Negative electrode body and method for producing negative electrode body

The negative electrode body with a roughened current collector, multilayer silicon oxide, and conductive ion layer, along with a solid electrolyte, addresses the capacity and stability issues of silicon-based lithium-ion batteries, achieving high capacity and safety by stabilizing the electrode structure and improving cycle characteristics.

JP2024170138AActive Publication Date: 2024-12-06SHIN ETSU CHEMICAL CO LTD
View PDF 28 Cites 0 Cited by

Patent Information

Application Number
JP2023087142
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries using silicon as a negative electrode material face challenges in maintaining high capacity while ensuring safety and stability due to volumetric expansion and irreversible capacity, leading to deteriorated cycle characteristics and safety concerns, especially when using liquid electrolytes.

Method used

A negative electrode body with a roughened current collector, a multilayer structure of silicon oxide and lithium compounds, and a conductive ion layer, combined with a solid electrolyte layer, to enhance ionic conductivity and stabilize the electrode during charging and discharging, reducing expansion and improving cycle characteristics.

Benefits of technology

The proposed design significantly increases battery capacity and maintains excellent cycle characteristics by stabilizing the electrode structure, reducing irreversible capacity, and enhancing safety through the use of a solid electrolyte layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170138000001_ABST
    Figure 2024170138000001_ABST
Patent Text Reader

Abstract

To provide a negative electrode body including a negative electrode that is capable of significantly increasing capacity while maintaining excellent battery characteristics and that is also capable of suppressing expansion when a battery is fully charged.SOLUTION: A negative electrode body includes: a negative electrode that includes a negative electrode current collector with a roughened surface, a negative electrode active material layer provided on the negative electrode current collector, and an ion conductive layer provided on a surface of the negative electrode active material layer and having lithium ion conductivity; and a solid electrolyte layer adjacent to the ion conductive layer. The negative electrode active material layer contains negative electrode active material particles including a compound containing lithium, silicon, and oxygen, and the negative electrode active material particles can be represented by SiOx1Liy1 where the value of x1 is more than 0.8 and 1.2 or less, and the value of y1 is 0.5 or more and 3.4 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anode body and a method for manufacturing the anode body. [Background technology]

[0002] In recent years, small electronic devices such as mobile terminals have become widespread, and there is a strong demand for further miniaturization, weight reduction, and longer life. In response to such market demands, development of secondary batteries that are small, lightweight, and capable of obtaining high energy density has been promoted. The application of these secondary batteries is being considered not only for small electronic devices, but also for large electronic devices such as automobiles and power storage systems such as homes.

[0003] Among these, lithium-ion secondary batteries are attracting great attention because they can be easily made small and have a high capacity, and because they can provide a higher energy density than lead batteries or nickel-cadmium batteries.

[0004] The lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte solution, and the negative electrode contains a negative electrode active material involved in charge and discharge reactions.

[0005] While carbon-based active materials are widely used as negative electrode active materials, recent market demands have called for further improvements in battery capacity. To improve battery capacity, the use of silicon as a negative electrode active material is being considered. This is because the theoretical capacity of silicon (4199mAh / g) is more than 10 times greater than the theoretical capacity of graphite (372mAh / g), and a significant improvement in battery capacity can be expected. In the development of silicon materials as negative electrode active materials, not only silicon itself but also compounds such as alloys and oxides are being considered. In addition, the active material shape is being considered, ranging from the standard coating type for carbon-based active materials to an integrated type that is directly deposited on the current collector.

[0006] However, when silicon is used as the main raw material for the negative electrode active material, the negative electrode active material expands and contracts during charging and discharging, making it prone to cracking, mainly near the surface layer of the negative electrode active material. In addition, ionic substances are generated inside the active material, making the negative electrode active material prone to cracking. When the surface layer of the negative electrode active material cracks, a new surface is created, increasing the reaction area of ​​the active material. At this time, a decomposition reaction of the electrolyte occurs on the new surface, and a coating, which is a decomposition product of the electrolyte, is formed on the new surface, consuming the electrolyte. This makes the cycle characteristics more likely to deteriorate.

[0007] To date, various studies have been conducted on negative electrode materials and electrode configurations for lithium-ion secondary batteries that use silicon materials as the main material in order to improve the initial battery efficiency and cycle characteristics.

[0008] Specifically, in order to obtain good cycle characteristics and high safety, silicon and amorphous silicon dioxide are simultaneously deposited using a gas phase method (see, for example, Patent Document 1). Also, in order to obtain high battery capacity and safety, a carbon material (electron conductive material) is provided on the surface layer of silicon oxide particles (see, for example, Patent Document 2). Furthermore, in order to improve cycle characteristics and obtain high input / output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer with a high oxygen ratio is formed near the current collector (see, for example, Patent Document 3). Also, in order to improve cycle characteristics, oxygen is contained in the silicon active material, and the active material is formed so that the average oxygen content is 40 at% or less and the oxygen content is high in the area close to the current collector (see, for example, Patent Document 4).

[0009] In addition, in order to improve the initial charge-discharge efficiency, a nano-composite containing Si phase, SiO2, and MyO metal oxide is used (see, for example, Patent Document 5). Also, for improving cycle characteristics, SiOx (0.8 ≦ x ≦ 1.5, particle size range = 1 μm to 50 μm) and a carbon material are mixed and fired at high temperature (see, for example, Patent Document 6). Further, for improving cycle characteristics, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1 to 1.2, and the active material is controlled within a range where the difference between the maximum value and the minimum value of the molar ratio near the interface between the active material and the current collector is 0.4 or less (see, for example, Patent Document 7). In addition, in order to improve the battery load characteristics, a metal oxide containing lithium is used (see, for example, Patent Document 8). Also, in order to improve cycle characteristics, a hydrophobic layer such as a silane compound is formed on the surface layer of the silicon material (see, for example, Patent Document 9). Further, for improving cycle characteristics, silicon oxide is used, and conductivity is imparted by forming a graphite film on its surface layer (see, for example, Patent Document 10). In Patent Document 10, regarding the shift value obtained from the RAMAN spectrum of the graphite film, broad peaks appear at 1330 cm-1 and 1580 cm-1, and the intensity ratio I1330 / I1580 satisfies 1.5 < I1330 / I1580 < 3. Also, for improving high battery capacity and cycle characteristics, particles having a silicon microcrystalline phase dispersed in silicon dioxide are used (see, for example, Patent Document 11). In addition, in order to improve overcharge and overdischarge characteristics, a silicon oxide in which the atomic ratio of silicon to oxygen is controlled to 1:y (0 < y < 2) is used (see, for example, Patent Document 12).

[0010] The lithium-ion secondary battery using silicon oxide was started to be shipped by Hitachi Maxell in June 2010 for a rectangular secondary battery for smartphones that employs a nano-silicon composite (see, for example, Non-Patent Document 1). The silicon oxide proposed by Hohl is Si 0+ ~Si 4+It is a composite material with various oxidation states (see Non-Patent Document 2). Kapaklis has also proposed a disproportionated structure in which silicon oxide is separated into Si and SiO2 by applying a thermal load to the silicon oxide (see Non-Patent Document 3). Miyachi et al. have focused on Si and SiO2, which contribute to charging and discharging, among silicon oxides with disproportionated structures (see Non-Patent Document 4), and Yamada et al. have proposed the following reaction formula between silicon oxide and Li (see Non-Patent Document 5).

[0011] 2SiO(Si+SiO2) + 6.85Li + + 6.85e - → 1.4Li 3.75 Si + 0.4Li4SiO4 + 0.2SiO2

[0012] The above reaction formula shows that Si and SiO2 that compose silicon oxide react with Li, and are separated into Li silicide, Li silicate, and some unreacted SiO2.

[0013] The Li silicate formed here is irreversible, and once formed, it is considered to be a stable substance that does not release Li. The capacity per weight calculated from this reaction formula is close to the experimental value, and is recognized as the reaction mechanism of silicon oxide. Kim et al. have defined the irreversible component, Li silicate, associated with the charge and discharge of silicon oxide as Li4SiO4, 7 Li-MAS-NMR and 29 The identification was carried out using Si-MAS-NMR (see Non-Patent Document 6).

[0014] This irreversible capacity is the weakest point of silicon oxide, and there is a need to improve it. Kim et al. have used a Li pre-doping method to form Li silicate in advance, which has significantly improved the initial efficiency of the battery and produced a negative electrode that can withstand practical use (see Non-Patent Document 7).

[0015] Also, instead of doping the electrode with Li, a method of treating the powder has been proposed, which has achieved an improvement in irreversible capacity (see Patent Document 13).

[0016] Silicon oxide, which has improved irreversible capacity, can be used to replace the carbon anode at a high ratio, significantly increasing the capacity of the battery. However, increasing the ratio of silicon oxide in the anode increases the risk of fire in the event of an abnormality in a battery that uses a liquid electrolyte, reducing the safety of the battery.

[0017] Therefore, in order to ensure the safety of batteries, various efforts are being made to develop all-solid-state batteries in which the liquid electrolyte is replaced with a solid electrolyte (see Patent Documents 14 to 17). [Prior art documents] [Patent documents]

[0018] [Patent Document 1] JP 2001-185127 A [Patent Document 2] JP 2002-042806 A [Patent Document 3] JP 2006-164954 A [Patent Document 4] JP 2006-114454 A [Patent Document 5] JP 2009-070825 A [Patent Document 6] JP 2008-282819 A [Patent Document 7] JP 2008-251369 A [Patent Document 8] JP 2008-177346 A [Patent Document 9] JP 2007-234255 A [Patent Document 10] JP 2009-212074 A [Patent Document 11] JP 2009-205950 A [Patent Document 12] Japanese Patent Application Publication No. 06-325765 [Patent Document 13] Japanese Patent Publication No. 2015-156355 [Patent Document 14] Special Publication No. 11-007942 [Patent Document 15] Japanese Patent Publication No. 2017-033647 [Patent Document 16] JP-2018-142431 [Patent Document 17] Special Publication No. 2022-165490 [Patent Document 18] Japanese Patent Publication No. 2003-059492 [Patent Document 19] JP-2015-220196 [Patent Document 20] Japanese Patent Publication No. 2017-068929 [Patent Document 21] JP-2020-068104 [Patent Document 22] JP-2020-030919 [Patent Document 23] JP-2021-128857

Non-licensed documents

[0019]

Non-patent document 1

Non-patent document 2

Non-patent document 3

Non-patent document 4

[0020] As mentioned above, in recent years, small electronic devices such as mobile terminals have been improved in performance and functionality, and lithium ion secondary batteries, which are the main power sources for these devices, are required to have increased battery capacity. As one method for solving this problem, the development of a lithium ion secondary battery consisting of a negative electrode mainly made of silicon material is desired. In addition, lithium ion secondary batteries using silicon materials are desired to have initial charge / discharge characteristics and cycle characteristics that are similar to those of lithium ion secondary batteries using carbon-based active materials. Therefore, by using silicon oxide modified by insertion and partial desorption of Li as the negative electrode active material, cycle characteristics and initial charge / discharge characteristics have been improved. Recently, silicon oxide is mainly used, Li is contained in advance, and Li silicate is generated, reducing the irreversible capacity, which is a disadvantage of silicon oxide, and it has actually begun to be put on the market. A battery was prototyped by replacing Li-SiO-C (Non-Patent Document 8), which uses Li in this silicon oxide, with a high proportion of carbon negative electrode material, and a significant increase in capacity was made possible, but increasing the amount of silicon oxide added reduces safety.

