Polyvinyl alcohol film and optical film produced from the same

By optimizing the saponification degree and temperature ranges of polyvinyl alcohol films, the film's mechanical strength and optical properties are enhanced, addressing breakage and leakage issues in the production of optical films.

JP2024169264AInactive Publication Date: 2024-12-05CHANG CHUN PETROCHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023133674
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-06
Filing Date
2023-08-18
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polyvinyl alcohol films often break during the stretching process in the production of optical films due to inadequate control of the storage modulus inflection point temperature and softening point temperature, leading to mechanical weakness and red light leakage issues.

Method used

Adjusting the polyvinyl alcohol film's saponification degree to 95 mol% or more, with an inflection point temperature of storage modulus (E') between 30°C to 55°C and a softening point temperature of 45°C or less, to enhance mechanical strength and reduce red light leakage.

Benefits of technology

The modified polyvinyl alcohol film exhibits improved resistance to breaking during stretching and reduced red light leakage, resulting in higher quality optical films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169264000001_ABST
    Figure 2024169264000001_ABST
Patent Text Reader

Abstract

To provide a polyvinyl alcohol film, and an optical film produced from the same.SOLUTION: There are provided a polyvinyl alcohol film and an optical film produced from the same, wherein the polyvinyl alcohol film contains a polyvinyl alcohol resin having a degree of saponification of 95 mol% or more, and a temperature indicated by the inflection point of the storage elastic modulus (E') in the range of 30°C to 55°C of the polyvinyl alcohol film in the water is 37 to 40°C. The polyvinyl alcohol film has such a characteristic as to prevent from being broken even if the film is drawn, and an optical film produced from the same has such a characteristic as to have less leakage of red light.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polyvinyl alcohol (PVA) products, and in particular, but not exclusively, to polyvinyl alcohol films and optical films made therefrom. [Background technology]

[0002] Polyvinyl alcohol (PVA) film is a hydrophilic material obtained by coating and drying an aqueous solution containing polyvinyl alcohol polymer and plasticizer. It has properties such as high transparency, mechanical strength, water solubility, and good processability, and is therefore widely used in packaging materials and various optical films for electronic devices, such as polarizing films.

[0003] The polarizing film obtained by processing the polyvinyl alcohol film through the polarizing process has the property of blocking only light from a specific direction, so that the brightness of the light that passes through can be controlled. Based on this property, the polarizing film is applied to various displays, glasses, and wearable terminals. The polarizing process generally includes processes such as swelling, stretching, and dyeing. Specifically, the polyvinyl alcohol film is placed in a solution and the above-mentioned process is carried out to diffuse the dye molecules into the molecules in the polyvinyl alcohol film, and a relatively regular arrangement is obtained by stretching, so that the polarizing film can absorb the light component parallel to the arrangement direction and pass the light component perpendicular to the arrangement direction to produce the property of polarization. However, polyvinyl alcohol-based films often have a problem of the film breaking due to stretching when producing polarizing films.

[0004] Prior art such as Patent Document 1 discloses a polyvinyl alcohol-based film. This film is produced by using a film-forming process in which an aqueous solution of a polyvinyl alcohol-based resin is formed into a film by a continuous casting method, a drying process in which the film obtained by film-forming is dried with a heating roller, and a heat treatment process in which the dried film is subjected to a heat treatment, and the ratio of elastic modulus and thickness is controlled to improve the problem of film breakage. In the drying process, the temperature at which the film obtained by film-forming is dried, i.e., the surface temperature of the heating roller with the highest temperature among the multiple heating rollers used, is 100°C to 115°C, the contact time of the film obtained by film-forming with the heating roller with the highest temperature in the drying process is 4 to 30 seconds, and the heat treatment process is a process in which the dried film is cooled to 50°C or less and then heated at 60 to 99°C.

[0005] In addition, the polarizing film must have appropriate optical properties. For this reason, the prior art also discloses that the optical properties are improved by changing the structure of polyvinyl alcohol or by adding a functional group (such as a cationic group). Prior art such as Patent Document 2 discloses a polarizing film that has good polarization performance and has little leakage of red light in a crossed Nicol state, and a method for producing the same. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Taiwan Patent Application Publication No. 201817576 [Patent Document 2] Taiwan Patent Application Publication No. 201719207 Summary of the Invention [Problem to be solved by the invention]

[0007] In the prior art, when a polyvinyl alcohol film is used to manufacture an optical film, the film often breaks during stretching. In this regard, the present inventors have found that the problem of the polyvinyl alcohol film being easily broken during stretching can be improved by adjusting the polyvinyl alcohol film so that the storage modulus (E') of the polyvinyl alcohol film in a specific temperature range has a specific range of inflection point temperature. [Means for solving the problem]

[0008] Specifically, one embodiment of the present invention provides a polyvinyl alcohol film comprising a polyvinyl alcohol resin having a degree of saponification of 95 mol % or more, and having an inflection point of storage modulus (E') in water at a temperature range of 30°C to 55°C of 37 to 40°C.

[0009] In one or more embodiments, the polyvinyl alcohol film has a softening point temperature of 45° C. or less.

[0010] In one or more embodiments, the degree of saponification of the polyvinyl alcohol resin is greater than 99.90 mol %.

[0011] In one or a plurality of embodiments, the polyvinyl alcohol resin has a degree of saponification of 99.95 mol % or more.

[0012] In one or more embodiments, the polyvinyl alcohol resin has a degree of saponification of 99.97 mol % or more.

[0013] In one or more embodiments, the polyvinyl alcohol resin has an average degree of polymerization of 2,000 to 3,300.

[0014] In one or more embodiments, the polyvinyl alcohol resin has an average degree of polymerization of 2,400 to 3,300.

[0015] In one or more embodiments, the polyvinyl alcohol film has a thickness of 40 to 75 μm.

[0016] Another aspect of the present invention provides an optical film made from the polyvinyl alcohol film described above.

[0017] In one or more embodiments, the optical film is a polarizing film.

