Adhesive for power storage device packaging material, power storage device packaging material, container for power storage device, and power storage device
The adhesive composition for power storage device packaging materials, using a polyisocyanate and polyol with specific partial structure, addresses issues of adhesiveness and durability, providing high adhesion and flexibility with reduced application, and maintaining performance under harsh conditions.
Patent Information
- Application Number
- JP2023087150
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Existing adhesives for power storage device packaging materials face challenges in achieving high adhesiveness and flexibility with reduced adhesive application, poor moldability, and insufficient long-term durability under harsh conditions, particularly in automotive applications.
The adhesive composition comprises a polyisocyanate and a polyol, with the polyol containing 20 to 60% polyester polyol and 0.5 to 12.0% of a specific partial structure, promoting rapid curing and enhancing cohesive force through urea bond formation, while maintaining flexibility and adhesion.
The adhesive achieves high adhesiveness, flexibility, and long-term durability even with reduced application, ensuring excellent moldability and resistance to high temperature and humidity.
Smart Images

Figure 2024170146000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive for packaging materials for electricity storage devices for forming containers for electricity storage devices such as lithium ion batteries, and relates to an adhesive for packaging materials for electricity storage devices that has a good appearance and excellent adhesive strength and formability. [Background technology]
[0002] The rapid growth of electronic devices such as mobile phones and portable personal computers has led to an increased demand for power storage devices such as secondary batteries, such as lithium ion batteries and nickel-metal hydride batteries, and electrochemical capacitors, such as electric double layer capacitors. Among these, small lithium ion batteries have attracted attention due to their high energy density and light weight. Traditionally, metal cans have been used as the exterior body of lithium ion batteries, but from the viewpoints of weight reduction and productivity, packaging materials made of laminated plastic films and metal foils are becoming mainstream.
[0003] In the field of packaging materials for such electricity storage devices, for example, Patent Document 1 discloses that a laminate adhesive composition for battery packaging containing a polyol-modified polyisocyanate, which is a compound of an aromatic isocyanate having three or more functional isocyanate groups in its molecular structure and a polyester polyol, and a polyester polyol, has excellent adhesion and heat resistance and can shorten the curing period. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-110086 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] In recent years, as applications such as in-vehicle and home power storage expand, there is a demand for larger capacity secondary batteries, and packaging materials for power storage devices are required to have good formability. On the other hand, further weight reduction is required for in-vehicle applications, and there is a demand for packaging materials that maintain the adhesive strength between layers of the plastic films and metal foils of the packaging material even after molding and long-term durability tests, even if the amount of adhesive applied is reduced, and that have no abnormalities in appearance. In addition, there is a demand for further shortening the curing period and improving productivity along with the reduction in the amount of adhesive applied.
[0006] However, the adhesive described in Patent Document 1 does not contain the partial structure represented by general formula (1), and therefore the urethane reaction does not proceed quickly. Therefore, in the harsh usage environments that have been required in recent years, such as reducing the amount of adhesive applied and shortening the curing period, it takes time for the adhesive to develop adhesion, and there is a problem that the adhesive strength after molding and after long-term durability testing decreases.
[0007] Therefore, an object of the present invention is to provide an adhesive for packaging materials for electricity storage devices that exhibits high adhesion and flexibility, and that combines excellent formability with long-term durability at high temperatures and high humidity, even when a small amount of adhesive is applied and the curing time is shortened, and to provide packaging materials for electricity storage devices, containers for electricity storage devices, and electricity storage devices that use the adhesive and have excellent formability and long-term durability. [Means for solving the problem]
[0008] As a result of intensive research aimed at solving the above problems, the present inventors have found that the above problems can be solved by the embodiments described below, and have thus completed the present invention.
[0009] <1> That is, the present invention relates to an adhesive for packaging materials for electricity storage devices that contains a polyisocyanate (A) and a polyol (B), wherein the polyol (B) contains a polyester polyol (b1), the polyol (B) accounts for 20 to 60 mass% based on the mass of the polyisocyanate (A), and the partial structure represented by the following general formula (1) accounts for 0.5 to 12.0 mass% based on the solids mass of the adhesive: General formula (1) [ka] [In general formula (1), R represents a hydrogen atom or a methyl group, and n represents an integer of 2 to 20.]
[0010] <2> The present invention relates to a polyisocyanate (A) comprising a reaction product of a polyisocyanate and a polyol including a polyester polyol (a2), <1> The present invention relates to an adhesive for packaging materials for electricity storage devices according to the above item 1.
[0011] <3> The present invention relates to a polyisocyanate (A) comprising a reaction product of a polyisocyanate containing an adduct (a1) of an aromatic polyisocyanate and a polyol containing a polyester polyol (a2). <1> or <2> The present invention relates to an adhesive for packaging materials for electricity storage devices according to the above item 1.
[0012] <4> The present invention relates to a polyhydric alcohol which is a constituent component of the polyester polyol (a2), and the polyhydric alcohol contains 5 to 30 mol % of a polyhydric alcohol having a partial structure represented by general formula (1) based on 100 mol % of the polyhydric alcohol. <2> or <3> The present invention relates to an adhesive for packaging materials for electricity storage devices according to the above item 1.
[0013] <5> The present invention relates to a polyol (B) which further contains a hydroxyl group-containing epoxy resin (b2) in an amount of 5 to 50 mass% based on the mass of the polyol (B). <1> ~ <3> The present invention relates to an adhesive for use in packaging materials for electricity storage devices according to any one of claims 1 to 5.
[0014] <6> The present invention relates to a hydroxyl group-containing epoxy resin (b2) which is a bisphenol A type epoxy resin. <5> The present invention relates to an adhesive for packaging materials for electricity storage devices according to the above item 1.
[0015] <7> The present invention relates to a packaging material for an electricity storage device having a configuration in which at least an outer layer resin film layer, an outer layer adhesive layer, a metal foil layer, an inner layer adhesive layer, and a heat seal layer are laminated in this order, and the outer layer adhesive layer is <1> ~ <6> The present invention relates to a packaging material for an electricity storage device, which is a cured product of the adhesive for use in packaging materials for electricity storage devices according to any one of claims 1 to 4.
[0016] <8> The present invention relates to <7> The present invention relates to a container for an electricity storage device formed from the packaging material for an electricity storage device according to claim 1, wherein the outer layer side resin film layer forms a convex surface and the heat seal layer forms a concave surface.
[0017] <9> The present invention relates to <8> The present invention relates to an electricity storage device comprising the electricity storage device container according to claim 1. Effect of the Invention
[0018] The present invention makes it possible to provide an adhesive for packaging materials for electricity storage devices that exhibits high adhesion and flexibility, and is capable of achieving both excellent formability and long-term durability at high temperatures and high humidity, even when a small amount of adhesive is applied and the curing time is shortened, as well as packaging materials for electricity storage devices, containers for electricity storage devices, and electricity storage devices that use the adhesive and have excellent formability and long-term durability. [Brief description of the drawings]
[0019] [Figure 1] 1 is a schematic cross-sectional view of a packaging material for an electricity storage device of the present invention. [Diagram 2] FIG. 1 is a schematic perspective view of one embodiment (tray-shaped) of a container for an electricity storage device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] <Adhesive for packaging materials for power storage devices> The adhesive for packaging materials for electricity storage devices (hereinafter also referred to as the adhesive) of the present invention is an adhesive containing a polyisocyanate (A) and a polyol (B), characterized in that the polyol (B) contains a polyester polyol (b1), the polyol (B) accounts for 20 to 60 mass% based on the mass of the polyisocyanate (A), and the partial structure represented by the above general formula (1) accounts for 0.5 to 12.0 mass% based on the solids mass of the adhesive.
