Polyolefin-based resin foam particle and polyolefin-based resin foam particle molding

Polyolefin resin foam particles with a NOR type hindered amine compound in a specific range address the challenge of maintaining flame retardancy and moldability, resulting in lightweight, moldable articles with enhanced fire resistance.

JP2024169939AActive Publication Date: 2024-12-06JSP CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023086812
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

Foamed particle molded bodies with reduced density and high carbon content tend to burn easily, and increasing the amount of NOR type hindered amine compound to enhance flame retardancy can compromise in-mold moldability.

Method used

Polyolefin resin foam particles containing a NOR type hindered amine compound within a specific content range (0.01% to 3% by mass) and a hydrocarbon group structure, which maintains flame retardancy while preserving moldability.

Benefits of technology

The solution achieves stable flame retardancy and excellent in-mold moldability, producing lightweight foamed particle molded articles suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169939000013
    Figure 2024169939000013
  • Figure 2024169939000001
    Figure 2024169939000001
  • Figure 2024169939000002
    Figure 2024169939000002
Patent Text Reader

Abstract

To provide polyolefin-based resin foam particles which enable provision of a foam particle molding that exhibits good in-mold moldability and excellent flame retardancy, and a polyolefin-based resin foam particle molding which is excellent in flame retardancy.SOLUTION: Polyolefin-based resin foam particles contain an NOR type hindered amine-based compound which has bulk density of 10 kg / m3 or more and 100 kg / m3 or less and is represented by a specific structural formula, wherein a content of the NOR type hindered amine-based compound in the polyolefin-based resin foam particles is 0.01 mass% or more and 3 mass% or less. A polyolefin-based resin foam particle molding has a density of 10 kg / m3 or more and 100 kg / m3 or less, and a content of the NOR type hindered amine-based compound represented by a specific structural formula in the polyolefin-based resin foam particle molding is 0.01 mass% or more and 3 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to expanded polyolefin resin beads containing a flame retardant, and to an expanded polyolefin resin bead molding having excellent flame retardancy obtained by molding the expanded polyolefin resin beads in a mold. [Background technology]

[0002] Polyolefin resin expanded bead moldings obtained by molding expanded polyolefin resin beads in a mold are used in various applications such as packaging materials, vehicle components, and building materials. This type of expanded bead molding may be colored with carbon black or the like. In addition, in order to make the expanded bead molding less flammable, a NOR-type hindered amine compound may be added as a flame retardant to the expanded polypropylene resin beads (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2004-263033 Summary of the Invention [Problem to be solved by the invention]

[0004] Expanded bead moldings that have a low density and are lightweight, and expanded bead moldings that contain a large amount of carbon materials such as carbon black, tend to be easily combustible. Therefore, in order to exhibit the desired flame retardancy, it may be necessary to increase the amount of NOR-type hindered amine compound added to the expanded beads. However, for example, when the amount of the NOR-type hindered amine compound described in Patent Document 1 is increased, there is a risk that the moldability of the expanded beads in the mold may decrease. That is, in order to maintain good moldability of the expanded beads in the mold, it is preferable to add a small amount of NOR-type hindered amine compound. However, when the amount of the NOR-type hindered amine compound added to the expanded beads is suppressed to a small amount in consideration of the influence on the moldability in the mold, etc., the expanded bead molding produced using the expanded beads is difficult to stably exhibit the desired flame retardancy.

[0005] The present invention has been made in view of the above background. That is, the present invention provides expanded polyolefin resin beads capable of giving an expanded bead molding which has excellent in-mold moldability and stably exhibits excellent flame retardancy, and an expanded polyolefin resin bead molding obtained by molding the expanded polyolefin resin beads in a mold. [Means for solving the problem]

[0006] The expanded polyolefin resin particles of the present invention have a bulk density of 10 kg / m 3 More than 100kg / m 3 The expanded polyolefin resin beads contain a NOR type hindered amine compound, the NOR type hindered amine compound being represented by the following general formula (I), and the content of the NOR type hindered amine compound in the expanded polyolefin resin beads is 0.01% by mass or more and 3% by mass or less. [ka] (In general formula (I), R 1 , R 2 , R 3 and R 4each independently represents a hydrocarbon group, and X represents an alkanolamine group.

[0007] The polyolefin resin foamed bead molding of the present invention has a density of 10 kg / m 3 More than 100kg / m 3 The expanded polyolefin resin bead molding contains a NOR type hindered amine compound, the NOR type hindered amine compound being represented by the following general formula (I), and the content of the NOR type hindered amine compound in the expanded polyolefin resin bead molding is 0.01% by mass or more and 3% by mass or less. [ka] (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group. Effect of the Invention

[0008] According to the present invention, there are provided expanded polyolefin resin beads which can give expanded bead moldings which have excellent in-mold moldability and which stably exhibit excellent flame retardancy, and an expanded polyolefin resin bead molding obtained by molding the expanded polyolefin resin beads in a mold. [Brief description of the drawings]

[0009] [Figure 1] 1 is a DSC curve obtained according to the method for measuring the heat of transition of plastics described in JIS K7122:1987 to obtain the total heat of fusion and the heat of fusion of the high-temperature peak of the polyolefin resin foamed beads according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The expanded polyolefin resin beads of the present invention (hereinafter, sometimes simply referred to as the expanded beads of the present invention) and the expanded polyolefin resin bead molding of the present invention (hereinafter, sometimes simply referred to as the expanded bead molding of the present invention) will be described below.

[0011] The expanded beads of the present invention have a bulk density of 10 kg / m 3 More than 100kg / m 3 and contains a NOR type hindered amine compound represented by the following general formula (I). In the following description, the NOR type hindered amine compound represented by the following general formula (I) may be referred to as a specific hindered amine compound. The content of the specific hindered amine compound in the expanded beads of the present invention is adjusted to 0.01% by mass or more and 3% by mass or less. [ka] (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.

[0012] The expanded beads of the present invention having the above-mentioned configuration are excellent in lightness and moldability in a mold, and also in flame retardancy. Therefore, the expanded beads of the present invention can provide an expanded bead molding having a low density, excellent fusion between expanded beads, and excellent flame retardancy that can be stably expressed. In other words, the present invention uses a specific hindered amine compound as a flame retardant, so that even if a relatively large amount of flame retardant is contained, the in-mold moldability of the expanded beads is not easily reduced. Therefore, the present invention can provide polyolefin resin expanded beads that can provide an expanded bead molding exhibiting the desired flame retardancy. In addition, even if a relatively small amount of flame retardant is contained, an expanded bead molding exhibiting the desired flame retardancy can be obtained. Therefore, the present invention can provide polyolefin resin expanded beads in which the decrease in in-mold moldability of the expanded beads caused by the flame retardant is more suppressed. The expanded beads of the present invention will be described in more detail below.

[0013] [Polyolefin resin] The expanded beads of the present invention contain a polyolefin resin as a base resin. In the present invention, the polyolefin resin refers to a homopolymer of an olefin monomer such as ethylene, propylene, butene, or pentene, or a copolymer containing 50 mol % or more of a component derived from an olefin monomer. The base resin may be one type of polyolefin resin or a mixed resin of two or more types of polyolefin resins.

[0014] The polyolefin resin is preferably a polyethylene resin and / or a polypropylene resin. Examples of polyethylene-based resins include resins containing 50 mol% or more of ethylene component units, and specific examples include high-density polyethylene, low-density polyethylene, linear low-density polyethylene, very low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer, etc. Among these, from the viewpoint of stably producing expanded beads with excellent moldability in a mold, it is preferable that the polyethylene-based resin contains linear low-density polyethylene as a main component. More specifically, the proportion of linear low-density polyethylene in the polyethylene-based resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more.

