Mold release agent for resin molding and manufacturing method of molded body using the same
A mold release agent with silicone and nonionic surfactant, optimized for minimal surface tension difference, addresses adhesion issues on high-temperature molds by suppressing the Leidenfrost phenomenon, ensuring effective mold release.
Patent Information
- Application Number
- JP2023087227
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
AI Technical Summary
Mold release agents fail to adhere effectively to high-temperature molds due to the formation of a water vapor layer, leading to reduced performance.
A mold release agent comprising silicone, nonionic surfactant, and water, with a specific surfactant content that minimizes the surface tension difference to 2 mN/m or less, ensuring the surfactant saturates the droplet surface and suppresses the Leidenfrost phenomenon, enhancing adhesion and mold release properties.
The agent improves adhesion to high-temperature molds, ensuring effective mold release even on vertical and sloped surfaces, maintaining excellent mold release properties.
Smart Images

Figure 2024170199000001 
Figure 2024170199000002 
Figure 2024170199000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a release agent for resin molding and a method for producing a molded article using the same. [Background technology]
[0002] When molding rubber, resin, etc., it is common to apply a release agent to the mold to facilitate release of the molded product from the mold. Silicone-based release agents have been proposed as such release agents (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2023-6360 Summary of the Invention [Problem to be solved by the invention]
[0004] For example, when a release agent is applied to a mold that has been heated to a high temperature, such as 200° C. or higher, a layer of water vapor is formed between the mold and the release agent, making it difficult for the active ingredients of the release agent to adhere to the mold, resulting in a problem that the performance of the release agent cannot be fully exhibited.
[0005] A main object of the present disclosure is to provide a release agent for resin molding which has improved adhesion and excellent releasability. [Means for solving the problem]
[0006] The aspects of the present disclosure that solve the above problems are as follows. [1] An emulsion containing silicone, a nonionic surfactant, and water, The content of the nonionic surfactant is such that the difference between the surface tension value at the content at which the surface tension is the minimum in the same blend system is 2 mN / m or less. A release agent for resin molding. [2] The release agent for resin molding according to the above [1], wherein the content of the nonionic surfactant is 0.45% by weight or more and 10% by weight or less. [3] The release agent for resin molding according to [1] or [2], which has a surface tension value of 26.6 mN / m or less. [4] The release agent for resin molding according to any one of [1] to [3], wherein the silicone content is from 0.70% by weight to 15% by weight. [5] The release agent for resin molding according to any one of [1] to [4], wherein the silicone is an amino-modified silicone or a dimethyl silicone. [6] The release agent for resin molding according to any one of the above [1] to [5], wherein the nonionic surfactant is a polyoxyalkylene alkyl ether. [7] An emulsion comprising a silicone, a nonionic surfactant, and water, The content of the nonionic surfactant is 0.48% by weight or more and 10% by weight or less, Surface tension value is 25.2mN / m or less A release agent for resin molding. [8] A step of applying the release agent for resin molding according to any one of [1] to [7] to a mold; placing a raw material for a compact in the die; and removing the hardened body from the mold. A method for producing a molded body. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a release agent for resin molding which has improved adhesion to a mold and excellent releasability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Preferred embodiments of the present invention will be described in detail below. However, the present invention is not limited to the following embodiments. The elements described below can be combined in any way, and the scope of the present invention is intended to include all modifications within the scope of the claims and equivalents to the scope of the claims. In addition, the upper and lower limit values exemplified for numerical ranges in this specification can be arbitrarily combined to form new numerical ranges.
[0009] The release agent for resin molding of the present disclosure is an emulsion containing silicone, a nonionic surfactant, and water, and is characterized in that the content of the nonionic surfactant is such that the difference in surface tension between the content of the nonionic surfactant that results in the minimum surface tension in the same blend system is 2.0 mN / m or less.
[0010] The surface tension in this specification can be measured by the Wilhelmy method (plate method) using a surface tensiometer in a 25° C. environment.
