Resin composite material and molded article of the same
By formulating resin composite materials with specific columnar pellet ratios and shapes, the issue of weight variation in molded products is resolved, ensuring consistent and reduced weight fluctuations.
Patent Information
- Application Number
- JP2023087162
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
AI Technical Summary
Conventional resin composite materials using multiple types of pellets result in significant weight variations in molded products, which is undesirable for consistent manufacturing.
A resin composite material composed of columnar pellets with specific gravity, length, and cross-sectional shape ratios, including thermoplastic resins and fibrous fillers, adhering to formulas (I) to (VI) to minimize weight variations.
The solution achieves molded products with weight variations reduced to less than 1.0%, suitable for industrial applications such as automobiles and electronic devices.
Smart Images

Figure 2024170157000001 
Figure 2024170157000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composite material and a molded article thereof. [Background technology]
[0002] Conventionally, a method for obtaining a molded product with an adjusted fiber content by using a resin composite material obtained by mixing pellets of a fiber-containing thermoplastic resin and pellets containing a thermoplastic resin has been known. For example, Patent Document 1 proposes a pellet mixture in which two types of fiber-containing resin pellets with different fiber contents are mixed, and the average fiber content of the mixed raw material and the pellet length of the two types of pellets are controlled within a certain range. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 06-23745 Summary of the Invention [Problem to be solved by the invention]
[0004] However, resin composite materials containing two or more types of pellets may produce molded products with varying weights. Therefore, an object of the present disclosure is to provide a resin composite material that produces molded products with small weight variations, and a molded product with small weight variations. [Means for solving the problem]
[0005] The present disclosure has the following aspects. [1] A resin composite material, The resin composite material is A cylindrical pellet (A) containing a thermoplastic resin (a1) and a fibrous filler (a2); and columnar pellets (B) containing a thermoplastic resin (b1), The cylindrical pellets (A) and (B) have a cylindrical shape other than a triangular cross-sectional shape or a rectangular cross-sectional shape, A resin composite material satisfying all of the following formulas (I) to (V): 0≦|SG A -SG B |≦0.50 (I) 1.0≦F B / F A ≦4.0 (II) 0.8≦L B / L A ≦1.5 (III) 0.6≦LD B / LD A ≦1.2 (IV) 0.6≦SD B / SD A ≦1.2 (V) (In formula (I), SG A represents the specific gravity of the cylindrical pellet (A), and SG B represents the specific gravity of the cylindrical pellets (B). In formula (II), F A represents the proportion (mass%) of the columnar pellets (A) in the resin composite material, and F B represents the proportion (mass %) of the columnar pellets (B) in the resin composite material. In formula (III), L A represents the length (mm) of the cylindrical pellet (A), and L B represents the length (mm) of the cylindrical pellet (B). In formula (IV), L-D A represents the major axis (mm) of the cross section of the cylindrical pellet (A), and LD B represents the major axis (mm) of the cross section of the columnar pellet (B). In formula (V), SD A represents the minor axis (mm) of the cross section of the cylindrical pellet (A), and SD B represents the minor axis (mm) of the cross section of the cylindrical pellet (B). [2] The resin composite material according to [1], wherein the thermoplastic resins (a1) and (b1) are at least one thermoplastic resin selected from the group consisting of polyamide resins, polyolefin resins, polystyrene resins, polycarbonate resins, polyester resins, polyacetal resins, polyarylene ether resins, polyarylene sulfide resins, polysulfone resins, polyarylene ether ketone resins, and liquid crystalline resins. [3] The resin composite material according to [1] or [2], wherein the thermoplastic resins (a1) and (b1) are at least one thermoplastic resin selected from the group consisting of polyamide 6 resin, polyamide 12 resin, polyamide 66 resin, polyamide 610 resin, polyamide 1010 resin, polyamide 6T resin, polyamide 9T resin, polyethylene resin, polypropylene resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyacetal copolymer, polyphenylene sulfide resin, polyether ether ketone resin, polyether ketone resin, liquid crystalline polyester resin, and liquid crystalline polyester amide resin. [4] The resin composite material according to any one of [1] to [3], wherein the thermoplastic resins (a1) and (b1) are the same thermoplastic resin. [5] The resin composite material according to any one of [1] to [4], further satisfying the following formula (VI): 50≦(F A +F B ) (VI) [6] The resin composite according to any one of [1] to [5], wherein the total amount of fillers, including the fibrous filler (a2), contained in the resin composite is 5 mass% or more relative to the total mass of the resin composite. [7] A molded product made of a resin composite material described in any one of [1] to [6]. Effect of the Invention
[0006] According to the present disclosure, it is possible to provide a resin composite material that can give a molded product with little weight variation, and a molded product with little weight variation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, an embodiment of the present disclosure will be described in detail, but the scope of the present disclosure is not limited to the embodiment described here, and various modifications can be made within the scope of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. In addition, when multiple upper and lower limit values are described for a specific parameter, any upper and lower limit values among these upper and lower limit values can be combined to form a suitable numerical range. In addition, the lower and / or upper limit values of the numerical range described in this disclosure are numerical values within the numerical range and may be replaced with numerical values shown in the examples. The expression "X to Y" indicating a numerical range means "X or more and Y or less". When a specific description described for one embodiment is also applicable to other embodiments, the description may be omitted in other embodiments. Each configuration and combination thereof in each embodiment is merely an example, and addition, omission, substitution, and other modifications of the configuration are possible as appropriate within the scope of the present disclosure. The present disclosure is not limited to the embodiments, but is limited only by the claims. Each feature disclosed herein may be combined with any other feature disclosed herein.