[0015] In addition, examples of polypropylene-based resins include resins containing 50 mol% or more of propylene component units, and specific examples include propylene homopolymers, impact-resistant polypropylenes in which rubber components such as ethylene-propylene rubber are dispersed in polypropylene, which are commercially available as block polypropylenes, propylene-ethylene random copolymers, propylene-ethylene block copolymers, propylene-butene random copolymers, propylene-butene block copolymers, propylene-ethylene-butene random copolymers, and the like. Among these, from the viewpoint of stably producing expanded beads with excellent moldability in a mold, it is preferable that the polypropylene-based resin is mainly composed of propylene-ethylene random copolymers and / or propylene-ethylene-butene random copolymers. More specifically, the proportion of propylene-ethylene random copolymers and / or propylene-ethylene-butene random copolymers in the polypropylene-based resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more.

[0016] From the viewpoint of obtaining an expanded bead molding that has an excellent balance between mechanical properties such as compressive strength and light weight and is particularly suitable for use in applications such as packaging materials, vehicle components, and building materials, it is preferable that the expanded beads in the present invention have a polypropylene-based resin as the base resin. In this case, the melting point of the polypropylene resin constituting the expanded beads is preferably from 125° C. to 160° C., more preferably from 130° C. to 155° C., and even more preferably from 135° C. to 150° C. By using a polypropylene resin having a melting point in the above range as the base resin, it is possible to achieve a good balance between good in-mold moldability of the expanded beads and good compression properties of the expanded bead molded article obtained by molding the expanded beads in a mold.

[0017] The melting point of the polypropylene resin constituting the expanded beads is measured based on JIS K 7121:2012. Specifically, the expanded beads are used as test pieces, and conditioning is performed based on "(2) Measurement of melting temperature after a certain heat treatment" in "3. Conditioning of test pieces" in JIS K 7121:2012. In conditioning, the test piece is heated from 23°C to 200°C at a heating rate of 10°C / min, kept at 200°C for 10 minutes, and then cooled to 23°C at a cooling rate of 10°C / min. After conditioning the test piece in this way, the test piece is heated again to 200°C at a heating rate of 10°C / min to obtain a DSC curve. The flow rate of nitrogen gas in the measurement environment is 30 mL per minute. The apex temperature of the melting peak that appears in the DSC curve obtained by the above is taken as the melting point of the polypropylene resin constituting the expanded beads. When a plurality of melting peaks appear in a DSC curve, the apex temperature of the melting peak having the highest height relative to the baseline is taken as the melting point of the polypropylene resin constituting the expanded beads.

[0018] The expanded beads of the present invention may contain, in addition to the base resin, other resins other than polyolefin resins, elastomers, etc., within the scope of not impairing the objects and effects of the present invention. Examples of resins other than polyolefin resins include thermoplastic resins such as polystyrene resins, vinyl acetate resins, thermoplastic polyester resins, acrylic acid ester resins, methacrylic acid ester resins, and polyarylene sulfide resins. Examples of the elastomer include olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, and amide-based thermoplastic elastomers. The resins and elastomers other than the olefin-based resins are preferably contained in an amount of 20 parts by mass or less, more preferably 10 parts by mass or less, per 100 parts by mass of the polyolefin-based resin (base resin). It is particularly preferable that the expanded beads of the present invention do not substantially contain any other resins or elastomers other than the polyolefin-based resin.

[0019] [NOR type hindered amine compounds] The expanded beads of the present invention contain the NOR type hindered amine compound represented by the following general formula (I) in the range of 0.01% by mass or more and 3% by mass or less. From the viewpoint of being able to exhibit flame retardancy that meets a high standard, the expanded beads of the present invention preferably contain the specific hindered amine compound in the range of 0.02% by mass or more, and more preferably contain it in the range of 0.03% by mass or more. In addition, from the viewpoint of being able to exhibit high flame retardancy and also showing sufficiently excellent moldability in a mold, the expanded beads of the present invention preferably contain the specific hindered amine compound in the range of 2% by mass or less, and more preferably contain it in the range of 1.5% by mass or less. When the expanded beads contain two or more specific NOR type hindered amine compounds, the total content of these compounds is defined as the content of the specific NOR type hindered amine compounds in the expanded beads. A hindered amine compound in which a nitrogen atom in a 2,2,6,6-tetramethyl-4-piperidine structure is bonded to a hydrocarbon group via an oxygen atom, as in the structure represented by the following general formula (I), is called a NOR-type hindered amine. [ka] (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.

[0020] The content of the NOR type hindered amine compound in the expanded beads can be determined, for example, by measuring the expanded beads using proton nuclear magnetic resonance ( 1 It can be determined by proton nuclear magnetic resonance ( 1 When determining the content of the NOR type hindered amine compound by 1 H-NMR, for example, the following method can be used. First, the frozen and crushed foam particles are subjected to Soxhlet extraction using chloroform as a solvent to remove the chloroform-insoluble polymer components. Next, the chloroform-soluble portion obtained by Soxhlet extraction is mixed with acetone to remove the acetone-insoluble portion. The solid obtained by removing the solvent from the acetone-soluble portion is used as a measurement sample and subjected to proton nuclear magnetic resonance ( 1 The content of NOR-type hindered amine compounds in the expanded beads can be determined from the relationship between the measurement results and those of a standard sample (internal standard sample) with a known concentration. 1 As an apparatus for performing the measurement by H-NMR, for example, the AL-400 model manufactured by JEOL Ltd. can be used. In the measurement, the following measurement conditions can be adopted: solvent: CDCl3, internal standard sample: tetrachloroethane (TCE).

[0021] The specific hindered amine compound used in the present invention is different from other NOR-type hindered amine compounds conventionally used as flame retardants, and X in the general formula (I) is an alkanolamine group. The reason why the flame retardancy of the expanded beads is improved and the moldability of the expanded beads is well maintained by using the specific hindered amine compound as a flame retardant is not clear. However, the reason why such excellent effects of the present invention are exhibited is presumed to be as follows. That is, it is presumed that X in the general formula (I) is an alkanolamine group, and the -OH group in this X acts as a catalyst to form a synthetic intermediate of a non-flammable gas during combustion of the expanded beads (expanded bead molding). Therefore, it is presumed that high flame retardancy is exhibited and good moldability is maintained even if the blending amount of the specific hindered amine compound is suppressed. In the above X, the -OH group is brought close to the -NH group to facilitate the above-mentioned catalytic action, and from the viewpoint of facilitating the production of expanded beads which stably exhibit excellent flame retardancy, the number of carbon atoms in X in the above general formula (I) is preferably 1 to 8, more preferably 1 to 6, and further preferably 1 to 4.

[0022] From the viewpoint of being able to more stably obtain expanded beads having good moldability in a mold and exhibiting flame retardancy that satisfies a high standard, R 1 and R 2 The number of carbon atoms in the hydrocarbon group is preferably 1 to 20, more preferably 2 to 16, and even more preferably 3 to 10. 1 and R 2 The hydrocarbon group is preferably an alkyl group or a cycloalkyl group. From the same viewpoint, R 3 and R 4 The number of carbon atoms in the hydrocarbon group is preferably 1 to 20, more preferably 2 to 10, and even more preferably 3 to 8. 3 and R 4 The hydrocarbon group is preferably an alkyl group or a cycloalkyl group. Moreover, it is more preferable that either the following aspect 1 or aspect 2 is satisfied, and it is particularly preferable that both are satisfied. Aspect 1: R in general formula (I) 1 and R 2 is a cyclohexyl group. Aspect 2: R in general formula (I) 3 and R 4 is a butyl group.

