Sealing Film
A single-layer sealing film with tailored moisture adsorbent distribution addresses the multiple-layer challenges in OLED encapsulation, ensuring effective moisture barrier, adhesion, and durability while maintaining thinness and reliability.
Patent Information
- Application Number
- JP2024518494
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-12-01
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-12-01
AI Technical Summary
Existing OLED encapsulation methods require multiple layers to achieve moisture barrier and adhesive properties, leading to increased costs, complexity, and reduced thinness, which compromises durability and reliability.
A single-layer sealing film with a specific distribution of moisture adsorbents, achieving excellent moisture barrier and adhesive properties by varying adsorbent concentration across the thickness direction, eliminating the need for separate layers.
The single-layer sealing film provides enhanced moisture barrier, adhesion, and durability while maintaining a thin design, reducing costs and process complexity, and preventing defects like white spots and panel failures.
Smart Images

Figure 2024535907000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to an encapsulating film, a method for producing the same, an organic electronic device including the same, and a method for producing the organic electronic device. [Background technology]
[0002] Organic electronic device (OED) refers to a device containing layers of organic materials that use holes and electrons to generate an alternating current of electric charge, examples of which include photovoltaic devices, rectifiers, transmitters, and organic light emitting diodes (OLEDs).
[0003] Among the organic electronic devices, organic light emitting diodes (OLEDs) consume less power and have a faster response speed than conventional light sources, which is advantageous for making displays or lighting thinner. In addition, OLEDs have excellent space utilization and are expected to be applied in various fields such as various portable devices, monitors, notebook computers, and televisions.
[0004] The biggest problem in commercializing OLEDs and expanding their applications is their durability. The organic materials and metal electrodes contained in OLEDs are easily oxidized by external factors such as moisture. Therefore, an encapsulation film with maximized moisture blocking properties is required.
[0005] In particular, in order to ensure excellent moisture barrier properties, the OLED encapsulant must include a layer having moisture barrier properties as an essential component, and the layer having moisture barrier properties must have excellent adhesive properties with the upper and / or lower components. It is possible to consider a method in which the layer having moisture barrier properties and the layer having adhesive properties are separately manufactured and then the layers are attached to each other to be integrated, but this method requires the manufacture of multiple layers to ensure the required functions, which can lead to problems such as increased costs, complicated processes, and reduced thinning efficiency. Summary of the Invention [Problem to be solved by the invention]
[0006] The present application provides an encapsulating film that can form a structure that can block moisture or oxygen from entering an organic electronic device from the outside and can maintain durability and reliability even in harsh environments. The encapsulating film according to the present application can exhibit excellent moisture blocking properties and adhesiveness with only a single layer, so that a device using the encapsulating film according to the present application can maintain a thin shape.
[0007] The technical problems of the present application are not limited to the technical problems mentioned above, and other technical problems not mentioned can be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0008] The present invention can be modified in various ways and may have various embodiments, and a specific embodiment will be illustrated in the drawings and described in detail. However, this is not intended to limit the present invention to a specific embodiment, and it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention. When an element such as a layer, region, or substrate is referred to as being "on" another component, it will be understood that this can be directly on the other element, or there can be intermediate elements therebetween.
[0009] The terms used in this application are merely used to describe specific embodiments and are not intended to limit the present invention. Singular expressions include plural expressions unless otherwise clearly indicated otherwise. In this application, terms such as "include" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood not to preclude the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0010] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms as defined in commonly used dictionaries should be understood to have a meaning consistent with the meaning they have in the relevant art, and should not be understood as idealized or overly formal unless expressly defined in this application.
[0011] The present application relates to an encapsulating film, which can be applied to encapsulate or seal an organic electronic device, such as an OLED. As used herein, the term "organic electronic device" refers to an article or device having a structure including an organic material layer that generates an alternating current of charge using holes and electrons between a pair of opposing electrodes, examples of which include, but are not limited to, photovoltaic cell devices, rectifiers, transmitters, and organic light-emitting diodes (OLEDs). In one example of the present application, the organic electronic device may be an OLED.
[0012] In order to ensure excellent moisture barrier properties, an OLED encapsulant must include a layer having moisture barrier properties as an essential component, and the layer having moisture barrier properties must have excellent adhesive properties with the upper and / or lower components. It is also possible to consider a method of separately manufacturing a layer having moisture barrier properties and a layer having adhesive properties, and then attaching each layer to each other to integrally bond them, but this method requires manufacturing multiple layers to ensure the required functions, which can lead to problems such as increased costs, complicated processes, and reduced thinning efficiency. Therefore, in order to solve these problems, the present application provides an encapsulant film that can exhibit excellent moisture barrier properties and adhesiveness with only a single layer.
[0013] An exemplary sealing film may include a sealing layer that is a cured product of a sealing composition, and the sealing composition may include a sealing resin and a moisture adsorbent. The sealing layer may be a single layer, and in Gaussian curve fitting to the distribution of the moisture adsorbent in the thickness (depth) direction in the sealing layer, the position distribution (σ value) of the moisture adsorbent in the thickness direction may be 2 or less.
[0014] As an example, in Gaussian curve fitting to the thickness distribution of the moisture adsorbent, the position distribution (σ value) in the thickness direction of the moisture adsorbent may be 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.1 or less, 1 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, 0.15 or less, or 0.1 or less, and the lower limit is not greatly limited, but may be 0.001 or more.
[0015] Here, the Gaussian curve fitting represents a function for the thickness of the encapsulation layer, as shown in Equation 1 below.
[0016]
number
[0017] In Equation 1, A and b are constants related to the absolute amount of the moisture adsorbent,
number
[0018] When the σ value in the Gaussian curve fitting to the thickness distribution of the moisture adsorbent satisfies the specific range as described above, the moisture adsorbent may be contained at a high content in the region corresponding to the center of the sealing film in the thickness direction, thereby achieving excellent moisture adsorption while at the same time improving the adhesive properties. That is, the sealing layer may include a first region, a second region, and a third region in which the concentration of the moisture adsorbent differs according to the thickness direction, and although the sealing layer is a single layer and not a laminated structure having a plurality of layers, the single layer may be arbitrarily divided into regions according to the concentration of the moisture adsorbent. As an example, the first region, the second region, and the third region constituting the single-layer sealing layer may have different contents of the moisture adsorbent. In this case, in relation to the division of the regions according to the content of the moisture adsorbent, the content of the moisture adsorbent may change continuously at the interface of each region, so that the interface of each region does not necessarily need to be clearly divided.
[0019] In one example, the second region may have a higher content of moisture adsorbent than the first and third regions. That is, the second region may have a higher content of moisture adsorbent than the first and second regions. In this case, it is sufficient that the first and second regions have a lower content of moisture adsorbent than the second region, and the first and second regions may have the same or different moisture adsorbent contents.
[0020] 1 is a diagram showing a single-layer sealing layer with regions distinguished according to the content of the moisture adsorbent, and referring to Fig. 1, second region 22, which is a region with a high content of moisture adsorbent, may be interposed between first region 21 and third region 23, which are regions with a low concentration of moisture adsorbent. In other words, first region 21 and third region 23, which are regions with a low content of moisture adsorbent, may be located on the upper or lower surface forming the uppermost or lowermost part of sealing layer 11, respectively, and may be in direct contact with other components that are in contact with the upper or lower part of the sealing layer. That is, according to the present invention, the moisture adsorbent contained in the sealing layer may be present in a particulate form in a state where it is not uniformly distributed in the sealing layer. Here, distribution refers to the manner in which particles fill the space, and is a concept that is different from dispersion. The uniform distribution state means that the moisture adsorbent is present in every part of the sealing layer or sealing film at the same or substantially the same density, the particles are separated as far as possible from each other, and are uniformly filled in the space.