[0008] [Resin composite material] The present embodiment relates to a resin composite material comprising columnar pellets (A) containing a thermoplastic resin (a1) and a fibrous filler (a2), and columnar pellets (B) containing a thermoplastic resin (b1), wherein the columnar pellets (A) and (B) have a columnar shape other than a triangular cross-sectional shape or a rectangular cross-sectional shape, and satisfy all of the following formulas (I) to (V). 0≦|SG A -SG B |≦0.50 (I) 1.0≦F B / F A ≦4.0 (II) 0.8≦L B / L A≦1.5 (III) 0.6≦LD B / LD A ≦1.2 (IV) 0.6≦SD B / SD A ≦1.2 (V) (In formula (I), SG A represents the specific gravity of the cylindrical pellet (A), and SG B represents the specific gravity of the cylindrical pellets (B). In formula (II), F A represents the proportion (mass%) of the columnar pellets (A) in the resin composite material, and F B represents the proportion (mass %) of the columnar pellets (B) in the resin composite material. In formula (III), L A represents the length (mm) of the cylindrical pellet (A), and L B represents the length (mm) of the cylindrical pellet (B). In formula (IV), L-D A represents the major axis (mm) of the cross section of the cylindrical pellet (A), and LD B represents the major axis (mm) of the cross section of the columnar pellet (B). In formula (V), SD A represents the minor axis (mm) of the cross section of the cylindrical pellet (A), and SD B represents the minor axis (mm) of the cross section of the cylindrical pellet (B). According to the resin composite material according to this embodiment, a molded product with small variation in weight can be obtained.
[0009] <Columnar pellets (A) and columnar pellets (B)> The resin composite material according to the present embodiment includes columnar pellets (A) containing a thermoplastic resin (a1) and a fibrous filler (a2), and columnar pellets (B) containing a thermoplastic resin (b1). Here, the term "columnar pellet" refers to a pellet having a shape similar to a column (a shape in which the length is greater than the width). The columnar pellets (A) and (B) are pellets having the same cross-sectional shape on one side and the same cross-sectional shape on the other side. In this specification, the "cross-sectional shape of the columnar pellet" refers to the cross-sectional shape when the columnar pellet is cut perpendicular to the length direction of the columnar pellet. Hereinafter, the cross-section on one side of the columnar pellets (A) and (B) will be described as "one end face" and the cross-section on the other side will be described as "the other end face".
[0010] The columnar pellets (A) and (B) according to this embodiment have a columnar shape other than a triangular column or a quadrangular column. A "triangular column" refers to a columnar shape in which one end face and the other end face have a triangular shape. A "quadrilateral column" refers to a columnar shape in which one end face and the other end face have a quadrangular shape (e.g., a rectangle, a square, a trapezoid, a rhombus, etc.). The area of one end face and the area of the other end face of the columnar pellets (A) and (B) may be the same or different, but from the viewpoint of easily obtaining molded products with smaller weight variation, it is preferable that the areas of the one end face and the other end face are the same.
[0011] In one embodiment, the cylindrical pellets (A) and (B) preferably have one end face and the other end face having a shape such as a circle, an ellipse, an oval, or a gourd shape, and more preferably a circle, an ellipse, or an oval. The term "gourd shape" refers to a shape in which two circles (which may be ellipses or ovals) are joined at a part of their circumference. Examples of cylindrical pellets having one end face and the other end face having the above shape include a cylinder, an elliptical cylinder, an oval cylinder, and a gourd-shaped cylinder (a structure in which two cylinders, elliptical cylinders, or oval cylinders are fused along the length direction). In one embodiment, the shape of one side and / or the shape of the other side of the cylindrical pellets (A) and (B) may be a sphere, an ellipsoid, or a three-dimensional irregular shape modified therefrom. Three-dimensional amorphous objects that are deformed from spheres or oval spheres include objects that have a concave, convex, or uneven surface on at least a part of the sphere or oval sphere, objects in which a part (including multiple parts) of the sphere or oval sphere has been cut, or objects that have both (objects in which a part of the sphere or oval sphere has been cut and which have a concave, convex, or uneven surface on at least a part).
[0012] In one embodiment, the shapes of the cylindrical pellets (A) and (B) may be the same or different. From the viewpoint of uniforming the contact points of the cylindrical pellets (A) and (B), it is preferable that they are the same, and it is more preferable that both the cylindrical pellets (A) and (B) have a cylindrical and / or elliptical cylindrical shape.
[0013] In the resin composite material according to this embodiment, the columnar pellets (A) and (B) satisfy all of the following formulae (I) to (V). 0≦|SG A -SG B |≦0.50 (I) 1.0≦F B / F A ≦4.0 (II) 0.8≦L B / L A ≦1.5 (III) 0.6≦LD B / LD A ≦1.2 (IV) 0.6≦SD B / SD A ≦1.2 (V) (In formula (I), SG A represents the specific gravity of the cylindrical pellet (A), and SG B represents the specific gravity of the cylindrical pellets (B). In formula (II), F A represents the proportion (mass%) of the columnar pellets (A) in the resin composite material, and F B represents the proportion (mass %) of the columnar pellets (B) in the resin composite material. In formula (III), L A represents the length (mm) of the cylindrical pellet (A), and L Brepresents the length (mm) of the cylindrical pellet (B). In formula (IV), L-D A represents the major axis (mm) of the cross section of the cylindrical pellet (A), and LD B represents the major axis (mm) of the cross section of the columnar pellet (B). In formula (V), SD A represents the minor axis (mm) of the cross section of the cylindrical pellet (A), and SD B represents the minor axis (mm) of the cross section of the cylindrical pellet (B).