[0023] In addition, X in the general formula (I) is an alkanolamine group that is a substituent having a hydroxyl group and an amino group in an alkane skeleton. The specific hindered amine compound used in the present invention is preferably an ethanolamine group in which the alkane skeleton of X has two carbon atoms, and more preferably an ethanolamine group in which the alkane skeleton of X has two carbon atoms and satisfies the above aspects 1 and 2.

[0024] The melting point of the specific hindered amine compound is preferably 60°C or more and 100°C or less, more preferably 70°C or more and 95°C or less, and even more preferably 75°C or more and 90°C or less. When the melting point of the specific hindered amine compound is in the above range, the hindered amine compound can be easily dispersed in the base resin, and expanded beads having excellent moldability in the mold can be stably obtained. In addition, in an expanded bead molding molded using the expanded beads thus obtained, the hindered amine compound tends not to migrate to the surface of the molding. As a result, an expanded bead molding exhibiting excellent flame retardant performance for a long period of time can be stably obtained. The melting point of the NOR type hindered amine compound can be measured by "(1) Visual inspection method" in "3. Melting point measurement method" of JIS K 0064:1992. In addition, the foam particles were analyzed by proton nuclear magnetic resonance ( 1 The structure of the NOR type hindered amine compound contained in the expanded beads may be identified by subjecting the expanded beads to NMR (H-NMR) or the like, and the melting point of the NOR type hindered amine compound having such a structure may be measured, thereby determining the melting point of the NOR type hindered amine compound contained in the expanded beads.

[0025] The molecular weight of the specific hindered amine compound is preferably 1000 or less, more preferably 900 or less. When the molecular weight of the specific hindered amine compound is within the above range, the hindered amine compound is easily dispersed and present in the base resin, and expanded beads having excellent moldability in the mold can be stably obtained. The lower limit of the molecular weight is about 550, and preferably 600. Here, the molecular weight of the NOR type hindered amine compound can be determined as the sum of the atomic weights of the atoms constituting the NOR type hindered amine compound. 1 The structure of the NOR type hindered amine compound contained in the expanded beads may be identified by subjecting the expanded beads to NMR (H-NMR) or the like, and the molecular weight of the NOR type hindered amine compound may be determined from the structure.

[0026] The expanded beads of the present invention contain one or more compounds selected from the specific hindered amine compounds represented by the general formula (I) as a flame retardant. In addition to the specific hindered amine compounds represented by the general formula (I), the expanded beads of the present invention may contain other flame retardants other than the specific hindered amine compounds, as long as the object and effect of the present invention are not impaired. Examples of other flame retardants include NOR-type hindered amine flame retardants other than the specific hindered amine compounds, halogen-based flame retardants, phosphorus-based flame retardants, metal hydroxides, etc. The amount of the flame retardant other than the specific hindered amine compound represented by formula (I) is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, further preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less, relative to 100 parts by mass of the specific hindered amine compound in the expanded beads. It is particularly preferable that the expanded beads of the present invention are substantially free of flame retardants other than the specific hindered amine compound.

[0027] [Carbon materials] The expanded beads of the present invention may further contain a carbon material. In general, expanded bead moldings obtained by molding expanded beads containing a carbon material in a mold tend to be easily flammable. However, the expanded beads of the present invention containing a specific hindered amine compound can exhibit excellent flame retardancy even when they contain a carbon material. The amount of the carbon material in the expanded beads of the present invention is not particularly limited, but from the viewpoint of easily exhibiting excellent flame retardancy, the content of the carbon material in the expanded beads is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.5% by mass or more and 7% by mass or less, and even more preferably 1% by mass or more and 5% by mass or less.

[0028] The carbon material may be, for example, at least one type of carbon powder selected from carbon black, carbon nanotubes, graphite, graphene, carbon nanofibers, carbon microfibers, carbon microcoils, and carbon nanocoils. Among them, the expanded beads of the present invention containing carbon black in the range of 1% by mass to 10% by mass, more preferably 1% by mass to 5% by mass, are preferred because they can provide a black expanded bead molding that is excellent in flame retardancy, fusibility, surface appearance, and recovery. The carbon material contained in the expanded beads of the present invention may be one type, or two or more types.

[0029] The carbon black includes gas furnace black, oil furnace black, acetylene black, channel black, roller black, thermal black, ketjen black, and the like.

[0030] The carbon material content in the expanded beads can be determined, for example, by a thermogravimetric differential thermal analyzer (i.e., TG-DTA). In this case, the expanded beads are first subjected to a measurement based on JIS K7120-1987. Then, the carbon material content in the expanded beads can be determined based on the mass loss rate in a predetermined temperature range (for example, from 400°C to 1000°C) of the TG curve obtained by the measurement.

[0031] [Other additives] The expanded beads of the present invention may contain any additives within the scope of not impairing the purpose and effect of the present invention. Examples of the optional additives include one or more additives selected from a flame retardant auxiliary, a cell regulator, a catalyst neutralizer, a lubricant, a crystal nucleating agent, an antistatic agent, an electrical conductivity imparting agent, an antioxidant, an ultraviolet absorber, etc.

[0032] [Fusing layer] The expanded beads of the present invention may have a fusion layer on the surface thereof for facilitating fusion of the expanded beads with each other even at a lower molding pressure during in-mold molding. The fusion layer may be present on the entire surface of the expanded beads, or may be present on a part of the surface. Examples of the resin constituting the fusion layer include a crystalline polyolefin resin having a melting point lower than that of the base resin constituting the expanded bead body (core layer), and an amorphous polyolefin resin having a softening point lower than that of the base resin constituting the expanded bead body (core layer). In addition, regarding the expanded beads having a fusion layer, the expanded bead body on which the fusion layer is provided on the surface may be referred to as a core layer. When the expanded beads have a fusion layer, the proportion of the fusion layer in the expanded beads is generally 0.5% by weight or more and 20% by weight or less, and preferably 1% by weight or more and 10% by weight or less. In addition, when the expanded beads have a fusion layer having a crystalline polyolefin resin as the base resin, the difference between the melting point of the base resin constituting the expanded bead body and the melting point of the base resin constituting the fusion layer is generally 1°C or more and 30°C or less, preferably 2°C or more and 25°C or less, and more preferably 5°C or more and 20°C or less. The method for forming a fusion layer on the surface of the expanded bead body is not particularly limited, and examples thereof include a method of foaming resin particles having a fusion layer on the surface, a method of obtaining expanded beads and then attaching a fusion layer to the surface of the expanded beads, etc. When foaming resin particles having a fusion layer on the surface to obtain expanded beads, it is preferable to adopt a method in which a fusion layer is laminated on the surface of the resin particles by co-extruding a molten mixture for forming a core layer and a resin melt for forming a fusion layer using an extrusion device capable of co-extrusion when producing the resin particles.

[0033] [Bulk density of foamed particles] The bulk density of the expanded beads of the present invention is 10 kg / m 3 More than 100kg / m 3The following is the results. Generally, as the bulk density of the expanded beads decreases, the amount of base resin constituting the expanded beads decreases, and therefore the burning rate of the expanded bead molding molded using the expanded beads with low bulk density tends to increase. However, the expanded beads of the present invention contain a specific hindered amine compound as a flame retardant. As a result, the present invention can suppress the increase in the burning rate of the expanded bead molding molded using the expanded beads, although the bulk density of the expanded beads is adjusted to the low range described above. In other words, the expanded beads of the present invention can provide an expanded bead molding that is lightweight and exhibits excellent flame retardancy.

