, the polymer portion (s) which is the branch polymer is too short, and the moisture content tends to be high. If (C / D) is more than 3.0, the polymer portion (s) is long, and the branch polymers become entangled with each other, so it may be necessary to increase the amount added to the sludge. The more preferable range for (C / D) is 0.6≦y≦2.8. Both the conventional crosslinked polymers and linear polymers are far outside the above range, which indicates that the polymer of the present invention has a unique structure.
[0053] Therefore, if the viscoelasticity of the aqueous solution of the polymer flocculant of the first invention satisfies the above-mentioned relationship, it can be determined that the polymer flocculant is composed of a comb polymer in which two or more polymer moieties (s) are bonded to a polymer moiety (m), and the invention can also be specified as follows. This polymer flocculant is not different from the above-mentioned first polymer flocculant of the present invention, but the method of specifying it has been changed. A polymer flocculant comprising a water-in-oil emulsion containing a polymer having at least a (meth)allyl sulfonate salt and a nonionic monomer or a cationic monomer as structural units, In a frequency dependency measurement (25° C.) using a rheometer, the angular frequency (A) at which the storage modulus and loss modulus of a 0.5% by mass aqueous solution of the polymer are equal to each other is divided by the angular frequency (B) at which the storage modulus and loss modulus of a 0.1% by mass aqueous solution of the polymer are equal to each other, and the value (A / B) is expressed by the following formula (1): 0.005 ≦ (A / B) ≦ 0.1 Formula (1) and a value (C / D) obtained by dividing a storage modulus (C) of a 0.5% by mass aqueous solution of the polymer at the angular frequency (A) by a storage modulus (D) of a 0.1% by mass aqueous solution of the polymer at the angular frequency (B) satisfies the following formula (2): 0.5 ≦ (C / D) ≦ 3.0 Formula (2) A polymer flocculant characterized by satisfying the above.
[0054] The polymer flocculant of the present invention (the polymer constituting it) can be produced by the following two-stage polymerization. First, in the first polymerization step, a polymer portion (s) that becomes a branch polymer is formed. That is, a first monomer composition containing at least a (meth)allyl sulfonate and a nonionic monomer or a cationic monomer is polymerized in the presence of an oil and a first surfactant to obtain a water-in-oil emulsion containing a first polymer. The water-in-oil emulsion obtained here is presumed to contain, in the water droplets of the emulsion, a macromonomer (first polymer) having a terminal double bond formed by chain transfer by the (meth)allyl sulfonate. Next, in the second polymerization step, the polymer portion (m) (trunk polymer) is formed and the first polymer (macromonomer) is bonded to the polymer portion (m) (trunk polymer). That is, the second surfactant and the second monomer composition containing at least a nonionic monomer or a cationic monomer are mixed with the water-in-oil emulsion containing the first polymer to carry out polymerization. As a result, it is presumed that the droplets (water droplets) of the water-in-oil emulsion containing the first polymer are swollen with the second monomer composition, and the macromonomer is copolymerized in the droplets to form the polymer portion (m) (trunk polymer), thereby obtaining a comb polymer in which the polymer portion (m) is the trunk polymer and the polymer portion (s) is the branch polymer. When the molecular weight is increased by such a structure, the viscosity of the solution increases. On the other hand, even if a chain transfer agent other than (meth)allyl sulfonate, such as sodium hypophosphite or isopropyl alcohol, is used in the first polymerization step, the polymer portion (s) and the polymer portion (m) are not bonded, and the viscosity of the solution does not increase. Therefore, when forming the polymer portion (s), the (meth)allyl sulfonate is an essential component.
[0055] The compositions of the first monomer composition and the second monomer composition are as described for the monomer units of the polymer.
[0056] As the first surfactant and the second surfactant, a conventionally known surfactant can be used. For example, nonionic surfactants such as polyoxyethylene alkyl ether, polyoxyalkylene derivative, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene sorbitol fatty acid ester, glycerin fatty acid ester, polyoxyethylene fatty acid ester, polyoxyethylene hardened castor oil, polyoxyethylene alkylamine, and fatty acid alkanolamide can be used. Among these, polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene alkylene alkyl ether, sorbitan monooleate, sorbitan sesquioleate, sorbitan monolaurate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan trioleate, polyoxyethylene sorbitan tetraoleate, polyethylene glycol monooleate, polyethylene glycol dioleate, oleic acid diethanolamide, lauric acid monoethanolamide, and stearic acid monoethanolamide are preferred. These surfactants may be used alone or in combination. The amount of surfactant used is preferably 0.2 to 15 mass %, more preferably 0.4 to 10 mass %, based on the total amount of the resulting water-in-oil emulsion.