[0014] Formula (I) Formula (I) represents the absolute value of the specific gravity difference between the cylindrical pellets (A) and (B). A -SG B is 0 to 0.50, preferably 0.10 to 0.50, more preferably 0.14 to 0.50, and further preferably 0.14 to 0.44. A ) and the specific gravity of the resin pellet (B) (SG B ) is measured in accordance with JIS K7112 using a measuring device (for example, product name "SD-120L" manufactured by Kensei Kogyo Co., Ltd.) to measure the specific gravity of 15 resin pellets by the water displacement method, and the average value is used. Formula (I) is easily achieved, for example, when columnar pellets containing a thermoplastic resin described below and glass fibers are used as columnar pellets (A), and columnar pellets containing a thermoplastic resin described below but not containing a fibrous filler are used as columnar pellets (B).
[0015] ·Formula (II) Formula (II) represents the mixing ratio (mass%) of the columnar pellets (A) to the mixing ratio (mass%) of the columnar pellets (B) in the resin composite material. B / F A is 1.0 to 4.0. That is, the resin composite material according to this embodiment contains 1.0 to 4.0 times as many columnar pellets (B) as the columnar pellets (A). In one embodiment, F B / F Amay be 1.0 to 2.3, or may be 2.3 to 4.0.
[0016] In one embodiment, the ratio of the cylindrical pellets (A) to the total mass of the resin composite (F A ) is preferably 20 to 90 mass%, more preferably 20 to 80 mass%, further preferably 20 to 50 mass%, particularly preferably 30 to 50 mass%. In addition, the ratio of the columnar pellets (B) to the total mass of the resin composite material (F B ) is preferably 20 to 90 mass%, more preferably 20 to 80 mass%, further preferably 50 to 80 mass%, particularly preferably 50 to 70 mass%. A and F B The above preferred ratios can be arbitrarily combined within the range satisfying formula (II).
[0017] ·Formula (III) L in formula (III) B / L A is 0.8 to 1.5, may be 0.8 to 1.0, or may be 1.0 to 1.4. The length (L) of the columnar pellets (A) and (B) refers to the length (mm) from the center of gravity of one end face of the columnar pellet to the center of gravity of the other end face. When the columnar pellets (A) and (B) are the above-mentioned three-dimensional indefinite object, the length of the longest part is taken as "L". The length (L) of the columnar pellets (A) and (B) is calculated by measuring the lengths of 15 resin pellets using a caliper, calculating the average value, and rounding off the first decimal place to the nearest tenth place. In one embodiment, L A is preferably 3 to 20 mm, more preferably 6 to 15 mm, and particularly preferably 9 to 11 mm. B is preferably 3 to 20 mm, more preferably 6 to 15 mm, and particularly preferably 9 to 13 mm. A and L B can be any combination of the above preferred values within a range satisfying formula (III).
[0018] ·Formula (IV) LD in formula (IV)B / LD A is 0.6 to 1.2, may be 0.7 to 1.2, or may be 0.8 to 1.2. The LD (long diameter at the end face) of the columnar pellets (A) and (B) refers to the longest diameter passing through the center of gravity at one end face or the other end face of the columnar pellets (A) and (B). That is, when the columnar pellets (A) and (B) are pellets having different areas at one end face and the other end face, the longest of the long diameters at the one end face or the other end face is taken as the long diameter (LD). The LD of the columnar pellets (A) and (B) is calculated by measuring the long diameters of 15 resin pellets, calculating the average value, and rounding off to one decimal place to the nearest decimal place. In one embodiment, LD A is preferably 1.0 to 4.0 mm, more preferably 2.0 to 4.0 mm, and particularly preferably 2.5 to 3.2 mm. B is preferably 1.0 to 4.0 mm, more preferably 1.5 to 3.5 mm, and particularly preferably 1.8 to 3.2 mm. A and L.D. B can be any combination of the above preferred values within a range satisfying formula (IV).
[0019] ·Formula (V) SD in formula (V) B / LD A is 0.6 to 1.2, may be 0.7 to 1.2, or may be 0.8 to 1.2. The SD (minor diameter at the end face) of the columnar pellets (A) and (B) refers to the shortest diameter passing through the center of gravity at one end face or the other end face of the columnar pellets (A) and (B). That is, when the columnar pellets (A) and (B) are pellets having different areas at one end face and the other end face, the shortest of the minor diameters at the one end face or the other end face is taken as the minor diameter (SD). The SD of the columnar pellets (A) and (B) is calculated by measuring the minor diameters of 15 resin pellets, calculating the average value, and rounding off to one decimal place to the nearest decimal place. In one embodiment, SD Ais preferably 1.0 to 4.0 mm, more preferably 1.5 to 3.0 mm, and particularly preferably 1.7 to 2.5 mm. B The SD is preferably from 1.0 to 4.0 mm, more preferably from 1.5 to 3.5 mm, and particularly preferably from 1.8 to 3.2 mm. A and S.D. B can be any combination of the above preferred values within a range satisfying formula (V).