[0021] First, by containing 0.5 to 12.0% by mass of the highly hydrophilic partial structure represented by the above general formula (1), the affinity with water is increased, and the reaction between the polyisocyanate (A) and water is promoted. This reaction forms a urea bond with high cohesive strength, and the self-crosslinking reaction proceeds during curing to improve the cohesive strength, so that high adhesiveness can be achieved even with a small application amount and a short curing time. Furthermore, since the partial structure has a flexible skeleton, by having a predetermined amount of such a flexible partial structure, excellent moldability can be achieved. The content of the partial structure is preferably 5.0 to 10.0% by mass. When it is 5.0% by mass or more, curing easily proceeds even with a short curing time, and when it is 10% by mass or less, excellent moist heat resistance is achieved. The partial structure of general formula (1) may be contained in at least one of the polyisocyanate (A) and the polyol (B), or may be contained in both. From the viewpoints of improving the compatibility between the polyisocyanate (A) and the polyol (B) and further improving the appearance, it is preferable that both the polyisocyanate (A) and the polyol (B) contain the partial structure of general formula (1). In general formula (1), R is preferably a hydrogen atom. When R is a hydrogen atom, the affinity with water is increased, which is preferable from the viewpoint of shortening the curing period, and the cohesive force of the adhesive layer is increased, improving the adhesion and moldability.
[0022] It is also important that the adhesive of the present invention contains 20 to 60 mass % of polyol (B) containing polyester polyol (b1) based on the mass of polyisocyanate (A), more preferably in the range of 25 to 45 mass %. If it is less than 20 mass %, the cured film becomes excessively rigid, and the adhesion and conformability to the substrate are insufficient, making it impossible to achieve both adhesive strength and moldability. If it exceeds 60 mass %, the cohesive strength of the adhesive decreases, and furthermore, the amount of hydroxyl groups in the adhesive increases and the amount of isocyanate groups decreases, so that the affinity with the substrate decreases, and the adhesive strength and moist heat resistance are insufficient. Furthermore, when polyol (B) contains polyester polyol (b1), the adhesion to the substrate is improved, and even when the application amount is small and the curing period is short, high adhesion and moldability can be exhibited.
[0023] In other words, the adhesive for packaging materials for electricity storage devices of the present invention has a synergistic effect based on the fact that the amount of polyol, including polyester polyol, relative to the polyisocyanate is 20 to 60 mass % and that the adhesive contains the partial structure represented by general formula (1) in an amount of 0.5 to 12.0 mass %, and even when the application amount is small and the curing period is short, the adhesive exhibits high cohesive strength, substrate conformability, and flexibility, and can achieve excellent adhesive strength, moldability, and moist heat resistance.
[0024] <Polyisocyanate (A)> Polyisocyanate (A) crosslinks with the hydroxyl groups in polyol (B) to increase the molecular weight of the adhesive layer and improve the internal cohesive strength that produces energy elasticity. In addition, the isocyanate groups in polyisocyanate (A) can react with water to form urea bonds with high cohesive strength, so the cohesive strength of the adhesive layer can be increased by self-crosslinking during curing. In this way, the use of polyisocyanate (A) makes it possible to form a strong adhesive layer and improve the adhesive strength.
[0025] Examples of the polyisocyanate (A) include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, araliphatic polyisocyanates, and various derivatives derived from the above polyisocyanates.
[0026] Examples of aliphatic polyisocyanates include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, and 2,6-diisocyanate methyl caproate.
[0027] Examples of alicyclic polyisocyanates include 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane, and 1,3-bis(isocyanatomethyl)cyclohexane.
[0028] Examples of aromatic polyisocyanates include m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate or a mixture thereof, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, 4,4'-diphenylether diisocyanate, triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanate benzene, 2,4,6-triisocyanate toluene, and 4,4'-diphenyldimethylmethane-2,2'-5,5'-tetraisocyanate.
[0029] Examples of araliphatic polyisocyanates include 1,3- or 1,4-xylylene diisocyanate or mixtures thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or mixtures thereof.
[0030] Examples of derivatives derived from the polyisocyanates include adducts of the polyisocyanates with low molecular weight polyols having a molecular weight of less than 200, such as ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolpropane, cyclohexanedimethanol, diethylene glycol, triethylene glycol, dipropylene glycol, glycerol, trimethylolpropane, pentaerythritol, and sorbitol, or castor oil; trimers (also called trimers or nurates) of the diisocyanates; biuret products; allophanate products; polyisocyanates having a 2,4,6-oxadiazinetrione ring obtained from carbon dioxide gas and the diisocyanates; and polyurethane polyisocyanates obtained by reacting polyisocyanates with polyols under conditions in which there is an excess of isocyanate groups.
[0031] The polyol to be reacted with the polyisocyanate may be any of the conventionally known polyols, such as polyester polyols, polyether polyols, polycarbonate polyols, acrylic polyols, and polybutadiene polyols.
[0032] (Polyester urethane polyisocyanate) From the viewpoint of achieving both excellent high-temperature durability and high cohesive strength and processability, the polyisocyanate (A) preferably contains a polyesterurethane polyisocyanate which is a reaction product of a polyisocyanate and a polyol containing a polyester polyol (a2). As the polyisocyanate for forming the polyesterurethane polyisocyanate, an aromatic polyisocyanate is preferably used, and among them, one containing an adduct (a1) of an aromatic polyisocyanate such as tolylene diisocyanate or MDI is particularly preferably used.
[0033] (Adduct of aromatic polyisocyanate (a1)) The adduct (a1) of the aromatic polyisocyanate may be an adduct obtained by adding an aromatic diisocyanate monomer to a polyhydric alcohol. Examples of the diisocyanate monomer include m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate or a mixture thereof, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, and 4,4'-diphenyl ether diisocyanate. Examples of the polyhydric alcohol include Examples include low molecular weight polyols having a molecular weight of less than 200, such as ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolpropane, cyclohexanedimethanol, diethylene glycol, triethylene glycol, dipropylene glycol, glycerol, trimethylolpropane, pentaerythritol, and sorbitol, and castor oil. As such an aromatic polyisocyanate adduct (a1), for example, an adduct of tolylene diisocyanate with trimethylolpropane, an adduct of tolylene diisocyanate with trimethylolpropane and diethylene glycol, an adduct of 4,4'-diphenyl diisocyanate with trimethylolpropane, dipropylene glycol and tripropylene glycol are preferably used. That is, the polyester urethane polyisocyanate is preferably a polyisocyanate obtained by reacting a polyisocyanate containing an aromatic polyisocyanate adduct (a1) with a polyol containing a polyester polyol (a2). By providing an ester structure derived from such a polyester polyol and a urethane structure, it is possible to combine flexibility and cohesive strength, and to exhibit excellent adhesive performance.