[0021] In addition, when the sealing layer in contact with the organic electronic element contains an excessive amount of moisture adsorbent in a uniformly distributed state, the moisture adsorbent is also present in excess on the upper and lower surfaces of the uppermost and / or lowermost sealing layers. In this case, the adhesive performance of the sealing layer is significantly reduced, which may cause a problem of reduced durability and reliability of the organic electronic element.
[0022] Therefore, a multi-layer structure including at least two sealing layers has been used as a sealing film in the past. That is, when a sealing film of a multi-layer structure is applied to an organic electronic element, the first sealing layer facing the organic electronic element does not contain a moisture adsorbent or contains only a small amount of the moisture adsorbent, and the second sealing layer located on the opposite side to the surface facing the organic electronic element is designed to contain a large amount of the moisture adsorbent, thereby ensuring adhesion from the first sealing layer in contact with the organic electronic element and moisture barrier properties from the second sealing layer. However, the sealing layer according to the present application is a single layer, and contains a moisture adsorbent at a high concentration in the center in the thickness (depth) direction of the sealing layer, and contains a moisture adsorbent at a low concentration on both surfaces of the sealing layer, so that the moisture adsorbent shows a specific distribution state. As a result, the present application can provide a sealing film that exhibits excellent adhesion above an appropriate level even without a separate pressure-sensitive adhesive layer or adhesive layer, while at the same time having excellent barrier properties.
[0023] In one example, the metal adhesion of the sealing layer may be 4,000 gf / in or more, 4,200 gf / in or more, 4,400 gf / in or more, 4,600 gf / in or more, 4,800 gf / in or more, 5,000 gf / in or more, 5,100 gf / in or more, 5,200 gf / in or more, 5,300 gf / in or more, 5,400 gf / in or more, or 5,500 gf / in or more. The upper limit is not particularly limited, but may be 10,000 gf / in or less or 8,000 gf / in or less. That is, as described above, the sealing layer according to the present application has a different content of moisture adsorbent in the thickness direction, and the upper surface or lower surface of the sealing layer is located in the first region or the third region, which is a low content region of the moisture adsorbent, so that the sealing layer of the present application can have excellent metal adhesion. The metal adhesion is the adhesion to a metal layer that can be added onto the sealing layer, as described below, and may be measured by fixing the sealing film that has been left in a constant temperature and humidity room at a temperature of 22±5°C and 50±10% for 30 minutes to a tensile machine (TA, Texture Analyser) and measuring it in Tension Mode at a temperature of 25°C and a tension speed of 5 mm / min.
[0024] In one example, the sealing layer prepared from the above may have a gel content of 60% or more as measured by the following general formula 1:
[0025] [General formula 1] Gel content (%) = A / B x 100
[0026] In the general formula 1, B is the mass of the sealing layer sample, and A is the dry mass of the insoluble portion of the sealing layer that does not pass through a 200-mesh screen after immersing the sample in toluene at 60° C. for 24 hours and then filtering the sample through a 200-mesh screen. In this specification, the unit mesh may be a unit based on the ASTM standard. The mass B of the sealing layer sample can be measured in 1 g. The gel content may be, for example, 63% or more, 65% or more, 67% or more, 70% or more, 72% or more, 75% or more, or 78% or more, and the upper limit may be, for example, 99% or less, 95% or less, 93% or less, 89% or less, 86% or less, 84% or less, 82% or less, or 80% or less. The present application can provide a sealing film that is excellent in not only moisture blocking property and stress absorption property but also curing physical property by adjusting the gel content.
[0027] In addition, the encapsulation layer according to the present application may have an acid value of 1 or less. The acid value may be, for example, 0.9 or less, 0.8 or less, or 0.7 or less, and the lower limit is not particularly limited, but may be 0.1 or more. Unlike the moisture barrier property and the occurrence of dark spots and bright spots of organic electronic devices, which have been problems in the past, white spots occurring from organic electronic devices have recently become the main cause of panel defects. The present application confirmed that the mechanism by which the white spots occur is due to an organic acid present in the encapsulation composition, and was able to effectively suppress the occurrence of white spots by adjusting the acid value of the encapsulation layer as well as the crosslinking degree of the encapsulation layer matrix by the gel content. In a specific example, the organic acid reaches the organic electronic device in the form of ions, and generates white spots by shifting the threshold voltage due to cracks that may be partially formed on the device. Such technical problems can be prevented by adjusting the acid value and gel content of the encapsulation layer that encapsulates the entire surface of the organic electronic device.
[0028] Furthermore, the sealing layer according to the present application may have excellent light transmittance in the visible light region. In one example, the sealing composition according to the present application may exhibit a light transmittance of 80% or more according to the JIS K7105 standard after curing. For example, the sealing composition may have a light transmittance of 85% or more, 90% or more, 92% or more, or 93% or more in the visible light region. The sealing layer according to the present application may exhibit low haze along with excellent light transmittance. In one example, the sealing composition may have a haze of 5% or less, 4% or less, 3% or less, or 1% or less according to the JIS K7105 standard after curing. The optical properties may be measured at 550 nm using a UV-Vis Spectrometer.
[0029] In one example, after curing of the organic electronic device encapsulating layer, the yellow index (△YI) value measured using a colorimeter according to ASTM D 1003 standard may be 1 or less, and the lower limit is not particularly limited, but may be -2 or more.
[0030] In one example, when the encapsulating layer is subjected to purge and trap at 100° C. for 60 minutes using a Purge & Trap sampler (JAI JTD-505III-GC / MSD system (Agilent 7890B / 5977A) measuring device, and then the total outgassing amount is measured using gas chromatography mass spectrometry, the measured outgassing amount may be less than 400 ppm, specifically, 300 ppm or less, 200 ppm or less, 100 ppm or less, 90 ppm or less, 80 ppm or less, 70 ppm or less, 50 ppm or less, 30 ppm or less, 20 ppm or less, or 10 ppm or less. That is, since the encapsulating layer according to the present invention contains a composition described below, the amount of outgassing generated from the encapsulating layer is extremely small, and therefore an organic electronic device to which the encapsulating layer is applied may have excellent reliability.
[0031] In one embodiment, the encapsulation layer may have a thickness of 30 μm or more and 500 μm or less. The encapsulation layer of the present application may have a thickness of 30 μm or more, 33 μm or more, 35 μm or more, 40 μm or more, 43 μm or more, 45 μm or more, 47 μm or more, 50 μm or more, 52 μm or more, 55 μm or more, 57 μm or more, or 60 μm or more, and the upper limit is not particularly limited, and may be 500 μm or less, 400 μm or less, 300 μm or less, 250 μm or less, or 200 μm or less. The present application realizes a gel content at a desired level while increasing the thickness of the encapsulation layer compared to the conventional one, thereby maximizing moisture barrier properties, and also provides an organic electronic device that absorbs stress and has high reliability when panel warpage occurs in a harsh environment such as high temperature. Conventionally, encapsulating films were coated to a certain thickness and then irradiated with UV light to form them, but this had problems such as UV not penetrating into the film, resulting in a significant decrease in curing properties, and the solvent remaining inside the film, resulting in some of the solvent remaining unvolatilized and uncured materials damaging the organic electronic device. In particular, the encapsulating composition of the present application seals the entire surface of the organic electronic device and can be in direct contact with one surface of the organic electronic device, and the encapsulating composition does not contain a separate dispersant as described below, but by using a solventless type having a composition described below, the reliability of the organic electronic device can be further improved, and the encapsulating composition shows an improved curing rate even at a certain thickness, thereby realizing excellent curing properties as well as moisture barrier properties and stress absorption.
