Continuous dissolution of cellulose derivatives
Patent Information
- Application Number
- JP2023540110
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-12-31
- Filing Date
- 2021-12-31
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-12-31
Smart Images

Figure 00000023_0000 
Figure 00000023_0001 
Figure 00000023_0002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for dissolving a cellulose derivative, and in particular to a method for continuously dissolving a cellulose carbamate. [Background technology]
[0002] Cellulose is the most widely used biopolymer in the world, and both cellulose and its derivatives, such as cellulose carbamate, cellulose acetate, ethers and esters, have found applications in various industries such as paper and cardboard industry, textile industry, etc. However, the use of cellulose in these industries requires dissolving the cellulose fibers to regenerate the structure. Dissolving cellulose is difficult due to its semi-crystalline structure, strong hydrogen bonds in the polymer sheet, and the presence of hydrophilic and hydrophobic ends in the polymer. For this reason, cellulose requires modification of its structure by derivatization or opening up the fibers and improving its reactivity.
[0003] Several derivatization methods are known, the most well-known being probably the viscose process, in which cellulose is first treated with alkali and then with carbon disulfide to produce cellulose xanthate. The viscose process is increasingly being avoided due to the toxicity of carbon disulfide and the unfavorable environmental impacts of the viscose process. Increasing attention is being paid to other derivatization processes, especially those that are cheap, do not have the toxicity and environmental issues of the viscose process, and can be carried out using available infrastructure, such as viscose wet spinning machines.
[0004] The carbamate process to produce cellulose carbamate is one such derivatization process. Cellulose carbamate is formed by reacting cellulose with urea. Methods for producing cellulose carbamate are described, for example, in Finnish Patents Nos. 112869 and 112795.
[0005] As mentioned above, cellulose or cellulose derivatives must be dissolved to regenerate the cellulose structure for use in various industrial applications. The procedure for dissolving cellulose in aqueous alkali is based on the freeze-thaw method. The solvent is pre-cooled below the freezing point of water before adding the cellulose and is kept at a low temperature until the polymer is completely dissolved. The temperature required for efficient dissolution in the freeze-thaw method was found to be around -30 °C for the entire mixture of cellulose carbamate in aqueous solution. Thus, freezing and thawing of polymer solutions on an industrial scale is energetically and economically impractical, since industrial-scale dope production requires the use of efficient freezing equipment that is not usually present in cellulosic fiber production plants. Both freezing and thawing consume energy and time, reducing the efficiency and sustainability of the entire process.
[0006] Traditional dissolution methods such as freeze-thaw often cause phase separation during the long freezing stage of the process and / or difficult temperature control during the freezing and thawing stages. This can result in variations in the composition of the resulting cellulose solution, particle agglomeration, i.e. particles that remain undissolved "stick" together to form clusters that are difficult or impossible to separate in a subsequent filtration process, and gelation of the resulting cellulose solution can be induced by undissolved particles and / or uncontrolled process temperatures. Nitrogen hydrolysis is simultaneously promoted by long freeze-thaw periods and / or uncontrolled process temperatures. The challenges associated with mitigating the undissolved residue have been partially overcome by making only very dilute solutions of cellulose or by gradually adding cellulose in a batch mixing process. Traditional freeze-thaw processes and operations with dilute cellulose solutions incur costs that are economically and time unacceptable. Summary of the Invention
[0007] It is an object of the present invention to overcome at least some of the problems mentioned above and to provide a method for continuously dissolving cellulose carbamate in an alkaline aqueous phase to form a solution.
[0008] The method includes mixing cellulose carbamate with an aqueous alkaline solution and passing the mixture thus formed through a mixing zone of a continuously operating kneader-type dissolution reactor to produce a solution of cellulose carbamate in the aqueous alkaline phase. The aqueous phase containing cellulose carbamate is recovered. The step of continuously passing the mixture through the mixing zone of the kneader-type dissolution reactor is carried out at a temperature of 10° C. or less.
[0009] The invention is defined by the features of the independent claims. Some particular embodiments are defined in the dependent claims.
[0010] According to a first aspect of the present invention, there is provided a method for continuously dissolving a cellulose carbamate polymer in an alkaline aqueous phase to form a solution, the method comprising the steps of providing a cellulose carbamate polymer, mixing the cellulose carbamate polymer with an alkaline aqueous solution to form a mixture, passing the mixture through a mixing zone of a kneader-type dissolution reactor operating continuously to produce a solution of the cellulose carbamate polymer in the alkaline aqueous phase, and recovering the dissolved cellulose carbamate polymer-containing aqueous phase. The step of continuously passing the mixture through the mixing zone of the kneader-type dissolution reactor of the method is carried out at a temperature of 10°C or less.
[0011] The present invention provides significant advantages. The present invention provides a method for continuously dissolving cellulose carbamate polymer in an alkaline solution. The cellulose carbamate polymer is an alkaline unstable cellulose derivative. It has been surprisingly found that the present invention can dissolve the cellulose carbamate polymer to a high cellulose consistency to obtain a cellulose carbamate spinning dope having a lower viscosity than mathematically and experimentally predicted by conventional dissolution methods known in the art. This has been demonstrated, especially when the dissolution operation is carried out under supercooled conditions.
[0012] Moreover, it was surprisingly found that the obtained cellulose carbamate spinning dope was stable for a long period of time even at room temperature. Normally, the cellulose carbamate dope must be stored at a reduced temperature to avoid gelation of the cellulose carbamate solution. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a flow diagram illustrating a process for continuous dissolution of cellulose carbamate, in accordance with at least some embodiments of the present invention. [Diagram 2] FIG. 1 is a flow diagram illustrating a process for continuous dissolution of cellulose carbamate, in accordance with at least some embodiments of the present invention. [Diagram 3] 1 is a microscopic image showing the effect of dissolution temperature and sodium hydroxide concentration on the dissolution of cellulose carbamate from regenerated cotton. [Figure 4] 13A-13C are microscopic images showing the stability of the pre-slurry in the two-stage dissolution process. [Diagram 5] 1 is a graph of the stability of cellulose carbamate polymer slurries in aqueous alkaline solutions in terms of viscosity as a function of shear rate. [Figure 6] 6A to 6C show micrographs of the recovered solutions of cellulose carbamate. [Figure 7] 7A-7F show micrographs of solutions of cellulose carbamate as disclosed in Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] definition As used herein, the following terms are defined to have the following meanings, unless otherwise stated.
[0015] "Low temperature conditions" means temperatures in the range of 5°C to -6.9°C.
[0016] "Supercooled conditions" refers to temperatures lower than temperatures generally found in low temperature conditions, and in particular to temperatures in the range of -7°C to -20°C.
[0017] Chemical pulp or dissolving pulp prepared from wood species such as pine, spruce, birch, beech, aspen, maple, larch, acacia, eucalyptus, hemlock, tupelo, oak, or non-wood such as stalk fibers (wheat straw, rice straw, barley straw, bamboo, bagasse, reed). The origin of the raw material is either virgin type chemical or dissolving pulp or recycled raw materials such as recycled paper and / or cardboard containing chemical or dissolving pulp.
[0018] Natural plant fibres are in the form of chemical or dissolving pulp or as such. The origin of natural plant fibres is either in virgin form or in textile products containing natural plant fibres or textile products containing regenerated natural fibres. Natural plant fibres include seed fibres such as cotton and kapok, bast fibres such as hemp, jute, kenaf, ramie, abaca and linen, leaf fibres such as manila, sisal, ananas and banana, and fruit fibres such as coir.
[0019] The cellulose carbamate solution having a relatively high cellulose carbamate concentration in the alkaline aqueous phase is produced by continuously dissolving the cellulose carbamate in an alkaline aqueous solution and passing the mixture of the cellulose carbamate and the alkaline aqueous solution through a mixing zone of a mixing kneader operated continuously at a temperature of 10° C. or less. The cellulose carbamate is usually completely dissolved with substantially no undissolved cellulose-derived particles remaining, ensuring improved filterability of the cellulose carbamate dope, which can be seen, for example, in the filterability index (K R Improved filterability is technically essential in regenerating cellulose carbamate from the recovered cellulose carbamate-containing aqueous phase.
[0020] FIG. 1 is a flow diagram illustrating a process for continuous dissolution of cellulose carbamate in accordance with at least some embodiments of the invention.