[0034] From the viewpoint of further improving the lightness of the foamed bead molding produced by molding the foamed beads of the present invention in a mold, the bulk density of the foamed beads is 80 kg / m 3 It is preferable that the thickness is less than 60 kg / m 3 More preferably, it is 50 kg / m or less. 3 It is even more preferable that: In order to improve the mechanical properties such as the compressive strength of the foamed bead molded article produced by molding the foamed bead of the present invention in a mold, the bulk density of the foamed bead is preferably 12 kg / m 3 It is preferable that the saturation temperature is 15 kg / m or more. 3 More preferably, it is 18 kg / m or more. 3 More preferably, it is equal to or greater than this.

[0035] The bulk density of the expanded beads described above is calculated by the following method. First, the expanded beads to be used for measurement are left to stand for 24 hours or more in an environment of 23°C temperature, 50% relative humidity, and 1 atm. The expanded beads thus obtained are filled into a measuring cylinder with a volume of 1 L or more to a bulk volume of 1 L or more, and after the height of the filled expanded beads is stabilized, the bulk volume (unit: L) of the expanded beads is read from the graduations on the measuring cylinder. The mass (unit: g) of the expanded beads in the measuring cylinder is then divided by the aforementioned bulk volume to obtain the bulk density of the expanded beads (unit: kg / m 3 ) can be obtained.

[0036] [Average bubble diameter of expanded particles] The average cell diameter of the expanded beads is preferably 50 μm or more and 250 μm or less, more preferably 55 μm or more and 200 μm or less, even more preferably 60 μm or more and 150 μm or less, and even more preferably 60 μm or more and 120 μm or less. When the average cell diameter of the expanded beads is within the above range, expanded beads that have good moldability in a mold and can be used to produce an expanded bead molding exhibiting excellent flame retardancy can be stably obtained. The average bubble diameter of the expanded beads can be measured by drawing multiple lines from the outermost surface of the expanded beads through the center to the outermost surface of the opposite side in an enlarged photograph of the cross section of the expanded beads divided into two, and dividing the number of bubbles intersecting each line by the total length of the line. Specifically, it can be measured by the method described in the Examples.

[0037] [High temperature peak of foamed particles] The expanded beads preferably have a crystal structure in which one or more melting peaks (hereinafter referred to as "high-temperature peaks") appear on the high-temperature side of the apex of the melting peak (hereinafter referred to as "intrinsic peak") inherent to the polyolefin resin in a DSC curve obtained by heat flux differential scanning calorimetry. By using expanded beads exhibiting a high-temperature peak for in-mold molding, the molding conditions for molding an expanded bead molding can be selected from a wide range, and the mechanical properties such as the compressive strength of the resulting expanded bead molding can be further improved. From this viewpoint, the heat of fusion of the high-temperature peak (hereinafter also referred to as "high-temperature peak heat") is preferably 5 J / g or more, more preferably 8 J / g or more. In addition, the high-temperature peak heat is preferably 50 J / g or less, more preferably 40 J / g or less.

[0038] The high-temperature peak calorific value of the expanded beads can be calculated by the following method. First, about 3 mg of expanded beads is used as a test piece, and a DSC curve is obtained when the test piece is heated and melted according to the transition heat measurement method for plastics specified in JIS K7122-1987. The temperature range of the DSC curve is from 23°C to a temperature 30°C higher than the temperature at the end of the melting peak, and the heating rate during heating is 10°C / min. In addition, the flow rate of nitrogen gas in the measurement environment is 30 mL per minute. When the expanded beads have a high-temperature peak, the DSC curve shows a characteristic peak a and a high-temperature peak b having a peak on the high-temperature side higher than the peak of the characteristic peak a, as shown in FIG. 1. Note that FIG. 1 is an example of a DSC curve measured based on heat flux differential scanning calorimetry of polyolefin resin expanded beads. Although one high-temperature peak b is shown in FIG. 1, the high-temperature peak b may be two or more.

[0039] Next, a straight line is drawn connecting point I, which corresponds to 80° C. on the DSC curve, and point II, which corresponds to the end temperature of melting of the expanded beads. The end temperature of melting is the high-temperature end point of high-temperature peak b, that is, the point at which high-temperature peak b returns to the high-temperature baseline on the DSC curve.

[0040] Next, as shown in FIG. 1, the intersection point between the line passing through the maximum point III between the intrinsic peak a and the high-temperature peak b and the line connecting points I and II is designated as IV. The area enclosed by the line connecting points I and IV, the line connecting points III and IV, and the DSC curve connecting points I and III is designated as the area of ​​intrinsic peak a. The area enclosed by the line connecting points IV and II, the line connecting points III and IV, and the DSC curve connecting points III and II (shaded area) is designated as the area of ​​high-temperature peak b. The total heat of fusion of the expanded beads is calculated from the sum of the areas of intrinsic peak a and high-temperature peak b obtained as described above, and the heat of fusion of high-temperature peak b is calculated from the area of ​​high-temperature peak b.

[0041] In addition, after obtaining a DSC curve by the above-mentioned method, if the expanded beads are cooled to 23°C at a cooling rate of 10°C / min and then heated again at a heating rate of 10°C / min to obtain a DSC curve, only the characteristic peak a appears in the DSC curve, and the high-temperature peak b disappears from the DSC curve.

[0042] [Polyolefin resin foamed bead moldings] Next, the foamed bead molding of the present invention will be described. The foamed bead molding of the present invention has a molding density of 10 kg / m 3 More than 100kg / m 3 and contains a NOR type hindered amine compound (specific hindered amine compound) represented by the following general formula (I): The content of the specific hindered amine compound in the expanded bead molding is 0.01% by mass or more and 3% by mass or less. [ka] (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.

[0043] The foamed bead molding of the present invention, which contains a specific hindered amine compound in a predetermined range of amount, is excellent in balance between light weight and mechanical properties such as compressive strength, and is also excellent in flame retardancy. The foamed bead molding of the present invention, which is produced by molding the foamed beads of the present invention in a mold, is also excellent in fusion property, surface appearance, and recovery property. Therefore, the foamed bead molding of the present invention can be suitably used for various applications such as vehicle parts and building materials. The content of the NOR type hindered amine compound in the expanded bead molding can be determined by, for example, subjecting the expanded bead molding to proton nuclear magnetic resonance ( 1 H-NMR) or the like.

[0044] As described above, the density of the expanded bead molding of the present invention is 10 kg / m3 More than 100kg / m 3 From the viewpoint of achieving a balance between light weight and mechanical properties such as rigidity, and also ensuring flame retardancy, the density is 12 kg / m 3 More than 80kg / m 3 It is preferable that the thickness is less than 15 kg / m 3 More than 60kg / m 3 It is more preferable that:

[0045] The density of the expanded bead molding is calculated by dividing the mass of the expanded bead molding by the volume calculated based on the outer dimensions.

[0046] <Flame retardancy> The flame retardancy of expanded bead moldings can be evaluated based on the position at which burning ends, the duration of burning, and the burning distance when a flammability test is conducted according to FMVSS (Federal Motor Vehicle Safety Standard) No. 302. The flammability test method according to FMVSS No. 302 is specifically as follows:

[0047] First, the foamed beads are molded in a mold, and then the foamed beads molded body is cut to prepare a plate-shaped test piece. Next, the test piece is left in an environment of 21°C and 50% relative humidity for 24 hours to adjust the condition of the test piece. After the condition is adjusted, a start line is drawn 38 mm away from the base end in the length direction of the test piece, and an end line is drawn 292 mm away from the base end. Next, the test piece is attached to the U-shaped frame of the FMVSS No. 302 dedicated chamber.