[0020] The resin composite material according to this embodiment satisfies all of the above-mentioned formulas (I) to (V), and thus makes it possible to obtain a molded product with small variation in weight.
[0021] In one embodiment, the resin composite preferably satisfies the following formula (VI). 50≦(F A +F B ) (VI) That is, the total amount of the columnar pellets (A) and (B) relative to the total mass of the resin composite material (F A +F B ) is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. A +F B ) may be 100% by mass. That is, (F A +F B ) is 50≦(F A +F B )≦100. By blending the columnar pellets (A) and (B) so as to satisfy the formulas (I) to (V) and the formula (IV), a molded product having a small variation in weight can be more easily obtained.
[0022] In one embodiment, when one end face of the cylindrical pellet (A) or (B) is elliptical, the ratio (LD / SD) of the major axis (LD) to the minor axis (SD) of the ellipse may be 1.1 to 1.6, 1.2 to 1.6, or 1.2 to 1.5, from the viewpoint of more easily obtaining molded products with less weight variation.
[0023] In one embodiment, the pellet length (L A ) and major axis (LD A ) and the ratio (L A / LD A ) may be 3.0 to 5.0, 3.4 to 5.0, or 3.4 to 4.5. In addition, the pellet length (L B ) and major axis (LD B ) and the ratio (L B / LD B ) may be 2.5 to 6.5, or may be 3.0 to 6.2.
[0024] (Thermoplastic resins (a1) and (b1)) The thermoplastic resins (a1) and (b1) contained in the columnar pellets (A) and (B) are preferably at least one thermoplastic resin selected from the group consisting of polyamide resin, polyolefin resin, polystyrene resin, polycarbonate resin, polyester resin, polyacetal resin, polyarylene ether resin, polyarylene sulfide resin, polysulfone resin, polyarylene ether ketone resin, and liquid crystalline resin.
[0025] Polyamide resin Examples of polyamide resins include aliphatic polyamide resins (polyamide 46 resin, polyamide 6 resin, polyamide 11 resin, polyamide 12 resin, polyamide 66 resin, polyamide 610 resin, polyamide 612 resin, polyamide 1010 resin, etc.); aromatic polyamide resins [polyamide resins obtained by reacting aromatic dicarboxylic acids (terephthalic acid, etc.) with aliphatic diamines (hexamethylenediamine, etc.), polyamide resins obtained by reacting aliphatic dicarboxylic acids (adipic acid, etc.) with aromatic diamines (metaxylylenediamine, paraxylylenediamine, etc.). For example, polyamide 6T resin, polyamide 9T resin, etc.]; and homopolymers or copolymers of lactams (ε-caprolactam, etc.). These may be used alone or in combination of two or more. The polyamide resin may be not only a homopolyamide resin but also a copolyamide resin. Of these, polyamide 6 resin, polyamide 12 resin, polyamide 66 resin, polyamide 610 resin, polyamide 1010 resin, polyamide 6T resin, or polyamide 9T resin is preferred, and polyamide 6 resin or polyamide 66 resin is more preferred.
[0026] Polyolefin resin The polyolefin resin is preferably, for example, a homopolymer of an olefin having 2 to 6 carbon atoms or a copolymer of an olefin having 2 to 6 carbon atoms, and more preferably a polyethylene resin or a polypropylene resin. The polypropylene resin may be a homopolypropylene resin, a block polypropylene resin, a random polypropylene resin, or a mixture thereof.
[0027] Polyester resin Examples of polyester resins include homopolyester resins or copolyester resins having repeating units of alkylene terephthalate (ethylene terephthalate, butylene terephthalate, etc.) or alkylene naphthalate (ethylene naphthalate, butylene naphthalate, etc.) (copolyesters having copolymerized components of aliphatic dicarboxylic acids having 6 to 12 carbon atoms such as adipic acid, asymmetric aromatic dicarboxylic acids such as phthalic acid and isophthalic acid, and alkylene glycols having 2 to 6 carbon atoms, polyoxyalkylene glycols, bisphenol A, etc.); aromatic polyesters (polyarylate-based resins produced by the reaction of aromatic diols such as bisphenol A with aromatic dicarboxylic acids such as terephthalic acid); and homopolyesters or copolymers of lactones (ε-caprolactone, etc.). These may be used alone or in combination of two or more. Among these, polyethylene terephthalate resins and polybutylene terephthalate resins are more preferable.
[0028] Polyacetal resin Examples of polyacetal resins include polyacetal homopolymers having only oxymethylene groups as constituent units, and polyacetal copolymers having oxyethylene groups and other constituent units in addition to oxymethylene groups. These may be used alone or in combination of two or more. Among these, polyacetal copolymers are preferred.
[0029] Polyarylene ether resin The polyarylene ether resin may be, for example, a polyphenylene ether resin, etc. The polyarylene ether resin may be used alone or in combination of two or more kinds.
[0030] Polyarylene sulfide resin Examples of polyarylene sulfide resins include polyphenylene sulfide resins, polyphenylene sulfide ketone resins, polybiphenylene sulfide resins, and polyphenylene sulfide sulfone resins. These may be used alone or in combination of two or more. Among these, polyphenylene sulfide resins are preferred.