[0021] Solid cellulose carbamate 100 is weighed and charged into the pulper 10. A total amount of sodium hydroxide aqueous solution 200 required to dissolve the weighed cellulose carbamate 100 is added to the pulper 10. The alkaline aqueous solution 200 may be added all at once or gradually. The pulper 10 is started, and a mixture 300 consisting of cellulose carbamate in an alkaline aqueous solution is formed. The mixture 300 is led to a storage tank 20 equipped with a mixer. The storage tank 20 may be a chest storage tank. After the mixture 300 is led to the storage tank 20, the pulper 10 is ready for the next batch of cellulose carbamate 100 and the sodium hydroxide aqueous solution 200. The storage tank 20 has a larger volume than the pulper 10 and can accommodate multiple batches of the mixture 300 sent from the pulper 10. The mixture 300 is continuously fed from the storage tank 20 to the mixing zone of the kneader-type dissolution reactor 40 by a pump 30. The temperature of mixture 300 is preferably reduced but maintained above the solubility limit of the system during the process steps prior to entering dissolution reactor 40. A solution of cellulose carbamate in aqueous alkaline solution 400 is continuously formed and withdrawn in dissolution reactor 40.
[0022] FIG. 2 is a flow diagram illustrating a process for continuous dissolution of cellulose carbamate in accordance with at least some embodiments of the invention.
[0023] Solid cellulose carbamate 100 is weighed and charged to pulper 10. The weighed amount of cellulose carbamate 100 and a first portion 2000 of aqueous sodium hydroxide solution required to form a preslurry are added to pulper 10. Pulper 10 is started and a preslurry 3000 is formed comprising cellulose carbamate in an aqueous alkaline solution.
[0024] The preliminary slurry 3000 is led to a storage tank 20 equipped with a mixer. After the preliminary slurry 3000 is led to the storage tank 20, the pulper 10 is ready for the next batch of cellulose carbamate 100 and the next first portion 2000 of the aqueous sodium hydroxide solution. The storage tank 20 has a larger volume than the pulper 10 and can accommodate multiple batches of the preliminary slurry 3000 sent from the pulper 10. The preliminary slurry is continuously fed from the storage tank 20 to the mixing zone of the kneader-type dissolution reactor 40 using a pump 30. A second portion 2200 of the alkaline solution is added to the dissolution reactor 40 together with the preliminary slurry 3000 to provide a mixture 330. The mixture 330 is formed in the dissolution reactor. The temperature of the preliminary slurry 3000 is kept above the solubility limit of the system in the process stage before the dissolution reactor 40. A solution of cellulose carbamate in the aqueous alkaline solution 400 is continuously formed and withdrawn in the dissolution reactor 40.
[0025] As described above, the present technology relates to a method for dissolving cellulose carbamate.
[0026] In general, the present technology provides a method for continuously dissolving cellulose carbamate in an alkaline aqueous phase to form a solution, the method comprising the steps of providing cellulose carbamate, mixing the cellulose carbamate with an alkaline aqueous solution to form a mixture, producing a solution of the cellulose carbamate in the alkaline aqueous phase from the mixture, and recovering a cellulose carbamate-containing aqueous phase, wherein the step of producing the solution is carried out at a temperature of 10° C. or less.
[0027] In one embodiment, a method for continuously dissolving cellulose carbamate in an alkaline aqueous phase to form a solution includes the steps of providing cellulose carbamate, mixing the cellulose carbamate with an alkaline aqueous solution to form a mixture, passing the mixture through a mixing zone of a continuously operating kneader-type mixing reactor to produce a solution of said cellulose carbamate in the alkaline aqueous phase, such as producing a cellulose carbamate dope or a cellulose carbamate spinning dope, and recovering the cellulose carbamate-containing aqueous phase.
[0028] In one embodiment, the step of continuously conducting the mixture through a mixing zone of a mixing kneader is carried out at a temperature of 10° C. or less.
[0029] In a further embodiment, the cooling is performed in the mixing zone of the mixing kneader.Thus, in one embodiment, the mixture passes through the mixing and cooling zones of the mixing kneader.
[0030] In one embodiment, the step of forming the solution from the mixture is carried out on a cooled metal surface or a cooled cylinder, for example a cooled rotating drum.
[0031] In embodiments, the cellulose carbamate may be cellulose carbamate produced from chemical or dissolving pulp prepared from wood or non-wood fibers, or cellulose carbamate derived from natural plant fibers as or in the form of chemical or dissolving pulp. The method embodiments can also be practiced with cellulose carbamate produced from any mixture of the various cellulosic fibers or pulps described above. In a preferred embodiment, cellulose carbamate is produced in a process comprising the steps of providing a pulp, adding an aqueous solution of urea and optionally hydrogen peroxide to the pulp (or optionally activated pulp) to provide a mixture, mechanically treating the mixture to provide a homogenous composition, heating the composition to a temperature in the range of 120°C to 155°C, typically 135°C, for a period in the range of 2 to 4 hours to produce cellulose carbamate, recovering the cellulose carbamate, optionally washing the cellulose carbamate with water, and drying in a dryer at a temperature below 155°C, preferably below 135°C, and suitably below 133°C.
[0032] In a further embodiment, the mixture formed by cellulose carbamate in the aqueous alkaline solution is subjected to low shear mixing in the mixing zone of a kneader-type mixing reactor by operating the mixer at a reduced mixer speed of 10 to 500 rpm, suitably 250 rpm or less, most suitably 100 rpm or less, preferably 50 rpm or less.
[0033] The target temperature level can be reached and / or maintained by mixing with low shear forces. Thus, the dissolution process according to the embodiments does not depend on high shear mixing. A typical technical approach is to use high speed mixing to obtain a good quality solution. However, in the embodiments, the dissolution temperature is the most important factor, not the mixing speed or high shear forces in the mixing. The more vigorous the mixing, the more difficult it is to reach and / or maintain a low dissolution temperature. Dissolving under low temperature and / or supercooling conditions provides a cellulose carbamate solution of a quality suitable for the spinning process. For example, in the embodiments, the recovered solution is subjected to a spinning process, such as a wet spinning process, to spin cellulose carbamate fibers.
[0034] The mixture of cellulose carbamate polymer and alkaline solution can be formed in a variety of ways, with each method of forming the mixture being compatible with the particular alkaline solution or solutions and the particular cellulose carbamate or carbamates forming the mixture.
[0035] In one specific embodiment, also referred to as the one-stage process, the cellulose carbamate is first mixed with an alkaline solution and the mixture thus obtained is fed into the mixing zone of a continuously operated kneader-type dissolution reactor.
[0036] In one embodiment, pre-cooling is accomplished in a first kneader, thereby obtaining partial dissolution, and after that step the mixture is transferred to a second kneader, in which the materials are typically completely or substantially completely dissolved.
[0037] Mixing the cellulose carbamate with an alkaline solution before feeding the mixture to the mixing zone of a continuous kneader-type dissolution reactor to provide a composition corresponding to the final target chemical composition set for the cellulose carbamate dope to be recovered allows for accurate control of the chemical composition of the resulting cellulose carbamate dope. Furthermore, the viscosity and slurry consistency of the slurry prepared to the final composition are low, making it technically easy to handle the slurry (e.g., pumping the mixture).
[0038] The mixing of the cellulose carbamate with the alkali solution, corresponding to the final target chemical composition set for the recovered cellulose carbamate dope, can be carried out in a batchwise manner in a mixing reactor, such as a pulper or another type of homogenizer, or in a suitable reactor, such as a xanthator type reactor or a suitable reactor connected to a homogenizer, by directly or gradually adjusting the sodium hydroxide and / or zinc oxide concentration in the preliminary slurry. In a xanthator type reactor, or a suitable reactor connected to a homogenizer, by directly or gradually adjusting the sodium hydroxide and / or zinc oxide concentration in the preliminary slurry, it can be carried out in a batchwise manner to affect the swelling properties of the cellulose carbamate derivative before adding the remaining alkali and water containing alkali and / or zinc oxide to reach the final target composition.
[0039] The temperature of the slurry in each slurrying stage can be controlled, for example, by the use of a pre-cooling solution and / or by external cooling of the pulper or other type of homogenizer or mixing reactor.
[0040] In a particular embodiment, which may be referred to as a two-stage process, cellulose carbamate is first mixed with a first portion of an alkaline solution or an alkaline solution containing zinc oxide, the thus obtained pre-slurry is fed into the mixing zone of a continuously operated kneader-type dissolution reactor, and a second portion of the alkaline solution or an alkaline solution containing zinc oxide is fed into the mixing zone of a continuously operated kneader-type dissolution reactor.
