Flame-retardant decorative laminate and decorative article including the same
The decorative laminate with a biomass-derived colored layer and phosphorus/boron-based flame retardants addresses the challenge of achieving effective and environmentally friendly flame retardancy, demonstrating improved heat release and rate performance.
Patent Information
- Application Number
- JP2023086987
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
AI Technical Summary
Existing decorative laminates face challenges in achieving both environmentally friendly and effective flame retardancy, particularly when using biomass-derived extender pigments.
A decorative laminate comprising a base material, a colored layer containing at least 15% by mass of phosphorus-based or boron-based flame retardants derived from biomass, and an adhesive layer, which enhances flame retardant performance.
The laminate achieves excellent flame retardant properties with a total heat release of about 8.0 MJ/m² or less and a maximum heat release rate of about 240 kW/m² or less, while being environmentally friendly.
Smart Images

Figure 2024170047000001 
Figure 2024170047000002
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE The present disclosure relates to flame retardant decorative laminates and decorative articles comprising the laminates. [Background technology]
[0002] 2. Description of the Related Art Conventionally, for example, decorative sheets having flame retardant properties have been developed, and such decorative sheets are used in a wide range of fields, such as interior and exterior products.
[0003] Patent Document 1 (JP 2015-182379 A) describes a decorative sheet in which a base sheet, a transparent resin layer, and a surface protective layer are laminated in that order, in which (1) the base sheet contains a resin component and a flame retardant, (2) the content of the flame retardant is 10 to 100 parts by mass per 100 parts by mass of the resin component, (3) the thickness of the base sheet is 15 to 150 μm, (4) the thickness of the transparent resin layer is 15 to 150 μm, and (5) the sum of the thickness of the base sheet, the thickness of the transparent resin layer, and the thickness of the surface protective layer is 40 to 200 μm.
[0004] Patent Document 2 (JP 2017-177527 A) describes a decorative sheet having a thermally foamable base film and a pressure-sensitive adhesive layer provided on at least one side of the base film. In the heat generation test described below, a laminate having a gypsum board and a decorative sheet laminated on the side of the gypsum board to which radiant heat is applied was used as a test piece, and the total heat generation amount of this test piece in a 20-minute test period was 7.2 MJ / m 2 The following decorative sheet is described: Heat generation test: Compliant with ISO 5660-1:2002 cone calorimeter method, with radiant heat conditions on the test piece surface of 50kW / m 2 A pyrogenic test that measures the total amount of heat generated.
[0005] In addition, as described in the background art section of Patent Document 3 (JP 2021-044191 A), for example, it is known that inorganic materials such as calcium carbonate can have flame retardant properties. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-182379 A [Patent Document 2] JP 2017-177527 A [Patent Document 3] Patent Publication No. 2021-044191 Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, against the background of environmental problems, materials that consider environmental problems have been used in materials that constitute decorative laminates. As described in Patent Document 3, inorganic materials such as calcium carbonate also have flame retardant properties, so it was expected that a decorative laminate with flame retardant properties that consider environmental problems could be obtained by using a biomass-derived extender pigment as a pigment to be blended in the colored layer of the decorative laminate. However, when a biomass-derived extender pigment is used, it has been difficult to achieve the flame retardant properties that have been required in recent years in decorative laminates.
[0008] The present disclosure provides a decorative laminate having excellent flame retardant performance with consideration given to environmental aspects, and a decorative article including the laminate. [Means for solving the problem]
[0009] According to one embodiment of the present disclosure, there is provided a flame-retardant decorative laminate comprising a substrate, a color layer, and an adhesive layer, the color layer comprising a biomass-derived extender pigment and at least about 15% by mass of at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants.
[0010] According to another embodiment of the present disclosure, there is provided a decorative article comprising a support member and the above-described decorative laminate adhered to the support member. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide a decorative laminate having excellent flame retardant performance while taking into consideration environmental aspects, and a decorative article including the laminate.
[0012] The above description should not be considered as a disclosure of all embodiments of the present invention and all advantages associated with the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Representative embodiments of the present disclosure will now be described in more detail for the purpose of illustrating the present disclosure, but the present disclosure is not limited to these embodiments.
[0014] In the present disclosure, for example, "on" in "the color layer is disposed on the adhesive layer" means that the color layer is disposed directly on the upper side of the adhesive layer, or that the color layer is disposed indirectly on the upper side of the adhesive layer via another layer.
[0015] In the present disclosure, for example, "under" in "the coloring layer is disposed under the substrate" means that the coloring layer is disposed directly under the substrate, or that the coloring layer is disposed indirectly under the substrate via another layer.
[0016] In the present disclosure, "transparent" refers to an average transmittance of about 80% or more, preferably about 85% or more, or about 90% or more, in the visible light region (wavelength 400 nm to 700 nm) measured in accordance with JIS K 7375. There is no particular limit to the upper limit of the average transmittance, but it can be, for example, less than about 100%, about 99% or less, or about 98% or less.
[0017] In the present disclosure, the term "semi-transparent" refers to an average transmittance in the visible light region (wavelength 400 nm to 700 nm) measured in accordance with JIS K 7375 of less than about 80%, desirably about 75% or less, and is intended to not completely conceal the base.
[0018] In this disclosure, "(meth)acrylic" means acrylic or methacrylic, and "(meth)acrylate" means acrylate or methacrylate.
[0019] In the present disclosure, the term "film" may also include a member called a "sheet."
[0020] Hereinafter, each component will be described in detail for the purpose of illustrating a representative embodiment of the flame-retardant decorative laminate of the present disclosure.
[0021] The flame-retardant decorative laminate of the present disclosure (which may be simply referred to as a "laminate" or "decorative laminate") comprises a substrate, a colored layer, and an adhesive layer, and the colored layer contains a biomass-derived extender pigment and contains at least about 15 mass% of at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants.
[0022] The inventors have discovered that by blending at least about 15 mass% of a specific flame retardant, i.e., at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants, together with a biomass-derived extender pigment in a colored layer, a decorative laminate having good flame retardant performance and being environmentally friendly can be obtained.
[0023] The flame retardancy of the laminate is, for example, based on the ISO 5660-1:2002 cone calorimeter method, and the radiant heat condition on the test piece surface is 50 kW / m 2 The flame retardant decorative laminate of the present disclosure can be evaluated by a heat generation test that measures the total heat generation (sometimes simply referred to as "THR") over a 20-minute test period. Here, the test specimen used in the test is a laminate having a gypsum board and a decorative laminate laminated on the side of the gypsum board to which radiant heat is applied. In some embodiments, the flame retardant decorative laminate of the present disclosure measures the total heat generation of such a test specimen over a 20-minute test period of about 8.0 MJ / m 2 Below, approximately 8.0MJ / m 2 Less than 7.9MJ / m 2 Below, approximately 7.8MJ / m 2 Below, approximately 7.7MJ / m 2 Below, approximately 7.6MJ / m2 or less than 7.5 MJ / m 2 The lower limit of the total calorific value is not particularly limited, and can be, for example, about 4.0 MJ / m 2 Above, approximately 4.5MJ / m 2 Above, approximately 5.0MJ / m 2 Above, approximately 5.5MJ / m 2 or more, or about 6.0 MJ / m 2 It can be more than that.
[0024] In some embodiments, the flame retardant decorative laminate of the present disclosure has a maximum heat release rate (sometimes simply referred to as "PHRR") of about 240 kW / m2 or less as determined by the heat release test described below. 2 Below, approximately 220kW / m 2 Below, approximately 200kW / m 2 Below, approximately 190kW / m 2 or less, or about 180kW / m 2 There is no particular lower limit to the maximum heat generation rate, and it can be, for example, about 100 kW / m 2 Approximately 110kW / m 2 or more, or about 120kW / m 2 It can be more than that.