[0018] In one or more embodiments, the polarizing film has a red light leakage rate of less than 5%. Effect of the Invention

[0019] The polyvinyl alcohol film of the present invention can be used for various applications, and is particularly suitable for use as an optical film such as a polarizing film. The polyvinyl alcohol film obtained based on the technical content of the present invention significantly improves the film breakage situation when used in the production of an optical film.

[0020] Furthermore, the present inventors have also found that when the polyvinyl alcohol film is adjusted to have a specific softening point temperature, an optical film produced from the polyvinyl alcohol film has the property of reducing red light leakage in a crossed Nicol state. [Brief description of the drawings]

[0021] [Figure 1] 1 is a graph showing the storage modulus (E') of a polyvinyl alcohol film according to a change in temperature analyzed in water in accordance with an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating a sample preparation method for analyzing the inflection point temperature of a polyvinyl alcohol film according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram illustrating a sample preparation method for analyzing the inflection point temperature of a polyvinyl alcohol film according to one embodiment of the present invention. [Figure 4]FIG. 2 is a schematic diagram illustrating a sample preparation method for analyzing the inflection point temperature of a polyvinyl alcohol film according to one embodiment of the present invention. [Diagram 5] 1 is a graph showing dimensional change versus temperature in a softening point temperature analysis of a polyvinyl alcohol film according to an embodiment of the present invention. [Figure 6] FIG. 2 is a schematic diagram illustrating sample preparation of polyvinyl alcohol film for red light leakage evaluation according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] In order to make the description of the present invention more detailed and complete, the following provides an illustrative description of the embodiments and specific examples of the present invention, which are not the only ways of implementing or operating the specific examples of the present invention. In this specification and the appended claims, "a" and "the" may also be interpreted as plural unless the context dictates otherwise.

[0023] The numerical ranges and parameters specifying the present invention are approximate, but the relevant numerical values ​​in the specific examples are presented as precisely as possible. However, any numerical value necessarily contains standard deviations inherent in each individual testing method. As used herein, the term "about" indicates that the actual value is within an acceptable standard error of the mean and is within the belief of one of ordinary skill in the art to which the present invention pertains.

[0024] [Polyvinyl alcohol film] One aspect of the present invention provides a polyvinyl alcohol film comprising a polyvinyl alcohol resin having a degree of saponification of 95 mol% or more, and having a temperature of an inflection point of a storage modulus (E') in water in the range of 30°C to 55°C of 37 to 40°C. According to some embodiments, the polyvinyl alcohol film of the present invention has a thickness of 40 to 75 μm. Specifically, the thickness is a value within a range between any two of the following values, for example, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, or 80 μm, and the above values ​​are merely examples and are not limiting.

[0025] The "elastic modulus" mentioned in this specification is a physical property used to analyze the relationship between stress and strain in material mechanics, and is the ratio of stress to strain. The elastic modulus obtained when the stress applied to the material is a normal force is represented by E. The "storage modulus (E')" is the component that the material absorbs and converts the applied energy and stores it inside the material, and is usually used to recover deformation and maintain the original appearance of the material, and is related to the elastic properties of the material and can also reflect the rigidity of the material. From the molecular point of view, the larger E' is, the stronger the intermolecular force is. In the case of polyvinyl alcohol, the larger E' is, the higher the degree of crystallinity and the degree of entanglement of molecular chains is.

[0026] The "temperature at which the inflection point of the storage modulus (E') in the range of 30°C to 55°C in water (hereinafter referred to as the E' inflection point temperature)" described in this specification is obtained by immersing a polyvinyl alcohol film in water and measuring the E' change of the polyvinyl alcohol film by a temperature increase method. After a large amount of water is absorbed into the film, hydrogen bonds are formed with the -OH group of the polyvinyl alcohol, the molecular chains of the polyvinyl alcohol swell and separate, and the entanglement between the molecular chains is reduced, so that the E' analysis of the polyvinyl alcohol immersed in water can be used to evaluate the change in crystallinity in the film at different temperatures. Furthermore, the analysis of the polyvinyl alcohol film in water has the characteristics shown in Figure 1, where the E' change curve according to temperature has two different slopes in the change curve between 30°C and 55°C, the tangent intersection of the two slopes is the E' inflection point, and the corresponding temperature is the E' inflection point temperature (the point indicated by the arrow in Figure 1).

[0027] The physical meaning expressed by the E' inflection point temperature includes the temperature at which the crystals in the polyvinyl alcohol film begin to dissolve in large quantities, and a higher E' inflection point temperature indicates that the average crystal grains in the film are larger, so that a large amount of crystal dissolution occurs only at a relatively high temperature. The inventors have found that when the E' inflection point temperature exceeds 40°C, the film is prone to break during the swelling and stretching process of the polyvinyl alcohol film in the manufacturing process of the polarizer. Without being bound by any theory, the film is likely to break because excessive stress is concentrated in the undissolved crystal regions. When the E' inflection point temperature is less than 37°C, the crystal grains are too small, resulting in insufficient mechanical strength of the film, and the film is too soft and prone to break during swelling and stretching.

[0028] Therefore, in order to improve the situation that the polyvinyl alcohol film is easily broken during stretching, it is necessary to control the E' inflection point temperature within a specific range, and specifically, the temperature indicated by the E' inflection point in the range of 30°C to 55°C (temperature range of the first stretch in the manufacturing process of the polarizer) of the polyvinyl alcohol film of the present invention in water is 37 to 40°C, for example, 37°C, 37.1°C, 37.3°C, 37.5°C, 37.7°C, 37.9°C, 38°C, 38.1°C, 38.3°C, 38.5°C, 38.7°C, 38.9°C, 39°C, 39.1°C, 39.3°C, 39.5°C, 39.7°C, 39.9°C, or 40°C, but is not limited thereto. If the measurement temperature exceeds 55°C, the crystallization of the polyvinyl alcohol film may completely disappear and the physical properties may change rapidly, so when analyzing the inflection point temperature, the analysis temperature range set does not exceed 55°C.