[0041] The pre-slurry of cellulose carbamate containing the first part of the alkaline solution is fed into the mixing zone of the continuously operating kneader, and the second part of the alkaline solution is fed separately into the mixing zone of the continuously operating kneader, providing an opportunity to pre-cool the pre-slurry containing the first part of the alkaline solution and the second part of the alkaline solution separately to a specific temperature according to their chemical composition before being added to the mixing zone of the kneader-type dissolution reactor.Furthermore, it is also possible to mix the pre-slurry and the second part of the alkaline solution in a homogenizer before the mixture thus obtained is fed into the kneader.
[0042] A pre-slurry, i.e. a slurry with a sodium hydroxide content below the solubility limit of the system, for example a pre-slurry with a sodium hydroxide content of about 2-6% by weight, for example about 3 or 4% by weight, can be cooled to near the freezing point of the mixture without starting to dissolve the cellulose carbamate. Sodium hydroxide, or a combination of sodium hydroxide and zinc oxide, lowers the freezing point of the aqueous solution. Cellulose carbamate raises the freezing point of the aqueous alkaline solution, so that the freezing point is higher than -6°C when the cellulose carbamate content in the pre-slurry is higher than 6% by weight. For example, a pre-slurry with a sodium hydroxide content of 3% by weight and a cellulose carbamate content of 6% by weight can be cooled to -6°C without freezing the mixture or starting to dissolve the cellulose carbamate.
[0043] In the second part of the alkaline solution, sodium hydroxide or a combination of sodium hydroxide and zinc oxide reduces the freezing point of the aqueous phase, and it is possible to pre-cool this second part of the alkaline solution to a temperature level between -30°C and -20°C. This further allows the concentration of the alkali, e.g. sodium hydroxide and / or zinc oxide, in the pre-slurry to be adjusted, which affects the freezing point and solubility limit of the pre-slurry as well as the swelling properties of the cellulose derivative. The alkali concentration in the pre-slurry is related to the temperature at which the cellulose derivative starts to dissolve. The higher the alkali concentration in the pre-slurry, the higher the temperature at which the cellulose derivative starts to dissolve, and similarly, the lower the alkali concentration in the pre-slurry, the lower the temperature at which the dissolution starts. This allows the swelling of the cellulose derivative to be optimized and the supply temperature of the pre-slurry to be optimized.
[0044] Preferably, the pre-slurry and the second part of the alkaline solution are fed simultaneously into the mixing zone of the continuous kneader. The chemical composition of the pre-slurry determines the chemical composition of the second part of the alkaline solution. One of the objectives of optimizing the temperature and the alkaline concentration of the pre-slurry is to prevent the start of dissolution before the mixing zone of the dissolution reactor, so as to avoid contamination of the pre-slurry handling system with the high viscosity cellulose carbamate solution.
[0045] The dissolution is carried out either under cryogenic or supercooled conditions.
[0046] By "low temperature conditions" is meant temperatures ranging from 5° C. to −6.9° C. or higher. Thus, in one embodiment, the temperature of the mixing zone is in the range of 5° C. to −6.9° C. In a particular embodiment, the temperature of the mixing zone is about 0° C. Temperatures around about 0° C., such as in the range of about 5° C. to −6.9° C., are particularly suitable for cellulose carbamate formed from chemical or dissolving pulps prepared from wood or non-wood fibers, such as commercial wood-based dissolving pulps, non-wood straw-based dissolving pulps, or dissolving pulps prepared from recycled paper and / or cardboard waste streams.
[0047] "Supercooled conditions" refers to a temperature below -7°C and above -20°C. In a further embodiment, the temperature of the mixing zone is below -7°C. Mixing zone temperatures below -7°C, typically in the range of -7°C to -20°C, are particularly suitable for cellulose carbamate formed from chemical or dissolving pulps that include or are derived from natural plant fibers, either from virgin sources, such as hemp, jute, or cotton-based sources, or recycled sources, such as recycled fibers.
[0048] In a preferred embodiment, the dissolution is carried out at about -15°C to about -20°C.
[0049] As described in some embodiments, the mixture of alkaline liquid and cellulose carbamate can be cooled by contacting it with a cooled surface, and it is generally preferred that such contact achieves cooling of the mixture to substantially the temperature of the cooled surface.
[0050] Thus, in one embodiment, cellulose carbamate is produced from cellulose having wood and / or non-wood fibers in the form of a dissolving pulp.
[0051] In a further embodiment, the cellulose carbamate is produced from cellulose having natural vegetable fibers, such as cotton, in the form of a dissolving pulp.
[0052] In a further embodiment, the cellulose carbamate is a mixture of cellulose carbamates made from both cellulose with wood and / or non-wood fibers, such as straw in the form of a dissolving pulp, and cellulose with natural vegetable fibers, such as cotton in the form of a dissolving pulp. In such an embodiment, the preferred temperature of the mixing zone is about -7°C or lower.
[0053] In a further embodiment, wood fiber derived materials such as dissolving wood pulp and / or non-wood fiber derived materials such as straw based dissolving pulp are dissolved at low temperature and natural plant fiber derived materials such as cotton derived dissolving pulp are dissolved under supercooling conditions and the separately obtained carbamate dopes are mixed after the dissolution process.
[0054] The materials that are soluble under low temperature conditions are also soluble under supercooled conditions.
[0055] It is preferred to provide cellulose carbamate with a certain range of substitution degree suitable for application in a particular embodiment.The substitution degree (DS) of cellulose carbamate polymer at least partially determines the physical and chemical conditions under which cellulose carbamate can be dissolved in alkaline aqueous solution.This also at least partially determines the concentration of the solution with respect to the cellulose moiety that can be formed from cellulose carbamate.
[0056] In one embodiment, the provided cellulose carbamate has a degree of substitution (DS) of 0.1 to 0.3, particularly about 0.25 or less. After dissolution, the DS of the cellulose carbamate decreases slightly. The degree of substitution of the cellulose carbamate is determined by total nitrogen content measurement according to SFS 5505:1988. A degree of substitution of 0.24 corresponds to a total nitrogen content of 2.0% per absolute dry water-insoluble fraction of the cellulose carbamate.
[0057] It is preferred to provide cellulose carbamate with a certain range of polymerization degree suitable for application in a particular embodiment.The polymerization degree (DP) of cellulose carbamate polymer at least partially determines the viscosity of the aqueous solution of recovered cellulose carbamate dope.The polymerization degree of cellulose carbamate polymer can be determined by intrinsic viscosity measurement according to ISO5351.
[0058] In one embodiment, the provided cellulose carbamate has a degree of polymerization (DP) of DP 200 to DP 400, particularly about DP 220 or more. A degree of polymerization value of DP 250 corresponds to an intrinsic viscosity of 197 ml / g. The mixture of cellulose carbamate dope (e.g., a mixture of cellulose carbamate, alkali, water, and possible surfactant-based additives such as polyethylene glycol (PEG), alkylamine or arylamine polyoxyethylene glycol, alcohol ethoxylate, fatty alcohol ether, etc.) has a cellulose carbamate content. In one embodiment, the mixture of cellulose carbamate has a cellulose carbamate content of 6 to 10 wt.% (in the mixture of cellulose carbamate and aqueous alkali in the mixing zone or in the cellulose carbamate dope recovered from the dissolution reactor). In a further embodiment, the mixture of cellulose carbamate dope has a cellulose carbamate content of 6 to 8 wt.%, which is a typical cellulose carbamate content obtained under low temperature or supercooling conditions. In a further embodiment, the mixture of cellulose carbamate dope has a cellulose carbamate content of 8-10 wt %, which is the preferred cellulose carbamate content under supercooling conditions.
[0059] In one embodiment, the aqueous alkaline solution, e.g., the cellulose carbamate dope, contains 5-10 wt. % NaOH. In a further embodiment, the aqueous alkaline solution, e.g., in the mixture of cellulose carbamate and aqueous alkali in the mixing zone or in the cellulose carbamate dope recovered from the dissolution reactor, contains 6-8 wt. % NaOH. In a particular embodiment, the aqueous alkaline solution contains 5-7% NaOH. This is the preferred amount of NaOH in the aqueous alkaline solution when supercooling conditions are applied.
[0060] In embodiments, the ratio of cellulose carbamate:NaOH can be important in ensuring complete dissolution of the cellulose carbamate. In embodiments, the mixture has a ratio of cellulose carbamate:NaOH of 6-10%:5-10% by weight. In certain embodiments, the mixture has a ratio of cellulose carbamate:NaOH of 8-10%:5-7% by weight, which is a preferred ratio under supercooling conditions.