[0031] Polysulfone resin Examples of polysulfone resins include polysulfone resins, polyethersulfone resins, polyphenylsulfone, etc. These may be used alone or in combination of two or more. Among these, polyethersulfone resins are preferred.
[0032] Polyarylene ether ketone resin Examples of polyarylene ether ketone resins include polyether ether ketone resins, polyether ketone resins, polyether ketone ketone resins, polyether ketone ether ketone ketone resins, and the like. These may be used alone or in combination of two or more. Among these, polyether ether ketone resins and polyether ketone resins are preferred.
[0033] Liquid crystal resin As the liquid crystal resin, liquid crystal polyester resin and liquid crystal polyester amide are preferable. These may be used alone or in combination of two or more. Particularly preferable is aromatic polyester or aromatic polyester amide having repeating units derived from one or more aromatic hydroxycarboxylic acids and their derivatives as a constituent.
[0034] In one embodiment, the thermoplastic resins (a1) and (b1) are preferably at least one thermoplastic resin selected from the group consisting of polyamide 6 resin, polyamide 12 resin, polyamide 66 resin, polyamide 610 resin, polyamide 1010 resin, polyamide 6T resin, polyamide 9T resin, polyethylene resin, polypropylene resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyacetal copolymer, polyphenylene sulfide resin, polyether ether ketone resin, polyether ketone resin, liquid crystal polyester resin, and liquid crystal polyester amide resin, and more preferably at least one thermoplastic resin selected from the group consisting of polyamide 6 resin, polyamide 66 resin, polyamide 1010 resin, polyamide 9T resin, polypropylene resin, polybutylene terephthalate resin, polyacetal copolymer, polyphenylene sulfide resin, liquid crystal polyester resin, and liquid crystal polyester amide resin. If the thermoplastic resins (a1) and (b1) are at least one of these thermoplastic resins, it is easier to satisfy the formula (I).
[0035] The thermoplastic resins (a1) and (b1) may be the same thermoplastic resin or may be different. From the viewpoint of easily obtaining a molded product with a smaller variation in weight, it is preferable that the thermoplastic resins (a1) and (b1) are the same thermoplastic resin, and it is more preferable that the thermoplastic resins (a1) and (b1) are both polyolefin resins. Here, the "same thermoplastic resin" includes those in which the monomer units constituting the thermoplastic resin are the same but the physical properties such as molecular weight are different. For example, when the thermoplastic resin (a1) is a polypropylene resin, the thermoplastic resin (b1) may also be a polypropylene resin. However, the average molecular weights (Mw and / or Mn) of these polypropylene resins may be different or the same. In addition, the thermoplastic resin (a1) may be a homopolypropylene resin, and the thermoplastic resin (b1) may be a block polypropylene resin.
[0036] (Fiber filler (a2)) The columnar pellet (A) contains a fibrous filler (a2). As the fibrous filler (a2), a conventionally known filler that is blended in a fiber-containing resin composition can be used. Specifically, glass fiber, carbon fiber, cellulose fiber, silicon carbide fiber, alumina fiber, silicon carbide whisker, silicon nitride whisker, potassium titanate whisker, wollastonite, metal fiber, etc. can be mentioned. Among these, from the viewpoint of easily achieving the above-mentioned formula (I), it is preferable to contain a fibrous filler having a specific gravity of less than 4.0, more preferably to contain glass fiber, carbon fiber, or cellulose fiber, even more preferably to contain glass fiber, and particularly preferably to contain long glass fiber.
[0037] In one embodiment, when the fibrous filler (a2) (hereinafter sometimes referred to as "filler (a2)") contains glass fibers, the average fiber diameter of the glass fibers is preferably 5 to 30 μm, more preferably 10 to 20 μm, from the viewpoints of the mechanical properties of the resulting molded article and the ease of handling during processing. The average fiber diameter of the glass fibers refers to the average value of the fiber diameters of 300 glass fibers measured by a method such as electron microscope observation.
[0038] In one embodiment, the ratio of the filler (a2) in the cylindrical pellets (A) is preferably 20 to 60 mass%, more preferably 20 to 50 mass%, based on the total mass of the cylindrical pellets (A). By setting the ratio of the filler (a2) in the cylindrical pellets (A) within the above range, the resulting resin composite material is more likely to satisfy formula (I). In addition, a molded product with small weight variation is more likely to be obtained.
[0039] In one embodiment, the columnar pellet (A) may be a pellet (resin-impregnated fiber bundle) obtained by impregnating a fiber bundle of a filler (a2) (preferably glass fiber) aligned in the length direction with a thermoplastic resin (a1) to integrate the fiber bundle. In this case, the number of the filler (a2) in the resin-impregnated fiber bundle is adjusted within the range satisfying the above-mentioned formulas (I) to (V), and is preferably 1,000 to 30,000, more preferably 1,000 to 24,000, and particularly preferably 2,000 to 12,000.
[0040] The columnar pellets (A), which are resin-impregnated fiber bundles, can be produced by a known production method using a die. Specifically, they may be produced by the production methods described in JP-A-6-293023 and JP-A-2013-107979.
