Nonlinear optical crystal of guanidine tetrafluoroborate, its manufacturing method and use

JP2024500986A5Active Publication Date: 2024-10-08XINJIANG TECH INST OF PHYSICS & CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023539044
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-12-26
Filing Date
2021-12-22
Publication Date
2024-10-08
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

Current ultraviolet and deep ultraviolet nonlinear optical crystals, such as LBO, CBO, CLBO, BBO, and KBBF, have limitations in birefringence and growth habits, restricting their application in the deep UV region, necessitating the development of new crystals with improved performance.

Method used

The development of a nonlinear optical crystal with the chemical formula [C(NH2)3]BF4, belonging to the trigonal system, featuring a UV cutoff edge of 200 nm, a frequency multiplication response 4-5 times that of KDP, and a large laser damage threshold, produced through methods like hydrothermal, room temperature solution, evaporation, or solvothermal processes.

Benefits of technology

The [C(NH2)3]BF4 crystal enables large-sized, high-quality optical crystals with stable physical and chemical properties, suitable for deep UV applications, and easy processing, offering wide wavelength range and high optical uniformity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A nonlinear optical crystal of guanidine tetrafluoroborate and its preparation method and use, the crystal has the chemical formula [C(NH2)3]BF4, a molecular weight of 146.89, belongs to the trigonal system, the space group is R3m, the crystal lattice parameters are a=7.4634(10)Å, b=7.4634(10)Å, c=9.1216(19)(6)Å, Z=3, the ultraviolet cutoff edge is 200nm, and the frequency doubling response is 4-5 times that of the commercialized nonlinear optical crystal KDP, and can be prepared by hydrothermal method, room temperature solution method, , or use of the crystals in the manufacture of a device for growing centimeter-sized crystals by an evaporation method or a solvothermal method, and producing a harmonic light output of doubled, tripled, quadrupled, quintupled, or sextupled frequency of 1064 nm fundamental frequency light output from a Nd:YAG laser device, or producing an output of ultraviolet and deep ultraviolet frequency multiplied light of less than 200 nm, or use of the crystals in the manufacture of a frequency multiplier, an up or down frequency converter, or an optical parametric oscillator.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims priority to Chinese Patent Application No. 202011568533.1, filed on December 26, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a compound having the molecular formula [C(NH 2 ) 3 ]BF 4 This invention relates to a nonlinear optical crystal of guanidine tetrafluoroborate and its preparation method and use, which belong to the technical field of crystal materials and the technical field of optics. [Background technology]

[0003] As 193nm photolithography technology, micro-nanometer fine laser processing, and modern instruments such as ultra-high energy resolution photoelectron spectroscopy and photoelectron emission microscopes are in high demand for deep ultraviolet laser sources (generally referring to wavelengths shorter than 200nm), the development of all-solid-state deep ultraviolet laser sources has become a recent research hotspot in the international laser science community. In the development of all-solid-state deep ultraviolet laser sources, deep ultraviolet nonlinear optical crystals are a very important component.

[0004] Currently, the ultraviolet and deep ultraviolet nonlinear optical crystals used in industry are mainly LiB 3 O 5 (LBO), CsB 3 O 5 (CBO), CsLiB 6 O 10 (CLBO), BaB 2 O 4 (BBO) and KBe 2 BO 3 F 2 LBO crystals have a wide optical transmission range, high optical uniformity, a larger effective frequency doubling factor (3KDP) and a high damage threshold (18.9GW / cm 2). However, due to its relatively low birefringence (Δn=0.04-0.05), it cannot realize phase matching in the deep ultraviolet region, and the shortest frequency-doubled wavelength is 276 nm. Similar to LBO crystal, CBO and CLBO crystals also have relatively low birefringence, which limits their application in the deep ultraviolet region. BBO crystal has a larger frequency-doubled coefficient and birefringence, but due to its relatively high ultraviolet absorption cut-off edge (189 nm), its shortest frequency-doubled wavelength is 204.8 nm, which limits its application in the deep ultraviolet region. Although KBBF can realize the direct output of 1064 nm fundamental frequency light at 6-fold frequency, KBBF has a layered growth habit and is difficult to grow large-sized crystals, which limits its application to a certain extent. Therefore, there is a strong need to develop new deep ultraviolet nonlinear optical crystals with excellent comprehensive performance. . Summary of the Invention [Problem to be solved by the invention]

[0005] The object of the present invention is to provide a nonlinear optical crystal of guanidine tetrafluoroborate, the crystal having the chemical formula [C(NH 2 ) 3 ]BF 4 It has a molecular weight of 146.89, belongs to a trigonal crystal system, and has a space group of R3m. The crystal lattice parameters are a=7.4634(10)Å, b=7.4634(10)Å, c=9.1216(19)(6)Å, and Z=3. The ultraviolet cutoff edge is 200 nm, and the frequency doubling response is 4-5 times that of the commercialized nonlinear optical crystal KDP. The crystal has a high laser damage threshold, suitable hardness, is easy to process, and is stable in air and not prone to deliquescence.