[0029] Regarding the method for measuring the E' inflection point temperature, since the polyethylene film absorbs moisture (including moisture in the air) and may affect the state of the crystal form, molecular arrangement, etc., the moisture content of each polyethylene film to be measured can be adjusted to the same by pretreatment before measuring the E' inflection point temperature of the polyethylene film, thereby making the state of each polyethylene film to be measured the same. The moisture content can usually be adjusted to about 8 to 9 wt%, but is not limited thereto in the present specification.

[0030] The "saponification degree" referred to in this specification means a measured value obtained by a test method described in the JIS K 6726 (1994) standard. In one or more embodiments, the saponification degree of the polyvinyl alcohol-based resin is 95 mol% or more in order to obtain better optical properties, for example, 95 mol% or more, 95.5 mol% or more, 96 mol% or more, 96.5 mol% or more, 97 mol% or more, 97.5 mol% or more, 98 mol% or more, 98.5 mol% or more, 99 mol% or more, or 99.5 mol% or more. When the saponification degree of the polyvinyl alcohol-based resin is 95% or more, the mechanical strength and optical properties of the film can be improved. According to one embodiment of the present invention, the saponification degree of the polyvinyl alcohol-based resin of the present invention is greater than 99.90 mol%, for example, greater than 99.90 mol%, greater than 99.92 mol%, greater than 99.94 mol%, greater than 99.96 mol%, or greater than 99.98 mol%. Preferably, the saponification degree of the polyvinyl alcohol-based resin is 99.95 mol% or more, for example, 99.95 mol% or more, 99.97 mol% or more, or 99.99 mol% or more. More preferably, the saponification degree of the polyvinyl alcohol-based resin is 99.97 mol% or more, for example, 99.97 mol% or more, 99.98 mol% or more, or 99.99 mol% or more.

[0031] According to one or more embodiments, the polyvinyl alcohol film of the present invention has a softening point temperature, and the softening point temperature is 45° C. or less. The "softening point temperature" referred to in this specification refers to the temperature (inflection temperature) at which the dimensions of the film begin to change significantly when a certain normal force is applied to the material and the temperature is gradually increased. The softening point temperature can be regarded as the temperature at which the molecular chains of the amorphous region begin to move significantly under the action of a certain normal force, and reflects the mechanical properties of the amorphous region. A high softening point temperature indicates that more energy is required for the molecular chains of the amorphous region to move significantly. If the softening point temperature of the polyvinyl alcohol film is too high, the molecular chains of the amorphous region become difficult to move, and the iodide ions used to dye the polyvinyl alcohol film during the swelling and stretching process of the polyvinyl alcohol film in the polarizer production are difficult to enter the amorphous region, and are adsorbed to the polymer chains, making it difficult to dye the polyvinyl alcohol film, which indicates that a problem of red light leakage occurs in the manufactured polarizer.

[0032] Therefore, in order to improve the red light leakage from the polarizer, it is necessary to control the softening point temperature to a specific value or lower. Specifically, the polyvinyl alcohol film of the present invention has a softening point temperature of 45°C or lower, for example, 45°C or lower, 44.5°C or lower, 44°C or lower, 43.5°C or lower, 43°C or lower, 42.5°C or lower, 42°C or lower, 41.5°C or lower, 41°C or lower, 40.5°C or lower, 40°C or lower, or 35.5°C or lower.

[0033] In one or more embodiments, the average degree of polymerization of the polyvinyl alcohol resin is 2000 to 3300, such as a value within a range between any two of the following values, for example, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, or 3300. Preferably, the degree of polymerization of the polyvinyl alcohol resin is 2400 to 3300, for example, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, or 3300. The "average degree of polymerization" described in this specification means a measured value obtained by a test method described in the JIS K 6726 (1994) standard.

[0034] The E' inflection point temperature and the softening point temperature can be adjusted by adjusting the particle size, degree of saponification and average degree of polymerization of the resin raw material of the polyvinyl alcohol film, and can also be adjusted by adjusting the stirring temperature and time of the raw material, the flow temperature of the dissolved material, and the maximum temperature of oven drying in the production process, but are not limited thereto.

[0035] [Method of manufacturing polyvinyl alcohol film] The method for producing a polyvinyl alcohol film of the present invention includes: (a) a dissolving step of heating and dissolving a polyvinyl alcohol-based resin and adjusting the concentration of the polyvinyl alcohol-based resin to form a polyvinyl alcohol casting solution; (b) a casting step of casting the polyvinyl alcohol casting solution onto a casting drum and peeling it off from the casting drum to obtain a preformed film; (c) a heating roller step of contacting the polyvinyl alcohol preformed film with a plurality of heating rollers to obtain a semi-formed polyvinyl alcohol film product; and (d) an oven step of placing the semi-formed polyvinyl alcohol film product in an oven to dry it and obtain a molded polyvinyl alcohol film product, and depending on the situation, it may further include (e) a temperature and humidity adjustment step of placing the polyvinyl alcohol film product in a temperature and humidity adjuster to adjust the temperature and humidity.

[0036] [Dissolution process] According to some embodiments, in the dissolving step, the temperature is raised to 130-165°C while stirring the polyvinyl alcohol resin, solvent, plasticizer, etc., and after uniformly dissolving, the resin is adjusted to an appropriate concentration to obtain a polyvinyl alcohol casting solution. The appropriate resin concentration is about 20wt%-50wt%, for example 20, 30, 40, or 50wt%. If the resin concentration is too low, the subsequent drying load of the film will be high, and conversely, if the resin concentration is too high, the viscosity will be too high, making film formation difficult.

[0037] In one or more embodiments, the polyvinyl alcohol resin used in the dissolving step is polymerized with a vinyl ester resin monomer to form a polyvinyl alcohol resin having an average degree of polymerization of 2000 to 3300, and then a saponification reaction is carried out to obtain a polyvinyl alcohol resin having a degree of saponification of preferably more than 95%. Examples of the vinyl ester resin monomer include vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, or vinyl octoate, or combinations thereof, and the present invention is not limited thereto. The use of vinyl acetate is preferred. In addition, a copolymer formed by copolymerization of an olefin compound or an acrylate derivative with the vinyl ester resin monomer can also be used, and the olefin compound can be ethylene, propylene, or butene, and the like, and the present invention is not limited thereto. The amount of the olefin compound added can be 2 to 4 mol%, for example, 2, 2.5, 3, 3.5, or 4 mol%, but is not limited thereto. Examples of the acrylate derivative include acrylic acid, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, and n-butyl acrylate, but the present invention is not limited thereto.