[0034] The polyisocyanate for forming the polyester urethane polyisocyanate may contain a polyisocyanate other than the adduct (a1) of an aromatic polyisocyanate. Examples of such a polyisocyanate include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, araliphatic polyisocyanates, and various derivatives derived from the polyisocyanates described above in the section <Polyisocyanate (A)>.
[0035] (Polyester polyol (a2)) In the present invention, the polyester polyol (a2) is not limited to the following, but examples thereof include polyester polyols obtained by reacting a polybasic acid with a polyhydric alcohol; and polyester polyols obtained by ring-opening polymerization of lactones such as polycaprolactone, polyvalerolactone, and poly(β-methyl-γ-valerolactone).
[0036] Examples of the polybasic acid include dibasic acids having an aromatic ring, such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, and phthalic anhydride; aliphatic dibasic acids, such as adipic acid, azelaic acid, sebacic acid, succinic acid, glutaric acid, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, maleic anhydride, and itaconic anhydride; or dialkyl esters thereof, or mixtures thereof.
[0037] Examples of the polyhydric alcohol include diols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, butylene glycol, neopentyl glycol, dineopentyl glycol, trimethylolpropane, glycerin, 1,6-hexanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolheptane, 1,9-nonanediol, polyoxyethylene glycol, polyoxypropylene glycol, polytetramethylene ether glycol, polyether polyol, polycarbonate polyol, polyolefin polyol, acrylic polyol, and polyurethane polyol; or mixtures thereof. The polybasic acids and polyhydric alcohols may each be used alone, but it is preferable to use two or more of them in combination.
[0038] The polyhydric alcohol constituting the polyester polyol (a2) preferably contains 5 to 30 mol % of a polyhydric alcohol having a partial structure represented by the following general formula (1) per 100 mol % of the polyhydric alcohol. When it is 5 mol % or more, the affinity with water is increased, and the effect of shortening the curing time is easily achieved. When it is 30 mol % or less, the polyisocyanate (A) does not become too flexible, and the adhesiveness at high temperatures is excellent.
[0039] General formula (1) [ka] [In general formula (1), R represents a hydrogen atom or a methyl group, and n represents an integer of 2 to 20.]
[0040] Examples of the polyhydric alcohol having the partial structure include diethylene glycol, triethylene glycol, dipropylene glycol, and tripropylene glycol. The polyhydric alcohol having the partial structure may be a polyoxyalkylene glycol obtained by polymerizing an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran with a low molecular weight polyol such as water, ethylene glycol, propylene glycol, trimethylolpropane, or glycerin as an initiator. From the viewpoint of reactivity and moderate hydrophilicity, those having an oxyethylene structure are preferred. From the viewpoint of compatibility between the polyhydric alcohol and other raw materials, diethylene glycol is preferred.
[0041] The weight average molecular weight (Mw) of the polyester polyol (a2) is preferably 5,000 to 30,000. When the weight average molecular weight is 5,000 or more, the adhesion to the substrate is further improved, and the processability is excellent. When the weight average molecular weight is 30,000 or less, the hydroxyl group concentration at the terminal of the polyester polyol (a2) can be easily prevented from being excessively low, and when the polyester polyol (a2) is reacted with the aromatic polyisocyanate (a1) having three or more functional groups to obtain the polyisocyanate (A), the reaction time can be easily prevented from being prolonged.
[0042] The hydroxyl value (OHV) of the polyester polyol (a2) is preferably 2 to 35 mgKOH / g, more preferably 10 to 20 mgKOH / g. The hydroxyl group is used in a reaction with the aromatic polyisocyanate (a1) having three or more functional groups, and as the reaction proceeds, the adhesive has a high molecular weight, and the heat resistance as a packaging material can be improved. The hydroxyl value can be determined by a method in accordance with JIS K 1557-1.
[0043] The glass transition temperature (Tg) of the polyester polyol (a2) is preferably in the range of −20 to 5° C., more preferably −10 to 0° C. Within the above range, the cohesive strength of the adhesive can be easily controlled, and an appropriate cohesive strength can be obtained depending on the adherend substrate, required performance, etc.
[0044] The reaction temperature for urethanization of the tri- or higher functional aromatic polyisocyanate (a1) and the polyester polyol (a2) is preferably 50 to 180° C., and more preferably 60 to 100° C. A temperature of 50 to 180° C. is preferable because the urethanization reaction proceeds efficiently.
[0045] The NCO% contained in the polyisocyanate (A) is preferably 1.0 to 8.0 mass% in terms of solid content, and more preferably 4.0 to 6.0 mass%. When it is 1.0 mass% or more, the amount of urethane bonds after curing becomes sufficient, the cohesive force increases, and the adhesive strength improves. When it is 8.0 mass% or less, the time required for curing can be shortened and poor appearance due to foaming can be suppressed.
[0046] <Polyol (B)> The polyol (B) used in the present invention is characterized by containing polyester polyol (b1). By containing polyester polyol (b1), the adhesion to the substrate is improved, and excellent adhesive strength and moldability can be exhibited. In addition, polyester polyol (b1) is preferable from the viewpoint of easy introduction of the partial structure of general formula (1).
[0047] (Polyester polyol (b1)) Examples of the polyester polyol (b1) include polyester polyols obtained by reacting a polybasic acid with a polyhydric alcohol, or polyester polyols obtained by ring-opening polymerization of lactones such as polycaprolactone, polyvalerolactone, poly(β-methyl-γ-valerolactone), etc. As such polyester polyol (b1), those described in the above section on (polyester polyol (a2)) of <Polyisocyanate (A)> can be used. Similarly to the polyester polyol (a2), the polyhydric alcohol constituting the polyester polyol (b1) may contain a polyhydric alcohol having a partial structure represented by the general formula (1) in the polyhydric alcohol constituting the polyester polyol (b1). The content of the polyhydric alcohol having a partial structure is preferably 5 to 30 mol % in 100 mol % of the polyhydric alcohol.
[0048] The weight-average molecular weight of the polyester polyol (b1) is preferably 5,000 to 60,000. When the weight-average molecular weight is 5,000 or more, the adhesion to the substrate is improved and the processability is excellent. When the weight-average molecular weight is 60,000 or less, the compatibility when mixed with the polyisocyanate (A) is excellent and the appearance is good.
[0049] The polyester polyol (b1) preferably has a hydroxyl value of 5 to 20 mgKOH / g, and a glass transition temperature of the polyester polyol (b1) preferably in the range of -20 to 50°C, more preferably -5 to 35°C.
[0050] (Hydroxyl-containing epoxy resin (b2)) From the viewpoint of adhesive strength and moist heat resistance, it is preferable that the polyol (B) further contains a hydroxyl-containing epoxy resin (b2). By using the hydroxyl-containing epoxy resin (b2) in combination, the high-temperature adhesive strength to metal materials such as metal foil, and the heat resistance and heat resistance durability of the molded product are improved. The content of the hydroxyl-containing epoxy resin (b2) is preferably 5 to 50 mass% based on the mass of the polyol (B). When it is 5 mass% or more, the adhesive strength and moist heat resistance are excellent. When it is 50 mass% or less, the moldability is excellent. From the viewpoint of the balance of adhesive strength, moldability, and moist heat resistance, it is more preferably 10 to 30 mass%.