[0057] As described above, in the second polymerization step, it is necessary to swell the droplets of the water-in-oil emulsion containing the first polymer. In order to perform this swelling appropriately without destroying the emulsion, it is preferable to use a surfactant with a predetermined HLB.
[0058] The HLB value of the surfactant present in the second polymerization step is preferably 7 to 10. The HLB value of the surfactant present in the second polymerization step means the HLB value of the surfactant including the first surfactant added in the first polymerization step and the second surfactant added in the second polymerization step. The HLB value when a plurality of surfactants are used is a weighted average value and can be calculated by the following formula (3). When the HLB value is lower than 7, it becomes difficult to swell the droplets of the water-in-oil emulsion containing the first polymer, and droplets containing only the second monomer composition are easily formed in addition to the droplets containing the first polymer. As a result, two peaks may occur in the volume particle size distribution of the emulsion. In this case, the first polymer and the second monomer composition do not coexist in the droplets, so that the desired comb polymer cannot be obtained. When the HLB value is higher than 10, the polymerization stability in the second polymerization step may be impaired, and the desired water-in-oil emulsion may not be obtained.
[0059] HLB value = Σ(HLBx × Wx) / ΣWx (3) (In formula (3), HLBx represents the HLB value of the surfactant X. Also, Wx represents the mass (g) of surfactant X having the HLBx value.
[0060] In particular, it is preferable to use a mixture of sorbitan sesquioleate and polyoxyethylene sorbitol tetraoleate as the second surfactant. The amount of the second surfactant used is preferably 0.2 to 15% by mass, more preferably 0.4 to 10% by mass, based on the total amount of the water-in-oil emulsion to be obtained.
[0061] Examples of the oil include paraffins, various mineral oils, and mixtures thereof, as well as hydrocarbon compounds such as n-hexane, cyclohexane, and n-heptane. The amount of oil used in the first and second polymerization steps is preferably 3 to 30% by mass relative to the total amount of the water-in-oil emulsion.
[0062] The average particle size of the emulsion in the first polymerization step is preferably 0.5 to 10 μm, more preferably 0.6 to 5 μm. The emulsion in the first polymerization step is preferably prepared by applying strong shear using a homomixer or the like. The average particle size of the emulsion in the second polymerization step is preferably 0.6 to 12 μm, more preferably 0.7 to 7 μm. The preparation of the emulsion in the second polymerization step is preferably carried out with relatively weak stirring. The average particle size here refers to the median size, which is the average particle size in volume distribution.
[0063] The polymerization conditions are appropriately set depending on the monomers and initiators used, and the physical properties of the polymer. The polymerization temperature is 0 to 100°C, and preferably 10 to 80°C. The monomer concentration is preferably 20 to 50% by mass, and more preferably 25 to 45% by mass, based on the final emulsion. The polymerization time is preferably 1 to 24 hours.
[0064] Examples of the polymerization initiator include known persulfates such as sodium persulfate and potassium persulfate, organic peroxides such as benzoyl peroxide, t-butyl hydroperoxide, and paramenthane hydroperoxide, azo compounds such as 2,2'-azobis-(amidinopropane) hydrochloride, azobiscyanovaleric acid, 2,2'-azobisisobutyronitrile, and 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and redox catalysts consisting of combinations of persulfates, organic peroxides, and sodium bisulfite, ferrous sulfate, sulfur dioxide, sodium disulfite, etc. These polymerization initiators may be used alone or in combination of two or more.
[0065] The molecular weight of the polymer portion (m) can be adjusted by using a known chain transfer agent, which includes thiol compounds such as mercaptoethanol and mercaptopropionic acid, reducing inorganic salts such as sodium sulfite, sodium hydrogensulfite and sodium hypophosphite, and alcohols such as ethanol and isopropyl alcohol.