[0038] The polyvinyl alcohol resin is granular, and the larger the particle size of the polyvinyl alcohol resin (i.e., the smaller the mesh number), the more likely it is that the raw material resin crystals will be incompletely dissolved, which will affect the crystal grain size and crystallinity of the processed molded product, causing the crystal grains of the molded product to become larger and the crystallinity to increase. In one or more embodiments, the particle size is defined by the sieve mesh and is 20 mesh or more, specifically, for example, 20 mesh or more, 30 mesh or more, or 40 mesh or more.

[0039] In one or more embodiments, the solvent used in the dissolving step is not particularly limited in the present invention, as long as it can dissolve polyvinyl alcohol resin. Examples of the solvent include, but are not limited to, water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylenediamine, diethylenetriamine, etc., and the above solvents can be used alone or in combination of two or more. Considering environmental and economical aspects, it is preferable to use water as the solvent in the present invention.

[0040] In one or more embodiments, the "plasticizer" described herein is specifically, but not limited to, glycerin, ethylene glycol, propylene glycol, diethylene glycol, diglycerol, triethylene glycol, tetraethylene glycol, trimethylolpropane, or the like, or a combination thereof. In the present invention, glycerin is preferred. In one or more embodiments, the amount of the plasticizer added is 5 to 15 wt% based on the weight of the polyvinyl alcohol resin, specifically, for example, 6, 7, 8, 9, 10, 11, 12, 13, 14, and 15 wt%, but not limited thereto. In a preferred embodiment, the amount of the plasticizer added is 10 wt% based on the weight of the polyvinyl alcohol resin.

[0041] In addition to the plasticizer, other additives including, but not limited to, surfactants may be added as necessary in the dissolution step. The surfactants include, but are not limited to, cationic, anionic or nonionic surfactants, and specifically include, but are not limited to, carboxylate types such as potassium laurate, sulfate types such as sodium lauryl sulfate, sulfonate types such as dodecylbenzenesulfonate, alkylphenyl ether types such as polyoxyethylene octylphenyl ether, alcohol phenyl ether types such as polyethylene glycol monooctylphenyl ether, alkyl ester types such as polyethylene glycol monolaurate, alkylamine types such as polyoxyethylene laurylamino ether, alkylamide types such as polyoxyethylene lauramide, polypropylene glycol ether types such as polyoxyethylene polyoxypropylene ether, alkanolamide types such as lauric acid diethanolamide and oleic acid diethanolamide, allyl phenyl ether types such as polyoxyallyl phenyl ether, or sodium lauryl alcohol polyoxyethylene ether sulfate.

[0042] In one or more embodiments, the temperature at which the polyvinyl alcohol-based resin aqueous solution is dissolved is preferably 130 to 165° C., and is a value within a range between any two of the following values, specifically, for example, 130° C., 135° C., 140° C., 145° C., 150° C., 155° C., 160° C., or 165° C. The dissolution temperature probably affects the dissolution of the polyvinyl alcohol resin and the dispersion of the additives. If the dissolution temperature is too low, the E' inflection point temperature and softening point temperature of the molded film will also be too high, and if the dissolution temperature is too high, partial yellowing will occur in the molded film.

[0043] In one or more embodiments, the time for dissolving the polyvinyl alcohol-based resin aqueous solution is preferably 1 to 5 hours, and is specifically, for example, 1 hour, 2 hours, 3 hours, 4 hours, or 5 hours, within a range between any two of the following values: If the dissolving time is too short, dissolution of the polyvinyl alcohol resin and dispersion of the additives will be poor, and the E' inflection point temperature and softening point temperature of the molded film will be too high.

[0044] [Casting process] According to some embodiments, the casting process mainly involves sending the polyvinyl alcohol casting solution to a twin-screw extruder, mixing the solution uniformly again in the extruder, degassing the solution (for example, but not limited to, degassing the solution in a twin-screw extruder), discharging the solution from a T-die lip, and casting the solution onto a rotating high-temperature casting drum (also called a casting drum) or a casting drum as a support such as an endless belt to obtain a polyvinyl alcohol preformed film. In one or more embodiments, the temperature of the polyvinyl alcohol casting solution during transportation is preferably at least 90°C or higher (for example, but not limited to, 90, 91, 92, 93, 94, 95, 96, 97, 98, or 99°C). The polyvinyl alcohol casting solution after being mixed uniformly again in the extruder and degassed must also be controlled to at least 90°C or higher (for example, but not limited to, 90, 91, 92, 93, 94, 95, 96, 97, or 98°C).

[0045] In one or more embodiments, when the polyvinyl alcohol casting solution is cast onto a rotating high-temperature casting drum, the temperature of the casting drum is preferably 85 to 95° C., and the residence time of the polyvinyl alcohol on the casting drum is preferably 0.6 to 1.2 minutes.

[0046] [Heating roller process] According to some embodiments, the heating roller process mainly involves contacting and drying the upper and lower surfaces of the polyvinyl alcohol preformed film peeled off from the casting drum with multiple heating rollers, and then obtaining a polyvinyl alcohol film semi-formed product. The temperature of the multiple heating rollers (e.g., 15 heating rollers) gradually decreases from high to low, with the first heating roller being the roller with the highest temperature among all the heating rollers (e.g., 90 to 99°C, but not limited thereto, specifically, for example, 90, 91, 92, 93, 94, 95, 96, 97, 98, or 99°C, but not limited thereto), and the temperature of the last heating roller being the lowest among all the heating rollers (e.g., 30 to 50°C, but not limited thereto, specifically, for example, 30, 35, 40, 45, or 50°C, but not limited thereto).

[0047] [Oven process] According to some embodiments, the oven process mainly involves drying the upper and lower surfaces of the polyvinyl alcohol film semi-molded product peeled off from the heated roller in an oven with hot air to obtain a polyvinyl alcohol film molded product.