[0032] In one example, the sealing layer of the present application may be a single layer, but is not limited thereto, and may be a multi-layer structure including at least two or more sealing layers. When the sealing layer includes two or more sealing layers, the sealing layer may include a first sealing layer that faces the organic electronic element when sealing the element, and a second sealing layer that is located on the opposite side of the first sealing layer that faces the element. In one specific example, the sealing film includes at least two or more sealing layers, and the sealing layer may include a first sealing layer that faces the organic electronic element when sealing, and a second sealing layer that does not face the organic electronic element. In addition, when two or more layers constitute the sealing layer, the composition of each layer of the sealing layer may be the same or different. In one example, the sealing layer may include a sealing resin and / or a moisture adsorbent, and the sealing layer may be a pressure-sensitive adhesive layer or an adhesive layer. For example, when the encapsulation film is applied onto an organic electronic device, the first encapsulation layer, which is the encapsulation layer facing the organic electronic device, may not contain a moisture adsorbent, or may contain a small amount of 5 wt % or less based on the total weight of the moisture adsorbent, or a large amount of a moisture adsorbent as described below may be contained in the second encapsulation layer.
[0033] In a specific example, the encapsulating film 1 of the present application may include an encapsulating layer 11 and a base layer 12, as shown in Figure 2. The encapsulating film can seal the entire surface of an organic electronic element formed on a substrate.
[0034] In one example, the encapsulating composition of the present application may include an encapsulating resin, which may be a crosslinkable or curable resin, and in an embodiment, may include an olefin-based resin.
[0035] In one example, the sealing composition may be a solventless type. In this specification, the solventless type means that the sealing composition does not contain a solvent or contains a solvent in an amount of 0.1 wt% or less or 0.01 wt% or less in the total composition. That is, the sealing composition contains a solid content of 99 wt% or more, 99.9 wt% or more, or 100 wt%, and the present application provides a sealing film that can be formed using only raw materials with a solid content of 99 wt% or more or 100 wt% without a separate solvent.
[0036] In one example, the sealing resin may have a glass transition temperature of less than 0° C., less than −10° C., or less than −30° C., less than −50° C., or less than −60° C. The lower limit is not particularly limited, and may be −150° C. or higher. The glass transition temperature may be the glass transition temperature after curing.
[0037] In one embodiment of the present application, the encapsulating resin may be an olefin-based resin. In one embodiment, the olefin-based resin may be a homopolymer of a butylene monomer; a copolymer obtained by copolymerizing a butylene monomer with another monomer polymerizable therewith; a reactive oligomer using a butylene monomer; or a mixture thereof. The butylene monomer may include, for example, 1-butene, 2-butene, or isobutylene. In one embodiment, the olefin-based resin may include an isobutylene monomer as a polymerization unit.
[0038] The other monomer polymerizable with the butylene monomer or derivative may include, for example, isoprene, styrene, butadiene, etc. By using the copolymer, physical properties such as processability and crosslinking degree can be maintained, and the heat resistance of the adhesive can be ensured when applied to an organic electronic device.
[0039] The reactive oligomer using butylene monomer may include a butylene polymer having a reactive functional group. The oligomer may have a weight average molecular weight in the range of 500 to 5000 g / mol. The butylene polymer may be bonded to another polymer having a reactive functional group. The other polymer may be, but is not limited to, an alkyl (meth)acrylate. The reactive functional group may be a hydroxyl group, a carboxyl group, an isocyanate group, or a nitrogen-containing group. The reactive oligomer and the other polymer may be crosslinked by a multifunctional crosslinking agent, and the multifunctional crosslinking agent may be one or more selected from the group consisting of an isocyanate crosslinking agent, an epoxy crosslinking agent, an aziridine crosslinking agent, and a metal chelate crosslinking agent.
[0040] In one example, the encapsulating resin of the present application may include a copolymer of a diene and an olefin-based compound containing one carbon-carbon double bond. Here, the olefin-based compound may include butylene, etc., and the diene may be a monomer polymerizable with the olefin-based compound, such as isoprene or butadiene, etc. For example, the copolymer of the olefin-based compound containing one carbon-carbon double bond and the diene may be butyl rubber.
[0041] The resin or elastomer component in the sealing layer may have a weight average molecular weight (Mw) that allows the pressure-sensitive adhesive composition to be molded into a film shape. For example, the resin or elastomer may have a weight average molecular weight of about 100,000 to 2,000,000 g / mol, 120,000 to 1,500,000 g / mol, 150,000 to 1,000,000 g / mol, 200,000 to 700,000 g / mol, 230,000 to 600,000 g / mol, 250,000 to 500,000 g / mol, or 300,000 to 470,000 g / mol. In this specification, the term weight average molecular weight means a converted value relative to standard polystyrene measured by GPC (Gel Permeation Chromatography), and the unit is g / mol unless otherwise specified. However, the resin or elastomer component does not necessarily have to have the weight average molecular weight mentioned above. For example, when the molecular weight of the resin or elastomer component is not at a level that allows it to form a film, a separate binder resin may be blended into the pressure-sensitive adhesive composition.
[0042] In one example, the encapsulating resin may be included in the encapsulating layer at 10 wt% or more, 13 wt% or more, 15 wt% or more, 17 wt% or more, 20 wt% or more, 21 wt% or more, 22 wt% or more, 23 wt% or more, or 24 wt% or more, and the upper limit may be 90 wt% or less, 80 wt% or less, 70 wt% or less, 60 wt% or less, 50 wt% or less, 40 wt% or less, or 30 wt% or less. The encapsulating resin has a good moisture barrier property but a disadvantage of poor heat resistance durability, so the present application adjusts the content of the encapsulating resin to fully realize the moisture barrier property of the resin while maintaining heat resistance durability at high temperature and high humidity.
[0043] In one example, the sealing film may include a moisture absorbent. As used herein, the term "moisture absorbent" may refer to, for example, a chemically reactive absorbent that can remove moisture or humidity that has permeated the sealing film through a chemical reaction, as described below.
[0044] In one embodiment, the moisture adsorbent may not have an organic acid on its surface. In general, the moisture adsorbent may be surface-treated with a dispersant so that it can be well dispersed in the composition, and in this case, an organic acid is present on the surface of the moisture adsorbent. Such organic acid permeates toward the element in the sealing layer that directly contacts the element, causing white spot defects in the OLED panel. In the present application, the moisture adsorbent does not include a dispersant or does not include an organic acid, thereby improving the reliability of the entire sealing composition and preventing OLED panel defects.
[0045] Examples of the moisture adsorbent that can be used in the above-mentioned method include metal oxides, sulfates, and organic metal oxides. Specifically, examples of the sulfates include magnesium sulfate, sodium sulfate, and nickel sulfate, and examples of the organic metal oxides include aluminum oxide octylate. Specific examples of the metal oxides include phosphorus pentoxide (P2O5), lithium oxide (Li2O), sodium oxide (Na2O), barium oxide (BaO), calcium oxide (CaO), and magnesium oxide (MgO), and examples of the metal salts include sulfates such as lithium sulfate (Li2SO4), sodium sulfate (Na2SO4), calcium sulfate (CaSO4), magnesium sulfate (MgSO4), cobalt sulfate (CoSO4), gallium sulfate (Ga2(SO4)3), titanium sulfate (Ti(SO4)2), and nickel sulfate (NiSO4), calcium chloride (CaCl2), magnesium chloride (MgCl2), and strontium chloride. Examples of the moisture adsorbent include, but are not limited to, metal halides such as cerium chloride (SrCl2), yttrium chloride (YCl3), copper chloride (CuCl2), cesium fluoride (CsF), tantalum fluoride (TaF5), niobium fluoride (NbF5), lithium bromide (LiBr), calcium bromide (CaBr2), cesium bromide (CeBr3), selenium bromide (SeBr4), vanadium bromide (VBr3), magnesium bromide (MgBr2), barium iodide (BaI2) or magnesium iodide (MgI2); or metal chlorates such as barium perchlorate (Ba(ClO4)2) or magnesium perchlorate (Mg(ClO4)2). As the moisture adsorbent that can be included in the sealing layer, one of the above-mentioned compositions can be used, or two or more can be used. In one example, when two or more types of moisture adsorbents are used, calcined dolomite, etc. can be used.