[0061] In an embodiment, the actual reaction rate depends on temperature, not time. Under low temperature or undercooling conditions, the entire mass must reach the target temperature. In an embodiment, the target temperature is the output temperature of the mixing zone of the dissolution kneader and depends on the chemical composition (cellulose carbamate:NaOH ratio) and the raw material base (wood and non-wood or natural plant fibers or mixtures thereof). In a further embodiment, the residence time in the mixing zone depends on at least the following characteristics: the mechanical properties and mechanical structure of the kneader type reactor, the heat exchange properties of the surfaces of the mixing and cooling zones, the thermal energy released into the system during mixing, the cooling power of the external cooling system, the feed temperature of the mixture or the feed temperature of the preliminary slurry and the alkaline solution.
[0062] In one embodiment, the residence time is from about 1 minute to 10 hours, such as from 2 minutes to 2 hours, in particular from 2 minutes to 60 minutes or from 2 minutes to 30 minutes.
[0063] In one embodiment, alkaline hydrolysis of the carbamate groups is inhibited, and preferably prevented, during the dissolution process.
[0064] In a further embodiment, the method includes the further step of adding zinc oxide to the mixture. The zinc oxide can be added to the cellulose carbamate, the aqueous alkali solution, or the mixture of cellulose carbamate and the aqueous alkali solution. Typically, the zinc oxide is dissolved in the aqueous alkali solution prior to use as a dissolution lye of the provided cellulose carbamate. In an embodiment, the addition of zinc oxide partially improves the solubility and filterability of the solution and may partially extend the storage time before gelation begins, which also affects the viscosity of the cellulose carbamate solution and the tenacity yield of the resulting wet-spun cellulose carbamate fibers. In one embodiment, the mixture has a zinc oxide content of 0.1-1.5% by weight of the mixture. In one embodiment, the mixture is at least partially defined by the ratio of cellulose carbamate to zinc oxide. Thus, in one embodiment, the cellulose carbamate has a ratio of cellulose carbamate:ZnO of 6-10%:0.1-1.5%, which means 0.01-0.25 t ZnO per t cellulose carbamate.
[0065] In one embodiment, there is provided a method for dissolving cellulose carbamate in an alkaline aqueous phase to form a solution, the method including the steps of providing cellulose carbamate by carbonization of raw cotton material, mixing the cellulose carbamate with an alkaline aqueous solution to form a mixture, producing a solution of cellulose carbamate in the alkaline aqueous phase, and recovering the cellulose carbamate-containing aqueous phase, wherein the step of producing the solution is performed at a temperature of −7° C. or less.
[0066] In one embodiment, there is further provided a method for dissolving cellulose carbamate in an alkaline aqueous phase to form a solution, the method comprising the steps of providing cellulose carbamate, mixing the cellulose carbamate with an alkaline aqueous solution to form a mixture, producing a solution of cellulose carbamate in the alkaline aqueous phase, and recovering the cellulose carbamate-containing aqueous phase, wherein the step of producing a solution is carried out at a temperature of 10°C or less, the cellulose carbamate is first mixed with a first portion of the alkaline aqueous solution to produce a pre-slurry, the pre-slurry thus obtained is fed to a mixing zone, a second portion of the alkaline aqueous solution is separately fed to the mixing zone, and the pre-slurry is held in the mixing zone at a temperature of -1°C to -6°C before the second portion is fed to the mixing zone.
[0067] In one embodiment, the continuous dissolution process is obtained by feeding the cellulose carbamate / zincate mixture, prepared in one or two steps, where the zincate comprises ZnO and NaOH, onto the surface of, for example, a rotating cylinder, where the temperature of the mixture is reduced to a target temperature in the range of -15°C to -20°C. The cooled material is removed from the cooling surface, for example scraped off, and the temperature of the solid material is optionally maintained at the target temperature or further cooled and then adjusted to a temperature suitable for further processing, for example by filtering, degassing, spinning. In addition to cylinders, various other devices can be used, such as drums, which generally have a flat or curved heat-conducting surface that can be cooled. The surface can be stationary or moving in a rotating manner. The above temperature range for cooling is particularly suitable for flocculent carbamates and is suitable for achieving a solution with a predetermined ratio between cellulose carbamate and sodium hydroxide and zinc oxide, as discussed herein.
[0068] In one embodiment, contacting the cellulose carbamate with the zincate solution can be efficiently accomplished by mixing, optionally with a stirrer or homogenizer, before adjusting the temperature of the mixture to a range that promotes dissolution. Generally, efficient mixing is preferred to improve contact between the phases and provide a homogenous mixture, but dissolution is already accomplished by cooling.
[0069] In the two-step process embodiment of combining the preslurry with the second portion of the zincate solution, it is preferred to use a homogenizer since the preslurry can be precooled at a low NaOH content without initiating dissolution of the cellulose carbamate. In such an embodiment, it is preferred to precool the second portion of the zincate to as low a temperature as practical, thereby achieving dissolution upon combining the preslurry with the second zincate portion.
[0070] In both the one-stage and two-stage methods, lowering the temperature of the mixture initiates at least partial dissolution of the cellulose carbamate, and in a preferred embodiment, is technically feasible to apply the mixture to the surface of a rotating drum.
[0071] Reducing the temperature of the mixture is also advantageous prior to application to a cooled metal surface. Thus, in one embodiment, the mixture delivered to the surface of a cooled metal surface or a cooled cylinder passes through a mixing and cooling zone to cool the mixture and achieve partial dissolution before the mixture is delivered to the surface of a cooled metal surface (e.g. a metal plate, typically a stainless steel plate) or a cooled cylinder (e.g. stainless steel).
[0072] In one embodiment, dissolution of the cellulose carbamate of the dissolving pulp is accomplished at a temperature higher than that typically applied to cotton carbamate (-15°C to -20°C).
[0073] Based on the above, in the method for continuously producing a solution of cellulose carbamate, the step of producing the solution from the mixture is carried out on a cooled metal surface or a cooled cylinder, such as the surface of a cooled rotating drum. For example, the mixture is fed onto the surface of a cooled metal surface or a cooled cylinder having a temperature of about 0° C. or below −7° C.
[0074] In one embodiment, the cellulose carbamate is first mixed with a first portion of the alkaline solution, the pre-slurry thus obtained is mixed with a second portion of the alkaline solution, and the mixture thus obtained is delivered to a cooled metal surface or to the surface of a cooled cylinder.
[0075] In one embodiment, the pre-slurry is cooled to a temperature of 0° C. to −6° C., such as −1° C. to −6° C., or −2° C. to −6° C. In one embodiment, the second portion of the alkaline solution is cooled to a temperature of −7° C. to −30° C. In one embodiment, the temperature of the cooled metal surface or the surface of the cooled cylinder is at least about −15° C., such as 15° C. to about −20° C. or less, to bring the mixture down to a target temperature in the range of −15° C. to −20° C.
[0076] In one embodiment, the mixture is contacted with the cooled metal surface or the surface of a cooled cylinder zone for a time between 1 minute and 10 hours, such as between 2 minutes and 2 hours, in particular between 2 minutes and 60 minutes or between 4 minutes and 30 minutes.
[0077] Dissolving under low temperature and / or supercooling conditions results in a cellulose carbamate solution of suitable quality for the spinning process. Dissolving cellulose carbamate at high cellulose consistency results in a cellulose carbamate spinning dope with a lower viscosity than would be mathematically and experimentally expected if dissolved in a conventional manner. Typically, the viscosity of a cellulose carbamate dope with a cellulose carbamate (DP 250, DS 0.2%) content of 8.5%, a NaOH content of 6.5%, and a ZnO content of 1.3%, recovered after dissolving in a conventional manner and then tempering at +20°C, is higher than 15 Pas. Preferably, technically suitable cellulose carbamate spinning dopes have a viscosity of less than 15 Pas. The viscosity of the cellulose carbamate spinning dope according to the embodiment is preferably <15 Pas. The viscosity of the cellulose carbamate spinning dope is measured by the Ballfall viscosity method at 20°C. Furthermore, the method of the present invention provides a cellulose spinning dope that is stable for a long period of time even at room temperature.
[0078] Typically, the temperature of the mixture is maintained at the target temperature for a period of from 1 minute to 30 minutes, for example from 3 minutes to 15 minutes.
[0079] The embodiments will now be described by the following examples.
[0080] Working Example
[0081] Example 1. Continuous dissolution of cellulose carbamate by a one-step method under supercooled conditions starting from cellulose carbamate derived from recycled cotton
[0082] The cellulose carbamate polymers were provided by the carbamate process carried out as described in Finnish Patents Nos. 112869, 112795, and Finnish Patent Applications Nos. 275376 and 20195717, and in International Patent Application PCT / FI2020 / 050560.