[0021] It has been reported that high safety can be achieved by using a solid electrolyte as the electrolyte to counter this decrease in safety (Patent Documents 18 to 20). However, when a graphite negative electrode is used, an increase in capacity like that of silicon oxide cannot be expected. With lithium negative electrodes or negative electrodes made of silicon-based compounds, even if the Coulomb efficiency can be improved, the deterioration of cycle characteristics due to disconnection of the conductive path caused by volume expansion becomes an issue (Patent Document 21). Even when volume expansion is suppressed using a silicon-based negative electrode, the energy density decreases due to the presence of a void layer or the mixing of a solid electrolyte into the negative electrode (Patent Documents 22 and 23).

[0022] The present invention has been made in consideration of the above problems, and has an object to provide an anode body having a negative electrode that can significantly increase capacity while maintaining excellent battery characteristics and can suppress expansion during full charge, and a method for manufacturing an anode body capable of manufacturing such an anode body. [Means for solving the problem]

[0023] In order to solve the above problems, the present invention provides an anode body having an anode including an anode current collector having a roughened surface, an anode active material layer provided on the anode current collector, and an ion conductive layer having lithium ion conductivity on the surface of the anode active material layer, and having a solid electrolyte layer adjacent to the ion conductive layer, wherein the anode active material layer includes anode active material particles having a compound containing lithium, silicon, and oxygen, and the anode active material particles are SiO x1 Li y1 The negative electrode body can be expressed by the following formula: x1 is greater than 0.8 and not greater than 1.2, and y1 is greater than or equal to 0.5 and not greater than 3.4.

[0024] Such an anode body has an anode active material layer containing anode active material particles having a compound of lithium, silicon, and oxygen, and therefore the battery capacity can be improved. In addition, the anode body of the present invention can directly support the anode active material layer on the roughened surface of the anode current collector without using a binder, a conductive assistant, etc., and can reduce the area not involved in charging and discharging in the electrode, and can also reduce excess voids, so that the energy density of the electrode can be significantly improved. In addition, the anode body of the present invention has a layer (ion conductive layer) having lithium ion conductivity on the surface (outermost surface) of the anode active material layer, and the ion conductive layer and the solid electrolyte layer are adjacent to each other, so that the ion conductivity between the solid electrolyte and the anode active material is improved compared to a conventional anode active material layer using silicon powder or silicon-based compound powder, and the battery characteristics can be improved. Furthermore, the anode body of the present invention can be an anode body capable of suppressing expansion during full charge. Furthermore, the anode body of the present invention can be an anode body capable of suppressing expansion during full charge. Furthermore, the anode body of the present invention can be an anode body capable of suppressing expansion during full charge, so that the composition formula of the anode active material particles is SiO x1 Li y1 When the value of x1 is more than 0.8 and not more than 1.2 and the value of y1 is 0.5 or more and not more than 3.4, excellent battery characteristics can be maintained. In the description of the present invention, the negative electrode and the solid electrolyte integrated together are referred to as a negative electrode body.

[0025] In this case, the negative electrode active material layer has a multilayer structure consisting of two or more layers, and when the negative electrode active material particles are defined as primary particles, the negative electrode active material layer forms secondary particles which are aggregates of the primary particles, and the secondary particles have a morphology separated from each other in an in-plane direction, and the thickness T1 of the negative electrode active material layer before charging and the thickness T2 when fully charged can have a relationship of T2 / T1≦1.4.

[0026] In this way, the negative electrode body of the present invention can have a multilayer structure, and the negative electrode active material particles can form secondary particles. The negative electrode active material layer having a multilayer structure consisting of two or more layers can mitigate the expansion and contraction of the negative electrode active material layer. Therefore, the negative electrode body of the present invention can suppress the change in thickness before and after charging. If the thickness T1 of the negative electrode active material layer before charging and the thickness T2 when fully charged have a relationship of T2 / T1≦1.4, the expansion and contraction of the active material during charging and discharging is suppressed, electronic contact is less likely to be broken, and excellent battery characteristics can be maintained.

[0027] In addition, it is preferable that the negative electrode active material layer having a multilayer structure has an interlayer lithium ion conductive layer having lithium ion conductivity between at least one of the layers constituting the multilayer structure.

[0028] Such a negative electrode body has improved ionic conductivity and can reduce the resistance between the negative electrode active material layers, thereby improving the battery performance.

[0029] Moreover, the negative electrode active material layer preferably contains at least one of Li4SiO4, Li2Si2O5, Li2SiO3, and Li6Si2O7.

[0030] By containing at least one of these Li silicates, the battery is stable during charging and discharging, and therefore exhibits excellent cycle characteristics.

[0031] In addition, the ion-conducting layer having lithium ion conductivity is preferably made of at least one of a carbonate of Li, a phosphate of Li, a fluoride of Li, a carbonate of Al, a phosphate of Al, a fluoride of Al, a compound having a silyl group, and a carbonized material containing a polycyclic aromatic hydrocarbon.

[0032] By using such an ion-conducting layer, reactions with moisture and oxygen can be suppressed, deterioration of the material can be suppressed, Li can be easily introduced, and excellent battery characteristics can be maintained.

[0033] Moreover, the secondary particles of the negative electrode active material layer preferably consist of four or more primary particles on average.

[0034] Such a negative electrode body can more effectively prevent electrode collapse due to charging and discharging, and can maintain a stable negative electrode active material layer.

[0035] In the negative electrode body of the present invention, the solid electrolyte layer may be made of a sulfide-based solid electrolyte.

[0036] There is a risk that the sulfide-based solid electrolyte will react with lithium released from the silicon-based active material and generate heat, but the negative electrode body of the present invention has an ion-conducting layer on its surface, which can suppress this reaction. This makes it possible to design a safe battery that does not easily generate heat while maintaining high ion conductivity.

[0037] In this case, the sulfide-based solid electrolyte may contain at least one of lithium, indium, sulfur, and phosphorus.

[0038] The sulfide-based solid electrolyte may include at least one of Li2S, P2S5, SiS2, LiI, LiBr, P2O5, Li3PO4, and GeS2.

[0039] In the negative electrode body of the present invention, the above-mentioned sulfide-based solid electrolyte can be suitably used.

[0040] Also, in the negative electrode body of the present invention, the solid electrolyte layer can be made of an oxide-based solid electrolyte.

[0041] Since the oxide-based solid electrolyte is stable in air and easy to handle, a safe battery can be designed.

[0042] At this time, the oxide-based solid electrolyte can have a perovskite structure.

[0043] At this time, the oxide-based solid electrolyte can contain at least one of lanthanum, lithium, magnesium, tungsten, niobium, and titanium.

[0044] Also, the oxide-based solid electrolyte has a composition formula of A x2 BO3 (0 < x2 < 1), and the element A contains at least one of La and Li, and the element B can contain at least one of Mg, W, Nb, and Ti.

[0045] Also, the oxide-based solid electrolyte can have a NASICON-type phosphate compound.

[0046] In this case, the solid electrolyte having the NASICON-type phosphate compound can contain at least one of lithium, aluminum, germanium, zirconium, titanium, and calcium.

[0047] Also, the NASICON-type phosphate compound is represented by Li (1+x3) M1 (x3) M2 (2-x3) (PO4)3, the element M1 contains at least one selected from the group consisting of Al, Y, Ga, and In, the element M2 contains at least one selected from the group consisting of Ti, Ge, and Zr, and x3 satisfies 0 ≦ x3 ≦ 2.

[0048] The oxide-based solid electrolyte may have a garnet-type crystal structure.

[0049] The solid electrolyte having a garnet-type crystal structure may contain at least one of lithium, lanthanum, calcium, zirconium, bismuth, aluminum, cerium, gallium, boron, and oxygen.

[0050] The solid electrolyte having a garnet-type crystal structure is Li (7-3x4+y4-z4) M x4 La (3-y4) A' (y4) Zr (2-z4) T (z4) O 12 (The element M is one or more of Al and Ga, the element A' is one of Ca and Sr, and T is one of Nb and Ta, and 0≦x4≦0.18, 0≦y4≦0.18, and 0≦z4≦1.5 are satisfied.)

[0051] In the negative electrode body of the present invention, the above-mentioned oxide-based solid electrolyte can be suitably used.

[0052] The present invention also provides a method for producing an anode body for producing any of the above-mentioned anode bodies, the method comprising the steps of: winding the anode current collector around a can roll having a curvature; vapor-phase growth of a film containing silicon and / or silicon monoxide having a multilayer structure consisting of two or more layers on the anode current collector while running the anode current collector on the can roll; spraying an oxygen-containing gas onto the film containing silicon and / or silicon monoxide to form a multilayer structure layer containing silicon dioxide on the upper part of each layer; inserting and desorbing lithium into and from the layer of the multilayer structure to form the anode active material layer; forming the ion conduction layer having lithium ion conductivity on a surface of the anode active material layer; and forming the solid electrolyte layer adjacent to the ion conduction layer.

[0053] The method for producing an anode body of the present invention makes it possible to produce an anode body that can maintain battery characteristics while significantly increasing capacity.

[0054] In this case, it is preferable that the method further comprises the steps of: in the step of forming layers of the multilayer structure, layers of the multilayer structure are formed, each layer containing a silicon oxide including silicon dioxide; and in the vapor phase growth step, a negative electrode active material layer containing silicon oxide is vapor-grown on the negative electrode current collector; the negative electrode active material layer containing silicon oxide is immersed in a solution containing lithium; and the silicon oxide is modified by an electrochemical method, thereby producing a compound containing lithium, silicon, and oxygen, and forming the ion conductive layer.

