Positive electrode material for sodium ion batteries, its manufacturing method, and applications

The production method for a sodium ion battery electrode material enhances conductivity and energy density by coating sodium vanadate and carbon on a polyanionic sodium manganese iron borate core, addressing the limitations of current sodium ion batteries and reducing costs.

JP2024536426AActive Publication Date: 2024-10-04HUBEI WANRUN NEW ENERGY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024521068
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-07-29
Filing Date
2023-07-27
Publication Date
2024-10-04
Estimated Expiration
2043-07-27

AI Technical Summary

Technical Problem

Current sodium ion batteries face issues with low energy density, poor cycle performance, and high cost due to the use of materials like lithium iron phosphate, which are scarce and expensive.

Method used

A method for producing a positive electrode material for sodium ion batteries involves polishing a mixture of sodium borohydride and ferromanganese hydroxide, followed by spray drying and firing, and then coating with sodium vanadate and carbon to enhance conductivity and form a protective layer, resulting in a polyanionic sodium manganese iron borate core.

Benefits of technology

The method improves ionic and electronic conductivity, increases energy density, and reduces production costs, making it comparable to lithium iron phosphate while offering better cycle performance and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536426000001_ABST
    Figure 2024536426000001_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of sodium ion batteries, in particular to a cathode material for sodium ion batteries and its manufacturing method and application. The cathode material for sodium ion batteries of the present invention includes the steps of (A) grinding a mixture of sodium borohydride and ferromanganese hydroxide to obtain a first slurry, which is spray-dried and calcined to obtain a first calcined product, and (B) grinding a mixture of the first calcined product, a carbon source, a vanadium source, sodium bicarbonate and water to obtain a second slurry, which is spray-dried, calcined, crushed, sieved and iron-removed in order to obtain the cathode material for sodium ion batteries. The method has simple steps and low cost, and the produced cathode material for sodium ion batteries has the characteristics of good conductivity, high capacity, high energy density and the like.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS-REFERENCE TO RELATED APPLICATIONS) This application claims priority to a Chinese patent application bearing application number 202210905141.2 and entitled "Positive electrode material for sodium ion batteries and its manufacturing method and application" filed with the China Patent Office on July 29, 2022, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to the technical field of sodium ion batteries, and in particular to a positive electrode material for sodium ion batteries and its manufacturing method and application. [Background technology]

[0003] The explosive growth in automobile production capacity has led to a rise in the price of lithium resources, and in addition to lithium, another rare metal, cobalt (Co), is also used in lithium batteries. Research has shown that it takes about 20 kg of lithium and about 40 kg of cobalt to manufacture one pure electric vehicle (EV) using current technology. Scarce energy sources such as lithium and cobalt will inevitably face resource depletion and price increases. Sodium, the second lightest metallic element after lithium, is present in an amount of 2.3-2.8%, 4-5 orders of magnitude more than lithium, and has physicochemical properties similar to those of lithium; therefore, sodium-ion batteries have attracted widespread attention.

[0004] As early as the 1970s and 1980s, sodium-ion batteries, known as "post-lithium batteries," were proposed and put into practical use almost simultaneously with lithium-ion batteries. However, as the commercialization of lithium-ion batteries became more successful, research into sodium-ion batteries gradually became less important.

[0005] At that time, the electrode materials that had been successfully applied to lithium-ion batteries were simply applied to sodium-ion batteries without considering the difference in requirements for the material lattice structure between sodium-ion batteries and lithium-ion batteries, resulting in low performance of sodium-ion batteries. In recent years, the shortage of lithium resources due to the large-scale application of lithium-ion batteries has been gradually recognized, and the electrode materials have been fully designed based on the characteristics of sodium-ion batteries to achieve better performance, so that sodium-ion batteries have once again become a research hotspot.

[0006] At present, layered sodium oxide battery materials have the advantage of high energy density, but poor cycle performance. Prussian blue structure sodium battery materials have too low energy density, unstable structure, and toxic and harmful raw materials. Polyanionic sodium battery materials have the advantages of stable structure and long cycle life, but generally have low capacity and low energy density.

[0007] In view of this, the present invention is proposed. Summary of the Invention [Means for solving the problem]

[0008] A first object of the present invention is to provide a method for preparing a positive electrode material for a sodium ion battery, which involves simple steps, is low cost, and provides the prepared positive electrode material for a sodium ion battery with good electrical conductivity, high capacity, high energy density and other characteristics.

[0009] A second object of the present invention is to provide a positive electrode material for a sodium ion battery produced by the above-mentioned method for producing a positive electrode material for a sodium ion battery.

[0010] A third object of the present invention is to provide a sodium ion battery including the above-mentioned positive electrode material for a sodium ion battery.

[0011] In order to achieve the above objectives of the present invention, in particular, the following technical solutions are adopted: The present invention provides a method for producing a cathode material for a sodium ion battery, the method comprising the steps of: (A) grinding a mixture of sodium borohydride and ferromanganese hydroxide to obtain a first slurry, which is then spray-dried and calcined to obtain a first calcined product; (B) grinding a mixture of the first fired product, a carbon source, a vanadium source, sodium bicarbonate, and water to obtain a second slurry, which is then spray-dried, fired, pulverized, sieved, and iron-removed in that order to obtain the sodium-ion battery positive electrode material.