[0011] The mechanism by which the release agent for resin molding of the present disclosure has excellent adhesion and releasability is not clear, but is presumed to be as follows. Silicone-based release agents come in oil, emulsion, and solvent types, and are particularly popular because they can be diluted with water and are easy to work with and economical to use. Generally, silicone emulsions are used as emulsion-type silicone release agents, which are made by dispersing silicone, a non-water-soluble release component, in water using an emulsifier. When a release agent is applied to a mold heated to about 200°C, the water in the emulsion droplets of the release agent (droplets of the release agent solution, which is an emulsion) on the mold evaporates explosively, forming a layer of water vapor between the release agent and the mold, and the emulsion droplets slide sideways without contacting the mold surface, which is known as the Leidenfrost phenomenon. As a result, the release component does not adhere sufficiently to the vertical and inclined surfaces of the mold, and the performance of the release agent is not fully expressed.
[0012] In order to suppress the above-mentioned Leidenfrost phenomenon in a resin molding release agent solution, which is an emulsion-type silicone-based release agent, it is considered effective to adsorb surfactant molecules to the emulsion droplet surface (air-liquid interface) and reduce the moisture present on the droplet surface. It is presumed that the evaporation of moisture on the droplet surface can be suppressed by saturating the surfactant present on the droplet surface and forming a surfactant layer on the droplet surface. This suppresses the Leidenfrost phenomenon, enables the resin molding release agent to come into contact with the mold surface, and improves adhesion and releasability.
[0013] In the case of an emulsion system, the surfactant molecules are adsorbed so as to reduce the energy of the entire system. The surfactant molecules are first adsorbed to the liquid-liquid interface and then adsorbed to the droplet surface so as to reduce the energy of the interface (liquid-liquid interface) between the emulsified material and the dispersion medium more than the energy of the emulsion droplet surface. The surfactant molecules are adsorbed to the droplet surface and reduce the surface tension of the resin molding release agent solution. When the surfactant is not sufficiently adsorbed to the droplet surface, the surface tension value is reduced by adding the surfactant to the resin molding release agent solution. When the droplet surface is saturated with the surfactant, the surface tension value hardly changes even if the surfactant is added to the resin molding release agent solution. In other words, when the concentration of the nonionic surfactant that can saturate the droplet surface with the nonionic surfactant (hereinafter also referred to as the saturation concentration) is exceeded, it is presumed that the surface tension value of the resin molding release agent solution is substantially constant, independent of the nonionic surfactant concentration.
[0014] In the resin molding release agent of the present disclosure, the nonionic surfactant is contained in an amount such that the change in the surface tension value of the resin molding release agent solution is equal to or less than a predetermined value. Specifically, the content of the nonionic surfactant is set to the surface tension value of the resin molding release agent at the content of the nonionic surfactant that gives the smallest surface tension value in the same blending system, and the content is the amount of the surface tension value that is 2.0 mN / m or less different from the reference surface tension value. The requirement for the content of the nonionic surfactant corresponds to a saturation concentration or higher. When the content of the nonionic surfactant satisfies the above requirement, the nonionic surfactant can be sufficiently present on the emulsion droplet surface, and the adhesion and releasability can be improved.
[0015] [Release agent for resin molding] The release agent for resin molding according to the embodiment contains silicone. Silicone can function as a release component. Silicone is a compound having a polysiloxane skeleton. Silicone may be silicone oil or silicone resin.
[0016] Examples of silicones include dimethyl silicone, methylphenyl silicone, modified silicone, etc. Examples of modified silicones include amino-modified, epoxy-modified, alkyl-modified, carboxyl-modified, polyether-modified, etc. Silicones may be used alone or in combination of two or more. From the viewpoint of releasability, the silicones are preferably amino-modified silicone, dimethyl silicone, or a combination thereof, and more preferably a combination of amino-modified silicone and dimethyl silicone.
[0017] The content of silicone in the resin molding release agent is preferably 0.70% by weight to 15% by weight, more preferably 0.80% by weight to 12% by weight, even more preferably 1.4% by weight to 10% by weight, still more preferably 1.6% by weight to 10% by weight, and even more preferably 5.0% by weight to 9.5% by weight, from the viewpoint of releasability. When two or more kinds are used in combination, the content means the total amount.