[0048] Next, the burner is ignited, and the amount of gas and air is adjusted so that the flame height is 38 mm. In this state, the burner is moved so that the center of the tip of the burner is at the center of the width direction at the base end of the test piece, and the burner flame is kept in contact with the test piece for 15 seconds. After that, the burner flame is removed from the test piece, and the duration of combustion is measured from when the test piece's combustion position reaches the start line until the combustion ends.

[0049] In the present invention, the flame retardancy of the expanded bead molding is evaluated in terms of self-extinguishing property and average burning rate. Specifically, if the test piece does not ignite, if the burning of the test piece ends before reaching the initiation line, or if the burning end position of the test piece is within 51 mm from the initiation line and the burning duration is within 60 seconds, the foamed bead molding is judged to have self-extinguishing properties. If the foamed bead molding does not have self-extinguishing properties, the burning distance from the initiation line is divided by the burning duration to obtain the burning rate. Ten or more test pieces are prepared, the burning rate of each is obtained, and the arithmetic mean of the obtained burning rates is taken as the average burning rate.

[0050] As a result of carrying out the flammability test specified in the FMVSS (Federal Motor Vehicle Safety Standard) No. 302, the burning rate is preferably 102 mm / min or less, more preferably less than 80 mm / min, and even more preferably exhibits self-extinguishing properties. Expanded bead moldings that are evaluated as having more favorable or even more favorable flammability can be suitably used in applications that require particularly high flame retardancy. In particular, expanded bead moldings having self-extinguishing properties are suitable for use as vehicle components, such as automobile bumpers and seat core materials.

[0051] The expanded bead molding of the present invention can be suitably produced, for example, by molding the expanded beads of the present invention in a mold. The expanded bead molding of the present invention produced by molding the expanded beads of the present invention in a mold enjoys the excellent effects of the expanded beads of the present invention described above. For example, the expanded bead molding of the present invention may be produced by molding the black expanded beads of the present invention in a mold. In this case, the expanded bead molding will not only be black, but also exhibit good flame retardancy. From this viewpoint, when the expanded bead molding contains a carbon material, the content of the carbon material in the expanded bead molding is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.5% by mass or more and 7% by mass or less, and even more preferably 1% by mass or more and 5% by mass or less. When the expanded bead molding contains carbon black, the content of carbon black in the expanded bead molding is preferably from 1 to 10% by mass, more preferably from 1 to 5% by mass.

[0052] [Method of manufacturing polyolefin resin foam particles] The method for producing the expanded beads of the present invention is not particularly limited as long as it is a method that can give expanded beads having a content of a specific NOR type hindered amine compound in a specific range. Examples of the method include a method of expanding resin particles containing a specific NOR type hindered amine compound and a method of impregnating expanded beads with a specific NOR type hindered amine compound. Next, a preferred embodiment of the method for producing the expanded beads of the present invention will be described. The expanded beads of the present invention can be obtained by expanding polyolefin resin particles containing a blowing agent. For example, the expanded beads can be produced by a manufacturing method having a foaming step in which polyolefin resin particles containing a blowing agent are released from a pressure vessel together with an aqueous medium under a pressure lower than that in the pressure vessel to be expanded. The polyolefin resin particles have at least a polyolefin resin as a base resin. In addition, it is preferable that the resin particles contain a specific NOR type hindered amine compound.

[0053] In the above-mentioned manufacturing method, the expanded particles obtained in the expansion step may be used as expanded particles as they are. As described later, the expanded particles obtained in the expansion step may be used as first-stage expanded particles, and the first-stage expanded particles may be used to produce expanded particles by performing a second-stage expansion step. From the viewpoint of obtaining expanded particles with a lower bulk density, it is preferable to perform the second-stage expansion step after the expansion step.

[0054] <Granulation process> The method for producing expanded beads preferably includes a granulation step prior to the expansion step, in which polyolefin resin is used as a base resin and polyolefin resin particles (hereinafter referred to as "resin particles") containing at least a specific NOR type hindered amine compound are produced. The method for producing the resin particles in the granulation step is not particularly limited. For example, a polyolefin resin and a specific NOR type hindered amine compound are kneaded and extruded by extrusion molding to produce strands, and then the strands are cut to desired dimensions using a pelletizer or the like to obtain the resin particles.

[0055] <Foaming process> In the foaming process, resin particles are first fed into a pressure vessel and dispersed in an aqueous dispersion medium such as water. At this time, a dispersant, a dispersion aid, a surfactant, or the like may be added to disperse the resin particles in the dispersion medium in the pressure vessel, if necessary.

[0056] As the dispersant, inorganic fine particles such as aluminum oxide, tricalcium phosphate, magnesium pyrophosphate, zinc oxide, kaolin, and mica can be used. These inorganic fine particles may be used alone or in combination of two or more. As the dispersion aid, for example, aluminum sulfate can be used. As the surfactant, for example, anionic surfactants such as sodium alkylbenzenesulfonate, sodium dodecylbenzenesulfonate, and sodium alkanesulfonate can be used. These surfactants may be used alone or in combination of two or more.

[0057] After sealing the pressure vessel, a foaming agent is added to the vessel. This allows the resin particles to be impregnated with the foaming agent. At this time, the impregnation of the resin particles with the foaming agent can be promoted by heating the inside of the pressure vessel. Note that resin particles that have already been impregnated with the foaming agent may be supplied to the pressure vessel.

[0058] After impregnating the resin particles with a predetermined amount of blowing agent, the contents of the pressure vessel are released under a pressure lower than the internal pressure of the vessel, thereby expanding the resin particles to obtain expanded particles (first-stage expanded particles).

[0059] Any additive such as carbon black can be blended into the resin particles, for example, by kneading it with the base resin in the granulation process.

[0060] The blowing agent used in the foaming step may be, for example, an organic physical blowing agent such as a hydrocarbon or a halogenated hydrocarbon, or an inorganic physical blowing agent such as carbon dioxide, nitrogen, air, or water. Examples of the hydrocarbon that may be used as the organic physical blowing agent include butane, pentane, and hexane. Examples of the halogenated hydrocarbon that may be used as the organic physical blowing agent include trichlorofluoromethane, dichlorofluoromethane, and tetrachlorodifluoroethane. The organic physical blowing agent may be one of the above-mentioned substances, or two or more of them may be used in combination. Similarly, the inorganic physical blowing agent may be one of the above-mentioned substances, or two or more of them may be used in combination.

[0061] In the production of the expanded beads of the present invention, the blowing agent is preferably an inorganic physical blowing agent, more preferably carbon dioxide. By expanding the resin beads using such a blowing agent, it is possible to easily obtain expanded beads that can finally produce an expanded bead molding having a high expansion ratio and good flame retardancy. In addition, since carbon dioxide is non-flammable, the use of carbon dioxide as the blowing agent can avoid the deterioration of the flame retardancy of the expanded bead molding caused by the blowing agent.

[0062] The amount of the foaming agent added can be appropriately set depending on the type of base resin, the type of foaming agent, the bulk density of the target expanded particles, etc. For example, when carbon dioxide is used as the foaming agent, the amount added is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 15 parts by mass or less, and even more preferably 1 part by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the resin particles.