[0025] In some embodiments, the flame retardant decorative laminate of the present disclosure has a heat release rate of 200 kW / m 2 The time exceeding the limit can be less than about 10.0 seconds, about 9.0 seconds or less, about 7.0 seconds or less, about 5.0 seconds or less, about 3.0 seconds or less, or about 1.0 second or less. There is no particular restriction on the lower limit of the time, and it can be, for example, about 0 seconds or more or more than about 0 seconds.
[0026] The thickness of the flame-retardant decorative laminate of the present disclosure is preferably, for example, about 200 micrometers or less, about 190 micrometers or less, about 180 micrometers or less, about 175 micrometers or less, or about 170 micrometers or less, from the viewpoint of flame retardancy. There is no particular limit to the lower limit of the thickness, and it can be, for example, about 100 micrometers or more, about 110 micrometers or more, or about 120 micrometers or more. Here, the thickness of the laminate refers to the thickness of the laminate in a state in which it is applied to an adherend, and for example, when a release liner is applied to the laminate, it refers to the thickness of the laminate excluding the liner.
[0027] The substrate of the present disclosure can be used as a member that supports the color layer, adhesive layer, and any other layer (for example, surface layer) that constitutes the decorative laminate.
[0028] The substrate is not particularly limited, and may be, for example, a substrate containing at least one selected from the group consisting of polyester resin (e.g., polyethylene terephthalate resin, polyethylene naphthalate resin, or polybutylene terephthalate resin), vinyl chloride resin, resin having a urethane bond, polyolefin resin, polycarbonate resin, (meth)acrylic resin, cellulose resin, polylactic acid resin, and fluororesin. Here, in the present disclosure, "resin having a urethane bond" may include, in addition to urethane resin, for example, a resin prepared using at least one selected from urethane (meth)acrylate and urethane (meth)acrylate oligomer, and the urethane resin may include (meth)acrylic urethane resin.
[0029] Among them, polyester resin is preferred, and polyethylene terephthalate resin (sometimes simply referred to as "PET resin") is more preferred. A substrate containing such a resin can contribute to improving the performance of the decorative laminate, such as its strength (e.g., its flexibility and tear resistance). On the other hand, PET resin, particularly recycled PET resin described below, is a resin that is more flammable than the vinyl chloride resin used as the material of the substrate constituting the conventional decorative laminate. Therefore, it is generally difficult to impart flame retardancy to a decorative laminate having a substrate containing PET resin. The decorative laminate of the present disclosure includes a colored layer that contains a biomass-derived extender pigment and at least one selected from the group consisting of a phosphorus-based flame retardant and a boron-based flame retardant in an amount of about 15% by mass or more, and thus can exhibit excellent flame retardant performance even when PET resin is used as the substrate material.
[0030] The substrate of the present disclosure may contain PET resin in an amount of about 50% by mass or more, about 70% by mass or more, or about 90% by mass or more based on the total amount of resin components of the substrate, or all of the resin components of the substrate may be PET resin.
[0031] The surface of the substrate may be subjected to a surface treatment such as a corona treatment, a plasma treatment, or a primer treatment.
[0032] The thickness of the substrate is not particularly limited, and from the viewpoint of the strength and handling of the decorative laminate, it is preferably about 10 micrometers or more, about 20 micrometers or more, about 30 micrometers or more, or about 40 micrometers or more. The upper limit of the thickness is not particularly limited, and from the viewpoint of flame retardancy, it is preferably about 180 micrometers or less, about 150 micrometers or less, about 100 micrometers or less, about 80 micrometers or less, or about 60 micrometers or less. The thickness of each layer in the flame-retardant decorative laminate of the present disclosure can be defined as the average value of the thicknesses of at least five arbitrary positions in the substrate, for example, measured with a thickness gauge (PC-465N manufactured by TECLOCK). When the layers constituting the laminate are thin and difficult to measure with a thickness gauge, it can also be defined as the average value of the thicknesses of at least five arbitrary positions in the target layer of the laminate, for example, the surface layer, measured with a scanning electron microscope.
[0033] In some embodiments, the substrate of the present disclosure contains recycled PET resin as the PET resin. The substrate of the present disclosure containing recycled PET resin can contribute to providing a decorative laminate that is environmentally friendly.
[0034] The substrate of the present disclosure may contain recycled PET resin in an amount of about 10% by mass or more, about 30% by mass or more, about 50% by mass or more, about 70% by mass or more, or about 90% by mass or more, based on the total amount of the PET resin components in the substrate, or all of the PET resin components may be recycled PET resin. The proportion of recycled PET resin components contained in the recycled PET resin may be about 50% by mass or more, about 70% by mass or more, or about 90% by mass or more, and about 100% by mass or less, based on the total amount of the PET resin components constituting the recycled PET resin. Here, the term "recycled PET resin" refers to a PET resin containing a recycled PET resin component, and may be either a mechanically recycled PET resin or a chemically recycled PET resin. "Mechanically recycled PET resin" refers to PET resin obtained by, for example, recovering used molded products and waste materials and then sorting, crushing, washing, filtering in a molten state, extracting with an organic solvent, and heat treating under reduced pressure, while "chemically recycled PET" refers to PET resin that has been regenerated by further depolymerization, etc.
[0035] The difference between recycled PET resin and virgin PET resin can be evaluated, for example, by using a differential scanning calorimeter (DSC). Recycled PET resin generally has a lower melting point than virgin PET resin because it contains impurities compared to virgin PET resin, or contains copolymer components (e.g., isophthalic acid) depending on the type of molded product from which it is collected. For example, the melting point (peak top) of recycled PET resin calculated from the second heating curve by DSC is about 250±about 5°C, which is about 2 to 3°C lower than the melting point calculated from virgin PET resin in the same manner.
[0036] As the recycled PET resin, recycled raw materials from PET bottles can be used. Such recycled raw materials are polyesters manufactured and molded by normal polymerization and solid-phase polymerization, preferably mainly composed of polyethylene terephthalate, and may contain other polyester components and copolymer components. The recycled raw materials may contain metal compounds such as antimony, germanium, and titanium as catalysts, and phosphorus compounds as stabilizers. Since germanium is often used as a catalyst in polyesters for normal PET bottles, the substrate prepared using recycled raw materials from PET bottles may contain germanium in an amount of about 1 ppm or more, or about 3 ppm or more, and about 100 ppm or less, or about 50 ppm or less, relative to the total amount of the substrate. Therefore, the use of recycled PET resins can be evaluated by examining the amount of germanium in the substrate. Here, the content of germanium in the substrate can be measured by the following analytical method: (Analysis method for germanium) 2g of sample is incinerated and decomposed in a platinum crucible, 5ml of 10% sodium bicarbonate solution is added and evaporated, and hydrochloric acid is further added to evaporate and dry. Heat from 400℃ to 950℃ in an electric furnace and leave for 30 minutes to melt. Dissolve in 10ml of water by heating and transfer to a germanium distillation apparatus (wash with 7.5ml of water x 2). Add 35ml of hydrochloric acid, distill and collect 25ml of distillate. Take an appropriate amount from it and add hydrochloric acid to make the final concentration 1mol / L to 1.5mol / L. Add 2.5ml of 0.25% polyvinyl alcohol solution, 2.5ml of 1% cetyltrimethylammonium chloride solution and 5ml of 0.04% phenylfluorone (2,3,7-trihydroxy-9-phenyl-6-fluorone) solution, and make up to 25ml with water. A yellow complex is formed with germanium, and the absorbance at 505 nm is measured using an absorption spectrophotometer (Shimadzu Corporation, UV-150-02) to perform colorimetric quantification.