[0055] Such a method for producing an anode body allows lithium to be inserted by an electrochemical method, so that an anode body capable of significantly increasing capacity while maintaining battery characteristics can be produced more reliably. Effect of the Invention

[0056] As described above, the anode body of the present invention can provide high initial efficiency, high capacity, and high cycle characteristics when used as a component of a secondary battery. Furthermore, the method for producing the anode body of the present invention can produce an anode body that has high capacity and good initial charge / discharge characteristics when used as an anode body constituting a secondary battery while providing good cycle characteristics. [Brief description of the drawings]

[0057] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a negative electrode body of the present invention. [Diagram 2] FIG. 1 is a schematic exploded view showing an example of the configuration of a lithium ion secondary battery including a negative electrode body of the present invention. [Diagram 3] 2 is a SEM image of the surface of a negative electrode active material layer of one example of the negative electrode body of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0058] As mentioned above, one method to increase the battery capacity of lithium-ion secondary batteries is to use a negative electrode that uses silicon oxide as the main material. Lithium-ion secondary batteries using silicon oxide are expected to have initial charge / discharge characteristics that are close to those of lithium-ion secondary batteries using carbon-based active materials. In addition, a significant increase in capacity can be expected by using Li-doped SiO, which can improve the initial charge / discharge characteristics, but further improvement in capacity is required when considering vehicle applications.

[0059] Therefore, the inventors have conducted extensive research in order to obtain a negative electrode that, when used as a negative electrode for a secondary battery, can obtain high cycle characteristics while improving initial charge / discharge characteristics and increasing battery capacity, and have arrived at the present invention.

[0060] That is, one aspect of the present invention is an anode body having an anode including an anode current collector having a roughened surface, an anode active material layer provided on the anode current collector, and an ion conductive layer having lithium ion conductivity on the surface of the anode active material layer, and having a solid electrolyte layer adjacent to the ion conductive layer, wherein the anode active material layer includes anode active material particles having a compound containing lithium, silicon, and oxygen, and the anode active material particles are SiO x1 Li y1 where the value of x1 is greater than 0.8 and less than or equal to 1.2, and the value of y1 is greater than or equal to 0.5 and less than or equal to 3.4. Thus, the negative electrode body of the present invention has a negative electrode and a solid electrolyte layer.

[0061] Another aspect of the present invention is a method for producing the above-mentioned anode body of the present invention, comprising the steps of: winding the anode current collector around a can roll having a curvature; vapor-phase growing a film containing silicon and / or silicon monoxide having a multilayer structure consisting of two or more layers on the anode current collector while running the anode current collector on the can roll; spraying an oxygen-containing gas onto the film containing silicon and / or silicon monoxide to form a multilayer structure layer containing silicon dioxide on the upper part of each layer; inserting and desorbing lithium into and from the layer of the multilayer structure to form the anode active material layer; forming the ion conduction layer having lithium ion conductivity on the surface of the anode active material layer; and forming the solid electrolyte layer adjacent to the ion conduction layer.

[0062] The present invention will be described in detail below, but the present invention is not limited thereto.

[0063] <Negative electrode> First, the configuration of the negative electrode body of the present invention will be described with reference to the drawings.

[0064] FIG. 1 shows a schematic cross-sectional view of an example of the anode body of the present invention. As shown in FIG. 1, the anode body 10 has a configuration including an anode current collector 11 and an anode active material layer 12 provided on a surface 11a of the anode current collector 11. The anode active material layer 12 may be provided on both surfaces 11a of the anode current collector 11 as shown in FIG. 1, or may be provided on only one surface 11a. Furthermore, the anode body 10 includes an ion conductive layer 14 having lithium ion conductivity on the surface of the anode active material layer 12. That is, the structure of the anode includes the anode current collector 11, the anode active material layer 12, and the ion conductive layer 14. The anode body 10 further includes a solid electrolyte layer 16 adjacent to the ion conductive layer 14.

[0065] The surface 11a of the negative electrode current collector 11 is a roughened surface. That is, the negative electrode active material layer 12 is provided on the roughened surface 11a of the negative electrode current collector 11.

[0066] The negative electrode current collector 11 and the negative electrode active material layer 12 will be described below.

[0067] [Negative electrode current collector] The negative electrode current collector 11 is made of a material having excellent electrical conductivity and excellent mechanical strength. Examples of the conductive material that can be used for the negative electrode current collector 11 include copper (Cu) and nickel (Ni). It is preferable that this conductive material is a material that does not form an intermetallic compound with lithium (Li).

[0068] The negative electrode current collector 11 preferably contains carbon (C) and / or sulfur (S) in addition to the main elements. This is because the physical strength of the negative electrode current collector is improved. In particular, when the current collector has an active material layer that expands during charging, if the current collector contains the above elements, this has the effect of suppressing deformation of the electrode including the current collector. The contents of the above contained elements are not particularly limited, but are preferably 100 mass ppm or more each. This is because a higher deformation suppression effect can be obtained. Such a deformation suppression effect can further improve cycle characteristics.

[0069] Moreover, the surface 11a of the negative electrode current collector 11 must be roughened, and preferably the ten-point average roughness Rz of the surface is 1.5 μm or more and 5.0 μm or less. If the negative electrode body 10 includes the negative electrode current collector 11 having the surface 11a with such a desirable average roughness Rz, not only can the negative electrode active material layer 12 be supported more stably, but also the density of the negative electrode active material particles in the negative electrode active material layer 12 can be made appropriate, and as a result, better battery characteristics can be exhibited. The roughened negative electrode current collector 11 is, for example, a metal foil that has been electrolytically treated, embossed, or chemically etched.

[0070] [Negative electrode active material layer] The negative electrode active material layer 12 of the negative electrode body 10 of the present invention contains negative electrode active material particles having a compound containing lithium, silicon, and oxygen (silicon compound particles). That is, the layer 12 contains silicon compound particles containing lithium and oxygen, and is provided on the negative electrode current collector 11. It can be said that the negative electrode body 10 has a structure in which the negative electrode active material particles are directly supported on the roughened surface 11a of the negative electrode current collector 11 as part of its structure.

[0071] The negative electrode body 10 of the present invention contains negative electrode active material particles that are silicon compound particles, and therefore can improve battery capacity. Moreover, unlike a typical electrode, the negative electrode body 10 of the present invention can directly support the negative electrode active material layer 12 on the roughened surface 11a of the negative electrode current collector 11 without using a binder, a conductive assistant, or the like, and can reduce the area of ​​the electrode that is not involved in charging and discharging, and can also reduce excess voids, thereby significantly improving the energy density of the electrode.

[0072] In this manner, by using a negative electrode body 10 having a densely supported negative electrode active material layer 12, it is possible to increase the energy density of the battery in a way that is not possible with, for example, a powder electrode.

[0073] In the negative electrode active material layer 12, the negative electrode active material particles having a compound containing lithium, silicon, and oxygen can be adjacent to each other. As described above, an ion conductive layer 14 having lithium ion conductivity is formed on the surface of the negative electrode active material layer 12, and the ion conductive layer 14 is preferably made of at least one of Li carbonate, Li phosphate, Li fluoride, Al carbonate, Al phosphate, Al fluoride, a compound having a silyl group, and a carbonized material containing a polycyclic aromatic hydrocarbon. Examples of the carbonized material include carbonized materials whose main component is an aromatic compound, and in particular, carbonized materials whose main component is a polycyclic aromatic hydrocarbon are preferable. The coating that becomes the ion conductive layer 14 plays a role as a protective layer that protects the interface between the negative electrode active material layer 12 and the solid electrolyte layer 16. Due to the presence of such a coating, the negative electrode body 10 of the present invention can exhibit excellent cycle characteristics.

[0074] The silyl group of the compound having the silyl group includes a silyl group having an organic group such as an alkyl group. In this case, a silyl group having an organic group having 1 to 5 carbon atoms is preferable. More preferably, the silyl group has an alkyl group having 1 to 5 carbon atoms. In this case, the alkyl group is preferably a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a tertiary butyl group, or an isobutyl group. Examples of the silyl group having such an alkyl group include trialkylsilyl groups such as a trimethylsilyl group and a triethylsilyl group. In this case, the three alkyls may be the same as described above or may be different. The organic group having 1 to 5 carbon atoms may include an unsaturated bond. The alkyl group may also include a fluorine atom.

[0075] Furthermore, in the negative electrode body 10 of the present invention, the negative electrode active material particles are SiO x1 Li y1 The formula can be expressed by the formula: x1 is more than 0.8 and 1.2 or less, and y1 is 0.5 or more and 3.4 or less. If x1 is a value exceeding 0.8, the oxygen ratio is higher than that of silicon alone, and the cycle characteristics are good. It is more preferable that x1 is 0.9 or more. If x1 is 1.2 or less, the resistance of the silicon oxide does not become too high, and therefore it is preferable. Among these, SiO x1 Li y1 The value of x1 is preferably close to 1, because this provides high cycle characteristics. The composition of the silicon compound in the present invention does not necessarily mean 100% purity, and may contain a small amount of impurity elements. If the value of y1 is 0.5 or more, the irreversible component of SiO generated during the initial charge and discharge can be fixed in advance, and the energy density of the electrode can be significantly improved. If the value of y1 is 3.4 or less, the negative electrode active material particles are stable against oxygen and moisture, so that a battery with a higher capacity can be assembled.

[0076] In other words, the negative electrode body 10 of the present invention can significantly increase the capacity while maintaining the battery characteristics.

[0077] On the other hand, if the value of x1 is 0.8 or less, the capacitance increases, but the Si 0+ The area that reacts with the electrolyte increases, deteriorating the cycle characteristics. Also, if the value of x1 exceeds 1.2, it becomes a load substance, which also deteriorates the battery characteristics. It is desirable for the value of x1 to be as close to 1 as possible.

[0078] In the negative electrode body 10 of the present invention, the negative electrode active material layer 12 preferably has a multilayer structure consisting of two or more layers. If the negative electrode body 10 has a negative electrode active material layer 12 with a multilayer structure, the expansion and contraction of the negative electrode active material layer 12 can be alleviated, and therefore the capacity retention rate can be improved, which is more preferable.

[0079] As described below, when manufacturing the anode body 10 of the present invention, Li is introduced into the anode active material layer 12, and in order to introduce Li more smoothly, it is preferable to form the anode active material layer 12 into a multilayer structure consisting of two or more layers at the timing of forming the anode active material layer 12. The anode active material layer 12 having a multilayer structure consisting of two or more layers can realize smooth insertion of Li while suppressing decomposition of the electrolyte.

[0080] When the negative electrode active material layer 12 has a multi-layer structure, each layer of the multi-layer structure preferably has a layer made of a high-value silicon compound containing at least one of lithium and oxygen on the surface. By having a layer made of a silicon compound on the surface, expansion and contraction of the negative electrode active material layer 12 due to charging and discharging can be mitigated, and a stable negative electrode active material layer 12 can be maintained.

[0081] Furthermore, when the above-mentioned negative electrode active material particles are defined as primary particles, the negative electrode active material layer 12 forms secondary particles which are aggregates of the primary particles, and it is preferable that the secondary particles have a morphology in which they are separated from each other in the in-plane direction.