[0063] The foaming step may include a step of generating the above-mentioned high-temperature peak before foaming the resin particles. As a method for generating a high-temperature peak, for example, a method of performing heat treatment by holding the resin particles in a dispersion medium within a specific temperature range in a pressure vessel can be adopted. The timing of the heat treatment is not particularly limited, and the heat treatment may be performed at any time before, during, or after the impregnation with the foaming agent, or may be performed across two or more of the above-mentioned times. This heat treatment can obtain expanded particles having a crystal structure that shows a melting peak (intrinsic peak) derived from crystals inherent to the polyolefin resin and a melting peak (high-temperature peak) located at a higher temperature than the inherent peak. Here, as the heat treatment, for example, after the resin particles are put into a pressure vessel, a temperature holding step of holding a predetermined temperature for a predetermined time during a temperature raising step of raising the temperature in the pressure vessel may be performed.

[0064] <Two-stage foaming process> The manufacturing method may further include a second-stage expansion step. The second-stage expansion step is carried out, for example, by pressurizing a pressure-resistant container filled with the first-stage expanded particles obtained in the expansion step with air or the like, impregnating the first-stage expanded particles with air or the like to increase the pressure in the bubbles, and then heating the pressurized first-stage expanded particles to expand them. The heating of the expanded particles in the second-stage expansion step may be carried out in a pressure-resistant container with an adjusted pressure, or may be carried out under a pressure lower than the pressure in the bubbles after removal from the pressure-resistant container. As the first-stage expanded particles used in the second-stage expansion step, it is preferable to use first-stage expanded particles that have been cured under atmospheric pressure after the expansion step is completed.

[0065] In the above-mentioned manufacturing method, the resin particles are expanded in two stages, that is, the expansion step and the second-stage expansion step, so that expanded particles having a low density can be obtained more easily. Although the two-stage expansion step has been described here, the expanded particles obtained in the two-stage expansion step may be used to further carry out a three-stage or more expansion step.

[0066] In this specification, the container used in the foaming step is called a "pressure container" and the container used in the second-stage foaming step is called a "pressure-resistant container", but either container may be used as long as it is sealable and capable of applying pressure.

[0067] [Method of manufacturing polyolefin resin foamed beads] The method for producing an expanded bead molding of the present invention is not particularly limited within the scope of the scope in which an expanded bead molding having the above-mentioned configuration can be obtained. For example, a preferred embodiment of the method for producing an expanded bead molding of the present invention is in-mold molding using the expanded beads of the present invention described above. The in-mold molding includes a wide range of known in-mold molding methods using expanded beads. For example, the in-mold molding of the expanded bead molding of the present invention can be carried out as follows.

[0068] First, the foamed beads of the present invention are filled into a mold having a cavity corresponding to the shape of the desired foamed bead molded product, and a predetermined molding pressure is applied to the foamed beads filled in the mold by a heating medium such as steam to heat them. In this way, the foamed beads in the cavity are heated to further expand and fuse the foamed beads to each other. Next, after the heating with steam or the like is completed, the pressure is released and cooling of the mold and the molded product in the mold is quickly started. When it is confirmed that the pressure (surface pressure) generated on the inner surface of the mold is equal to or lower than a predetermined value, the cooling is stopped, the mold is opened, and the foamed bead molded product is removed from the mold. The cooling method here is not particularly limited, but examples thereof include water cooling. Through such a series of molding steps, a foamed bead molded product corresponding to the shape of the cavity is obtained. EXAMPLES

[0069] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. Tables 1 and 2 show the NOR type hindered amine compounds used and the content (mass %) of the NOR type hindered amine compounds in 100 mass % of the expanded beads.

[0070] Example 1 <Granulation process> A polypropylene resin, carbon black, a NOR-type hindered amine compound, and a cell regulator were fed into an extruder, and the mixture was kneaded and extruded in the extruder to produce strands containing the resin. The strands were then cut using a pelletizer to obtain resin particles with a length / diameter ratio of 2.0 and an average mass of 1.0 mg. As the polypropylene resin, a propylene-ethylene random copolymer having a melting point of 143°C and a melt flow rate of 7g / 10min at 230°C and a load of 2.16kg was used. As the carbon black, furnace black was used and added so that the content of carbon black in the expanded beads was 3% by mass. As the NOR type hindered amine compound, a compound having the structure of the above-mentioned general formula (I) and showing the structure of the following chemical formula (II) (product name: Tinuvin 152, manufactured by BASF, melting point 83°C, molecular weight 757) was used. The NOR type hindered amine compound was added so that the content in the expanded beads was the value shown in Table 1. As the cell regulator, zinc borate powder was used and added so that the content in the expanded beads was 0.05% by mass. [ka]

[0071] <Foaming process> Into an autoclave (pressure vessel) having an internal volume of 5 L, 0.3 parts by mass of a dispersant, 0.01 parts by mass of a dispersion aid, 0.004 parts by mass of a surfactant, and 300 parts by mass of a dispersion medium were sealed relative to 100 parts by mass of resin particles. The dispersant was kaolin, the dispersion aid was aluminum sulfate, the surfactant was sodium dodecylbenzenesulfonate, and the dispersion medium was water. Next, carbon dioxide was supplied as a foaming agent into the autoclave, and the inside of the autoclave was pressurized to a gauge pressure of 1.0 MPa (G). Thereafter, the temperature inside the autoclave was raised at a temperature increase rate of 2°C / min while stirring the inside of the autoclave until it reached 144°C. After the temperature inside the autoclave reached 144°C, this temperature was maintained for 15 minutes while continuing to stir. Next, while stirring inside the autoclave, the temperature inside the autoclave was increased at a rate of 2°C / min until it reached 149°C. After the temperature inside the autoclave reached 149°C, the temperature of 149°C was maintained for 15 minutes while adjusting the pressure inside the autoclave to 2.7 MPa (G) by supplying carbon dioxide into the autoclave. The autoclave was then opened and the contents were released under atmospheric pressure. As a result, the resin particles were expanded to a bulk density of 45 kg / m 3 In this specification, the unit of pressure marked with (G) means a gauge pressure, that is, a pressure value based on atmospheric pressure.

[0072] <Two-stage foaming process> The first-stage expanded particles obtained in the expansion process were left to stand for 24 hours in an environment of 23°C temperature, 50% relative humidity, and 1 atm to cure, and then the cured first-stage expanded particles were filled into a pressure vessel. Air was then injected into the pressure vessel, and the pressure in the pressure vessel was increased from normal pressure to 0.60 MPa (G) over 24 hours. This pressure was maintained for 24 hours to allow the air to permeate the bubbles. Next, the first-stage expanded particles taken out from the pressure vessel were loaded into a second-stage expansion machine, and the first-stage expanded particles were further expanded by supplying steam at a pressure of 0.15 MPa (G) to obtain second-stage expanded particles. Table 1 shows the bulk density, average cell diameter, and heat of fusion of the high-temperature peak of the obtained second-stage expanded particles.