[0037] Typically, recycled raw materials from PET bottles may be subjected to alkaline washing using a sodium hydroxide solution and / or a potassium hydroxide solution during the manufacturing stage of the recycled raw materials. As a result, the recycled raw materials may contain sodium and / or potassium in an amount greater than 0 ppm, about 3 ppm or more, or about 5 ppm or more, about 150 ppm or less, about 120 ppm or less, or about 80 ppm or less. Therefore, the use of recycled PET resin can be evaluated by examining the amount of sodium and / or potassium in the substrate. Here, the amount of sodium and / or potassium in the substrate can be measured by the following analytical method: (Analysis of sodium and potassium) The substrate is molded into a disk shape with a thickness of about 5 mm on a smooth metal plate, and the smooth surface is measured with an X-ray fluorescence analyzer. A calibration curve is created using a standard sample whose concentration has been confirmed in advance by emission plasma analysis.
[0038] The substrate of the present disclosure may contain optional components such as fillers, reinforcing materials, antioxidants, UV absorbers, flame retardants, light stabilizers, heat stabilizers, dispersants, plasticizers, flow improvers, surfactants, leveling agents, silane coupling agents, catalysts, pigments, dyes, etc., within the range that does not adversely affect the effects of the present disclosure. The optional components may be used alone or in combination of two or more. The individual and total amounts of the optional components may be determined within the range that does not impair the properties required for the substrate.
[0039] In some embodiments, the substrate of the present disclosure has a flame retardant content of about 10% by mass or less, about 5% by mass or less, about 3% by mass or less, about 1% by mass or less, or about 0.5% by mass or less, or the substrate of the present disclosure does not contain a flame retardant. Substrates containing flame retardants at such ratios or not containing flame retardants have excellent transparency, so that it is possible to reduce or suppress the deterioration of decorative performance caused by a colored layer or the like disposed above or below the substrate. The decorative laminate of the present disclosure includes a biomass-derived extender pigment and a colored layer containing at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants in an amount of about 15% by mass or more, so that it is possible to exhibit excellent flame retardant performance even if the content of the flame retardant in the substrate is low or the substrate does not contain a flame retardant.
[0040] The colored layer of the present disclosure contains a biomass-derived extender pigment and contains at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants in an amount of about 15% by mass or more. The colored layer may be a colored layer, and may be transparent or semi-transparent, or may be opaque, i.e., have concealing properties. The colored layer may be a layer exhibiting a light color such as white or yellow, or a dark color such as red, brown, green, blue, gray, or black. The colored layer may be applied partially to the decorative laminate, but from the viewpoint of flame retardancy, it is preferable that the colored layer is applied to the entire surface of the decorative laminate. The colored layer may have a single layer structure or a laminate structure. The colored layer may be applied directly or indirectly to one side or both sides of the above-mentioned substrate.
[0041] The colored layer can be applied directly or indirectly to one or both sides of the above-mentioned substrate. The method of application to the substrate is not particularly limited, and known methods such as knife coating, bar coating, blade coating, doctor coating, roll coating, and cast coating can be used.
[0042] In the present disclosure, the term "biomass-derived extender pigment" refers to an extender pigment manufactured using biomass, which is a renewable resource derived from plants and animals, as a raw material. Such an extender pigment may be prepared using all of its raw materials derived from biomass, or may be prepared using at least a portion of its raw materials derived from biomass. That is, when at least a portion of the raw materials for the extender pigment are biomass-derived raw materials, the extender pigment may contain biomass components in an amount of about 50% by mass or more, about 70% by mass or more, or about 90% by mass or more, and less than about 100% by mass or about 95% by mass or less, based on the total amount of the components constituting the extender pigment. The biomass-derived extender pigment may be used alone or in combination of two or more kinds.
[0043] There is no particular limitation on the biomass as a raw material, and for example, shells of scallops, oysters, etc., egg shells, wood materials, etc. can be used. From the viewpoint of flame retardancy, the biomass-derived extender pigment preferably contains an inorganic extender pigment derived from biomass (e.g., calcium carbonate, silicon dioxide, calcium oxide), and more preferably contains calcium carbonate derived from biomass. As such extender pigments, for example, products such as scallop powder, oyster shell nanopowder, and pearl powder are commercially available. In some embodiments, the biomass-derived inorganic extender pigment is preferably an uncalcined inorganic extender pigment from the viewpoint of processability, and more preferably an uncalcined calcium carbonate. Here, "uncalcined" means that the biomass pigment has not been calcined at the time of becoming a biomass pigment. Since the uncalcined extender pigment does not undergo a calcination process, it can also contribute to reducing costs and environmental loads.
[0044] The amount of the biomass-derived inorganic body pigment (e.g., calcium carbonate) can be about 50% by mass or more, about 70% by mass or more, or about 90% by mass or more, based on the total amount of the biomass-derived body pigment, and can be about 100% by mass or less, or less than about 100% by mass.
[0045] In some embodiments, the average particle size D50 of the biomass-derived body pigment can be about 100 micrometers or less, and from the viewpoint of decorativeness, it can be preferably about 60 micrometers or less, and more preferably about 40 micrometers or less. Here, the average particle size D50 of the body pigment can be measured using a laser diffraction scattering type particle size distribution measuring device "Microtrac MT3300EX II series" manufactured by Microtrac Bell under measurement conditions conforming to JIS Z 8825:2013.
[0046] Biomass-derived extender pigments contain more impurities than virgin extender pigments, so the difference between them and virgin extender pigments can be evaluated by, for example, thermogravimetry (TG) measurement using a thermal analyzer (TG8120, Rigaku Corporation, Akishima, Tokyo, Japan). TG measurement can be performed by placing about 10 mg of a sample in an aluminum pan, raising the temperature at a rate of 20°C / min, and reaching a maximum temperature of 500°C. Mass loss is slight in virgin extender pigments, but mass loss of several percent is observed in biomass-derived extender pigments. In addition, biomass-derived extender pigments contain more impurities than virgin extender pigments, so more trace elements are detected. Therefore, the difference between biomass-derived extender pigments and virgin extender pigments can also be evaluated by comparing the types and / or amounts of trace elements detected using ICP-MS (ionization radiation analysis by mass spectrometry). In addition, shell-derived extender pigments are sometimes observed to contain a larger amount of at least one element selected from the group consisting of magnesium, manganese, phosphorus, and sodium than industrially produced virgin extender pigments (e.g., calcium carbonate produced by a carbon dioxide gas process).
[0047] The amount of the biomass-derived extender pigment to be blended is preferably, for example, from the standpoint of flame retardancy and coloring property, about 5.0% by mass or more, about 10% by mass or more, about 15% by mass or more, about 17% by mass or more, or about 20% by mass or more and about 40% by mass or less, about 35% by mass or less, about 30% by mass or less, or about 28% by mass or less, relative to the total amount of the colored layer.
[0048] The colored layer of the present disclosure may contain at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants in an amount of about 15% by mass or more, about 17% by mass or more, or about 20% by mass or more. The upper limit of such an amount may be, for example, about 50% by mass or less, about 45% by mass or less, about 40% by mass or less, or about 35% by mass or less. When either the phosphorus-based flame retardant or the boron-based flame retardant is used alone, the blending amount refers to the amount of the single flame retardant, and when the phosphorus-based flame retardant and the boron-based flame retardant are used in combination, the blending ratio of these flame retardants may be set within a range of, for example, 90:10, 80:20, 70:30, 60:40, 50:50, 40:60, 30:70, 20:80, or 10:90 by mass ratio.