[0066] After polymerization, a hydrophilic surfactant called a phase inversion agent can be added to make the emulsion particles more compatible with water and easier to dissolve in water. Examples of hydrophilic surfactants include cationic surfactants and nonionic surfactants with an HLB value of 9 to 17.
[0067] In addition, additives such as stabilizers, pH adjusters, and antioxidants may be added within a range that does not impair the effects of the present invention.
[0068] In the method for dehydrating sludge by adding at least one polymer flocculant obtained by the present invention, the sludge to be treated is not particularly limited. In addition to sludge generated in sewage treatment, human waste treatment, and domestic wastewater treatment, various sludges can be treated, such as sludge generated in various industrial wastewater treatments in food factories, meat processing plants, and chemical plants, raw human waste generated in livestock farming such as pig farms and sludge generated in the wastewater treatment thereof, and sludge generated in the pulp or paper industry. There is also no limitation on the type of sludge, and primary settling sludge, excess sludge, and mixed sludge thereof, thickened sludge, and digested sludge treated with anaerobic microorganisms can all be treated.
[0069] The sludge dewatering method of the present invention is characterized in that at least one of the polymer flocculants obtained by the present invention is added to the above-mentioned various sludges and dewatered. Specific examples of the dewatering method include the following methods. That is, an inorganic flocculant is added to the sludge as necessary, and the pH is preferably adjusted to 4 to 7. Then, the polymer flocculant of the present invention is added to the sludge, and the polymer flocculant acts on the suspended matter in the sludge by stirring and / or mixing by a known method to form sludge flocs. The formed sludge flocs are mechanically dehydrated by a known means to separate them into treated water and dehydrated cake. When using the polymer flocculant of the present invention in which the polymer portion (s) and / or the polymer (m) is an amphoteric polymer portion, it is preferable to use the inorganic flocculant in combination. In addition, when the purpose is deodorization, dephosphorization, denitrification, etc., it is preferable to adjust the pH of the sludge to less than 5. Examples of inorganic flocculants include, but are not limited to, ferric chloride, ferrous sulfate, polyferric sulfate, etc. Examples of dehydration devices include, but are not limited to, screw press type dehydrators, belt press type dehydrators, filter press type dehydrators, screw decanters, multiple disks, etc. EXAMPLES
[0070] The present invention will be described in more detail below using Production Examples and Examples, but the present invention is not limited thereto. The tests described in the Examples were carried out in the following manner. The temperature condition for measuring various physical properties was 25°C unless otherwise specified.
[0071] [Viscosity of 0.5% by mass aqueous solution] The viscosity of a 0.5% by mass aqueous solution of the polymer at 25° C. was measured using a Brookfield viscometer (using a No. 3 rotor, rotation speed: 12 rpm).
[0072] [Standard viscosity] The polymer was dissolved in a 1N aqueous sodium chloride solution at 0.1% by mass. The viscosity of this aqueous solution at 25° C. was measured using a B-type viscometer (using a BL adapter, rotation speed: 60 rpm).
[0073] [Method of measuring the strain rate dependence and angular frequency dependence of viscoelasticity] An aqueous solution in which the polymer was dissolved at 0.1% by mass and 0.5% by mass was prepared using an Anton Paar MCR rheometer, and the angular frequency dependence of the viscoelasticity of the aqueous solution was measured. <Viscoelasticity measuring device> Anton Paar MCR302 type rheometer, control software RheoPlus32 (ver. 3.62) <Measurement conditions> Fixture: 50 mmφ_0.5° cone plate Measurement temperature: 25 °C Strain rate: 1% <Determination of A> In the range of angular frequency from 0.01 to 100 rad / s, the storage modulus and loss modulus of the 0.5% by mass sample solution were measured respectively. The angular frequency at the point where the storage modulus is equal to the loss modulus, that is, the point where the curve of the storage modulus intersects the curve of the loss modulus, was taken as (A). <Determination of B> In the range of angular frequency from 0.01 to 100 rad / s, the storage modulus and loss modulus of the 0.1% by mass sample solution were measured respectively. The angular frequency at the point where the storage modulus is equal to the loss modulus, that is, the point where the curve of the storage modulus intersects the curve of the loss modulus, was taken as (B). <Determination of C> The storage modulus (equal to the loss modulus, unit: Pa) at the angular frequency (A) was taken as (C). <Determination of D> The storage modulus (equal to the loss modulus, unit: Pa) at the angular frequency (B) was taken as (D).