[0051] Examples of the hydroxyl-containing epoxy resin (b2) include bisphenol A type epoxy resin, bisphenol F type epoxy resin, polyglycerol polyglycidyl ether, sorbitol polyglycidyl ether, and trimethylolpropane polyglycidyl ether. From the viewpoint of adhesiveness and durability of molded products, bisphenol A type epoxy resin is preferable. These hydroxyl-containing epoxy resins may be used alone or in combination of two or more kinds.
[0052] (Other polyols) The polyol (B) may further contain a known polyol other than (b1) and (b2) within the range not impairing the effects of the present invention. Examples of such polyols include polyether polyols, polyurethane polyols, polycarbonate polyols, and acrylic polyols, and may further be reacted with polyisocyanates to introduce urethane bonds.
[0053] <Solvent> The adhesive of the present invention may contain a solvent within a range that does not affect the substrate during the drying process in order to adjust the viscosity of the coating liquid to an appropriate level when the adhesive is applied to the substrate. Examples of the solvent include ketone compounds such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester compounds such as methyl acetate, ethyl acetate, butyl acetate, ethyl lactate, and methoxyethyl acetate; ether compounds such as diethyl ether and ethylene glycol dimethyl ether; aromatic compounds such as toluene and xylene; aliphatic compounds such as pentane and hexane; and halogenated hydrocarbon compounds such as methylene chloride, chlorobenzene, and chloroform.
[0054] <Manufacture of adhesives for packaging materials for power storage devices> The adhesive of the present invention contains at least the polyisocyanate (A) and a polyol (B) containing the polyester polyol (b1), and the content of the polyol (B) is 20 to 60 mass% based on the mass of the polyisocyanate (A), and the content of the partial structure represented by the general formula (1) is 0.5 to 12.0 mass% based on the solids mass of the adhesive.
[0055] In the adhesive of the present invention, when polyisocyanate (A) and polyol (B) are blended, the ratio of the number of isocyanate groups in polyisocyanate (A) to the number of hydroxyl groups in polyol (B) (number of moles of NCO / number of moles of OH) is preferably 5 to 20, more preferably 8 to 12. When it is 5 or more, the amount of urethane bonds after curing becomes sufficient, the cohesive force increases, and the heat resistance and heat resistance durability of the molded product improve. When it is 20 or less, the time required for curing can be shortened and poor appearance due to foaming and the like can be suppressed.
[0056] The adhesive of the present invention may further contain other components within the range that does not impair the effects of the present invention. Such optional components may be blended with either or both of the polyisocyanate (A) and the polyol (B), or may be added when blending the polyisocyanate (A) and the polyol (B). Each of these may be used alone or in combination of two or more.
[0057] (Antioxidants) The adhesive of the present invention may contain an antioxidant to suppress thermal oxidation deterioration. Examples of the antioxidant include monophenol-based antioxidants such as 2,6-di-t-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-t-butyl-4-ethylphenol, and stearin-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate; 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), and 3,9-bis[1,1-dimethyl-2-[β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]2,4,8,10-tetrahydrofuran; Examples of the antioxidants include bisphenol-based antioxidants such as laxaspiro[5,5]undecane; and polymeric phenol-based antioxidants such as 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, bis[3,3'-bis-(4'-hydroxy-3'-t-butylphenyl)butyric acid]glycol ester, and 1,3,5-tris(3',5'-di-t-butyl-4'-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione and triphenol. Among these, tetraphenol-based and triphenol-based high molecular weight hindered phenol-based antioxidants are preferably used.
[0058] (Reaction accelerator) The adhesive of the present invention may further contain a reaction accelerator to promote the urethanization reaction. Examples of reaction accelerators include metal catalysts such as dibutyltin diacetate, dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin dimaleate; tertiary amines such as 1,8-diaza-bicyclo(5,4,0)undecene-7, 1,5-diazabicyclo(4,3,0)nonene-5, and 6-dibutylamino-1,8-diazabicyclo(5,4,0)undecene-7; and reactive tertiary amines such as triethanolamine.
[0059] (Silane coupling agent) The adhesive of the present invention may further contain a silane coupling agent in order to improve the adhesive strength to metal-based materials such as metal foil. Examples of the silane coupling agent include trialkoxysilanes having a vinyl group, such as vinyltrimethoxysilane and vinyltriethoxysilane; trialkoxysilanes having an amino group, such as 3-aminopropyltriethoxysilane and N-(2-aminoethyl)3-aminopropyltrimethoxysilane; and trialkoxysilanes having a glycidyl group, such as 3-glycidoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane. The content of the silane coupling agent is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 3 parts by mass, per 100 parts by mass of the solid content of the adhesive for packaging materials for electricity storage devices. By adding the silane coupling agent in the above range, the adhesive strength to the metal foil can be further improved.
[0060] (Phosphorus oxygen acid or its derivatives) The adhesive of the present invention may contain a phosphorus oxyacid or a derivative thereof in order to improve the adhesive strength to metal-based materials such as metal foil. The phosphorus oxyacid may be any acid having at least one free oxyacid, and examples of such acids include phosphoric acids such as hypophosphorous acid, phosphorous acid, orthophosphoric acid, and hypophosphoric acid; and condensed phosphoric acids such as metaphosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, and ultraphosphoric acid. In addition, examples of derivatives of phosphorus oxyacids include those obtained by partially esterifying the above phosphorus oxyacids with alcohols while leaving at least one free oxyacid. Examples of the alcohols include aliphatic alcohols such as methanol, ethanol, ethylene glycol, and glycerin; and aromatic alcohols such as phenol, xylenol, hydroquinone, catechol, and phloroglucinol. The content of the phosphorus oxyacid or its derivative is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.05 to 1 part by mass, relative to 100 parts by mass of the solid content of the adhesive for packaging materials for electricity storage devices.
[0061] (Leveling agent or defoamer) The adhesive of the present invention may further contain a leveling agent or an antifoaming agent in order to improve the laminate appearance of the packaging material. Examples of the leveling agent include polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, aralkyl-modified polymethylalkylsiloxane, polyester-modified hydroxyl-containing polydimethylsiloxane, polyetherester-modified hydroxyl-containing polydimethylsiloxane, acrylic copolymer, methacrylic copolymer, polyether-modified polymethylalkylsiloxane, acrylic acid alkyl ester copolymer, methacrylic acid alkyl ester copolymer, and lecithin. Examples of the defoaming agent include silicone resin, silicone solution, and copolymers of alkyl vinyl ether, alkyl acrylate, and alkyl methacrylate.
[0062] (Additives) The adhesive of the present invention may contain various additives within a range that does not impair the effects of the present invention. Examples of additives include inorganic fillers such as silica, alumina, mica, talc, aluminum flakes, and glass flakes, layered inorganic compounds, stabilizers (antioxidants, heat stabilizers, ultraviolet absorbers, hydrolysis inhibitors, etc.), rust inhibitors, thickeners, plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, crystal nucleating agents, and catalysts for adjusting the curing reaction.