[0049] Examples of phosphorus-based flame retardants include monomer-type phosphoric acid ester-based flame retardants such as triaryl phosphate, condensed phosphoric acid ester-based flame retardants such as resorcinol diphenyl phosphate and bisphenol A diphenyl phosphate, phosphonate-type flame retardants, metal phosphonate-based flame retardants, phosphinate-based flame retardants, metal phosphinate-based flame retardants, red phosphorus, and ammonium polyphosphate. Here, as ammonium polyphosphate, surface-coated ammonium polyphosphate (e.g., melamine-coated ammonium polyphosphate) can also be used. In addition, phosphorus nitrogen-based flame retardants that are substituted for melamine polyphosphate, phosphazene compounds, and the like can also be used. Among these, from the viewpoint of flame retardancy, metal phosphinate, melamine polyphosphate, ammonium polyphosphate, and melamine-coated ammonium polyphosphate are preferred, metal phosphinate and melamine polyphosphate are more preferred, and from the viewpoint of water resistance, melamine polyphosphate is particularly preferred. The phosphorus-based flame retardants can be used alone or in combination of two or more.
[0050] A boron-based flame retardant is a flame retardant containing a component containing a boron atom. Examples of boron-based flame retardants include boric acids, borates, boron-based nonmetallic compounds, borate minerals, and organic boron-based compounds. Examples of boric acids include boric acid, orthoboric acid, and metaboric acid. Examples of borates include salts of the above-mentioned borates with metal ions or ammonium ions. Among these, examples of metal species constituting the metal ions include sodium, potassium, calcium, magnesium, barium, aluminum, and zinc. Examples of boron-based nonmetallic compounds include boron oxide and boron nitride. Examples of borate minerals include borax, colemanite, and ulexite. Examples of organic boron-based compounds include borate esters, boronates, and boroxines. Among these, from the viewpoint of flame retardancy, borates are preferred, metal salts of boric acid are more preferred, and zinc borate and alkaline earth metal borate are particularly preferred. The boron-based flame retardants may be used alone or in combination of two or more.
[0051] The colored layer of the present disclosure may contain one or more of various resins. Examples of such resins include thermoplastic resins, thermosetting resins, and radiation curable resins. Specific examples include fluorine-based resins, polyester-based resins such as PET and PEN, (meth)acrylic resins, polyolefin-based resins such as polyethylene and polypropylene, thermoplastic elastomers, polycarbonate resins, polyamide resins, ABS resins, acrylonitrile-styrene resins, polystyrene resins, vinyl chloride-based resins, and resins having urethane bonds. Among these, vinyl chloride-based resins are preferred from the viewpoint of flame retardancy. Here, in the present disclosure, the term "vinyl chloride-based resin" may include, in addition to a homopolymer of vinyl chloride, a copolymer of a vinyl chloride monomer and another monomer copolymerizable therewith. As the other monomer copolymerizable with the vinyl chloride monomer, any monomer that has been commonly used in the past may be used without any particular limitation. Examples of the monomers include vinyl esters such as vinyl acetate, alkyl vinyl ethers such as ethyl vinyl ether and octyl vinyl ether, α-olefins such as ethylene and propylene, monounsaturated acids such as acrylic acid and methacrylic acid, and alkyl esters such as methyl esters of these monounsaturated acids, diunsaturated acids such as maleic acid and itaconic acid, and alkyl esters such as methyl esters of these diunsaturated acids, vinylidene compounds such as vinylidene chloride, and unsaturated nitriles such as acrylonitrile, either alone or in combination. There are no particular limitations on the proportion of these monomers used, and they can be used, for example, in a proportion of about 30% by mass or less or about 20% by mass or less relative to the vinyl chloride monomer.
[0052] The colored layer of the present disclosure may contain optional components such as fillers, reinforcing materials, antioxidants, ultraviolet absorbers, flame retardants other than those mentioned above, light stabilizers, heat stabilizers, dispersants, plasticizers, flow improvers, surfactants, leveling agents, silane coupling agents, catalysts, pigments other than those mentioned above, dyes, etc., within the range that does not adversely affect the effects of the present disclosure. The optional components may be used alone or in combination of two or more. The individual and total amounts of the optional components may be determined within the range that does not impair the properties required for the colored layer.
[0053] The flame-retardant decorative laminate of the present disclosure has a colored layer containing a biomass-derived extender pigment and at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants in an amount of about 15% by mass or more, and therefore can exhibit excellent flame retardant performance. As a result, the colored layer does not need to contain other flame retardants, or, if other flame retardants are contained, the amount of such flame retardants can be less than about 15% by mass, about 10% by mass or less, about 5% by mass or less, about 3% by mass or less, about 1% by mass or less, or about 0.5% by mass or less, based on the total amount of the colored layer.
[0054] The thickness of the colored layer can be, for example, about 15 micrometers or more, about 20 micrometers or more, about 23 micrometers or more, or about 25 micrometers or more, and can be about 90 micrometers or less, about 85 micrometers or less, about 80 micrometers or less, about 75 micrometers or less, about 70 micrometers or less, about 65 micrometers or less, or about 60 micrometers or less. From the viewpoint of flame retardancy, the thickness of the colored layer is preferably about 20 micrometers or more and about 85 micrometers or less.
[0055] In some embodiments, the colored layer of the present disclosure has a ratio of the thickness of the colored layer to the thickness of the decorative laminate that satisfies the range of about 0.20 to about 0.80. When the colored layer of the present disclosure that exhibits flame retardant performance satisfies such a ratio, the flame retardant performance of the decorative laminate can be further improved. Such a ratio can be about 0.20 or more, about 0.21 or more, or about 0.22 or more, and can be about 0.80 or less, about 0.70 or less, about 0.60 or less, or about 0.50 or less.
[0056] The flame retardant decorative laminate of the present disclosure includes an adhesive layer. The adhesive layer is typically a layer that is applied to an adherend, such as a support member of an article described below. The adhesive layer may be transparent or translucent, or may be opaque, i.e., have a hiding property. The adhesive layer may be applied partially or entirely to the decorative laminate. The adhesive layer may be a single layer structure or a laminate structure.
[0057] The adhesive layer can be applied directly or indirectly to one side of the above-mentioned substrate, i.e., the side to be applied to the adherend (the side opposite to the side to be viewed). There is no particular limitation on the method of applying the adhesive layer, and known methods such as knife coating, bar coating, blade coating, doctor coating, roll coating, cast coating, etc. can be used.
[0058] There is no particular limitation on the material of the adhesive layer, and for example, a solvent-based, emulsion-based, pressure-sensitive, heat-sensitive, heat-curing, or ultraviolet-curing adhesive using a commonly used (meth)acrylic polymer, polyolefin polymer, resin having a urethane bond (polyurethane polymer), polyester polymer, polyether polymer, rubber material (e.g., natural rubber, synthetic rubber), silicone polymer, etc. can be used. Among such materials, pressure-sensitive adhesives and heat-sensitive adhesives are preferred from the viewpoint of ease of attachment to an adherend, and pressure-sensitive adhesives and heat-sensitive adhesives prepared using (meth)acrylic polymers are more preferred. Here, in the present disclosure, the term "pressure-sensitive adhesive" refers to an adhesive that is permanently tacky at room temperature (e.g., about 20°C), adheres to various surfaces with light pressure, and does not undergo a phase change (from liquid to solid). In the present disclosure, the term "heat-sensitive adhesive" refers to an adhesive that can develop adhesiveness (tackiness) by heating.
[0059] The adhesive layer of the present disclosure may contain optional components such as tackifier resins, crosslinking agents, conductive fillers, thermally conductive fillers, and other fillers (filling agents), silane coupling agents, plasticizers, thickeners, pigments, dyes, flame retardants, antioxidants, UV absorbers, stabilizers, and the like, within the range that does not adversely affect the effects of the present disclosure. The optional components may be used alone or in combination of two or more. The individual and total amounts of the optional components may be determined within the range that does not impair the properties required for the adhesive layer.
[0060] In some embodiments, the adhesive layer of the present disclosure contains flame retardant in an amount of about 10% by weight or less, about 5% by weight or less, about 3% by weight or less, about 1% by weight or less, or about 0.5% by weight or less, or does not contain flame retardant. The decorative laminate of the present disclosure contains a biomass-derived extender pigment and a colored layer containing at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants in an amount of about 15% by weight or more, so that it can exhibit excellent flame retardant performance even if the amount of flame retardant in the adhesive layer is low or the substrate does not contain a flame retardant.
[0061] The thickness of the adhesive layer of the present disclosure can be, for example, about 5 micrometers or more, about 10 micrometers or more, or about 20 micrometers or more, and can be about 100 micrometers or less, about 80 micrometers or less, or about 50 micrometers or less.
[0062] In some embodiments, the flame-retardant decorative laminate of the present disclosure may include any additional layer other than the above-mentioned layers, provided that the effects of the present invention are not adversely affected. Such additional layers may include, for example, at least one selected from the group consisting of a surface layer, a decorative layer (e.g., a pattern layer, a relief layer), a glittering layer, a bonding layer, and a release liner. The additional layer may be applied to the entire surface or a part of the laminate. The additional layer may have a three-dimensional shape, such as an embossed pattern, on its surface.
[0063] The flame-retardant decorative laminate of the present disclosure has a colored layer containing a biomass-derived extender pigment and at least one selected from the group consisting of phosphorus-based flame retardants and boron-based flame retardants in an amount of about 15% by mass or more, and therefore can exhibit excellent flame retardant performance. As a result, the additional layer does not need to contain other flame retardants, or, if other flame retardants are contained, the amount of such flame retardants contained can be less than about 15% by mass, about 10% by mass or less, about 5% by mass or less, about 3% by mass or less, about 1% by mass or less, or about 0.5% by mass or less, based on the total amount of each additional layer. In particular, if the surface layer contains a high concentration of flame retardant, there is a risk that the performance such as scratch resistance will be reduced. Since the surface layer of the present disclosure can be made to contain a low amount of flame retardant or no flame retardant, the deterioration of the performance such as scratch resistance during use of the decorative article to which the decorative laminate is applied can be reduced or suppressed.
[0064] The material for the surface layer is not particularly limited, and examples thereof include (meth)acrylic resins including polymethyl methacrylate (PMMA) and (meth)acrylic copolymers, resins having urethane bonds (e.g., polyurethane), fluororesins such as ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), and methyl methacrylate-vinylidene fluoride copolymer (PMMA / PVDF), silicone resins, vinyl chloride resins (e.g., polyvinyl chloride (PVC)), polyolefins such as polycarbonate (PC), polyethylene (PE), and polypropylene (PP), polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyamides such as nylon, ethylene / acrylic acid copolymer (EAA) and its ionomers, and copolymers such as ethylene-ethyl acrylate copolymer, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer (EVOH), which can be used alone or in a blend of two or more.
[0065] The surface layer may have a multi-layer structure. For example, the surface layer may be a laminate of films formed from the above resins, or a multi-layer coating of the above resins. The surface layer may have a three-dimensional uneven shape such as an embossed pattern on the entire surface or a part of the surface.
[0066] The surface layer can be formed, for example, by coating the resin composition on the above-mentioned colored layer or substrate directly or via a bonding layer or the like. The coating of the surface layer can be performed before or after applying the decorative laminate to an adherend (for example, a support member described later). Alternatively, the resin composition can be coated on a release liner to form a surface layer film, and the film can be laminated to the colored layer or substrate via a bonding layer. For example, when the colored layer has adhesiveness to the surface layer film, the surface layer film can be laminated directly to the colored layer without a bonding layer. The surface layer film can be formed, for example, by coating a resin material such as a curable (meth)acrylic resin composition or a reactive polyurethane composition on a release liner or the like by knife coating, bar coating, blade coating, doctor coating, roll coating, cast coating, or the like, and curing with light or heat as necessary.
[0067] The surface layer may be a film formed in advance by extrusion, stretching, or the like. Such a film can be laminated to the colored layer or the substrate via a bonding layer. Alternatively, when the colored layer has adhesiveness to such a film, the film can be directly laminated to the colored layer without a bonding layer. By using a film with high flatness as such a film, an appearance with higher surface flatness can be given to the article (structure). The surface layer can also be formed by multilayer extrusion with other layers. As the other layer, for example, a (meth)acrylic film can be used. As the (meth)acrylic film, for example, a resin containing polymethyl methacrylate (PMMA), polybutyl acrylate, (meth)acrylic copolymer, ethylene / acrylic copolymer, ethylene vinyl acetate / acrylic copolymer, etc. can be used in the form of a film. The (meth)acrylic film has excellent transparency and / or scratch resistance, is resistant to heat and / or light, and is unlikely to fade and / or change in gloss. In addition, it has excellent moldability without the use of a plasticizer, and also has excellent contamination resistance because it does not require the use of a plasticizer. Among them, those containing PMMA as the main component are preferable. For example, when a (meth)acrylic resin having excellent scratch resistance is used for the other layer and a fluororesin such as ETFE, PVDF, or PMMA / PVDF having excellent chemical resistance is used for the surface layer, the formed surface layer can have the properties of both layers.
[0068] The surface layer of the present disclosure may contain, as optional components, for example, fillers, matting agents (matting agents), antioxidants, ultraviolet absorbers, flame retardants, light stabilizers, heat stabilizers, rheology modifiers, surface modifiers, hard coat materials, gloss-imparting agents, dispersants, plasticizers, flow improvers, surfactants, leveling agents, silane coupling agents, catalysts, pigments, dyes, etc., within the scope of not adversely affecting the effects of the present disclosure. In particular, by using ultraviolet absorbers such as benzotriazole, Tinuvin (registered trademark) 1130 (manufactured by BASF), and hindered amine light stabilizers (HALS) such as Tinuvin (registered trademark) 292 (manufactured by BASF), discoloration, fading, deterioration, etc. of the colored layer located in the lower layer can be effectively prevented. In addition, by using rheology modifiers such as ACRYSOL (trademark) RM-8W, surfactants such as Dynol (trademark) 604, etc., coatability can be improved. The hard coat material may be contained in the surface layer, or may be applied as a hard coat layer by being separately coated on the surface layer.
[0069] The surface layer may be partially opaque, but is preferably translucent or transparent from the viewpoint of visibility of the colored layer or any decorative layer.
[0070] The thickness of the surface layer is not particularly limited, and may be, for example, about 1 micrometer or more, about 5 micrometers or more, or about 10 micrometers or more, and may be about 150 micrometers or less, about 100 micrometers or less, about 80 micrometers or less, about 50 micrometers or less, about 30 micrometers or less, or about 20 micrometers or less. From the viewpoint of flame retardancy, it is advantageous for the surface layer to be thin, and it is preferable that the surface layer is, for example, about 50 micrometers or less, about 30 micrometers or less, or about 20 micrometers or less.