[0048] In one or more embodiments, the oven is preferably a floating oven, and the temperature is controlled in the range of 100°C to 120°C, specifically, a value within the range between any two of the following values, for example, 100, 105, 110, 115 or 120°C. During the oven drying process, recrystallization of polyvinyl alcohol occurs, and the maximum temperature of this process probably affects the effect of recrystallization, and if the temperature is too high, the crystal grains may become too large and the crystallinity may become too high, and if the temperature is too low, the crystal grains may become too small and the crystallinity may become too low. Note that the arrangement of polyvinyl alcohol in the film is fixed before it is placed in the oven, so the temperature adjustment does not have a significant effect on the softening point temperature.

[0049] [Temperature and humidity adjustment process] According to a preferred embodiment of the present invention, the polyvinyl alcohol film product can be further placed in a temperature and humidity regulator to adjust the temperature and humidity after the above steps.

[0050] In one or more embodiments, the temperature of the temperature and humidity regulator is in the range of 35 to 45°C, specifically, a value within a range between any two of the following values, for example, 35, 40, or 45°C, and preferably 45°C. In one or more embodiments, the relative humidity of the temperature and humidity regulator is in the range between any two of the following values, for example, 40, 45, 50, 55, or 60%, and preferably in the range of 40 to 60%. In one or more embodiments, the time for which the polyvinyl alcohol film is left in the temperature and humidity regulator is, for example, 20, 25, 30, 35, or 40 minutes, and preferably in the range of 20 to 40 minutes. In one or more embodiments, for example, the polyvinyl alcohol film is left in a temperature and humidity regulator at a temperature of 45°C and a relative humidity of 50% for 40 minutes.

[0051] [Optical film and its manufacturing method] Another object of the present invention is to provide an optical film manufactured from the polyvinyl alcohol film. The "optical film" described in this specification may be a polarizing film, a retardation film, a viewing angle widening film, or a brightness increasing film, and is particularly a polarizing film. According to some embodiments, the "method of manufacturing an optical film" of the present invention refers to a method of manufacturing a polarizing film, and further, a polyvinyl alcohol film is manufactured into a polarizing film, and the breakage state due to pulling / stretching during the manufacturing process and the degree of red light leakage of the film are evaluated. The manufacturing method includes a dyeing step of adsorbing iodide ions, a boric acid treatment step, and a water washing step, and a stretching step of uniaxial stretching can be performed in the boric acid treatment step or in the stage before this. Preferably, a swelling step of swelling the polyvinyl alcohol film with water can be provided before the dyeing step. In addition, a final drying step is usually provided after the water washing step.

[0052] In the swelling step, the polyvinyl alcohol film is immersed in a treatment bath (e.g., pure water) at a temperature of 30°C to 55°C, for example, to wash the film surface and perform a swelling treatment. The swelling treatment time is usually 5 to 300 seconds, preferably 20 to 240 seconds. According to some embodiments, a plurality of guide rollers are arranged in a swelling tank containing the treatment bath in order to transport the polyvinyl alcohol film. Next, the polyvinyl alcohol film is stretched in the machine direction (MD) to 1.05 to 2.5 times its original length, and then a dyeing step is performed.

[0053] In the dyeing process, the polyvinyl alcohol film that has been through the swelling process is immersed in a dyeing tank containing a dye bath. The dyeing conditions can be determined within a range in which iodine is adsorbed onto the polyvinyl alcohol film and does not cause defects such as extreme dissolution or devitrification of the film. The dye bath in the dyeing process can be, for example, an aqueous solution containing iodine and potassium iodide, and the concentration of iodine in the dye bath is preferably 0.01 to 0.5 wt%, and the concentration of potassium iodide is preferably 0.01 to 10 wt%. Specific examples include, but are not limited to, an aqueous solution containing 0.037 wt% iodine and 1.85 wt% potassium iodide. In place of potassium iodide, other iodides such as zinc iodide may be used, or other iodides may be used in addition to potassium iodide. The temperature of the dye bath is usually 20 to 40° C., for example, 20, 30 or 40° C., and the time of the dyeing treatment (dyeing time) is usually 10 to 600 seconds, preferably 30 to 200 seconds. Next, the polyvinyl alcohol film is stretched in the machine direction to 2 to 4 times its original length, and then a boric acid treatment and a stretching step are carried out.

[0054] In the boric acid treatment and stretching process, the polyvinyl alcohol film dyed with iodine is treated with a boric acid-containing aqueous solution to crosslink, and the adsorbed iodine is fixed to the resin. The process is usually carried out by immersing the polyvinyl alcohol film that has been subjected to the dyeing process in a fixing tank containing a boric acid-containing treatment bath. The boric acid treatment bath preferably contains iodide in addition to boric acid, and examples of the iodide used here include potassium iodide or zinc iodide, and examples of the iodide include aqueous solutions containing boric acid and potassium iodide at a concentration of 5.5 wt% each. In addition, compounds other than iodide, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, sodium sulfite, potassium sulfate, sodium sulfate, etc., may also be present in the boric acid treatment bath. The boric acid treatment and stretching process are usually carried out at 50 to 70°C, for example at a temperature of 55°C, and the treatment time is usually 10 to 600 seconds, preferably 20 to 300 seconds, and more preferably 20 to 100 seconds. Next, the polyvinyl alcohol film is stretched in the machine direction to 3 times or more of the original length, and the subsequent process is carried out. The upper limit of the stretching ratio is not particularly limited, but is preferably less than 8 times, for example. The stretching ratio includes, but is not limited to, 3.3 times or more, for example, 3.3 to 8.0 times, more preferably 3.5 to 6.0 times, and particularly preferably 4.0 to 5.5 times.