[0082] In the manufacturing method of the anode body 10 of the present invention described later, the anode active material particles grow in a vapor phase due to the roughened portion of the surface 11a of the anode current collector 11. When these are defined as primary particles, it is preferable that they form secondary particles which are aggregates of the primary particles. This can be controlled by changing the roughened state of the surface 11a of the anode current collector 11; for example, if the roughened interval is wide, the secondary particle group becomes small. On the other hand, if the roughened interval is narrow and the primary particles are too densely packed, it becomes difficult to generate secondary particles during charging and discharging.

[0083] It is desirable that these secondary particles are separated from each other in the in-plane direction. By performing charge and discharge in this state, a stable negative electrode active material layer 12 can be maintained.

[0084] With this configuration, the anode body 10 of the present invention can suppress the change in thickness of the anode active material layer 12 due to charging and discharging. In particular, the thickness T1 of the anode active material layer 12 before charging and the thickness T2 when fully charged can be in the relationship T2 / T1≦1.4. With this configuration, the expansion during full charging can be suppressed to a state close to that of graphite.

[0085] In the anode body 10 of the present invention, the number of primary particles forming the secondary particles of the anode active material particles in the anode active material layer 12 is preferably four or more on average. If this number is four or more, the surface area of ​​the anode active material layer becomes appropriate, and deterioration of the material due to charging and discharging of the battery can be suppressed. In other words, if this number is four or more, stable battery characteristics can be exhibited while suppressing deterioration of the material. The average number of primary particles in the secondary particles can be measured by observation with a scanning electron microscope. FIG. 3 shows a surface SEM image of the anode active material layer 12 constituting the anode body 10 of the present invention.

[0086] In addition, the negative electrode active material layer 12 preferably contains at least one of Li4SiO4, Li2Si2O5, Li2SiO3, and Li6Si2O7. In addition to Li2SiO3, Li silicates such as Li4SiO4 and Li6Si2O7 are relatively more stable than other Li compounds, so silicon-based active materials containing these Li compounds can obtain more stable battery characteristics. These Li compounds can be obtained by selectively changing a part of the SiO2 component generated inside the silicon compound to a Li compound and modifying the silicon compound.

[0087] In the anode body 10 of the present invention, when the anode active material layer 12 has a multilayer structure, it is preferable that at least one of the layers constituting the multilayer has an ion-conducting layer (interlayer lithium ion-conducting layer) having lithium ion conductivity. In this way, the presence of an ion-conducting layer (interlayer lithium ion-conducting layer) between layers of the multilayer structure facilitates the movement of lithium between the layers, thereby improving the battery characteristics.

[0088] [Solid electrolyte layer] The solid electrolyte layer 16 shown in FIG. 1 is adjacent to the ion-conducting layer 14 on the outermost surface of the negative electrode active material.

[0089] The solid electrolyte constituting the solid electrolyte layer 16 is preferably either a sulfide-based solid electrolyte or an oxide-based solid electrolyte.

[0090] [Sulfide solid electrolyte] First, a case where the solid electrolyte layer 16 is made of a sulfide-based solid electrolyte will be described. A known sulfide-based solid electrolyte can be used as the sulfide-based solid electrolyte. The sulfide-based solid electrolyte may react with lithium released from the silicon-based active material to generate heat, but the negative electrode body of the present invention has an ion-conducting layer on the surface, which can suppress this reaction, and a safe battery that does not easily generate heat while maintaining high ion conductivity can be designed.

[0091] The sulfide-based solid electrolyte can have at least one of lithium, indium, sulfur, and phosphorus. Further, the sulfide-based solid electrolyte can have at least one of Li2S, P2S5, SiS2, LiI, LiBr, P2O5, Li3PO4, and GeS2. Examples of the sulfide-based solid electrolyte include Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Si2S-P2S5, Li2S-P2S5-LiI-LiBr, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5-GeS2, etc.

[0092] [Oxide-based solid electrolyte] Next, the case where the solid electrolyte layer 16 is made of an oxide-based solid electrolyte will be described. Since the oxide-based solid electrolyte is stable in air and easy to handle, a safe battery can be designed.

[0093] [Compound having a perovskite structure] The oxide-based solid electrolyte that can be used in the present invention can have a perovskite structure. The compound having a perovskite structure has a composition formula represented by the general formula A X2 BO3 (where 0 < X2 < 1 is satisfied). In this compound having a perovskite structure, at least one of La and Li is included in element A, and at least one of Mg, W, Nb, and Ti is included in element B. By including Li in element A, Li ion conductivity can be imparted. Further, it is preferable to include Mg and W as element B. This perovskite-type ion conductive oxide (solid electrolyte) has a basic composition formula (Li 3a ,La 2 / 3-a )(Mg b ,W 1-b)It may be represented by O3 (where 0 < a ≤ 1 / 3 and 0.4 ≤ b ≤ 0.6 are satisfied). At this time, the substitution amount a of Li is preferably 0.04 or more, more preferably in the range of 0.05 or more and 0.30 or less, and still more preferably in the range of 0.07 or more and 0.22 or less. In such a range, it is preferable because the Li ion conductivity can be further increased. Also, the blending amount b of Mg is preferably in the range of 0.48 or more and 0.52 or less, and the closer Mg and W are to an equal amount, the more preferable, and more preferably 0.5. This perovskite-type ion-conductive oxide has a basic composition formula (Li3a,La 2 / 3-a )(Mg 1 / 2 ,W 1 / 2 )O3 (where a is 1 / 6, 1 / 4, 1 / 3), and those represented thereby are more preferable. Although the structure of the basic composition formula (La 2 / 3 )(Mg 1 / 2 ,W 1 / 2 )O3 was shown, the perovskite-type ion-conductive oxide of the present disclosure has a structure in which a part of La is substituted with Li.

[0094] [Phosphate compound having a NASICON-type crystal structure] The oxide-based solid electrolyte that can be used in the present invention can have a NASICON-type phosphate compound. The phosphate compound having a NASICON-type crystal structure is not particularly limited as long as it is a NASICON-type phosphate compound. For example, it can have at least one of lithium, aluminum, germanium, zirconium, titanium, and calcium. Further, this NASICON-type phosphate compound is preferably a NASICON-type phosphate compound represented by the general formula (1) Li 1+x3 M1 x3 M2 2-x3 (PO4)3 (in formula (1), M1 is at least one selected from the group consisting of Al, Y, Ga, and In, M2 is at least one selected from the group consisting of Ti, Ge, and Zr, and x3 is 0 ≤ x3 ≤ 2).

[0095] The metal M1 is preferably at least one selected from the group consisting of Al, Y and Ga, and more preferably Al. The metal M2 is preferably at least one selected from the group consisting of Ge and Ti, and more preferably Ge. That is, the general formula (2) Li 1+x3 Al x3 Ge 2-x3 A Nasicon-type phosphate compound (LAGP) represented by (PO4)3 (wherein 0≦x3≦2 in formula (2)) is preferred. Among Nasicon-type phosphate compounds, the compound represented by formula (2) has high ionic conductivity.

[0096] The range of x3 is preferably 0.1≦x3≦1.9, and more preferably 0.3≦x3≦0.7. In particular, the solid electrolyte material is Li 1.5 Al 0.5 Ge 1.5 It is preferably (PO4)3.

[0097] [Compounds with garnet-type crystal structure] The oxide-based solid electrolyte that can be used in the present invention can be a solid electrolyte having a garnet-type crystal structure. The solid electrolyte having a garnet-type crystal structure preferably has at least one of lithium, lanthanum, calcium, zirconium, bismuth, aluminum, cerium, gallium, boron, and oxygen. The compound having a garnet-type crystal structure is preferably Li (7-3x4+y4-z4) M x4 La (3-y4) A' (y4) Zr (2-z4) T (z4) O 12 (The element M is one or more of Al and Ga, the element A' is one of Ca and Sr, and T is one of Nb and Ta, and 0≦x4≦0.18, 0≦y4≦0.18, and 0≦z4≦1.5 are satisfied.) In particular, the solid electrolyte having a garnet-type crystal structure is preferably one of the following compositions: Li 7-3x4+α La3Zr2Al x4 O 12-y4Li3BO3 (wherein 0≦x4<2, 1.1<(7-3x4+α) / (7-3x4)≦1.5, and 0.3≦y4≦2.0). When a compound having a garnet-type crystal structure has the above composition, it becomes a cubic crystal at room temperature, and therefore has the effect of having high ionic conductivity at room temperature. In addition, the compound having a garnet-type crystal structure according to the embodiment of the present invention has the composition formula: Li 7-3x4+α La3Zr2Al x4 O 12-y4 In Li3BO3, the stoichiometric ratio of Li is "Li 7-3x4 " has Li in excess of "α" compared to "Li3BO3", and is Li-excessive. In addition, in the above formula, 0≦x4<1 may be satisfied. In addition, "y4", which indicates the substance ratio of Li3BO3, may be satisfied in the range of 0.3≦y4≦1.5.

[0098] [Method of manufacturing negative electrode body] The method for producing the anode body of the present invention preferably includes the steps of winding the anode current collector around a can roll having a curvature, vapor-phase growth of a multilayered film containing silicon and / or silicon monoxide consisting of two or more layers on the anode current collector while running the anode current collector on the can roll, spraying an oxygen-containing gas onto the silicon and / or silicon monoxide-containing film to form a multilayered layer containing silicon dioxide on the top of each layer, inserting and desorbing lithium into and from the multilayered layer to form the anode active material layer, forming the ion-conducting layer having lithium ion conductivity on the surface of the anode active material layer, and forming the solid electrolyte layer adjacent to the ion-conducting layer. Such a method for producing the anode body of the present invention can produce an anode body that can significantly increase capacity while maintaining battery characteristics.

[0099] In this case, it is preferable to include a step of forming the multilayered layer, in which each layer contains silicon oxide including silicon dioxide, in the step of forming the multilayered layer, and a step of vapor-growth the silicon oxide-containing anode active material layer on the anode current collector, immersing the silicon oxide-containing anode active material layer in a solution containing lithium, and modifying the silicon oxide by an electrochemical method to produce a compound containing lithium, silicon, and oxygen, and to form the ion-conducting layer. With such a method of manufacturing an anode body, lithium can be inserted by an electrochemical method, so that an anode body capable of significantly increasing capacity while maintaining battery characteristics can be more reliably manufactured.

[0100] The negative electrode body of the present invention can be manufactured by the above-described method for manufacturing the negative electrode body of the present invention. However, the method for manufacturing the negative electrode body of the present invention is not limited to the manufacturing method of the present invention described here.

[0101] Hereinafter, one example of a method for producing an anode body of the present invention will be specifically described, but the method for producing an anode body of the present invention is not limited to the example described below.

[0102] First, a film containing silicon and / or silicon monoxide having a multilayer structure consisting of two or more layers is produced. Here, a film containing silicon and / or silicon monoxide having a multilayer structure is vapor-phase grown on a negative electrode current collector. The film containing silicon can contain silicon particles. The film containing silicon monoxide can contain silicon monoxide particles, which are silicon compound (silicon oxide) particles containing oxygen. Therefore, the film containing silicon and / or silicon monoxide having a multilayer structure consisting of two or more layers can contain silicon-containing particles.