[0012] The present invention further provides a positive electrode material for a sodium ion battery produced by the above-mentioned method for producing a positive electrode material for a sodium ion battery.

[0013] The present invention further provides a sodium ion battery comprising the above-mentioned positive electrode material for sodium ion batteries. Effect of the Invention

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: In the manufacturing method of the positive electrode material for sodium ion batteries provided by the present invention, by doping with metal ions and coating with sodium vanadate and carbon, the ionic conductivity and electronic conductivity can be significantly improved, and the primary particle size of the positive electrode material for sodium ion batteries can be appropriately increased, thereby improving the compaction density and the resistance to oxygen and moisture. The energy density of the positive electrode material for sodium ion batteries thus manufactured is close to that of lithium iron phosphate material, reaching 170wh / kg, and the cost is also lower than that of lithium iron phosphate material.

[0015] The positive electrode material for sodium ion batteries produced by the method for producing a positive electrode material for sodium ion batteries of the present invention has a polyanionic sodium battery material, i.e., sodium iron manganese borate, as a core, and the surface of the polyanionic sodium battery material is simultaneously coated with sodium vanadate and carbon to form a single protective layer, which can protect the polyanionic sodium battery with sodium vanadate as the core from contact with oxygen and moisture, and is helpful in improving ionic conductivity, electronic conductivity, capacity and cycle performance, and carbon can further improve electronic conductivity, so that the positive electrode material for sodium ion batteries has excellent electrochemical performance. [Brief description of the drawings]

[0016] In order to more clearly describe the specific embodiments of the present invention or the technical solutions of the prior art, the following briefly introduces drawings necessary for describing the specific embodiments or the prior art. Obviously, the drawings described below are only some embodiments of the present invention, and those skilled in the art can obtain other drawings based on these drawings without creative efforts. [Figure 1] 1 is a SEM image of ferromanganese (II) hydroxide prepared in Example 1 of the present invention. [Diagram 2] 1 is a SEM image of a first fired product prepared in Example 1 of the present invention. [Diagram 3] 1 is a SEM image of the spray material prepared in Example 1 of the present invention. [Figure 4] 1 is a SEM image of the positive electrode material for a sodium ion battery prepared in Example 1 of the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing the relationship between the capacity retention rate and the number of cycles of the positive electrode material for a thorium ion battery produced in Example 1 of the present invention. [Figure 6] 2 is a charge / discharge curve graph of the positive electrode material for a thorium ion battery prepared in Example 1 of the present invention; [Figure 7] FIG. 2 is a schematic diagram of the DC resistance at 50% remaining capacity of the positive electrode material for a thorium ion battery produced in Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The following provides a clear and complete description of the technical solutions of the present invention in combination with drawings and specific embodiments. Those skilled in the art should understand that the embodiments described below are only some of the embodiments of the present invention, but not all of the embodiments, and are only for illustrating the present invention, and should not be regarded as limiting the scope of the present invention.

[0018] Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without any creative effort belong to the scope of protection of the present invention. If no specific conditions are shown in the embodiments, they shall follow the conventional conditions or the conditions recommended by the manufacturers. Reagents or equipment without the manufacturer's name are all conventional products available on the market.

[0019] Hereinafter, the positive electrode material for a sodium ion battery according to the embodiment of the present invention, its manufacturing method, and applications will be specifically described.

[0020] In some embodiments of the present invention, a method for producing a cathode material for a sodium-ion battery is provided, the method comprising the steps of: (A) grinding a mixture of sodium borohydride and ferromanganese hydroxide to obtain a first slurry, which is then spray-dried and calcined to obtain a first calcined product; (B) grinding a mixture of the first fired product, a carbon source, a vanadium source, a sodium source, and water to obtain a second slurry, which is then spray-dried, fired, pulverized, sieved, and iron-removed in that order to obtain a positive electrode material for a sodium ion battery.

[0021] In the method for producing a positive electrode material for a sodium ion battery provided by the present invention, sodium borohydride and ferromanganese (II) hydroxide are used to produce a first calcined product, i.e., sodium iron manganese borate (Na(Fe,Mn)BO3), and sodium borohydride is used as a boron source and a sodium source, and sodium borohydride is used as a reducing agent, thereby: The oxidation of manganese ions and ferrous ions can be avoided, high purity sodium manganese ferrous borate can be obtained, and uniform doping of ferromanganese can be achieved. Then, the prepared sodium manganese ferrous borate is mixed with components such as a carbon source, a vanadium source, and a sodium source, and then polished, spray-dried, and calcined. Then, the surface of the sodium manganese ferrous borate is simultaneously coated with sodium vanadate and carbon to form a protective layer. The sodium vanadate coated on the surface of the sodium manganese ferrous borate can protect the polyanionic sodium battery core from contact with oxygen and moisture. At the same time, the sodium vanadate has the characteristics of good ionic conductivity and electronic conductivity, high capacity, and excellent cycle performance. The carbon coated on the surface of the polyanionic sodium battery material can further improve the electronic conductivity, so that the prepared sodium ion battery positive electrode material has excellent electrochemical performance.