[0063] <Packaging materials for power storage devices> The adhesive of the present invention can be used as an adhesive for forming an adhesive layer of a packaging material for an electricity storage device. In particular, it can be suitably used as an outer layer side adhesive that forms an outer layer side adhesive layer of a packaging material for an electricity storage device. The packaging material for an electricity storage device of the present invention has a configuration in which at least an outer layer side resin film layer, an outer layer side adhesive layer, a metal foil layer, and a heat seal layer are laminated in this order from the outside, and is characterized in that the outer layer side adhesive layer is a cured product of the adhesive for packaging materials for electricity storage devices described above. The method for producing the packaging material for an electricity storage device is not particularly limited, and the material can be produced by a known method. For example, an outer layer resin film layer and a metal foil layer can be laminated using an adhesive for packaging materials for electricity storage devices that forms the above-mentioned outer layer adhesive layer to obtain an intermediate laminate having a configuration of outer layer resin film layer / outer layer adhesive layer / metal foil layer, and then a heat seal layer can be laminated on the metal foil layer surface of the intermediate laminate using an inner layer adhesive (hereinafter, manufacturing method 1). Alternatively, the packaging material can be produced by laminating a metal foil layer and a heat seal layer using an inner layer adhesive to obtain an intermediate laminate having a configuration of metal foil layer / inner layer adhesive layer / heat seal layer, and then laminating the metal foil layer of the intermediate laminate and an outer layer resin film layer using an adhesive for packaging materials for electricity storage devices (hereinafter, Production Method 2).
[0064] In the case of manufacturing method 1, it is preferable to apply the adhesive for electricity storage device packaging materials to one side of the substrate of either the outer layer side resin film layer or the metal foil layer, volatilize the solvent, and then laminate the other substrate onto the uncured outer layer side adhesive layer under heat and pressure, and then age the outer layer side adhesive layer at room temperature to less than 100° C. If the aging temperature is less than 100° C., heat shrinkage of the outer layer side resin film layer does not occur, so there is no decrease in breaking elongation or breaking stress that affects molding, and no decrease in molding productivity due to film curling. The amount of adhesive applied after drying on the outer layer is 1 to 15 g / m 2 It is preferable that the amount is about 100%. Similarly, in the case of production method 2, the adhesive for a packaging material for an electricity storage device may be applied to either the outer layer side resin film layer or the metal foil layer surface of the intermediate laminate.
[0065] Examples of methods for forming the outer adhesive layer include methods using a comma coater, dry laminator, roll knife coater, die coater, roll coater, bar coater, gravure roll coater, reverse roll coater, blade coater, gravure coater, and microgravure coater.
[0066] [Outer resin film layer] The outer resin film layer is not particularly limited, but is preferably at least one stretched film selected from the group consisting of polyamide, polyester, and polyimide, and more preferably a polyester film from the viewpoints of stretchability and heat resistance during molding. Examples of polyester include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polytrimethylene terephthalate, and polycyclohexanedimethylene terephthalate. The outer resin film layer may be colored with a pigment such as carbon black or titanium oxide. The non-laminated surface of the outer resin film layer may be coated with a coating agent for preventing scratches or electrolyte resistance, or with a slip agent for providing slipperiness during molding, or may be coated with a printing ink for design purposes. The outer resin film layer may be a laminated film in which two or more layers of film are laminated in advance. The thickness of the outer resin film layer is not particularly limited, but is preferably 12 to 100 μm.
[0067] [Metal foil layer] The metal foil layer is not particularly limited, but is a stainless steel foil layer or an aluminum foil layer. The thickness of the metal foil layer is not particularly limited, but is preferably 20 to 80 μm. In addition, the surface of the metal foil layer is preferably subjected to a known antiseptic treatment such as chromate phosphate treatment, chromate chromate treatment, trivalent chromium treatment, zinc phosphate treatment, zirconium phosphate treatment, zirconium oxide treatment, titanium phosphate treatment, hydrofluoric acid treatment, cerium treatment, and hydrotalcite treatment. By being subjected to the antiseptic treatment, it is possible to suppress the corrosion deterioration of the metal foil surface due to the electrolyte of the battery. Furthermore, it is preferable that a known organic component such as a phenol resin, an amide resin, an acrylic resin, polyvinyl alcohol, or a coupling agent is applied to the antiseptic treatment surface, or a mixture of the antiseptic treatment component and the organic component is applied to the metal foil layer at a high temperature of about 200 ° C. By applying such an organic primer treatment, the metal foil and the adhesive can be more firmly bonded, and the lift between the metal foil and the adhesive can be further suppressed.
[0068] [Heat seal layer] The heat seal layer is not particularly limited, and is preferably an unstretched film made of at least one thermoplastic resin selected from the group consisting of polyester, polyethylene, polypropylene, olefin copolymers, acid modified products thereof, and ionomers. The thickness of the heat seal layer is not particularly limited, and is preferably 20 to 150 μm.
[0069] [Inner adhesive layer] The adhesive that forms the inner adhesive layer is not particularly limited, but it is preferable that the adhesive strength between the metal foil layer and the heat seal layer is not reduced by the electrolyte of the electricity storage device. In addition to the adhesive for electricity storage device packaging materials of the present invention, known adhesives can be used. The inner layer side adhesive layer can be formed, for example, by applying an adhesive made of a combination of a polyolefin resin and a polyisocyanate or an adhesive made of a combination of a polyol and a polyisocyanate to a metal foil layer using a gravure coater or the like, drying the solvent, laminating a heat seal layer on the adhesive layer under heat and pressure, and then aging the resulting mixture at room temperature or under elevated temperature. Alternatively, an adhesive such as acid-modified polypropylene can be melt-extruded onto a metal foil layer using a T-die extruder to form an adhesive layer, a heat seal layer can be superimposed on the adhesive layer, and the metal foil layer and the heat seal layer can be bonded together to form an inner layer adhesive layer. When both the outer layer adhesive layer and the inner layer adhesive layer require aging, they may be aged together after obtaining a laminate having a configuration in which the outer layer resin film layer, the uncured outer layer adhesive layer, the metal foil layer, the uncured inner layer adhesive layer, and the heat seal layer are laminated from the outside in this order.
[0070] <Containers for electricity storage devices> The container for an electricity storage device of the present invention can be obtained by using the packaging material for an electricity storage device of the present invention and molding it so that the outer layer side resin film layer forms a convex surface and the heat seal layer forms a concave surface. Note that the "concave surface" in the present invention means a surface having a depression capable of containing an electrolyte solution when the packaging material for an electricity storage device in a flat state is molded into a tray shape as shown in Fig. 2, and the "convex surface" in the present invention means the back surface of the surface having the depression.