[0103] This multilayered film containing silicon and / or silicon monoxide can be formed by depositing, for example, a silicon vapor flow or silicon oxide gas on a negative electrode current collector having a roughened surface, for example, a roughened foil (for example, a roughened copper foil) having a surface ten-point average roughness Rz of 1.5 μm to 5.0 μm (for example, 2.5 μm). In the method for producing a negative electrode body of the present invention, the negative electrode current collector is wound around a can roll having a curvature. The curvature (R) of the can roll is, for example, 4 m. -1 More than 20m -1 It is preferable that:

[0104] A specific example of a method for forming a multi-layered film containing silicon and / or silicon monoxide is as follows.

[0105] A silicon monoxide film can be formed, for example, by the following procedure. First, a raw material that generates silicon oxide gas is heated at a temperature of 1100°C or higher under reduced pressure to generate silicon oxide gas. At this time, a mixture of metal silicon powder and silicon dioxide powder can be used as the raw material. Considering the presence of oxygen on the surface of the metal silicon powder and trace amounts of oxygen in the reactor, it is desirable for the mixture molar ratio to be in the range of 0.9<metal silicon powder / silicon dioxide powder<1.2.

[0106] Silicon oxide can also be formed by vapor deposition using metal silicon and introducing oxygen gas to the deposited silicon, but in this case, the valence cannot be controlled, and as a result, a composite is formed in which silicon is separated into a zero-valent state and a tetravalent compound state. Similarly, it is possible to introduce a reducing gas (hydrogen) into silicon dioxide gas, but it is difficult to introduce sufficient hydrogen into steam that moves close to the speed of sound. As a result, in the method for producing the anode body of the present invention, it is preferable to use metal silicon and silicon dioxide powder as raw materials for the silicon monoxide film.

[0107] The silicon oxide gas generated as described above is deposited on the roughened portion of the surface of the negative electrode current collector, and becomes primary particles having a columnar structure.

[0108] Also, a silicon film can be formed by vapor deposition using, for example, metallic silicon.

[0109] When forming the silicon film and / or silicon monoxide film, the structure of the primary particles can also be changed by changing the roughened structure of the surface of the negative electrode current collector.

[0110] The solidification heat during deposition and the radiant heat from the heating unit promote the crystallization of the negative electrode active material layer. Therefore, in the method for producing the negative electrode body of the present invention, the negative electrode current collector is run on a can roll having a curvature, and the vapor phase growth can be performed without causing crystallization of Si while reducing the thermal load.

[0111] In particular, silicon oxide, unlike silicon, is sublimable, allowing for rapid deposition, and there is no need to worry about radiant heat from molten silicon, which is an issue with silicon films. Therefore, silicon oxide is suitable for forming active materials by vapor deposition.

[0112] In the method for producing a negative electrode of the present invention, multilayer film formation (for example, reciprocating multilayer film formation) is performed while the negative electrode current collector is running on a can roll having a curve, so that part of the surface of each layer is deposited at an angle, causing voids.

[0113] Deposition can also be performed on both roughened surfaces of the negative electrode current collector, for example, deposition can be performed on one roughened surface of the negative electrode current collector, then the negative electrode current collector can be turned over and deposition can be performed on the other roughened surface of the negative electrode current collector.

[0114] A gas containing oxygen is sprayed onto the film containing silicon and / or silicon monoxide thus formed, to form a multi-layer structure containing silicon dioxide on the top of each layer.

[0115] The oxygen-containing gas is not particularly limited as long as it contains oxygen, but may be, for example, nitrogen gas containing oxygen.

[0116] By blowing the oxygen-containing gas, oxygen can enter the voids in the upper part of each layer, and oxygen can be introduced into each layer. This also allows at least a part of the silicon and / or silicon monoxide to be converted to silicon dioxide in the upper part of each layer. In other words, by blowing the oxygen-containing gas, a multi-layer structure can be formed in which each layer contains silicon oxide including silicon dioxide.

[0117] Next, Li is doped (inserted) into the multilayer structure containing silicon dioxide on the top of each layer prepared as described above. This results in a negative electrode active material layer containing negative electrode active material particles containing silicon oxide particles with lithium inserted therein. In other words, this modifies the silicon oxide particles, and a Li compound is generated inside the silicon oxide particles.

[0118] [Modification by electrochemical methods] In the electrochemical modification, the negative electrode active material layer containing silicon oxide particles is first immersed in a liquid non-aqueous electrolyte (electrolyte) as the anode and lithium metal cathode, and lithium can be inserted by supplying a current. This electrolyte contains an electrolyte salt dissolved in a solvent and may contain other materials such as additives.

[0119] The solvent may be, for example, a non-aqueous solvent. Examples of non-aqueous solvents include ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane, and tetrahydrofuran. Among these, it is desirable to use at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. This is because better characteristics can be obtained. In this case, more advantageous characteristics can be obtained by combining a high-viscosity solvent such as ethylene carbonate or propylene carbonate with a low-viscosity solvent such as dimethyl carbonate, ethyl methyl carbonate, or diethyl carbonate. This is because the dissociation and ion mobility of the electrolyte salt are improved.

[0120] In particular, it is desirable that the solvent contains at least one of halogenated chain carbonates or halogenated cyclic carbonates. This allows a stable coating to be formed on the surface of the negative electrode active material during charging and discharging, particularly during charging. Here, the halogenated chain carbonate is a chain carbonate having a halogen as a constituent element (at least one hydrogen is substituted with a halogen). In addition, the halogenated cyclic carbonate is a cyclic carbonate having a halogen as a constituent element (i.e., at least one hydrogen is substituted with a halogen).

[0121] The type of halogen is not particularly limited, but fluorine is preferred because it forms a better coating than other halogens. Also, the more halogens there are, the more desirable they are because the resulting coating is more stable and the decomposition reaction of the electrolyte is reduced.

[0122] Examples of halogenated chain carbonates include fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, etc. Examples of halogenated cyclic carbonates include 4-fluoro-1,3-dioxolan-2-one, 4,5-difluoro-1,3-dioxolan-2-one, etc.

[0123] It is preferable that the solvent additive contains an unsaturated carbon-bonded cyclic carbonate. This is because a stable coating is formed on the surface of the negative electrode active material layer during charging and discharging, and the decomposition reaction of the electrolyte can be suppressed. Examples of the unsaturated carbon-bonded cyclic carbonate include vinylene carbonate and vinylethylene carbonate.

[0124] It is also preferable that the solvent additive contains sultone (cyclic sulfonic acid ester), because this improves the chemical stability of the battery. Examples of sultones include propane sultone and propene sultone.

[0125] Furthermore, it is preferable that the solvent contains an acid anhydride, because this improves the chemical stability of the electrolyte. As the acid anhydride, for example, propane disulfonic acid anhydride can be mentioned.

[0126] The electrolyte salt may include at least one of light metal salts such as lithium salts, for example. Examples of the lithium salt include lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4).

[0127] The content of the electrolyte salt is preferably 0.5 mol / kg or more and 2.5 mol / kg or less relative to the solvent, because high ionic conductivity can be obtained.

[0128] After lithium insertion, lithium can be desorbed by supplying a current to the negative electrode active material layer containing silicon oxide particles as the cathode and the lithium metal anode. At this time, the state of the filled coating (composite compound) can be controlled by adjusting the temperature of the solvent, the type and concentration of the polyphenylene compound or polycyclic aromatic compound contained in the solvent, and the concentration of the polycyclic aromatic compound complexed with Li. The obtained silicon active material particles may be heat-treated in an inert gas atmosphere. The Li compound can be stabilized by heat treatment.

[0129] The resulting complex compound may contain multiple types of compounds.

[0130] [Formation of a coating with lithium ion conductivity] A coating (ion conductive layer) with lithium ion conductivity is formed on the negative electrode active material layer obtained by electrochemical modification. A lithium carbonate coating can be formed on the surface and between the layers by spraying carbon dioxide gas onto the negative electrode active material layer. The coating can also be formed by adding aluminum phosphate to the electrolyte when lithium is inserted and extracted. A coating made of Li3PO4, LiF, and Li2CO3 can be formed on the surface by not removing the electrolyte salt after lithium insertion and extraction.

[0131] The compound having a silyl group is preferably formed by alkylsilazane treatment. In this way, the treatment occurs on the surface of the material, and a layer containing a compound having a silyl group can be efficiently formed. More specifically, for example, a layer containing a compound having a silyl group can be formed by the following procedure. It is considered that OH groups exist on the surface of the negative electrode active material layer, and the OH groups react with the decomposition product of the alkylsilazane, and trialkylsilyl groups are introduced on the surface of the silicon compound particles or the carbon material.

[0132] First, dehydrated toluene, a negative electrode active material with a mass equivalent to one-fourth of the dehydrated toluene, and HMDS (hexamethyldisilazane) equivalent to 3 mass% of the negative electrode active material are put into a container and left to stand for one hour. After that, the negative electrode active material layer is dried to form a coating of a compound having a silyl group.

[0133] The carbonized material whose main component is an aromatic compound (polycyclic aromatic hydrocarbon) is preferably formed by coal tar pitch treatment. Specifically, a coating can be formed by applying coal tar or pitch to the negative electrode active material layer and heat treating it. The coal tar or pitch is thermally decomposed to form a carbonized material which is an aromatic compound (polycyclic aromatic hydrocarbon), and a coating is formed on the negative electrode active material layer. The thermal decomposition temperature is not particularly limited.

[0134] [Formation of solid electrolyte layer] After forming the ion-conducting layer, a solid electrolyte layer is formed adjacent to the ion-conducting layer, which can be performed by, for example, applying pressure to the solid electrolyte layer after disposing the solid electrolyte layer adjacent to the ion-conducting layer.

[0135] In this manner, the negative electrode body of the present invention can be produced.

[0136] <Lithium-ion secondary battery> The negative electrode body of the present invention can be used in the negative electrode body of an all-solid-state battery, for example, a lithium-ion secondary battery.

[0137] Next, an example of an all-solid-state battery in which the negative electrode body of the present invention can be used will be described.

[0138] The structure of the lithium secondary battery is not particularly limited, but may be, for example, the structure shown in FIG. 2. FIG. 2 is an explanatory diagram showing an example of the structure of an all-solid-state lithium secondary battery 20. This all-solid-state lithium secondary battery has the above-mentioned solid electrolyte layer 16, a positive electrode active material layer 21 formed on one surface of the solid electrolyte layer 16 and containing a positive electrode active material that absorbs and releases lithium, and a negative electrode active material layer 12 formed on the other surface of the solid electrolyte layer 16 and containing a negative electrode active material that absorbs and releases lithium. A positive electrode current collector 22 is formed on the surface of the positive electrode active material layer 21, and a negative electrode current collector 11 is formed on the surface of the negative electrode active material layer 12. The solid electrolyte layer 16 and the negative electrode active material layer 12 may form a composite negative electrode body 10. EXAMPLES

[0139] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.