[0074] <Production Example 1> ·First polymerization step Weighed 14.3 g of sorbitan sesquioleate with HLB 3.7, 5.7 g of polyethylene glycol monooleate with HLB 13.5, and 0.015 g of para-menthane hydroperoxide as an initiator into a five-neck separable flask, added 179.4 g of paraffin oil and dissolved them to prepare an oil phase. In a separate container, 292.1 g of a 79% by mass dimethylaminoethyl acrylate methyl chloride quaternary salt aqueous solution, 138.6 g of a 50% by mass acrylamide aqueous solution, 0.36 g of sodium methallylsulfonate, 0.15 g of EDTA as a chelating agent, and ion-exchanged water were mixed, and the pH was adjusted to 4.0 with 98% sulfuric acid to prepare 498.5 g of an aqueous phase. While stirring the oil phase, the water phase was added to the oil phase, and the mixture was stirred at high speed using a homogenizer to prepare a water-in-oil emulsion. Next, a nitrogen gas inlet tube, a reflux condenser, and a thermometer were attached to the flask, and degassing was started by supplying nitrogen gas while stirring with a stirring blade. After sufficient degassing, while supplying nitrogen gas, nitrogen gas containing 0.02 vol% sulfur dioxide was further blown into the emulsion at a supply rate of 45 mL / min to start polymerization. After reaching 50°C, this temperature was maintained for 2 hours, and then the supply rate of nitrogen gas containing sulfur dioxide was increased to 230 mL / min, and the mixture was further maintained at 50°C for 1 hour, after which the supply of nitrogen gas and nitrogen gas containing sulfur dioxide was stopped, and polymerization was terminated.
[0075] ·Second polymerization step While stirring the emulsion obtained in the first polymerization step with a stirring blade, 189.0 g of paraffin oil was added to dilute the emulsion, and 5.5 g of sorbitan sesquioleate with an HLB of 3.7 and 19.4 g of polyoxyethylene sorbitol tetraoleate with an HLB of 10.5 were further added and dissolved therein. In a separate container, 292.1 g of a 79 mass% dimethylaminoethyl acrylate methyl chloride quaternary salt solution, 138.6 g of a 50 mass% acrylamide aqueous solution, 0.15 g of EDTA, 0.53 g of IPA, 0.015 g of t-butyl hydroperoxide as an initiator, and ion-exchanged water were mixed and adjusted to pH 4.0 with 98% sulfuric acid to prepare 498.5 g of an aqueous phase. While stirring the emulsion, the aqueous phase was added to the emulsion. As a result, the particles containing the polymer took up the aqueous phase and swelled. Nitrogen gas was supplied to start degassing, and after sufficient degassing, nitrogen gas containing 0.02 vol% sulfur dioxide was further blown into the emulsion at a supply rate of 45 mL / min while supplying nitrogen gas, to start polymerization. After reaching 48°C, the supply rate of nitrogen gas containing sulfur dioxide was increased to 230 mL / min, and after maintaining for 1 hour, the supply of nitrogen gas and nitrogen gas containing sulfur dioxide was stopped. Furthermore, 6.0 g of a 1% aqueous solution of sodium disulfite was added, and after maintaining for 30 minutes, the supply of nitrogen gas was stopped to terminate the polymerization. Thereafter, 56.7 g of 50% by mass malic acid and 27.1 g of polyethylene glycol monooleate as a phase inversion agent were added to the obtained emulsion while stirring, and the mixture was stirred to produce a water-in-oil emulsion with a polymer purity of 40% by mass.
[0076] <Production Examples 2 to 6> Production was carried out in the same manner as in Production Example 1, except that the amounts of ingredients were changed to the ratios shown in Table 1.