[0055] After the polyvinyl alcohol film is subjected to the above process and the subsequent washing and drying processes, a polarizing film is formed. In the washing and drying processes, the iodine solution and boric acid remaining on the film surface are washed with water or an aqueous solution containing iodide (for example, but not limited to, washing with an aqueous potassium iodide solution having a concentration of 5.5 wt%). Next, after a drying process (for example, but not limited to, drying in an oven at a temperature of 60° C. for 5 minutes), a polarizing film is formed. Furthermore, a protective layer can be formed on at least one surface of the polarizing film to manufacture a finished polarizing film (also called a polarizer). In detail, the protective layer has a function such as preventing wear of the surface of the polarizing film, and is preferably a component containing a transparent resin. According to different embodiments, the protective layer is provided on only one surface of the polarizing film, but it is preferable that the protective layer is formed on both surfaces of the polarizing film. The protective layer can be a protective film made of a transparent resin material. The transparent resin may be an acrylic resin such as a methyl methacrylate resin, an olefin resin, a polyvinyl chloride resin, a cellulose resin, a styrene resin, an acrylonitrile-butadiene-styrene copolymer resin, an acrylonitrile-styrene copolymer resin, a polyvinyl acetate resin, a polyvinylidene chloride resin, a polyamide resin, a polyacetal resin, a polycarbonate resin, a modified polyphenylene ether resin, a polyester resin (such as a polybutylene terephthalate resin or a polyethylene terephthalate resin), a polysulfone resin, a polyethersulfone resin, a polyarylate resin, a polyimideimide resin, a polyimide resin, an epoxy resin, an oxetane resin, or the like, and a cellulose resin such as cellulose triacetate (TAC) is preferred. EXAMPLES

[0056] The present invention will be described in detail below with reference to specific examples. However, it should be understood that these specific examples are intended to aid in the understanding of the present invention and are not intended to limit the scope of the present invention in any way.

[0057] 1. Preparation of Polyvinyl Alcohol Film Here, the present invention provides a non-limiting method for preparing polyvinyl alcohol films. The polyvinyl alcohol films of the non-limiting examples (Examples 1-16) and the polyvinyl alcohol films of the comparative examples (Comparative Examples 1-8) are prepared in a manner similar to that disclosed below.

[0058] The following are the main steps of producing polyvinyl alcohol films in this embodiment and the comparative example, and the following Table 1 details the differences in one or more process parameters between this embodiment and the comparative example.

[0059] 1. First, 1800 kg of polyvinyl alcohol resin having a specific particle size, saponification degree, and polymerization degree of 2000 to 3000 (specific polymerization degrees are shown in Table 1), 4000 kg of water, and 180 kg of plasticizer glycerol were added to a dissolution barrel, and the dissolution temperature was raised to a specified temperature while stirring, the dissolution time was controlled, and the mixture was uniformly dissolved. Then, water was added to adjust the resin concentration to 30 wt%, and a polyvinyl alcohol casting solution (also called a film-forming stock solution) was obtained. The polyvinyl alcohol resin in the examples and comparative examples is a polyvinyl alcohol resin that is polymerized with vinyl acetate and is not modified (i.e., does not contain other comonomers). The specific particle size, saponification degree, polymerization degree, dissolution temperature, and dissolution time of the polyvinyl alcohol resin are shown in Table 1.

[0060] 2. The polyvinyl alcohol casting solution is transported to a twin screw extruder, and the transport temperature is 99℃. The polyvinyl alcohol casting solution is mixed uniformly again in the extruder, degassed, and the temperature of the casting solution is controlled to 98℃. Then, the casting solution is discharged from a T-die lip and cast onto a rotating high-temperature casting drum, and dried and cast to form a preformed film.

[0061] 3. After the polyvinyl alcohol preformed film is peeled off from the casting drum, the top and bottom surfaces of the film are dried by contacting them with 15 heated rollers. The first heated roller is the hottest roller (95°C) among all the heated rollers, and the temperature of the subsequent heated rollers gradually decreases from high to low, until the temperature of the 15th heated roller decreases to 40°C.

[0062] 4. Next, the upper and lower surfaces of the polyvinyl alcohol preformed film were dried with hot air in a floating oven to produce a polyvinyl alcohol film product. The specific maximum drying temperature of the oven is shown in Table 1.

[0063] 5. Thereafter, the polyvinyl alcohol film molded product was placed in a temperature and humidity controller at a temperature of 45° C. and a relative humidity of 50% for 40 minutes to obtain a polyvinyl alcohol film.

[0064] [Table 1]

[0065] 2. Preparation of Polarizers Here, the present invention provides a non-limiting preparation method for preparing a polarizer from a polyvinyl alcohol film. According to the method disclosed below, the polyvinyl alcohol films of the non-limiting examples (Examples 1 to 16) and the polyvinyl alcohol films of the comparative examples (Comparative Examples 1 to 8) are prepared into corresponding polarizers.

[0066] The main steps common to the preparation of polarizers in the examples and comparative examples of the present invention are as follows. After unwinding the polyvinyl alcohol film, it is put into a swelling tank filled with pure water at 30°C for water washing and swelling treatment on the film surface. After stretching the polyvinyl alcohol film 1.2 times its original length in the machine direction, the temperature is then controlled at 30°C, and it is put into a dyeing tank containing an aqueous solution of 0.037 wt% iodine and 1.85 wt% potassium iodide for dyeing while stretching the polyvinyl alcohol film 3.4 times its original length in the machine direction. After dyeing, the temperature is controlled at 55°C, and it is put into a stretching tank containing an aqueous solution of potassium iodide with a concentration of 5.5 wt% each of boric acid and potassium iodide, and the polyvinyl alcohol film is stretched 6 times its original length along the machine direction. Then, the iodine water and boric acid remaining on the film surface are washed with an aqueous solution containing 5.5 wt% potassium iodide. Next, it is dried in an oven at 60°C for 5 minutes, and cellulose triacetate protective films are laminated on the upper and lower surfaces and dried to produce a polarizer.

[0067] 3. Analysis method Here, the present invention provides an analysis and test method for the polyvinyl alcohol films of the above Examples 1 to 16 and Comparative Examples 1 to 8.

[0068] <Resin particle size> Specifically, "pass" shown in Table 1 means that the particle size of the resin raw material is less than or equal to the mesh opening of the sieve used for measurement, and "residual" means that the particle size of the resin raw material is greater than or equal to the mesh opening of the sieve used for measurement.

[0069] <Saponification degree> The measurement method of the saponification degree of the present invention is based on the test method described in JIS K 6726 (1994) standard.