[0046] Such moisture adsorbents can be controlled to an appropriate size depending on the application. In one example, the average particle size of the moisture adsorbent can be controlled to 100 to 15,000 nm, 500 nm to 10,000 nm, 800 nm to 8,000 nm, 1 μm to 7 μm, 2 μm to 5 μm, or 2.5 μm to 4.5 μm. Moisture adsorbents having a size in the above range do not react very quickly with moisture, so they are easy to store and do not damage the device to be encapsulated. In this specification, unless otherwise specified, the particle size may mean the average particle size, and may be measured by a known method using a D50 particle size analyzer.
[0047] The content of the moisture adsorbent is not particularly limited and can be appropriately selected in consideration of the intended blocking properties. The moisture adsorbent may be included in an amount of 110 parts by weight or more relative to 100 parts by weight of the sealing resin, and may be included in an amount of 113 to 800 parts by weight, 115 to 750 parts by weight, 117 to 700 parts by weight, 120 to 650 parts by weight, 123 to 600 parts by weight, 125 to 550 parts by weight, 127 to 500 parts by weight, 130 to 470 parts by weight, 133 to 450 parts by weight, 135 to 430 parts by weight, 137 to 400 parts by weight, 140 to 370 parts by weight, 143 to 350 parts by weight, 145 to 330 parts by weight, 147 to 300 parts by weight, 150 to 270 parts by weight, 153 to 250 parts by weight, or 155 to 240 parts by weight. That is, the encapsulation film according to the present application can exhibit excellent compatibility with other compositions in the encapsulation layer while containing a larger amount of moisture adsorbent than conventional ones, and at the same time, can exhibit excellent dispersibility without a separate dispersant for the moisture adsorbent, thereby realizing an excellent moisture blocking effect.
[0048] In one example, the sealing film may further include a tackifier. The tackifier may be, for example, a compound having a softening point of 70° C. or more, and in a specific example, the softening point may be 75° C. or more, 78° C. or more, 83° C. or more, 85° C. or more, 90° C. or more, or 95° C. or more, and the upper limit is not particularly limited, but may be 150° C. or less, 145° C. or less, 140° C. or less, 135° C. or less, 130° C. or less, or 125° C. The tackifier may be a compound having a cyclic structure in its molecular structure, and the cyclic structure may have a carbon number in the range of 5 to 15. The carbon number may be, for example, in the range of 6 to 14, 7 to 13, or 8 to 12. The cyclic structure may be a monocyclic compound, but is not limited thereto, and may be a bicyclic or tricyclic compound. The tackifier may also be an olefin-based polymer, and the polymer may be a homopolymer or a copolymer. The tackifier of the present application may also be a hydrogenated compound. The hydrogenated compound may be a partially or completely hydrogenated compound. Such a tackifier can have excellent moisture blocking properties and external stress relaxation properties while having good compatibility with other components in the sealing film. Specific examples of the tackifier include hydrogenated terpene resins, hydrogenated ester resins, and hydrogenated dicyclopentadiene resins. The weight average molecular weight of the tackifier may be within the range of about 200 to 5,000 g / mol, 300 to 4,000 g / mol, 400 to 3,000 g / mol, or 500 to 2,000 g / mol. The content of the tackifier can be appropriately adjusted as necessary. For example, the content of the tackifier may be 15 to 200 parts by weight, 20 to 190 parts by weight, 25 to 180 parts by weight, or 30 to 150 parts by weight relative to 100 parts by weight of the sealing resin. The present application can provide a sealing film having excellent moisture blocking properties and external stress relaxation properties by using the specific tackifier.
[0049] In the encapsulating film of the present application, the encapsulating layer may include a bright spot inhibitor. The bright spot inhibitor may have an adsorption energy of 0 eV or less with respect to outgassing calculated by density functional theory. The lower limit of the adsorption energy is not particularly limited, but may be -20 eV. The type of outgassing is not particularly limited, but may include oxygen, H atoms, H2 molecules, and / or NH3. In the present application, the encapsulating film includes the bright spot inhibitor, so that bright spots caused by outgassing generated from an organic electronic device can be prevented.
[0050] In the specific example of the present application, the adsorption energy between the bright spot inhibitor and the bright spot-causing atom or molecule can be calculated using electronic structure calculations based on density functional theory. The calculations can be performed by methods known in the art. For example, the present application creates a two-dimensional slab structure in which the close-packed surface of the bright spot inhibitor having a crystalline structure appears on the surface, then performs structural optimization, and performs structural optimization on the structure in which the bright spot-causing molecule is adsorbed on the surface in a vacuum state, and defines the difference in total energy between the two systems minus the total energy of the bright spot-causing molecule as the adsorption energy. To calculate the total energy for each system, a revised-PBE function, which is a function of the GGA (generalized gradient approximation) series in exchange-correlation that simulates electron-electron interactions, was used, and the cutoff of the electron kinetic energy was set to 500 eV, and only the gamma point corresponding to the origin of the reciprocal space was included in the calculation. To optimize the atomic structure of each system, the conjugate gradient method was used, and calculations were repeated until the interatomic forces were less than 0.01 eV / Å. A series of calculations were performed using the conventional code VASP.
[0051] The material of the bright spot inhibitor is not limited as long as the encapsulation film is applied to an organic electronic device and has the effect of preventing bright spots on the panel of the organic electronic device. For example, the bright spot inhibitor is an outgas generated in an inorganic deposition layer of silicon oxide, silicon nitride, or silicon oxynitride deposited on an electrode of an organic electronic device, and is, for example, oxygen, H2 gas, ammonia (NH3) gas, H + , N.H. 2+ , NHR2 or NH2R, where R may be an organic group, such as, but not limited to, an alkyl group, an alkenyl group, or an alkynyl group.
[0052] In one embodiment, the material of the bright spot inhibitor is not limited as long as it satisfies the adsorption energy value, and may be metal or nonmetal. The bright spot inhibitor may include, for example, Li, Ni, Ti, Rb, Be, Mg, Ca, Sr, Ba, Al, Zn, In, Pt, Pd, Fe, Cr, Si or a combination thereof, or may include an oxide or nitride of the material, or may include an alloy of the material. In one embodiment, the bright spot inhibitor may include nickel particles, nickel oxide particles, titanium nitride, titanium-based iron-titanium alloy particles, manganese-based iron-manganese alloy particles, magnesium-nickel magnesium-based alloy particles, rare earth-based alloy particles, carbon nanotubes, graphite, aluminophosphate molecular sieve particles, or mesosilica particles. The bright spot inhibitor may be included in an amount of 3 to 150 parts by weight, 6 to 143 parts by weight, 8 to 131 parts by weight, 9 to 123 parts by weight, 10 to 116 parts by weight, 10 to 95 parts by weight, 10 to 50 parts by weight, or 10 to 35 parts by weight, based on 100 parts by weight of the encapsulating resin. In the present application, within the above content range, the adhesive strength and durability of the film can be improved, and bright spot prevention of the organic electronic device can be realized. In addition, the particle diameter of the bright spot inhibitor may be within the range of 10 nm to 30 μm, 50 nm to 21 μm, 105 nm to 18 μm, 110 nm to 12 μm, 120 nm to 9 μm, 140 nm to 4 μm, 150 nm to 2 μm, 180 nm to 900 nm, 230 nm to 700 nm, or 270 nm to 400 nm. The particle diameter may be determined by D50 particle size analysis. By including the bright spot inhibitor, the present application can efficiently adsorb hydrogen generated within an organic electronic device while simultaneously realizing moisture barrier properties and durability reliability of the encapsulation film.