[0077] <Comparative Manufacturing Example 1> 28.5 g of sorbitan sesquioleate and 11.4 g of polyethylene glycol monooleate were weighed into a five-necked separable flask, and 358.9 g of paraffin oil was added and dissolved to prepare an oil phase. In a separate container, 584.1 g of 79% by mass dimethylaminoethyl acrylate methyl chloride quaternary salt aqueous solution, 227.1 g of 50% by mass acrylamide aqueous solution, 0.012 g of methylenebisacrylamide, 3.6 g of isopropyl alcohol, and 0.3 g of EDTA as a chelating agent were mixed, and ion-exchanged water was added and the pH was adjusted to 4.0 with 98% sulfuric acid. Furthermore, 0.015 g of t-butyl hydroperoxide was added as an initiator to prepare 997.0 g of an aqueous phase. While stirring the oil phase, the aqueous phase was added to the oil phase, and the mixture was stirred at high speed using a homogenizer to prepare a water-in-oil emulsion. A nitrogen gas inlet tube, reflux condenser, and thermometer were attached to the flask, and degassing was started by supplying nitrogen gas while stirring with a stirring blade. After sufficient degassing, nitrogen gas containing 0.02 vol% sulfur dioxide was further blown into the emulsion at a supply rate of 20 mL / min while supplying nitrogen gas, to start polymerization. After reaching 50°C, the temperature was maintained for 2 hours, and then the supply rate of nitrogen gas containing sulfur dioxide was increased to 280 mL / min, and the temperature was maintained at 50°C for another 1 hour, after which the supply of nitrogen gas containing sulfur dioxide was stopped, and 5.8 g of a 1% aqueous solution of sodium disulfite was added, and the temperature was maintained at 50°C for 30 minutes, after which the supply of nitrogen gas was stopped to terminate the polymerization. Thereafter, 58.4 g of 50% by mass malic acid and 39.9 g of polyethylene glycol monooleate as a phase inversion agent were added to the obtained emulsion while stirring, and the mixture was stirred to produce a water-in-oil emulsion with a polymer purity of 40% by mass.
[0078] <Comparative Manufacturing Example 2> The same production as in Production Example 1 was carried out, except that methylenebisacrylamide was removed from Example 1 and the amount of isopropyl alcohol was added so as to satisfy the ratio in Table 1.
[0079] <Comparative Manufacturing Example 3> Production was carried out in the same manner as in Production Example 1, except that the amounts of ingredients were changed to the ratios shown in Table 1 and sodium hypophosphite monohydrate was used instead of sodium methallylsulfonate.
[0080] <Comparative Manufacturing Examples 4 and 5> Production was carried out in the same manner as in Production Example 1, except that the amounts of ingredients were changed to the ratios shown in Table 1.
[0081] In Tables 1 and 2, the abbreviations stand for the following: DAC: Dimethylaminoethyl acrylate methyl chloride quaternary salt AM: Acrylamide SMS: Sodium methallyl sulfonate SAS: Sodium allyl sulfonate MBA: Methylenebisacrylamide IPA: Isopropyl alcohol NaH 2 PO 2 : Sodium hypophosphite monohydrate
[0082] [Table 1]
[0083] [Table 2]
[0084] <Examples 1 to 5 and Comparative Examples 1 to 5> Table tests of coagulation filtration and dewatering treatment were carried out on mixed sludge, which was a mixture of primary sludge and excess sludge collected from Public Sewage Treatment Plant 1. The properties of the sludge were pH = 5.9, TS (Total Solids) = 13,500 mg / L, VTS (Volatile Total Solids) / TS = 91.1 mass%, SS (Suspended Solids) = 12,600 mg / L, VSS (Volatile Suspended Solids) / SS = 91.3 mass%, fiber content / SS = 1.7 mass%.
[0085] 100 mL of this sludge was placed in a 200 mL beaker, and the polymers produced in Production Examples 1 to 5 and Comparative Production Examples 1 to 5 were added to this in an amount of 120 ppm relative to the sludge mass. The sludge was stirred at 1000 rpm for 30 seconds using a stirrer TYPE131 manufactured by Triton Electronics, to form sludge flocs. The floc diameter of the formed sludge flocs was measured visually. Next, the entire amount of the flocculated sludge was poured into a stainless steel sieve with an inner diameter of 75 mm, a depth of 100 mm, and an opening of 250 μm at once, and gravity filtration was performed. At this time, the funnel was set so that the filtrate would enter a 200 mL graduated cylinder, and the volume (mass) of the filtrate 10 seconds after the start of filtration was measured to evaluate the gravity filterability. The appearance (visual observation) of the filtrate was evaluated according to the following criteria. ○: No leakage of suspended solids (SS) into the filtrate was observed. △: A small amount of suspended solids (SS) was observed in the filtrate. ×: A large amount of suspended solids (SS) was observed in the filtrate.