[0083] A mixture of cellulose carbamate polymer and aqueous alkaline solution was formed as follows: a cellulose carbamate polymer with a degree of polymerization (DP) of 250 (determined as intrinsic viscosity according to ISO 5351), corresponding to 850 g of absolute dry substance, and a degree of substitution (DS) of 0.22 (determined as total nitrogen content according to SFS5505:1988) was mixed with 9150 g of aqueous alkaline solution containing 650 g of sodium hydroxide, 110 g of zinc oxide and 8390 g of water, and stirred in a homogenizer at a mixing speed of 700 rpm for 40 minutes at room temperature of about 20°C.
[0084] As a kneader-type dissolution reactor, a twin-screw extruder model of Berstroff ZE 25x49.5 was used. Its cooling and mixing zone consisted of 12 separate barrel units arranged in series. The cylinder walls of each barrel unit were cooled to the desired temperature by an ethylene glycol refrigerant circuit using an external cooler. For continuous dissolution operation, the mixing zone was precooled to -20 °C. The twin-screw extruder was equipped with a funnel, and the mixture of cellulose carbamate polymer in an aqueous alkali solution was fed into the precooled mixing zone, the temperature of which was maintained by an external cooler. By adjusting the screw rotation speed to 16 rpm, the feed rate was set at 3.9-4.0 kg / h, the moment was 50-53%, and the motor power consumption was 415 W.
[0085] The mixture of cellulose carbamate polymer in alkaline aqueous solution was continuously fed into the system for 140 minutes, and the cellulose carbamate solution in alkaline aqueous solution was collected at a rate of 3.9-4.0 kg / h. The residence time of the mixture in the mixing zone was 6±0.5 minutes. The temperature of the collected solution was -15.3°C to -17.5°C at the mixing zone exit of the extruder. The collected solution was immediately thermostated to a temperature of +10°C.
[0086] The recovered cellulose carbamate solution was sampled and its properties were examined, with the results being as follows: The recovered cellulose carbamate solution had a cellulose carbamate content of 8.5%, a sodium hydroxide content of 6.5%, a zinc oxide content of 1.1%, a ballfall viscosity measured at +20°C of 8.7 Pas, and a filterability index (K R ) was 0.30.
[0087] For cellulose carbamate fiber wet spinning, a second portion of the carbamate solution corresponding to the characterized composition was filtered through a 10 μm filter medium and degassed at +10 °C for 12 h. Wet spinning of the filtered and degassed cellulose carbamate dope was performed using a spin bath optimized for the cellulose carbamate process, e.g., containing sodium sulfate and free sulfuric acid. The godet drawing stress at fiber harvest was 68-71% under hot bath drawing conditions. The resulting filament fineness was 1.3 dtex. The fiber breaking strength measured from the filament samples was >20 cN / tex (SFS-EN ISO 5079).
[0088] Example 2. Continuous dissolution of cellulose carbamate by a two-step method under supercooling conditions starting from cellulose carbamate derived from recycled cotton
[0089] The cellulose carbamate polymers were provided by the carbamate process carried out as described in Finnish Patents Nos. 112869, 112795, and Finnish Patent Applications Nos. 275376 and 20195717, and in International Patent Application PCT / FI2020 / 050560.
[0090] The preliminary slurry, i.e. a mixture of cellulose carbamate polymer and aqueous alkaline solution, was formed as follows: Cellulose carbamate with a degree of polymerization (DP) of 333 (determined as intrinsic viscosity according to ISO 5351) in an amount corresponding to 3840 g of absolute dry matter with a degree of substitution (DS) of 0.24 (determined as total nitrogen content according to SFS 5505:1988) was mixed with a first portion of 46076 g of aqueous alkaline solution containing 1497 g of sodium hydroxide, 508 g of zinc oxide and 44071 g of water in a homogenizer equipped with a cooling jacket for 30 minutes. To prevent phase separation, the preliminary slurry was cooled and tempered to a temperature of +0.6°C before gentle mixing. The content of cellulose carbamate in the preliminary slurry was 7.7% by weight, the content of sodium hydroxide was 3.0% by weight and the content of zinc oxide was 1.0% by weight. A second portion of the aqueous alkaline solution was prepared separately and cooled to -16.3°C. This aqueous solution contained 3620 g of sodium hydroxide, 324 g of zinc oxide, and 10141 g of water, with a sodium hydroxide content of 25.7% by weight and a zinc oxide content of 2.30% by weight.
[0091] As a kneader-type dissolution reactor, a kneader-type dissolution reactor manufactured by LIST Technology was used, which was equipped with a 14-liter dissolution chamber with a cooling jacket, two co-rotating shafts capable of temperature control, and a discharge screw capable of continuous operation. The ethylene glycol coolant was cooled to -10°C by an external cooler and passed through the jacket of the dissolution reactor and its shaft. The cellulose carbamate slurried with the alkaline aqueous solution of the first part and the alkaline aqueous solution of the second part were continuously fed at a predetermined rate to the mixing and cooling zone of the dissolution reactor using two separate peristaltic pumps. The feed rate of the preliminary slurry was 22.62 kg / h, and the feed rate of the second part was 6.39 kg / h.
[0092] The continuous mode operation included the following steps: first, the kneader was filled to the desired filling level of 80% for a given residence time of 25 min, then the discharge screw was rotated and its speed was adjusted to maintain the filling level. After stabilizing the reaction for a time equal to the residence time with constant feed and discharge, the recovery of the cellulose carbamate solution was started at a rate of 29.0 kg / h. The speed of the rotating shaft was 20 rpm. Recovery was possible as long as the feed was stable. If one or more parameters changed during the continuous dissolution process, a stabilization period equal to the residence time is necessary to recover a representative product. The temperature of the recovered solution was -7.9 °C at the output of the mixing zone of the dissolution reactor.
[0093] The recovered cellulose carbamate solution was sampled and its properties were examined, with the results being as follows: The recovered cellulose carbamate solution had a cellulose carbamate content of 6.2%, a sodium hydroxide content of 8.1%, a zinc oxide content of 1.3%, a Ballfall viscosity measured at +20°C of 3.3 Pas, and a filterability index (K R ) was 1.49.
[0094] Example 3: Batch dissolution of cellulose carbamate in a two-step process under low temperature conditions starting with dissolving cellulose carbamate derived from wood pulp (pine: spruce)
[0095] The cellulose carbamate polymers were provided by a carbamate process carried out as described in Finnish Patents Nos. 112869, 112795 and International Patent Application PCT / FI2020 / 050560.
[0096] The preliminary slurry, i.e., a mixture of cellulose carbamate polymer and aqueous alkaline solution, was formed as follows: Cellulose carbamate with a degree of polymerization (DP) (determined as intrinsic viscosity according to ISO 5351) of 270, in an amount corresponding to 29.3 kg of absolute dry matter with a degree of substitution (DS) (determined as total nitrogen content according to SFS 5505:1988) of 0.17, was mixed in two stages with a first portion of 310.2 kg of aqueous alkaline solution containing 10.3 kg of sodium hydroxide, 1.92 kg of zinc oxide, and 300 kg of water in a 500 L batch dissolution reactor tank equipped with a cooling jacket and a propeller mixing unit. As a result, the sodium hydroxide concentration in the preliminary slurry was 3.0 wt%, the zinc oxide concentration was 0.57 wt%, and the cellulose carbamate content was 8.6 wt%. The ethylene glycol coolant was cooled to -9°C by a separate chiller and flowed through the jacket of the dissolution reactor. The alkaline aqueous solution was pre-cooled to -2.9°C before mixing with the cellulose carbamate polymer in the dissolution reactor, and the resulting pre-slurry was stirred at about 250 rpm to adjust the temperature to a temperature level of -1°C to -2°C, and left to stand with gentle stirring to prevent phase separation.
[0097] The second part of the aqueous alkali solution was prepared separately and cooled to -18°C. The total amount of the second liquid was 108 kg, containing 25.7 kg of sodium hydroxide, 3.9 kg of zinc oxide, and 78.4 kg of water, i.e., sodium hydroxide concentration of 23.8 wt% and zinc oxide concentration of 3.64 wt%. The second part of the aqueous alkali solution was added to the dissolution reactor while continuously mixing with the preliminary slurry at a stirring speed of 375 rpm. The temperature of the resulting aqueous alkali solution of cellulose carbamate was -4.5°C at the beginning of mixing the two parts together, but the temperature of the solution rose to 0°C during the prolonged mixing. The resulting solution was collected at a temperature of 0°C. The target cellulose dope quality was obtained 15 minutes after the second addition of the aqueous alkali solution.
