Wood for processing and its manufacturing method, wood molding product and its manufacturing method, and composite comprising thereof

By controlling hemicellulose content and moisture in wood processing, the method addresses cracking and splitting issues, enabling high-quality wood molded products with enhanced grain and color tone, suitable for various applications.

JP2024180348APending Publication Date: 2024-12-26CHIYODA IND +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024095854
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-14
Filing Date
2024-06-13
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Wood molded products made from wood with removed hemicellulose suffer from defects such as cracking and splitting during compression or bending processing, limiting the production of high-quality products with good appearance.

Method used

Process wood with a controlled hemicellulose content of 14-21% for softwoods and 13-20% for hardwoods by hydrolyzing with sulfuric acid and adjusting moisture content, followed by compression or bending processing to suppress defects and enhance wood grain and color tone.

Benefits of technology

The method produces wood molded products with excellent appearance and stability, reducing manufacturing costs by avoiding the need for adhesives and enabling the production of items like tableware, furniture, and decorative items without cracking or splitting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024180348000001_ABST
    Figure 2024180348000001_ABST
Patent Text Reader

Abstract

To provide a wood for processing providing a wood molded product excellent in appearance of grain and color tone by suppressing defects such as cracking and splitting by compression processing or bending processing, and to provide a method for producing a wood molded product by using the same.SOLUTION: A wood for processing of the present invention is made of a coniferous tree or broad-leaved tree and is used as a raw material for producing the wood molded product, and is characterized in that when the processing wood is hydrolyzed with sulfuric acid, then the sulfuric acid is removed from the obtained processing liquid, and the recovered liquid is subjected to liquid chromatography, the ratio of the total amount of the sugar components derived from hemicellulose to the total amount of the sugar components is 14 to 21 mass% for softwoods and 13 to 20 mass% for hardwoods.SELECTED DRAWING: Figure 10
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wood molded product having excellent appearance, a wood material for processing which can provide the same, a method for producing the same, and a composite material. [Background technology]

[0002] Traditionally, efforts have been made to make effective use of biomass resources as a measure to reduce carbon dioxide emissions in order to curb global warming. For example, attempts have been made to manufacture various wooden molded products using waste materials, scraps, wood powder, etc. generated during the cutting and processing of wood as raw materials.

[0003] Since wooden molded products are usually required to have dimensional stability and durability without warping, for example, wood for processing that has been pretreated, such as acetylated or formalized, is sometimes used as a raw material to manufacture wooden molded products. This method has been seldom adopted from the viewpoint of production costs.

[0004] As a modification treatment method for pre-treatment of wood, Patent Document 1 describes a method in which wood is subjected to a pressure of 5 to 25 kgf / cm 2 and then compressing and molding the wood under high pressure conditions to fix the deformation. 2 In one embodiment, the wood is softened in a water vapor atmosphere at room temperature, compressed and molded under normal pressure, and then placed in a water vapor atmosphere again in this state to fix the deformation. In addition, Patent Document 2 discloses a wood modification treatment method that includes a first heat treatment step of decomposing hemicellulose in wood to a lower molecular weight by heating at a temperature equal to or lower than the decomposition temperature of cellulose, a removal treatment step of removing the decomposed hemicellulose in the wood, and a second heat treatment step of forming a hydrophobic structure in the wood by heating at a temperature equal to or lower than the decomposition temperature of cellulose. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 3-231802 [Patent Document 2] JP 2010-30081 A Summary of the Invention [Problem to be solved by the invention]

[0006] When the wood from which the hemicellulose has been removed is subjected to compression or bending, defects such as cracks and splits occur, and it is not possible to obtain a wood molded product with a good appearance. The object of the present invention is to provide a wood material for processing and a manufacturing method thereof, a wood molded product and a manufacturing method thereof, which can be compressed or bent to produce a wood molded product having excellent appearance in terms of grain and color tone while suppressing defects such as cracking and splitting, and a composite material including the wood molded product. In this specification, the term "compressing or bending" includes both compressing and bending. [Means for solving the problem]

[0007] The inventors have discovered that when using coniferous or broad-leaved trees as raw materials to manufacture wood molded products by compression or bending, if wood for processing is used in which the ratio of the total amount of hemicellulose-derived sugar components (arabinose, rhamnose, galactose, xylose and mannose) to the total amount of sugar components is within a specific range, defects such as cracks and splits are suppressed and wood molded products with excellent appearance in terms of grain and color tone can be obtained.

[0008] The present invention is as follows. (1) Wood for processing made of softwood or hardwood and used as a raw material for manufacturing wooden molded products, The processed wood is characterized in that, when the processed wood is hydrolyzed with sulfuric acid, and the sulfuric acid is then removed from the resulting treatment liquid, the recovered liquid is subjected to liquid chromatography, and the ratio of the total amount of sugar components derived from hemicellulose to the total amount of sugar components is 14 to 21 mass% for softwood and 13 to 20 mass% for hardwood. (2) A method for producing the lumber for processing described in (1) above, comprising a step of contacting raw material lumber made of a coniferous or broad-leaved tree with a basic liquid. (3) A method for producing a wooden molded product, comprising a shaping step of subjecting the wood to be processed described in (1) above to a compression process or a bending process. (4) The method for producing a molded wooden product according to (3) above, further comprising a moisture adjustment step of adjusting the moisture content of the wood to be processed to 10% by mass or more prior to the shaping step. (5) A wooden molded product obtained by the method described in (3) above. (6) A wooden molded product according to the above (5) having a curved surface. (7) A wooden molded product according to the above (5), which has a coating on at least a part of its surface. (8) A composite body comprising the wooden molded product according to (5) above and another article integrated therewith. Effect of the Invention

[0009] The wood for processing of the present invention is suitable as a manufacturing material that can be used to produce wood molded products with excellent appearance in terms of grain and color tone by compression or bending, while suppressing defects such as cracks and splits. The wood for processing of the present invention is useful when producing wood molded products with curved surfaces. According to the method for producing a wooden molded product of the present invention, it is sufficient to apply compression processing or bending processing using a general-purpose mold or the like, and shaping can be easily performed without the use of an adhesive, thereby achieving the effect of reducing production costs. In addition, the number of processed wood pieces used in the shaping step may be one (1 piece) or two (2 pieces) or more, and a wooden molded product with excellent integrity and shape stability can be produced. The wood molded products of the present invention have excellent appearance regardless of their shape, and are therefore useful as everyday items such as tableware, cutlery, and trays, or as parts for ornaments, decorations, furniture, musical instruments, audio equipment, electrical appliances, vehicle interior parts, housing equipment, bathroom and washroom supplies, pet supplies, and cosmetic tools. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of compression processing (a method for manufacturing the wooden spoons used in Examples 3-1 and 3-2). [Diagram 2] FIG. 4 is a schematic cross-sectional view showing a cavity for a wooden spoon in the manufacturing method of FIGS. 1 and 3. [Diagram 3] FIG. 11 is a schematic cross-sectional view showing another example of compression processing (a manufacturing method for the wooden spoon used in Example 3-3). [Figure 4] 1 is a surface image of the convex portion of the bent softwood plate obtained in Example 2-1. [Diagram 5] 1 is a surface image of the convex portion of the bent softwood board obtained in Comparative Example 2-1. [Figure 6] 1 is a surface image of the convex portion of the hardwood bent plate obtained in Example 2-2. [Figure 7] 1 is a surface image of the convex portion of the hardwood bent plate obtained in Comparative Example 2-3. [Figure 8] 1 is a surface image of the convex portion of the hardwood bent plate obtained in Comparative Example 2-4. [Figure 9] 1 is a surface image of the convex portion of the hardwood bent plate obtained in Comparative Example 2-5. [Figure 10] 1 is an oblique image of the front surface of the coniferous wooden spoon obtained in Example 3-1. [Figure 11] 1 is an oblique image of the back surface of the coniferous wooden spoon obtained in Example 3-1. [Figure 12] 1 is an oblique image of the front surface of the hardwood wooden spoon obtained in Example 3-2. [Figure 13] 1 is an oblique image of the back surface of the hardwood wooden spoon obtained in Example 3-2. [Figure 14] 1 is an oblique image of the front surface of the hardwood wooden spoon obtained in Example 3-3. [Figure 15] 1 is an oblique image of the back surface of the hardwood wooden spoon obtained in Example 3-3. [Figure 16] 1 is an oblique image of the curved softwood material obtained in Example 4-1. [Figure 17]1 is an oblique image of the curved softwood material obtained in Example 4-2. [Figure 18] 1 is an oblique image of the curved softwood material obtained in Comparative Example 4-1. [Figure 19] 1 is an oblique image of the hardwood curved material obtained in Example 4-3. [Figure 20] 1 is an oblique image of the hardwood curved material obtained in Example 4-4. [Figure 21] FIG. 2 is a schematic cross-sectional view showing a manufacturing method for the wooden coaster used in Examples 5-1 and 5-2. [Figure 22] 22 is a schematic cross-sectional view showing a cavity for a wooden coaster in the manufacturing method of FIG. 21. [Diagram 23] 1 is a planar image of the coniferous coaster obtained in Example 5-1. [Figure 24] 1 is a planar image of the hardwood coaster obtained in Example 5-2. [Diagram 25] FIG. 1 is a schematic cross-sectional view showing a manufacturing method of the wooden salad bowl used in Example 6-1. [Figure 26] FIG. 26 is a schematic cross-sectional view showing a cavity for a wooden salad bowl in the manufacturing method of FIG. 25. [Figure 27] 1 is an oblique image of the front surface of the hardwood salad bowl obtained in Example 6-1. [Figure 28] 1 is an oblique image of the back surface of the hardwood salad bowl obtained in Example 6-1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The wood for processing of the present invention is a processed product made from a raw material of a coniferous or broad-leaved tree, and is used as a raw material (manufacturing material) for manufacturing a wooden molded product by compression processing or bending processing. The wood for processing of the present invention is hydrolyzed with sulfuric acid, and then the sulfuric acid is removed from the resulting treatment liquid, and the liquid recovered is subjected to liquid chromatography to quantify the detected glucose, arabinose, rhamnose, galactose, xylose, and mannose. The total amount of these neutral sugars, that is, the ratio of the total amount of hemicellulose-derived sugar components (arabinose, rhamnose, galactose, xylose, and mannose) to the total amount of sugar components (hereinafter referred to as "hemicellulose content"), is within a specific range. That is, when the raw material is a coniferous tree, the hemicellulose content of the wood for processing of the present invention is 14 to 21% by mass, preferably 15 to 20% by mass, and when the raw material is a broad-leaved tree, the hemicellulose content of the wood for processing of the present invention is 13 to 20% by mass, preferably 14 to 19% by mass.

[0012] The wood for processing of the present invention can be said to be "wood from which hemicellulose has been partially removed" because the hemicellulose content is lower than that of the raw wood. The inventors believe that the wood for processing having a hemicellulose content in each of the above ranges has a structure in which a part of the hemicellulose that was bonded to the cellulose by hydrogen bonds has been removed from the cellulose around the cellulose in the raw wood, although the content of the lignin having a three-dimensional network structure is not significantly different from that of the raw wood. For example, on the surface of a board-shaped material, although the lines of the annual rings may be slightly meandering, the formation of the removed part of hemicellulose makes the lignin easier to move, and when such wood for processing is subjected to compression processing, the shape retention of the wood molded product due to the lignin is improved, and a wood molded product with clear wood grain can be obtained. In addition, defects such as cracks and splits are suppressed in both compression processing and bending processing. Note that when the hemicellulose content exceeds the upper limit, cracks, splits, etc. are more likely to occur due to compression processing or bending processing. Furthermore, wood for processing that falls below the lower limit may have tree rings that are significantly meandering or crushed, and although it is possible to obtain a wood product by compression or bending, the wood product will not have a clear grain.

[0013] The method for measuring the hemicellulose content is as follows. After preferably pulverizing the wood to be processed, the powder sample is brought into contact with a 60 to 85% by mass aqueous sulfuric acid solution to carry out primary hydrolysis. Next, water is added to the aqueous sulfuric acid solution to dilute the sulfuric acid concentration to 2 to 10% by mass to carry out secondary hydrolysis, after which the wood to be processed is removed and the treatment liquid containing sulfuric acid is collected. Then, this treatment liquid is brought into contact with an anion exchange resin to remove sulfuric acid and collect the effluent. The effluent is then subjected to liquid chromatography for sugar analysis. As the anion exchange resin, an acetate-type anion exchange resin that adsorbs sulfate ions is preferably used.

[0014] As described above, the wood for processing of the present invention is made from coniferous or broad-leaved trees. As coniferous trees, cedar, cypress, pine, larch, Yezo spruce, Todomatsu, Tsuga, fir, ginkgo, Japanese zelkova, etc. can be used. As broad-leaved trees, magnolia, beech, oak, cherry, paulownia, zelkova, maple, chestnut, etc. can be used.

[0015] The shape of the wood to be processed of the present invention is not particularly limited. The shape of the wood to be processed may be a block, a plate, a line (rod), or a deformed shape (irregular shape) thereof. When the wood to be processed is a block, it may be a polyhedron, a cone, a sphere, or the like. When the wood to be processed is a deformed shape, it may be a polyhedron or a sphere with a through hole, a cylinder, a cylinder with a bottom, or the like. The surface of the wood to be processed when manufacturing a wood molded product by compression processing may be either a smooth surface or a rough surface.

[0016] The size of the processed wood material of the present invention is not particularly limited, but from the viewpoint of moldability by compression and bending and the shape stability of the resulting wood molded product, the maximum thickness in the compression direction during production of the wood molded product is preferably 100 mm, more preferably 30 mm, even more preferably 15 mm, and particularly preferably 7 mm.

[0017] The wood material for processing of the present invention is preferably a plate-shaped material or a linear material. In the case of a plate-shaped material, it may be a plate having a uniform cross-sectional shape and thickness from one end to the other end, or a plate having a portion of non-uniform thickness (such as a plate having one or more curved portions on the surface).

[0018] The wood to be processed according to the present invention may be either bone dry or hydrated.

[0019] The method for producing wood for processing of the present invention (hereinafter referred to as "the method for producing wood for processing of the present invention") comprises a step of contacting raw wood made of a softwood or hardwood with a basic liquid (hereinafter referred to as "basic liquid contact step"). After the basic liquid contact step, the method for producing wood for processing of the present invention can further comprise a step of removing the basic liquid adhering to the wood for processing (hereinafter referred to as "basic liquid removal step"), a step of drying the wood for processing (hereinafter referred to as "drying step"), etc., as necessary.

[0020] The raw wood material is made of the above-mentioned coniferous or broad-leaved trees, and although its shape is not particularly limited, it is preferable that the raw wood material has a shape in which the cross grain and straight grain can be recognized. The raw wood material may be in the form of a block, a plate, a line (rod), or a deformed shape (irregular shape) thereof. When the raw wood material is in the form of a block, it may be in the form of a polyhedron, a cone, a sphere, or the like. When the raw wood material is in the form of a deformed shape, it may be in the form of a body having a notch, a body having a through hole, a cylinder, a cylinder with a bottom, or the like. The raw wood material in the present invention may be scrap wood from a lumber mill or the like.

[0021] The size of the raw wood material is not particularly limited, but in order to efficiently obtain wood material suitable for compression and bending processing, for example, the maximum thickness of the raw wood material when obtaining wood material to be thinned by compression processing is preferably 110 mm, more preferably 50 mm, and even more preferably 25 mm.

[0022] The basic liquid used in the basic liquid contact step according to the present invention may contain at least one basic compound selected from inorganic materials and organic materials, which dissolves in a medium and exhibits basicity, or a basic liquid organic compound. The pH of the basic liquid is not particularly limited, but in the present invention, it is preferably a basic aqueous solution in which a basic compound is dissolved in water as a medium. In this case, the medium may contain a water-soluble organic solvent as necessary.

[0023] The basic liquid according to the present invention is preferably a basic aqueous solution in which an inorganic material is dissolved in water. Examples of the inorganic material include metal hydroxides, metal hydrogen carbonates, and metal carbonates. The basic liquid may contain only one type of inorganic material or two or more types of inorganic materials.

[0024] Examples of the metal hydroxide include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide; and alkaline earth metal hydroxides such as magnesium hydroxide and calcium hydroxide. Examples of the metal hydrogen carbonate include alkali metal hydrogen carbonate such as sodium hydrogen carbonate and potassium hydrogen carbonate; and alkaline earth metal hydrogen carbonate such as magnesium hydrogen carbonate and calcium hydrogen carbonate. Examples of the metal carbonate include alkali metal carbonates such as sodium carbonate and potassium carbonate; and alkaline earth metal carbonates such as magnesium carbonate, calcium carbonate and barium carbonate.

[0025] In the basic liquid contacting step, the raw wood material is preferably contacted with the basic liquid under mild conditions as described below. That is, in order to avoid excessive removal of lignin from the raw wood material and to release a portion of the hemicellulose bonded to cellulose by hydrogen bonds, for example, mild conditions can be configured by adjusting the concentration of the basic compound in the basic liquid, the temperature of the basic liquid contacted with the raw wood material, and the contact time between the raw wood material and the basic liquid, and wood material for processing that can be used to produce wood molded products with excellent appearance by compressing or bending the raw wood material, i.e., wood material from which hemicellulose has been partially removed, can be obtained.

[0026] The concentration of the basic compound in the basic liquid is preferably 0.04 to 6.5 mol / L, more preferably 0.5 to 2.0 mol / L, and even more preferably 0.7 to 1.2 mol / L. The temperature of the basic liquid brought into contact with the raw wood is preferably 20°C to 170°C, more preferably 50°C to 160°C, and even more preferably 80°C to 150°C. Therefore, the contact time between the raw wood and the basic liquid is preferably 0.5 to 48 hours.

[0027] In the basic liquid contacting step, the method of contacting the raw wood with the basic liquid is not particularly limited. For example, the raw wood may be contacted with the basic liquid in a container, or the basic liquid may be continuously applied to the raw wood placed (fixed) at a predetermined position.

[0028] As described above, the method for producing wood for processing of the present invention can further include, after the basic liquid contacting step, a basic liquid removing step, a drying step, etc. Since the basic liquid contacting step produces wood for processing wet with the basic liquid (wood from which hemicellulose has been partially removed), it is preferable to include a basic liquid removing step for removing the basic liquid adhering to the wood for processing in order to obtain clean wood for processing.

[0029] In the basic liquid removal step, a method of washing with a neutral liquid, an acidic liquid, or the like can be applied. The neutral liquid can be water, and the acidic liquid can be an aqueous citric acid solution. This basic liquid removal step can be a step using one type of neutral liquid (preferably water), or a multi-stage step using two or more types of neutral liquid. In the case of a multi-stage step, it is preferable to use water at the end. In the basic liquid removal step, ultrasonic vibration can be used. The neutral liquid and the acidic liquid used can be heated.

[0030] When water is used in the basic liquid removal step, it is possible to obtain wood from which hemicellulose has been partially removed in a hydrated state. As described above, the wood for processing of the present invention may be a hydrated material, and therefore the production of the wood for processing can be completed by the basic liquid removal step using water.

[0031] When manufacturing wood for processing having a low moisture content or wood for processing in an absolutely dry state, it is preferable to carry out a drying step after the basic liquid removal step. In this drying step, heat drying, reduced pressure drying, air drying, etc. can be applied.

[0032] The method for producing a wooden molded product of the present invention (hereinafter referred to as the "method for producing a wooden molded product of the present invention") comprises a shaping step in which wood to be processed is subjected to compression or bending. After the shaping step, the method for producing a wooden molded product of the present invention may further comprise a shape adjustment step of polishing the wooden molded product or the like, a film formation step of forming a protective film or the like on the surface of the wooden molded product, etc., as necessary.

[0033] In the shaping process according to the present invention, at least one of compression and bending is usually performed on the grain surface or end surface of the wood to be processed, and this may involve not only simple thinning and bending but also deformation such as twisting. The wood to be processed used in this shaping process may be one (one sheet) or two (two sheets) or more. Even if multiple pieces of wood to be processed are combined and compressed, an integrated wood molded product with excellent appearance and shape stability can be produced. In the present invention, such a wood molded product can be obtained without using an adhesive.

[0034] When compression processing is performed, a mold having a cavity having the shape of the wooden molded product to be produced or a shape slightly larger than the shape is preferably used. Figures 1 and 2 are cross-sectional views showing an example of a method for producing a wooden molded product (wooden spoon) having the shape of the cavity 17 in Figure 2 by subjecting one piece of wood to be processed 11 to compression processing using a mold having an upper mold 13 and a lower mold 15. Figure 3 is a cross-sectional view showing an example of a method for producing a wooden molded product (wooden spoon) having the shape of the cavity 17 in Figure 2 by subjecting a plurality of pieces of wood to be processed 11X to compression processing using a mold having an upper mold 13 and a lower mold 15. In the present invention, even if a wooden molded product has a curved surface like a spoon, defects such as cracks and splits are suppressed, and it is possible to efficiently produce a wooden molded product having excellent appearance in terms of grain and color tone.

[0035] In the case of compression processing, shearing may occur during compression processing depending on the shape of the wood product to be produced and the shape of the wood used for production. For example, in order to produce a wood product with a recess, punching is performed on the center of a block of wood to be processed or on the center of a plurality of stacked plank-shaped wood to be processed to form a recess reflecting the shape of the tip of the punch, in the punching process, the side surface of the periphery of the tip of the punch that bites into the wood to be processed may cause sliding shear deformation. In the present invention, even if such shearing occurs, a wood product with excellent appearance can be produced.

[0036] In the case of bending, it is preferable to fix at least two points of the peripheral portion of the wood to be processed. A mold used in compression processing may also be used.

[0037] In the shaping step, the compression or bending process may be performed while heating, as long as the wood to be processed is not deteriorated. The upper limit of the heating temperature is preferably 180° C., more preferably 150° C. When shaping is performed using a mold, it is preferable to perform the molding at 60° C. or higher.

[0038] The wood to be processed in the shaping step is preferably a water-containing material from the viewpoint of moldability. In this case, the lower limit of the moisture content of the wood to be processed is preferably 10% by mass, more preferably 15% by mass, and even more preferably 20% by mass. In addition, when the wood to be processed in the shaping step is a bone-dry material or the like, which has a low moisture content, it is preferable to provide a moisture adjustment step for adjusting the moisture content of the wood to be processed to 10% by mass or more before the shaping step. In order to achieve such a moisture content, water or a mixture of water and an organic solvent can be used. Examples of the method of contacting the wood to be processed with water or the like include a method of contacting the wood to be processed with water or the mixture in a container, a method of spraying the wood to be processed with water or the mixture, and a method of exposing the wood to an atmosphere containing water vapor.

[0039] The shaping step according to the present invention may be a step in which compression or bending is performed only once, or may be a step in which compression or bending is performed in multiple stages depending on the shape of the wooden molded product to be manufactured. In the latter case, it is preferable to bring the wood to be processed into contact with water or the above-mentioned mixed liquid before the second and subsequent processing.

[0040] As described above, the method for producing a molded wooden product of the present invention can further include, after the shaping step, a shape adjusting step, a painting step, etc. Since the molded wooden product obtained by the present invention can be used alone or can be combined with other articles to be used as a component of an integrated composite product, it is preferable to include a shape adjusting step of polishing, drilling, etc. In the film formation process, paint or the like is applied to at least a portion of the surface of the wooden molded product and dried, and if necessary, radiation (ultraviolet rays, etc.) or heating can be performed. If the film is transparent, the clear wood grain of the wooden molded product before coating can be easily seen.

[0041] As described above, the wood molded product of the present invention can be not only a structure having a curved surface and a structure having a coating on at least a portion of its surface, but also a structure with clear ridges, a structure with varying board thickness, etc.

[0042] The composite of the present invention is a product in which a wood molded product having excellent appearance is integrated with another article. This integration can be achieved by using an adhesive, a joining member, or by fitting. The material of the other article is not particularly limited. EXAMPLES

[0043] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0044] 1. Manufacturing of wood for processing The logs were cut and processed to produce softwood boards and hardwood boards with cross grain or straight grain, respectively, from Japanese cedar (coniferous tree) and magnolia (broad-leaved tree), and then each board was immersed in an aqueous solution of sodium hydroxide or sodium carbonate to obtain softwood processing lumber and hardwood processing lumber. The hemicellulose content in each processing lumber was then quantified by high performance liquid chromatography using the following method. The hemicellulose content was also measured for the logs.

[0045] <Method for measuring hemicellulose content> The object to be analyzed (log or wood for processing) was dried to an air-dry state, and then the dried sample was crushed, and the powder that passed through a 40 mesh screen was used as the measurement sample. After that, 3 ml of 72% by mass sulfuric acid was added to 0.35 g of the sample according to the method based on JAPAN TAPPI Paper Pulp Test Method No. 42, and hydrolysis was performed (30°C, 1 hour). Then, 84 ml of pure water was added to this reaction solution, and it was placed in a sterilization autoclave and further hydrolysis was performed (121°C, 103±7 kPa, 1 hour). Next, the hydrolyzed liquid was cooled to room temperature and filtered to recover the filtrate. The filtrate was then placed in a measuring flask, and pure water was added to make a total of 200 milliliters (hereinafter referred to as "sugar component-containing liquid"). Then, 2 milliliters of this sugar component-containing liquid was passed through a column filled with 20 milliliters of an acetic acid preparation of an anion exchange resin "Amberlite IRA400" (trade name) to remove sulfate ions, and the ion exchange resin was washed with 10 milliliters of a 5% by mass aqueous acetic acid solution and 100 milliliters or more of pure water to obtain a sugar component solution. Then, this solution was evaporated to dryness, and the dried product was dissolved in 2 milliliters of pure water, and this aqueous solution was subjected to the following liquid chromatography. This allowed the detection of glucose, arabinose, rhamnose, galactose, xylose and mannose, and the resulting chromatogram was analyzed. The total amount of hemicellulose-derived sugar components (arabinose, rhamnose, galactose, xylose and mannose) not converted into anhydrous sugars was divided by the total amount of glucose, arabinose, rhamnose, galactose, xylose and mannose not converted into anhydrous sugars, and the percentage was calculated to be the "hemicellulose content." Column: Thermo Scientific (Dionex) "CarbPac TM PA1" (Size: φ4mm x 250mm) Eluent: Water (flow rate: 0.6 ml / min), 0.6 M sodium hydroxide solution added at 0.3 ml / min post-column Detector: Pulsed electrochemical detector with gold working electrode

[0046] Example 1-1 (Production of softwood lumber for processing) A number of sheets (softwood sheets) measuring 90 mm (lengthwise direction of fibers) x 60 mm (orthogonal direction of fibers) x 6 mm (thickness) or a number of sheets (softwood sheets) measuring 180 mm (lengthwise direction of fibers) x 50 mm (orthogonal direction of fibers) x 10 mm (thickness) were placed in a reaction vessel containing 1M-NaOH aqueous solution and immersed at 130°C for 2 hours, then removed and washed with water. The alkali-treated wood was then sandwiched between two wire meshes and dried at 30°C to obtain softwood processing wood with a hemicellulose content of 19.6% by mass.

[0047] Example 1-2 (Production of softwood lumber for processing) The same operations as in Example 1-1 were carried out using multiple sheets of board material (coniferous board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction to the fibers) x 6 mm (thickness), except that the temperature of the 1M NaOH aqueous solution was set to 150°C, to obtain coniferous processing lumber with a hemicellulose content of 19.1% by mass.

[0048] Example 1-3 (Production of softwood lumber for processing) The same operations as in Example 1-1 were carried out using multiple sheets of board material (coniferous board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction of the fibers) x 6 mm (thickness), and except that the temperature of the 1M NaOH aqueous solution was 140°C and the immersion time was 4 hours, coniferous processing lumber with a hemicellulose content of 18.1% by mass was obtained.

[0049] Example 1-4 (Production of softwood lumber for processing) A plate material (coniferous plate material) measuring 105 mm (lengthwise direction of the fibers) x 105 mm (orthogonal direction of the fibers) x 12 mm (thickness) was used, and the same operation as in Example 1-1 was carried out, except that the temperature of the 1M NaOH aqueous solution was set to 150°C, to obtain coniferous processing lumber with a hemicellulose content of 20.1% by mass.

[0050] Comparative Example 1-1 (Production of softwood lumber for processing) Using multiple sheets of softwood boards measuring 90 mm (lengthwise direction of fibers) x 60 mm (orthogonal direction of fibers) x 6 mm (thickness), 1M-NaOH solution at 130°C was replaced with 0.5M-Na 2 CO 3 The same procedure as in Example 1-1 was carried out except that an aqueous solution was used, to obtain softwood lumber for processing having a hemicellulose content of 22.4 mass %.

[0051] Comparative Example 1-2 (Production of softwood lumber for processing) The same operations as in Example 1-1 were carried out using multiple sheets (softwood sheets) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction to the fibers) x 6 mm (thickness), and the temperature of the 1M NaOH aqueous solution was 160°C, and the immersion time was 4 hours, to obtain softwood processing lumber with a hemicellulose content of 13.4% by mass.

[0052] Example 1-5 (Production of hardwood lumber for processing) A similar procedure to that of Example 1-1 was carried out using multiple pieces of board material (hardwood board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction of the fibers) x 6 mm (thickness), or multiple pieces of board material (coniferous wood board material) measuring 180 mm (lengthwise direction of the fibers) x 50 mm (orthogonal direction of the fibers) x 10 mm (thickness), and except that the temperature of the 1M NaOH aqueous solution was set to 140°C, hardwood processing lumber with a hemicellulose content of 17.8% by mass was obtained.

[0053] Example 1-6 (Production of hardwood lumber for processing) The same operations as in Example 1-1 were carried out using multiple sheets of board material (hardwood board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction of the fibers) x 6 mm (thickness), except that the temperature of the 1M NaOH aqueous solution was set to 150°C, and hardwood processing lumber with a hemicellulose content of 16.1% by mass was obtained.

[0054] Example 1-7 (Production of hardwood lumber for processing) The same operations as in Example 1-1 were carried out using multiple sheets of board material (hardwood board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction of the fibers) x 6 mm (thickness), with the exception that the temperature of the 1M NaOH aqueous solution was 130°C and the immersion time was 4 hours, to obtain hardwood processing lumber with a hemicellulose content of 19.3% by mass.

[0055] Example 1-8 (Production of hardwood lumber for processing) The same operations as in Example 1-1 were carried out using multiple sheets of board material (hardwood board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction of the fibers) x 6 mm (thickness) and a 2.68 M aqueous NaOH solution, with the exception that the temperature of the NaOH aqueous solution was 80°C and the immersion time was 4 hours, to obtain hardwood processing lumber with a hemicellulose content of 20.0 mass%.

[0056] Example 1-9 (Production of hardwood lumber for processing) The same procedure as in Example 1-1 was carried out using multiple sheets of board material (hardwood board material) measuring 180 mm (lengthwise direction of the fibers) x 50 mm (orthogonal direction of the fibers) x 3 mm (thickness) and a 1M aqueous NaOH solution, with the exception that the temperature of the NaOH aqueous solution was 100°C and the immersion time was 4 hours, to obtain hardwood processing lumber with a hemicellulose content of 17.0% by mass.

[0057] Example 1-10 (Production of hardwood lumber for processing) A plate material (hardwood plate material) measuring 105 mm (lengthwise direction of the fibers) x 105 mm (orthogonal direction of the fibers) x 12 mm (thickness) was used, and the same operations as in Example 1-1 were carried out, except that the temperature of the 1M NaOH aqueous solution was set to 150°C, to obtain hardwood processing lumber with a hemicellulose content of 17.1% by mass.

[0058] Example 1-11 (Production of hardwood lumber for processing) A board material (hardwood board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction of the fibers) x 6 mm (thickness) and a 1M aqueous NaOH solution were used. Except for setting the temperature of the NaOH aqueous solution to 130°C and the immersion time to 4 hours, the same procedure as in Example 1-1 was carried out to obtain hardwood processing lumber with a hemicellulose content of 15.6% by mass.

[0059] Comparative Example 1-3 (Manufacture of hardwood lumber for processing) The same operations as in Example 1-1 were carried out using multiple sheets of board material (hardwood board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction to the fibers) x 6 mm (thickness), with the exception that the temperature of the 1M NaOH aqueous solution was 160°C and the immersion time was 4 hours, to obtain hardwood processing lumber with a hemicellulose content of 11.9% by mass.

[0060] Comparative Example 1-4 (Manufacture of hardwood lumber for processing) Using multiple sheets of hardwood boards measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction of the fibers) x 6 mm (thickness), 1M-Na 2 CO 3 The same procedure as in Example 1-1 was carried out except that the temperature of the aqueous solution was 130° C. and the immersion time was 2 hours, to obtain hardwood lumber for processing having a hemicellulose content of 20.7 mass %.

[0061] Comparative Example 1-5 (Manufacture of hardwood lumber for processing) The same operations as in Example 1-1 were carried out using multiple sheets of board material (hardwood board material) measuring 90 mm (lengthwise direction of the fibers) x 60 mm (orthogonal direction of the fibers) x 6 mm (thickness), with the exception that the temperature of the 0.05 M NaOH aqueous solution was 120°C and the immersion time was 3 hours, to obtain hardwood processing lumber with a hemicellulose content of 22.0 mass%.

[0062] The hemicellulose contents of the above-mentioned softwood and hardwood logs were measured and found to be 28.3% by mass and 25.1% by mass, respectively.

[0063] 2. Manufacturing and evaluation of wood molded products The softwood or hardwood processing wood obtained in Examples 1-1 to 1-11 and Comparative Examples 1-1 to 1-5 was subjected to compression or bending to produce wooden molded products, and their appearance was evaluated visually.

[0064] Example 2-1 The softwood processing lumber (hemicellulose content: 19.6% by mass) produced in Example 1-1 was cut and processed into a disk (diameter: 53 mm, thickness: 6 mm). The disk was then placed in a thermostatic chamber and left to stand under conditions of a temperature of 40°C and a humidity of 90%. After 48 hours, it was removed to obtain a softwood processing raw material with a moisture content of 30%. The raw material for processing softwood was then placed in a mold (set temperature: 90°C) that formed a hemispherical cavity with a radius of curvature of 40 mm, and the upper mold was lowered at a speed of 30 mm per second to compress the raw material for processing softwood. When the load reached 2 tons, the upper mold was held in place, and one minute later, the temperature of the mold was cooled to about 30°C. After five minutes, the mold was removed to obtain a bent board (see Figure 4). As is clear from Figure 4, the bent board obtained had no cracks or splits and had excellent grain and color.

[0065] Comparative Example 2-1 A bent plate was obtained by the same procedure as in Example 2-1, except that a disk (diameter: 53 mm, thickness: 6 mm) made of the softwood board material (untreated material) used in the manufacture of softwood processing wood (hemicellulose content: 19.6% by mass) in Example 1-1 was used instead of the softwood processing wood (see FIG. 5). As is clear from FIG. 5, cracks were confirmed on the surface.

[0066] Example 2-2 Except for using the disk (diameter: 53 mm, thickness: 6 mm) made of hardwood processing wood (hemicellulose content: 17.8 mass%) prepared in Example 1-5 instead of the softwood processing wood, the same operation as in Example 2-1 was carried out to prepare a hardwood processing raw material, and then a bent board was obtained (see FIG. 6). As is clear from FIG. 6, the obtained bent board had no cracks or splits and had excellent grain and color.

[0067] Comparative Example 2-2 A bent plate was obtained by the same procedure as in Example 2-1, except that a disk (diameter: 53 mm, thickness: 6 mm) made of the hardwood plank material (untreated material) used in the manufacture of hardwood plank material (hemicellulose content: 17.8% by mass) in Example 1-5 was used instead of the softwood plank material (see FIG. 7). As is clear from FIG. 7, cracks were confirmed on the surface.

[0068] Comparative Example 2-3 Except for using a disk (diameter: 53 mm, thickness: 6 mm) made of hardwood processing wood (hemicellulose content: 20.7 mass%) prepared in Comparative Example 1-4 instead of softwood processing wood, the same operation as in Example 2-1 was carried out to prepare a hardwood processing raw material, and then a bent board was obtained (see FIG. 8). As is clear from FIG. 8, cracks were confirmed on the surface.

[0069] Comparative Example 2-4 Except for using a disk (diameter: 53 mm, thickness: 6 mm) made of hardwood processing wood (hemicellulose content: 22.0 mass%) prepared in Comparative Example 1-5 instead of softwood processing wood, the same operation as in Example 2-1 was carried out to prepare a hardwood processing raw material, and then a bent board was obtained (see FIG. 9). As is clear from FIG. 9, cracks were confirmed on the surface.

[0070] Example 3-1 The softwood processing lumber (hemicellulose content: 19.6% by mass) produced in Example 1-1 was cut and processed into a rectangular board (length: 180 mm, width: 50 mm, thickness: 10 mm). This board was then placed in a thermo-hygrostat and left to stand under conditions of a temperature of 40°C and a humidity of 90%. After 48 hours, it was removed to obtain a softwood processing raw material with a moisture content of 30%. Then, as shown in FIG. 1, the raw material for processing of softwood (material 11) was subjected to compression processing using a spoon manufacturing mold equipped with an upper mold 13 and a lower mold 15 to manufacture a wooden spoon reflecting the cavity shape of FIG. 2. The manufacturing method is as follows. After the spoon manufacturing mold was heated to 120°C in advance, the material 11 was placed at a predetermined position on the lower mold 15, and the upper mold was lowered at a speed of 5 mm per second to compress the material 11. The mold was clamped for 15 minutes, after which the temperature of the mold was cooled to about 30°C, and the mold was demolded to obtain a wooden spoon derived from softwood (see FIG. 10 and FIG. 11). As is clear from FIG. 10 showing the front side of the wooden spoon and FIG. 11 showing the back side of the wooden spoon, the obtained wooden spoon had no cracks or splits and had excellent grain and color.

[0071] Example 3-2 Instead of the softwood processing wood, the hardwood processing wood (hemicellulose content: 17.8% by mass) prepared in Example 1-3 was subjected to the same operation as in Example 3-1 to prepare a processing material 11, and then a hardwood-derived wooden spoon was obtained (see Figs. 12 and 13). As is clear from Fig. 12 showing the front side of the wooden spoon and Fig. 13 showing the back side of the wooden spoon, the obtained wooden spoon had no cracks or splits and had excellent grain and color.

[0072] Example 3-3 The hardwood processing lumber (hemicellulose content: 17.0% by mass) produced in Example 1-9 was cut and processed into a rectangular board (length: 180 mm, width: 50 mm, thickness: 3 mm). This board was then placed in a thermo-hygrostat and left to stand under conditions of a temperature of 40°C and a humidity of 90%. After 48 hours, it was removed to obtain a hardwood processing raw material (processing material 11X) with a moisture content of 30%. Thereafter, as shown in Fig. 3, four sheets of the blank 11X were stacked and compressed using a spoon manufacturing die equipped with an upper die 13 and a lower die 15 to manufacture a wooden spoon reflecting the cavity shape of Fig. 2. The specific manufacturing method is as follows. After the spoon manufacturing mold was heated to 90°C in advance, the four sheets of processing material 11X were placed in a stacked state on the lower mold 15 at a predetermined position, and the upper mold was lowered at a speed of 5 mm per second to perform compression processing. The mold was clamped for 15 minutes, after which the temperature of the mold was cooled to about 30°C, and the mold was demolded to obtain a wooden spoon derived from hardwood (see Figures 14 and 15). As is clear from Figure 14 showing the front side of the wooden spoon and Figure 15 showing the back side of the wooden spoon, the obtained wooden spoon had no cracks or splits and had excellent wood grain and color. In addition, the bonding state of the four sheets of processing material 11X, which are raw materials, was good, and there was no problem of peeling at the adhesive interface.

[0073] Example 4-1 The softwood processing wood (hemicellulose content: 19.1% by mass) produced in Example 1-2 was cut and processed into linear material (length: 50 mm, width: 10 mm, thickness: 6 mm), and then this linear material was subjected to a moisture-imparting treatment similar to that in Example 2-1 to obtain softwood processing linear material with a moisture content of 30%. The wire material was then placed in a die (set temperature: 120°C) that formed a hemispherical cavity with a radius of curvature of 40 mm, and the upper die was lowered at a speed of 30 mm per second to bend the wire material. The upper die was then held when the clearance became 6 mm, and one minute later, the die temperature was cooled to about 30°C. After five minutes, the wire material was removed from the die to obtain a curved material (see Figure 16). As is clear from Figure 16, the curved material obtained had no cracks or splits and had excellent grain and color.

[0074] Example 4-2 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the softwood processing wood (hemicellulose content: 19.6% by mass) produced in Example 1-1 was subjected to the same operation as in Example 4-1 to produce a softwood processing wire material with a moisture content of 30%. The wire material was then bent to obtain a curved material (see FIG. 17). As is clear from FIG. 17, the curved material obtained had no cracks or splits and had excellent grain and color.

[0075] Example 4-3 The softwood processing wood (hemicellulose content: 19.1% by mass) produced in Example 1-2 was cut and processed to form a linear material (length: 50 mm, width: 10 mm, thickness: 6 mm). The linear material was then placed in a thermohygrostat and left to stand under conditions of a temperature of 22°C and a humidity of 60%, and after 48 hours, it was removed to obtain a softwood processing linear material with a moisture content of 10%. Thereafter, the softwood processing linear material was bent in the same manner as in Example 4-1 to obtain a curved material. The obtained curved material had no cracks or splits and had excellent grain and color (not shown).

[0076] Example 4-4 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the softwood processing wood (hemicellulose content: 18.1% by mass) produced in Example 1-3 was subjected to the same operation as in Example 4-1 to produce a softwood processing wire material with a moisture content of 30%. The wire material was then bent to obtain a curved material. The curved material obtained was free of cracks and splits and had excellent grain and color (not shown).

[0077] Comparative Example 4-1 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the softwood processing wood (hemicellulose content: 22.4% by mass) produced in Comparative Example 1-1 was subjected to the same operation as in Example 4-1 to produce a softwood processing wire with a moisture content of 30%. When the wire was then bent, cracks occurred and a softwood curved wire was not obtained (see FIG. 18).

[0078] Comparative Example 4-2 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the softwood processing wood (hemicellulose content: 13.4% by mass) produced in Comparative Example 1-2 was subjected to the same operation as in Example 4-1 to produce a softwood processing linear material. When bending was then performed, cracks occurred and a softwood curved material was not obtained (not shown).

[0079] Examples 4-5 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the hardwood processing wood (hemicellulose content: 16.1% by mass) produced in Example 1-6 was subjected to the same operation as in Example 4-1 to produce a hardwood processing wire material with a moisture content of 30%. The wire material was then bent to obtain a hardwood curved material (see FIG. 19). As is clear from FIG. 19, the curved material obtained had no cracks or splits and had excellent grain and color.

[0080] Examples 4-6 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the hardwood processing wood (hemicellulose content: 16.1% by mass) produced in Example 1-6 was subjected to the same operation as in Example 4-3 to produce a hardwood processing wire material with a moisture content of 10%. The wire material was then bent to obtain a hardwood curved material. The curved material obtained was free of cracks and splits and had excellent grain and color (not shown).

[0081] Examples 4-7 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the hardwood processing wood (hemicellulose content: 17.8% by mass) produced in Example 1-5 was subjected to the same operation as in Example 4-1 to produce a hardwood processing wire material with a moisture content of 30%. The wire material was then bent to obtain a hardwood curved material (see FIG. 20). As is clear from FIG. 20, the curved material obtained had no cracks or splits and had excellent grain and color.

[0082] Examples 4-8 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the hardwood processing wood (hemicellulose content: 19.3% by mass) produced in Example 1-7 was subjected to the same operation as in Example 4-1 to produce a hardwood processing wire material with a moisture content of 30%. The wire material was then bent to obtain a hardwood curved material. The curved material obtained was free of cracks and splits and had excellent grain and color (not shown).

[0083] Examples 4-9 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the hardwood processing wood (hemicellulose content: 20.0% by mass) produced in Example 1-8 was subjected to the same operation as in Example 4-3 to produce a hardwood processing linear material with a moisture content of 10%. The hardwood was then bent to produce a curved material. The curved material obtained was free of cracks and splits and had excellent grain and color (not shown).

[0084] Comparative Example 4-3 Instead of the softwood processing wood (hemicellulose content: 19.1% by mass), the hardwood processing wood (hemicellulose content: 11.9% by mass) produced in Comparative Example 1-3 was subjected to the same operation as in Example 4-1 to produce a hardwood processing wire with a moisture content of 30%. When the wire was then bent, cracks occurred and a hardwood curved wire was not obtained (not shown).

[0085] Example 5-1 The softwood processing lumber (hemicellulose content: 20.1% by mass) produced in Example 1-4 was cut and processed into a square board (length: 150 mm, width: 150 mm, thickness: 12 mm). This board was then placed in a thermostatic and hygrostatic chamber and left to stand under conditions of a temperature of 40°C and a humidity of 90%. After 48 hours, it was removed to obtain a softwood processing raw material with a moisture content of 30%. Then, as shown in FIG. 21, this raw material for processing of softwood (material 11) was subjected to compression processing using a coaster manufacturing die equipped with an upper die 13 and a lower die 15 to produce a wooden coaster reflecting the cavity shape 17 of FIG. 22. The manufacturing method is as follows. After the coaster manufacturing die is heated to 120°C in advance, the material 11 was placed at a predetermined position on the lower die 15, and the upper die was lowered at a speed of 5 mm per second to compress the material 11. The die was clamped for 1 minute, after which the temperature of the die was cooled to about 30°C, and the product was demolded to obtain a softwood-derived wooden coaster (see FIG. 23). As is clear from FIG. 23, the obtained wooden coaster had no cracks or splits and had excellent grain and color.

[0086] Example 5-2 A square board (length: 150 mm, width: 150 mm, thickness: 12 mm) obtained by cutting and processing the hardwood processing lumber (hemicellulose content: 17.1% by mass) prepared in Example 1-10 was used instead of the softwood processing raw material, and the same operation as in Example 5-1 was carried out to obtain a wooden coaster derived from hardwood (see FIG. 24). As is clear from FIG. 24, the obtained wooden coaster had no cracks or splits and had excellent grain and color.

[0087] Example 6-1 The hardwood processing lumber (hemicellulose content: 15.6% by mass) produced in Example 1-11 was cut and processed into a circular board (diameter: 200 mm, thickness: 6 mm). This board was then placed in a thermostatic and hygrostatic chamber and left to stand under conditions of a temperature of 40°C and a humidity of 90%. After 48 hours, it was removed to obtain a hardwood processing raw material with a moisture content of 30%. Then, as shown in FIG. 25, this hardwood raw material (working material 11) was compressed using a salad bowl manufacturing mold equipped with upper mold 13 and lower mold 15 to produce a wooden salad bowl reflecting the cavity shape 17 of FIG. 26. The manufacturing method is as follows. After the salad bowl manufacturing mold was preheated to 90° C., the processing material 11 was placed in a predetermined position on the lower mold 15, and the upper mold was lowered at a speed of 1 mm per second to compress the processing material 11. The mold was clamped for 20 minutes, after which the temperature of the mold was cooled to about 30° C. and the mold was demolded to obtain a wooden salad bowl derived from hardwood (see FIG. 27 and FIG. 28). As is clear from FIG. 27, which shows the front side of the wooden salad bowl, and FIG. 28, which shows the back side of the wooden salad bowl, the obtained wooden salad bowl was free of cracks and splits and had excellent grain and color. [Industrial Applicability]

[0088] The wood for processing of the present invention is suitable as a material for producing wooden molded products having excellent appearance in terms of grain and color tone. The wood molded product of the present invention, and a composite body obtained by integrating this wood molded product with other articles, are useful as daily necessities (tableware, cutlery, trays, etc.), ornaments, decorations, furniture, musical instruments, audio equipment, electrical appliances, vehicle interior parts, housing equipment, bathroom and washroom supplies, pet supplies, cosmetic tools, etc. [Explanation of symbols]

[0089] 11:Material for processing 13: Upper mold 15: Lower mold 17: Spoon-shaped, coaster-shaped or salad bowl-shaped cavity

Claims

1. A processed wood material made of coniferous or broad-leaved trees and used as a raw material for manufacturing wooden molded products, The processed wood is characterized in that, when the processed wood is hydrolyzed with sulfuric acid, and then the sulfuric acid is removed from the resulting treatment liquid, and the recovered liquid is subjected to liquid chromatography, the ratio of the total amount of sugar components derived from hemicellulose to the total amount of sugar components is 14 to 21 mass% for softwood and 13 to 20 mass% for hardwood.

2. 2. A method for producing the lumber for processing according to claim 1, comprising a step of contacting raw material lumber made of a softwood or hardwood with a basic liquid.

3. 13. A method for producing a molded wooden product, comprising a shaping step of subjecting the wood to be processed according to claim 1 to a compression process or a bending process.

4. The method for producing a molded wooden product according to claim 3, further comprising a moisture adjustment step of adjusting the moisture content of the wood to be processed to 10% by mass or more prior to the shaping step.

5. A wooden molded product obtained by the method according to claim 3.

6. 6. The wooden molded product according to claim 5, having a curved surface.

7. 6. The wooden molded product according to claim 5, which has a coating on at least a portion of its surface.

8. A composite body comprising the wooden molded product according to claim 1 and another article.

Citation Information

Patent Citations

  • Modifying method for timber

    JP1991231802A

  • Method for reforming lumber

    JP2010030081A