[0071] <Electricity storage device> The electricity storage device of the present invention uses the container for electricity storage devices, and examples of the container include secondary batteries such as lithium ion batteries, nickel hydrogen batteries, and lead storage batteries, and electrochemical capacitors such as electric double layer capacitors. A typical electricity storage device includes a battery element including an electrode, leads extending from the electrode, and a container that houses the battery element, and in the electricity storage device of the present invention, the container for electricity storage devices is used as the container for housing. The container for housing may be formed from a packaging material for electricity storage devices with the heat seal layer facing on the inside, and may be obtained by overlapping the heat seal layers of two packaging materials facing each other and heat fusing the peripheral portions of the overlapped packaging materials, or one packaging material may be folded back and overlapped, and the peripheral portions of the packaging materials may be heat fusing in the same manner. EXAMPLES
[0072] The present invention will be described in more detail below with reference to examples and comparative examples. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.
[0073] <Acid value (AV) measurement> Approximately 1 g of sample (polyester polyol solution) was precisely weighed and placed in a stoppered Erlenmeyer flask, and 100 ml of a toluene / ethanol (volume ratio: toluene / ethanol = 2 / 1) mixture was added to dissolve it. Phenolphthalein test solution was added as an indicator and the solution was held for 30 seconds. After that, the solution was titrated with 0.1N alcoholic potassium hydroxide solution until it turned a light pink color, and the acid value (mgKOH / g) was calculated using the following formula. Acid value (mgKOH / g)=(5.611×a×F) / S Where S is the amount of sample taken (g) a: Consumption of 0.1N alcoholic potassium hydroxide solution (ml) F: Potency of 0.1N alcoholic potassium hydroxide solution
[0074] <Measurement of hydroxyl value (OHV)> Precisely weigh approximately 1 g of a sample (such as polyester polyol or hydroxyl group-containing urethane resin) into a conical flask with a joint, add 100 ml of a toluene / ethanol (volume ratio: toluene / ethanol = 2 / 1) mixed solution, and dissolve it. Further, accurately add 5 ml of an acetylating agent (a solution prepared by dissolving 25 g of acetic anhydride in pyridine to make a volume of 100 ml), and stir for about 1 hour. Add phenolphthalein test solution as an indicator and hold for 30 seconds. Then, titrate with a 0.5 N alcoholic potassium hydroxide solution until the solution turns light pink, and determine the hydroxyl value (mgKOH / g) according to the following formula. Hydroxyl value (mgKOH / g) = [{(b - a) × F × 28.05} / S] + D However, S: Sampling amount of the sample (g) a: Consumption volume of 0.5 N alcoholic potassium hydroxide solution (ml) b: Consumption volume of 0.5 N alcoholic potassium hydroxide solution in the blank experiment (ml) F: Normality of 0.5 N alcoholic potassium hydroxide solution D: Acid value (mgKOH / g)
[0075] <Method for measuring NCO content (mass%)> Weigh approximately 1 g of a sample into a 200 mL conical flask, add 10 mL of a toluene solution of 0.5 N di-n-butylamine and 10 mL of toluene thereto, and dissolve. Next, add phenolphthalein test solution as an indicator, hold for 30 seconds, and then titrate with a 0.25 N hydrochloric acid solution until the solution turns light pink. The NCO content (mass%) was determined by the following (Formula 3). (Formula 3): NCO (mass%) = {(b - a) × 4.202 × F × 0.25} / S However, S: Sampling amount of the sample (g) a: Consumption volume of 0.25 N hydrochloric acid solution (ml) b: Consumption volume of 0.25 N hydrochloric acid solution in the blank experiment (ml) F: Normality of 0.25 N hydrochloric acid solution
[0076] <Measurement of weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn)> The weight average molecular weight and number average molecular weight were measured using Showdex (registered trademark) (manufactured by Showa Denko K.K.), columns: KF-805L, KF-803L, and KF-802 (all trade names, manufactured by Showa Denko K.K.), with a column temperature of 40° C., THF as eluent, a flow rate of 0.2 ml / min, detection by RI, and a sample concentration of 0.02% by mass, in terms of standard polystyrene. The molecular weight distribution was calculated from the obtained values.
[0077] <Glass transition temperature (Tg)> The glass transition temperature was measured by DSC (differential scanning calorimeter). Specifically, about 2 mg of the compound to be measured was weighed on an aluminum pan, the aluminum pan was set in a DSC measurement holder, and the endothermic peak of the chart obtained under the temperature increase condition of 5°C / min was read, and the peak temperature at this time was determined as the glass transition temperature.
[0078] <<Production of Polyisocyanate (A)>> <Synthesis of aromatic polyisocyanate adduct (a1)> (Adduct of aromatic polyisocyanate (a1-1)) 239 parts of tolylene diisocyanate was charged, and 61 parts of molten trimethylolpropane was added dropwise while stirring at room temperature, and the reaction was carried out at 60°C for 2 hours. The mixture was then diluted with ethyl acetate to adjust the non-volatile content to 50% and taken out. The NCO% of the resulting aromatic polyisocyanate adduct (a1-1) in terms of solid content was 19.0%, and the amount of the partial structure of general formula (1) was 0%.
[0079] (Adduct of aromatic polyisocyanate (a1-2)) 238 parts of tolylene diisocyanate was charged, and a mixture of 46 parts of molten trimethylolpropane and 15 parts of diethylene glycol was added dropwise while stirring at room temperature, and the reaction was carried out at 60°C for 2 hours. The mixture was then diluted with ethyl acetate to adjust the non-volatile content to 50% and taken out. The NCO% of the resulting aromatic polyisocyanate adduct (a1-2) was 19.4% in terms of solid content, and the amount of the partial structure of general formula (1) was 4.4%.
[0080] (Adduct of aromatic polyisocyanate (a1-3)) 244 parts of 4,4'-diphenylmethane diisocyanate was charged, and a mixture of 32 parts of molten trimethylolpropane and 15 parts of dipropylene glycol was added dropwise while stirring at 40°C, and the reaction was carried out at 60°C for 2 hours. The mixture was then diluted with ethyl acetate to adjust the non-volatile content to 50% and taken out. The NCO% of the resulting aromatic polyisocyanate adduct (a1-3) in terms of solid content was 14.0%, and the amount of the partial structure of general formula (1) was 5.9%.
[0081] <Synthesis of polyester polyol (a2)> (Polyester polyol (a2-1)) 166 parts of isophthalic acid, 166 parts of terephthalic acid, 293 parts of adipic acid, 87 parts of ethylene glycol, 146 parts of neopentyl glycol, and 142 parts of 1,6-hexanediol were charged and subjected to an esterification reaction for 8 hours at 170 to 230 ° C. After a predetermined amount of water was distilled off, 0.13 parts of tetraisobutyl titanate was added, the pressure was gradually reduced, and an ester exchange reaction was performed for 3 hours at 1.3 to 2.6 hPa and 230 to 250 ° C. to obtain a polyester polyol (a2-1) having a number average molecular weight of 9,620, a weight average molecular weight of 190,700, a molecular weight distribution of 2.05, a hydroxyl value of 10.1 mg KOH / g, and a glass transition temperature of -1.2 ° C. Assuming that the total of the polybasic acid and the polyhydric alcohol is 200 mol %, the composition of the obtained polyester polyol (a2-1) is isophthalic acid: terephthalic acid: adipic acid: ethylene glycol: neopentyl glycol: 1,6-hexanediol = 30:30:40:35:35:30 (mol %), as shown in Table 1-2.