[0022] In the manufacturing method of the positive electrode material for sodium ion batteries provided by the present invention, the voltage platform, ionic conductivity and electronic conductivity can be improved by doping manganese and coating with sodium vanadate and carbon, and the primary particle size of the positive electrode material for sodium ion batteries can be appropriately increased, thereby improving the compaction density and further improving the resistance to oxygen and moisture. The positive electrode material for sodium ion batteries manufactured by this method has the characteristics of high capacity and high energy density, and its energy density is close to that of lithium iron phosphate material, and its cost is also significantly reduced compared with lithium iron phosphate material.

[0023] Calculated based on the current prices of various raw materials, the raw material cost, energy consumption, equipment depreciation cost and labor cost of the sodium ion battery positive electrode material of the present invention is about 39,500 yuan / ton in total, while the raw material cost, energy consumption, equipment depreciation cost and labor cost of the lithium iron phosphate material are about 132,000 yuan / ton in total, and the production cost of the sodium ion battery positive electrode material of the present invention is significantly lower than the production cost of the lithium iron phosphate material.

[0024] In some embodiments of the present invention, in step (A), the firing includes heating to 400-500°C in a nitrogen atmosphere, maintaining the temperature for 4-5 hours, then heating to 650-700°C and maintaining the temperature for 3-5 hours, and then cooling to 120°C or lower. Preferably, the relative humidity during firing is 3%-5%.

[0025] In some specific embodiments of the present invention, in step (A), the firing includes heating in a nitrogen atmosphere to 400-500°C at a rate of 1-3°C / min and maintaining the temperature for 4-5 hours, then heating to 650-700°C at a rate of 1-3°C / min and maintaining the temperature for 3-5 hours, and then cooling to 120°C or less at a rate of 1-3°C / min to finish.

[0026] In the manufacturing method of the sodium ion battery positive electrode material of the present invention, in the above-mentioned calcination process, nitrogen having a certain humidity is used as a protective gas and a reactant, which can react with sodium borohydride to obtain a reducing gas, thereby protecting manganese ions and ferrous ions from being oxidized.

[0027] In some embodiments of the present invention, in step (A), a mixture of sodium borohydride and ferromanganese hydroxide is ground to obtain a first slurry. Preferably, the concentration of the aqueous sodium borohydride solution is 1 to 1.5 mol / L.

[0028] In some embodiments of the present invention, in step (A), the ratio of the sum of the moles of Fe and Mn in the ferromanganese hydroxide (II) to the moles of Na in the sodium borohydride is 0.97 to 1.02:1, and is typical but not limiting, for example, the ratio of the sum of the moles of Fe and Mn in the ferromanganese hydroxide (II) to the moles of Na in the sodium borohydride is 0.97:1, 0.98:1, 0.99:1, 1:1, 1.01:1, or 1.02:1, etc.

[0029] In some embodiments of the present invention, in step (A), the particle size of the first slurry is 200-300 nm, typically but not limited to, for example, in step (A), the particle size of the first slurry is 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, or 300 nm.

[0030] In some embodiments of the present invention, in step (A), the method for producing ferromanganese (II) hydroxide comprises: The method includes reacting a manganese salt, a ferrous salt, a complexing agent, sodium hydroxide, hydrazine hydrate, aqueous ammonia, and titanyl sulfate in an aqueous phase to obtain ferric manganese (II) hydroxide.

[0031] The present invention can prepare ferromanganese hydroxide with uniform co-precipitation of ferromanganese by co-precipitation, and then react with sodium borohydride to achieve uniform doping of ferromanganese, thereby avoiding the separate presence of sodium manganese borate concentrate at certain points, which would cause capacity reduction.

[0032] In some embodiments of the present invention, in the method for producing ferromanganese (II) hydroxide, the reaction temperature is 50 to 60° C., and the reaction time is 15 to 150 minutes.

[0033] In some embodiments of the present invention, in the method for producing ferromanganese hydroxide, the molar ratio of Mn in the manganese salt to Fe in the ferrous salt is 1:1.5-4, including, but not limited to, typical but non-limiting examples of the molar ratio of Mn in the manganese salt to Fe in the ferrous salt are 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, or 1:4.

[0034] In some embodiments of the present invention, in the method for producing ferromanganese hydroxide, the ratio of the sum of the moles of Mn in the manganese salt and Fe in the ferrous salt to the number of moles of Ti in titanyl sulfate is 100:0.1-0.2.

[0035] In some embodiments of the present invention, in the method for producing ferromanganese hydroxide, the molar ratio of manganese salt, complexing agent, sodium hydroxide, hydrazine hydrate and NH3·H2O in ammonia water is 1:0.01-0.1:5.5-10.5:0.01-0.1:0.05-0.5.