[0140] Comparative Example 1 To serve as a reference for the examples, the following particulate coated active material was first produced.

[0141] (Preparation of negative electrode structure) A coated active material was prepared using a particle composite device (NOB-MINI, manufactured by Hosokawa Micron Corporation). First, a negative electrode active material (a powder of Li-doped SiO coated with carbon (referred to as "Li-SiO-C")), a sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5), average particle size 0.5 μm), and a conductive assistant (spherical carbon, specific surface area 93 m2 / g) were added to the treatment container of the device in the ratios shown in Table 1 below so that the total amount was 30 g. Next, the gap between the rotating blades (blades) of the compression shear rotor and the inner wall of the treatment container was set to 1 mm, the pressure was 100 Pa, the blade circumferential speed was 26.4 m / s, and the treatment time was 12.5 minutes, and a compression shear treatment was performed to obtain a coated active material.

[0142] Li-SiO-C was prepared as follows. First, silicon and silicon dioxide were mixed as raw materials, vaporized at 1300℃, and then deposited on a deposition substrate and quenched to produce SiO blocks. The SiO blocks were crushed to a median diameter of 7μm, and then doped with Li using an oxidation-reduction method. After doping, samples were prepared by heat treatment to stabilize the Li silicate.

[0143] The obtained active material, sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5), average particle size 0.5 μm), conductive additive (VGCF), and binder (PVdF) were prepared, and these were weighed out so that the weight ratio of negative electrode active material: sulfide solid electrolyte: conductive additive: binder = 53:41:4:2, and mixed with a dispersion medium (heptane). The obtained mixture was dispersed with an ultrasonic homogenizer (UH-50, manufactured by SMT Co., Ltd.) to obtain a negative electrode slurry.

[0144] The obtained negative electrode slurry was applied onto a negative electrode current collector (copper foil) and dried at 100°C for 30 minutes. 2 The negative electrode structure having the negative electrode layer and the negative electrode current collector was obtained by punching out the negative electrode layer into a size of 1 cm. 2 A sulfide solid electrolyte (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5), average particle size 0.5μm) was placed in a cylindrical plastic tube and subjected to 4ton / cm 2 A solid electrolyte layer (thickness 15 μm) was obtained by pressing with a pressure of 4 ton / cm. The obtained solid electrolyte layer and the negative electrode structure were arranged. 2 The negative electrode layer was pressed at 46 μm in thickness.

[0145] (Preparation of positive electrode structure) Cathode active material (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3The positive electrode active material (10LiI-15LiBr-75 (0.75Li2S-0.25P2S5), average particle size 0.5μm), conductive additive (VGCF), and binder (PVdF) were prepared and weighed out to a weight ratio of positive electrode active material:sulfide solid electrolyte:conductive additive:binder = 85:13:1:1, and mixed with a dispersion medium (heptane). The resulting mixture was dispersed with an ultrasonic homogenizer (UH-50, manufactured by SMT Co., Ltd.) to obtain a positive electrode slurry.

[0146] The obtained positive electrode slurry was applied onto a positive electrode current collector (aluminum foil) and dried at 100°C for 30 minutes. 2 A positive electrode structure having a positive electrode layer and a positive electrode current collector was obtained by punching out the positive electrode layer to a size of 50 μm. The thickness of the positive electrode layer was 50 μm.

[0147] (Preparation of evaluation battery) The positive and negative electrode structures are arranged and subjected to 4 ton / cm 2 Then, a stainless steel rod was inserted into each of the positive and negative electrodes, and the electrodes were restrained at 5 MPa to obtain an all-solid-state battery (battery for evaluation).

[0148] Comparative Example 2 The negative electrode body of the electrode of Comparative Example 2 was produced by the following procedure: A surface-roughened copper foil having a ten-point average roughness (roughness) Rz of 2.5 μm was used as the negative electrode current collector.

[0149] [Preparation of negative electrode active material layer] Gravel-like silicon metal was placed in a carbon crucible, and the silicon was melted and vaporized under vacuum using an electron gun. Using a movable device, a surface-roughened copper foil (to become the negative electrode current collector) was placed on a roll, and five layers of silicon film were formed on the surface-roughened copper foil while the roll was moving.

[0150] [Lithium insertion and extraction] Ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed to prepare a non-aqueous solvent, and then an electrolyte salt (lithium hexafluorophosphate: LiPF6) was dissolved in the non-aqueous solvent to prepare an electrolyte solution (non-aqueous electrolyte). In this case, the composition of the solvent was EC:DMC=30:70 in volume ratio, and the content of the electrolyte salt was 1 mol / kg relative to the solvent. The obtained negative electrode active material layer was modified by inserting and desorbing lithium into the silicon compound particles by an electrochemical method using this electrolyte. The lithium insertion was completed when the potential difference between the anode and the cathode became zero. The lithium desorption was completed when the potential difference between the anode and the cathode became 1.2 V. The negative electrode active material layer obtained after the completion of lithium desorption was washed with dimethyl carbonate non-aqueous solvent to remove the electrolyte salt.

[0151] [Formation of surface coating (ion conductive layer)] By spraying carbon dioxide gas onto the negative electrode active material layer obtained by electrochemical modification, a lithium carbonate coating (ion conductive layer) was formed on the surface and between the layers (between each layer of the multilayer structure).

[0152] The obtained negative electrode structure and the solid electrolyte layer were placed adjacent to each other, and 4 ton / cm 2 The negative electrode body was obtained by pressing with a pressure of 1000.

[0153] Comparative Example 3 In Comparative Example 3, metal silicon and silicon dioxide were placed in a carbon crucible and heated for 10 -2 The vapor was taken out by heating at 1200° C. in an atmosphere with a vacuum degree of 100 Pa. The vapor was directly supported on the roughened copper foil as in Comparative Example 2, and five layers were formed.

[0154] In Comparative Example 3, the roughened copper foil, the negative electrode active material layer containing silicon oxide and the solid electrolyte layer provided on the roughened copper foil were disposed adjacent to each other, and a pressure of 4 ton / cm was applied. 2 The negative electrode body was obtained by pressing with a pressure of 1000.

[0155] (Comparative Examples 4 and 5 and Example 1) In Comparative Examples 4 and 5 and Example 1, anode bodies were produced in the same manner as in Comparative Example 2, except that water vapor was introduced into the silicon vapor flow during film formation to attempt forced oxidation.

[0156] Example 2 In Example 2, a roughened copper foil was obtained in the same manner as in Comparative Example 3, and a negative electrode active material layer containing silicon oxide was provided on the roughened copper foil. Lithium was inserted and removed, and a surface coating (ion conductive layer) was formed in the same manner as in Comparative Example 2. The obtained negative electrode structure and a solid electrolyte layer were disposed adjacent to each other, and a 4 ton / cm 2 The negative electrode body was obtained by pressing with a pressure of 1000.

[0157] Comparative Example 6 In Comparative Example 6, a negative electrode body was produced in the same manner as in Example 2, except that no surface coating (ion conductive layer) was formed.

[0158] (Examples 3 and 4 and Comparative Example 7) In Examples 3 and 4 and Comparative Example 7, the SiO x1 Li y1 A negative electrode body was produced in the same manner as in Example 2, except that the film formation rate was adjusted so that the value of x1 became the value shown in Table 1, and hydrogen or oxygen was blown into the steam as necessary to form the film.

[0159] (Examples 5 and 6) In Examples 5 and 6, the negative electrode bodies were produced in the same manner as in Example 2, except that the film formation rate was controlled to form one layer and 20 layers, respectively, in the formation of the negative electrode active material layer.

[0160] Example 7 In Example 7, a negative electrode body was produced in the same manner as in Example 2, except that the roughness Rz of the surface-roughened copper foil was set to 0.5.

[0161] (Examples 8 to 10) In Examples 8 to 10, each negative electrode body was produced in the same manner as in Example 2, except that the thickness (T1) before battery charging and the thickness (T2) at full charge were adjusted to vary by changing the charge depth when lithium was inserted. The charge depth before charging was defined as 0%, and the amount of Li inserted when the potential difference between the anode and cathode became zero was defined as 100%.

[0162] (Examples 11 to 14) In Example 11, a negative electrode body was prepared in the same manner as in Example 2, except that aluminum phosphate was added to the electrolyte during the insertion and desorption of lithium, and carbon dioxide gas was not sprayed. In Example 12, a negative electrode body having a negative electrode active material layer on the surface of which a coating (ion conductive layer) made of Li3PO4, LiF, and Li2CO3 was present was prepared in the same manner as in Example 2, except that the electrolyte salt was not removed after the insertion and desorption of lithium. In Example 13, a negative electrode body was prepared in the same manner as in Example 2, except that the negative electrode active material layer obtained after the insertion and desorption of lithium was treated with alkylsilazane. In Example 14, a negative electrode body was prepared in the same manner as in Example 2, except that the negative electrode active material layer obtained after the insertion and desorption of lithium was washed with a nonaqueous solvent of dimethyl carbonate containing 3 vol% of tar, the electrolyte salt was removed, and the layer was heat-treated.

[0163] Example 15 In Example 15, a negative electrode body was produced in the same manner as in Example 2, except that the carbon dioxide gas to be sprayed onto the negative electrode active material layer obtained by the electrochemical modification was mixed with Ar and diluted to a concentration of 1.0 vol %, thereby forming a lithium carbonate coating (ion conductive layer) only on the surface.

[0164] (Examples 16 to 18) In Examples 16 to 18, negative electrode bodies were produced in the same manner as in Example 2, except that the average number of primary particles in the secondary particles was adjusted by setting the roughness Rz of the surface-roughened copper foil to 1.0, 1.5, and 2.5, respectively.

[0165] (Example 19) In Example 19, the solid electrolyte adjacent to the ion conductive layer on the outermost surface of the negative electrode active material is Li 0.5La 0.5 Mg 0.5 W 0.5 A negative electrode body was produced in the same manner as in Example 2, except that O3 was used.

[0166] [Preparation of compounds with perovskite structure] Basic composition formula Li 0.5 La 0.5 Mg 0.5 W 0.5 Li2CO3 (Kojundo Chemical), La(OH)3 (Kojundo Chemical), MgO (Kojundo Chemical), and WO3 (Kojundo Chemical) were weighed out so that the powder was 03.03. Next, a ZrO2 ball mill pot and beads (3mmf) were prepared, and the weighed powder was put in, and ethanol was put in as a solvent. The powder was stirred at 300 rpm for 3 minutes and then rested for 2 minutes, and the grinding process was repeated 20 times. The contents were poured into a SUS (stainless steel) tray and dried in a dryer at 90°C for 2 hours. The powder was collected by sieving (#500 mesh). Next, the obtained powder was placed in an alumina crucible and heated in the air at 900°C for 10 hours, and the above-mentioned grinding process was performed. Next, the obtained powder was pressed at 10 MPa in a mold molding machine and molded into a pellet-shaped molded body. This molded body was sintered at 1100°C for 12 hours.