[0082] (Polyester polyols (a2-2) to (a2-14)) Polyester polyols (a2-2) to (a2-14) were obtained by reacting polybasic acids and polyhydric alcohols in the same manner as for polyester polyol (a2-1), except that the amounts of each component were changed so that the mole percentages of each component when the total of the polybasic acid and polyhydric alcohol was 200 mole % were as shown in Table 1-2.
[0083] The composition ratio (mass %) and composition ratio (mol %) of the resulting polyester polyol (a2) are shown in Tables 1-1 and 1-2 (hereinafter abbreviated as Table 1).
[0084] [Table 1-1]
[0085] [Table 1-2]
[0086] The abbreviations in Table 1 and Table 3 described below are as follows. PA: Phthalic anhydride IPA: Isophthalic acid TPA: Terephthalic acid AdA: adipic acid SeA: Sebacic acid AzA: Azelaic acid EG: Ethylene glycol NPG: Neopentyl glycol 1,6-HD: 1,6-Hexanediol MPO: 2-methyl-1,3-propanediol DEG: Diethylene glycol TEG: Triethylene glycol PEG: Polyethylene glycol (hydroxyl value 281 mg KOH / g, molecular weight 400) PPG: Polypropylene glycol (hydroxyl value 280 mg KOH / g, molecular weight 400)
[0087] <Synthesis of polyisocyanate (A)> (Polyisocyanate (A-1)) 100 parts of polyester polyol (a2-1), 2.5 parts of 1,4-butanediol, and 102.5 parts of ethyl acetate were charged into a four-neck flask, heated to 100°C, and stirred until the solution became homogeneous. 65 parts of aromatic polyisocyanate adduct (a1-1) was added in solid form, and the reaction was carried out at 80°C for 4 hours. After the reaction was completed, the non-volatile content was adjusted to 50% with ethyl acetate and the mixture was taken out. The obtained polyisocyanate (A-1) had an NCO% of 5.6% in solid form, and a content of the partial structure represented by general formula (1) of 0.0% by mass.
[0088] (Polyisocyanates (A-2) to (A-22)) Except for changing the blending amounts shown in Table 2, polyol and polyisocyanate were reacted in the same manner as for polyisocyanate (A-1), and polyisocyanates (A-2) to (A-22) were obtained in which the non-volatile content was adjusted to 50% with ethyl acetate.
[0089] [Table 2]
[0090] The abbreviations in Table 2 are as follows. 1,4-BD: 1,4-butanediol NPG: Neopentyl glycol
[0091] <<Production of Polyol (B)>> <Synthesis of polyester polyol (b1)> (Polyester polyols (b1-1) to (b1-8)) Polyester polyols (b1-1) to (b1-8) were obtained by reacting polybasic acids and polyhydric alcohols in the same manner as for polyester polyol (a2-1), except that the amounts of each component were changed so that the mole percentages of each component when the total of the polybasic acid and polyhydric alcohol was 200 mole % were as shown in Table 2-2.
[0092] The composition ratio (mass %) and composition ratio (mol %) of the obtained polyester polyol (b1) are shown in Tables 3-1 and 3-2.
[0093] [Table 3-1]
[0094] [Table 3-2]
[0095] <Preparation of Polyol (B)> (Polyols (B-1) to (B-16)) Polyester polyol (b1), hydroxyl group-containing epoxy resin (b2), and ethyl acetate as a solvent were mixed and dissolved in the amounts shown in Table 4, and the non-volatile content was adjusted to 50%, thereby obtaining polyols (B-1) to (B-16).
[0096] [Table 4]
[0097] The abbreviations in Table 4 are as follows. NPEL-134: Bisphenol A type epoxy resin (manufactured by NANYA PLASTICS, epoxy equivalent 230~270) jER152: Phenol novolac type multifunctional epoxy resin (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 178)
[0098] <Manufacture of adhesives for packaging materials for power storage devices> [Example 1] 100 parts of a 50% non-volatile solution of polyisocyanate (A-1), 36 parts of a 50% non-volatile solution of polyol (B-3), 1.0 part of glycidopropyltrimethoxysilane (Si coupling agent) as an additive, 0.010 parts of dibutyltin dilaurate (DBTDL) as a catalyst, and ethyl acetate were adjusted to a solids concentration of 30%, and stirred for 10 minutes to obtain an adhesive.
[0099] [Examples 2 to 38, Comparative Examples 1 to 7] An adhesive with a solids concentration of 30% was obtained in the same manner as in Example 1, except that the polyisocyanate (A), polyol (B), Si coupling agent, and catalyst type and amount were changed to those shown in Tables 5 and 6.
[0100] <Evaluation of adhesives for packaging materials for power storage devices> The obtained adhesive was used to manufacture packaging materials, which were then subjected to the following evaluations. The results are shown in Tables 5 and 6.
[0101] [Manufacturing of packaging materials] The adhesive obtained above was applied to one side of an aluminum foil having a thickness of 40 μm using a dry laminator for use as an outer adhesive layer. After the solvent was evaporated, a stretched polyamide film having a thickness of 30 μm was laminated thereon to obtain an intermediate laminate. The amount of the adhesive applied after drying was 3 g / m. 2 Next, an adhesive for the inner layer side adhesive layer, which will be described later, was applied to the other side of the aluminum foil of the obtained intermediate laminate using a dry laminator. After the solvent was evaporated, a 30 μm-thick unstretched polypropylene film was laminated to obtain a laminate. The amount of the adhesive applied after drying was 4 g / m 2 It was decided. Next, the laminate was aged for 2 and 4 days under conditions of 40°C and 60% RH (relative humidity) to harden the adhesive layers on the outer and inner layers, thereby obtaining a packaging material having a configuration of outer resin film layer / outer adhesive layer / metal foil layer / inner adhesive layer / heat seal layer.
[0102] <<Adhesive for inner adhesive layer>> AD-502 (product name, polyester polyol, manufactured by Toyo-Morton Co., Ltd.) was used as the base agent, and CAT-10L (product name, isocyanate-based curing agent, manufactured by Toyo-Morton Co., Ltd.) was used as the curing agent, mixed at a base agent / curing agent ratio of 100 / 10 (mass ratio) and adjusted to a solids concentration of 30% with ethyl acetate, and used as the adhesive for the inner adhesive layer.