[0041] The columnar pellets (A) may contain known resin additives other than the thermoplastic resin (a1) and the filler (a2). Examples of resin additives include granular or plate-like fillers, pigments, colorants (including color concentrates), flame retardants, heat, light and ultraviolet stabilizers, compatibilizers, lubricants, foaming agents, antibacterial agents, etc. These may be contained alone or in combination of two or more. Among these, it is more preferable to contain a lubricant and a colorant from the viewpoint of enabling fine adjustments at the molding site and expanding the range of molding conditions.
[0042] In one embodiment, the cylindrical pellets (B) may contain only the thermoplastic resin (b1), or may contain a filler (hereinafter referred to as "filler (b2)") or the above-mentioned resin additives. The cylindrical pellets (B) may be blended as a diluent to adjust the fiber content of the cylindrical pellets (A).
[0043] (Filling material (b2)) In one embodiment, when the columnar pellets (B) contain a filler (b2), the filler (b2) preferably contains at least one filler selected from a fibrous filler, a plate-like filler, and a granular filler. Examples of the fibrous filler include the same as those of the above-mentioned filler (a2), and preferred examples are also the same. Examples of the plate-like filler include talc, mica, glass flakes, graphite, and various metal foils (e.g., aluminum foil, iron foil, copper foil). These may be used alone or in combination of two or more. Among these, talc and glass flakes are preferred. Examples of the granular filler include glass beads, silica, alumina, etc. These may be used alone or in combination of two or more. Among these, glass beads and silica are preferred.
[0044] When the columnar pellets (B) contain a filler (b2), the proportion of the filler (b2) relative to the total mass of the columnar pellets (B) is preferably 0 to 20 mass%, more preferably 0 to 10 mass%, from the viewpoint of maintaining mechanical properties.
[0045] The amounts of the columnar pellets (A) and the columnar pellets (B) blended in the resin composite material can be adjusted as desired within the range satisfying the above formula (II) or the above formulas (II) and (VI).
[0046] In one embodiment, the total amount of the fillers including the fibrous filler (a2) contained in the resin composite is preferably 5% by mass or more, more preferably 10% by mass or more, based on the total mass of the resin composite. In one embodiment, the total amount may be 5 to 30% by mass, 5 to 25% by mass, or 10 to 25% by mass. By setting the total amount of the fillers in the resin composite within the above range, the effect of maintaining good appearance of the molded product can be easily obtained.
[0047] In one embodiment, the columnar pellets (A) and (B) may contain recycled materials. The recycled materials are repelletized pulverized molded products containing the above-mentioned thermoplastic resin (b1) that are recovered after use for the intended purpose. The original use of the molded product is not particularly limited, and may include automobile parts, electric devices, electrical appliances, office supplies, packaging supplies, etc. Also, it may be molded as a test piece for measuring physical properties. When the columnar pellets (A) and (B) contain recycled materials, the ratio of the recycled materials is preferably 25 to 75 mass% with respect to the total mass of the thermoplastic resins (a1) and (b1) from the viewpoint of reducing the environmental load. Also, the ratio of the recycled materials with respect to the total mass of the thermoplastic resins (a1) and (b1) is preferably 25 to 50 mass% from the viewpoint of maintaining physical properties.
[0048] In one embodiment, the resin composite may contain any component other than the cylindrical pellets (A) and (B). From the viewpoint of obtaining a molded product with a smaller variation in weight, it is preferable that the resin composite contains only the cylindrical pellets (A) and (B).
[0049] [Manufacturing method of resin composite material] The resin composite material according to this embodiment can be obtained by dry blending the columnar pellets (A) and (B) and, if necessary, any optional components.
[0050] [Molded products] The molded product according to this embodiment is obtained by molding the above-mentioned resin composite material by a known resin molding method such as injection molding. The shape of the molded product according to this embodiment is not particularly limited, and it can be molded into a shape according to the application. The molded product according to this embodiment has a small variation in weight during molding. In one embodiment, the weight variation rate ((standard deviation / average value)×100(%)) of the molded product in 100 shots is preferably 1.0% or less, more preferably less than 1.0%. The weight of a molded article obtained from a conventional resin composite material may vary by about 2 to 3%. However, the weight variation rate of a molded article obtained from the resin composite material according to this embodiment can be suppressed to 1.0% or less.
[0051] <Application> As described above, the molded article according to this embodiment has a small variation in weight. Such molded articles are particularly suitable for use in the fields of industrial parts, particularly automobiles and electronic devices.