[0086] Next, the sludge wet cake remaining on the stainless steel sieve after evaluating the gravity filterability was taken out, and using a centrifugal settling tube with a nylon filter cloth with a mesh size of 180 μm set inside, it was squeezed at 2000 rpm for 10 minutes using a tabletop test centrifuge to obtain a dehydrated cake. The moisture content of the obtained dehydrated cake was measured. These evaluation results are shown in Table 3.
[0087] [Table 3]
[0088] The polymers (A1 to A6) used in the examples have larger floc particle diameters and a larger amount of liquid after 10 seconds than the polymers (B1 to B5) used in the comparative examples, and therefore have excellent filterability. In addition, the appearance of the filtrate is excellent, and the water content of the obtained dehydrated cake is low. Therefore, the polymers used in the examples have better performance as polymer flocculants than the polymers used in the comparative examples.
Claims
1. a polymer segment (s) having at least a (meth)allyl sulfonate salt and a nonionic monomer or a cationic monomer as constituent units, and not containing a monomer unit derived from a crosslinkable monomer; a polymer segment (m) having at least a nonionic monomer or a cationic monomer as a constituent unit and not containing a monomer unit derived from a crosslinkable monomer; The molecule has both of the following: A polymer flocculant comprising a water-in-oil emulsion containing a comb polymer in which two or more of the polymer portions (s) are bonded to the polymer portion (m), the polymer portion (m) serves as a trunk polymer, and the polymer portion (s) serves as a branch polymer.
2. 2. The polymer flocculant according to claim 1, wherein a ratio of the monomer unit constituting the polymer portion (s) to the monomer unit constituting the polymer portion (m) is 25 / 75 to 70 / 30 in mass ratio.
3. The polymer flocculant according to claim 1, wherein the content of the monomer unit derived from the (meth)allylsulfonate salt is 300 to 5000 ppm relative to the monomer unit constituting the polymer portion (s).
4. The cationic monomer is represented by the following general formula (1): CH 2 =CR 1 -CO-X-Q-N + R 2 R 3 R 4 ·Z - ・・・Chemical reaction (1) (In the general formula (1), R 1 is a hydrogen atom or a methyl group, R 2 and R 3 each independently represents an alkyl group having 1 to 3 carbon atoms or a benzyl group; R 4 represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different. X represents an oxygen atom or NH, Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms, Z - indicates the counter anion.) The polymer flocculant according to claim 1, comprising one or more cationic monomers represented by the following formula:
5. 5. The polymer flocculant according to claim 4, wherein the cationic monomer is at least one of a quaternary salt of methyl chloride of dimethylaminoethyl acrylate and a quaternary salt of methyl chloride of dimethylaminoethyl methacrylate.
6. The polymer flocculant according to claim 1, wherein the content of the monomer units derived from the cationic monomer in the polymer portion (s) is 35 mol % or more relative to the monomer units constituting the polymer portion (s).
7. The polymer flocculant according to claim 1, wherein the content of the monomer units derived from the cationic monomer in the polymer portion (m) is 30 mol % or more relative to the monomer units constituting the polymer portion (m).
8. The polymer flocculant according to claim 1, wherein the content of the monomer units derived from the cationic monomer in the polymer is 31 mol% or more relative to the total amount of the monomer units constituting the polymer portion (s) and the polymer portion (m).
9. In a frequency dependency measurement (25° C.) using a rheometer, the angular frequency (A) at which the storage modulus and loss modulus of a 0.5% by mass aqueous solution of the polymer are equal to each other is divided by the angular frequency (B) at which the storage modulus and loss modulus of a 0.1% by mass aqueous solution of the polymer are equal to each other, and the value (A / B) satisfies the following formula (1): 0.005≦(A / B)≦0.1 ... Formula (1) and a value (C / D) obtained by dividing a storage modulus (C) of a 0.5% by mass aqueous solution of the polymer at the angular frequency (A) by a storage modulus (D) of a 0.1% by mass aqueous solution of the polymer at the angular frequency (B) satisfies the following formula (2): 0.5≦(C / D)≦3.0 ... Formula (2) The polymer flocculant according to claim 1 , which satisfies the above.
10. A polymer flocculant comprising a water-in-oil emulsion containing a polymer having at least a (meth)allyl sulfonate salt and a nonionic monomer or a cationic monomer as structural units, In a frequency dependency measurement (25° C.) using a rheometer, the angular frequency (A) at which the storage modulus and loss modulus of a 0.5% by mass aqueous solution of the polymer are equal to each other is divided by the angular frequency (B) at which the storage modulus and loss modulus of a 0.1% by mass aqueous solution of the polymer are equal to each other, and the value (A / B) satisfies the following formula (1): 0.005≦(A / B)≦0.1 ... Formula (1) and a value (C / D) obtained by dividing a storage modulus (C) of a 0.5% by mass aqueous solution of the polymer at the angular frequency (A) by a storage modulus (D) of a 0.1% by mass aqueous solution of the polymer at the angular frequency (B) satisfies the following formula (2): 0.5≦(C / D)≦3.0 ... Formula (2) A polymer flocculant characterized by satisfying the above.
11. The polymeric flocculant according to claim 10, wherein the polymer does not contain any monomer units derived from a crosslinkable monomer.
12. The polymeric flocculant according to claim 10, wherein the polymer is a comb polymer having a trunk polymer and a branch polymer.
13. The cationic monomer is represented by the following general formula (1): CH 2 =CR 1 -CO-X-Q-N + R 2 R 3 R 4 ·Z - ・・・ Chemical reaction (1) (In the general formula (1), R 1 is a hydrogen atom or a methyl group, R 2 and R 3 each independently represents an alkyl group having 1 to 3 carbon atoms or a benzyl group; R 4 represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a benzyl group, and may be the same or different. X represents an oxygen atom or NH, Q represents an alkylene group having 1 to 4 carbon atoms or a hydroxyalkylene group having 2 to 4 carbon atoms, Z - indicates the counter anion.) The polymer flocculant according to claim 10, comprising one or more cationic monomers represented by the following formula:
14. 14. The polymeric flocculant according to claim 13, wherein the cationic monomer is at least one of a quaternary salt of methyl chloride of dimethylaminoethyl acrylate and a quaternary salt of methyl chloride of dimethylaminoethyl methacrylate.
15. The polymer flocculant according to claim 10, wherein the content of the monomer units derived from the cationic monomer in the polymer is 31 mol% or more based on the total amount of the monomer units constituting the polymer.
16. A method for producing the polymer flocculant according to any one of claims 1 to 15, a first polymerization step of subjecting a first monomer composition containing at least a (meth)allylsulfonate salt and a nonionic monomer or a cationic monomer to water-in-oil emulsion polymerization in the presence of an oil and a first surfactant to obtain a water-in-oil emulsion containing a first polymer; a second polymerization step of mixing the water-in-oil emulsion containing the first polymer with a second surfactant and a second monomer composition containing at least a nonionic monomer or a cationic monomer to carry out polymerization; A method for producing a polymer flocculant, comprising the steps of:
17. The method for producing a polymer flocculant according to claim 16, wherein the surfactant present in the second polymerization step is a nonionic surfactant having an HLB value of 7 to 10.
18. The method for producing a polymer flocculant according to claim 16, wherein the second surfactant is a combination of sorbitan sesquioleate and polyoxyethylene sorbitol tetraoleate.
19. A method for dewatering sludge, comprising adding the polymer flocculant according to claim 1 to the sludge.
Citation Information
Patent Citations
Polymer emulsion composition and polymer flocculant
JP1995062254A
Waste water treatment method
JP2013180260A
Waste water treatment method
JP2013180261A
Wastewater treatment method using organic coagulant
JP2013184160A
Organic coagulant and waste water treatment method using the same
JP2015066549A