[0103] [Laminate strength] The packaging materials aged for 2 days at 40°C, 60% RH were each cut into pieces of 200 mm x 15 mm, and a T-peel test was performed using a tensile tester to measure the peel strength (N / 15 mm width) between the stretched polyamide film and the aluminum foil. The measurement was performed in an environment of 20°C, 65% RH, with a loading speed of 300 mm / min, and the average value of five test pieces was used to evaluate according to the following criteria. S: Average peel strength is 7N or more (very good) A: Average peel strength is 4N or more and less than 7N (good) B: Average peel strength is 2N or more and less than 4N (usable) C: Average peel strength is less than 2N (unusable)
[0104] [Moldability] The packaging material aged for 2 days at 40°C and 60% RH, and the packaging material aged for 4 days under the same environment were each cut to a size of 80 x 80 mm, and with the stretched polyamide film facing outward, they were molded into a one-stage overhang using a straight mold with a free molding height. The maximum molding height at which the aluminum foil did not break or the layers did not float was determined, and moldability was evaluated according to the following criteria. The punch shape of the mold used was a square with sides of 30 mm, a corner R of 2 mm, and a punch shoulder R of 1 mm.The die hole shape of the mold used was a square with sides of 34 mm, a die hole corner R of 2 mm, and a die hole shoulder R of 1 mm.The clearance between the punch and the die hole was 2 mm on each side, and this clearance caused a slope according to the molding height. S: The maximum molding height is 6 mm or more (very good) A: The maximum molding height is 4 mm or more and less than 6 mm (good). B: The maximum molding height is 2 mm or more and less than 4 mm (usable). C: The maximum molding height is less than 2 mm (unusable)
[0105] [Moisture and heat resistance] The packaging materials aged for 2 days at 40°C and 60% RH were each cut to a size of 80 x 80 mm, and molded into one stage with a free molding height straight mold with the stretched polyamide film on the outside, with a molding height of 3 mm, to obtain a molded product. The molded product was then placed in a thermo-hygrostat under an atmosphere of 85°C and 85% RH and left to stand for 168 hours, after which it was removed from the thermo-hygrostat and visually inspected for any floating and evaluated according to the following criteria. The punch shape of the mold used was a square with sides of 30 mm, a corner R of 2 mm, and a punch shoulder R of 1 mm, and the die hole shape of the mold used was a square with sides of 34 mm, a die hole corner R of 2 mm, and a die hole shoulder R of 1 mm. S: No floating (very good) A: One of the four sides is lifted (good) B: Two of the four sides are loose (usable) C: Three or more of the four sides are raised (unusable)
[0106] [Table 5]
[0107] [Table 6]
[0108] According to Tables 5 and 6, the adhesive of the present invention, in which the polyol (B) contains a polyester polyol (b1), is 20 to 60% by mass relative to the polyisocyanate (A), and further contains 0.5 to 12.0% by mass of a partial structure represented by the general formula (1), has a coating amount of the adhesive of 3 g / m 2 Even when the curing time was shortened to two days, the adhesive exhibited high adhesion and flexibility, and was able to achieve both excellent moldability and long-term durability under high temperature and humidity conditions. In particular, those containing the hydroxyl group-containing epoxy resin (b2) in the range of 5 to 50% by mass relative to the polyol (B) were excellent in lamination strength and moist heat resistance. Moreover, the use of bisphenol A type epoxy resin as the hydroxyl group-containing epoxy resin (b2) was excellent in lamination strength and moldability.
[0109] On the other hand, since Comparative Example 1 does not have the partial structure represented by general formula (1), the curing reaction does not proceed sufficiently, and when the amount of adhesive applied is reduced and the curing period is shortened to two days, the laminate strength and moldability cannot be satisfied. Comparative Examples 5 and 6 correspond to examples of JP 2018-110086 A, and do not have the partial structure represented by general formula (1) like Comparative Example 1. Therefore, when the amount of adhesive applied is reduced and the curing period is shortened to 2 days, the curing reaction does not proceed sufficiently, and satisfactory adhesive performance cannot be achieved. In Comparative Example 2, in which the amount of the partial structure represented by general formula (1) exceeds 12.0 mass%, the affinity with water is too high, so that the material is prone to trap moisture in the air and cannot obtain satisfactory moist heat resistance. In Comparative Example 3, in which the amount of polyol (B) is less than 20%, the adhesive layer becomes too rigid, and therefore both the adhesive strength and moldability cannot be achieved. In Comparative Example 4, in which the amount of polyol (B) exceeds 60%, the urethane concentration in the adhesive layer decreases, and the cohesive strength of the adhesive decreases. In addition, the affinity with the substrate also decreases, and therefore the adhesive strength and moist heat resistance cannot be satisfied. Comparative Example 7 contains a hydroxyl group-containing epoxy resin (b2) but does not contain a polyester polyol (b1), and therefore the flexibility of the adhesive layer is reduced. Therefore, when the amount of adhesive applied is reduced and the curing period is shortened to two days, it is not possible to achieve both moldability and the moist heat resistance of the molded product. [Explanation of symbols]
[0110] (1): Outer resin film layer (2):Outer adhesive layer (3):Metal foil layer (4): Inner layer adhesive layer (5): Heat seal layer
Claims
1. An adhesive for packaging materials for electric storage devices, comprising a polyisocyanate (A) and a polyol (B), The polyol (B) contains a polyester polyol (b1), The polyol (B) is contained in an amount of 20 to 60% by mass based on the mass of the polyisocyanate (A), An adhesive for packaging materials for electrical storage devices, comprising a partial structure represented by the following general formula (1) in an amount of 0.5 to 12.0 mass % based on the solid content mass of the adhesive: General formula (1) 【Chemistry 1】 [In general formula (1), R represents a hydrogen atom or a methyl group, and n represents an integer of 2 to 20.]
2. The adhesive for packaging materials for electric storage devices according to claim 1 , wherein the polyisocyanate (A) comprises a reaction product of a polyisocyanate and a polyol including a polyester polyol (a2).
3. 2. The adhesive for packaging materials for electric storage devices according to claim 1, wherein the polyisocyanate (A) comprises a reaction product of a polyisocyanate including an adduct (a1) of an aromatic polyisocyanate and a polyol including a polyester polyol (a2).
4. The adhesive for packaging materials for electric storage devices according to claim 2 or 3, wherein the polyhydric alcohol which is a component of the polyester polyol (a2) contains 5 to 30 mol % of a polyhydric alcohol having a partial structure represented by general formula (1) based on 100 mol % of the polyhydric alcohol.
5. The adhesive for use in packaging materials for electric storage devices according to any one of claims 1 to 3, wherein the polyol (B) further contains a hydroxyl group-containing epoxy resin (b2) in an amount of 5 to 50 mass% based on the mass of the polyol (B).
6. The adhesive for packaging materials for electric storage devices according to claim 5 , wherein the hydroxyl group-containing epoxy resin (b2) is a bisphenol A type epoxy resin.
7. A packaging material for an electricity storage device, comprising at least an outer layer resin film layer, an outer layer adhesive layer, a metal foil layer, an inner layer adhesive layer, and a heat seal layer laminated in this order, The packaging material for an electricity storage device, wherein the outer adhesive layer is a cured product of the adhesive for use in packaging materials for electricity storage devices according to any one of claims 1 to 3.
8. 8. A container for an electricity storage device formed from the electricity storage device packaging material according to claim 7, wherein the outer resin film layer forms a convex surface and the heat seal layer forms a concave surface.
9. An electricity storage device comprising the electricity storage device container according to claim 8 .
Citation Information
Patent Citations
Polyisocyanate curing agent and polyurethane coating composition and polyurethane adhesive composition using the same
JP1994199987A
Packing material for electronic parts
JP2002187233A
Packing material for battery case and battery case molded with packing material
JP2005063685A
Covering material for lithium ion battery
JP2011187385A
Laminated film
JP2019188658A