[0167] (Example 20) In Example 20, the negative electrode body was prepared in the same manner as in Example 2, except that the solid electrolyte adjacent to the ion-conducting layer on the outermost surface of the negative electrode active material was changed to Li3In2(PO4)3, a Nasicon-type phosphate compound.

[0168] [Preparation of Nasicon-type phosphate compounds] In was used as the In-containing active material, and glassy Li was used as the amorphous phosphate compound. 1.5 Al 0.5 Ge 1.5 An intermediate body is prepared by using (PO4)3(LAGP) in which In and LAGP are in contact with each other. The intermediate body is then fired at a predetermined temperature to react In and LAGP, thereby obtaining a sintered body for a battery containing an active material having a Li3In2(PO4)3 crystal phase.

[0169] Example 21 In Example 21, the solid electrolyte adjacent to the ion-conducting layer on the outermost surface of the negative electrode active material is Li 6.8 (La 2.95 Ca 0.05 )(Zr 1.75 Nb 0.25 )O 12 A negative electrode body was produced in the same manner as in Example 2, except that the electrolyte was changed to (LLZ-CN).

[0170] [Preparation of compounds with garnet-type crystal structure] The starting materials used were LiOH(H2O), La(OH)3, Ca(OH)2, ZrO2, and Nb2O5. The starting materials were weighed to obtain the stoichiometric ratio, mixed, and pulverized. Mixing and pulverization were performed in ethanol using zirconia balls in a planetary ball mill (300 rpm) for 1 hour. Then, pre-sintering (700°C, 48 h) was performed. After pre-sintering, LiOH(H2O) was added in excess to the powder so that the Li content in the composition was 10 at% in order to compensate for the Li deficiency caused by sintering. Then, mixing and pulverization were performed again under the same conditions. Then, pre-sintering (700°C, 10 h) was performed again. The powder that had been pre-sintered twice was identified by XRD to identify the crystal phase, and it was confirmed that no unreacted raw materials remained. Then, the LLZ-CN powder was immersed in water to exchange Li for H. The immersion conditions were 4 g of LLZ-CN to 50 mg of water, and the material was left to stand at room temperature (around 25°C) for 30 minutes to exchange Li and H. Analysis of the composition after the Li and H exchange under these conditions revealed the following: (Li 5.6 ,H 1.2 )(La 2.95 ,Ca 0.05 )(Zr 1.75 ,Nb 0.25 )O 12(LLZ-HCN). Here, the amount of H was identified as follows. First, the powder after H substitution was subjected to TG·DTA-MASS measurement, and the temperature range in which HO (molecular weight 18) evaporated from the sample was determined by the MASS measurement, and the weight loss in that temperature range was quantified at Tg. The atomic weight of the amount of H contained in LLZ-HCN was calculated from the mass and molecular weight of LLZ-CN and the mass and molecular weight of evaporated water.

[0171] [Evaluation of discharge capacity and cycle characteristics] The prepared evaluation battery was placed in a thermostatic chamber at 25°C and discharged until the final potential reached 2.0 V (vs. Li / Li + ), charge end potential 4.8V (vs.Li / Li + ), CC charging and discharging was repeated at a current density of 0.1 C. The first discharge capacity was taken as the reference (100%), and the retention rate (%) of the discharge capacity after 100 cycles was calculated.

[0172] [Table 1] [Table 2]

[0173] [result] The above Tables 1 and 2 show the results of the capacity retention rate and discharge capacity up to 100 cycles.

[0174] As is clear from Tables 1 and 2, the negative electrode bodies of Examples 1 to 21 all maintained a capacity retention rate of 80% after 100 cycles, while providing battery characteristics of a discharge capacity of 240 mAh / g.

[0175] On the other hand, the negative electrode body of Comparative Example 1, which was made using powdered Li-SiO, had a lower discharge capacity than the negative electrode bodies of Examples 1 to 20. This is believed to be because the negative electrode body of Comparative Example 1 used powder instead of vapor deposition, and therefore contained a binder that is not involved in charge and discharge, and further had many excess voids.

[0176] Moreover, the negative electrode body of Comparative Example 2 was significantly inferior in cycle characteristics to Examples 1-21.

[0177] In Comparative Example 3, both the cycle characteristics and the discharge capacity were significantly lower than those in Examples 1 to 21. This is believed to be because Li was not inserted into the silicon oxide.

[0178] Silicon oxide is produced from silicon and silicon dioxide, so it is difficult to increase or decrease the amount of oxygen. x1 Li y1 In the case of silicon oxide in which x1 is 0.7 (Comparative Example 4), the valence could not be controlled, and a significant amount of silicon element remained.

[0179] To achieve even lower oxygen levels, it is necessary not only to introduce hydrogen into the steam for active reduction, but also to significantly reduce the deposition rate.

[0180] The negative electrode bodies of Comparative Examples 4 and 5 were made of SiO x1 Li y1 When x1 was set to 0.7 and 0.8, the discharge capacity was lower than that of the negative electrodes of Examples 1 and 2. This is because the negative electrode bodies of Comparative Examples 4 and 5 had a SiO x1 Li y1 This is thought to be due to the fact that, because x1 was set to 0.7 and 0.8, the area over which zero-valent Si reacts with the electrolyte became too large, causing the conductive path to be broken during discharge.

[0181] On the other hand, when the amount of oxygen was increased, the deposition rate was also decreased and oxygen was blown directly into the vapor flow, but as the amount of oxygen increased, it became difficult to prepare a silicon oxide film.

[0182] The negative electrode body of Comparative Example 7 was made of SiO x1 Li y1 As a result of setting x1 to 1.3, the discharge capacity was lower than that of the negative electrode bodies of Examples 1 to 4. This is because the negative electrode body of Comparative Example 7 had a SiO x1 Li y1This is thought to be due to the fact that the amount of load material was too large because x1 was set to 1.3. Since there is a tendency for the discharge capacity to decrease as x is increased, it is preferable to set x1 to 1.2 or less.

[0183] The discharge capacity of the negative electrode body of Comparative Example 6 was reduced due to the absence of the ion-conductive layer on the outermost surface of the negative electrode active material layer. This is believed to be due to an increase in interfacial resistance with the solid electrolyte caused by the absence of the ion-conductive layer on the outermost surface of the negative electrode active material layer in the negative electrode body of Comparative Example 6.

[0184] The negative electrode bodies of Examples 1 to 4 have a lower SiO x1 Li y1 As a result of setting x1 to 0.9 to 1.2, the irreversible components of the negative electrode body are suppressed, and both the initial efficiency and the cycle characteristics can be improved.

[0185] In Example 5, the negative electrode active material layer is a single layer film, which reduces the interlayer resistance and improves the discharge capacity, but makes it difficult to alleviate the expansion and contraction during charging and discharging, resulting in a decrease in the capacity retention rate. A negative electrode body having a multilayer structure as in Examples 2 and 6 is more preferable because it can alleviate the expansion and contraction of the negative electrode active material layer in the negative electrode body and therefore improves the capacity retention rate.

[0186] It is considered that the capacity retention rate of Example 7 was decreased because secondary particles were not formed and the structure was such that it was difficult to alleviate the expansion and contraction of the negative electrode active material layer in the negative electrode body, as compared with Example 2. It is preferable that secondary particles are formed as in Example 2.

[0187] Examples 8 to 10 are examples aimed at finding optimal thicknesses (T1) of the negative electrode active material before charging and (T2) of the negative electrode active material after full charging.

[0188] It is believed that the smaller the T2 / T1 value, the more the expansion and contraction during charging and discharging is suppressed, and therefore the more the capacity retention rate can be improved.

[0189] It is believed that the presence of the coating (ion-conducting layer) shown in Examples 3 and 11 to 14 on the outermost layer of the negative electrode active material layer suppresses reactions with moisture and oxygen, suppresses deterioration of the material, and maintains excellent battery characteristics. Therefore, it is preferable to have such a coating (ion-conducting layer).

[0190] The negative electrode body of Example 15 has a lower discharge capacity than that of Example 3 due to the absence of an ion conductive layer between the negative electrode active material layers. Therefore, it is considered that the negative electrode body in which an ion conductive layer exists between the negative electrode active material layers as in Example 3 has improved ion conductivity and can maintain excellent battery characteristics. Therefore, it is preferable to have an ion conductive layer between the negative electrode active material layers.

[0191] Examples 16 to 18 are examples aimed at finding an optimal number of primary particles in secondary particles. It is believed that a large number of primary particles in secondary particles can alleviate the stress of expansion during charging and discharging, thereby improving the capacity retention rate.

[0192] Examples 19 to 21 are examples aimed at exploring the type of solid electrolyte adjacent to the ion-conducting layer. The negative electrode active materials of Examples 19 to 21 can exhibit excellent battery characteristics when combined with any solid electrolyte to form a negative electrode.

[0193] The present specification includes the following aspects. [1]: A negative electrode current collector having a roughened surface; a negative electrode active material layer provided on the negative electrode current collector; an ion conductive layer having lithium ion conductivity on the surface of the negative electrode active material layer; and a solid electrolyte layer adjacent to the ion conductive layer, The negative electrode active material layer includes negative electrode active material particles having a compound containing lithium, silicon, and oxygen, and the negative electrode active material particles are SiO x1 Li y1 wherein the value of x1 is greater than 0.8 and less than or equal to 1.2, and the value of y1 is greater than or equal to 0.5 and less than or equal to 3.4. [2]: the negative electrode active material layer has a multilayer structure consisting of two or more layers, When the negative electrode active material particles are defined as primary particles, the negative electrode active material layer forms secondary particles that are aggregates of the primary particles, The secondary particles are separated from each other in the in-plane direction, The negative electrode body of [1] above, wherein a thickness T1 of the negative electrode active material layer before charging and a thickness T2 of the negative electrode active material layer when fully charged satisfy the relationship T2 / T1≦1.4. [3]: The anode body according to the above [2], wherein the anode active material layer having a multilayer structure has an interlayer lithium ion conductive layer having lithium ion conductivity between at least one of the layers constituting the multilayer. [4]: The negative electrode body according to any one of the above [1] to [3], wherein the negative electrode active material layer contains at least one of Li4SiO4, Li2Si2O5, Li2SiO3, and Li6Si2O7. [5]: The negative electrode body according to any one of the above [1] to [4], wherein the ion-conducting layer having lithium ion conductivity comprises at least one of a carbonate of Li, a phosphate of Li, a fluoride of Li, a carbonate of Al, a phosphate of Al, a fluoride of Al, a compound having a silyl group, and a carbonized material containing a polycyclic aromatic hydrocarbon. [6]: The negative electrode element according to any one of the above [2] to [5], wherein the secondary particles of the negative electrode active material layer are composed of, on average, four or more primary particles. [7]: The negative electrode element according to any one of the above [1] to [6], wherein the solid electrolyte layer is made of a sulfide-based solid electrolyte. [8]: The negative electrode body according to [7] above, wherein the sulfide-based solid electrolyte contains at least one of lithium, indium, sulfur, and phosphorus. [9]: The negative electrode body according to [7] or [8] above, wherein the sulfide-based solid electrolyte contains at least one of Li2S, P2S5, SiS2, LiI, LiBr, P2O5, Li3PO4, and GeS2.