[0098] The recovered cellulose carbamate solution was sampled and its properties were examined, with the results being as follows: The recovered cellulose carbamate solution had a cellulose carbamate content of 6.5%, a sodium hydroxide content of 8.0%, a zinc oxide content of 1.3%, a ballfall viscosity measured at +20°C of 2.5 Pas, and a filterability index (K R ) was 3.4.
[0099] For cellulose carbamate fiber wet spinning, the cellulose carbamate solution corresponding to the characteristic composition was subsequently filtered using a two-stage backflush filtration process using a 15 μm filter medium in the second filtration stage. Wet spinning of the filtered and degassed cellulose carbamate dope was carried out using a spin bath optimized for the cellulose carbamate process, e.g., containing sodium sulfate and free sulfuric acid. The godet drawing stress at fiber harvest was 72-78% under hot bath drawing conditions. The resulting filament fineness was 1.3 dtex. The fiber breaking strength measured from the filament samples was >20 cN / tex (SFS-EN ISO 5079).
[0100] Example 4. Batch dissolution of cellulose carbamate solution by a two-step process under supercooled temperature conditions starting from cellulose carbamate derived from recycled cotton
[0101] The cellulose carbamate polymers were provided by the carbamate process carried out as described in Finnish Patents Nos. 112869, 112795, and Finnish Patent Applications Nos. 275376 and 20195717, and in International Patent Application PCT / FI2020 / 050560.
[0102] The preliminary slurry, i.e., a mixture of cellulose carbamate polymer and aqueous alkaline solution, was formed as follows: Cellulose carbamate with a degree of polymerization (DP) (determined as intrinsic viscosity according to ISO 5351) of DP 265, in an amount equivalent to 27 kg of absolute dry material with a degree of substitution (DS) (determined as total nitrogen content according to SFS 5505:1988) of 0.19, was mixed in two stages with a first portion of 285 kg of aqueous alkaline solution containing 9.45 kg of sodium hydroxide, 3.27 kg of zinc oxide, and 276 kg of water in a 500 L batch dissolution reactor tank equipped with a cooling jacket and a propeller mixing unit. Thus, the sodium hydroxide concentration in the preliminary slurry was 3.0 wt%, the zinc oxide concentration was 1.0 wt%, and the cellulose carbamate content was 8.7 wt%. The ethylene glycol coolant was cooled to -9°C by a separate cooler and flowed through the jacket of the dissolution reactor. The aqueous alkaline solution was pre-cooled to −2.5° C. before mixing with the cellulose carbamate polymer in the dissolution reaction tank, and the resulting pre-slurry was allowed to stand without mixing after a 10-minute cooling period, and then was adjusted to a temperature of approximately −2° C. by pulse mode stirring at 375 rpm for 10 seconds.
[0103] A second portion of the alkaline aqueous solution was prepared separately and cooled to -26.6°C. A total of 135 kg of aqueous solution was prepared, containing 26.4 kg of sodium hydroxide, 2.6 kg of zinc oxide, and 106 kg of water, i.e., 19.7% sodium hydroxide and 1.9% zinc oxide by weight. The second portion of the alkaline aqueous solution was added to the dissolution reactor while continuously stirring with the pre-slurry at a stirring speed of 375 rpm. The resulting solution was collected at a temperature of -7.5°C. The desired cellulose dope quality was obtained 15 minutes after the second addition of the alkaline solution.
[0104] The recovered cellulose carbamate solution was sampled and its properties were examined, with the results being as follows: the cellulose carbamate content in the recovered cellulose carbamate solution was 6.0%, the sodium hydroxide content was 8.0%, the zinc oxide content was 1.3%, the Ballfall viscosity measured at +20°C was 1.9 Pas, and the filterability index (K R) was 2.3.
[0105] For cellulose carbamate fiber wet spinning, the cellulose carbamate solution corresponding to the characteristic composition was subsequently filtered using a two-stage backflush filtration process using a 15 μm filter medium in the second filtration stage. Wet spinning of the filtered and degassed cellulose carbamate dope was carried out using a spin bath optimized for the cellulose carbamate process containing, for example, sodium sulfate and free sulfuric acid. The godet drawing stress at the time of fiber sampling was 80-88% under hot bath drawing conditions. The resulting filament fineness was 1.3 dtex. The fiber breaking strength measured from the filament samples was >20 cN / tex (SFS-EN ISO 5079).
[0106] Example 5. Effect of dissolution temperature and sodium hydroxide concentration on the dissolution of cellulose carbamate derived from regenerated cotton
[0107] FIG. 3 shows the effect of dissolution temperature and sodium hydroxide concentration on the dissolution of cellulose carbamate from regenerated cotton. The figure includes 27 micrographs arranged in a matrix of 4 columns and 7 rows. The first column shows micrographs of samples at temperatures of -10°C, and the next three columns show micrographs of samples at temperatures of -5°C, 0°C, and 5°C. The rows are arranged such that the sample in the first row contains 3.92 wt% NaOH, and the next six rows contain 4.81 wt%, 5.66 wt%, 6.48 wt%, 7.27 wt%, 8.04 wt%, and 8.77 wt%, respectively, from top to bottom. It can be seen that the lower the dissolution temperature used, the lower the sodium hydroxide content required to dissolve the cellulose carbamate polymer in the aqueous alkaline solution. It can be further seen that the aqueous cellulose carbamate solution with a sodium hydroxide content of 8.04% or more recovered at temperatures below -5°C and above -10°C still contains undissolved cellulose carbamate-based fragments.
[0108] Example 6. Stability of pre-slurry in a two-stage dissolution process
[0109] Figure 4 shows the stability of the pre-slurry for the two-stage dissolution process. The figure includes microscopic images of cellulose carbamate samples at four different temperatures, namely, -5°C, -6°C, -7°C and -8°C. The cellulose carbamate was slurried in an aqueous alkaline solution corresponding to a composition of 3 wt% sodium hydroxide, 1.0 wt% zinc oxide and 6 wt% cellulose carbamate. As is evident from the microscopic images in Figure 4, the fibrous structure of the cellulose carbamate from regenerated cotton remained undissolved at temperature levels up to -6°C, at temperatures below -7°C the cellulose carbamate polymer started to dissolve slightly, and at temperatures below -8°C the pre-slurry froze.
[0110] Example 7. Stability of Cellulose Carbamate Polymer Slurry in Aqueous Alkaline Solution
[0111] Figure 5 shows the stability of cellulose carbamate polymer slurries. The samples were prepared in a one-step dissolution process up to the final chemical composition for the dissolution process. For each sample, rheometric shear flow curves were obtained for a mixture of 8.5 wt% cellulose carbamate with an aqueous solution containing 6.5 wt% sodium hydroxide and 1.1 wt% zinc oxide as a function of temperature (shear flow measured at +20°C, +15°C, +10°C, +5°C, 0°C and -5°C). As can be seen, the viscosity measured for both increasing (inc.) and decreasing (dec.) shear rates is constant at temperatures above +5°C. At temperatures below 0°C, the solution begins to resist mixing and at the same time an increase in viscosity is detected.
[0112] Example 8. Micrograph of cellulose carbamate solution
[0113] Micrographs of the recovered solutions of cellulose carbamate obtained by phase contrast mode are shown in Figures 6A-6C. The micrographs show the K measured from the recovered cellulose carbamate solutions as described in Examples 1-4. R It reflects the index.
[0114] Figure 4A shows a cellulose carbamate solution in which the cellulose carbamate polymer has very good solubility in an alkaline aqueous solution. Figure 4B shows a cellulose carbamate solution in which the cellulose carbamate polymer has good solubility in an alkaline aqueous solution. Figure 4C shows a cellulose carbamate solution in which the cellulose carbamate polymer has poor solubility in an alkaline aqueous solution.
[0115] K W value and K R Index (K R is the viscosity correction K W The filterability of the cellulose carbamate solution is indicated by the β-value (corresponding to the β-value). A lower value means that the amount of unreacted particles of filter-clogging size (>10 μm) is smaller in the recovered cellulose carbamate solution.
[0116] Measured K was collected as described in Example 1 (continuous dissolution of cellulose carbamate in a one-step process under supercooling conditions starting from cellulose carbamate derived from regenerated cotton). R The cellulose carbamate solution with an index of 0.30 corresponds to the visual transparency image shown in FIG. 4A.