[0052] A preferred embodiment of the resin composite material according to the present embodiment is as follows. <1> A resin composite material, The resin composite material is A cylindrical pellet (A) containing a thermoplastic resin (a1) and a fibrous filler (a2); and columnar pellets (B) containing a thermoplastic resin (b1), The cylindrical pellets (A) and (B) have a shape selected from a circular cylinder, an elliptical cylinder, an oblong cylinder, or a gourd-shaped cylinder, A resin composite material satisfying all of the following formulas (I) to (VI): 0≦|SG A -SG B |≦0.50 (I) 1.0≦F B / F A ≦4.0 (II) 0.8≦L B / L A ≦1.5 (III) 0.6≦LD B / LD A ≦1.2 (IV) 0.6≦SD B / SD A ≦1.2 (V) 50≦(F A +F B ) (VI) (In formula (I), SG A represents the specific gravity of the cylindrical pellet (A), and SG B represents the specific gravity of the cylindrical pellets (B). In formulas (II) and (VI), F A represents the proportion (mass%) of the columnar pellets (A) in the resin composite material, and F B represents the proportion (mass %) of the columnar pellets (B) in the resin composite material. In formula (III), L A represents the length (mm) of the cylindrical pellet (A), and L B represents the length (mm) of the cylindrical pellet (B). In formula (IV), L-D A represents the major axis (mm) of the cross section of the cylindrical pellet (A), and LD B represents the major axis (mm) of the cross section of the columnar pellet (B). In formula (V), SD A represents the minor axis (mm) of the cross section of the cylindrical pellet (A), and SD B represents the minor axis (mm) of the cross section of the cylindrical pellet (B). <2> The length (L A ) is 5 to 20 mm, and the length (L B ) is 4 to 30 mm, <1> The resin composite material according to claim 1. <3> The major axis (LD) of the cylindrical pellet (A) A ) is 2.0 to 4.0 mm, and the major axis (LD B ) is 1.2~4.8mm, <1> or <2> The resin composite material according to claim 1. <4> The short diameter (SD A ) is 1.5 to 3.0 mm, and the major axis (LD B ) is 0.9~3.6mm, <1> from <3> 13. The resin composite material according to claim 12 . <5> The thermoplastic resins (a1) and (b1) are at least one thermoplastic resin selected from the group consisting of polyamide resins and polyolefin resins. <1> from <4> 13. The resin composite material according to claim 12 . <6> <1> from <5> A molded article of the resin composite material according to any one of claims 1 to 5. EXAMPLES
[0053] The following were used as the raw material for the cylindrical pellets (A) and the cylindrical pellets (B). [Columnar pellets (A)] <Thermoplastic resin (a1)> Polyethersulfone resin (PES): Manufactured by Sumitomo Chemical Co., Ltd., product name "3600G". - Polypropylene resin (PP): Manufactured by Sunallomer Co., Ltd., product name "PMB60A". -Polyamide 66 resin (PA66): Manufactured by INVISTA, product name "U3600". <Fibrous filler (a2)> Glass fiber: Average fiber diameter 17μm, bundle of approximately 4000 fibers. Stainless steel fiber: Diameter 11μm, fiber bundle of approximately 7000 fibers.
[0054] [Columnar pellets (B)] The thermoplastic resin (b1) was fed into a twin-screw extruder, melt-kneaded, and the resulting strand was cooled and then cut into strands having the length (L B ) to obtain a cylindrical pellet (B) in the form of an elliptical cylinder (an ellipse having the same area at one end and the other end). Specific gravity (SG) of columnar pellets (B-1) to (B-4) B ), length (L B ), major axis (LD B ), and minor axis (SD B ) were measured according to the conditions described below. The results are shown in Tables 1 and 2.
[0055] Production Example 1: Production of columnar pellets (A-1) While pulling the glass fiber (fibrous filler (a2)) through the crosshead die, PA66 was fed in a molten state from the twin-screw extruder to the crosshead die to impregnate the glass fiber with PA66. After that, the strand obtained by passing through the shaping die was cooled and then cut to the length (L A ) to obtain cylindrical pellets (A-1) as elliptical cylinders (ellipses with the same area at one end and the other end). The content of glass fiber (fibrous filler (a2)) relative to the total mass of the cylindrical pellets (A-1) was 50 mass%.
[0056] Production Example 2: Production of columnar pellets (A-2) Cylindrical pellets (A-2) were obtained in the same manner as in Production Example 1, except that PP was used as the thermoplastic resin (a1) and the resin was impregnated so that the glass fiber content was 20 mass %.
[0057] Production Example 3: Production of columnar pellets (A-3) Cylindrical pellets (A-3) were obtained in the same manner as in Production Example 1, except that PP was used as the thermoplastic resin (a1) and the resin was impregnated so that the glass fiber content was 50 mass %.
[0058] Production Example 4: Production of columnar pellets (A-4) Cylindrical pellets (A-4) were obtained in the same manner as in Production Example 1, except that PP was used as the thermoplastic resin (a1) and stainless steel fiber was used as the filler (a2) and the resin was impregnated so that the stainless steel fiber content was 50 mass%.
[0059] Production Example 5: Production of columnar pellets (A-5) A cylindrical pellet (A-5) was obtained in the same manner as in Production Example 1, except that PES was used as the thermoplastic resin (a1) and the resin was impregnated so that the glass fiber content was 50 mass %.
[0060] Production Example 6: Production of columnar pellets (A-6) Glass fibers (fibrous filler (a2)) were passed through a crosshead die. At this time, molten PES was supplied from a twin-screw extruder to the crosshead die to obtain pellets in which the glass fibers were impregnated with PES. After that, the pellets were shaped using a shaping nozzle at the exit of the crosshead die to obtain pellets with the length (L A ) to obtain a columnar pellet (A-6) having a quadrilateral (square) cross section (a square having the same area at one end face and the other end face). The content of glass fiber (fibrous filler (a2)) relative to the total mass of the columnar pellet (A-6) was 50 mass%.