[10] : The negative electrode element according to any one of the above [1] to [6], wherein the solid electrolyte layer is made of an oxide-based solid electrolyte.

[11] : The oxide-based solid electrolyte is the negative electrode body of the above

[10] having a perovskite structure.

[12] : The oxide-based solid electrolyte is the negative electrode body of the above

[10] or

[11] having at least one of lanthanum, lithium, magnesium, tungsten, niobium, and titanium.

[13] : The oxide-based solid electrolyte has a composition formula of A x2 BO3 (0 < x2 < 1), the element A includes La and Li, and the element B includes Mg, W, Nb, and Ti. It is the negative electrode body of any of the above

[10] to

[12] .

[14] : The oxide-based solid electrolyte is the negative electrode body of the above

[10] having a NASICON-type phosphate compound.

[15] : The solid electrolyte having the NASICON-type phosphate compound is the negative electrode body of the above

[14] having at least one of lithium, aluminum, germanium, zirconium, titanium, and calcium.

[16] : The NASICON-type phosphate compound is Li (1+x3) M1 (x3) M2 (2-x3) (PO4)3, the element M1 includes at least one selected from the group consisting of Al, Y, Ga, and In, the element M2 includes at least one selected from the group consisting of Ti, Ge, and Zr, and x3 is 0 ≦ x3 ≦ 2. It is the negative electrode body of the above

[14] or

[15] .

[17] : The oxide-based solid electrolyte is the negative electrode body of the above

[10] having a garnet-type crystal structure.

[18] : The solid electrolyte having the garnet-type crystal structure is the negative electrode body of the above

[17] having at least one of lithium, lanthanum, calcium, zirconium, bismuth, aluminum, cerium, gallium, boron, and oxygen.

[19] : The solid electrolyte having the garnet-type crystal structure is Li (7-3x4+y4-z4) M x4 La (3-y4) A’ (y4) Zr (2-z4) T (z4) O 12The negative electrode body of the above

[17] or

[18] , wherein the element M is one or more of Al and Ga, the element A' is one of Ca and Sr, and T is one of Nb and Ta, and 0≦x4≦0.18, 0≦y4≦0.18, and 0≦z4≦1.5 are satisfied.

[20] : A method for producing a negative electrode body according to any one of [1] to

[19] above, A step of winding the negative electrode current collector around a can roll having a curvature; a vapor phase growth step of vapor-growing a film containing silicon and / or silicon monoxide having a multilayer structure consisting of two or more layers on the negative electrode current collector while the negative electrode current collector is running on the can roll; A step of blowing an oxygen-containing gas onto the silicon and / or silicon monoxide-containing film to form a multi-layer structure containing silicon dioxide on the top of each layer; forming the negative electrode active material layer by inserting and extracting lithium into and from the layers of the multilayer structure; forming an ion conductive layer having lithium ion conductivity on a surface of the negative electrode active material layer; forming the solid electrolyte layer adjacent to the ion conductive layer; A method for producing a negative electrode body comprising the steps of:

[21] : In the step of forming layers of the multilayer structure, the layers of the multilayer structure are formed such that each layer contains a silicon oxide including the silicon dioxide; In the vapor phase growth step, a negative electrode active material layer containing silicon oxide is vapor-grown on the negative electrode current collector; a step of immersing the negative electrode active material layer containing the silicon oxide in a solution containing lithium, and modifying the silicon oxide by an electrochemical method to generate the compound containing lithium, silicon, and oxygen and to form the ion conductive layer; The method for producing the negative electrode body according to

[20] above, comprising:

[0194] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0195] 10... negative electrode body, 11... negative electrode current collector, 11a... surface of negative electrode current collector, 12...Negative electrode active material layer, 14...Ion conductive layer, 16...Solid electrolyte, 20...Lithium-ion secondary battery, 21...Positive electrode material layer, 22...Positive electrode current collector.

Claims

1. a negative electrode current collector having a roughened surface; a negative electrode active material layer provided on the negative electrode current collector; an ion conductive layer having lithium ion conductivity on the surface of the negative electrode active material layer; and a solid electrolyte layer adjacent to the ion conductive layer, The negative electrode active material layer includes negative electrode active material particles having a compound containing lithium, silicon, and oxygen, and the negative electrode active material particles are SiO x1 Li y1 wherein the value of x1 is greater than 0.8 and less than or equal to 1.2, and the value of y1 is greater than or equal to 0.5 and less than or equal to 3.

4.

2. The negative electrode active material layer has a multilayer structure consisting of two or more layers, When the negative electrode active material particles are defined as primary particles, the negative electrode active material layer forms secondary particles which are aggregates of the primary particles, The secondary particles are separated from each other in the in-plane direction, 2. The negative electrode body according to claim 1, wherein a thickness T1 of the negative electrode active material layer before charging and a thickness T2 of the negative electrode active material layer when fully charged satisfy a relationship of T2 / T1≦1.

4.

3. 3. The negative electrode body according to claim 2, wherein the negative electrode active material layer having a multilayer structure has an interlayer lithium ion conductive layer having lithium ion conductivity between at least one of the layers constituting the multilayer.

4. The negative electrode active material layer is 4 SiO 4 , Li 2 S 2 O 5 , Li 2 SiO 3 and Li 6 S 2 O 7 2. The negative electrode body according to claim 1, comprising at least one of the following:

5. 2. The negative electrode body according to claim 1, wherein the ion conduction layer having lithium ion conductivity is made of at least one of a carbonate of Li, a phosphate of Li, a fluoride of Li, a carbonate of Al, a phosphate of Al, a fluoride of Al, a compound having a silyl group, and a carbonized material containing a polycyclic aromatic hydrocarbon.

6. 3. The negative electrode body according to claim 2, wherein the secondary particles of the negative electrode active material layer are composed of, on average, four or more primary particles.

7. 2. The negative electrode body according to claim 1, wherein the solid electrolyte layer is made of a sulfide-based solid electrolyte.

8. 8. The negative electrode body according to claim 7, wherein the sulfide-based solid electrolyte contains at least one of lithium, indium, sulfur, and phosphorus.

9. The sulfide-based solid electrolyte is Li 2 S, P 2 S 5 , SiS 2 , LiI, LiBr, P 2 O 5 , Li 3 P.O. 4 and GeS 2 8. The negative electrode body according to claim 7, characterized in that it has at least one of the following:

10. 2. The negative electrode body according to claim 1, wherein the solid electrolyte layer is made of an oxide-based solid electrolyte.

11. 11. The negative electrode body according to claim 10, wherein the oxide-based solid electrolyte has a perovskite structure.

12. 11. The negative electrode body according to claim 10, wherein the oxide-based solid electrolyte contains at least one of lanthanum, lithium, magnesium, tungsten, niobium, and titanium.

13. The oxide-based solid electrolyte has a composition formula of A x2 B.O. 3 (0<x2<1), the element A includes at least one of La and Li, and the element B includes at least one of Mg, W, Nb, and Ti. The negative electrode body according to claim 10,

14. 11. The negative electrode body according to claim 10, wherein the oxide-based solid electrolyte contains a Nasicon-type phosphate compound.

15. 15. The negative electrode body according to claim 14, wherein the solid electrolyte having a Nasicon-type phosphate compound contains at least one of lithium, aluminum, germanium, zirconium, titanium, and calcium.

16. The Nasicon-type phosphate compound is Li (1+x3) M1 (x3) M2 (2-x3) (P.O. 4 ) 3 wherein the element M1 includes at least one selected from the group consisting of Al, Y, Ga, and In, the element M2 includes at least one selected from the group consisting of Ti, Ge, and Zr, and x3 satisfies 0≦x3≦2.

17. 11. The negative electrode body according to claim 10, wherein the oxide-based solid electrolyte has a garnet-type crystal structure.

18. 18. The negative electrode body according to claim 17, wherein the solid electrolyte having a garnet-type crystal structure contains at least one of lithium, lanthanum, calcium, zirconium, bismuth, aluminum, cerium, gallium, boron, and oxygen.

19. The solid electrolyte having a garnet-type crystal structure is Li (7-3x4+y4-z4) M x4 La (3-y4) A' ((y4) Zr (2-z4) T (z4) O 12 The negative electrode body according to claim 17, characterized in that the element M is one or more of Al and Ga, the element A' is one of Ca and Sr, T is one of Nb and Ta, and 0≦x4≦0.18, 0≦y4≦0.18, and 0≦z4≦1.5 are satisfied.

20. A method for producing the anode body according to any one of claims 1 to 19, comprising the steps of: A step of winding the negative electrode current collector around a can roll having a curvature; a vapor phase growth step of vapor-growing a film containing silicon and / or silicon monoxide having a multilayer structure consisting of two or more layers on the negative electrode current collector while the negative electrode current collector is running on the can roll; A step of blowing an oxygen-containing gas onto the silicon and / or silicon monoxide-containing film to form a multi-layer structure containing silicon dioxide on the top of each layer; forming the negative electrode active material layer by inserting and extracting lithium into and from the layers of the multilayer structure; forming an ion conductive layer having lithium ion conductivity on a surface of the negative electrode active material layer; forming the solid electrolyte layer adjacent to the ion conductive layer; A method for producing a negative electrode body comprising the steps of:

21. In the step of forming layers of the multilayer structure, layers of the multilayer structure are formed, each layer of which contains a silicon oxide including the silicon dioxide; In the vapor phase growth step, a negative electrode active material layer containing silicon oxide is vapor-grown on the negative electrode current collector; a step of immersing the negative electrode active material layer containing the silicon oxide in a solution containing lithium, and modifying the silicon oxide by an electrochemical method to generate the compound containing lithium, silicon, and oxygen and to form the ion conductive layer; The method for producing a negative electrode body according to claim 20, further comprising:

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery and method of manufacture

    JP2003157898A

  • Storage element and storage element system

    JP2013041781A

  • Negative electrode mixture, negative electrode, and lithium ion battery

    JP2014067687A

  • Negative electrode and negative electrode manufacturing method

    JP2023026832A

  • Power storage device

    JP2023053492A