[0117] The cellulose carbamate solutions recovered as described in Examples 2-4 were as follows: Example 2: Continuous dissolution of cellulose carbamate by a two-stage process under supercooled conditions starting from cellulose carbamate from regenerated cotton. Example 3: Batch dissolution of cellulose carbamate by a two-stage process under low temperature conditions starting from cellulose carbamate from dissolving wood pulp (pine: spruce). Example 4: Batch dissolution of cellulose carbamate solution by a two-stage process under supercooled temperature conditions starting from cellulose carbamate from regenerated cotton. For these examples, the measured KR index was 1.49-3.4, which corresponds to the visual transparency image in FIG. 4B.
[0118] Example 9. Continuous dissolution of cellulose derivatives
[0119] Cellulose carbamate (powder) obtained from 100% cotton-based fiber pulp with a DP of 245 and a DS of 0.20 was used in the following tests.
[0120] Formation of CCA-Chlorite Slurry in One Step:
[0121] a) CCA powder was slurried in aqueous sodium zincate solution by a one-step process to obtain a slurry with 8.5 wt% CCA content, 6.5 wt% NaOH content, and 1.3 wt% ZnO content. The carbamate-zincate slurry at a temperature of +15°C was instantly cooled on a metal surface that was pre-cooled to a temperature of -20°C before being applied onto the metal surface. The contact time on the metal surface was 20 seconds during which the temperature of the slurry reached that of the metal surface, and the formed CCA dope was tempered at +15°C for microscopic observation (as can be seen in the photograph of Figure 7A, the dissolution of CCA is not complete).
[0122] b) The CCA powder was slurried in an aqueous sodium zincate solution in a one-step process to obtain a slurry with a CCA content of 8.5 wt%, a NaOH content of 6.5 wt%, and a ZnO content of 1.3 wt%. The slurry was pre-cooled to a temperature of -5.5°C before being applied onto a steel surface pre-cooled to -20°C. The contact time on the steel surface was 20 seconds, during which the temperature of the slurry reached that of the steel surface, and the formed CCA dope was thermostated to +15°C for microscopic examination (as can be seen in the photograph of Figure 7B, the dissolution of CCA was more complete than in the case of the slurry initially at +15°C).
[0123] c) The CCA powder was slurried in an aqueous sodium zincate solution in a one-step process to obtain a slurry with a CCA content of 8.5 wt.%, a NaOH content of 6.5 wt.%, and a ZnO content of 1.3 wt.%. This slurry was pre-cooled to a temperature of -5.5°C before being applied to a steel surface pre-cooled to a temperature of -20°C. The contact time on the surface was 20 seconds, during which the temperature of the slurry reached the temperature of the steel surface, and the cooled mixture was then immediately removed from contact with the surface and the temperature was maintained at -20°C for 5 minutes before temperature-conditioning the formed CCA dope to +15°C for microscopic examination (as can be seen in the photograph of Figure 7C, the dissolution of the CCA was more complete than in test b with a contact time of 20 seconds at -20°C).
[0124] Formation of CCA-Chlorite Slurry in Two Stages:
[0125] d) A preliminary slurry with a CCA content of 10.8 wt.%, a NaOH content of 3.5 wt.% and a ZnO content of 1.2 wt.% was prepared and pre-cooled to -0.5°C, and a second portion of the aqueous zincate solution was added by mixing (pre-cooled to +5°C) to obtain the final target composition (8.5 wt.% CCA, 6.5 wt.% NaOH and 1.3 wt.% ZnO). The temperature of the mixture constituting the final target composition was +1°C before application to the steel surface pre-cooled to -20°C. The photograph in Figure 7D shows the dissolution rate in the mixture before surface contact (dissolution is not yet complete as can be seen in the photograph).
[0126] The photograph in FIG. 7E shows the dissolution rate of the CCA dope after 20 seconds of surface contact time at a temperature of −20° C. (As can be seen in the photograph, the dissolution was complete with improved transparency compared to the one-step process.) During the contact time, the temperature of the slurry reached that of the steel surface.
[0127] The photograph in Figure 7F shows the dissolution rate of the CCA dope after 20 seconds of surface contact time at a temperature of -20 °C, followed by 5 minutes of rest at -20 °C after surface contact (as seen in Figure 1F, the visual transparency of the CCA dope did not increase significantly with an additional 5 minutes of rest at -20 °C).
[0128] It is to be understood that the disclosed embodiments of the invention are not limited to the particular structures, process steps, or materials disclosed herein, but extend to equivalents thereof that would be recognized by one of ordinary skill in the relevant arts. It is also to be understood that the terminology used herein is used for the purpose of describing particular embodiments only, and is not intended to be limiting.
[0129] Throughout this specification, a reference to an embodiment or an embodiment means that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the present invention. Thus, although the phrases "in one embodiment" or "in an embodiment" appear in various places throughout this specification, they do not necessarily all refer to the same embodiment. For example, when a numerical value is referred to using terms such as about, substantially, the exact numerical value is also disclosed.
[0130] As used herein, a plurality of items, structural elements, components, and / or materials may be presented in a common list for convenience. However, these lists should be construed as if each member of the list were individually identified as a separate and unique member. Thus, the individual members of such lists should not be construed as de facto equivalents of other members of the same list solely based on their presentation in a common group, absent a contrary indication. Furthermore, various embodiments and examples of the invention may be referred to herein along with alternatives of its various components. It should be understood that such embodiments, examples, and alternatives are not construed as de facto equivalents of each other, but are considered as separate and autonomous representations of the invention.
[0131] Furthermore, the described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, numerous specific details, such as examples of lengths, widths, shapes, etc., are provided to provide a thorough understanding of embodiments of the invention. However, one of ordinary skill in the relevant art will recognize that the invention can be practiced without one or more of the specific details, or with other methods, components, materials, etc. In other instances, well-known structures, materials, or operations are not shown or described in detail to avoid obscuring aspects of the invention.
[0132] While the above-described examples illustrate the principles of the present invention in one or more particular applications, it will be apparent to those skilled in the art that numerous changes in form, use and details of implementation may be made without the exercise of inventive faculty and without departing from the principles and concepts of the present invention. Accordingly, it is not intended that the present invention be limited except as by the scope of the claims which follow.
[0133] In this specification, the verbs "comprise" and "have" are used as open limitations that do not exclude or require the presence of any unrecited features. Features recited in the claims may be freely combined with each other unless otherwise expressly stated. Furthermore, it is to be understood that the use of "a" or "an" throughout this specification, i.e., the singular form, does not exclude the plural form.
[0134] Below, some further embodiments are disclosed.
[0135] 1. A method for dissolving cellulose carbamate in an alkaline aqueous phase to form a solution, comprising the steps of: providing cellulose carbamate by carbonization of raw cotton material; mixing cellulose carbamate with an aqueous alkaline solution to form a mixture; forming a solution of cellulose carbamate in an alkaline aqueous phase; and recovering the cellulose carbamate containing aqueous phase, The method wherein the step of forming the solution is carried out at a temperature of -7°C or lower.
[0136] 2. The method of embodiment 1, wherein the cotton feedstock comprises virgin cotton, recycled cotton, cotton-containing textiles, or cotton-containing textile waste, or a combination thereof.
[0137] 3. The process according to embodiment 1 or 2, wherein the cotton raw material comprises up to 50% by weight, preferably 40% by weight or less, of non-cotton cellulosic material, e.g. wood fiber-derived material as dissolving wood pulp, and / or non-wood fiber-derived material, e.g. straw-based dissolving pulp.
[0138] 4. The method of any of the preceding embodiments, wherein the step of generating the solution is carried out at a temperature of -7°C or lower, preferably -8°C or lower.
[0139] 5. The method of any of the preceding embodiments, wherein the step of producing a solution of cellulose is carried out in a mixing zone, and the mixing zone is operated in a batch mode, semi-continuously or continuously.
[0140] 6. The method according to any of the preceding embodiments, wherein the cellulose carbamate is mixed with a first portion of an alkaline solution to produce a pre-slurry, and the pre-slurry thus obtained is fed to the mixing zone, and a second portion of the alkaline solution is fed separately to the mixing zone.
[0141] 7. The method of claim 6, wherein the pre-slurry is cooled to a temperature of 0°C to -6°C, such as -1°C to -6°C or -2°C to -6°C.
[0142] 8. The method of embodiment 6 or 7, wherein the second portion of the alkaline solution is cooled to a temperature of -7°C to -30°C.