[0018] Silicone can be obtained by a known synthesis method, or a commercially available product can be used. As a commercially available silicone product, a silicone emulsion obtained by adding an emulsifier to silicone and dispersing it in water can be used. As commercially available silicone emulsions, "PolonMF-14", "PolonMF-14E", "PolonMF-32", "PolonMF-33", "PolonMF-55", "KM-752T", "KM-2002-L-1", "KM-780", "KM-785", "KM-787", "KM-860A", "KM-9717", "KM-9729", "KM-9737A", and "KM-9738" (all manufactured by Shin-Etsu Chemical Co., Ltd.), "R 2701", "R 2703" (all manufactured by Asahi Kasei Wacker Silicone Co., Ltd.), "DOWSIL TM BY 22-840 SR Emulsion”, “DOWSIL TM DK Q2-103-22 Emulsion”, “DOWSIL TM IE-7170 Emulsion”, “DOWSIL TM SM 7001 EX Emulsion”, “DOWSIL TM SM 7060 EX Emulsion”, “DOWSIL TM SM 8701 EX Emulsion”, “DOWSIL TM SM 8709 SR Emulsion" (both manufactured by Dow Toray Industries, Inc.), etc.
[0019] The release agent for resin molding of the embodiment contains a nonionic surfactant. Examples of the nonionic surfactant include ethers, esters, and amides. Among them, ethers are preferred. Examples of the ethers include alkyl ethers, polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, and polyoxyethylene polyoxypropylene glycols. Among them, polyoxyethylene alkyl ethers are preferred from the viewpoint of adhesion. Examples of the esters include fatty acid glycerin esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and polyoxyethylene fatty acid esters. Examples of the amides include fatty acid alkanolamides. The nonionic surfactants may be used alone or in combination of two or more.
[0020] Commercially available nonionic surfactants include "Noigen SD-80", "Noigen SD-60", "Noigen SD-70", "Noigen SD-110", "Noigen XL-40", "Noigen XL-41", "Noigen XL-61", "Noigen XL-70", "Noigen XL-100", "Noigen XL-140", "Noigen ET-89", "Noigen EA-109", "Noigen EA-150", and "Noigen TD-120D" (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), "Finesurf TD-75", "Finesurf TDE-1033", "Finesurf 270", "Finesurf NDB-800", "Finesurf 250", "Finesurf 270", and "Finesurf 290" (all manufactured by Aoki Oil Industries Co., Ltd.).
[0021] The content of the nonionic surfactant is the content at which the difference between the surface tension value at the content at which the surface tension value ...
[0022] The content of the nonionic surfactant in the resin molding release agent is preferably 0.45% by weight or more and 10% by weight or less, more preferably 0.48% by weight or more and 9.5% by weight or less, even more preferably 1.0% by weight or more and 9.0% by weight or less, even more preferably 2.1% by weight or more and 8.5% by weight or less, and even more preferably 3.5% by weight or more and 8.0% by weight or less. When two or more kinds are used in combination, the content means the total amount. When the content of the nonionic surfactant is within the above range, the Leidenfrost phenomenon is well suppressed and the adhesion is improved, and an effect commensurate with the use can be obtained.
[0023] The minimum surface tension value and the content at which the minimum surface tension value is obtained in the same blending system can be found by measuring the surface tension of a resin molding release agent solution at various nonionic surfactant concentrations in the same blending system and comparing the measurement results. As an example, a resin molding release agent containing a nonionic surfactant of a specific concentration and two or more release agent dilutions obtained by diluting the nonionic surfactant of the specific concentration at multiple dilution ratios are prepared, and the surface tension at each concentration is measured. Based on the relationship between each measured surface tension value and the nonionic surfactant concentration, a region where the surface tension value is almost constant and a region where the surface tension value changes are obtained. The minimum surface tension value in the obtained region where the surface tension value is almost constant is taken as the minimum surface tension value in the same blending system. In addition, the content value of the nonionic surfactant showing the minimum surface tension value is taken as the content at which the minimum surface tension value is obtained in the same blending system.
[0024] When determining the minimum surface tension value, the content of the nonionic surfactant in the release agent for resin molding before dilution is preferably near the upper limit of the range of the content of the nonionic surfactant. The dilution ratio is preferably 3 times or more, more preferably 5 times or more, between the minimum dilution ratio and the maximum dilution ratio. The dilution ratio preferably includes at least a dilution ratio within the range of the content of the nonionic surfactant and a dilution ratio outside the range of the content of the nonionic surfactant. The dilution ratio within the range of the content of the nonionic surfactant is preferably 1.5 times or more and 10 times or less, more preferably 2 times or more and 6 times or less, and even more preferably 2 times or more and 3 times or less.