[0071] In some embodiments, the surface layer includes a matte agent. By incorporating a matte agent, the surface layer can exhibit a matte property. Here, in the present disclosure, the term "matte property" refers to a surface layer that exhibits a lower surface gloss than a surface layer that does not include a matte agent.
[0072] The mattness can be evaluated, for example, by the surface glossiness at a measurement angle of 60 degrees, i.e., the 60-degree surface glossiness. In some embodiments, the surface layer of the decorative laminate of the present disclosure exhibits a 60-degree surface glossiness of about 10.0GU or less, about 8.0GU or less, about 5.0GU or less, about 4.5GU or less, or about 4.0GU or less. There is no particular limit to the lower limit of the surface glossiness, and it can be, for example, about 0.1GU or more, about 0.5GU or more, or about 1.0GU or more. The surface glossiness is a value measured using a portable glossmeter GMX-203 (Murakami Color Research Institute Co., Ltd., Chuo-ku, Tokyo, Japan).
[0073] As the matting agent, for example, resin beads and inorganic particles can be used. The matting agents can be used alone or in combination of two or more kinds.
[0074] The resin beads are not particularly limited, and examples thereof include resin beads prepared from a resin having a urethane bond, a styrene resin, a nylon resin, a polyester resin, a melamine resin, a silicone resin, a (meth)acrylic resin, and the like. The resin beads may be solid or may have voids, and may be used alone or in combination of two or more. Among them, resin beads containing a resin having a urethane bond (sometimes referred to as "urethane resin beads") are preferred from the viewpoints of matte finish, scratch resistance, and conformability when the surface layer is stretched. The surface of the resin beads may be modified with a known surface modifier.
[0075] As the urethane resin beads, crosslinked urethane resin beads obtained by suspension polymerization, seed polymerization, emulsion polymerization, etc. Such resin beads are excellent in flexibility, toughness, scratch resistance, etc., and can impart these properties to the surface layer.
[0076] When the resin beads and the binder are the same type of resin components, for example, when the resin beads and binder contain a urethane component, or when the resin beads and binder contain a (meth)acrylic component, the resin beads have excellent affinity with the binder, and therefore can improve the adhesion with the binder. As a result, even if the laminate is stretched or deformed, the detachment of the resin beads from the binder can be reduced or suppressed. Here, the term "same type of resin components" does not necessarily mean that the constituent components of the resin are completely the same, but also includes cases where one or more common resin components exist in the components constituting the resin. For example, since the resin beads prepared from urethane acrylate contain two types of components, a urethane component and an acrylic component, such resin beads can be said to be the same type of resin component as the urethane resin binder and the same type of resin component as the acrylic resin binder.
[0077] When a light scattering or refraction effect due to resin beads inside the surface layer is expected in addition to the light scattering effect due to the unevenness of the surface layer, it is preferable that the refractive index of the resin beads is different from that of the binder.
[0078] The inorganic particles are not particularly limited, and examples thereof include inorganic oxide particles, mixed oxide particles containing two or more metal elements, or mixtures thereof. Examples of inorganic oxide particles include at least one selected from the group consisting of alumina particles, tin oxide particles, antimony oxide particles, silica particles, zirconia particles, titania particles, and ferrite particles. Examples of mixed oxide particles containing two or more metal elements include mixed oxide particles containing at least two metal elements selected from the group consisting of aluminum, tin, antimony, silicon, zirconium, titanium, and iron. The inorganic particles can be used alone or in combination of two or more. Among them, alumina particles are preferred from the viewpoint of matte property and scratch resistance.
[0079] The average particle size of the matting agent can be about 3 micrometers or more, about 5 micrometers or more, about 7 micrometers or more, about 10 micrometers or more, about 15 micrometers or more, about 16 micrometers or more, about 18 micrometers or more, about 20 micrometers or more, about 23 micrometers or more, or about 25 micrometers or more, and can be about 50 micrometers or less, about 45 micrometers or less, about 40 micrometers or less, about 35 micrometers or less, about 30 micrometers or less, about 25 micrometers or less, about 20 micrometers or less, about 18 micrometers or less, about 17 micrometers or less, about 16 micrometers or less, about 15 micrometers or less, about 14 micrometers or less, about 13 micrometers or less, about 12 micrometers or less, about 11 micrometers or less, or about 10 micrometers or less. The average particle size of the matting agent is the cumulative volume 50% particle size measured using a laser diffraction particle size distribution measuring device.
[0080] The amount of the matting agent can be about 10% by weight or more, about 20% by weight or more, about 30% by weight or more, about 40% by weight or more, about 45% by weight or more, or about 50% by weight or more, and can be about 70% by weight or less, about 65% by weight or less, about 60% by weight or less, about 55% by weight or less, or about 50% by weight or less, relative to the total amount of the surface layer.
[0081] The decorative layer as an additional layer is intended to be a layer capable of imparting decoration other than the decoration by the colored layer described above. Examples of such decorative layers include, but are not limited to, a pattern layer that imparts a pattern such as wood grain, stone grain, geometric pattern, leather pattern, logo, picture, etc. to an article, a relief layer having a concave-convex shape on the surface, and combinations thereof.
[0082] The decorative layer can be applied to the entire surface or part of a layer constituting the decorative laminate, such as, but not limited to, a surface layer, a colored layer, a base material, an adhesive layer, etc., directly or via a bonding layer, etc.
[0083] The pattern layer is not limited to the following, but may be, for example, a pattern such as a design, logo, or picture directly applied to a surface layer, metallic layer, adhesive layer, or the like using a printing method such as gravure direct printing, gravure offset printing, inkjet printing, laser printing, or screen printing. Alternatively, a film, sheet, or the like having a pattern, logo, or picture formed by coating such as gravure coating, roll coating, die coating, bar coating, or knife coating, punching, etching, or the like may be used.
[0084] Materials for the pattern layer include, but are not limited to, inorganic pigments such as carbon black, yellow lead, yellow iron oxide, red iron oxide, and red iron oxide; phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green; organic pigments such as azo lake pigments, indigo pigments, perinone pigments, perylene pigments, quinophthalone pigments, dioxazine pigments, and quinacridone pigments such as quinacridone red; and other pigments dispersed in a binder resin such as a (meth)acrylic resin or a resin having a urethane bond.
[0085] The relief layer may be a thermoplastic resin film having a surface texture formed by a conventional method such as embossing, scratching, laser processing, dry etching, or hot pressing. The relief layer may also be formed by applying a thermosetting or radiation curing resin such as a curable (meth)acrylic resin to a release liner having a texture, curing the resin by heating or irradiating it with radiation, and removing the release liner.
[0086] The thermoplastic resin, thermosetting resin, and radiation curable resin used in the relief layer are not particularly limited, and examples thereof include fluorine-based resins, polyester-based resins such as PET and PEN, (meth)acrylic resins, polyolefin-based resins such as polyethylene and polypropylene, thermoplastic elastomers, polycarbonate resins, polyamide resins, ABS resins, acrylonitrile-styrene resins, polystyrene resins, vinyl chloride-based resins, resins having urethane bonds, etc. The relief layer may contain at least one of the pigments used in the pattern layer.