[0073] The bulk density of the second-stage expanded beads was measured according to the method for measuring the bulk density of expanded beads described above. Specifically, the expanded beads were first left in an environment of 23°C temperature, 50% relative humidity, and 1 atm for 24 hours or more. The expanded beads thus obtained were filled into a measuring cylinder marked with 1 L graduations, and the bottom of the measuring cylinder was lightly tapped on the floor several times to stabilize the height of the expanded beads filled in the measuring cylinder at the 1 L graduation. The mass (unit: g) of the expanded beads thus obtained in the measuring cylinder with a bulk volume of 1 L was measured, and the bulk density of the expanded beads (unit: kg / m) was calculated by converting the unit. 3 ) was calculated. The heat of fusion of the high-temperature peak of the second-stage expanded beads was measured according to the method for measuring the heat of fusion of high-temperature peak b described above. The average bubble diameter of the second-stage expanded beads was measured as follows. First, 30 expanded beads were randomly selected. The expanded beads were cut through the center to divide them into two, and an enlarged photograph of one cross section was taken. In each cross section photograph, four lines were drawn from the outermost surface of the expanded beads through the center to the outermost surface on the opposite side so that the angles between the two adjacent lines were equal. The number of bubbles intersecting each line was counted, and the total length of the four lines was divided by the total number of bubbles intersecting the lines to obtain the average bubble diameter of each expanded bead. The average bubble diameter of each expanded bead was then calculated by arithmetically averaging the values ​​of the average bubble diameter of each expanded bead.

[0074] <In-mold molding> The second-stage expanded beads obtained by the above-mentioned method were filled into a mold capable of forming a flat plate of 350 mm in length, 250 mm in width, and 50 mm in thickness, and heated by the following heating method to produce an expanded bead molding. First, with the drain valves on both sides of the mold open, steam was supplied to the mold to perform preheating (exhaust process). After that, steam was supplied from one side of the mold to heat it, and then steam was supplied from the other side of the mold to heat it. Next, steam was supplied from both sides of the mold at a predetermined molding pressure (molding steam pressure) to heat it (main heating). After the main heating was completed, the pressure was released and the mold was water-cooled until the pressure generated on the molding surface of the mold was 0.04 MPa (G), and then the mold was opened and the expanded bead molding was taken out. The obtained molding was cured in an oven at 80°C for 12 hours to obtain an expanded bead molding. The molding pressure range of the expanded beads was evaluated by the following method.

[0075] (Molding pressure range (the range of molding steam pressure that can produce a good product)) In the in-mold molding described above, the molding pressure during in-mold molding was changed by 0.01 MPa to mold an expanded bead molding, and the obtained expanded bead molding was evaluated for fusion, surface appearance, and recovery properties as described below. The molding pressure (molding steam pressure) during in-mold molding that allowed for molding an expanded bead molding that passed all three of the following criteria was confirmed, and the range from the lower limit to the upper limit of the molding steam pressure was defined as the molding pressure range. This confirmed the in-mold moldability of the expanded beads used. The wider the range from the lower limit to the upper limit of the molding steam pressure capable of molding an expanded bead molding that meets the pass standard, the wider the range of molding steam pressure capable of molding a good product, and the more preferable it is. Also, the lower the lower limit of the molding steam pressure capable of molding a good product, the more excellent the productivity is, since a good expanded bead molding can be obtained even at a low molding steam pressure. The range from the lower limit to the upper limit of the molding steam pressure (molding pressure range) at which an expanded bead molding that meets the acceptance standard can be molded is preferably 0.02 MPa or more, more preferably 0.03 MPa or more, and even more preferably 0.04 MPa or more.

[0076] Weldability: The obtained foamed bead molding was folded and broken, and the number of foamed beads present on the broken surface (C1) and the number of broken foamed beads (C2) were determined. The ratio of the number of broken foamed beads to the number of foamed beads (C2 / C1×100) was calculated as the material failure rate. The above measurement was carried out five times using different test pieces, and the material failure rates were calculated for each. When the material failure rate, which was the arithmetic average of the measured values, was 80% or more, it was deemed to have passed, and when it was less than 80%, it was deemed to have failed.

[0077] Surface Appearance: A 100 mm x 100 mm square was drawn in the center of the obtained expanded bead molding, a line was drawn diagonally from one corner of the square, and the number of voids (gaps) of 1 mm x 1 mm or more on the line was counted. A sample with less than 5 voids and no irregularities on the surface was considered to pass, and any other sample was considered to fail.

[0078] Resilience: The thickness of the expanded bead molding obtained by in-mold molding in a flat plate shape with a length of 350 mm, a width of 250 mm, and a thickness of 50 mm was measured near the four corners and at the center. The vicinity of the four corners refers to a region 10 mm inward from the corners of the expanded bead molding toward the center of the plate surface. The center refers to the intersection of a line dividing the expanded bead molding in half in the vertical direction and a line dividing the expanded bead molding in half in the horizontal direction. Next, the ratio (%) of the thickness at the center to the thickness of the thickest part near the four corners was calculated. A ratio of 95% or more was considered to be acceptable, and a ratio of less than 95% was considered to be unacceptable.

[0079] (density) Within the above-mentioned moldable range, molding was performed in the mold at the lowest molding pressure to obtain an expanded bead molding. This expanded bead molding was dried in an environment of 80°C for 24 hours, and then the mass (unit: g) of the expanded bead molding was measured. The mass of the expanded bead molding was then divided by the volume (unit: L) calculated from the external dimensions of the expanded bead molding, and the density (unit: kg / m) of the molding was calculated by converting the units. 3 ) was calculated.

[0080] (50% compressive strength) The foamed bead molding was performed in the mold at the lowest molding pressure within the above-mentioned moldable range to obtain a foamed bead molding. After drying the foamed bead molding for 24 hours in an environment of 80°C, a rectangular parallelepiped test piece with a length of 50 mm, a width of 50 mm, and a thickness of 25 mm was taken from the center of the foamed bead molding. A compression test was performed on the test piece at a compression speed of 10 mm / min based on the method specified in JIS K7220:2006 to obtain a stress-strain curve. The compression test was performed in a laboratory at 23°C. The 50% deformation compression stress of the test piece was calculated based on this stress-strain curve, and this value was taken as the 50% compression strength of the molding.

[0081] (FMVSS test) The flame retardancy was evaluated by a method conforming to the flammability test method specified in FMVSS (Federal Motor Vehicle Safety Standard) No. 302. Specifically, the foamed bead molding was first cut to prepare a test piece having a plate shape of 350 mm in length, 102 mm in width, and 12.7 mm in thickness, with one side surrounded by a side of 350 mm in length and a side of 102 mm in width being a skin surface. A start line was drawn on this test piece at a position 38 mm away from the base end in the length direction, and an end line was drawn at a position 292 mm away from the base end. Using this test piece, a flammability test was performed by a method similar to FMVSS No. 302, with the skin surface in contact with the flame of a burner.

[0082] Average burning rate and self-extinguishing rate: The FMVSS test was performed 10 times, and the average burning rate and self-extinguishing rate were calculated based on the test results. The average burning rate was determined by arithmetically averaging the burning rates measured for each test piece. The burning rate of the test piece was calculated by the following formula (1). [Number 1] B = 60 × D / T (1)

[0083] In the above formula (1), the symbol B is the burning speed (unit: mm / min), the symbol D is the distance the flame traveled (unit: mm), and the symbol T is the time (unit: seconds) required for the flame to travel D mm. If the test piece self-extinguished, the burning rate was treated as 0 mm / min. Here, the test piece was judged to have self-extinguished if "the test piece did not ignite", "the burning of the test piece ended before reaching the burning time measurement start position (i.e., the above-mentioned start line)", or "the burning of the test piece ended within 60 seconds after reaching the burning time measurement start position, and the distance from the measurement start position to the burning end position was within 51 mm".

[0084] The self-extinguishing rate was calculated by dividing the number of tests that were rated as "self-extinguishing" by the total number of tests (10) and expressing the result as a percentage.