[0053] In one example, the sealing layer of the present application may contain an active energy ray-polymerizable compound that is highly compatible with the sealing resin and can form a specific crosslinked structure together with the sealing resin. For example, the sealing layer of the present application may contain, together with the sealing resin, a polyfunctional active energy ray-polymerizable compound that can be polymerized by irradiation with active energy rays. The active energy ray-polymerizable compound may mean, for example, a compound containing two or more functional groups that can participate in a polymerization reaction by irradiation with active energy rays, such as a functional group containing an ethylenically unsaturated double bond, such as an acryloyl group or a methacryloyl group, an epoxy group, or an oxetane group.
[0054] As the multifunctional active energy ray-polymerizable compound, for example, a multifunctional acrylate (MFA) can be used. The active energy ray polymerizable compound may be contained in an amount of 0.5 to 10 parts by weight, 0.7 to 9 parts by weight, 1 to 8 parts by weight, 1.3 to 7 parts by weight, or 1.5 to 6 parts by weight relative to 100 parts by weight of the sealing resin. Within the above range, the present application provides a sealing film having excellent durability and reliability even under severe conditions such as high temperature and high humidity.
[0055] The polyfunctional active energy ray-polymerizable compound that can be polymerized by irradiation with active energy rays can be used without any limitation. For example, the compound may include 1,4-butanediol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate (HDDA), 1,8-octanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, cyclohexane-1,4-dimethanol di(meth)acrylate, tricyclodecane dimethanol (meth)diacrylate, dimethylol dicyclopentane di(meth)acrylate, neopentyl glycol modified trimethylpropane di(meth)acrylate, adamantane di(meth)acrylate, trimethylolpropane tri(meth)acrylate (TMPTA), or mixtures thereof.
[0056] As the polyfunctional active energy ray polymerizable compound, for example, a compound having a molecular weight of 100 or more and less than 1,000 g / mol and containing two or more functional groups can be used. The ring structure contained in the polyfunctional active energy ray polymerizable compound may be a carbocyclic structure or a heterocyclic structure; or a monocyclic or polycyclic structure.
[0057] In the specific example of the present application, the sealing layer may further include a radical initiator. The radical initiator may be a photoinitiator or a thermal initiator. The specific type of photoinitiator may be appropriately selected in consideration of the curing speed and the possibility of yellowing. For example, a benzoin-based, hydroxyketone-based, aminoketone-based, or phosphine oxide-based photoinitiator may be used, and specifically, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2 ... Pyrketone, benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone] and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, etc., can be used.
[0058] The radical initiator may be included in an amount of 0.2 to 20 parts by weight, 0.5 to 18 parts by weight, 1 to 15 parts by weight, or 2 to 13 parts by weight, based on 100 parts by weight of the active energy ray-polymerizable compound, thereby effectively inducing the reaction of the active energy ray-polymerizable compound and preventing the physical properties of the sealing layer composition from being deteriorated due to remaining components after curing.
[0059] In addition to the above-mentioned components, the encapsulating layer may contain various additives depending on the intended use and the manufacturing process of the encapsulating film described below. For example, the encapsulating layer may contain a curable material, a crosslinking agent, a filler, etc. in an appropriate range of content depending on the desired physical properties.
[0060] In one embodiment, the sealing composition is heated at 170° C. and 50 s -1 The viscosity measured at a shear rate may be in the range of 1,000 to 2,000 Pa·s, and for example, the lower limit of the viscosity may be 1,100 Pa·s or more, 1,200 Pa·s or more, 1,300 Pa·s or more, 1,400 Pa·s or more, or 1,500 Pa·s or more. Although not limited thereto, the viscosity may be a value measured by an ARES (Advanced Rheometric Expansion System). Thus, despite the encapsulating composition being a high-viscosity liquid phase, the present application allows the moisture adsorbent to exhibit uniform dispersion in the encapsulating composition through the extrusion process as described above.
[0061] In a specific example of the present application, the sealing film may further include a metal layer formed on the sealing layer. The metal layer of the present application may have a thermal conductivity of 20 W / m·K or more, 50 W / m·K or more, 60 W / m·K or more, 70 W / m·K or more, 80 W / m·K or more, 90 W / m·K or more, 100 W / m·K or more, 110 W / m·K or more, 120 W / m·K or more, 130 W / m·K or more, 140 W / m·K or more, 150 W / m·K or more, 200 W / m·K or more, or 210 W / m·K or more. The upper limit of the thermal conductivity is not particularly limited, and may be 800 W / m·K or less. By having such a high thermal conductivity, heat generated at the bonding interface during the metal layer bonding process can be released more quickly. In addition, the high thermal conductivity allows heat accumulated during the operation of the organic electronic device to be quickly released to the outside, thereby allowing the temperature of the organic electronic device to be kept lower, and the occurrence of cracks and defects can be reduced. The thermal conductivity may be measured at any one of temperatures in the range of 15 to 30°C.
[0062] The term "thermal conductivity" as used herein refers to the degree to which a material can transfer heat by conduction, and can be expressed in units of W / m K. The unit indicates the degree to which a material transfers heat at the same temperature and distance, and refers to the unit of heat (watts) relative to the unit of distance (meters) and the unit of temperature (calvin).
[0063] In a specific example of the present application, the metal layer of the sealing film may be transparent or opaque. The thickness of the metal layer may be within a range of 3 μm to 200 μm, 10 μm to 100 μm, 20 μm to 90 μm, 30 μm to 80 μm, or 40 μm to 75 μm. The present application provides a thin sealing film in which the heat dissipation effect is fully realized by controlling the thickness of the metal layer. The metal layer may be a thin metal foil or a polymer substrate layer on which a metal is deposited. The metal layer is not particularly limited as long as it satisfies the above-mentioned thermal conductivity and is a material containing a metal. The metal layer may include any one of metal, metal oxide, metal nitride, metal carbide, metal oxynitride, metal oxyboride, and combinations thereof. For example, the metal layer may include an alloy in which one metal is added with one or more metal elements or nonmetal elements, and may include, for example, stainless steel (SUS). Also, in one example, the metal layer may include iron, chromium, copper, aluminum nickel, iron oxide, chromium oxide, silicon oxide, aluminum oxide, titanium oxide, indium oxide, tin oxide, indium tin oxide, tantalum oxide, zirconium oxide, niobium oxide, and combinations thereof. The metal layer may be deposited by electrolysis, rolling, thermal evaporation, e-beam evaporation, sputtering, reactive sputtering, chemical vapor deposition, plasma enhanced chemical vapor deposition, or electron cyclotron resonance source plasma enhanced chemical vapor deposition means. In one embodiment of the present application, the metal layer may be deposited by reactive sputtering.
[0064] The sealing film may have a structure in which the sealing layer is formed on a substrate film or a release film (hereinafter also referred to as a "first film"), and the sealing film is formed on the substrate or the release film. The structure may also include a substrate film, a protective film, or a release film (hereinafter also referred to as a "second film") formed on the metal layer.
[0065] The specific type of the first film that can be used in the present application is not particularly limited. In the present application, for example, a general polymer film in this field can be used as the first film. In the present application, for example, a polyethylene terephthalate film, a polytetrafluoroethylene film, a polyethylene film, a polypropylene film, a polybutene film, a polybutadiene film, a vinyl chloride copolymer film, a polyurethane film, an ethylene-vinyl acetate film, an ethylene-propylene copolymer film, an ethylene-ethyl acrylate copolymer film, an ethylene-methyl acrylate copolymer film, or a polyimide film can be used as the base material or release film. In addition, one or both sides of the base material film or release film of the present application may be subjected to an appropriate release treatment. Examples of the release agent used in the release treatment of the base material film include alkyd-based, silicone-based, fluorine-based, unsaturated ester-based, polyolefin-based, and wax-based release agents, and among these, from the viewpoint of heat resistance, it is preferable to use an alkyd-based, silicone-based, or fluorine-based release agent, but the present application is not limited thereto.
[0066] In the present application, the thickness of the base film or release film (first film) as described above is not particularly limited and can be appropriately selected depending on the application. For example, in the present application, the thickness of the first film may be about 10 μm to 500 μm, preferably about 20 μm to 200 μm. If the thickness is less than 10 μm, deformation of the base film may easily occur during the manufacturing process, and if it exceeds 500 μm, the economic efficiency is poor.
[0067] In a specific example of the present application, the sealing layer of the sealing film may be an extrusion product. In one example, the sealing layer may be formed by extruding the above-mentioned solvent-free sealing composition. An extrudate or extrusion product means a product in which the sealing composition is extruded, and the present application may produce a film or sheet-shaped sealing film by extrusion. The present application provides a solvent-free film that contains a large amount of moisture adsorbent compared to conventional films. Such a film may be provided through extrusion.
[0068] The present application relates to a method for producing a sealing film. In a specific example of the present application, the method for producing a sealing film may include a step of mixing the sealing resin and the moisture adsorbent in a single step to produce a solventless sealing composition. Here, mixing the sealing resin and the moisture adsorbent in a single step means that the sealing resin and the moisture adsorbent are added simultaneously, or are added and mixed successively immediately after the other one is added, or at least within 5 minutes, 3 minutes, or 100 seconds. That is, this is different from a process in which the moisture adsorbent is dissolved using a solvent or the like to produce a separate mixture, and the mixture in which the moisture adsorbent is dissolved is mixed with a resin or a solution in which a resin is dissolved to produce a sealing material composition.
[0069] One of the main challenges for OLED encapsulation films is to maximize moisture barrier properties and ensure long-term reliability. To ensure moisture barrier properties, the encapsulation film must contain a moisture adsorbent that can remove moisture and humidity that has permeated the encapsulation film. In particular, to maximize moisture barrier properties, the moisture adsorbent must be sufficiently dispersed within the composition. Here, "dispersed" refers to a state in which particles are not aggregated to form clumps, but are uniformly scattered, and if dispersion is good, each particle may be separated from the others.
[0070] Conventionally, in order to prepare an encapsulating composition, a method was adopted in which an encapsulating resin was dissolved in a solvent to prepare a solvent-type resin solution, and a mixture in which a moisture adsorbent was dispersed in a solvent using a dispersant was added to the resin solution to form a coating liquid containing a resin and a moisture adsorbent, and two or more steps were required to form the coating liquid. That is, in order to increase the dispersibility of the moisture adsorbent, a separate dispersant such as an organic acid had to be used, but due to the high viscosity characteristic of the coating liquid, there was a limit to improving the dispersibility of the moisture adsorbent even if a separate dispersant was used. Furthermore, when a mixture was formed using a solvent, even if a solvent drying process was performed afterwards, the solvent remained inside the film, and a problem occurred in which the organic electronic device was damaged due to the solvent that did not volatilize. Therefore, the present application provides an organic electronic device in which the dispersibility of the moisture adsorbent is maximized and long-term reliability can be effectively secured by preparing an encapsulating layer through extrusion as described below while using a solvent-free encapsulating composition by mixing an encapsulating resin and a moisture adsorbent in a single step.
[0071] In one embodiment, the step of preparing the encapsulating composition may be performed under high temperature conditions, for example, at a temperature of 50° C. or more and a pressure of 5 bar or more. The temperature may be higher than the melting point of the resin, for example, 60° C. or more, 70° C. or more, 80° C. or more, 90° C. or more, 100° C. or more, 110° C. or more, 120° C. or more, 125° C. or more, 130° C. or more, 135° C. or more, 140° C. or more, 145° C. or more, or 150° C. or more. The upper limit of the temperature may be appropriately adjusted to a temperature at which the components added to the encapsulating composition are not thermally decomposed, for example, 200° C. or less or 180° C. or less. The pressure may be 7 bar or more, 10 bar or more, 13 bar or more, 15 bar or more, 17 bar or more, or 20 bar or more. The upper limit of the pressure may be appropriately adjusted depending on the purpose, for example, 30 bar or less. As an example, but not limited thereto, the step of preparing the encapsulating composition may be performed by feeding the encapsulating composition into a kneader such as a kneader or a Banbury and kneading the composition, and the temperature of 50° C. or more and the pressure of 5 bar or more may be the temperature or pressure inside the kneader. In the present application, by performing the step of preparing the encapsulating composition at a specific temperature or more as described above, the components in the encapsulating composition are melt-kneaded, the dispersibility of the moisture adsorbent is further improved, the compatibility between the components in the composition is excellent, and the workability in the extrusion process is also excellent.
[0072] In one embodiment, the method for producing a seal film according to the present application may include a step of transferring the seal composition prepared in the step of preparing the seal composition to an extruder, compounding the compound, and extruding the compound at a temperature of 90° C. or more to prepare a seal layer.
[0073] The extrusion temperature in the step of preparing the sealing layer may refer to the internal temperature of the extruder or the molding temperature. Here, the internal temperature of the extruder may refer to the temperature in the section where the sealing composition transferred from the kneader to the extruder is blended while moving toward the discharge part by the screw in the extruder. In addition, the molding temperature refers to the temperature of the molding part attached to the discharge part of the extruder, and may refer to the temperature of the T-die, for example. The molding temperature may refer to the temperature in the section where the composition is discharged and molded into a film form by the molding part. That is, the sealing composition according to the present invention is first kneaded in a kneader to uniformly disperse the moisture adsorbent, and then transferred to an extruder, where it is secondarily kneaded by a screw installed inside the extruder, thereby further improving the dispersion degree of the moisture adsorbent.
[0074] As an example, but not limited thereto, the extruder may be a single screw extruder or a twin screw extruder, but a twin screw extruder is preferred because of its excellent productivity and uniformity. The type and rotation direction of the screw in the twin screw extruder can be appropriately selected depending on the components to be fed.
[0075] In one example, the temperature for producing the sealing layer by extrusion may be 100°C or more, 110°C or more, 120°C or more, 125°C or more, 130°C or more, 135°C or more, 140°C or more, 145°C or more, 150°C or more, 155°C or more, 160°C or more, 165°C or more, 170°C or more, 175°C or more, or 180°C or more, and the upper limit of the temperature may be appropriately adjusted to a temperature at which the components added to the sealing composition are not thermally decomposed, and may be 200°C or less or 180°C or less, for example. For example, the extruder internal temperature may be 140°C or more, and the molding temperature may be 150°C or more. Also, for example, the difference between the extruder internal temperature and the molding temperature may be within 50°C or 30°C. In the present application, the extruder internal temperature satisfies the above range, so that the moisture adsorbent can be uniformly dispersed in the sealing composition, and the molding temperature is controlled within the above range, so that the film properties can be improved.
[0076] In one example, the step of producing the encapsulating layer by extrusion is performed at a high pressure of 5 bar or more, and the viscosity of the encapsulating composition can be controlled within the range described below, thereby further improving the dispersibility of the moisture adsorbent. As an example, but not limited thereto, the pressure in the extrusion step may be 6 bar or more, 7 bar or more, 10 bar or more, 11 bar or more, 12 bar or more, 13 bar or more, 14 bar or more, 15 bar or more, 16 bar or more, 17 bar or more, 18 bar or more, or 20 bar or more, and the upper limit of the pressure may be appropriately adjusted depending on the purpose, and may be 30 bar or less, for example.
[0077] In one example, the rotation speed of the screw of the extruder may be within a range of 100 to 400 rpm, 150 to 350 rpm, 170 to 320 rpm, 200 to 300 rpm, or 230 to 270 rpm. In the present application, the moisture adsorbent can be uniformly dispersed in the sealing composition even in the case of a solventless type by using a strong shear force caused by the rotation of the screw in the extruder.
[0078] The method may further include a curing step of, for example, irradiating the extruded sealing layer with an electron beam or UV light. The electron beam or UV light may be irradiated by a known method.
[0079] The present application also relates to organic electronic devices. As shown in Fig. 3, the organic electronic device may include a substrate 31; an organic electronic element 32 formed on the substrate 31; and a sealing film 33 manufactured by the above-mentioned manufacturing method for sealing the organic electronic element 32. The sealing film may include a sealing layer 33, and may further include a metal layer 34. In this case, the sealing film including the sealing layer 33 and the metal layer 34 together can seal the organic electronic element 32. When the sealing film includes a metal layer, the organic electronic device may include the substrate 31, the organic electronic element 32, the sealing layer 33, and the metal layer 34 in that order.
[0080] For example, the encapsulation film may encapsulate the entire surface, for example, the top and sides, of the organic electronic element formed on the substrate. The encapsulation film may include an encapsulation layer containing a pressure-sensitive adhesive composition or an adhesive composition in a crosslinked or cured state. The encapsulation layer may be brought into contact with and sealed over the entire surface of the organic electronic element formed on the substrate to form an organic electronic device.
[0081] In a specific example of the present application, the organic electronic element may include a pair of electrodes, an organic layer including at least an emitting layer, and a passivation film. Specifically, the organic electronic element may include a first electrode layer, an organic layer formed on the first electrode layer and including at least an emitting layer, and a second electrode layer formed on the organic layer, and a passivation film on the second electrode layer that protects the electrode and the organic layer. The first electrode layer may be a transparent electrode layer or a reflective electrode layer, and the second electrode layer may also be a transparent electrode layer or a reflective electrode layer. More specifically, the organic electronic element may include a transparent electrode layer formed on a substrate, an organic layer formed on the transparent electrode layer and including at least an emitting layer, and a reflective electrode layer formed on the organic layer.
[0082] The organic electronic device may be, for example, an organic light emitting device.
[0083] The passivation film may include an inorganic film and an organic film. In one specific example, the inorganic film may be one or more metal oxides or nitrides selected from the group consisting of Al, Zr, Ti, Hf, Ta, In, Sn, Zn, and Si. The thickness of the inorganic film may be 0.01 μm to 50 μm, 0.1 μm to 20 μm, or 1 μm to 10 μm. In one example, the inorganic film of the present application may be an inorganic material that does not contain a dopant, or an inorganic material that contains a dopant. The dopant that can be doped may be, but is not limited to, one or more elements selected from the group consisting of Ga, Si, Ge, Al, Sn, Ge, B, In, Tl, Sc, V, Cr, Mn, Fe, Co, and Ni, or oxides of the elements. The organic film is distinguished from the organic layer that includes at least the above-mentioned light-emitting layer in that it does not include a light-emitting layer, and may be an organic deposition layer that includes an epoxy compound.
[0084] The inorganic film or organic film may be formed by chemical vapor deposition (CVD). For example, the inorganic film may use silicon nitride (SiNx). In one example, silicon nitride (SiNx) used as the inorganic film may be deposited to a thickness of 0.01 μm to 50 μm. In one example, the thickness of the organic film may be within a range of 2 μm to 20 μm, 2.5 μm to 15 μm, or 2.8 μm to 9 μm.
[0085] The present application also provides a method for manufacturing an organic electronic device. The method may include applying an encapsulation film obtained by the method to a substrate having an organic electronic device formed thereon so as to cover the organic electronic device. The method may also include curing the encapsulation film. The curing step of the encapsulation film may refer to the curing of an encapsulation layer and may be performed before or after the encapsulation film covers the organic electronic device.
[0086] As used herein, the term "curing" may mean that the adhesive composition of the present invention forms a crosslinked structure through a heating or UV irradiation process, and is prepared in the form of an adhesive, or that the adhesive composition is solidified and attached as an adhesive.
[0087] Specifically, an electrode is formed on a glass or polymer film used as a substrate by a method such as vacuum deposition or sputtering, and a layer of a light-emitting organic material composed of, for example, a hole transport layer, a light-emitting layer, and an electron transport layer is formed on the electrode, and then an electrode layer is further formed thereon to form an organic electronic device. Next, the entire surface of the organic electronic device on the substrate that has undergone the above process is positioned so that it is covered with the sealing layer of the sealing film. Effect of the Invention
[0088] The present application provides an encapsulation film capable of forming a structure capable of blocking moisture or oxygen from entering an organic electronic device from the outside, thereby ensuring long-term reliability of the organic electronic device.
[0089] However, the effects of the present invention are not limited to those mentioned above, and other effects not mentioned will be clearly understood by those skilled in the art from the following description. [Brief description of the drawings]
[0090] [Figure 1] FIG. 1 is a cross-sectional view of an encapsulation layer according to one example of the present application. [Diagram 2] FIG. 2 is a cross-sectional view showing the sealing film. [Diagram 3] FIG. 3 is a cross-sectional view of an organic electronic device according to one example of the present application. [Figure 4] FIG. 4 is a graph showing Gaussian curve fitting according to the first embodiment. [Diagram 5] FIG. 5 is a graph showing Gaussian curve fitting according to the second embodiment. [Figure 6] FIG. 6 is a graph showing Gaussian curve fitting according to the third embodiment. [Figure 7] FIG. 7 is a graph showing Gaussian curve fitting according to Comparative Example 1. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0091] The present invention will be described in more detail below based on examples according to the present invention and comparative examples not according to the present invention, but the scope of the present invention is not limited to the examples presented below.
[0092] Example 1 100 parts by weight of butyl rubber resin (Mw: 410,000 g / mol, glass transition temperature: -65°C), 100 parts by weight of tackifier resin (SU525, softening point: 125°C, Kolon), 3 parts by weight of multifunctional acrylate (tricyclodecane dimethanol diacrylate, Miwon), 1 part by weight of photoinitiator (Irgacure 651, Ciba), and 200 parts by weight of CaO were added to a pressure kneader set at 150°C and 20 bar, and then melt-kneaded for 30 minutes, and then heated at 170°C and 50 s. -1 A sealing composition was produced with a viscosity of 1500 Pa·s at a shear rate. The sealing composition was transferred to a twin-screw extruder (TEK30, SM Platek) set at a temperature of 180° C. and a screw rotation speed of 250 rpm, compounded, and extruded at a temperature of 160° C. and a pressure of 20 bar using a T-die attached to the twin-screw extruder to produce a film-shaped sealing layer with a thickness of 50 μm. 2 The film was irradiated with ultraviolet light to produce a sealing film.
[0093] Example 2 A film was produced in the same manner as in Example 1, except that the T-die temperature was set to 170°C.
[0094] Example 3 A film was produced in the same manner as in Example 1, except that the T-die temperature was set to 180°C.
[0095] Example 4 A film was prepared in the same manner as in Example 1, except that the sealing composition contained Kristalex F115 (softening point: 115° C.) from EASTman as a tackifier.
[0096] Comparative Example 1 A film was produced in the same manner as in Example 1, except that the T-die temperature was set to 150°C.
[0097] Comparative Example 2 100 parts by weight of butyl rubber resin (Mw: 410,000 g / mol), 100 parts by weight of tackifier resin (SU525, softening point: 125°C, Kolon), 3 parts by weight of multifunctional acrylate (tricyclodecane dimethanol diacrylate, Miwon), 1 part by weight of photoinitiator (Irgacure 651, Ciba), and 200 parts by weight of CaO were blended in 600 parts by weight of toluene and thoroughly mixed to prepare a solution with a solid content of 40 wt%. The solution was coated onto a release PET sheet, dried in an oven at 120°C, and then subjected to a pressure of 1.5 J / cm 2 The film was irradiated with ultraviolet light to produce a sealing film.
[0098] Comparative Example 3 A sealing layer was prepared in the same manner as in Example 1, except that the moisture adsorbent was contained at 80 parts by weight.
[0099] Experimental example 1: σ in Gaussian curve fitting The Gaussian curve fitting is for the distribution of the moisture adsorbent in the thickness (depth) direction of the encapsulation layer, where the x-axis is the thickness of the encapsulation layer, and the f(x) function is as shown in Equation 1 below.
[0100]
number
[0101] where A and b are constants related to the absolute amount of moisture adsorbent,
number
[0102] 4 to 7 are diagrams showing graphs by Gaussian curve fitting according to Example 1, Example 2, Example 3 and Comparative Example 1, respectively.
[0103] Experimental Example 2: Measurement of gel content The sealing films of the examples and comparative examples were prepared into test pieces with a size of 50 mm x 50 mm, and 0.3 to 0.4 g of the sealing film (initial weight: A) was taken from each sealing film test piece, and the sealing film was immersed in 70 g of toluene at 60 ° C for 3 hours. After that, the gel part was filtered through a 200 mesh wire net (weight of wire net: M) and then dried in an oven at 125 ° C for 1 hour. After measuring the weight (G) of the gel and the wire net, the gel content (unit: %) was calculated using the dry mass (B = GM) of the insoluble part of the sealing film that did not pass through the net according to the following general formula 1.
[0104] [General formula 1] Gel content (unit: %) = (B / A) x 100
[0105] In the general formula 1, A represents the initial mass of the sealing film test piece, and B represents the dry mass of the insoluble portion of the sealing film that does not pass through a 200 mesh (pore size 200 μm) net after immersing the sealing film test piece in 70 g of toluene at 60° C. for 3 hours and then filtering the same through a 200 mesh (pore size 200 μm) net.
[0106] Experimental Example 3: Measurement of swelling index A certain amount of the sealing film according to the embodiment or comparative example was placed in a bottle, filled with toluene, and stored for 24 hours to obtain a sol-gel solution. After that, the weight (X) of the gel sample was measured immediately after separating it from the sol-gel solution using a 200 mesh (pore size 200 μm). The obtained gel sample was dried in an oven at 80° C. for 12 hours, and the weight (Y) of the gel sample immediately after drying was measured. The swelling index was calculated using the above values according to the following general formula 2.
[0107] [General formula 2] Swelling index = weight of gel sample immediately after separation from sol-gel solution (X) / weight of gel sample immediately after drying (Y)
[0108] Experimental Example 4: Measurement of storage modulus The sealing films according to the examples and comparative examples were laminated to a thickness of 600 μm to obtain test pieces, and the test pieces were measured using parallel plates in the Temp Sweep mode of ARES (Advanced Rheometric Expansion System, ARES-G2 manufactured by TA Corp.). Specifically, the storage modulus was measured after applying a deformation of 15.0 rad / s at a deformation rate (strain) of 0.1% in the temperature range of 30 to 100°C, and the value at a temperature of 50°C was shown.
[0109] Experimental example 5: Moisture permeability The sealing films of the examples and comparative examples, each measuring 30 mm×60 mm, were left in a constant temperature and humidity chamber at a temperature of 85° C. and a relative humidity of 85%, respectively, for 895 hours, and the distance through which moisture had penetrated was measured using a microscope.
[0110] Experimental Example 6: Metal Adhesion The sealing films according to the examples and comparative examples were thermally laminated at 75°C on a Cu surface measuring 200mm x 220mm, cut to 25mm, and then further laminated on the Cu surface using a 2Kg roller to prepare a test specimen. The test specimen was left for 30 minutes in a constant temperature and humidity room at 22±5°C and 50±10%, and then fixed to a tensile machine (TA, Texture Analyser) and measured in Tension Mode at a temperature of 25°C and a tensile speed of 5mm / min.
[0111] The following Table 1 summarizes the results of the above-mentioned experimental examples for the sealing films produced in the examples and comparative examples.
[0112] [Table 1] [Explanation of symbols]
[0113] 1. Sealing film 11 Sealing layer 12 Base material layer 21, 23 1st or 3rd Zone 22 Second area 3 Organic electronic devices 31 Substrate 32 Organic Electronic Devices 33 Sealing layer 34 Metal Layer
Claims
1. The sealing layer is a cured product of the sealing composition, The encapsulating composition includes an encapsulating resin and a moisture adsorbent, The sealing layer is a single layer, and is a sealing film including a first region, a second region, and a third region in which the concentration of the moisture adsorbent differs depending on the thickness direction.
2. The seal film of claim 1 comprising, in order, a first region, a second region and a third region.
3. The encapsulation film of claim 1 , wherein the second region has a higher moisture adsorbent content than the first and third regions.
4. The encapsulating film according to claim 1 , wherein a position distribution (σ value) of the moisture adsorbent in the thickness direction in Gaussian curve fitting of the moisture adsorbent in the thickness direction in the encapsulating layer is 2 or less.
5. The sealing film according to claim 1 , wherein the sealing composition is a solvent-free type.
6. The sealing film according to claim 1 , having a metal adhesion strength of 4,000 gf / in or more.
7. The sealing film according to claim 1 , wherein the sealing resin comprises an olefin-based resin.
8. The sealing film according to claim 1 , wherein the sealing resin is contained in the sealing material in an amount of 10% by weight or more.
9. The sealing film of claim 1 , wherein the moisture adsorbent is a chemically reactive adsorbent.
10. The sealing film according to claim 1 , wherein the moisture adsorbent is contained in an amount of 90 parts by weight or more based on 100 parts by weight of the sealing resin.
11. The sealing film of claim 1 , wherein the sealing composition further comprises a tackifier.
12. The sealing film according to claim 11, wherein the tackifier is contained in the range of 15 to 200 parts by weight per 100 parts by weight of the sealing resin.
13. The sealing film according to claim 1 , wherein the sealing composition further comprises an active energy ray-polymerizable compound.
14. The sealing film according to claim 13, wherein the active energy ray polymerizable compound is contained in a range of 0.5 to 10 parts by weight based on 100 parts by weight of the sealing resin.
15. The sealing film of claim 1 , wherein the sealing composition further comprises a radical initiator.
16. The sealing film according to claim 1, wherein the sealing layer has a gel content of 60% or more as measured by the following general formula 1: [General formula 1] Gel content (%) = A / B x 100 In the general formula 1, B is the mass of the sealing layer sample, and A is the dry mass of the insoluble portion of the sealing layer that does not pass through a 200 mesh screen after the sample is immersed in toluene at 60°C for 24 hours and then filtered through a 200 mesh screen.
17. The sealing composition was heated at 170° C. for 50 s -1 The seal film according to claim 1, having a viscosity measured at shear rate in the range of 1,000 to 2,000 Pa·s.
18. The seal film of claim 1 , wherein the seal layer is an extrusion.
19. The encapsulating film of claim 1 further comprising a metal layer.
20. The method of claim 1 comprising extruding a sealing composition to produce a sealing layer.
21. The method for producing an encapsulating film according to claim 20, wherein the encapsulating composition is produced by mixing the encapsulating resin and the moisture adsorbent in a single step.
22. The method of claim 20, wherein the step of preparing the sealing composition is performed at a temperature of 50° C. or more and a pressure of 5 bar or more.
23. The method of claim 20, wherein the extruding step of producing the sealing layer is performed at a pressure of 5 bar or more.
24. An organic electronic device comprising: a substrate; an organic electronic element formed on the substrate; and the encapsulation film according to claim 1 encapsulating an entire surface of the organic electronic element.
25. 13. A method for manufacturing an organic electronic device, comprising: applying the encapsulation film of claim 1 to a substrate having an organic electronic device formed thereon so as to cover the organic electronic device.
Citation Information
Patent Citations
Organic electroluminescent device and method for manufacturing the same
JP2015133260A
encapsulant film
JP2016509335A
Adhesive Film and Method for Manufacturing Organic Electronic Device Using the Same
JP2016531980A
Seal components
JP2021508348A
Organic el device
WO2015136581A1