[0087] The decorative layer of the present disclosure may contain optional components, such as fillers, reinforcing agents, antioxidants, UV absorbers, flame retardants, light stabilizers, heat stabilizers, dispersants, plasticizers, flow improvers, surfactants, leveling agents, silane coupling agents, catalysts, etc., within the scope of the present disclosure that does not adversely affect the effects of the present disclosure.
[0088] The thickness of the decorative layer may be appropriately adjusted depending on the required decorativeness, etc., and is not particularly limited, but can be, for example, about 1.0 micrometer or more, about 3.0 micrometers or more, or about 5.0 micrometers or more, and can be about 50 micrometers or less, about 40 micrometers or less, or about 30 micrometers or less.
[0089] The lustrous layer may be, but is not limited to, a layer that contains a metal selected from aluminum, nickel, gold, silver, copper, platinum, chromium, iron, tin, indium, titanium, lead, zinc, germanium, etc., or an alloy or compound thereof, formed on the entire surface or part of a layer constituting the decorative laminate, for example, the base material or colored layer, by vacuum deposition, sputtering, ion plating, plating, etc. The thickness of the lustrous layer can be appropriately selected depending on the required decorativeness, brightness, etc.
[0090] The flame-retardant decorative laminate of the present disclosure can use a bonding layer (sometimes called a "primer layer") to bond the layers constituting the laminate. As the bonding layer, a solvent-based, emulsion-based, pressure-sensitive, heat-sensitive, heat-curing, or UV-curing adhesive such as a commonly used (meth)acrylic polymer, polyolefin-based polymer, resin having a urethane bond (polyurethane-based polymer), polyester-based polymer, or rubber-based material can be used. The bonding layer can be applied by a known coating method or the like.
[0091] The flame retardant decorative laminate of the present disclosure can typically have a release liner applied to the adhesive layer. The release liner can include, for example, paper; plastic materials such as polyethylene, polypropylene, polyester (e.g., PET), and cellulose acetate; and paper coated with such plastic materials. These liners can have a release-treated surface with a release agent such as silicone. The thickness of the release liner can generally be about 5 micrometers or more, about 15 micrometers or more, or about 25 micrometers or more, and can be about 500 micrometers or less, about 300 micrometers or less, or about 250 micrometers or less.
[0092] The flame retardant decorative laminate of the present disclosure may be, for example, a sheet product, a rolled product, or a three-dimensional shape.
[0093] The following manufacturing method will be described as an example, but the manufacturing method of the flame-retardant decorative laminate of the present disclosure is not limited thereto.
[0094] For example, in the case of a laminate having a structure including a release liner, an adhesive layer, a substrate, a colored layer, and a surface layer in this order, an adhesive is coated on the substrate, and a drying step and a curing step are performed as necessary, and then the release liner is attached to the adhesive layer to form the laminate A. A colored layer composition containing a biomass-derived extender pigment and a specific flame retardant is coated on the substrate surface of the laminate A, and a colored layer is formed by performing a drying step and a curing step as necessary, and then a surface layer composition is coated on the colored layer, and a surface layer is formed by performing a drying step and a curing step as necessary to form a decorative laminate. Alternatively, a colored layer may be applied to the substrate, and then an adhesive may be applied to the colored layer, and then a surface layer may be applied to the substrate surface opposite to the adhesive layer.
[0095] In some embodiments, a decorative article is provided that includes a support member and a flame retardant decorative laminate of the present disclosure adhered to the support member. Such a decorative article can exhibit flame retardant properties. The material for the support member is not particularly limited, and examples thereof include resin materials (e.g., polyolefin resin, polyester resin, (meth)acrylic resin, polycarbonate resin, acrylonitrile-butadiene-styrene copolymer), inorganic materials (e.g., glass, ceramic, concrete, gypsum, calcium silicate, natural stone, asphalt), rubber materials, fabric materials (e.g., woven fabric, knitted fabric, nonwoven fabric), metal or metal alloy materials (e.g., iron, aluminum, stainless steel), and wood materials including paper.
[0096] The shape or configuration of the support member is not particularly limited, and may be, for example, a film shape, a plate shape, a curved shape, an irregular shape, or a three-dimensional shape, and may be a single-layer structure, a laminated structure, or a composite structure in which multiple members of different shapes or materials are combined.
[0097] The article to which the decorative laminate of the present disclosure is applied can be used in various applications. Examples of such applications include signs (e.g., internally illuminated signs and externally illuminated signs); signs (e.g., internally illuminated signs and externally illuminated signs); various interior or exterior parts, such as interior or exterior parts of vehicles such as automobiles, railways, aircraft, and ships (e.g., roof members, pillar members, door trim members, instrument panel members, front members such as bonnets, bumper members, fender members, side sill members, and interior panel members), and interior or exterior parts of buildings (e.g., roof members such as window glass, doors, sashes, and tiles, exterior wall members, wallpaper, etc.); electrical appliances such as personal computers, smartphones, mobile phones, refrigerators, and air conditioners; stationery; furniture; desks; various containers such as cans, etc. Among them, the decorative laminate of the present disclosure has excellent flame retardant performance, so that the article to which the decorative laminate of the present disclosure is applied can be suitably used as an interior or exterior part of a building.
[0098] The method of applying the flame-retardant decorative laminate of the present disclosure to a supporting member (adherend) constituting a decorative article is not particularly limited, and any known method can be used as appropriate. For example, hand application, injection molding methods such as insert injection molding, in-mold molding, over-mold molding, two-color injection molding, core-back injection molding, and sandwich injection molding, lamination, and three-dimensional thermal stretch molding (TOM) can be mentioned. EXAMPLES
[0099] The following examples illustrate specific embodiments of the present disclosure, but are not intended to limit the present invention. All parts and percentages are by weight unless otherwise specified. Numerical values inherently contain errors resulting from measurement principles and measuring devices. Numerical values are presented with significant digits with normal rounding.
[0100] The products used in this example are shown in Table 1 below.
[0101] [Table 1]
[0102] Examples 1 to 15 and Comparative Examples 1 to 5 <Production of PET film substrate with colored layer> A formulation containing each component constituting the colored layer shown in Table 2 and methyl ethyl ketone (MEK) was mixed for about 3 minutes using a Thinky (trademark) AR-250 (Thinky Corporation, Chiyoda-ku, Tokyo, Japan) to obtain a coating liquid for the colored layer. This coating liquid was applied by knife coating onto a transparent PET film substrate (Reshine (registered trademark) TA-065) containing recycled PET. The substrate was dried at about 65°C for about 1.5 minutes and at about 155°C for about 2 minutes to obtain a PET film substrate with a colored layer. The thickness of the colored layer used in each example and comparative example is shown in Table 2.
[0103] Example 1 A formulation containing 20 parts by weight of ETERNACOLL (registered trademark) UW-1005E, 15 parts by weight of Art Pearl (registered trademark) C-800T, 18 parts by weight of Takenate (registered trademark) WB-3936, 34 parts by weight of pure water, 7 parts by weight of isopropyl alcohol (IPA), 3 parts by weight of a rheology modifier, and 3 parts by weight of a surfactant was mixed for about 2 minutes using a Thinky (trademark) AR-250 (manufactured by Thinky Corporation, Chiyoda-ku, Tokyo, Japan) to obtain a coating liquid for the surface layer. This coating liquid was applied by knife coating onto the colored layer of the PET film substrate having the above-mentioned colored layer. The mixture was dried at about 65°C for about 2 minutes and at about 150°C for about 5 minutes to form a surface layer with a thickness of about 12 micrometers.