[0025] The release agent for resin molding according to the embodiment contains water. Examples of water include tap water, industrial water, ion-exchanged water, distilled water, and sterilized purified water, and may be hard water or soft water. One type of water may be used alone, or two or more types may be used in combination.
[0026] The content of water in the resin molding release agent is preferably from 40% by weight to 95% by weight, more preferably from 42% by weight to 93% by weight, and even more preferably from 45% by weight to 90% by weight, from the viewpoint of releasability. When two or more kinds are used in combination, the content means the total amount.
[0027] In the resin molding release agent of the embodiment, the weight ratio of the silicone content to the nonionic surfactant content (silicone / nonionic surfactant) is preferably 1.0 or more and 4.0 or less, more preferably 1.3 or more and 3.0 or less, from the viewpoints of adhesion and releasability.
[0028] In the release agent for resin molding according to the embodiment, the weight ratio of the content of the nonionic surfactant to the content of water (nonionic surfactant / water) is preferably 0.01 or more and 0.3 or less, more preferably 0.03 or more and 0.1 or less, from the viewpoints of adhesion and economy.
[0029] The release agent for resin molding according to the embodiment may contain a surfactant other than the nonionic surfactant as necessary within a range that does not impair the effects of the present invention. Examples of surfactants other than nonionic surfactants include anionic surfactants and cationic surfactants. Examples of anionic surfactants include polyoxyethylene alkyl ether carboxylic acid, polyoxyethylene alkyl ether phosphoric acid, alkyl sulfonic acid, alkyl benzene sulfonic acid, α-olefin sulfonic acid, and salts thereof. Examples of cationic surfactants include alkyl amine salts, alkyl ammonium salts, alkyl trimethyl ammonium salts, dialkyl dimethyl ammonium salts, and alkyl dimethyl benzyl ammonium salts. The surfactants other than nonionic surfactants may be used alone or in combination of two or more.
[0030] The content of the surfactant other than the nonionic surfactant in the resin molding release agent is preferably 0.01% by weight to 1% by weight, more preferably 0.02% by weight to 0.5% by weight, even more preferably 0.08% by weight to 0.5% by weight, and still more preferably 0.1% by weight to 0.4% by weight, from the viewpoints of emulsion stability and economic efficiency. When two or more kinds are used in combination, the content means the total amount.
[0031] The release agent for resin molding according to the embodiment may further contain a release component other than the silicone, as necessary, within a range that does not impair the effects of the present invention. Examples of other release components include fats and oils, mineral oils, waxes, fatty acids, and fatty acid esters. Examples of fats and oils include animal oils such as beef tallow, lanolin, and lard, and vegetable oils such as castor oil, soybean oil, rapeseed oil, and palm oil. Examples of mineral oils include turbine oil, machine oil, cylinder oil, paraffin oil, and gear oil. Examples of waxes include petroleum waxes such as paraffin wax, olefin wax, polyethylene wax, polystyrene wax, and polypropylene wax, oxidized waxes such as polyethylene oxide wax and polypropylene oxide, and natural waxes such as carnauba wax and montan wax. Examples of fatty acids include carboxylic acids, oleic acid, stearic acid, ricinoleic acid, linoleic acid, palmitic acid, and lauric acid. Examples of fatty acid esters include monohydric or polyhydric alcohol (or glycerin) esters of the above fatty acids. The other release components may be used alone or in combination of two or more.
[0032] When other release components are contained, the total content of the silicone and the other release components in the resin molding release agent is, from the viewpoint of releasability, preferably 0.70% by weight or more and 15% by weight or less, more preferably 0.80% by weight or more and 12% by weight or less, even more preferably 1.4% by weight or more and 10% by weight or less, still more preferably 1.6% by weight or more and 10% by weight or less, and even more preferably 5.0% by weight or more and 9.5% by weight or less. When two or more kinds are used in combination, the content means the total amount.
[0033] In addition to the above-mentioned components, the release agent for resin molding according to the embodiment may contain various additives as necessary within the range that does not impair the effects of the present invention. Examples of additives include defoamers, antioxidants, and preservatives. The amount of each additive may be appropriately selected according to the conventional technology.
[0034] From the viewpoint of adhesion, the surface tension of the release agent for resin molding of the embodiment is preferably 26.6 mN / m or less, more preferably 25.2 mN / m or less. The lower limit of the surface tension is not particularly limited, but 15.0 mN / m is the substantial lower limit.
[0035] The surface tension of the release agent for resin molding according to the embodiment is set to the minimum surface tension value in the same blend system, and the difference between the minimum surface tension value and the reference surface tension value is 2.0 mN / m or less. When the difference between the surface tension of the release agent for resin molding and the minimum surface tension value is 2.0 mN / m or less, the surface of the release agent for resin molding is saturated with the nonionic surfactant, and the Leidenfrost phenomenon can be effectively suppressed. Therefore, the adhesion of the release agent for resin molding to the mold is improved.
[0036] Another aspect of the release agent for resin molding of the embodiment is an emulsion containing silicone, a nonionic surfactant, and water, characterized in that the content of the nonionic surfactant is 0.48% by weight or more and 10% by weight or less, and the surface tension value is 25.2 mN / m or less. In the above aspect, the content of the silicone may be 0.70% by weight or more and 15% by weight or less.
[0037] The release agent for resin molding according to the embodiment is an emulsion obtained by emulsifying a release component containing silicone using a nonionic surfactant and / or other surfactants as an optional component, and dispersing the silicone uniformly in water. The release agent for resin molding may be obtained by emulsion polymerization of silicone dispersed in water using a surfactant using a polymerization initiator. The release agent for resin molding may be obtained by further mixing a nonionic surfactant, water, and other release components with a silicone emulsion composition containing silicone. The emulsification and emulsion polymerization of silicone can be carried out by a known method. Examples of the polymerization initiator used in emulsion polymerization include potassium persulfate and ammonium persulfate, which are used in normal radical polymerization.
[0038] The release agent for resin molding according to the embodiment can be obtained by mixing and stirring the above-mentioned components. The order of adding the components is not particularly limited.
[0039] The release agent for resin molding of the embodiment has excellent adhesion and releasability, and therefore can be suitably used for resin molding to coat the surface of a mold. The release agent for resin molding of the embodiment is water-based and can be used as it is for the production of a molded body.
[0040] Examples of resins that are used as raw materials for the molded body include rubber, thermoplastic resins, and thermosetting resins. Examples of rubber include synthetic rubbers such as natural rubber, isoprene, butadiene, and styrene butadiene. Examples of thermoplastic resins include polyethylene resins and polypropylene resins. Examples of thermosetting resins include polyurethane resins, epoxy resins, and phenolic resins. The raw material for the molded body may be a mixture of the above-mentioned thermoplastic resins and fibers, or a mixture of the above-mentioned thermosetting resins and fibers. Examples of fibers include carbon fibers and glass fibers. The raw resin material may be liquid or solid.
[0041] The release agent for resin molding according to the embodiment may be applied to a mold by spray coating, brush coating, or the like. The amount of the release agent for resin molding applied to a mold is preferably 0.1 g / m2 in terms of solid content from the viewpoints of releasability and surface aesthetics. 2 More than 50g / m 2 Less than 0.5 g / m 2 More than 40g / m 2 The following is the result.
[0042] The mold temperature when applying the release agent for resin molding of the embodiment is not particularly limited, but is, for example, 130° C. to 280° C., preferably 150° C. to 270° C. The release agent for resin molding of the embodiment has an excellent effect of suppressing the Leidenfrost phenomenon, so that it adheres well to the mold surface even when applied to a mold at a high temperature as described above. It can also exhibit excellent adhesion when applied to the vertical or inclined surface of the mold.
[0043] [Method of manufacturing molded body] The method for producing a molded body according to the embodiment includes the steps of: A step of applying the resin molding release agent to a mold; placing a raw material for a compact in the die; and releasing the hardened body of the molded body raw material from the mold.
[0044] The method of applying the release agent for resin molding to the mold can be appropriately applied by the above-mentioned spray application, brush application, etc. As a result, a release agent film containing the release agent for resin molding is formed on the surface of the mold.
[0045] The method for placing the molding raw material is not limited, but can be a known method depending on the properties and type of the molding raw material, such as placing a solid resin raw material in the mold or filling the mold by injecting a liquid raw material.
[0046] In the step of demolding from the mold, the molded body raw material placed in the mold is hardened, and the obtained hardened body is demolded. Heat hardening is used as a method for hardening the molded body raw material. Specifically, the molded body raw material is hardened by heating it in the molds facing each other. The mold temperature when hardening the molded body raw material can be appropriately set according to the molded body raw material to be hardened, and can be, for example, 130°C to 280°C, preferably 150°C to 270°C. The hardening time when hardening the molded body raw material may be a time that provides a sufficient hardening rate of the obtained hardened molded body. The hardened body can be demolded by a known method. EXAMPLES
[0047] The present invention will be described in more detail below with reference to examples and comparative examples, but it is not intended that the present invention be limited to these examples. In the following description and tables, "parts" and "%" are by weight unless otherwise specified.
[0048] [Preparation of release agent for resin molding] Each component shown in the following Tables 1 to 9 was weighed out so as to obtain the composition (in weight %) shown in the same table, and mixed in a stirrer until it became uniform, thereby obtaining the release agents for resin molding of Examples 1 to 33 and Comparative Examples 1 to 28. Examples 1 to 4 and Comparative Examples 1 to 3 belong to Blend 1, Examples 5 to 8 and Comparative Examples 4 to 5 belong to Blend 2, Examples 9 to 11 and Comparative Examples 6 to 9 belong to Blend 3, Examples 12 to 14 and Comparative Examples 10 to 13 belong to Blend 4, Examples 15 to 17 and Comparative Examples 14 to 17 belong to Blend 5, Examples 18 to 21 and Comparative Examples 18 to 19 belong to Blend 6, Examples 22 to 26 and Comparative Examples 20 to 21 belong to Blend 7, Examples 27 to 31 and Comparative Examples 22 to 23 belong to Blend 8, and Examples 32 to 33 and Comparative Examples 24 to 28 belong to Blend 9. Those with the same blend number are the same blend system. In the same blend system, the release agent for resin molding with the smallest number of the example was used as the stock solution, and the stock solution was diluted at different dilution concentrations to prepare the release agents for resin molding of other examples and comparative examples in the same blend system. The middle rows of Tables 1 to 9 show the total content of silicone, nonionic surfactant, other surfactants, and other release components in the resin molding release agent. Note that other surfactants refer to surfactants other than nonionic surfactants, and other release components refer to release components other than silicone. The total content of nonionic surfactants is the sum of the content of nonionic surfactants in component (A) and the content of component (B).
[0049] Details of each component shown in Tables 1 to 9 are as follows. <Component (A): Silicone emulsion> A-1: Amino-modified silicone emulsion (silicone content 30% by weight, non-ionic surfactant content 2.25% by weight) A-2: Straight silicone emulsion ("KM-752T" manufactured by Shin-Etsu Chemical Co., Ltd., silicone content 29.5% by weight, nonionic surfactant content 0% by weight, anionic surfactant content 2.5% by weight) A-3: Silicone resin emulsion ("R-2701" manufactured by Wacker Asahi Kasei Silicone Co., Ltd., silicone content 35% by weight, nonionic surfactant content 2.5% by weight, anionic surfactant content 2.5% by weight) A-4: Amino-modified silicone emulsion (PolonMF-14E, manufactured by Shin-Etsu Chemical Co., Ltd., silicone content 15% by weight, non-ionic surfactant content 3% by weight) A-5: Amino-modified silicone emulsion (silicone content 30% by weight, non-ionic surfactant content 6% by weight) A-6: Amino-modified silicone emulsion (silicone content 30% by weight, nonionic surfactant content 4.5% by weight) <Component (B): Nonionic surfactant> B-1: Polyoxyethylene isodecyl ether ("Noigen SD-80" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) B-2: Polyoxyethylene isodecyl ether ("Noigen SD-60" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) <Component (C): Other release components> Castor oil condensate ("KF-4500" manufactured by KF Trading Co., Ltd., polyricinoleate, solid content 100%)
[0050] [Test Method] The surface tension, adhesion (wettability), and releasability of each of the release agents for resin molding obtained in the examples and comparative examples were measured and evaluated by the methods described below.
[0051] <Surface tension> Using an automatic surface tensiometer ("DY-300" manufactured by Kyowa Interface Science Co., Ltd.), static surface tension was measured by the plate method (Wilhelmy method) in an atmosphere of 25°C. The obtained surface tensions were compared to determine the minimum surface tension value in each blend system, and the difference in surface tension value from the minimum surface tension value was calculated for each Example and Comparative Example. The results are shown in Tables 1 to 9. In Tables 1 to 9, a value with a difference from the minimum value of 0 means that the surface tension value is the minimum in the same blend system.
[0052] <Evaluation of adhesion> Each release agent for resin molding was sprayed at 0.15 g / sec from a position at 45 degrees and 15 cm away from the surface of the test piece (SUS304, 0.8 mm x 70 mm x 150 mm) placed on a hot plate with a surface temperature of 240°C using a gravity-type hand spray gun ("W-101", manufactured by Anest Iwata), and the time until the release agent for resin molding adhered to the test piece was measured. The time until adhesion was evaluated according to the following criteria. The results are shown in Tables 1 to 9. The shorter the adhesion time, the better the adhesion. ◎: Adhesion time less than 1.75 seconds ○: Adhesion time 1.75 seconds or more and less than 3.20 seconds ×: Adhesion time 3.20 seconds or more
[0053] <Evaluation of releasability> Each release agent for resin molding was sprayed at 0.4 g / sec for 2.0 seconds onto a test piece (SUS304, 0.8 mm x 70 mm x 150 mm) placed on a hot plate with a surface temperature of 240°C using a gravity-type hand spray gun ("W-101", manufactured by Anest Iwata) and then left to stand for 30 seconds to form a uniform coating. Then, felt (weight per unit area: 1200 g / m2) was applied to the test piece. 2 ) was placed on the test piece and a load of 0.12 MPa was applied for 1 minute. The felt was then lifted upward to remove it from the test piece, and the release state was visually confirmed to evaluate the releasability according to the following criteria. The results are shown in Tables 1 to 9. ○: Felt did not stick to the test piece and came off ×: The test piece was lifted up
[0054] [Table 1]
[0055] [Table 2]
[0056] [Table 3]
[0057] [Table 4]
[0058] [Table 5]
[0059] [Table 6]
[0060] [Table 7]
[0061] [Table 8]
[0062] [Table 9]
[0063] As is clear from Tables 1 to 9, all of the resin molding release agents of the examples had excellent adhesion and good releasability. In the comparative examples, the nonionic surfactant was not blended in an amount that would result in a difference of 2.0 mN / m or less from the surface tension value at the content that would result in the minimum surface tension value in the same blend system, and the adhesion and releasability were reduced. From the examples and comparative examples of each blend system, it was found that the adhesion and releasability improved as the content of silicone and nonionic surfactant increased.
[0064] From the above, it was confirmed that the release agent for resin molding of the present disclosure improves adhesion to a mold and has excellent releasability.
Claims
1. An emulsion comprising a silicone, a nonionic surfactant and water, The content of the nonionic surfactant is such that the difference between the surface tension value at the content at which the surface tension value is the minimum in the same blend system is 2 mN / m or less. A release agent for resin molding.
2. The content of the nonionic surfactant is 0.45% by weight or more and 10% by weight or less. The release agent for resin molding according to claim 1 .
3. Surface tension value is 26.6 mN / m or less The release agent for resin molding according to claim 1 or 2.
4. The content of the silicone is 0.70% by weight or more and 15% by weight or less. The release agent for resin molding according to claim 1 or 2.
5. The silicone is an amino-modified silicone or a dimethyl silicone. The release agent for resin molding according to claim 1 or 2.
6. The nonionic surfactant is a polyoxyalkylene alkyl ether. The release agent for resin molding according to claim 1 or 2.
7. An emulsion comprising a silicone, a nonionic surfactant and water, The content of the nonionic surfactant is 0.48% by weight or more and 10% by weight or less, Surface tension value is 25.2 mN / m or less A release agent for resin molding.
8. A step of applying the release agent for resin molding according to claim 1 or claim 7 to a mold; placing a raw material for a molded body in the mold; and removing the hardened body from the mold. A method for producing a molded body.
Citation Information
Patent Citations
Mold release agent for rubber belt and mold release agent-spraying device
JP2000326338A
Mold release agent composition for molding vulcanization of rubber product and use thereof
JP2017024204A
Silicone emulsion composition for mold-release agent for metal mold formation
JP2023006360A