[0036] In some embodiments of the present invention, in the method for producing ferromanganese hydroxide, the ratio of the sum of the mass of the manganese salt, the ferrous salt, the complexing agent, the sodium hydroxide, the hydrazine hydrate, the aqueous ammonia, and the titanyl acid to the mass of water is 10:1.5-3.

[0037] In some embodiments of the present invention, the method for producing ferromanganese hydroxide includes at least one of manganese sulfate, manganese chloride, and manganese acetate, the ferrous salt includes at least one of ferrous sulfate, ferrous chloride, and ferrous acetate, and the complexing agent includes at least one of ethylenediaminetetraacetic acid (EDTA), disodium ethylenediaminetetraacetate, sodium hexametaphosphate, and triethanolamine.

[0038] In some specific embodiments of the present invention, in the method for producing ferromanganese (II) hydroxide, the concentration of aqueous ammonia is 5 to 8 mol / L.

[0039] In some specific embodiments of the present invention, the method for producing ferromanganese(II) hydroxide comprises the steps of: The method includes the steps of slowly adding a mixed solution of manganese salt, ferrous salt, complexing agent, sodium hydroxide, hydrazine hydrate, ammonia water, titanyl sulfate and water to a reaction kettle, making the pH of the mixed solution 9.5-10, controlling the temperature at 50°C during the addition, and continuing the reaction at 50-60°C for 15-30 min after the addition is completed, and controlling the concentration of free ammonia in the mixed solution to 8-12 g / L during the reaction. During the reaction, the reaction occurs, and ammonia water and metal ions precipitate, resulting in ammonium radicals that are not free ammonia, and at the same time, part of the ammonia also volatilizes, so it is necessary to constantly adjust the amount of ammonia water added to adjust the free ammonia in the solution.

[0040] In some embodiments of the present invention, in step (B), the vanadium source comprises ammonium metavanadate.

[0041] In some embodiments of the present invention, in step (B), the sodium source comprises at least one of sodium bicarbonate, sodium hydroxide, sodium acetate, and sodium nitrate, preferably, the sodium source comprises sodium bicarbonate.

[0042] In some embodiments of the present invention, in step (B), the carbon source comprises nano-hydrophilic graphite and / or polyethylene glycol, and preferably, the mass ratio of nano-hydrophilic graphite to polyethylene glycol is 1:5-10.

[0043] In the method for preparing a positive electrode material for a sodium ion battery provided by the present invention, an inorganic carbon source is introduced before calcination in step (B), which can greatly improve the conductivity of the coating layer. Conventional carbon obtained by pyrolysis of an organic carbon source is amorphous carbon with a very low degree of graphitization and a lower conductivity than graphitized carbon, but in the present invention, an inorganic carbon source is directly introduced, and polyethylene glycol is added at the same time to achieve dispersion, and polyethylene glycol is also pyrolyzed in the secondary calcination process to obtain carbon, thereby realizing the composite of the inorganic carbon source and the organic carbon source, and the organic carbon source forms a carbon network to bond with the inorganic carbon source, thereby solving the problem of non-uniform coating of the inorganic carbon source in the coating layer.

[0044] In some embodiments of the present invention, in step (B), the molar ratio of sodium in the first calcined product, vanadium in the vanadium source, and sodium in the sodium source is 1:0.02-0.03:0.06-0.09.

[0045] In some embodiments of the present invention, in step (B), the mass ratio of the carbon source to the first calcined product is 3 to 10:100, and preferably the mass ratio of the carbon source to the first calcined product is 5 to 8:100.

[0046] In some embodiments of the present invention, in step (B), the ratio of the total mass of the first calcined product, the carbon source, the vanadium source and the sodium source to the mass of water is 1:2-3.

[0047] In some embodiments of the present invention, in step (B), the firing comprises increasing the temperature to 720-750°C in a nitrogen atmosphere, maintaining the temperature for 2-4 hours, and then cooling to 80°C or lower. Preferably, in step (B), the firing comprises increasing the temperature to 720-750°C at a rate of 1-3°C / min in a nitrogen atmosphere, maintaining the temperature for 2-4 hours, and then cooling to 80°C at a rate of 1-3°C / min.

[0048] In some embodiments of the present invention, in step (B), the particle size of the second slurry is 100 to 200 nm.

[0049] In some embodiments of the present invention, in step (B), the particle size of the second slurry after spray drying is 5-10 μm, and preferably, a pressurized spray dryer is used for spray drying.

[0050] In some embodiments of the present invention, in step (B), the pulverization includes pulverization by an airflow pulverizer, and preferably, the pulverization is performed until the particle size of the second slurry after spray drying is 0.5 to 2 μm, more preferably, the pulverization temperature is 120 to 150° C., the pulverization pressure is 0.25 to 0.5 MPa, and the pulverization includes pulverization in a nitrogen atmosphere.

[0051] In some embodiments of the present invention, in step (B), sieving includes sieving with an ultrasonic vibrating sieve of 100 to 200 mesh.

[0052] In some embodiments of the present invention, in step (B), removing iron comprises removing iron using an electromagnetic iron remover to ≦1 ppm of magnetic material in the second slurry after milling.

[0053] In some embodiments of the present invention, there is also provided a positive electrode material for a sodium ion battery produced by the above-mentioned method for producing a positive electrode material for a sodium ion battery.

[0054] In some embodiments of the present invention, the primary particle size of the sodium ion battery positive electrode material is 150 to 250 nm.

[0055] The positive electrode material for a sodium ion battery of the present invention is configured so that it has layered oxide sodium vanadate and carbon on the surface and a polyanionic sodium battery material as the core, and the surface of the polyanionic sodium battery material is coated with sodium vanadate and carbon to form a single protective layer.

[0056] In some embodiments of the present invention, a sodium-ion battery including the above-described sodium-ion battery positive electrode material is also provided.

[0057] Example 1 The method for preparing a positive electrode material for a sodium ion battery provided by this embodiment includes the following steps: (A) A 1.3 mol / L aqueous solution of sodium borohydride is mixed with ferromanganese (II) hydroxide, and the mixture is added to a sand mill for sanding to obtain a first slurry having a particle size of 252 nm. The first slurry is then spray-dried, and in nitrogen with a relative humidity of 4.1%, the mixture is first heated to 450°C at a rate of 3°C / min and kept at that temperature for 5 hours, then heated to 680°C at a rate of 2°C / min and kept at that temperature for 4 hours, and then cooled to 120°C at a rate of 3°C / min, and finished to obtain a first fired product.

[0058] Here, the ratio of the sum of the moles of Mn and Fe in ferromanganese(II) hydroxide to the moles of sodium borohydride is 1.01:1.

[0059] The method for producing ferromanganese (II) hydroxide is as follows: a mixture of manganese sulfate, ferrous sulfate, EDTA, sodium hydroxide, ammonia water (concentration: 6 mol / L), hydrazine hydrate, titanyl sulfate and deionized water is added to a reaction vessel, and the molar ratio of NH3·H2O in manganese sulfate, ferrous sulfate, EDTA, sodium hydroxide, hydrazine hydrate and ammonia water is 1:2.52:0.05:7.58:0.04:0.18, and the molar sum of Mn in manganese sulfate and Fe in ferrous sulfate and the molar sum of Fe in titanyl sulfate are 1:2.52:0.05:7.58:0.04:0.18. The molar ratio of Ti is 100:0.2, the addition time is 95 min, the pH of the mixed solution during addition is 9.76, the stirring speed is 500 r / min, the temperature is 55°C, after the addition is completed, the reaction is continued at 55°C for 25 min to obtain a reaction solution, and the concentration of free ammonia in the solution is controlled at 10 g / L during the reaction; the reaction solution is filtered to obtain a filter cake, which is washed with 0.015 mol / L hydrazine hydrate and dried in a vacuum oven to obtain ferromanganese(II) hydroxide.

[0060] (B) The first fired product, carbon source, ammonium metavanadate, sodium bicarbonate and water are mixed and added to a sand mill for sanding to obtain a second slurry with a particle size of 183 nm. The second slurry is spray-dried using a pressurized spray dryer to obtain a spray material with a particle size of 8.7 μm. In a nitrogen atmosphere, the spray material is first heated to 735°C at a rate of 3°C / min and kept at that temperature for 3 hours, then cooled to 80°C at a rate of 3°C / min, and finished to obtain a second fired product. The second fired product is pulverized at 145°C in a nitrogen atmosphere at a pressure of 0.35 MPa until the particle size of the second fired product is 1.2 μm. Next, iron is removed using a 150-mesh ultrasonic vibrating sieve and then an electromagnetic iron removal device until the magnetic material in the second fired product is 0.21 ppm, and the product is vacuum-packed to obtain a positive electrode material for a sodium-ion battery.

[0061] Here, the carbon source is nano-hydrophilic graphite and polyethylene glycol in a mass ratio of 1:7, the molar ratio of sodium in the first fired product, vanadium in ammonium metavanadate, and sodium bicarbonate is 1:0.025:0.08, the mass ratio of the carbon source to the first fired product is 6:100, and the ratio of the total mass of the first fired product, the carbon source, ammonium metavanadate, and sodium bicarbonate to the mass of water is 1:2.5.

[0062] Example 2 The method for producing the positive electrode material for a sodium ion battery of this embodiment includes the following steps: (A) A 1 mol / L aqueous solution of sodium borohydride and ferromanganese (II) hydroxide are mixed and added to a sand mill for sanding to obtain a first slurry having a particle size of 200 nm. The first slurry is spray-dried and then heated to 400°C at a rate of 1.5°C / min in nitrogen with a relative humidity of 3%, and kept at that temperature for 5 hours, then heated to 650°C at a rate of 1°C / min and kept at that temperature for 5 hours, and then cooled to 120°C at a rate of 3°C / min, and finished to obtain a first fired product.

[0063] Here, the ratio of the sum of the moles of Mn and Fe in ferromanganese(II) hydroxide to the moles of sodium borohydride is 0.97:1.

[0064] The method for producing ferromanganese (II) hydroxide is as follows: a mixture of manganese chloride, ferrous sulfate, EDTA, sodium hydroxide, aqueous ammonia (concentration: 5 mol / L), hydrazine hydrate, titanyl sulfate and deionized water is added to a reaction vessel, and the molar ratio of NH3·H2O in the manganese chloride, ferrous sulfate, EDTA, sodium hydroxide, hydrazine hydrate and aqueous ammonia is 1:1.5:0.01:5.5:0.01:0.05, and the molar sum of Mn in manganese chloride and Fe in ferrous sulfate and the molar sum of Fe in titanyl sulfate are 1:1.5:0.01:5.5:0.01:0.05. The molar ratio of Ti in the mixture is 100:0.1, the addition time is 60 min, the pH of the mixed solution during the addition is 9.6, the stirring speed is 600 r / min, the temperature is 60°C, after the addition is completed, the reaction is continued at 60°C for 30 min to obtain a reaction solution, and the concentration of free ammonia in the solution is controlled at 10 g / L during the reaction; and the reaction solution is filtered to obtain a filter cake, which is washed with 0.01 mol / L hydrazine hydrate and dried in a vacuum oven to obtain ferromanganese(II) hydroxide.

[0065] (B) The first fired product, a carbon source, ammonium metavanadate, sodium bicarbonate and water are mixed and added to a sand mill for sanding to obtain a second slurry with a particle size of 100 nm. The second slurry is spray-dried using a pressurized spray dryer to obtain a spray material with a particle size of 5 μm. In a nitrogen atmosphere, the spray material is first heated to 720°C at a rate of 3°C / min and kept at that temperature for 2 hours, then cooled to 80°C at a rate of 3°C / min, and finished to obtain a second fired product. The second fired product is pulverized at 145°C in a nitrogen atmosphere at a pressure of 0.35 MPa until the particle size of the second fired product is 1.1 μm. Next, iron is removed using a 150-mesh ultrasonic vibrating sieve and then an electromagnetic iron removal device until the magnetic material in the second fired product is 0.3 ppm, and the product is vacuum-packed to obtain a positive electrode material for a sodium-ion battery.

[0066] Here, the carbon source is nano-hydrophilic graphite and polyethylene glycol in a mass ratio of 1:5, the molar ratio of sodium in the first fired product, vanadium in ammonium metavanadate, and sodium bicarbonate is 1:0.02:0.06, the mass ratio of the carbon source to the first fired product is 3:100, and the ratio of the total mass of the first fired product, carbon source, ammonium metavanadate, and sodium bicarbonate to the mass of water is 1:2.

[0067] Example 3 The method for producing the positive electrode material for a sodium ion battery of this embodiment includes the following steps: (A) A 1.5 mol / L aqueous solution of sodium borohydride and ferromanganese (II) hydroxide are mixed and added to a sand mill for sanding to obtain a first slurry having a particle size of 300 nm. The first slurry is then spray-dried and, in nitrogen with a relative humidity of 5%, firstly, heated to 500°C at a rate of 3°C / min and kept at that temperature for 5 hours, then heated to 700°C at a rate of 1°C / min and kept at that temperature for 4 hours, and then cooled to 120°C at a rate of 1°C / min, and finished to obtain a first fired product.

[0068] Here, the ratio of the sum of the moles of Mn and Fe in ferromanganese(II) hydroxide to the moles of sodium borohydride is 1.02:1.

[0069] The method for producing ferromanganese (II) hydroxide is as follows: a mixture of manganese acetate, ferrous chloride, triethanolamine, sodium hydroxide, aqueous ammonia (concentration: 8 mol / L), hydrazine hydrate, titanyl sulfate and deionized water is added to a reaction vessel, and the molar ratio of NH3·H2O in the manganese acetate, ferrous chloride, triethanolamine, sodium hydroxide, hydrazine hydrate and aqueous ammonia is 1:4:0.1:10.5:0.1:0.5, and the molar ratio of Mn in the manganese chloride and Fe in the ferrous sulfate is 1:4:0.1:10.5:0.1:0.5. the molar ratio of Ti in is 100:0.2, the addition time is 120min, the pH of the mixed solution during addition is 9.9, the stirring speed is 550r / min, and the temperature is 50℃; after the addition is completed, the reaction is continued at 50℃ for 25min to obtain a reaction solution, and the concentration of free ammonia in the solution is controlled at 10g / L during the reaction; and the reaction solution is filtered to obtain a filter cake, which is washed with 0.015mol / L hydrazine hydrate and dried in a vacuum oven to obtain ferromanganese(II) hydroxide.

[0070] (B) The first fired product, a carbon source, ammonium metavanadate, sodium bicarbonate and water are mixed and added to a sand mill for sanding to obtain a second slurry with a particle size of 200 nm. The second slurry is spray-dried using a pressurized spray dryer to obtain a spray material with a particle size of 10 μm. In a nitrogen atmosphere, the spray material is first heated to 750°C at a rate of 3°C / min and kept at that temperature for 3 hours, then cooled to 80°C at a rate of 3°C / min, and finished to obtain a second fired product. The second fired product is pulverized at 145°C in a nitrogen atmosphere at a pressure of 0.35 MPa until the particle size of the second fired product is 1.3 μm. Next, iron is removed using a 150-mesh ultrasonic vibrating sieve and then an electromagnetic iron removal device until the magnetic material in the second fired product is 0.2 ppm, and the product is vacuum-packed to obtain a positive electrode material for a sodium-ion battery.

[0071] Here, the carbon source is nano-hydrophilic graphite and polyethylene glycol in a mass ratio of 1:10, the molar ratio of sodium in the first fired product, vanadium in ammonium metavanadate, and sodium bicarbonate is 1:0.03:0.09, the mass ratio of the carbon source to the first fired product is 10:100, and the ratio of the total mass of the first fired product, carbon source, ammonium metavanadate, and sodium bicarbonate to the mass of water is 1:3.

[0072] Comparative Example 1 The preparation method of the positive electrode material for sodium ion batteries provided by this comparative example is different from that of Example 1 only in that ammonium metavanadate is not added in step (B).

[0073] Test Example 1 The ferromanganese (II) hydroxide produced in Example 1 was subjected to a scanning test, the results of which are shown in FIG.

[0074] As can be seen from FIG. 1, the ferromanganese (II) hydroxide produced by the present invention is in the form of spherical, cotton-like aggregates having a large specific surface area, a small primary particle size, and high reactivity.

[0075] The properties of the ferromanganese (II) hydroxide produced in Example 1 were tested and the results are shown in Table 1.

[0076] [Table 1]

[0077] Test Example 2 A scanning test was performed on the first fired product produced in Example 1, the results of which are shown in Figure 2. The properties of the first fired product produced in Example 1 were also performed, the results of which are shown in Table 2. The compacted density is the density of the powder product at 3T pressure.

[0078] [Table 2]

[0079] Test Example 3 The spray material produced in Example 1 was subjected to a scanning test, the results of which are shown in Figure 3. The sodium ion battery positive electrode material produced in Example 1 was subjected to a scanning test, the results of which are shown in Figure 4. The properties of the sodium ion battery positive electrode material produced in Example 1 were tested, the results of which are shown in Table 3. The compacted density is the density of the powder product at 3T pressure.

[0080] [Table 3]

[0081] The positive electrode material for sodium ion batteries prepared in Example 1 and the positive electrode material for sodium ion batteries prepared in Comparative Example 1 are respectively prepared using carbon-coated aluminum foil as a current collector, and at the same time, sodium hexafluorophosphate is used as an electrolyte, and hard carbon is used as an anode to prepare a 3 Ah soft-pack battery. The cycle performance test is carried out at 25°C and 1C magnification.

[0082] Figure 5 is a schematic diagram of the relationship between the capacity retention rate and the number of cycles of the positive electrode material for a thorium ion battery manufactured in Example 1. Figure 6 is a graph of the charge and discharge curves of the positive electrode material for a thorium ion battery manufactured in Example 1, where A1 and A are charge and discharge curves at 0.2C magnification, and B1 and B are charge and discharge curves at 1C magnification. Next, the direct current resistance (DCR) at 50% SOC (residual capacity 50%) was detected, the discharge magnification was 2C, the battery was 3Ah, A is two parallel experiments performed on the battery prepared for the first time, and D is two parallel experiments performed on the battery prepared for the second time with the same material, and the results are shown in Figure 7.

[0083] As can be seen from Figure 5, the positive electrode material for sodium ion batteries of the present invention has excellent cycle performance, with a capacity retention rate of ≧95% after 500 cycles under 1C conditions. As can be seen from Figure 6, the positive electrode material for sodium ion batteries of the present invention has a high capacity of about 118mAh / g at 1C, while the positive electrode material for sodium ion batteries of Comparative Example 1 has a capacity retention rate of only 91% after 500 cycles under 1C conditions, and a discharge capacity of only 110.5mAh / g at 1C.

[0084] As can be seen from Figure 7, all DCRs are low at 16mΩ.

[0085] As can be seen from Table 3 and Figures 5-7, the positive electrode material for sodium ion batteries of the present invention has a high compaction density of 2.37g / mL, and the expected electrode sheet can reach a compaction density of 2.45g / mL or more when used. In addition, the positive electrode material for sodium ion batteries of the present invention has excellent cycle performance, large capacity, and high voltage platform. At the same time, according to calculations, the cost of the positive electrode material for sodium ion batteries of the present invention is only 30% of the cost of lithium iron phosphate, and has excellent cost performance, and can be applied in fields such as motorcycles, electric buses, and electric vehicles with short driving ranges.

[0086] Finally, it should be noted that the above embodiments are only for illustrating the technical solutions of the present invention, and are not intended to limit the same. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should still understand that the technical solutions described in the above embodiments can be modified or equivalently replaced with some or all of the technical features therein, and such modifications or replacements do not cause the essence of the corresponding technical solutions to depart from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for producing a positive electrode material for a sodium ion battery, comprising the steps of: (A) grinding a mixture of sodium borohydride and ferromanganese hydroxide to obtain a first slurry, which is then spray-dried and calcined to obtain a first calcined product; (B) grinding the mixture of the first fired product, a carbon source, a vanadium source, a sodium source, and water to obtain a second slurry, which is then spray-dried, fired, pulverized, sieved, and iron-removed to obtain the sodium ion battery positive electrode material; A method for producing positive electrode materials for sodium ion batteries.

2. In step (A), the firing includes heating the material to 400-500° C. in a nitrogen atmosphere, maintaining the temperature for 4-5 h, then heating the material to 650-700° C., maintaining the temperature for 3-5 h, and then cooling the material to 120° C. or less; Preferably, the relative humidity of the baking is between 3% and 5%; Preferably, the firing step includes heating the mixture in a nitrogen atmosphere to 400-500° C. at a rate of 1-3° C. / min, maintaining the temperature for 4-5 h, then heating the mixture to 650-700° C. at a rate of 1-3° C. / min, maintaining the temperature for 3-5 h, and then cooling the mixture to 120° C. or less at a rate of 1-3° C. / min to obtain a positive electrode material. A method for producing the positive electrode material for a sodium ion battery according to claim 1.

3. In step (A), the ratio of the sum of the moles of Fe and Mn in said ferromanganese hydroxide to the moles of Na in said sodium borohydride is 0.97 to 1.02:1; Preferably, the particle size of the first slurry is 200 to 300 nm. A method for producing the positive electrode material for a sodium ion battery according to claim 1.

4. In step (A), the method for producing ferromanganese hydroxide comprises: reacting a manganese salt, a ferrous salt, a complexing agent, sodium hydroxide, hydrazine hydrate, aqueous ammonia and titanyl sulfate in an aqueous phase to obtain said ferromanganese hydroxide; Preferably, the reaction temperature is 50-60° C. and the reaction time is 15-150 min. A method for producing the positive electrode material for a sodium ion battery according to claim 1.

5. the molar ratio of Mn in the manganese salt to Fe in the ferrous salt is 1:1.5-4; Preferably, the ratio of the sum of the moles of Mn in the manganese salt and Fe in the ferrous salt to the moles of Ti in the titanyl sulfate is 100:0.1-0.2; Preferably, the manganese salt, the complexing agent, the sodium hydroxide, the hydrazine hydrate and the NH 3 ・H 2 The molar ratio of O is 1:0.01-0.1:5.5-10.5:0.01-0.1:0.05-0.5, Preferably, the manganese salt comprises at least one of manganese sulfate, manganese chloride, and manganese acetate; Preferably, the ferrous salt comprises at least one of ferrous sulfate, ferrous chloride, and ferrous acetate; Preferably, the complexing agent comprises at least one of ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, sodium hexametaphosphate, and triethanolamine. The method for producing the positive electrode material for a sodium ion battery according to claim 4.

6. In step (B), the vanadium source comprises ammonium metavanadate; Preferably, the sodium source comprises at least one of sodium bicarbonate, sodium hydroxide, sodium acetate and sodium nitrate; Preferably, the carbon source comprises nano-hydrophilic graphite and / or polyethylene glycol; Preferably, the mass ratio of the nano-hydrophilic graphite to the polyethylene glycol is 1:5-10; A method for producing the positive electrode material for a sodium ion battery according to claim 1.

7. In step (B), the molar ratio of sodium in the first calcined product, vanadium in the vanadium source, and sodium in the sodium source is 1:0.02-0.03:0.06-0.09; Preferably, the mass ratio of the carbon source to the first fired product is 3 to 10:100; Preferably, the ratio of the total mass of the first calcined product, the carbon source, the vanadium source and the sodium source to the mass of the water is 1:2 to 3. A method for producing the positive electrode material for a sodium ion battery according to claim 1.

8. In step (B), the firing step includes heating the mixture to 720-750° C. in a nitrogen atmosphere, maintaining the temperature for 2-4 hours, and then cooling the mixture to 80° C. or less; Preferably, the firing is performed in a nitrogen atmosphere by increasing the temperature to 720 to 750° C. at a rate of 1 to 3° C. / min, maintaining the temperature for 2 to 4 hours, and then cooling to 80° C. or less at a rate of 1 to 3° C. / min. Preferably, the particle size of the second slurry is 100 to 200 nm; Preferably, the particle size of the second slurry after spray drying is 5 to 10 μm. A method for producing the positive electrode material for a sodium ion battery according to claim 1.

9. Produced by the method for producing a positive electrode material for a sodium ion battery according to any one of claims 1 to 8, Positive electrode material for sodium ion batteries.

10. The positive electrode material for a sodium ion battery according to claim 9, Sodium ion battery.

Citation Information

Patent Citations

  • Monocrystalline sodium ion battery positive electrode material and preparation method and application thereof

    CN115275134A

  • Boron-doped sodium-ion cathode material, method of producing same and its use

    EP3415470A1

  • Positive electrode material for lithium secondary battery, and lithium secondary battery

    JP2013187032A

  • Na excess p3-type layered oxides na xm yo z with x ≥ 0.66; 0.8 ≤ y ≤ 1.0 and z ≤ 2 as cathode materials for sodium ion batteries

    WO2021150168A1