[0006] Another object of the present invention is to provide a method for producing the nonlinear optical crystal of guanidine tetrafluoroborate.

[0007] Yet another object of the present invention is to provide a use of the nonlinear optical crystal of guanidine tetrafluoroborate. [Means for solving the problem]

[0008] The present invention provides a nonlinear optical crystal of guanidine tetrafluoroborate, the crystal having the chemical formula [C(NH 2 ) 3 ]BF 4 It has a molecular weight of 146.89, a trigonal crystal system, a space group of R3m, crystal lattice parameters of a = 7.4634(10) Å, b = 7.4634(10) Å, c = 9.1216(19)(6) Å, Z = 3, and an ultraviolet cutoff edge of 200 nm.

[0009] A method for producing the nonlinear optical crystal of guanidine tetrafluoroborate, comprising the steps of: producing the crystal by a hydrothermal method, a room temperature solution method, an evaporation method, or a solvothermal method; The method for producing a nonlinear optical crystal of guanidine tetrafluoroborate by a hydrothermal method specifically includes the following steps: NH 2 Group-containing compounds and BF 4 group-containing compound as NH 2 :BF 4 Step a) Mix the ZnO powder homogeneously in a molar ratio of 0.1:0.1 and thoroughly grind it, then add 10-50 mL of deionized water and thoroughly mix it to dissolve it; Among them, the NH 2 The group-containing compound is guanidine carbonate, guanidine sulfate, guanidine nitrate, or guanidine phosphate, and BF 4 the group-containing compound is tetrafluoroboric acid, ammonium tetrafluoroborate, lithium tetrafluoroborate, or sodium tetrafluoroborate; Step b: transferring the mixed solution in step a to a polytetrafluoroethylene lining of a high-pressure reactor having a volume of 25 to 100 mL, and sealing the opening of the reactor by squeezing; Step c: placing the high-pressure reaction vessel in step b in a thermostatic chamber, heating the vessel to 50-230°C at a rate of 20-60°C / h, maintaining the temperature constant for 3-15 days, and then cooling the vessel to room temperature at a rate of 10-100°C / day; Open the high-pressure reactor and obtain a nonlinear optical crystal of guanidine tetrafluoroborate with a centimeter-level large size from the colorless supernatant solution. The preparation of nonlinear optical crystals of guanidine tetrafluoroborate by room temperature solution method specifically includes: NH 2 Group-containing compounds and BF 4 group-containing compound as NH 2 :BF 4 Step a) Mix the ZnO powder homogeneously in a molar ratio of 0.1:0.1 and thoroughly grind it, then add 10-200 mL of deionized water and thoroughly mix it to dissolve it; Among them, the NH 2 The group-containing compound is guanidine carbonate, guanidine sulfate, guanidine nitrate, or guanidine phosphate, and BF 4 the group-containing compound is tetrafluoroboric acid, ammonium tetrafluoroborate, lithium tetrafluoroborate, or sodium tetrafluoroborate; The mixed solution in step a is transferred to a beaker with a volume of 50-300 mL and ultrasonicated, and then mixed thoroughly to dissolve it, and the pH value of the solution is adjusted to 1-11, filtered through qualitative filter paper, and then the opening is sealed with polyvinyl chloride film, and placed in a static environment without shaking, pollution, and air convection, and some holes are pierced in the sealed opening to adjust the volatilization speed of the solvent in the solution, and the solution is kept at room temperature and kept still. When the growth is completed, the size of the beaker is 1-20 mm. 3 A nonlinear optical crystal of guanidine tetrafluoroborate is obtained according to step b. The method for producing a nonlinear optical crystal of guanidine tetrafluoroborate by the evaporation method specifically includes: NH 2 Group-containing compounds and BF 4 group-containing compound as NH 2 :BF 4 Step a) Mix the ZnO powder homogeneously in a molar ratio of 0.1:0.1 and thoroughly grind it, then add 10-200 mL of deionized water and thoroughly mix it to dissolve it; Among them, the NH 2The group-containing compound is guanidine carbonate, guanidine sulfate, guanidine nitrate, or guanidine phosphate, and BF 4 the group-containing compound is tetrafluoroboric acid, ammonium tetrafluoroborate, lithium tetrafluoroborate, or sodium tetrafluoroborate; Step b: moving the mixed solution in step a to a beaker with a volume of 50 to 300 mL and sonicating it to mix and dissolve it thoroughly, and filtering it with qualitative filter paper; The beaker in step b is placed in a thermostatic chamber, the temperature of the thermostatic chamber is raised to 50-120°C at a rate of 5-10°C / h, and the thermostatic chamber is kept at the constant temperature for 3-15 days. When the growth is completed, the size of the beaker is 1-20 mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step c. The production of nonlinear optical crystals of guanidine tetrafluoroborate by the solvothermal method specifically includes: NH 2 Group-containing compounds and BF 4 group-containing compound as NH 2 :BF 4 Step a: uniformly mix the fluorine-containing amines with a molar ratio of 0.1:0.1 and thoroughly grind them, then add 10-200 mL of solvent and thoroughly mix to dissolve them; Among them, the NH 2 The group-containing compound is guanidine carbonate, guanidine sulfate, guanidine nitrate, or guanidine phosphate, and BF 4 the group-containing compound is tetrafluoroboric acid, ammonium tetrafluoroborate, lithium tetrafluoroborate, or sodium tetrafluoroborate, and the solvent is deionized water, absolute ethanol, hydrofluoric acid, or tetrafluoroboric acid; The mixed solution in step a is transferred to a beaker with a volume of 50-300 mL, and ultrasonically treated to mix and dissolve it thoroughly, adjust the pH value of the solution to 1-11, filter it with qualitative filter paper, and then seal the opening with polyvinyl chloride film, place it in a static environment without shaking, pollution, and air convection, puncture some holes in the sealed opening to adjust the volatilization rate of the solvent in the solution, and keep it at room temperature. When the growth is completed, the size of the beaker is 1-20 mm. 3The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b. The use of said guanidine tetrafluoroborate nonlinear optical crystal in the manufacture of a multi-band frequency doubling device or optical element.

[0010] The nonlinear optical crystal of guanidine tetrafluoroborate is used in the manufacture of a 1064 nm fundamental frequency light output by a Nd:YAG laser device, which produces a harmonic light output having a frequency doubled, tripled, quadrupled, quintupled or sextupled.

[0011] The nonlinear optical crystal of guanidine tetrafluoroborate is used in the manufacture of a deep ultraviolet upconverted light output of less than 200 nm.

[0012] The use of said guanidine tetrafluoroborate nonlinear optical crystal in the manufacture of a frequency doubler, an up- or down-frequency converter or an optical parametric oscillator.

[0013] According to the nonlinear optical crystal of guanidine tetrafluoroborate and the preparation method and use of the present invention, the crystal has the characteristics of high quality, large crystal size, high optical uniformity, etc., which can meet the needs of device manufacturing, and is easy to be widely applied in infrared-visible-deep ultraviolet-deep ultraviolet wavelength range. Effect of the Invention

[0014] According to the method for producing nonlinear optical crystal of guanidine tetrafluoroborate of the present invention, the nonlinear optical crystal of guanidine tetrafluoroborate can be obtained with a size of centimeter level, and does not have obvious layered growth habit. By using a large-sized container to extend the crystal growth cycle, the corresponding large-sized nonlinear optical crystal of guanidine tetrafluoroborate can be obtained. In the growth of the nonlinear optical crystal, the crystal is easy to grow, transparent and not enveloped, has the advantages of fast growth speed, low cost, and easy to obtain large-sized crystal.

[0015] According to the manufacturing method of the nonlinear optical crystal of guanidine tetrafluoroborate of the present invention, a large-sized nonlinear optical crystal is obtained, and the crystal workpiece is oriented according to the crystallographic data of the crystal, the crystal is cut according to the required angle, thickness and cross-sectional dimension, and the light-transmitting surface of the crystal is buffed and polished, so that it can be used as a nonlinear optical device. The nonlinear optical crystal of guanidine tetrafluoroborate has the advantages of a wider light-transmitting wavelength range, stable physical and chemical properties, high mechanical hardness, not easily fractured or deliquesced, and easy to cut, buff and store. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is an XRD spectrum according to the present invention, which matches the theoretical XRD chromatogram and proves the presence of the compound guanidine tetrafluoroborate. [Diagram 2] FIG. 2 is a photograph of the nonlinear optical crystal of guanidine tetrafluoroborate according to the present invention. [Diagram 3] FIG. 3 is a diagram showing the operation principle of a nonlinear optical device manufactured using the nonlinear optical crystal of guanidine tetrafluoroborate according to the present invention, in which 1 is a laser device, 2 is an emission beam, 3 is a nonlinear optical crystal of guanidine tetrafluoroborate, 4 is an output beam, and 5 is a filter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Example 1 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by the hydrothermal method includes the following steps: Guanidine carbonate and tetrafluoroboric acid were dissolved in NH 2 :BF 4 Step a: homogeneously mixing the ZnO-containing ferromagnetic metal complex with a molar ratio of 0.1:0.1 and thoroughly grinding the ferromagnetic metal complex with 0.1:0.1, then adding 10 mL of deionized water and thoroughly mixing to dissolve the ferromagnetic metal complex with 0.1:0.1; Step b: transferring the mixed solution in step a to the polytetrafluoroethylene lining of a high-pressure reactor having a volume of 25 mL, and sealing the opening of the reactor by squeezing; Step c: placing the high-pressure reactor in step b in a thermostatic chamber, heating it to 50°C at a rate of 20°C / h, keeping it at constant temperature for 3 days, and then cooling it to room temperature at a rate of 10°C / day; The high-pressure reactor was opened, and a 11×10×12 mm sample was taken from the colorless supernatant. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained according to steps d and e.

[0018] Example 2 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by the hydrothermal method includes the following steps: Guanidine sulfate and lithium tetrafluoroborate were dissolved in NH 2 :BF 4 Step a: homogeneously mixing the ZnO-containing ferromagnetic metal complex with a molar ratio of 0.1:0.1 and thoroughly grinding the ferromagnetic metal complex with 0.1:0.1, then adding 50 mL of deionized water and thoroughly mixing to dissolve the ferromagnetic metal complex with 0.1:0.1; Step b: transferring the mixed solution in step a to the polytetrafluoroethylene lining of a 100 mL high-pressure reactor and sealing the opening of the reactor by squeezing; Step c: placing the high-pressure reactor in step b in a thermostatic chamber, heating it to 230°C at a rate of 60°C / h, keeping it at constant temperature for 15 days, and then cooling it to room temperature at a rate of 100°C / day; The high-pressure reactor was opened, and a 18×20×33 mm sample was taken from the colorless supernatant. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained according to steps d and e.

[0019] Example 3 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by the hydrothermal method includes the following steps: Guanidine nitrate and ammonium tetrafluoroborate (NH 2 :BF 4After mixing uniformly at a molar ratio of 3:1 and thoroughly grinding, add 40 mL of deionized water and mix thoroughly to dissolve, step a; Step b: transferring the mixed solution in step a to the polytetrafluoroethylene lining of a high-pressure reactor having a volume of 70 mL, and sealing the opening of the reactor by squeezing; Step c: placing the high-pressure reactor in step b in a thermostatic chamber, heating it to 150°C at a rate of 40°C / h, keeping it at constant temperature for 7 days, and then cooling it to room temperature at a rate of 60°C / day; Open the high-pressure reactor and extract the large 11 x 22 x 23 mm granules from the colorless supernatant. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained according to steps d and e.

[0020] Example 4 The method for producing a nonlinear optical crystal of guanidine tetrafluoroborate by a hydrothermal method specifically includes the following steps: Guanidine phosphate and sodium tetrafluoroborate in NH 2 :BF 4 Step a) Mix the ZnO powder homogeneously in a molar ratio of 0.1:0.1 and thoroughly grind it, then add 10-50 mL of deionized water and thoroughly mix it to dissolve it; transferring the mixed solution in step a to a polytetrafluoroethylene lining of a high-pressure reactor having a volume of 50 mL, and sealing the opening of the reactor by squeezing; Step c: placing the high-pressure reactor in step b in a thermostatic chamber, heating it to 200°C at a rate of 50°C / h, keeping it at constant temperature for 7 days, and then cooling it to room temperature at a rate of 80°C / day; The high-pressure reactor was opened, and from the colorless supernatant solution, a large particle with centimeter-level dimensions of 10 x 21 x 22 mm was obtained. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained according to steps d and e.

[0021] Example 5 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by room temperature solution method is Guanidine phosphate and sodium tetrafluoroborate in NH 2 :BF 4 Step a: homogeneously mixing the ZnO-containing ferromagnetic metal complex with a molar ratio of 0.1:0.1 and thoroughly grinding the ferromagnetic metal complex with 0.1:0.1, then adding 10 mL of deionized water and thoroughly mixing to dissolve the ferromagnetic metal complex with 0.1:0.1; The mixed solution in step a is transferred to a 50mL beaker and ultrasonically treated to mix and dissolve it thoroughly, the pH value of the solution is adjusted to 1, filtered with qualitative filter paper, and then the opening is sealed with polyvinyl chloride film, placed in a static environment without shaking, pollution, and air convection, and some holes are pierced in the sealed opening to adjust the volatilization rate of the solvent in the solution, and kept at room temperature. When the growth is completed, the crystals with a size of 1mm are formed. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b.

[0022] Example 6 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by room temperature solution method is Guanidine sulfate and lithium tetrafluoroborate were dissolved in NH 2 :BF 4 Step a: homogeneously mixing the ZnO-containing ferromagnetic particles in a molar ratio of 0.1:0.1 and thoroughly grinding the ferromagnetic particles, then adding 200 mL of deionized water and thoroughly mixing to dissolve the ferromagnetic particles; The mixed solution in step a is transferred to a 300 mL beaker and ultrasonically treated to mix and dissolve it thoroughly, the pH value of the solution is adjusted to 11, filtered with qualitative filter paper, and then the opening is sealed with polyvinyl chloride film, placed in a static environment without shaking, pollution, and air convection, and some holes are pierced in the sealed opening to adjust the volatilization rate of the solvent in the solution, and kept at room temperature. When the growth is completed, the crystals are formed into a crystal with a size of 20 mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b.

[0023] Example 7 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by room temperature solution method is Guanidine nitrate and lithium tetrafluoroborate (NH 2 :BF 4 Step a: homogeneously mixing the ZnO / ZnO molar ratio at 3:1 and thoroughly grinding the ZnO / ZnO molar ratio, then adding 100 mL of deionized water and thoroughly mixing to dissolve the ZnO / ZnO molar ratio; The mixed solution in step a is transferred to a 200mL beaker and ultrasonically treated to mix and dissolve it thoroughly, the pH value of the solution is adjusted to 5, filtered with qualitative filter paper, and then the opening is sealed with polyvinyl chloride film, placed in a static environment without shaking, pollution, and air convection, some holes are pierced in the sealed opening to adjust the volatilization rate of the solvent in the solution, and kept at room temperature. When the growth is completed, the crystals with a size of 12 mm are formed. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b.

[0024] Example 8 The preparation of nonlinear optical crystals of guanidine tetrafluoroborate by room temperature solution method specifically includes: Guanidine carbonate and sodium tetrafluoroborate were dissolved in NH 2 :BF 4 Step a) Mix the ZnO powder homogeneously in a molar ratio of 0.1:0.1 and thoroughly grind it, then add 10-200 mL of deionized water and thoroughly mix it to dissolve it; The mixed solution in step a is transferred to a 150mL beaker and ultrasonically treated to mix and dissolve it thoroughly, the pH value of the solution is adjusted to 10, filtered with qualitative filter paper, and then the opening is sealed with polyvinyl chloride film, placed in a static environment without shaking, pollution, and air convection, some holes are pierced in the sealed opening to adjust the volatilization rate of the solvent in the solution, and kept at room temperature. When the growth is completed, the crystals are formed into a crystal with a size of 15mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b.

[0025] Example 9 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by the evaporation method includes the following steps: Guanidine nitrate and tetrafluoroboric acid (NH2 :BF 4 Step a: homogeneously mixing the ZnO-containing ferromagnetic metal complex with a molar ratio of 0.1:0.1 and thoroughly grinding the ferromagnetic metal complex with 0.1:0.1, then adding 10 mL of deionized water and thoroughly mixing to dissolve the ferromagnetic metal complex with 0.1:0.1; Step b: transferring the mixed solution in step a to a 50 mL beaker and sonicating it to mix and dissolve it thoroughly, and filtering it through qualitative filter paper; The beaker in step b is placed in a thermostatic chamber, the temperature of the thermostatic chamber is raised to 50°C at a rate of 5°C / h, and the temperature is kept constant for 3 days. When the growth is completed, the size of the beaker is 1 mm. 3 A nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step c.

[0026] Example 10 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by the evaporation method includes the following steps: Guanidine sulfate and ammonium tetrafluoroborate were dissolved in NH 2 :BF 4 Step a: homogeneously mixing the ZnO-containing ferromagnetic particles in a molar ratio of 0.1:0.1 and thoroughly grinding the ferromagnetic particles, then adding 200 mL of deionized water and thoroughly mixing to dissolve the ferromagnetic particles; Step b: transferring the mixed solution in step a to a 300 mL beaker and sonicating it to mix and dissolve it thoroughly, and filtering it through qualitative filter paper; The beaker in step b is placed in a thermostatic chamber, and the temperature of the thermostatic chamber is raised to 120°C at a rate of 10°C / h, and the temperature is kept constant for 15 days. When the growth is completed, the size of the beaker is 20 mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step c.

[0027] Example 11 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by the evaporation method includes the following steps: Guanidine carbonate and sodium tetrafluoroborate were dissolved in NH 2 :BF 4Step a: homogeneously mixing the ZnO-containing ferromagnetic particles in a molar ratio of 0.01:0.1 and thoroughly grinding the ferromagnetic particles, then adding 120 mL of deionized water and thoroughly mixing to dissolve the ferromagnetic particles; Step b: transferring the mixed solution in step a to a beaker of 250 mL volume and sonicating it to mix and dissolve it thoroughly, and filtering it through qualitative filter paper; The beaker in step b is placed in a thermostatic chamber, and the temperature of the thermostatic chamber is raised to 100°C at a rate of 10°C / h, and the temperature is kept constant for 13 days. When the growth is completed, the size of the beaker is 14 mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step c.

[0028] Example 12 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by the evaporation method includes the following steps: Guanidine phosphate and lithium tetrafluoroborate were dissolved in NH 2 :BF 4 Step a) Mix the ZnO powder homogeneously in a molar ratio of 0.1:0.1 and thoroughly grind it, then add 10-200 mL of deionized water and thoroughly mix it to dissolve it; Step b: transferring the mixed solution in step a to a beaker of 180 mL volume and sonicating it to mix and dissolve it thoroughly, and filtering it through qualitative filter paper; The beaker in step b is placed in a thermostatic chamber, the temperature of the thermostatic chamber is raised to 100°C at a rate of 8°C / h, and the thermostatic chamber is kept at the constant temperature for 12 days. When the growth is completed, the size of the beaker is 12 mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step c.

[0029] Example 13 Specifically, the growth of nonlinear optical crystals of guanidine tetrafluoroborate by the solvothermal method includes the following steps: Guanidine sulfate and lithium tetrafluoroborate were dissolved in NH 2 :BF 4 Step a: homogeneously mixing the ZnO-containing ferromagnetic metal complex with a molar ratio of 0.1:0.1 and thoroughly grinding the ferromagnetic metal complex with 0.1:0.1, then adding 10 mL of deionized water and thoroughly mixing to dissolve the ferromagnetic metal complex with 0.1:0.1; The mixed solution in step a is transferred to a 50mL beaker and ultrasonically treated to mix and dissolve it thoroughly, the pH value of the solution is adjusted to 1, filtered with qualitative filter paper, and then the opening is sealed with polyvinyl chloride film, placed in a static environment without shaking, pollution, and air convection, some holes are pierced in the sealed opening to adjust the volatilization rate of the solvent in the solution, and kept at room temperature. When the growth is completed, the crystals are formed into a crystal with a size of 10 mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b.

[0030] Example 14 The production of nonlinear optical crystals of guanidine tetrafluoroborate by the solvothermal method specifically includes: Guanidine carbonate and sodium tetrafluoroborate were dissolved in NH 2 :BF 4 Step a: homogeneously mix the mixture in a molar ratio of 0.1:0.1 and thoroughly grind it, then add 50 mL of absolute ethanol and thoroughly mix it to dissolve it; The mixed solution in step a is transferred to a 200mL beaker and ultrasonically treated to mix and dissolve it thoroughly, the pH value of the solution is adjusted to 11, filtered with qualitative filter paper, and then the opening is sealed with polyvinyl chloride film, placed in a static environment without shaking, pollution, and air convection, and some holes are pierced in the sealed opening to adjust the volatilization rate of the solvent in the solution, and kept at room temperature. When the growth is completed, the crystals with a size of 1mm are formed. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b.

[0031] Example 15 The production of nonlinear optical crystals of guanidine tetrafluoroborate by the solvothermal method specifically includes: Guanidine sulfate and ammonium tetrafluoroborate were dissolved in NH 2 :BF 4 a) uniformly mixing the mixture in a molar ratio of 0.1:0.1 and thoroughly grinding it, and then adding 10 mL of hydrofluoric acid and thoroughly mixing it to dissolve it; The mixed solution in step a is transferred to a 300mL beaker and ultrasonically treated to mix and dissolve it thoroughly, the pH value of the solution is adjusted to 7, filtered with qualitative filter paper, and then the opening is sealed with polyvinyl chloride film, placed in a static environment without shaking, pollution, and air convection, and some holes are pierced in the sealed opening to adjust the volatilization rate of the solvent in the solution, and kept at room temperature. When the growth is completed, the crystals are formed into a crystal with a size of 20 mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b.

[0032] Example 16 The production of nonlinear optical crystals of guanidine tetrafluoroborate by the solvothermal method specifically includes: Guanidine carbonate and lithium tetrafluoroborate were dissolved in NH 2 :BF 4 Step a: homogeneously mixing the mixture in a molar ratio of 0.1:0.1 and thoroughly grinding the mixture, then adding 10 mL of tetrafluoroboric acid and thoroughly mixing to dissolve it; The mixed solution in step a is transferred to a beaker with a volume of 170 mL, and then ultrasonically treated to mix and dissolve it thoroughly, adjust the pH value of the solution to 10, filter it with qualitative filter paper, and then seal the opening with polyvinyl chloride film, place it in a static environment without shaking, pollution, and air convection, puncture some holes in the sealed opening to adjust the volatilization rate of the solvent in the solution, and keep it at room temperature. When the growth is finished, the size of the beaker is 13 mm. 3 The nonlinear optical crystal of guanidine tetrafluoroborate is obtained based on step b.

[0033] Example 17 The nonlinear optical crystals of guanidine tetrafluoroborate [C(NH 2 ) 3 ]BF 4(Fig. 2) according to the alignment direction, and placed at position 3 as shown in Fig. 3. A Q-switched Nd:YAG laser device is used as the light source at room temperature. The incident wavelength is 1064 nm. The infrared beam 2 of the wavelength 1064 nm emitted by the Q-switched Nd:YAG laser device 1 is [C(NH 2 ) 3 ]BF 4 When incident on the single crystal 3, it generates green frequency-doubled light with a wavelength of 532 nm, and the output intensity is approximately 4.3 times that of KDP under equivalent conditions.

[0034] Example 18 The nonlinear optical crystals of guanidine tetrafluoroborate [C(NH 2 ) 3 ]BF 4 (Fig. 2) according to the alignment direction, and placed at position 3 as shown in Fig. 3. A Q-switched Nd:YAG laser device is used as the light source at room temperature, and the incident wavelength is 532 nm. The infrared beam 2 of the wavelength 532 nm emitted by the Q-switched Nd:YAG laser device 1 is [C(NH 2 ) 3 ]BF 4 The light is incident on the single crystal 3, generating frequency-doubled light with a wavelength of 266 nm, and the output intensity is approximately 1.2 times that of BBO under equivalent conditions. [Explanation of symbols]

[0035] 1 Laser device 2 Light Beam 3. Nonlinear optical crystals of guanidine tetrafluoroborate 4. Exit beam 5. Filters

Claims

1. A nonlinear optical crystal of guanidine tetrafluoroborate, The crystals have the chemical formula [C(NH 2 ) 3 ]B.F. 4 and has a molecular weight of 146.89; A nonlinear optical crystal of guanidine tetrafluoroborate, which belongs to a trigonal crystal system, has a space group of R3m, has crystal lattice parameters of a = 7.4634(10) Å, b = 7.4634(10) Å, c = 9.1216(19)(6) Å, and Z = 3, and can produce frequency-doubled light having a frequency two or four times that of an Nd:YAG laser (wavelength 1064 nm).

2. A method for producing the nonlinear optical crystal of guanidine tetrafluoroborate according to claim 1, comprising the steps of: The method comprises producing crystals by hydrothermal, room temperature solution, evaporation or solvothermal methods; The method for producing a nonlinear optical crystal of guanidine tetrafluoroborate by a hydrothermal method specifically includes the following steps: N.H. 2 Group-containing compound and BF 4 group-containing compound as NH 2 : BF 4 Step a: uniformly mixing the cellulose acetate and cellulose acetate in a molar ratio of 3:1 and grinding thoroughly, then adding 10-50 mL of deionized water and mixing thoroughly to dissolve it; Among them, the NH 2 The group-containing compound is guanidine carbonate, guanidine sulfate, guanidine nitrate, or guanidine phosphate, and BF 4 the group-containing compound is tetrafluoroboric acid, ammonium tetrafluoroborate, lithium tetrafluoroborate, or sodium tetrafluoroborate; Step b: transferring the mixed solution in step a to a polytetrafluoroethylene lining of a high-pressure reactor having a volume of 25 to 100 mL, and sealing the opening of the reactor by squeezing; Step c: placing the high-pressure reaction vessel in step b in a thermostatic chamber, heating the vessel to 50-230° C. at a rate of 20-60° C. / h, maintaining the vessel at this temperature for 3-15 days, and then cooling the vessel to room temperature at a rate of 10-100° C. / day; and (d) opening the high-pressure reactor to obtain a nonlinear optical crystal of guanidine tetrafluoroborate with a large size of centimeter level from the colorless supernatant solution; The preparation of nonlinear optical crystals of guanidine tetrafluoroborate by room temperature solution method specifically includes: N.H. 2 Group-containing compound and BF 4 group-containing compound as NH 2 : BF 4 Step a: uniformly mixing the cellulose acetate and cellulose acetate in a molar ratio of 3:1 and grinding thoroughly, then adding 10-200 mL of deionized water and mixing thoroughly to dissolve it; Among them, the NH 2 The group-containing compound is guanidine carbonate, guanidine sulfate, guanidine nitrate, or guanidine phosphate, and BF 4 the group-containing compound is tetrafluoroboric acid, ammonium tetrafluoroborate, lithium tetrafluoroborate, or sodium tetrafluoroborate; The mixed solution in step a is transferred to a beaker with a volume of 50-300 mL, and ultrasonically treated to mix and dissolve it thoroughly, and the pH value of the solution is adjusted to 1-11. The solution is filtered through qualitative filter paper, and then the opening is sealed with a polyvinyl chloride film, and placed in a static environment without shaking, contamination, and air convection, and a few holes are pierced in the sealed opening to adjust the volatilization rate of the solvent in the solution, and the solution is left to stand at room temperature and kept. When the growth is completed, the size of the beaker is 1-20 mm. 3 and b) obtaining a nonlinear optical crystal of guanidine tetrafluoroborate of The method for producing a nonlinear optical crystal of guanidine tetrafluoroborate by the evaporation method specifically includes: N.H. 2 Group-containing compound and BF 4 group-containing compound as NH 2 : BF 4 Step a: uniformly mixing the cellulose acetate and cellulose acetate in a molar ratio of 3:1 and grinding thoroughly, then adding 10-200 mL of deionized water and mixing thoroughly to dissolve it; Among them, the NH 2 The group-containing compound is guanidine carbonate, guanidine sulfate, guanidine nitrate, or guanidine phosphate, and BF 4 the group-containing compound is tetrafluoroboric acid, ammonium tetrafluoroborate, lithium tetrafluoroborate, or sodium tetrafluoroborate; Step b: transferring the mixed solution in step a to a beaker with a volume of 50-300 mL and sonicating it to mix and dissolve it thoroughly, and filtering it through qualitative filter paper; The beaker in step b is placed in a thermostatic chamber, the temperature of the thermostatic chamber is raised to 50 to 120° C. at a rate of 5 to 10° C. / h, and the thermostatic chamber is left at the constant temperature for 3 to 15 days. When the growth is completed, the size of the beaker is 1 to 20 mm. 3 and c) obtaining a nonlinear optical crystal of guanidine tetrafluoroborate of The production of nonlinear optical crystals of guanidine tetrafluoroborate by the solvothermal method specifically includes: N.H. 2 Group-containing compound and BF 4 group-containing compound as NH 2 : BF 4 Step a: homogeneously mixing the cellulose acetate and cellulose acetate in a molar ratio of 3:1 and thoroughly grinding the mixture, then adding 10-200 mL of a solvent and thoroughly mixing to dissolve the mixture; Among them, the NH 2 The group-containing compound is guanidine carbonate, guanidine sulfate, guanidine nitrate, or guanidine phosphate, and BF 4 the group-containing compound is tetrafluoroboric acid, ammonium tetrafluoroborate, lithium tetrafluoroborate, or sodium tetrafluoroborate, and the solvent is deionized water, absolute ethanol, hydrofluoric acid, or tetrafluoroboric acid; The mixed solution in step a is transferred to a beaker with a volume of 50-300 mL, and ultrasonically treated to mix and dissolve it thoroughly, adjust the pH value of the solution to 1-11, filter with qualitative filter paper, and then seal the opening with polyvinyl chloride film, place in a static environment without shaking, contamination, and air convection, puncture some holes in the sealed opening to adjust the volatilization rate of the solvent in the solution, and keep at room temperature. When the growth is completed, the size of the beaker is 1-20 mm. 3 2. The method for producing a nonlinear optical crystal of guanidine tetrafluoroborate according to claim 1, characterized in that the method is carried out based on the steps of: obtaining a nonlinear optical crystal of guanidine tetrafluoroborate of the step (a) and (b).

3. 2. Use of the nonlinear optical crystal of guanidine tetrafluoroborate according to claim 1 in the manufacture of a multi-band frequency doubling device or optical element.

4. Use of the nonlinear optical crystal of guanidine tetrafluoroborate described in claim 3 in the manufacture of a harmonic optical output having a frequency doubled, tripled, quadrupled, quintupled or sextupled from the fundamental frequency light of 1064 nm outputted by an Nd:YAG laser device.

5. 4. Use of the nonlinear optical crystal of guanidine tetrafluoroborate according to claim 3 in the manufacture of a deep ultraviolet frequency-doubled light output of less than 200 nm.

6. 4. Use of the nonlinear optical crystal of guanidine tetrafluoroborate according to claim 3 in the manufacture of a frequency doubler, an up- or down-frequency converter or an optical parametric oscillator.