[0070] <Average degree of polymerization> The measurement method of the average degree of polymerization of the present invention is based on the test method described in JIS K 6726 (1994) standard.

[0071] <E’ inflection point temperature> Equipment and its brand: DMA 850 of TA Instruments Sample preparation method: A polyvinyl alcohol film is cut into a long strip of 5 cm in the machine direction (MD) and 5 mm in the transverse direction (TD), and the moisture content of the polyvinyl alcohol film is adjusted to 8-9 wt% before being set in the machine to make the state of the polyvinyl alcohol film consistent. Next, referring to FIG. 2, one end of the polyvinyl alcohol film 2 is fixed with a dovetail clip 3 weighing about 1.11 g, and the other end is inserted into the immersion stretching jig 1, and a part of the polyvinyl alcohol film 2 is placed between the upper fixed shaft 1a and the lower fixed shaft 1b, and the bottom end 3a of the dovetail clip 3 is 1 cm away from the immersion stretching jig 1 (distance a shown in FIG. 2), leaving a space between the upper end 2a of the polyvinyl alcohol film 2 and the upper end of the immersion stretching jig 1. Next, the upper fixed shaft 1a is tightened to fix the polyvinyl alcohol film 2. 3, the entire immersion stretching jig 1, the polyvinyl alcohol film 2 held therein, and the dovetail clip 3 are placed vertically in a 100 mL beaker 4 filled with pure water so that the liquid level of the beaker is located at the upper fixed shaft 1a, the beaker 4 is temperature-controlled in a thermostatic water bath (not shown) at 30° C., and a load (weight of the dovetail clip 3) is applied to the polyvinyl alcohol film 2 to cause it to swell for 20 minutes. Finally, referring to FIG. 4, the immersion stretching jig 1 is removed from the beaker 4 and held vertically, and the polyvinyl alcohol film 2 is stretched by the weight of the dovetail clip 3. After confirming that the polyvinyl alcohol film 2 is in the center, the lower fixed shaft 1b of the immersion stretching jig 1 is tightened, and the excess polyvinyl alcohol film 2c (the mesh-like portion in FIG. 4) is cut off, and the sample is the polyvinyl alcohol film 2b clamped to the immersion stretching jig 1 and subjected to the load and swelling.

[0072] Test conditions: When the above sample is still fixed in the immersion and stretching fixture, select the vibration heating mode, place the sample and the immersion stretching fixture 1 holding the sample together in an immersion bath filled with deionized water, set the frequency to 1Hz, the amplitude to 200μm, the force track to 200%, set the temperature to measure from 30℃ to 65℃, stretch the film with a static force of 0.15N before analysis, then start analyzing with a heating rate of 1℃ / min, and draw the storage modulus (E') vs. temperature change curve. Here, the detection end of the thermocouple is placed at a height of 5mm from the bottom of the water bath.

[0073] Data processing: Convert the storage modulus (E') coordinate axis into a linear coordinate axis, use the onset analysis built into the software provided with the instrument, and set the onset analysis temperature range to 30-45°C. The software will automatically input the inflection point temperature.

[0074] <Softening point temperature> Equipment and brand: TA Equipment TMA Q400

[0075] Sample preparation method: Cut the polyvinyl alcohol film into a circle with a diameter of 5 mm using a punching machine, and adjust the moisture content of the film to 8 to 9 wt% before setting it in the device.

[0076] Test conditions: Using a penetrating probe with a fixed normal force of 0.05 N and a nitrogen flow rate of 100 mL / min, place the above circular sample on a quartz stage with the concave surface (this concave surface is formed by the natural warping of the circular film cut out with a punching machine during the above sample preparation) facing up at room temperature, and then place the measurement tip of the penetrating probe at the center of the sample to measure. Here, the analysis temperature is set to 10 to 150°C, and the heating rate is 10°C / min.

[0077] Data processing: Click the Tg analysis button in the analysis software universal analysis, set the analysis temperature to 15℃~120℃, and plot the temperature together with the dimension change. As shown in Figure 5, the lowest temperature analyzed by the instrument is the softening point temperature (the circled area is the softening point temperature).

[0078] 4. Evaluation method and results Here, the present invention provides evaluation methods for polyvinyl alcohol films and polarizers in Examples and Comparative Examples, and the results of correlation with the above-mentioned analysis contents.

[0079] <Film breakage evaluation> Test conditions: A polyvinyl alcohol film is stretched continuously for 8,000 m to produce a polarizing film.

[0080] Evaluation criteria ◎: No tears during manufacturing process ○: One break occurred during the manufacturing process ×: The product is torn more than once during the manufacturing process.

[0081] Furthermore, Table 2 shows the break evaluation results and E' inflection point temperatures of the polyvinyl alcohol films of Examples 1 to 16 and Comparative Examples 1 to 8 of the present specification.

[0082] [Table 2]

[0083] As can be seen from Table 2, the E' inflection point temperature parameters measured in the E' inflection point temperature analysis of the polyvinyl alcohol film samples of Examples 1 to 16 were all in the range of 37 to 40°C, and it was observed that these polyvinyl alcohol vinyl film samples obtained good film breakage evaluation results. On the other hand, the E' inflection point temperature parameters measured in the E' inflection point temperature analysis of the polyvinyl alcohol film samples of Comparative Examples 1 to 5 were all outside the range of 37 to 40°C, and none of these polyvinyl alcohol film samples obtained good results in the film breakage evaluation. In view of this, the film breakage situation during stretching can be improved simply by controlling the temperature indicated by the inflection point of the storage modulus (E') of the polyvinyl alcohol film in water at 30°C to 55°C to be 37°C to 40°C.

[0084] <Red light leakage evaluation> Preparation of samples: The polyvinyl alcohol films of the embodiment and the comparative example of the present invention are prepared into polarizers according to the above-mentioned manufacturing process of the polarizer, and cut into two samples (FIG. 6) with an area of ​​2×2 cm2 at three locations in the horizontal direction: a location 5 cm away from the left end (distance x shown in FIG. 6), the center, and a location 5 cm away from the right end (distance x shown in FIG. 6). Next, the two polarizers cut out at the same locations are used as test samples.