[0061] · Measurement of specific gravity (SG) of cylindrical pellets (A) and (B) In accordance with JIS K7112, the specific gravities of 15 pellets were measured by the water displacement method using a specific gravity meter (manufactured by Kensei Kogyo Co., Ltd., product name "SD-120L"), and the average value was calculated. · Measurement of the length (L) of cylindrical pellets (A) and (B) The lengths of 15 pellets were measured using a caliper (manufactured by Mitutoyo Corporation, product name "CD-15CX"), the average value was calculated, and the value was rounded off to the nearest tenth place. · Measurement of the long diameter (LD) of cylindrical pellets (A) and (B) Using a vernier caliper (manufactured by Mitutoyo Corporation, product name "CD-15CX"), the major axis of 15 pellets was measured, the average value was calculated, and the value was rounded off to one decimal place. · Measurement of the minor axis (SD) of cylindrical pellets (A) and (B) The short diameters of 15 pellets were measured using a caliper (manufactured by Mitutoyo Corporation, product name "CD-15CX"), the average value was calculated, and the value was rounded off to one decimal place.
[0062] [Examples 1 to 10 and Comparative Examples 1 to 14] The cylindrical pellets (A) and (B) were mixed in the ratios shown in Tables 1 and 2 to obtain a resin composite material. The obtained resin composite material was injection molded under the following conditions to obtain a molded article. The weight variation rate ((standard deviation / average value)×100(%)) of the molded article over 100 shots was calculated. The results are shown in Tables 1 and 2.
[0063] [Table 1]
[0064] [Table 2]
[0065] As shown in Table 1, the molded products obtained from the resin composite material according to the present embodiment had a weight variation rate of less than 1.0%, and thus had small weight variations. On the other hand, in Comparative Examples 1 to 2, 4 to 14, which do not satisfy one or more of the formulas (I) to (V), and Comparative Example 3, which contains columnar pellets (A) that are rectangular cross-sectional columns, the weight variation rate of the molded products all exceeded 1.0%, and the weight variation rate values were higher than those of the Examples. Among them, Comparative Example 4, which contains columnar pellets (A) containing stainless steel fibers, had the highest weight variation rate. From these results, it was confirmed that a molded product with small weight variations can be obtained if the resin composite material contains columnar pellets (A) and (B) that satisfy the formulas (I) to (V) and have a cross-sectional shape other than the specific one. [Industrial Applicability]
[0066] Since the resin composite material according to this embodiment can produce molded products with small variations in weight, it can be suitably used in fields such as industrial parts, mainly for automobiles and electronic devices.
Claims
1. A resin composite material, The resin composite material is A columnar pellet (A) containing a thermoplastic resin (a1) and a fibrous filler (a2); and columnar pellets (B) containing a thermoplastic resin (b1), The cylindrical pellets (A) and (B) have a cylindrical shape other than a triangular cross-sectional shape or a rectangular cross-sectional shape, A resin composite material satisfying all of the following formulas (I) to (V): 0≦|SG A -SG B |≦0.50 ・・・(I) 1.0≦F B / F A ≦4.0 ・・・(II) 0.8≦L B / L A ≦1.5 ・・・ (III) 0.6≦LD B / LD A ≦1.2 ・・・(IV) 0.6≦SD B / SD A ≦1.2 ・・・(V) (In formula (I), SG A represents the specific gravity of the cylindrical pellet (A), and SG B represents the specific gravity of the cylindrical pellets (B). In formula (II), F A represents the proportion (mass%) of the columnar pellets (A) in the resin composite material, and F B represents the proportion (mass%) of the columnar pellets (B) in the resin composite material. In formula (III), L A represents the length (mm) of the cylindrical pellet (A), L B represents the length (mm) of the cylindrical pellet (B). In formula (IV), L A represents the major axis (mm) of the cross section of the columnar pellet (A), and L B represents the major axis (mm) of the cross section of the columnar pellet (B). In formula (V), S.D. A represents the minor axis (mm) of the cross section of the cylindrical pellet (A), and SD B represents the minor axis (mm) of the cross section of the columnar pellet (B).
2. The thermoplastic resins (a1) and (b1) are at least one thermoplastic resin selected from the group consisting of polyamide resins, polyolefin resins, polystyrene resins, polycarbonate resins, polyester resins, polyacetal resins, polyarylene ether resins, polyarylene sulfide resins, polysulfone resins, polyarylene ether ketone resins, and liquid crystal resins. The resin composite material according to claim 1.
3. The thermoplastic resins (a1) and (b1) are at least one thermoplastic resin selected from the group consisting of polyamide 6 resin, polyamide 12 resin, polyamide 66 resin, polyamide 610 resin, polyamide 1010 resin, polyamide 6T resin, polyamide 9T resin, polyethylene resin, polypropylene resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyacetal copolymer, polyphenylene sulfide resin, polyether ether ketone resin, polyether ketone resin, liquid crystalline polyester resin, and liquid crystalline polyester amide resin. The resin composite material according to claim 1 or 2.
4. The resin composite material according to claim 1 or 2, wherein the thermoplastic resins (a1) and (b1) are the same thermoplastic resin.
5. The resin composite material according to claim 1 or 2, further satisfying the following formula (VI): 50≦(F) A +F B ) ・・・(VI)
6. The resin composite according to claim 1 or 2, wherein the total amount of fillers including the fibrous filler (a2) contained in the resin composite is 5 mass% or more with respect to the total mass of the resin composite.
7. A molded article made of the resin composite material according to claim 1 or 2.
Citation Information
Patent Citations
Polyolefin mixture
JP1998212359A
Polyamide resin pellet for small size component
JP2002249598A
Mixture of masterbatch pellet
JP2004346314A
Method for producing molded item of propylene polymer composition
JP2010090197A
Method for producing molded item of propylene polymer composition
JP2010090198A