[0085] (Examples 2 to 4) First-stage and second-stage expanded beads were produced in the same manner as in Example 1, except that the content of the NOR-type hindered amine compound in the expanded beads was changed to the value shown in Table 1. Using these second-stage expanded beads, molding in a mold was carried out in the same manner as in Example 1 to obtain expanded bead moldings. These were designated Examples 2 to 4, respectively.

[0086] Example 5 Except for using resin particles produced by the following method, first-stage expanded beads and second-stage expanded beads were produced in the same manner as in Example 1. Using these second-stage expanded beads, molding in a mold was carried out in the same manner as in Example 1 to obtain an expanded bead molding. The polypropylene resin, carbon black, NOR type hindered amine compound, and cell regulator used in Example 5 for forming the core layer were the same as those used in Example 1.

[0087] First, a manufacturing apparatus was prepared, which was equipped with an extruder for forming a core layer, a die for forming a multilayer strand attached to the downstream side of the extruder for forming a core layer, and an extruder for forming a fusion layer. The downstream side of the extruder for forming a fusion layer was connected to the die for forming a multilayer strand, and the manufacturing apparatus was configured to be capable of laminating the resin melt for forming each layer in the die and to be capable of co-extrusion.

[0088] As materials for forming the core layer, polypropylene resin, carbon black, a specific NOR type hindered amine compound, and a cell regulator were fed to an extruder for forming the core layer, and melt-kneaded to obtain a polypropylene resin melt. At this time, the amounts of the materials were adjusted so that the content of carbon black in the core layer of the resulting expanded beads was 3% by mass, the content of the specific NOR type hindered amine compound was 0.1% by mass, and the content of the cell regulator was 0.05% by mass. In addition, polypropylene resin, carbon black, and a specific NOR type hindered amine compound were fed to an extruder for forming a fusion layer as materials for forming the fusion layer, and melt-kneaded to obtain a polypropylene resin melt. At this time, the amounts of the materials were adjusted so that the carbon black content was 3 mass% and the specific NOR type hindered amine compound content was 0.1 mass% in the fusion layer of the resulting expanded beads. As the polypropylene-based resin for forming the fusion layer, a propylene-ethylene-butene random copolymer having a melting point of 133° C. and a melt flow rate of 6 g / 10 min at 230° C. and a load of 2.16 kg was used.

[0089] The resin melts for forming each layer formed as described above were introduced into a die for forming a multilayer strand and merged inside the die, and a multilayer strand having a two-layer structure (fusion layer / core layer structure) was extruded from the holes in the die attached to the downstream side of the die. The extruded strand was cooled with water and cut with a pelletizer to obtain polypropylene resin particles (core layer / fusion layer=95 / 5) with a length / diameter ratio of 2.0 and an average mass of 1.0 mg.

[0090] Example 6 Except for not using carbon black, first-stage expanded beads and second-stage expanded beads were produced in the same manner as in Example 1. Using these second-stage expanded beads, molding in a mold was carried out in the same manner as in Example 1 to obtain an expanded bead molding. This was designated Example 6.

[0091] Example 7 The first-stage expanded beads produced in the manufacturing process of Example 1 were used for in-mold molding in the same manner as in Example 1 to obtain an expanded bead molding. This was designated Example 7.

[0092] (Comparative Examples 1 to 4) With regard to the NOR type hindered amine compound used, except that the content was changed as shown in Table 2, first-stage expanded beads and second-stage expanded beads were produced in the same manner as in Example 1. Using these second-stage expanded beads, molding in a mold was carried out in the same manner as in Example 1 to obtain expanded bead moldings. These were designated Comparative Examples 1 to 4. In addition, NOR type hindered amine compounds not having the structure of the above-mentioned general formula (I) were used in Comparative Examples 1 to 4. Specifically, the NOR type hindered amine compound used in Comparative Examples 1 and 2 was "product name: NOR116FF, manufactured by BASF, melting point 108°C, molecular weight 2261", the NOR type hindered amine compound used in Comparative Example 3 was "product name: EVERSORB95, manufactured by Everlight Chemical, liquid at room temperature, molecular weight 737", and the NOR type hindered amine compound used in Comparative Example 4 was a polymer type hindered amine compound, "product name: NOR371FF, manufactured by BASF, melting point 91°C, molecular weight 2800 to 4000".

[0093] For Examples 2 to 7 and Comparative Examples 1 to 4, the high temperature peak, bulk density, and average cell diameter of the expanded beads, and the density, molding pressure range, 50% compressive strength, and FMVSS tests of the expanded bead-based molded bodies were carried out in the same manner as in Example 1. Note that, since the two-stage expansion process was not carried out in Example 7, the first-stage expanded beads were used for each of the above-mentioned measurements.

[0094] [Table 1]

[0095] [Table 2]

[0096] The present invention described above encompasses the following technical ideas. (1) Bulk density is 10kg / m 3 More than 100kg / m 3 The polyolefin resin expanded particles contain a NOR type hindered amine compound, The NOR type hindered amine compound is represented by the following general formula (I): The expanded polyolefin resin particles have a content of the NOR type hindered amine compound of 0.01% by mass or more and 3% by mass or less. [ka] (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group. (2) The expanded polyolefin resin particles according to (1) above, wherein the melting point of the NOR type hindered amine compound is 60° C. or higher and 100° C. or lower. (3) The expanded polyolefin resin particles according to (1) or (2), wherein the molecular weight of the NOR type hindered amine compound is 1,000 or less. (4) The expanded polyolefin resin particles according to any one of (1) to (3), wherein X in the general formula (I) is an ethanolamine group. (5) The expanded polyolefin resin particles according to any one of (1) to (4), further comprising a carbon material. (6) Density is 10 kg / m 3 More than 100kg / m 3 A polyolefin resin foamed bead molding containing a NOR type hindered amine compound, The NOR type hindered amine compound is represented by the following general formula (I): The expanded polyolefin resin bead molding has a content of the NOR type hindered amine compound of 0.01% by mass or more and 3% by mass or less. [ka] (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.

Claims

1. Bulk density is 10 kg / m 3 More than 100kg / m 3 The expanded polyolefin resin particles contain a NOR type hindered amine compound, The NOR type hindered amine compound is represented by the following general formula (I): The expanded polyolefin resin particles have a content of the NOR type hindered amine compound of 0.01% by mass or more and 3% by mass or less. [Formula 1] (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.

2. 2. The expanded polyolefin resin particles according to claim 1, wherein the melting point of the NOR type hindered amine compound is 60° C. or higher and 100° C. or lower.

3. 3. The expanded polyolefin resin particles according to claim 1, wherein the molecular weight of the NOR type hindered amine compound is 1,000 or less.

4. 3. The expanded polyolefin resin particles according to claim 1, wherein X in the general formula (I) is an ethanolamine group.

5. The expanded polyolefin resin beads according to claim 1 or 2, further comprising a carbon material.

6. Density is 10 kg / m 3 More than 100kg / m 3 A polyolefin resin foamed bead molding containing a NOR type hindered amine compound, The NOR type hindered amine compound is represented by the following general formula (I): The expanded polyolefin resin bead molding has a content of the NOR type hindered amine compound of 0.01% by mass or more and 3% by mass or less. [Case 2] (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.

Citation Information

Patent Citations

  • In-mold foam molding of polyolefin-based resin

    JP2004263033A

  • Flooring material

    JP2012140815A

  • Laminate and decorative sheet

    JP2019030998A

  • Method for producing polypropylene-based resin foam particle, and method for producing polypropylene-based resin in-mold foam molded body

    JP2022135455A

  • Polypropylene resin foamed particle, method for producing polypropylene resin foamed particle, and molded body of polypropylene resin foamed particle

    JP2023025507A