[0085] Test equipment: Spectrophotometer Jasco V-7100.

[0086] <Test Method> Transmittance Ts (%): According to JIS Z 8722 (measurement method for object color), luminosity correction was performed in the visible light region with a C light source and a 2-degree visual field. It was assumed that the direction of light was the x-axis, the virtual vertical normal perpendicular to the direction of light was the z-axis, and the y-axis was perpendicular to the x-axis and z-axis. One sample was taken from one location and placed on the yz plane, and the direction of light was used as the rotation axis, and the sample was rotated forward so that the angle between the slow axis (here, the MD direction) and the virtual vertical normal (z-axis) was +45°, and the light transmittance was measured. The sample was also rotated backward so that the angle between the slow axis and the virtual vertical normal (z-axis) was +45°, and another light transmittance was measured, and the average value of both was calculated to obtain Y1. Another sample was taken from the same location, and two light transmittances were obtained in the same manner as above, and the average value of the two light transmittances was calculated to obtain Y2. Next, the average value of Y1 and Y2 was calculated to obtain the transmittance Ts (%) of the location.

[0087] Transmittance T700⊥(%): Take two test samples from the same location and stack them on top of each other. Rotate one sample forward so that the angle between the slow axes of the two samples is +45°, and measure the transmittance T45 of 700 nm light. Rotate one polarizer backward so that the angle between the slow axes of the polarizers is -45°, and measure the transmittance T-45 of 700 nm light. Calculate the average value of T45 and T-45 to obtain the transmittance T700⊥(%).

[0088] Red light leakage rate: With transmittance Ts (%) on the horizontal axis and transmittance T700⊥ (%) on the vertical axis, an approximate line was created from the analysis values ​​at three points, and the transmittance T700⊥ (%) obtained from the approximate line when the transmittance was 44% (i.e., the orthogonal transmittance of light with a wavelength of 700 nm) was the red light leakage rate.

[0089] Evaluation criteria: It is preferable that the red light leakage rate (ie, the red light leakage ratio) is less than 5%.

[0090] Furthermore, the evaluation results of red light leakage of the polarizers of Examples 1 to 16 and Comparative Examples 1 to 8 in this specification are shown in Table 3 together with their softening points.

[0091] [Table 3]

[0092] As can be seen from Table 3, when the softening point temperature of the polyvinyl alcohol film is controlled to 45°C or less, the red light leakage rate is less than 5% after the film is manufactured into a polarizer, as shown in Examples 1 to 16 and Comparative Examples 3, 4, and 6 to 8 (although the red light leakage rate of Comparative Examples 3, 4, and 6 to 8 is less than 5%, these are considered to be poor comparative examples because the film breakage evaluation was poor as described above). Conversely, when the softening point temperature of the polyvinyl alcohol film exceeds 45°C, there is a problem that the red light leakage rate exceeds 5% after the film is manufactured into a polarizer (Comparative Examples 1, 2, and 5). In view of this, when the softening point temperature is controlled to 45°C or less, the problem of red light leakage after the polyvinyl alcohol film is manufactured into a polarizer can be improved.

[0093] All ranges provided herein are intended to include each specific range within the stated range, and combinations of subranges between the stated ranges. Also, any range explicitly stated herein includes the endpoints unless otherwise indicated. Thus, the range 1-5 specifically includes 1, 2, 3, 4, and 5, as well as subranges 2-5, 3-5, 2-3, 2-4, 1-4, etc.

[0094] All publications and patents cited in this specification are incorporated herein by reference and for all purposes each individual publication or patent is specifically and individually indicated to be incorporated herein by reference. In the event of a conflict between the present specification and a publication or patent incorporated herein by reference, the present specification will control.

[0095] 1. Immersion stretching jig 1a Upper fixed shaft 1b Lower fixed shaft 2 Polyvinyl alcohol film 2a top edge 2b Polyvinyl alcohol film after loading and swelling 2c Extra polyvinyl alcohol film 3 Dovetail Clips 3a bottom edge 4 Beaker

Claims

1. A polyvinyl alcohol film comprising a polyvinyl alcohol resin having a degree of saponification of 95 mol % or more, the temperature at which the inflection point of the storage modulus (E') in water in the range of 30°C to 55°C is 37 to 40°C.

2. 2. The polyvinyl alcohol film of claim 1, having a softening point temperature of 45° C. or less.

3. The polyvinyl alcohol film according to claim 1 , wherein the polyvinyl alcohol resin has a degree of saponification of more than 99.90 mol %.

4. 4. The polyvinyl alcohol film according to claim 3, wherein the polyvinyl alcohol resin has a degree of saponification of 99.95 mol % or more.

5. 5. The polyvinyl alcohol film according to claim 4, wherein the polyvinyl alcohol resin has a degree of saponification of 99.97 mol % or more.

6. 2. The polyvinyl alcohol film according to claim 1, wherein the polyvinyl alcohol resin has an average degree of polymerization of 2,000 to 3,300.

7. 2. The polyvinyl alcohol film according to claim 1, wherein the average polymerization degree of the polyvinyl alcohol resin is 2,400 to 3,300.

8. The polyvinyl alcohol film according to any one of claims 1 to 3, wherein the polyvinyl alcohol film has a thickness of 40 to 75 µm.

9. An optical film produced from the polyvinyl alcohol film according to any one of claims 1 to 8.

10. 10. The optical film of claim 9 which is a polarizing film.

11. The optical film of claim 10 , wherein the polarizing film has a red light leakage rate of less than 5%.

Citation Information

Patent Citations

  • Recording material

    JP1985245586A

  • Polyvinyl alcohol film and method for producing polarizing film

    JP2022033365A

  • Polyvinyl alcohol resin for production of polarizing film, method for producing same, polyvinyl alcohol film, method for producing polyvinyl alcohol film, polarizing film and polyvinyl alcohol resin

    WO2017033552A1

  • Adhesive and polarizing plate

    WO2020184657A1

  • Layered object, polarizing film, and process for producing polarizing film

    TW201719207A