[0104] A monomer mixture of butyl acrylate and acrylate was copolymerized in ethyl acetate to prepare an acrylic pressure-sensitive adhesive composition containing about 38% by weight of an acrylic copolymer. The resulting composition was applied by knife coating to the surface of the PET film substrate opposite to the surface to which the colored layer was applied so that the thickness after drying was about 38 micrometers, to prepare a decorative laminate. In Table 2, the layer structure of the laminate is classified into the following three types, and the layer structure of Example 1 corresponds to layer structure A: Layer composition A: Surface layer / colored layer / PET base material / adhesive layer Layer composition B: Surface layer / PET base material / colored layer / adhesive layer Layer configuration C: colored layer / PET base material / adhesive layer
[0105] Examples 2 to 7 and Comparative Examples 1 to 3 Each decorative laminate was produced in the same manner as in Example 1, except that the composition and thickness of the colored layer were changed as shown in Table 2.
[0106] Example 8 The surface layer coating liquid obtained in Example 1 was applied by knife coating to the surface opposite to the surface to which the colored layer was applied in the PET film substrate having the above-mentioned colored layer. It was dried at about 65°C for about 2 minutes and at about 150°C for about 5 minutes to form a surface layer with a thickness of about 14 micrometers. Next, the acrylic pressure-sensitive adhesive composition obtained in Example 1 was applied by knife coating on the colored layer so that the thickness after drying was about 38 micrometers, to prepare a decorative laminate.
[0107] Examples 9, 10 and 12 to 15 Each decorative laminate was produced in the same manner as in Example 8, except that the composition and thickness of the colored layer were changed as shown in Table 2.
[0108] Example 11 A PET film substrate with a colored layer was prepared so as to have the composition and thickness shown in Table 2. Next, the acrylic pressure-sensitive adhesive composition obtained in Example 1 was applied by knife coating to the surface of the PET film substrate opposite to the surface to which the colored layer was applied so as to have a thickness after drying of about 38 micrometers, thereby producing a decorative laminate.
[0109] Comparative Example 4 A decorative laminate was produced in the same manner as in Example 11, except that the composition of the colored layer was changed as shown in Table 2.
[0110] Comparative Example 5 A decorative laminate was produced in the same manner as in Example 1, except that the thickness of the surface layer and the composition and thickness of the colored layer were changed as shown in Table 2.
[0111] <Physical property evaluation test> The properties of each decorative laminate were evaluated by carrying out the following tests, the results of which are shown in Table 2.
[0112] (Heat generation test: flame retardant) Test pieces were prepared by layering each decorative laminate cut to 99mm ± 1mm squares on a 12.5mm thick fireproof certified gypsum board (a fireproof material as defined in Ministry of Construction Notification No. 1400 of 2000) cut to 99mm ± 1mm squares.
[0113] After leaving the test piece in an environment of 23°C and 50% relative humidity for at least one week, the test piece was measured using a cone calorimeter (manufactured by Toyo Seiki Seisakusho Co., Ltd., Kita-ku, Tokyo, Japan) in accordance with ISO 5660-1:2002 Cone Calorimeter Method to determine whether the radiant heat condition on the surface of the decorative laminate side of the test piece was 50 kW / m 2 From this test, the total heat generation rate (THR), maximum heat generation rate (PHRR) and maximum heat release rate (200 kW / m2) of the test specimens in the 20-minute test period were measured. 2 The time it took for each of these to exceed this limit was calculated, and the results are shown in Table 2.
[0114] (60 degree gloss test: matte) The 60 degree gloss of the surface layer or colored layer of the decorative laminate was measured using a portable gloss meter GMX-203 manufactured by Murakami Color Laboratory in accordance with JIS Z8741. The gloss was measured at three points, and the average value was used as the representative value. The results are shown in Table 2.
[0115] [Table 2]
[0116] It will be apparent to those skilled in the art that the above-described embodiments and examples can be modified in various ways without departing from the basic principles of the present invention, and that various improvements and modifications of the present invention can be made without departing from the spirit and scope of the present invention.
[0117] Some embodiments of the present disclosure are described in [Item 1] to [Item 9] below. [Item 1] A substrate, a color layer, and an adhesive layer, The colored layer contains a biomass-derived extender pigment and contains 15 mass% or more of at least one selected from the group consisting of a phosphorus-based flame retardant and a boron-based flame retardant. Flame retardant decorative laminates. [Item 2] Item 2. The laminate according to item 1, wherein the thickness of the colored layer is 20 micrometers or more and 85 micrometers or less, the thickness of the laminate is 200 micrometers or less, and the ratio of the thickness of the colored layer to the thickness of the laminate is 0.20 to 0.80. [Item 3] 3. The laminate according to item 1 or 2, wherein the content of the flame retardant in the substrate is 10% by mass or less. [Item 4] 4. The laminate according to any one of items 1 to 3, wherein the colored layer contains a vinyl chloride resin. [Item 5] 5. The laminate according to claim 1, wherein the substrate comprises a polyethylene terephthalate resin. [Item 6] Item 6. The laminate of item 5, wherein the polyethylene terephthalate resin comprises recycled polyethylene terephthalate resin. [Item 7] 7. The laminate according to any one of items 1 to 6, wherein the biomass-derived body pigment contains biomass-derived calcium carbonate. [Item 8] In the heat generation test described below, a laminate having a gypsum board and the laminate laminated on the side of the gypsum board to which radiant heat is applied was used as a test specimen, and the total heat generation amount of the test specimen in a test period of 20 minutes was 8.0 MJ / m 2 8. The laminate according to any one of items 1 to 7, which is: Heat generation test: Compliant with ISO 5660-1:2002 cone calorimeter method, with radiant heat conditions on the test piece surface of 50kW / m 2A heat generation test in which the total heat generation is measured. [Item 9] A support member; The flame-retardant decorative laminate according to any one of items 1 to 8 is attached to the support member. Decorative items.
Claims
1. A substrate, a color layer, and an adhesive layer, The colored layer contains a biomass-derived extender pigment and 15% by mass or more of at least one selected from the group consisting of a phosphorus-based flame retardant and a boron-based flame retardant. Flame retardant decorative laminates.
2. The thickness of the colored layer is 20 micrometers or more and 85 micrometers or less, the thickness of the laminate is 200 micrometers or less, and the ratio of the thickness of the colored layer to the thickness of the laminate is 0.20 to 0.
80. The laminate according to claim 1.
3. The laminate according to claim 1 or 2, wherein the content of the flame retardant in the substrate is 10% by mass or less.
4. The laminate according to claim 1 or 2, wherein the colored layer comprises a vinyl chloride resin.
5. The laminate according to claim 1 or 2, wherein the substrate comprises a polyethylene terephthalate resin.
6. 6. The laminate of claim 5, wherein the polyethylene terephthalate resin comprises recycled polyethylene terephthalate resin.
7. The laminate according to claim 1 or 2, wherein the biomass-derived body pigment comprises biomass-derived calcium carbonate.
8. In the heat generation test described below, a laminate having a gypsum board and the laminate laminated on the side of the gypsum board to which radiant heat is applied was used as a test specimen, and the total heat generation amount of the test specimen in a test period of 20 minutes was 8.0 MJ / m 2 3. The laminate according to claim 1 or 2, which is: Heat generation test: According to ISO 5660-1:2002 cone calorimeter method, the radiant heat condition on the test piece surface is 50kW / m 2 A heat generation test in which the total heat generation is measured.
9. A support member; The flame-retardant decorative laminate according to claim 1 or 2, which is adhered to the support member; A decorative article comprising:
Citation Information
Patent Citations
Decorative sheet and decorative laminate
JP2015182379A
Decorative sheet and manufacturing method thereof