[0143] 9. The method of any of embodiments 6-8, wherein the preliminary slurry has an alkali concentration, such as NaOH, of 2-6 wt. % and / or the second portion has an alkali concentration, such as NaOH, of 10-30 wt. %.
[0144] 10. The method of any of the preceding embodiments, wherein the provided cellulose carbamate has a degree of polymerization (DP) of about 200 or more, particularly DP 250 to DP 400.
[0145] 11. The method of any of the preceding embodiments, wherein the mixture of cellulose carbamates has a cellulose carbamate content of 6 to 10 wt%, such as a cellulose carbamate content of 6 to 8 wt%, or a cellulose carbamate content of 8 to 10 wt%.
[0146] 12. The method of any of the preceding embodiments, wherein the aqueous alkaline solution contains 5-10 wt% NaOH, e.g., the aqueous alkaline solution contains 7-10 wt% NaOH, or the aqueous alkaline solution contains 5-7 wt% NaOH.
[0147] 13. The method according to any of the preceding embodiments, wherein the mixture has a ratio of cellulose carbamate to NaOH of 6-10% by weight:5-10% by weight, preferably 6-8%:7-10%, for example 8-10%:5-7%, especially when operating continuously.
[0148] 14. A method for dissolving cellulose carbamate in an alkaline aqueous phase to form a solution, comprising: providing a cellulose carbamate; mixing cellulose carbamate with an aqueous alkaline solution to form a mixture; forming a solution of cellulose carbamate in an alkaline aqueous phase; and recovering the cellulose carbamate-containing aqueous phase; The step of forming the solution is carried out at a temperature of 10° C. or less; 1. A method according to claim 1, wherein cellulose carbamate is first mixed with a first portion of an aqueous alkaline solution to form a pre-slurry, the pre-slurry thus obtained is fed to a mixing zone, and a second portion of the aqueous alkaline solution is separately fed to the mixing zone, and the pre-slurry is maintained at a temperature of -1°C to -6°C in the mixing zone before the second portion is fed to the mixing zone.
[0149] 15. The method of embodiment 14, wherein the second portion fed to the mixing zone has a temperature of -7 to -30°C.
[0150] 16. The method of embodiment 14 or 15, wherein the pre-slurry has a concentration of NaOH of 2-6 wt. % based on the weight of the pre-slurry and / or the second portion has a concentration of NaOH of 10-30 wt. % based on the weight of the second portion.
[0151] 17. The method according to any of embodiments 14 to 16, wherein the mixture has a ratio of cellulose carbamate to NaOH of 6-10% by weight:5-10% by weight, for example 6-8% by weight:7-10% by weight, for example 8-10% by weight:5-7% by weight, especially when operating continuously.
[0152] 18. The method according to any of embodiments 14 to 17, wherein the dissolution is carried out at a temperature of about -15°C to about -20°C.
[0153] 19. Providing a cellulose carbamate; mixing cellulose carbamate with an alkaline aqueous solution to form a mixture; passing said mixture through a mixing zone of a continuously operated kneader-type dissolution reactor to produce a solution of said cellulose carbamate in an alkaline aqueous phase; and recovering the cellulose carbamate-containing aqueous phase. [Explanation of symbols]
[0154] 10 Pulper 20 Storage Tank 30 Pump 40 Dissolution Reactor 100 Cellulose carbamate 200 Alkaline solution (total) 300 Alkali / Cellulose Carbamate Mixture 330 Alkaline aqueous solution (total) / Cellulose carbamate mixture 400 Cellulose carbamate in alkaline aqueous solution 2000 First portion of alkaline solution 2200 Second part of alkaline solution 3000 Preliminary slurry of cellulose carbamate and aqueous alkali solution [Industrial Applicability]
[0155] At least some embodiments of the present invention find industrial application, particularly in the regeneration of cellulosic fiber derivatives for use in the textile and nonwoven industries or the pulp and paper industries.
Claims
1. 1. A method for continuously dissolving cellulose carbamate in an alkaline aqueous phase to form a solution, comprising: providing a cellulose carbamate; mixing cellulose carbamate with an aqueous alkaline solution to form a mixture; forming a solution of the cellulose carbamate in an alkaline aqueous phase from the mixture; and recovering the cellulose carbamate-containing aqueous phase, The method wherein the step of forming the solution is carried out by directing said mixture through a mixing zone of a continuously operated kneader-type dissolution reactor at a mixing speed of 10 to 500 rpm and at a temperature of 10° C. or less.
2. The method according to claim 1, characterized in that the mixture formed by cellulose carbamate in the aqueous alkaline solution is subjected to mixing in the mixing zone of the kneader-type dissolution reactor at a mixer speed of not more than 250 rpm, most suitably not more than 100 rpm, preferably not more than 50 rpm.
3. 2. The method according to any of the preceding claims, characterized in that the mixture formed by cellulose carbamate in the aqueous alkaline solution is subjected to cooling in the mixing zone of the kneader-type dissolution reactor.
4. The cellulose carbamate is first mixed with a first portion of an alkaline solution, the pre-slurry thus obtained is fed into a mixing zone of a continuously operating mixer kneader, and a second portion of the alkaline solution is fed into a mixing zone of a continuously operating mixer kneader, 10. The method according to any of the preceding claims, characterized in that the pre-slurry is preferably mixed with a second portion of the alkaline solution in a homogenizer before feeding the mixture thus obtained into the kneader. method.
5. 5. The method according to claim 4, characterized in that the pre-slurry is cooled to a temperature of 0°C to -6°C, for example 1°C to -6°C, or -2°C to -6°C, and the second portion of the alkaline solution is cooled to a temperature of -7°C to -30°C.
6. the temperature of the mixture in the mixing zone is about 0° C., or the temperature of the mixture in the mixing zone is about -7°C or less; or 2. The process according to any of the preceding claims, characterized in that the temperature of the mixture in the mixing zone is from about -15°C to about -20°C.
7. 10. The method according to any of the preceding claims, characterized in that a pre-cooling is achieved in a first kneader, whereby a partial dissolution is obtained, and after that step the mixture is transferred to a second kneader, in which the materials are typically completely or substantially completely dissolved.
8. The cellulose carbamate is produced from a dissolving pulp derived from cellulose fibers other than natural plant fibers, 10. The method according to any of the preceding claims, characterized in that the provided cellulose carbamate preferably has a degree of polymerization (DP) of about DP 200 or more, in particular DP 220 to DP 400.
9. the mixture of cellulose carbamates has a cellulose carbamate content of 6 to 10 wt%, for example a cellulose carbamate content of 6 to 8 wt%, or a cellulose carbamate content of 8 to 10 wt%, 5. The method according to any of the preceding claims, characterized in that the aqueous alkaline solution contains 5 to 10 wt. % NaOH, such as the aqueous alkaline solution contains 7 to 10 wt. % NaOH, or the aqueous alkaline solution contains 5 to 7 wt. % NaOH.
10. 10. The method according to any of the preceding claims, characterized in that the mixture has a ratio of cellulose carbamate:NaOH of 6-10%:5-10% by weight, such as 6-8%:7-10% by weight, or 8-10%:5-7% by weight.
11. 10. The method according to claim 9, wherein the residence time of the mixture in the mixing zone of the mixing kneader is adapted to the temperature of the mixture in the mixing zone, in particular the residence time is about 1 min to 10 h, for example 2 min to 2 h, in particular 2 min to 60 min or 4 min to 30 min.
12. 10. A method according to any of the preceding claims, characterised in that the temperature of the mixture is maintained at the target temperature for a period of from 1 to 60 minutes, such as from 5 to 30 minutes.
13. adding zinc oxide to the mixture; 10. The method according to any of the preceding claims, characterized in that the mixture of cellulose carbamate solutions preferably has a zinc oxide content of 0.1 to 1.5% by weight.
14. 10. The method according to any of the preceding claims, characterized in that the mixture of cellulose carbamate has a ratio of cellulose carbamate:ZnO of 6-10%:0.1-1.5%.
15. Cellulose carbamate is Providing a pulp; adding an aqueous solution of urea and optionally hydrogen peroxide to the pulp to provide a mixture; mechanically processing the mixture to provide a homogenous composition; heating the composition to a temperature in the range of 120° C. to 155° C. and mixing for 2 to 4 hours, typically at a temperature of 135° C., to produce a cellulose carbamate; recovering the cellulose carbamate; and optionally washing the cellulose carbamate with water and drying in a dryer at a temperature of 155° C. or less, preferably 135° C. or less, and suitably 133° C. or less; 2. The method according to any of the preceding claims, characterized in that it is produced by a process comprising: