High temperature superconductor field coil

JP2024503776A5Active Publication Date: 2024-10-25TOKAMAK ENERGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023523607
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-20
Filing Date
2021-10-20
Publication Date
2024-10-25
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

Existing HTS field coils are prone to rapid quenching and damage due to hot spots, which can be caused by excessive current, thermal stress, or radiation, leading to inefficient energy dissipation and potential destruction of the magnet.

Method used

Incorporating a layer of insulating material with temperature-dependent resistivity and conductive paths between turns, such as europium dicarbide or magnetoresistive materials, to rapidly increase resistance and divert current away from hot spots, allowing for controlled energy dissipation.

Benefits of technology

The solution effectively reduces the risk of coil damage by quickly dissipating energy and preventing excessive heating, enabling safer operation and more efficient energy management in large HTS magnets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A high temperature superconductor (HTS) field coil having turns including an HTS material wound about an axis of the coil, the turns being separated from one another along a direction perpendicular to the axis by a layer of insulating material having a first resistivity at a temperature below an onset temperature of the HTS material and a second lower resistivity at a second temperature above an onset temperature of the HTS material. The HTS field coil further includes one or more conductive elements arranged to provide one or more conductive paths extending through the layer of insulating material from one turn to an adjacent turn. In response to a voltage difference developed across the one or more conductive paths, a current is driven through the one or more conductive elements to heat the layer of insulating material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to high temperature superconductor (HTS) field coils. [Background technology]

[0002] Fusion power generation is an incredibly complex challenge, and although many alternative devices have been proposed, none have yet produced results comparable to the best currently operating tokamaks, such as JET.

[0003] Global fusion research has entered a new phase after the start of construction of ITER, the largest and most expensive (15 billion euros) tokamak ever built. A successful route to a commercial fusion reactor requires long-pulse, stable operation combined with the high efficiency needed to make power production economical. Achieving these three conditions simultaneously is particularly difficult, and the planned program will require many years of theoretical and technological research as well as experimental studies on ITER and other fusion facilities. It is widely expected that a commercial fusion reactor developed along this route will not be built before 2050.

[0004] To obtain the fusion reaction necessary for economical electricity generation (i.e., power output much greater than power input), conventional tokamaks must be massive (as exemplified by ITER) so that the energy confinement time (roughly proportional to the plasma volume) is long enough for the plasma to become hot enough for thermal melting to occur.

[0005] US Patent No. 5,399,633 describes an alternative approach involving the use of compact spherical tokamaks for use as neutron or energy sources. The low aspect ratio plasma shape in spherical tokamaks improves particle confinement times and allows for net power generation in very small machines. However, a small diameter central column is required, which presents a challenge for the design of plasma confinement magnets. High temperature superconductor (HTS) field coils are a promising technology for such magnets.

[0006] Superconducting materials are usually classified as "high temperature superconductors" (HTS) and "low temperature superconductors" (LTS). LTS materials, such as Nb and NbTi, are metals or metal alloys whose superconductivity can be explained by the BCS theory. All low temperature superconductors have a critical temperature below about 30 K (the temperature above which the material cannot become superconducting, even in zero magnetic field). In contrast, the behavior of HTS materials is not explained by the BCS theory, and such materials may have critical temperatures above about 30 K (although it should be noted that it is not the critical temperature that defines HTS and LTS materials, but rather the physical differences in composition and superconducting behavior). The most commonly used HTS are "copper oxide superconductors", which are ceramics based on copper oxides (compounds containing a copper oxide group), such as BSCCO or ReBCO (Re is a rare earth element, usually Y or Gd). Other HTS materials are iron pnictides (e.g., FeAs and FeSe) and magnesium diboride (MgB 2 ).

[0007] ReBCO is typically manufactured as a tape with a structure as shown in Figure 1. Such a tape 100 is typically about 100 microns (micrometers) thick and includes a substrate 101 (usually electropolished Hastelloy about 50 microns (micrometers) thick) on top of which is deposited by ion beam assisted deposition (IBAD), magnetron sputtering, or other suitable technique a series of buffer layers about 0.2 microns (micrometers) thick, known as a buffer stack 102. An epitaxial ReBCO-HTS layer 103 (deposited by MOCVD or other suitable technique) covers the buffer stack and is typically 1 micron (micrometers) thick. A 1-2 micron (micrometer) silver layer 104 is deposited on the HTS layers by sputtering or other suitable technique, and a copper layer 105 is deposited on the tape by electroplating or other suitable technique, often completely encapsulating the tape.

[0008] The substrate 101 provides a mechanical backbone that can be fed through a manufacturing line and allows the growth of subsequent layers. The buffer stack 102 provides a biaxially oriented crystalline template on which to grow the HTS layers, preventing chemical diffusion of elements from the substrate into the HTS that would impair its superconducting properties. The silver layer 104 provides a low resistance interface from the ReBCO to the stabilization layer, and the stabilization layer 105 provides an alternative current path in case any portion of the ReBCO becomes non-superconducting (becomes "normal").

[0009] Additionally, a "peeled-off" HTS tape can be fabricated that lacks the substrate and buffer stack, but instead has a silver layer on either side of the HTS layer. The tape with the substrate is referred to as a "substrate-attached" HTS tape.

[0010] HTS tapes can be arranged in HTS cables. HTS cables contain one or more HTS tapes, connected along their length by a conductive material (usually copper). HTS tapes can be stacked (i.e. arranged so that the HTS layers are parallel) or have other tape arrangements that vary along the length of the cable. Notable special cases of HTS cables are single HTS tapes and HTS pairs. HTS pairs contain a pair of HTS tapes arranged so that the HTS layers are parallel. When substrated tapes are used, the HTS pairs can be type 0 (HTS layers facing each other), type 1 (HTS layer of one tape facing the substrate of the other tape), or type 2 (substrates facing each other). Cables containing three or more tapes can have some or all of the tapes arranged in HTS pairs. Stacked HTS tapes can contain various arrangements of HTS pairs, most commonly either a stack of type 1 pairs or a stack of type 0 pairs (or equivalently type 2 pairs). HTS cables can also have a mixture of substrate and release tapes.

[0011] The following terminology is used in describing coils herein:

[0012] "HTS Cable" - a cable containing one or more HTS tapes. For purposes of this definition, a standalone HTS tape is an HTS cable. · "Turn" - The portion of the HTS cable within the coil that encircles the inside of the coil (i.e., can be modeled as a complete loop). · "Arc" - A continuous length of coil that is less than the entire field coil. · "Inner / Outer Radius" - the distance from the center of the coil to the inner / outer side of the HTS cable. · "Inner / Outer Circumference" - The distance measured around the inner / outer circumference of the coil. · "Thickness" - the radial depth of all turns of the coil, i.e. the difference between the inner and outer radii. "Critical current" - the current at which the HTS becomes normally conductive at a given temperature and external magnetic field. In this case, the HTS is the current at which the tape becomes non-conductive. 0 The transition point at which the superconducting transition occurs is considered to be "normal". 0 The choice of is somewhat arbitrary, but is typically set to 10 or 100 microvolts per meter. "Critical temperature" - the temperature T at which the HTS becomes normally conductive at a given magnetic field and current. c (Strictly speaking, the term "critical temperature" is formally defined relative to zero magnetic field, but for convenience we use the term more generally here). · "Peak Critical Temperature" - The temperature at which the HTS becomes normally conducting in the absence of an external magnetic field and with negligible current.

[0013] The onset temperature of an HTS material refers to the temperature at which the HTS material becomes normally conductive (i.e., is no longer considered a superconductor) and generates a significant voltage. In particular, the onset temperature is the temperature at which the transport current I 0 The critical electric field E 0 (V / m) is the temperature at which the current occurs. As mentioned above, E 0 is the chosen threshold and the critical electric field E 0 When I 0 =I c So, the critical current I cThe onset temperature is therefore determined by many factors that affect the critical current, including the local magnetic field strength (B) and the angle (θ) that the magnetic field makes with the c-axis of the HTS material. The onset temperature is also determined by the n-value of the HTS superconductor, which characterizes how abrupt the transition from superconducting to normal conducting behavior is. When the current reaches the critical current (I c ) and a magnetic field strength of about 20 T, a typical onset temperature of about 35 K is observed for the ReBCO material in the HTS field coil 200.

[0014] Superconducting magnets are formed by arranging HTS cable into a coil, either by winding HTS cable (or individual HTS tapes, which for the purposes of this description can be treated as a single tape cable), or by providing multiple sections of coils made from HTS cable and joining them together. There are three main classes of HTS coils:

[0015] Insulation, having electrically insulating material between the turns (so that current can only flow in a “helical path” through the HTS cable). Non-insulated, where the turns are connected radially as well as along the cable (e.g. by connecting the copper stabilization layer in HTS cables). Partial insulation, where the turns are radially connected with a controlled resistance, either by using a material with a high resistivity (compared to copper, for example) or by providing intermittent insulation between the coils.

[0016] A non-insulated coil can also be considered as a low resistance case of a partially insulated coil. Partially insulated field coils are described in US Pat. No. 5,393,366.

[0017] HTS field coils are typically designed so that all HTS tapes operate below the local critical current Ic in all turns, and the local critical current I c varies around the coil due to the non-uniform magnetic field B and the coil temperature T. However, various fault conditions can cause the current in the HTS tape to exceed the critical current.

[0018] · Increase T (locally or globally) and thereby I c Reduces cooling failure. ·Transport current I 0 A temporary increase in current, for example due to an overcurrent fault in a power supply. Damage to HTS materials (e.g. due to stress cracking, fatigue due to thermal or current cycling in magnets, or radiation-induced degradation such as may be caused by neutron bombardment or runaway electrons in fusion devices). A localized energy deposition sufficient to cause thermal runaway. This "minimum quench energy" is on the order of 10 J, and disruption of the plasma can release this amount of energy into the HTS magnets, either inductively or via radiation (e.g. runaway electrons).

[0019] If the current in one of the tapes exceeds the critical current I c When the HTS material layer exceeds this value, a voltage can be generated in the HTS material layer, causing some of the current to be transported to the metal layers of the tape (mainly the copper layers, which have a much lower resistance than the Hastelloy substrate). The current is then transported through the "spare I" of the other tape in that turn. c The current flowing between the tapes through the layer of "normally conducting" (i.e. resistive) conductor generates heat and the local critical current I c Eventually, all of the tapes in the affected turn of the HTS field coil near the original defect become normally conducting within a timescale typically measured in milliseconds to seconds, depending on the material mix and geometry of the laminated tape cable.

[0020] The area of ​​the HTS tape that is first affected by a fault condition is known as the "hot spot". Early detection of the hot spot is important so that damage to the HTS magnet can be avoided by "quenching" the magnet and dissipating its energy. Various approaches to detect hot spots are known, for example using temperature sensors, strain sensors, or voltage taps. For example, a network of sensors and voltage taps distributed around the coil can be used to detect and pinpoint the location of hot spots that could lead to harmful thermal runaway and quenching. The amount of energy stored in an HTS magnet during operation depends on the size and shape of the magnet and is proportional to the integral of the square of the magnetic flux over the volume of the magnet. Large HTS magnets can store large amounts of magnetic energy that must be safely and quickly dissipated in the event of a quench.

[0021] US Patent No. 5,399,633 describes a superconducting coil that includes a metal-insulator transition (MIT) material layer interposed between the turns of the coil. The resistivity of the MIT material is significantly reduced above the transition temperature. When a current is applied to the superconducting coil, the formation of a resistive "hot spot" (i.e., a normal conducting zone) in one of the turns can cause localized heating of the MIT material layer that raises its temperature above the transition temperature, thereby lowering the resistance of the MIT material layer and allowing the current in the coil to flow through the MIT material layer to the adjacent turn, bypassing the normal conducting zone and slowing the rate of its temperature rise.

[0022] One problem with the superconducting coil described in US Pat. No. 6,399,663 is that the electrical resistivity of the MIT material layer does not decrease quickly enough to avoid damage to the coil and / or to prevent runaway heating in the coil, which may lead to a quench. Another problem with existing HTS coil designs is that there is a trade-off between the turn-to-turn resistance of the coil being low enough to allow rapid lateral (radial) propagation of hot spots, or being high enough to allow the coil to be energized / de-energized quickly, i.e., high enough so that the coil's time constant L / R is small (where L and R are the coil's inductance and resistance). The need for a small time constant is particularly important for large, high-inductance coils. [Prior art documents] [Patent documents]

[0023] [Patent Document 1] International Publication No. 2013 / 030554 [Patent Document 2] International Publication No. 2019 / 150123 [Patent Document 3] International Publication No. 2017 / 039299 Summary of the Invention [Problem to be solved by the invention]

[0024] It is an object of the present invention to provide an HTS field coil that addresses or at least mitigates the above problems. [Means for solving the problem]

[0025] According to a first aspect of the invention, there is provided a high temperature superconductor (HTS) field coil having turns including an HTS material wound around an axis of the coil. The turns are separated from one another along a direction perpendicular to the axis by a layer of insulating material having a first resistivity at a temperature below an onset temperature of the HTS material and a second lower resistivity at a second temperature above an onset temperature of the HTS material. The HTS field coil further includes one or more conductor elements arranged to provide one or more conductive paths extending through the layer of insulating material from one turn to an adjacent turn. In response to a voltage difference developed across the one or more conductive paths, a current is driven (i.e., flows) through the one or more conductor elements to heat the layer of insulating material. The voltage difference may be generated, for example, by one or more "hot spots" forming (or beginning to form) in the HTS material.

[0026] Rapid heating of the conductive elements by the radial current increases the temperature of the insulating material near the conductive elements, causing a rapid decrease in turn-to-turn resistance of at least a portion of the coil (e.g., the insulation) adjacent the hot spot. A radial current is then driven through the insulating material, causing the HTS material in the turns to become normally conducting.

[0027] The second resistivity of the insulator material may be less than 0.1 of the first resistivity, preferably less than 0.01 of the first resistivity.

[0028] The insulator material can have a first metallic phase below a phase transition temperature and a second insulating or semiconducting phase above the phase transition temperature, which can be below an onset temperature of the HTS material such that the insulator material is in the second insulating or semiconducting phase when the HTS field coil is operated.

[0029] Alternatively, the insulator material can have a first insulating or semiconducting phase below a phase transition temperature and a second metallic phase above the phase transition temperature, the phase transition temperature being greater than the onset temperature of the HTS material. The insulator material can be a magnetoresistive material that has an electrical resistivity that decreases in response to an applied magnetic field below the onset temperature of the HTS material, whereby the electrical resistance between the turns along a direction perpendicular to the axis decreases when a current is applied to the coil.

[0030] The insulator material can be or can include europium dicarbide, which can be non-stoichiometric with an atomic ratio of europium to carbon of 1:2.0 to 1:2.6.

[0031] The insulator material can be or can include vanadium oxide.

[0032] The one or more electrical conductor elements may each comprise a metal or alloy, which may preferably comprise one or more of copper, brass, steel, stainless steel, Hastelloy, and nickel.

[0033] The one or more conductive elements may each include a semiconductor.

[0034] The or each conductor element may extend through the layer of insulating material from one turn to an adjacent turn.

[0035] The or each conductor element may include a conductive layer on which a layer of insulating material is provided, the layer of insulating material including one or more windows through which electrical contact can be made to one of the turns, i.e. the conductor element may further include a portion within the window.

[0036] The conductive layer is provided between the layer of insulating material and the layer of other insulating material, the layer of other insulating material including one or more windows through which electrical contact can be made to adjacent turns. The or each window in the layer of other insulating material can be offset from the or each window in the layer of insulating material, and the or each conductive element can include a portion within the window.

[0037] Thus, the or each conductive path may include a number of conductive elements provided within a layer of insulating material.

[0038] Instead of, or in addition to, a window, a plurality of conductive elements may be provided dispersed within the insulating material.

[0039] The electrical resistivity of the or each conductor element may be less than the first resistivity of the insulator material at the generation temperature of the HTS material.

[0040] At least a portion of the, or each, conductive path within the layer of insulating material may have a component (portion) that extends in a direction perpendicular to the radius of the axis of the coil. The conductive path may meander within the layer of insulating material.

[0041] The HTS material can be ReBCO.

[0042] The first temperature can be 25K or less and the second temperature can be 40K or more.

[0043] The onset temperature of the HTS material can be the onset temperature of the HTS material at zero applied magnetic field.

[0044] The turns of the HTS material provide a primary coil and may further include a secondary coil inductively coupled to the primary coil with a flux coupling coefficient greater than 0.5, preferably greater than 0.9.

[0045] The HTS field coils can have dimensions greater than 50 cm, greater than 2 m, or greater than 5 m.

[0046] According to a second aspect of the present invention there is provided a cable for carrying current to a coil of a magnet, the cable comprising: a high temperature superconductor (HTS) layer of HTS material extending along the length of the cable; a layer of insulating material extending along the length of the cable and parallel to the HTS layer, the insulating material having a first resistivity at a temperature below an onset temperature of the HTS material and a second, lower resistivity at a second temperature above the onset temperature of the HTS material; one or more conductive elements arranged to provide one or more conductive paths through the layer of insulating material from a side of the layer of insulating material in electrical contact with the HTS material to an opposite side of the layer of insulating material; Includes.

[0047] According to a third aspect of the present invention there is provided an insulation tape for co-winding with a high temperature superconductor (HTS) tape comprising an HTS material to produce an HTS field coil according to the first aspect of the present invention, comprising: a layer of insulator material having a first resistivity at a temperature below an onset temperature of the HTS material and a second, lower resistivity at a second temperature above an onset temperature of the HTS material; one or more conductive elements arranged to provide one or more conductive paths through the layer of insulating material from one side of the layer of insulating material to an opposite side of the insulating material; An insulation tape is provided that includes

[0048] In response to a voltage differential developed across one or more conductive paths, a current is driven through one or more conductive elements, heating the layer of insulating material.

[0049] According to a fourth aspect of the invention, there is provided a high temperature superconductor (HTS) field coil having turns comprising an HTS material wound about an axis of the coil. The turns are separated from one another along a direction perpendicular to the axis by one or more layers comprising a magnetoresistive material. The magnetoresistive material has an electrical resistivity that decreases in response to an applied magnetic field at a temperature below a generating temperature of the HTS material, such that the electrical resistance between the turns along a direction perpendicular to the axis decreases when a current is supplied to the coil.

[0050] The term magnetoresistance refers to the change in resistance of a (magnetoresistance) material in response to an applied magnetic field. It can be quantified by the relative change in the resistance (or resistivity) of the material as a function of the applied magnetic field. For example, the magnetoresistance of a material can be expressed as ((ρ(B)-ρ(0)))(ρ(0)), where ρ(B) is the resistivity of the material in an applied magnetic field B (e.g., 1 T) and ρ(0) is the resistivity of the material in zero applied magnetic field. The term giant magnetoresistance (CMR) is used herein to describe the magnetoresistance of a material that exhibits unconventional large (or extreme) magnetoresistance, e.g., an absolute change in electrical resistivity of more than 5% in an applied magnetic field of 1 T.

[0051] The relative decrease in electrical resistivity of the magnetoresistive material at said temperature in response to an applied magnetic field of 1 T may be greater than 5%, greater than 50%, more preferably greater than 99%.

[0052] The electrical resistivity of a magnetoresistive material at a temperature of 20K is 10 3 Greater than 10 Ohm cm 4 Greater than ohm cm, more preferably 10 5 It can be greater than ohm cm.

[0053] The magnetoresistive material is europium dicarbide (EuC). 2 or europium dicarbide EuC 2 The europium dicarbide can be non-stoichiometric, with an atomic ratio of europium to carbon of 1:2.0 to 1:2.6.

[0054] The HTS material can be ReBCO.

[0055] The magnetoresistive material can have a first resistivity at a temperature below an onset temperature of the HTS material and a lower resistivity at a second temperature above an onset temperature of the HTS material.

[0056] The magnetoresistive material has a first metallic phase below a phase transition temperature and a second insulating or semiconducting phase above the phase transition temperature, and the phase transition temperature can be below the onset temperature of the HTS material such that the insulating material is in the second insulating or semiconducting phase when the HTS field coil is operated. The temperature above the phase transition temperature at which the magnetoresistive material has a decreasing electrical resistivity in response to an applied magnetic field.

[0057] The onset temperature of an HTS material refers to the temperature at which the HTS material begins to generate a large voltage by becoming normally conducting (i.e., no longer completely superconducting).

[0058] The turns may be formed from one or more lengths of HTS tape that include the HTS material as a layer on a flexible substrate.

[0059] Each layer containing magnetoresistive material may be provided on a flexible substrate that is co-wound with one or more lengths of HTS tape around the axis of the coil.

[0060] Each layer containing magnetoresistive material can have a thickness of from 5 microns (micrometers) to 100 microns (micrometers).

[0061] According to a fifth aspect of the invention, there is provided a high temperature superconductor (HTS) cable for winding into an HTS field coil. The cable has a stack of layers including a flexible substrate, a layer of HTS material, and a layer of magnetoresistive material (e.g. europium dicarbide) as described above for the fourth aspect. The magnetoresistive material has an electrical resistivity that decreases in response to an applied magnetic field at a temperature below the onset temperature of the HTS material.

[0062] According to a sixth aspect of the present invention there is provided an electromagnet including one or more HTS field coils according to the first or fourth aspects.

[0063] According to a seventh aspect of the present invention, there is provided a system comprising a plasma vessel and a set of field coils for generating a magnetic field within the plasma vessel, each field coil being an HTS field coil according to the first or fourth aspect of the present invention.

[0064] According to an eighth aspect of the present invention there is provided a Tokamak fusion reactor comprising an HTS field coil according to the first or fourth aspect of the present invention, the HTS field coil being either a toroidal field coil or a poloidal field coil.

[0065] According to a ninth aspect of the present invention, there is provided a high temperature superconductor (HTS) magnet system comprising: A high temperature superconductor (HTS) field coil according to the first or fourth aspect of the present invention; a detection unit configured to detect loss of superconductivity in the HTS material of at least a portion of one turn of the HTS field coil; a quench protection unit configured to shift current from the HTS field coil to an external resistive load in response to said detection; An HTS magnet system is provided that includes:

[0066] The HTS field coil can have a radius greater than 50 cm.

[0067] The external resistive load can be a varistor (ie, a resistor whose resistance depends on the applied voltage).

[0068] According to a tenth aspect of the present invention there is provided a method of protecting a high temperature superconductor (HTS) field coil according to the first or fourth aspects of the present invention from damage following loss of superconductivity in one or more turns of the HTS field coil, the method comprising: detecting a loss of superconductivity in the HTS material of at least one turn of the HTS field coil; electrically connecting the HTS field coil to an external resistive load in response to said detecting. Includes.

[0069] According to an eleventh aspect of the present invention, there is provided an HTS magnet system including a high temperature superconductor (HTS) field coil, the HTS field coil including a plurality of turns including an HTS material wound around an axis of the coil, the turns being separated from one another along a direction perpendicular to the axis by a layer of insulating material, and one or more conductive elements arranged to provide respective conductive paths extending through the layer of insulating material from one turn to an adjacent turn. The HTS magnet system includes a quench protection circuit including a varistor connected across at least some of the turns of the HTS field coil. The varistor is configured to have a decreasing resistance in response to a voltage developed across at least some of the turns, whereby a proportion of the current driven by the voltage through the one or more conductive elements decreases as the voltage increases, relative to the current through the varistor.

[0070] The HTS magnet system may further include a secondary coil inductively coupled to the HTS field coil, preferably with a flux coupling coefficient greater than 0.5, more preferably greater than 0.9.

[0071] The resistance of the varistor at zero applied voltage can be greater than the resistance of each of the one or more conductive elements at the generating temperature of the HTS material.

[0072] The HTS field coil may be an HTS field coil according to the first aspect of the invention described above.

[0073] The quench protection circuit may further include a power source for supplying current to the HTS field coil, a detection unit configured to detect loss of superconductivity in the HTS material of at least a portion of a turn of the HTS field coil, and a circuit breaker configured to disconnect the power source from the HTS field coil in response to the detection unit detecting loss of superconductivity in the HTS material of at least a portion of a turn of the HTS field coil.

[0074] Also described herein is an HTS field coil having turns comprising an HTS material wound about an axis of the coil, the turns separated from one another along a direction perpendicular to the axis by one or more layers comprising a material having a first metallic phase below a phase transition temperature and a second insulating or semiconducting phase above a phase transition temperature, the phase transition temperature being below an onset temperature of the HTS material.

[0075] Also described herein is an HTS field coil having turns including an HTS material wound about an axis of the coil, the turns being separated from one another along a direction perpendicular to the axis by one or more layers including europium dicarbide. [Brief description of the drawings]

[0076] [Figure 1] FIG. 1 is a schematic diagram of a known HTS tape. [Diagram 2] 2 is a schematic radial cross-sectional view of a coil according to an embodiment of the present invention; [Diagram 3] FIG. 3A is a schematic diagram of an insulation tape according to one embodiment of the present invention.

[0077] FIG. 3B is a schematic side view of the insulation tape of FIG. 3A. [Figure 4] 4 is a schematic radial cross-sectional view of a coil according to another embodiment of the present invention; [Diagram 5] 1 is a schematic cross-sectional view of a Tokamak fusion reactor. [Figure 6]13 is a graph showing calculations of energy in a toroidal field coil during dumping of magnetic energy into an external resistance. [Figure 7] 1 is a graph showing the calculated temperature of the HTS and insulating tape during the dumping of magnetic energy to an external resistor. [Figure 8] FIG. 1 is a circuit diagram of a quench protection system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0078] Partial insulation by conductive elements Proposed herein is a field coil in which adjacent turns of the HTS field coil are separated from one another by a "partial insulation" layer having a conductivity that can rapidly increase as a result of current flowing between the turns during or after the formation of a hot spot. The partial insulation layer includes a layer of insulating material and a conductor element that provides a conductive path through the layer of insulating material. When a hot spot forms in one of the turns of the coil, current will at least to some extent bypass the affected turn, thereby allowing current to flow from that turn to an adjacent turn (or turns) through the conductor element. The insulating material is selected to have a first resistivity at a temperature below the onset temperature of the HTS material and a second, lower resistivity at a second temperature above the onset temperature of the HTS material. Resistive heating of the conductor element increases the temperature of the surrounding insulating material, thereby decreasing the inter-turn resistance of the coil.

[0079] FIG. 2 shows a radial cross-section of a coil 200 formed by winding an HTS tape 100 (in this case a ReBCO tape) around an axis Z (axis of the coil) in a manner similar to a spool of ribbon. For clarity, only two turns 201A, 201B are shown in the figure, but any number of turns can be used. The turns 201A, 201B nest within each other to form a generally planar coil 200, often referred to as a "pancake" coil. The HTS tape 100 can be an HTS tape (or a peeled version thereof) as described above with respect to FIG. 1. The inner circumference of the coil 200 is circular, but can generally be any two-dimensional shape, for example, a "D" shape.

[0080] Insulation tape 203 is co-wound with the HTS tape such that each turn 201A, 201B of the HTS tape 100 is radially (i.e., perpendicular to and through axis Z) separated from one another by a turn of insulator tape 203. Insulation tape 203 has a width (i.e., length along the Z axis) substantially equal to the width of the HTS tape (12 mm in this case). Insulation tape 203 includes an insulating material 207 that electrically insulates turns 201A, 201B from one another when the coil is operating under normal cold conditions (i.e., without hot spots). In this example, the insulating material is europium dicarbide (EuC 2 ), but other suitable insulator materials may be used in addition to or in place of europium dicarbide. For example, the insulator material may be of various stoichiometries (e.g., V 2 O 3 , V 3 O 5 , V 2n O 2n+1 …VO). Other insulating materials that can be used depending on the requirements include semiconductors such as germanium, or Fe 3 O 4 , RNiO 3 (R=La, Sm, Nd, Pr), La 1-x Sr x NiO4, NiSe 1-x Sex , BaVS 3 Alternatively or additionally, carbides, oxides, or nitrides of other transition metals or rare earth elements may be suitable insulator materials in some cases.

[0081] Europium dicarbide is a preferred insulator material because it has high electrical resistivity at low temperatures, but very low resistivity at high temperatures. In particular, europium dicarbide has a first resistivity at a temperature below the onset temperature of the HTS material (ReBCO) and a very low resistivity at a second temperature above the onset temperature of the HTS material (the first resistivity and second resistivity are relative to europium dicarbide 207 at a constant applied magnetic field, e.g., zero applied magnetic field). For example, the electrical resistivity of europium dicarbide (measured at zero magnetic field) is about 10 at a temperature of 15 K. 7 It has a maximum electrical resistivity of 1 Ohm-cm (or less for non-zero magnetic fields), but is less than about 1 Ohm-cm at a temperature of 300 K. This behavior allows the EuC coil to be used when operated at low temperatures (e.g., below 40 K). 2 207 can electrically insulate the turns 201A, 201B from each other, i.e., EuC 2 207 substantially prevents current from flowing radially between the turns, so that most (e.g., >95%) of the current flows circumferentially around the turns. At higher temperatures, EuC 2 207 provides a substantially lower resistance between turns 201A, 201B, thereby allowing a larger current to flow radially between the turns when there is a loss of superconductivity (and therefore an increase in electrical resistance) in the HTS material layer 103.

[0082] The insulator tape 203 further includes copper bridges 205A-205C passing through the europium dicarbide 207 in a radial direction relative to the coil axis Z to electrically connect the turns 201A, 201B. The copper bridges 205A-205C may extend lengthwise and uninterrupted within the insulator tape so as to be circumferentially disposed around each turn of the insulator tape 203, i.e., to span at least 360 degrees around the coil axis Z. Alternatively, the copper bridges 205A-205C may extend only a short distance in the circumferential direction, i.e., each copper bridge 205A-205C fills a respective window (through hole) in the insulator material 207, and there may be circumferentially spaced copper bridges 205A-205C. In the latter case, there may be radial cross sections that do not include copper bridges (i.e., the insulator material 207 extends uninterruptedly from the top to the bottom of the field coil in these radial cross sections). Although only three copper bridges are visible in the radial cross section shown in Figure 2, it will be understood that any number of bridges may be present in such a cross section. Thus, the insulator tape 203 as a whole functions as a "partial" insulator at low temperatures due to the relatively high resistivity of the europium dicarbide 207 along with the relatively high electrical conductivity of the copper bridges 205A-205C.

[0083] If a hot spot forms in the HTS material layer 103 of one of the turns 201A, 201B, at least a portion of the current flowing through the affected turn bypasses the hot spot and is transferred to the adjacent turn through the copper bridges 205A-205C as a result of the voltage developed between the turns, i.e., the copper bridges 205A-205C transfer the current radially between the turns 201A, 201B. The copper bridges 205A-205C are rapidly heated by the radial current, which increases the temperature of the europium dicarbide 207 surrounding the copper bridges 205A-205C and rapidly reduces the inter-turn resistance of at least a portion of the coil 200 adjacent the hot spot. The magnetic energy stored in the coil 200 then drives a radial current through the insulator material, rapidly turning the HTS material of the turns 207A, 207B normally conductive. This process then continues until the HTS material becomes normally conductive for the majority of the coil.

[0084] Due to the significant reduction in resistivity of europium dicarbide 207 following heating by copper bridges 205A-205C, at least a portion of the radial inter-turn current flows instead through europium dicarbide 207. That is, the current flowing through copper bridges 205A-205C is reduced compared to the current that would flow if the resistivity of europium dicarbide 207 remained very high. This reduction significantly reduces or eliminates the risk that copper bridges 205A-205C (or other portions of coil 200) will be damaged or "burned out" by very large currents flowing through the resistive material of copper bridges 205A-205C.

[0085] Limiting the current through the copper bridges 205A-205C is particularly important to avoid excessive heating because the resistance of the copper bridges 205A-205C increases with temperature (e.g., by a factor of about 15 between 20K and 200K). These concerns are most critical for very large coils that can store enormous amounts of magnetic energy, e.g., the Tokamak TF coil, which has a height of about 6 m, capable of storing about 1.5 GJ of magnetic energy. Some of the issues for larger coils can be understood by considering how the coil properties change as the coil's characteristic linear dimension (e.g., radius) increases. The stored magnetic energy rises as the cube of the linear dimension, but the mass of the coil that must absorb that energy rises only linearly or squared with the coil dimension. It is therefore important to ensure that the heat during a quench is distributed evenly throughout the coil.

[0086] The combination of europium dicarbide 207 and copper bridges 205A-205C significantly increases the speed at which the insulator tape 203 can respond to localized heating caused by the formation (or initiation) of hot spots. That is, the speed at which the resistance of the insulator tape 203 decreases is increased by the copper bridges 205A-205C heating the europium dicarbide 207. For existing forms of temperature-dependent inter-turn insulation without the copper bridges, more heat must be generated by the current flowing in the cladding (e.g., silver layer 104 or copper layer 105) of the HTS tape 100 before the insulation heats up sufficiently to cause a significant decrease in the coil's inter-turn resistance. Such localized and relatively long-term heating can lead to increased damage to the HTS tape 100. Another benefit resulting from the improved (i.e., reduced) "response time" of the insulator tape 203 is the reduced time it takes for unbalanced forces to build up between different portions of the HTS field coil 200, which can result in mechanical damage to the HTS magnet.

[0087] The inter-turn resistance of the HTS field coil 200 can be varied in many different ways, such as by varying the number density of the bridges 205A-205C in the insulation tape 203, by varying the thickness of the insulation tape 203, or by using a resistive material other than copper for the bridges, such as brass, stainless steel, Hastelloy, nickel, or a semiconducting material. The bridges can have a substantially constant cross-sectional area along their length (i.e., along the horizontal radial direction shown in FIG. 2) and can take any shape. By increasing (or decreasing) the cross-sectional area of ​​the bridges, the inter-turn resistance can be increased (or decreased) as desired. In some cases, some of the bridges can extend to the ends of the insulation tape 203, i.e., each of these bridges can be free of being surrounded by insulation material on one side.

[0088] The length of the conductive path through the insulator material can also be increased by configuring the bridges 205A-205C to follow a serpentine path within the insulator material (e.g., a winding or "snake" path that folds back on itself one or more times within the insulator material). This type of arrangement allows heat generated at the bridges to be transferred to the insulator material over a larger area compared to a non-tortuous path.

[0089] The metal bridges described above may be varied along the insulator tape 203 to ensure that the turn-to-turn resistance provided by the insulator tape 203 remains (at least approximately) constant for each turn.

[0090] The two coils 200 may be arranged as a "double pancake coil," with one coil 200 stacked on top of the other with a layer of insulation between the two coils 200. The two pancake coils 200 are wound in opposite directions, and the inner terminals of the coils 200 (i.e., the end of the innermost turn of each coil) are connected together such that a current can be supplied to the coils by applying a voltage to their respective outer terminals (i.e., the end of the outermost turn of each coil).

[0091] The insulator tape 203 includes a substrate on which europium dicarbide 207 (or other insulator material) is layered and may include through holes (i.e., windows) that allow the copper bridges 205A-205C to pass through both the substrate and the europium dicarbide 207. The substrate may be formed from or include another thermally conductive material, such as copper, to facilitate heat transfer from the copper bridges 205A-205C to the europium dicarbide 207. The substrate may also be electrically conductive, in which case each of the copper bridges 205A-205C may be in electrical contact with the substrate such that no through holes are required in the substrate. In one embodiment, the substrate is made of Hastelloy and has a thickness of 100 microns (micrometers), while the copper bridges 205A-205C may be made of copper. 2 Layer 207 has a thickness of 20 microns (micrometers). 2 The thickness of layer 207 can be adjusted according to the desired inter-turn resistance, and can be, for example, 1 micron (micrometer) to 100 microns (micrometers). 2 A layer 207 may be provided. 2 Layer 207 can be formed, for example, by reaction of elemental europium with graphite at 1673 K, as described by Wander et al., Inorganic Chemistry (2010) 49, 1, 312-318.

[0092] Alternatively (or additionally), rather than providing the insulator tape 203 separately from the HTS tape 100, 2 The layer 207 and the copper bridges 205A-205C are bonded to one side of the HTS tape 100 or provided on both sides of the HTS tape 100, i.e., EuC 2Layer 207 and copper bridges 205A-205C may be provided. A cable may also be made that includes one or more such tapes and one or more HTS tapes 100 in a stacked arrangement (i.e., arranged so that the HTS layers of each tape are parallel). Such a cable may be particularly useful for manufacturing large field coils.

[0093] Another method of forming the insulator tape 203 includes depositing a mixture of an insulator material (e.g., europium dicarbide) and metal particles (e.g., copper powder) onto a copper layer or substrate such as the HTS tape 100. The metal particles are dispersed within the europium dicarbide to form small conductive "tracks" that provide a conductive path through the europium dicarbide. This method can be easily incorporated into existing methods of manufacturing the HTS tape 100, e.g., REBCO tape. The number density and / or size of the metal particles within the europium dicarbide can be non-uniform such that certain portions of the insulator tape 203 are more conductive. The number density and / or size of the metal particles can also be varied to provide a (substantially) constant turn-to-turn resistance when the insulator tape 203 is wound on the HTS field coil 200.

[0094] 3A and 3B show a metal (e.g., copper) strip 301 (which can be considered a substrate, as discussed above for insulation tape 203) with an insulating material (e.g., EuC) on at least the side that faces the HTS cable when the coil is wound. 23B shows an insulation tape 300 provided with a thin coating of insulating material (insulating film) 302. The insulating coating is removed (or not applied) over windows or "through holes" 303 spaced apart on each side of the metal strip 301. The windows can have any shape and can optionally extend to the ends of the insulation tape 300. The locations of the windows 303 on either side of the metal strip 301 are staggered (i.e., the windows are offset from one another) as shown in FIG. 3B, such that the path 310 for electrical current flowing from one window to another includes a portion that runs parallel to the length of the metal strip 301. This arrangement increases the resistance of the overall insulation tape 300 (compared to an uninsulated strip or a strip with windows directly opposite each other) and causes greater heating of the insulation material coating.

[0095] The metal strips can be soldered to the HTS cable (e.g., during winding) to ensure good electrical contact. Alternatively, contact can be achieved simply by pressure within the coil once wound. As a further alternative, additional conductive inserts can be added to the window, or the metal strips can have protrusions that extend into the window. The inserts or protrusions can fill the entire window, or only a portion of the window. For example, if the window is a "lane," the inserts can be spaced along the lane, so that the inserts can, in effect, reduce the size of the window and be used to tune the turn-to-turn resistance provided by the insulation tape 303.

[0096] Insulation tapes similar to the insulation tape 300 of FIG. 3 can be manufactured as flexible printed circuit boards (PCBs) and include insulation materials (e.g., EuC 2) 302 is bonded to the metal strip with an adhesive, then etched to form windows, and further metal elements are bonded to the insulating coating or metal strip as needed to make electrical contact with the metal strip. Alternatively, a coating of insulator material can have windows pre-cut (or be sized to create "lanes" when applied to the strip) and then bonded to the metal strip with an adhesive during winding. Other manufacturing methods can also be used.

[0097] As mentioned above, HTS coils can be uninsulated, partially insulated, or insulated, depending on the material provided between adjacent turns of HTS material. These different types of HTS coils can behave significantly differently after hot spots form in a portion of the HTS material, and require different approaches to safely and effectively respond to the formation of hot spots.

[0098] In the case of a fully insulated magnet, if a hot spot forms in a part of the HTS tape 100, the current will bypass the normally conducting zone of the HTS material and will preferentially flow through another layer of the HTS tape or HTS cable. For example, in a magnet wound using a laminated tape cable without the addition of so-called "stabilizing" metals (such as copper or aluminum), the transport current will preferentially flow through the copper (if present) and Hastelloy (or nickel-tungsten) substrate of the outer shell of the HTS tape. Joule heating within the other layers of the HTS tape or HTS cable will cause the temperature of the hot spot to rise rapidly, exceeding the melting point of copper, usually within 10-1000 milliseconds, depending on the cable construction and the amount of magnetic energy stored in the magnet. If enough stored magnetic energy is available, the turn will vaporize at its hottest point and a destructive arc will form, irreparably damaging the magnet. This problem is particularly acute with HTS magnets, since they can maintain their superconducting state at high temperatures (generally up to 30-60 K, depending on the magnet design). At these temperatures, most materials have a significantly increased heat capacity compared to the lower temperatures at which conventional low-temperature superconducting (LTS) magnets operate, such as 1.2-4.2 K. This higher heat capacity means that the hot spot typically propagates very slowly (e.g., at speeds of about 10-100 mm / s) around a turn and between adjacent turns, resulting in a large temperature gradient forming between the peak temperature of the hot spot and the surrounding HTS material, which is still superconducting and has no dissipation.

[0099] These problems can be mitigated, for fully insulated magnets, by adding additional highly conductive normal (i.e., non-superconducting) metal (e.g., copper) to the HTS cable to reduce Joule heating and slow the rate of temperature rise, thereby increasing the time to detect a hot spot and initiate a safe shutdown of the magnet. However, larger magnets require significant amounts of additional highly conductive metal to be added to each turn to allow an acceptable time frame to detect a hot spot and initiate a quench. The additional metal significantly reduces the winding pack current density, i.e., the current carried by the cable divided by the cross-sectional area of ​​the cable, but serves no purpose until a hot spot occurs. Furthermore, the metals best suited for this purpose (copper and aluminum) have relatively low Young's moduli, so in many cases the cable must be jacketed with a high-strength material to withstand the high electromagnetic stresses found, further reducing the current density of the HTS cable. These problems can be avoided by using field coils such as field coils 200, 400 described above in which the layers of insulating material between the turns of the HTS tape 100 are relatively thin, for example having a thickness of less than 1 mm or a thickness of 5 microns (micrometers) to 100 microns (micrometers).

[0100] For the central pillar of a compact Spherical Tokamak (ST) Toroidal Field (TF) magnet, the resulting current density is typically <50A / mm 2 and is definitely <100A / mm 2 However, the average current density required for larger STs is much higher. For example, for a ST with a semi-major axis (R 0 ) and R 0 The ST with a magnetic field of 4 T is 400 A / mm 2 This requires an average current density of about 100 Å. Therefore, adding large amounts of additional conductors is not practical for larger STs. Therefore, field coils such as field coil 200 described above (and field coil 400 described below) are particularly well suited for compact spherical tokamaks.

[0101] HTS field coils containing magnetoresistive materials Another solution to some of the above problems is proposed herein, which uses a magnetoresistive material layer to provide inter-turn electrical insulation of the HTS coil. The electrical resistivity of the magnetoresistive material decreases in response to an applied magnetic field at temperatures lower than the generation temperature of the HTS coil. The magnetoresistive material layer provides high electrical resistance between the turns of the HTS coil (i.e., the coil is an "insulated" coil) when the amount of current supplied to the HTS coil (and thus the magnetic field generated by the coil) is small. However, as more current is supplied to the HTS coil, the magnetic field generated by the HTS coil causes the electrical resistance of the magnetoresistive material layer to decrease (and the coil becomes an "uninsulated" or only "partially insulated" coil). This behavior allows current to be supplied to the coil quickly during the initial phase of ramp-up (i.e., when the current increases from a low value to a high value) and then at a slower rate as the inter-turn resistance of the coil decreases to a lower final resistance (and thus the L / R ratio increases). Therefore, the overall ramp-up time of the HTS coil is reduced compared to other HTS coils that have the same turn-to-turn resistance as the final turn-to-turn resistance reached by the HTS coil, but do not contain any magnetoresistive material.

[0102] For example, an HTS coil may have an inductance L and a final inter-turn resistance R to allow current to flow between the turns if, for example, a hot spot forms in the HTS layer 103. 1 Assume that the HTS coil, including the magnetoresistive material layers, has a final turn-to-turn resistance R 1 The initial inter-turn resistance (at zero current) is higher than R 0 Therefore, the average time constant of the HTS coil is L / R 0 and L / R 1 In contrast, the constant inter-turn resistance R 1 A comparable HTS coil with a larger time constant L / R 1Preferably, the magnetoresistive material can exhibit giant magnetoresistance (CMR). For example, the decrease in electrical resistivity of the magnetoresistive material when going from an applied magnetic field of strength 0 T to an applied magnetic field of strength 1 T can exceed 5%.

[0103] 4 shows a radial cross-section of a coil 400 including multiple turns 401A, 401B of HTS tape 100. This coil is identical to coil 200 described above with respect to FIG. 2, except that insulator tape 403 does not include a copper bridge. That is, insulator tape 403 includes a conductive (e.g., copper or Hastelloy) substrate 405 and an insulator material (e.g., europium dicarbide) layer 407.

[0104] Insulating materials are magnetoresistive materials, i.e., materials that exhibit magnetoresistance, a change in electrical resistivity due to the application of an external magnetic field. Europium dicarbide is a preferred choice of magnetoresistive material because it exhibits a very large change in electrical resistivity due to the application of a large magnetic field, the so-called colossal magnetoresistance (CMR). For example, at a temperature of 20 K, europium dicarbide exhibits a large change in electrical resistivity of about 10 7 It has an electrical resistivity of ohm cm, but in a 1 T magnetic field it is about 10 4 It has a low efficiency of 10 to 100 ohm cm in a magnetic field of 14 T.

[0105] The magnetic reluctance of the insulation tape 403 means that current can be supplied to the coil 400 at first quickly and then at a slower rate as the inter-turn resistance of the HTS coil 400 decreases in response to the magnetic field generated by the HTS field coil 400. Also, the very low inter-turn resistance when the HTS coil 400 is operated at high currents (i.e., high magnetic fields) allows for some current sharing between adjacent turns 401A, 401B of the HTS tape, which makes the HTS coil 400 more resistant to hot spot formation, as described below.

[0106] If an area of ​​one turn 401A, 401B of the HTS tape 100 forms a "hot spot," i.e., becomes warmer than the rest of the HTS tape 100, the hot spot can spread around the turn until enough heat is generated that the HTS tape 100 is no longer superconducting, i.e., exceeds the onset temperature of the HTS material 103. However, the insulator tape 403 helps to mitigate this problem because the heat generated at the hot spot causes the insulator tape 403 adjacent to the hot spot (e.g., on either side of the hot spot) to become more conductive, which causes some of the current in the turn 401A, 401B containing the hot spot to bypass the hot spot and move to the adjacent turns 401A, 401B (i.e., current flows radially).

[0107] As discussed above, the magnetic field generated by the current flowing through the HTS coil 100 significantly reduces the resistance of the magnetoresistive layer 407. This reduction in resistance means that only a relatively small temperature increase is required before the electrical resistance of the magnetoresistive layer 407 is low enough for current to move between adjacent turns 401A, 401B during or after hot spot formation. The magnetoresistance of layer 407 thus helps to prevent excessive localized heating before the current is redirected substantially away from the hot spot. This behavior contrasts with the behavior of non-magnetoresistive materials, which may require a relatively large temperature increase before the resistance of the material is low enough for significant current movement to occur between adjacent turns.

[0108] 4, each turn 401A, 401B has a single layer of HTS tape, however, the coil 400 may also be formed from a cable including two or more layers of HTS tape 400 stacked in a face-to-face arrangement such that each turn 401A, 401B includes two or more layers of HTS tape. Preferably, the cable includes HTS tapes arranged such that the HTS layers 103 face each other (i.e., the HTS layers 103 are between each of the Hastelloy layers 101 of the HTS tape 100).

[0109] The resistivity of europium dicarbide is about 10 at 20K. 6 Ohm-cm, approximately 10 at 35K 3 ohm-cm. Therefore, hot spots occurring in the HTS tape are 2 Because the resistance between the turns provided by layer 407 remains relatively high, the hotspot initially tends to spread relatively slowly (e.g., at a speed of about 10 to 50 cm / s) around turns 401A, 401B. This means that the current continues to flow through the turns and the magnetic field generated by coil 400 remains approximately constant at about 20 T. As the temperature of the hotspot increases, the EuC 2 The temperature of layer 407 increases and its resistivity decreases, for example to about 10 ohm cm at about 70 K. 2 The lower resistance of layer 407 allows a significant amount of current to flow radially from the turn 401A, 401B in which the hot spot is formed, through the insulator tape 403, and into one or more adjacent turns 401A, 401B of the HTS tape. Portions of these turns near the hot spot then exceed their critical current and become normally conducting themselves. Thus, the hot spot can expand radially across the coil 200 (i.e., in a direction perpendicular to both the Z-axis and the tangent of one or more turns) before a quench occurs.

[0110] Vanadium oxide (e.g., V 2 O 3In contrast to other metal-insulator transition (MIT) materials such as vanadium oxide, the decrease in the electrical resistivity of europium dicarbide is not limited to a narrow temperature range, but begins at lower temperatures, specifically around 15-25 K, where the best compromise between cooling and conductor costs occurs for REBCO-based magnets. In particular, europium dicarbide has a phase transition temperature of about 15 K, significantly lower than other metal-insulator transition materials, and undergoes a phase transition from a metallic phase below the transition temperature to an insulating or semiconducting phase above the transition temperature. The electrical resistivity of europium dicarbide in this latter phase decreases significantly with increasing temperature, as discussed above. As a result, in europium dicarbide, current leakage between the turns occurs more rapidly after the onset temperature is exceeded (and the HTS material transitions from the superconducting to the normal conducting state). This allows the europium dicarbide layer 407 to have a better "damping" effect on the increase in hot spot temperature than, for example, vanadium oxide. Although the disclosure in this portion of the application focuses on europium dicarbide, other magnetoresistive materials may be used (depending on the temperature at which the HTS material is generated). For example, other carbides, oxides, or nitrides of other rare earth or transition materials may be suitable insulator materials in some cases.

[0111] Quench Protection As mentioned above, partially insulated coils provide a way to reduce the heat generated near hot spots by reducing the resistance of the insulation between the turns, allowing current to bypass the turn with the hot spot by flowing radially to adjacent turns. Thus, when a magnet has partial insulation between the turns, the rate at which the temperature of a local "hot spot" (normally conducting zone) increases is greatly reduced, since current can travel not only between turns but also between tapes within one turn. This reduction provides a much longer time to detect the hot spot and take protective action before a potentially harmful quench occurs.

[0112] If the presence of a local hot spot growing in a non-insulated or partially insulated magnet is detected, the sequence of events is different from that which occurs in a fully insulated coil. The non-insulated option is only applicable to coils with very low inductance. This is because the charging (or ramping) time of the magnet is determined by the ratio of the inductance of the superconducting helical path to the resistive radial path, the L / R time constant. The radial resistance R is determined by the inverse of the magnet dimension (e.g. the length of the turn), but since L varies as the cube of the magnet dimension, L / R varies as the fourth power of the linear magnet dimension. The inductance allows very high transport currents I 0 The hotspot temperature can be reduced by choosing to operate at 100 kA, but this approach has practical limits (around 100 kA) because the current leads connecting the cryogenic coils to the room temperature power supply would become too large (causing unacceptable thermal leakage). For tokamaks, even with very high transport currents, the L / R time constant of a non-insulated TF coil is too long to ramp the magnet in a practical time frame. In practice, a compromise needs to be found between reasonable ramp times (requiring a higher R) and slowing down the rate of rise of the hotspot temperature to allow a reasonable detection window (requiring a lower R). A suitable compromise value for R (which we call R c Finding the critical current (called the critical temperature), requires complex modelling using a thermoelectric network model that takes into account the critical current of each element.

[0113] Shutdown typically involves disconnecting power and redirecting the magnet current through a resistive shunt external to the magnet, absorbing and dissipating the energy stored in the magnetic field. The rate of heating of the hot spot slows down rapidly as the magnet's energy is released to an external dump. Magnet designers must ensure that the peak temperature of the hot spot does not exceed a maximum allowable temperature (usually 100K, with a maximum of 200K chosen) to avoid excessive differential thermal stresses. This usually involves designing a quench protection system that detects the hot spot and activates an energy dump within a certain time frame (usually less than a second for HTS magnets). The stored energy depends on the size and shape of the magnet (proportional to the integral of the square of the magnetic flux over the volume).

[0114] Partial insulation has the added advantage that it can divert current away from the turn containing the hot spot, not just at the location of the hot spot, but at all points around the turn. Once the presence of a hot spot is detected and a magnet dump is initiated, this creates distributed heating around the entire turn, leading to a faster and more distributed propagation of the magnet quench. This occurs when the local magnetic field value, magnetic field angle, or temperature changes at various points around the coil, causing the critical current I c This is especially important for magnets where the I 0 / I c Quenches initiate at the points where the heat is highest and must propagate fast to avoid localized burnout, so the distributed heating around the turns provided by partial insulation is an important feature.

[0115] When the power supply unit (PSU) is disconnected and / or the dump resistor R d The behavior of an uninsulated or partially insulated magnet when replaced by an R is complex. Each turn is connected in series with the next, and is tightly magnetically coupled with all the other turns, resulting in a R tt and forms a shorted loop. Thus, in the simple case of an axisymmetric coil, every point around each turn has a nominally equal I0 / I c If the current of each turn is the inductance of the turn, the current is the tube resistance R tt The current is then returned to the turn via R. The coil thus acts like a series of nested resistive loops with high mutual inductance. tt Each turn is quenched at a slightly different time due to Joule heating caused by the current flowing through it. A normally conducting "shock wave" propagates radially inwards and outwards until the entire coil is quenched. It is important to note that in this mode, the effective inductance of the magnet is greatly reduced. This means that the voltage developed across the coil is also greatly reduced, by a factor roughly equal to 1 / N (where N is the number of turns), compared to a quenched insulated coil of the same dimensions and ampere turns. This behavior provides many very important advantages to superconducting magnets, such as reduced ground wrap breakdown insulation voltage ratings (useful in nuclear devices where neutron exposure reduces the effectiveness of organic insulation).

[0116] A drawback of partial insulation with a nominally constant inter-turn resistance is that when dumping is initiated, it is not possible to channel all of the stored energy in the magnets to the external resistor R. d When connected between the coil terminals, R d appears parallel to the radial resistance R. Therefore, the magnet current flows through R and R d The energy dissipated in R heats up the cold mass of the magnet, while the energy dissipated in R d The energy dissipated in is dissipated outside the magnet. In some cases, a compromise value R is chosen that satisfies all constraints simultaneously. c is difficult to find.

[0117] This problem can be mitigated if the turn-to-turn resistance of the partial insulation, such as that described above for insulation tapes 203, 303, 403, can be made to vary significantly with temperature and / or magnetic field. The surface resistivity between turns, ρ, is simply the radial resistance R divided by the number of turns in the coil multiplied by the area of ​​one turn. A compromise R that is achieved with insulation that is insensitive to temperature and magnetic fields is c The surface resistivity of c Then, the local coil temperature is T <T c When ρ>ρ c , T>T c When ρ<ρ c This arrangement is particularly beneficial when the turns are in a protective dump. This arrangement facilitates current sharing between turns only near the hot spot, achieving the goal of slowing the rate of temperature rise in the hot spot without compromising the magnet's ramping time. It also allows most of the magnet's energy to be dumped into an external resistor rather than being dumped into the magnet, which could overheat during the dump phase. This reduces the overall magnet risk and also reduces the time required to recover from a protective dump (as the magnet has less time to re-cool before re-ramping).

[0118] We now consider the use of HTS field coils, such as HTS field coils 200, 400 described above in connection with Figures 2 and 4 (and the field coil formed using the insulating tape 300 described in connection with Figure 3), in tokamak fusion reactors and plasma chambers, particularly spherical tokamaks. The tokamak has two sets of magnets: poloidal field coils that are generally circular and aligned to generate a poloidal magnetic field, and toroidal field coils that include a central pillar and multiple return limbs and are arranged to generate a toroidal magnetic field. HTS magnets can be used for either set of field coils, but are particularly useful due to the severe space limitations of the toroidal field coils in small tokamaks. The improved current density and / or reduced cooling requirements of HTS greatly aid in such limitations.

[0119] 5 shows a vertical cross section through a spherical tokamak 500 including a toroidal field (TF) coil 501, a poloidal field (PF) coil 503, and a toroidal plasma chamber 505 located within the toroidal field coil 501. The tokamak 500 also includes a central pillar 507 that extends through the center of the plasma chamber 505 and the toroidal field coils 501 and the poloidal field coils 503. Each of the generally D-shaped toroidal field coils 501 includes turns arranged such that each coil 501 has a "straight" portion 509 that extends along the axis A-A' of the central pillar 507, and a curved portion 511 that is electrically connected to both ends of the straight portion 509 to form a D-shaped coil. In practice, the straight portion 509 may be slightly curved, for example, having a radius of curvature that is larger (e.g., two times, five times, or ten times larger) than the radius of curvature of the curved portion 511.

[0120] Conventionally, the toroidal field coils 503 may contain extra copper material (in addition to the copper cladding of the HTS tape 100) to temporarily carry heat generated in the normal zone formed in the HTS tape 100. The thicker the copper layer, the slower the rate of temperature rise in the hot spot (i.e., the portion of the tape containing the normal zone). In the absence of a hot spot, all transport current flows through the superconducting layer and there is no current in the copper layer. The copper layer carries current only for the short period of time that the hot spot forms. If localized cooling is insufficient to stabilize the temperature of the hot spot, thermal runaway occurs and eventually the copper layer melts and an arc forms. The time until this occurs can be extended by making the copper layer thicker, but this has several disadvantages: reduced current density in the HTS cable (a key factor in tokamak size) and reduced composite Young's modulus of the cable due to the relatively very low modulus of elasticity of high purity copper compared to Hastelloy. However, the use of insulation tapes as described above (e.g., insulation tapes 207, 407) allows the thickness of this extra copper material to be reduced or even eliminated altogether. This allows for more compact and higher current density TF coils.

[0121] Considering the TF coil 501, the magnetic energy stored in the TF coil 501 can be several GJ. When a hot spot is detected, in the case of an insulated coil, this energy can be dumped into an external resistor (preferably a varistor) when the power supply unit that powers the insulated TF coil 301 is disconnected. Assuming that the external resistor has a resistance of 0.167 Ohms and a maximum voltage drop across the TF coil 501 of 5 kV, the time constant associated with the removal of energy from the TF coil 501 is about 20 seconds, and the overall damping process can take on the order of 100 seconds. This time scale may be too long to prevent the hot spot from damaging the HTS tape 100.

[0122] 6 is a graph showing the calculated magnetic energy stored in TF coil 501 during a quench. TF coil 501 includes leakage insulation tape 407 and HTS tape 100 as described above for HTS field coil 400, and has the following parameters: Thickness of europium dicarbide layer 407: 20 microns (micrometers) · Thickness of substrate 105: 100 microns (micrometers) Width of the insulation tape 403 (i.e., length along the coil axis): 12mm Turn circumference (length): 16m -Transport current: 30kA Number of HTS tapes: 43 ·HTS tape thickness: 110 microns (micrometers) Current per tape: 700A Stored energy: 1.5GJ Inductance 3.3H

[0123] The graph has a curve 600 showing the decay of the magnet's energy and a curve 602 showing the rise of the energy dissipated in the external resistor over time (in seconds). These curves 600 and 602 are associated with the left vertical axis with units of GJ. Another curve 604 shows the energy dissipated inside the TF coil 501 over time and is associated with the right axis with units of kJ. Most of the energy previously stored in the magnetic field is dissipated in the external resistor over the course of about 20 seconds. The energy dissipated in the TF coil 501 only reaches about 2 kJ at this point.

[0124] 6 is a graph showing the calculated temperature (K) of the HTS tape 100 and the leaky insulator tape 407 in the area of ​​the hot spot (initial length 1 cm) as a function of time (in milliseconds). The temperature of the insulator tape 407 (line 500) rises from about 25 K initially to about 150 K after about 40 ms, while the temperature of the HTS tape 100 (line 502) rises from about 25 K to about 50 K over this time.

[0125] The external resistor is connected from the TF coil 501 to the varistor and magnet cable and EuC 2The external resistance may be a varistor (voltage dependent resistor) that can be changed over time to control the rate of energy dissipated in the insulator (or other insulating material mentioned above). Alternatively or additionally, the external resistor may be initially disconnected from the TF coil 501 and then briefly connected after the hot spot has formed (so that current flows from the TF coil through the external resistor). This provides a way to initially provide a very high (effectively infinite) resistance and then a lower (finite) resistance after the hot spot has formed. More generally, the external resistor may include multiple resistors arranged in parallel with each other, each of which may be connected or disconnected from the other resistors with a respective switch, such that the overall resistance across the multiple resistors may be changed by switching each of the switches. A quench detection system for initiating energy dissipation after detecting loss of superconductivity in at least a portion of the HTS material of one turn of the HTS field coil is described, for example, in WO 2018 / 078327.

[0126] Another method of reducing peak coil temperature, which can be used in combination with using an external resistor (such as a varistor) as described above, is to inductively couple the magnet current to a secondary coil that is tightly inductively (magnetically) coupled to the electromagnetic coil. Such a secondary coil is sometimes called a "closely coupled secondary" (CCS) coil. In this method, the secondary coil is usually a single turn of a normal conducting metal such as copper or aluminum. The two coils act as a transformer. During the time-consuming ramping of the primary coil, current is induced in the secondary coil, but it decays quickly because it is resistive. However, once the primary coil becomes fully (or almost) normal, a current is induced in the secondary coil due to the collapsing magnetic field. The effect is that the current moves (or "jumps") from the primary coil to the secondary coil quickly, reducing the heating of hot spots in the primary coil. This method requires that the flux coupling coefficient k between the primary and secondary coils be very high (>0.9), which means that the coils must be very close together so that most of the magnetic flux generated by the primary coil couples to the secondary coil.

[0127] While this method of protection may be suitable for LTS magnets, where the normal zone propagates quickly, it is generally not suitable for use with insulated HTS coils, where the normal zone propagates very slowly. However, the partially insulated HTS coils 200, 400 described above (and other field coils that include the insulation tape 300 described above) allow the normal zone to propagate very quickly, which makes quench protection with CCS coils much more feasible.

[0128] FIG. 8 illustrates a quench protection circuit 800 for dissipating energy in a superconducting field coil 802 following a loss (or partial loss) of superconductivity in the HTS material of the field coil 802. The field coil 802 includes turns of HTS tape wound around an axis to form a helical path for current to be supplied to the field coil 802. When the coil is in use, a magnetic field is generated by the circulation of current around the helical path of the turns. The field coil 802 is partially insulated, i.e., the turns of the coil are electrically connected radially to one another. This is accomplished by providing the field coil 802 with conductor elements (such as copper bridges 205A-C) or conductive "tracks" that extend through layers of insulating material located between the turns and provide a conductive path from one turn to an adjacent turn. The field coil 802 can be, for example, a field coil 200, 300 as described above in connection with FIGS. 2, 3A, and 3B. When the resistance of the helical path increases as a result of hot spot formation, at least a portion of the current circulating within coil 802 can flow radially to adjacent turns, bypassing the affected portion of the turn.

[0129] The field coil 802 is represented in the circuit diagram by an inductor 802A and a resistor 802B. The current through the inductor 802A corresponds to the current flowing around the helical path provided by the turns of the field coil 802, while the current through the resistor 802B corresponds to the current flowing radially between two or more turns of the field coil 802. If the coil 802 is fully superconducting, the current flows mainly around the helical path of the coil 802. If the coil 802 is no longer superconducting, the resistance of the helical path increases and the current flows preferentially radially between the turns. In this case, the resistance of the resistor 802B in FIG. 8 corresponds, to a first approximation, to the number of turns of the field coil 802 multiplied by the inter-turn or "radial" resistance between adjacent pairs of turns, i.e., the combined resistance of the conductive elements (such as the copper bridges 205A-205C) connecting the adjacent turns.

[0130] The quench protection circuit 800 further includes a power supply 804 that supplies current to the field coil 802. A circuit breaker 806 is provided so that the power supply 804 can be disconnected if a hot spot forms in the field coil 802. The circuit breaker is preferably operated automatically by a quench detection system as described above. A dump resistor 808, preferably a varistor, is connected in parallel with the field coil 802 between the power supply 804 and the circuit breaker 806. The dump resistor 808 can be thermally isolated from the field coil 802 so that heat generated in the dump resistor 808 does not result in any heating (or at most minimal heating) of the field coil 802.

[0131] The quench protection circuit 800 also includes a closely coupled secondary (CCS) coil 810, represented in FIG 8 by (in this example) inductor 810A and resistor 810B. The CCS coil 810 is inductively coupled to the field coil 802 such that changes in the magnetic field produced by the field coil 802 induce a current in the CCS coil 810.

[0132] When the field coil 802 is in use, the circuit breaker 806 is initially closed to allow current to be provided to the superconducting field coil 802 from the power supply 804. As described above, the formation of a "hot spot" due to loss of superconductivity within a portion of one or more turns of the coil will cause a portion of the current to flow radially from the affected turn to an adjacent turn (e.g., through copper bridges 205A-C (or other such bridges made of resistive materials other than copper) in the field coil). When a hot spot is detected, the power supply 804 is disconnected by opening the circuit breaker 806. Current can then flow from the field coil 802 (i.e., from inductor 802A) through the dump resistor 808. However, at least a portion of the current from the field coil 802 can return to the field coil 802 by flowing radially between the turns of the coil. This current corresponds to the current in FIG. 8 from inductor 802A through resistor 802B and back to inductor 802A. The percentage of current that flows along this path (i.e., through resistor 802B) is inversely proportional to the resistance of dump resistor 808 relative to the resistance of resistor 802B. The resistance of dump resistor 808 is selected so that sufficient current flows radially between the turns of coil 802 to heat the conductive elements (e.g., copper bridges 205A-205C) to cause more of the HTS material in coil 802 to become normally conductive (e.g., as described above for the first aspect of the invention). For example, the resistance of dump resistor 808 can be (at least initially) greater than the resistance of resistor 802B such that a significant percentage (e.g., more than 10% or more than 50%) of the current flows radially between two or more turns of field coil 802. This radial or "turn-to-turn" current heats the conductive elements, raising their temperature and increasing their resistivity. Generally, the conductive elements have a relatively low electrical resistance at the operating temperature of HTS field coil 802, but a very high resistance at higher temperatures. For example, if the conductive elements are made of copper, the turn-to-turn resistance of the field coil 802 can increase by approximately 15 times when increasing the temperature from 20K to 200K.

[0133] As the turn-to-turn (radial) resistance of the field coil 802 increases, a greater proportion of the current flows from the coil 802 to the dump resistor 808, thereby reducing the amount of heating provided to the coil 802. The dump resistor 808 can be configured to effectively dissipate heat (e.g., by mounting it to a heat sink or providing fast cooling), so that the temperature rise of the dump resistor 808 can be minimized or limited to an acceptable range. Thus, the heating of the conductive elements by the turn-to-turn current creates a form of negative feedback in which the level of heating of the conductive elements is reduced as a result of the increase in the turn-to-turn resistance of the coil 802 relative to the resistance of the dump resistor 802. This process avoids the conductive elements in the coil 802 (e.g., copper bridges 205A-205C) being "burned out" by the current, while still allowing for rapid heating of the coil 802 after hot spot formation. The duration and magnitude of the heating pulse can be optimized to heat the turns of the coil 802 above the onset temperature of the HTS material as rapidly as possible, while ensuring that the temperature of the conductive elements does not exceed a threshold value.

[0134] Preferably, the resistance of the damp resistor 808 changes over time to further limit the current flowing between the turns of the coil 802 (i.e., through resistor 802B). This can be accomplished, for example, by using a varistor as the damp resistor 808, the varistor being configured such that its resistance decreases as the voltage across the coil 802 increases after a hot spot forms. Suitable varistors are available, for example, from Metrosil®.

[0135] In response to the heating caused by the radial current and hot spots, more of the HTS material in the coil becomes normally conducting (i.e., becomes non-superconducting), causing the current circulating around the turns of field coil 802 to decay, leading to the collapse of the magnetic field generated by coil 802. As this occurs, energy is inductively transferred from field coil 802 to CCS coil 810 and is ultimately dissipated in resistor 810B of the CCS coil 810 circuit. Thus, dump resistor 808 and CCS coil 810 act synergistically to efficiently dissipate the electromagnetic energy stored in field coil 802. In particular, by limiting the turn-to-turn current, dump resistor 808 prevents the temperature of field coil 801 from increasing excessively before significant inductive transfer of energy to CCS coil 810 can occur. Conversely, the rate at which field coil 802 heats up is further reduced as energy is transferred to CCS coil 810, further limiting the temperature rise of field coil 802 to an acceptable level.

[0136] The above disclosure can be applied to various HTS magnet systems. In addition to the tokamak fusion reactors mentioned above as examples, it can be used in HTS coils for nuclear magnetic resonance imaging (NMR / MRI) machines, for the operation of magnetic devices in non-magnetic media via magnetic fields (e.g., robotic magnetic navigation systems for operating medical equipment inside a patient's body), and magnets for electric motors (e.g., for electric aircraft). As a further example, the present disclosure can be applied to proton beam therapy (PBT) machines including HTS magnet systems including the disclosed features, where the HTS magnet system is used in the accelerator of the PBT machine, the quadrupole or dipole steering magnet of the PBT machine, or other magnets of the PBT machine.

[0137] While various embodiments of the present invention have been described above, it should be understood that they have been presented by way of example, and not limitation. It will be apparent to those skilled in the art that various changes in form and detail can be made therein without departing from the spirit and scope of the invention.

Claims

1. A high temperature superconductor (HTS) field coil, a turn including an HTS material wound around an axis of the coil; 1. An HTS field coil, wherein the turns are separated from one another along a direction perpendicular to the axis by one or more layers comprising a magnetoresistive material having an electrical resistivity that decreases in response to an applied magnetic field at a temperature below a generating temperature of the HTS material, whereby electrical resistance between the turns along a direction perpendicular to the axis decreases when an electric current is supplied to the coil.

2. The magnetoresistive material is europium dicarbide, EuC 2 or europium dicarbide, EuC 2 2. The HTS field coil of claim 1 including:

3. 3. An HTS field coil as claimed in claim 1 or 2, wherein the magnetoresistive material has a first metallic phase below a phase transition temperature and a second insulating or semiconducting phase above the phase transition temperature, the phase transition temperature being below a generation temperature of the HTS material.

4. 4. The HTS field coil of claim 1, wherein the temperature at which the magnetoresistive material has an electrical resistivity that decreases in response to an applied magnetic field is greater than the phase transition temperature.

5. 5. An HTS field coil as claimed in claim 3 or 4, wherein the magnetoresistive material has a first resistivity at a temperature below an onset temperature of the HTS material and a lower resistivity at a second temperature above an onset temperature of the HTS material.

6. 6. An HTS field coil as claimed in any one of claims 3 to 5, wherein the turns are formed from one or more HTS tapes including the HTS material as a layer on a flexible substrate.

7. 7. The HTS field coil of claim 6, wherein each layer containing the magnetoresistive material is provided on a flexible substrate that is co-wound with one or more HTS tapes about the axis of the coil.

8. 1. A high temperature superconductor (HTS) cable for winding into an HTS field coil, the cable having a stack of layers including a flexible substrate, a layer of HTS material, and a layer of magnetoresistive material, the magnetoresistive material having an electrical resistivity that decreases in response to an applied magnetic field at a temperature below a generation temperature of the HTS material.

9. 8. An electromagnet comprising one or more HTS field coils according to any one of claims 1 to 7.

10. 8. A system comprising a plasma vessel and a set of field coils for generating a magnetic field within the plasma vessel, each field coil being an HTS field coil according to any one of claims 1 to 7.

11. 8. A tokamak fusion reactor including an HTS field coil according to any one of claims 1 to 7, wherein the HTS field coil is either a toroidal field coil or a poloidal field coil.

12. A high temperature superconductor (HTS) magnet system A high temperature superconductor (HTS) field coil according to any one of claims 1 to 7; a detection unit configured to detect loss of superconductivity in an HTS material of at least a portion of one turn of the HTS field coil; a quench protection unit configured to transfer current from the HTS field coil to an external resistive load in response to said detecting; 1. An HTS magnet system comprising:

13. 13. The HTS magnet system of claim 12, wherein the external resistive load is a varistor.

14. 8. A method of protecting a high temperature superconductor (HTS) field coil according to any one of claims 1 to 7 from damage following loss of superconductivity in one or more turns of the HTS field coil, comprising: detecting a loss of superconductivity in an HTS material of at least one turn of the HTS field coil; electrically connecting the HTS field coil to an external resistive load in response to said detecting; The method includes: