Borate-free aqueous compositions for cleaning and treating metal substrates - Patents.com

A borate-free aqueous composition with metasilicates and phosphates forms a silicon-containing layer on aluminum surfaces, addressing the complexity and environmental issues of existing treatments, improving adhesive bond strength and durability.

JP2024536855APending Publication Date: 2024-10-08CHEMETALL GMBH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024518742
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-27
Filing Date
2022-09-26
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing methods for cleaning and treating aluminum surfaces to enhance adhesive bonding are complex, environmentally restrictive, and fail to prevent the growth of weak hydroxide layers, leading to reduced bond strength and durability, while also requiring silanization steps and using borates that are regulated by REACH.

Method used

A borate-free aqueous cleaning and treatment composition comprising metasilicates, orthophosphates, diphosphates, triphosphates, and surfactants, with a pH range of 11.0-12.8, forms a silicon-containing layer on metal surfaces, improving adhesion without silanization and avoiding borates.

Benefits of technology

The composition effectively forms a homogeneous silicon-containing layer, enhancing adhesive bond strength and durability, while being environmentally friendly and avoiding regulatory constraints, without requiring additional treatment steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536855000001
    Figure 2024536855000001
  • Figure 2024536855000002
    Figure 2024536855000002
  • Figure 2024536855000003
    Figure 2024536855000003
Patent Text Reader

Abstract

The present invention relates to a borate-free aqueous cleaning and treating composition comprising at least one metasilicate (A), at least one orthophosphate (B), at least one phosphate (C) selected from the group consisting of diphosphates and triphosphates, and at least one surfactant (D) selected from the group consisting of anionic surfactants and nonionic surfactants. The aqueous cleaning and treating composition has a pH value in the range of 11.0 to 12.8 at 20°C and a molar ratio of Si atoms to P atoms of 0.75:1 to 1:0.75 for the total of the Si-containing metasilicate (A) and the total of the P-containing orthophosphate (B), diphosphate (C), and triphosphate (C). The present invention further relates to a solid mixture. The present invention also relates to a method for cleaning and treating a metal substrate using the above composition, and a method for treating a metal substrate by cleaning the metal substrate and forming a Si-containing layer on the surface of the metal substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a borate-free aqueous composition for cleaning and treating metal substrates, preferably aluminum-based metal substrates, such as aluminum and its alloys. The present invention further relates to the preparation of the composition, a solid mixture for preparing the composition, and a method for cleaning and treating metal substrates utilizing the borate-free aqueous composition. A further object of the present invention is the use of the composition of the present invention for cleaning and treating metal substrates. [Background technology]

[0002] In making various structures from metals, it is important to have the ability to bond to metal substrates, including bonding metal substrates to other metallic materials and bonding non-metallic materials to metal substrates.

[0003] In many applications, it is possible to use simple mechanical fastening mechanisms, such as bolts, screws, or rivets. In other applications, concerns about the added mass of mechanical fasteners make the use of adhesives more viable. A variety of adhesives are known and commonly used in the art for bonding metal to metal or for bonding non-metallic materials to metal. For example, a variety of epoxy-based adhesives are widely used for these applications.

[0004] When bonding metals using adhesives, it is generally important to achieve the strongest bond possible. In general, it is difficult to ensure a strong bond when using adhesives. For example, process conditions during bond manufacturing often dramatically reduce bond strength. This is especially true when bonding to metals such as aluminum or its alloys. Bonding to aluminum and aluminum alloys poses special challenges.

[0005] Aluminum and aluminum alloys are considered difficult metals to bond to because aluminum surfaces tend to form a weakly hydrated surface layer of aluminum oxide. The morphology of the surface, and therefore the durability of the adhesive bond, depends on the type of surface cleaning and treatment that is performed prior to bonding.

[0006] The oxide commonly found in aluminum is aluminum oxide (Al2O3). This oxide is stable to bonding. However, with time and humidity, this oxide hydrates to form a less stable and mechanically weak layer of AlOOH (boehmite) and aluminum trihydroxide (bayerite). The thickness of this layer typically ranges from about 10 nm to about 150 nm, depending on the environment. When an adhesive is applied over this film, a weak boundary layer is built into the bonding system. The presence of this weak boundary layer reduces bond strength, reduces fracture toughness, and reduces bond durability over time. Similarly, providing a bond of sufficient initial strength is often problematic.

[0007] Commonly used treatments for aluminum surfaces involve vapor degreasing and grit blasting, but these methods do not prevent the further growth of the boehmite and bayerite layers on the aluminum surface.

[0008] Available cleaning solvents and solutions used in this process are becoming more restrictive due to environmental regulations regarding chemical waste disposal. Thus, the combination of process sensitivity, limited bond durability, and environmental constraints raises concerns about the continued use of traditional surface preparation processes.

[0009] Alternative methods for cleaning and preparing aluminum surfaces are limited. Some such other methods of preparing aluminum surfaces involve the formation of a stable, moisture-resistant oxide layer. These methods include sulfuric acid, chromic acid, and phosphoric acid anodization. These electrolytic processes inhibit further growth of the hydroxide layer and improve initial bond strength and bond durability. In addition, the phosphoric acid process creates a honeycomb-like surface that is believed to improve bond strength through mechanical interlocking.

[0010] However, these processes generally consist of a complex series of treatments that include degreasing, alkaline cleaning, acid etching, acid anodization, and in some instances, post-treatment processes.

[0011] Thus, what is needed in the art is an effective and efficient method of cleaning and treating aluminum and other metal surfaces to provide a stable adhesive bond to the metal substrate. In that regard, it would be a significant advancement in the art to provide a surface treatment and cleaning method that is relatively simple and uses readily available materials.

[0012] It would be a further advancement in the art to provide a surface cleaning and treatment method that improves bond strength to an adhesive layer.

[0013] A further object of the present invention is to provide a solid mixture of cleaning and treatment agents, which can be simply dissolved in water at the application site to form a cleaning and treatment composition for metal substrates. The solid mixture can be simply supplemented with an acid or base to adjust the pH value, which is optimal for cleaning and treatment, especially for aluminum-based substrates. Providing a solid mixture instead of a liquid concentrate offers great advantages when shipping the mixture, since it is not diluted with water, so the volume is optimized and it can therefore be shipped without moisture. The water required for the preparation of the cleaning and / or treatment bath can be supplemented at any application site. Providing such a solid mixture or dry concentrate thus adds to the environmentally friendly aspect of the present invention. Of course, such a composition should have a reduced tendency to form agglomerates.

[0014] Yet another object of the present invention is to provide an aqueous cleaning and treatment composition that is free of borates, which are to be avoided according to the recent plans of the European Union's REACH regulation, which addresses the manufacture and use of chemicals and their potential impacts on both human health and the environment.

[0015] Furthermore, besides the possibility of cleaning metal substrates, in particular, but not limited to, aluminum-based substrates, the composition should be suitable for forming a silicon-containing surface layer, e.g., a silicate layer, allowing better adhesion of a subsequent adhesive or coating layer. Such a silicon-containing layer should be uniform in silicon content, expressed as Si and determined by XRF spectroscopy, at the surface of the metal substrate, and preferably have a silicon content of about 2-7 mg / m, in particular on the commonly used aluminum alloy AA6014. 2 This Si-based layer significantly improves the adhesion of the thus treated metal substrate surface to the adhesive.

[0016] Additionally, the cleaning and treatment compositions should not exhibit excessive pickling.

[0017] DE 19642723 A1 relates to a method for bonding a paint or adhesive to a part of the surface of a workpiece made of aluminum or an aluminum alloy, in particular an aluminum-magnesium alloy, in which said part of the metal surface is presilicified with polymerized silicic acid having a degree of polymerization of at least 1 to produce an adhesion-improving layer. The silica was produced by pyrolyzing a mixture of tetraethoxysilane, tetramethoxysilane and dimethylethoxysilane in a detonating flame (H2:O2=2:1) ​​with a concentration ratio of 1:2:1, a partial pressure of 5 mbar and a pyrolysis time of 0.2 seconds. Before treatment with the polymerized silica, the substrate was degreased with isopropanol.

[0018] WO2019 / 042951A1 discloses a method for substantially nickel-free phosphating of metal surfaces, in which the metal surfaces are successively treated with the following compositions: i) an alkaline aqueous detergent composition containing at least a water-soluble silicate, and ii) an acidic, aqueous, substantially nickel-free phosphating composition containing zinc ions, manganese ions and phosphate ions. As another substrate, aluminum alloys were also treated. The alkaline aqueous cleaning composition used in the method according to WO2019 / 042951A1 is based on a waterglass-based composition mixed with pyrophosphate or polyphosphate and / or boric acid.

[0019] US 5,520,768 discloses a two-step surface preparation process, particularly for aluminum and aluminum alloy substrates, in which the metal surface is first treated with an alkali metal metasilicate solution, followed by treatment with an organofunctional silane to improve the bond strength, fracture toughness, durability and failure mode of the adhesive bond. The primary objective of the first step was to provide a very thin silicate layer on the surface of the metal substrate. The composition used in this process may also contain cleaning additives, such as detergents, emulsifiers and terpenes such as D-limonene.

[0020] In particular, in view of the aforementioned US 5,520,768, the present invention was to provide a method for cleaning and treating metal surfaces that does not require a silane treatment step other than that described in US 5,520,768. The cleaning and provision of good adhesion to further layers of adhesive and / or coating material should not depend on carrying out a second treatment step, for example with silane. Other than the use of surfactants, such as anionic or nonionic surfactants, no organic compounds should be necessary in the cleaning and treating compositions of the present invention. [Prior art documents] [Patent documents]

[0021] [Patent Document 1] DE19642723A1 [Patent Document 2] WO2019 / 042951A1 [Patent Document 3] US5,520,768 Summary of the Invention [Means for solving the problem]

[0022] The above specific objects and objects of overcoming the drawbacks of the prior art are achieved by providing a borate-free aqueous cleaning and treatment composition comprising at least one metasilicate (A), at least one orthophosphate (B), at least one phosphate (C) selected from the group consisting of diphosphates and triphosphates, and at least one surfactant (D) selected from the group consisting of anionic surfactants and nonionic surfactants, the aqueous cleaning and treatment composition having a pH value in the range of 11.0 to 12.8 at 20°C and a molar ratio of Si atoms to P atoms of 0.75:1 to 1:0.75 for the sum of the Si-containing metasilicate (A) and the sum of the P-containing orthophosphate (B), diphosphate (C) and triphosphate (C).

[0023] Hereinafter, this composition will also be referred to as the composition according to the invention.

[0024] A further object of the invention is a method for preparing said composition according to the invention, comprising dissolving in a first step (I) a solid mixture (M) comprising at least one metasilicate (A), at least one orthophosphate (B), and at least one phosphate (C) selected from the group consisting of diphosphates and triphosphates, and at least one surfactant (D) selected from the group consisting of anionic and nonionic surfactants, in water to obtain an aqueous solution, and, in a second step (II), if necessary, adjusting the pH value of the aqueous solution obtained in the first step (I) to the ranges indicated for the composition according to the invention, preferably by addition of phosphoric acid or an aqueous solution thereof or by addition of an aqueous solution of an alkali metal hydroxide.

[0025] Hereinafter, this method is also referred to as the method for preparing the composition according to the invention.

[0026] Yet another object of the invention is a solid mixture (M) for use in the process for preparing a composition according to the invention, which solid mixture (M) comprises at least one metasilicate (A), preferably at least one orthophosphate (B), at least one phosphate (C) selected from the group consisting of diphosphates and triphosphates, and at least one surfactant (D) selected from the group consisting of anionic and nonionic surfactants, at least each species (A), (B) and (C) being solid at 20° C.

[0027] Hereinafter, this mixture is also referred to as the mixture according to the invention. The term "solid" refers to the state of each component at room temperature (23°C). The surfactant (D) may be liquid at room temperature, but the other components of the solid mixture (M), namely at least one metasilicate (A), preferably at least one orthophosphate (B) and at least one phosphate (C) selected from the group consisting of diphosphates and triphosphates, are typically solid in the above sense and thus form the solid mixture (M) together with the surfactant (D). When used, the liquid surfactant (D) is preferably applied to the surface of one or more solid components.

[0028] A further object of the present invention is a method for cleaning and treating a metal substrate, comprising the steps of contacting the metal substrate with a borate-free aqueous cleaning and treatment composition according to the present invention or prepared by the method for preparing a composition as defined above to obtain a cleaned and surface-treated metal substrate, and contacting the thus cleaned and surface-treated metal substrate with an aqueous rinsing composition to remove excess cleaning and treatment composition.

[0029] Yet another object of the invention is the use of the composition according to the invention for cleaning and treating metal substrates, which will be referred to as the use according to the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The objects of the present invention are described in more detail below, in particular the preferred components contained in the compositions and mixtures according to the invention, and the preferred method steps and process conditions.

[0031] Borate-free aqueous cleaning and treatment compositions The borate-free aqueous cleaning and treatment composition according to the present invention contains at least one metasilicate (A), at least one orthophosphate (B), and at least one phosphate (C) selected from the group consisting of diphosphates and triphosphates. (A), (B) and (C) used in the cleaning and treatment composition according to the present invention preferably have a water solubility of at least 50 g / L at 20° C. and are therefore completely soluble in the composition according to the present invention at 20° C.

[0032] The surfactant (D) is also soluble in the borate-free aqueous cleaning and treatment composition according to the invention, for example in the form of micelles.

[0033] The inventors have found that the optimum performance of the composition in terms of cleaning and treatment effect is achieved when the pH value of the composition is in the range of 11.0-12.8 at 20°C, preferably 11.3-12.5, and most preferably 11.6-12.2. If the pH value is lower than 11.0 at 20°C, the pH value of the composition at 80°C may be too low to prevent irreversible precipitation of metasilicate (A). If the pH value is higher than 12.8 at 20°C, pickling at 80°C may be too strong. If the pH value is kept in the preferred and most preferred ranges, there is a good balance between cleaning effect, precipitation of Si-containing layer, and pickling that may occur to some extent.

[0034] Furthermore, the cleaning and treatment composition according to the present invention has a molar ratio of Si atoms to P atoms relative to the sum of the Si-containing metasilicate (A) and the sum of the P-containing orthophosphate (B), diphosphate (C) and triphosphate (C) of 0.75:1.0 to 1.0:0.75, preferably 0.8:1.0 to 1.0:0.8, more preferably 0.85:1.0 to 1.0:0.85, for example 0.9:1.0 to 1.0:0.9.

[0035] Metasilicate (A) The essential component of the borate-free aqueous cleaning and treatment composition according to the present invention is at least one metasilicate (A). Most preferred are alkali metal metasilicates, such as sodium metasilicate, potassium metasilicate or lithium metasilicate. Of the aforementioned metasilicates, sodium metasilicate and potassium metasilicate are preferred, with sodium metasilicate being the most preferred metasilicate. As long as it is available, metasilicates containing water of crystallization, such as sodium metasilicate-pentahydrate, may be used to prepare the composition according to the present invention.

[0036] Preferably, at least one metasilicate (A) contained in the composition according to the present invention is the main Si-containing compound based on the total mass of the Si-containing compounds.The term "main Si-containing compound" means that at least 50 mass%, more preferably at least 75 mass%, and most preferably at least 95 mass% of the total mass of the Si-containing compounds in the composition according to the present invention is at least one metasilicate (A).When other Si-containing compounds other than metasilicate (A) are present in the composition according to the present invention, such Si-containing compounds are preferably other water-soluble silicates that are completely dissolved in the composition at 20 ° C.

[0037] Most preferably, the only Si-containing compound in the cleaning and treatment composition according to the present invention is metasilicate (A).Typically, a technical grade of metasilicate can be used, so that metasilicate (A) is still considered as the only Si-containing compound even if it contains some Si-containing impurities present due to the manufacturing process of metasilicate (A).

[0038] Orthophosphate (B) A further essential component of the borate-free aqueous cleaning and treatment composition according to the invention is at least one orthophosphate (B).

[0039] The orthophosphate (B) can also be formed in situ, for example when phosphoric acid or an aqueous phosphoric acid solution is used to adjust the pH value to the required range.

[0040] However, preferably, alkali metal salts of phosphoric acid are used, such as the mono-, di- and tri-alkali metal orthophosphates, with sodium, potassium and lithium orthophosphate being preferred, and sodium and potassium orthophosphate being most preferred, of which sodium orthophosphate is most preferred.

[0041] Phosphate(C) The essential phosphate (C) is selected from the group consisting of triphosphates and diphosphates.

[0042] Preferably, alkali metal diphosphates and / or alkali metal triphosphates are used, such as sodium triphosphate, potassium triphosphate, sodium diphosphate and potassium diphosphate, however, less preferably, the corresponding lithium phosphates may also be used.

[0043] Most preferably, the compositions of the present invention contain a combination of diphosphates and triphosphates.

[0044] Examples of suitable phosphates (C) are penta-sodium triphosphate, penta-potassium triphosphate, tetra-sodium diphosphate and tetra-potassium diphosphate.

[0045] Surfactant (D) Furthermore, at least one surfactant (D) is contained in the cleaning and treatment composition according to the invention. Suitable surfactants are selected from the group consisting of anionic surfactants and nonionic surfactants.

[0046] Anionic Surfactants (D) Such surfactants are suitably selected from alkali metal salts of linear alkylbenzene sulfonic acids, secondary alkyl sulfonates, fatty alcohol sulfates and alkyl ether sulfates. The anionic surfactants are typically and preferably solid.

[0047] Nonionic surfactants (D) Such surfactants are suitably selected from polyalkoxylated alcohols, such as poly(ethoxylated / propoxylated) alcohols, preferably polyethoxylated alcohols, said alcohols preferably containing 6 to 20 carbon atoms, linear or branched, and preferably primary or secondary alcohols, and ethoxylated fatty amines. Nonionic surfactants are typically liquid. This does not affect the overall solid state of the solid mixture of the present invention. Preferably, liquid surfactants, especially nonionic liquid surfactants, are applied to the surface of the solid components, for example by spray application.

[0048] Carbonate (E) The inventors have also found that water soluble carbonates can be advantageously included in the cleaning and treatment compositions of the present invention.

[0049] Suitable carbonates are, for example, alkali metal carbonates and hydrogen carbonates, such as sodium carbonate, sodium hydrogen carbonate, potassium carbonate and potassium hydrogen carbonate.

[0050] pH adjuster In order to adjust the pH value of the cleaning and processing composition of the present invention to the required and preferred ranges mentioned above, inorganic acids and bases can be suitably used.

[0051] The most preferred acid is phosphoric acid, and the most preferred bases are sodium hydroxide and potassium hydroxide. The most preferred acids and bases are used in a form diluted with water. When phosphoric acid is used, orthophosphate is generated in situ at the preferred pH range. Thus, phosphoric acid as a pH adjuster adds phosphate to the composition according to the present invention, which is taken into account when calculating the molar ratio based on P atoms. Because the orthophosphate introduced by the addition of phosphoric acid (i.e., orthophosphoric acid) is indistinguishable from the orthophosphate introduced by the addition of a salt of orthophosphoric acid, it is treated the same as the addition of such a salt.

[0052] A complementary mixture of solids including metasilicates and phosphates, and hydroxides such as sodium hydroxide, are preferably added for pH adjustment during the cleaning and treatment process.

[0053] General Aspects of Cleaning and Treatment Compositions Preferably, the total amount of solids contained in the cleaning and treatment compositions of the present invention is in the range of 10-60 g / L, more preferably 15-50 g / L, and most preferably 20-45 g / L, for example 25-40 g / L.

[0054] The total amount of solids is the calculated amount of salts or other components, e.g. components added as surfactants (D), even if the surfactants are in liquid form to prepare the compositions according to the invention, and non-volatile components, e.g. the phosphate content of phosphoric acid used to adjust the pH value or the alkali metal ion content of the respective hydroxide to adjust the pH value.

[0055] In general, the molar concentration of Si atoms from metasilicate (A) contained in the composition according to the present invention is preferably in the range of 50-200 mmol / L, more preferably 70-190 mmol / L, and most preferably 80-180 mmol / L, for example 90-170 mmol / L. It should be understood that the chemical formula of metasilicate (A) contains one Si atom, and therefore the molar amount of Si atoms from metasilicate (A) is equal to the molar amount of metasilicate (A).

[0056] Generally, it is preferred that the molar concentration of P atoms from orthophosphate (B), contained in the composition according to the invention and derived from either a solid salt or orthophosphoric acid, is in the range of 25-75 mmol / L, more preferably 30-70 mmol / L, and most preferably 35-65 mmol / L, for example 40-60 mmol / L. It should be understood that the chemical formula of orthophosphate (B) contains one P atom, and thus the molar amount of P atoms from orthophosphate (B) is equal to the molar amount of orthophosphate (B).

[0057] In general, the molar concentration of P atoms from the phosphate (C) contained in the composition according to the invention is preferably in the range of 30-130 mmol / L, more preferably 40-125 mmol / L, and most preferably 45-120 mmol / L, for example 50-115 mmol / L. It should be understood that the formula of the diphosphate (C) contains two P atoms, and therefore the molar amount of P atoms from the diphosphate (C) is twice the molar amount of the diphosphate (C). It should be understood that the formula of the triphosphate (C) contains three P atoms, and therefore the molar amount of P atoms from the triphosphate (C) is three times the molar amount of the triphosphate (C).

[0058] When both diphosphate (C) and triphosphate (C) are used, the molar amount of P atoms from triphosphate (C) preferably exceeds the molar amount of P atoms from diphosphate (C) by at least 20 mol%, even more preferably by at least 25 mol%, and most preferably by at least 30 mol%.

[0059] Preferably, the molar amount of P atoms from the orthophosphate (B) to the molar amount of P atoms from the phosphate (C) is 1:1.2 to 1:3.5, more preferably 1:1.3 to 1:3.0, even more preferably 1:1.4 to 1:2.8.

[0060] The total amount of surfactant (D) is typically in the range of 0.5 to 10 g / L of the composition of the present invention, more preferably 1 to 8 g / L of the composition of the present invention, even more preferably 2 to 6 g / L, for example 3 to 5 g / L.

[0061] When carbonate (E) is present in the composition of the invention, its molar concentration is preferably in the range of 15 to 100 mmol / L, more preferably 20 to 90 mmol / L, even more preferably 25 to 80 mmol / L and most preferably 30 to 70 mmol / L of the composition according to the invention.

[0062] Solid mixture (M) The solid mixture (M) of the present invention typically contains the above-mentioned metasilicate (A), preferably the orthophosphate (B), the phosphate (C), the surfactant (D) and preferably the carbonate (E) in the form of the alkali metal salts already mentioned above.

[0063] An exceptional component is the orthophosphate (B), which does not necessarily have to be contained in the solid mixture (M), since it is possible to introduce the orthophosphate into the cleaning and treatment composition of the present invention by adding phosphoric acid, i.e. orthophosphoric acid, to the solution of the solid mixture (M) in water to adjust the pH value to the above-mentioned range, thus introducing part or all of the orthophosphate (B) using phosphoric acid.

[0064] Components (A), (B), (C) and, if used, (E) are solid at 20° C. and preferably have a water solubility of at least 50 g / L in water at 20° C. The composition according to the invention formed by dissolving the solid mixture (M) of the invention and adjusting the pH value, if necessary, should typically not contain undissolved material from the solid mixture (M).

[0065] The surfactant (D) contained in the solid mixture (M) of the present invention can be liquid or solid, and is typically liquid.It can also be easily dissolved in water when forming the composition of the present invention by dissolving the solid mixture (M) of the present invention.The term "soluble" in this context includes the formation of micelles, which are not considered as solid particles but are the typical structure that surfactant molecules form in water due to their amphiphilic properties.

[0066] The solid mixture may further comprise a solid carbonate (E), preferably an alkali metal carbonate (including an alkali metal bicarbonate).

[0067] Methods for preparing cleaning and treatment compositions The method for preparing the borate-free aqueous cleaning and treatment composition according to the present invention comprises, as a first step (I), dissolving the solid mixture (M) according to the present invention in water or an aqueous medium and, if necessary, as a second step (II), adjusting the pH value to the desired and above disclosed range by adding an acid or base, preferably an inorganic acid or an inorganic base, which is preferably added in the form of its dilution in water and most preferably selected from phosphoric acid and alkali metal hydroxides.

[0068] Method for cleaning and treating metal substrates The present invention further comprises the steps of: (a) contacting a metal substrate with a borate-free aqueous cleaning and treatment composition of the present invention or prepared by the method defined above to obtain a cleaned metal substrate; and (b) contacting the thus cleaned metal substrate with an aqueous rinsing composition to remove any excess cleaning and treating composition. The present invention relates to a method for cleaning and treating a metal substrate, comprising:

[0069] Optionally, step (a) may be preceded by any suitable cleaning step.A wide variety of cleaning formulations for different types of substrates are commercially available.

[0070] Preferably, step (a) of "contacting" the metal substrate with the composition according to the invention (step (a)) is carried out by immersing the substrate in a bath containing the composition according to the invention. However, other types of contact are also possible, for example spraying the composition according to the invention onto the surface of the metal substrate.

[0071] The term "immersing the substrate in a bath" includes the possibility that one or more separate baths may be used subsequently in step (a). Without being limited thereto, this is particularly preferred when the substrate contains impurities such as oils and greases on its surface prior to the contacting step (a). Such impurities are particularly removed in the first bath(s) so that subsequent baths remain cleaner.

[0072] The contact step (a) is preferably carried out for 1 to 45 minutes, more preferably 5 to 40 minutes, even more preferably 10 to 30 minutes, and most preferably 15 to 25 minutes. Shorter contact times typically require substrates that have no or only a small amount of impurities on the surface. When the contact time is short, it is preferable to carry out the optional washing step described above before carrying out step (a).

[0073] Preferably, the temperature of the composition according to the present invention in the contacting step (a) is in the range of 40-90° C., more preferably 50-85° C., and most preferably 60-80° C. In general, it can be concluded that the higher the contact temperature, the shorter the contact time can be.

[0074] Preferably, the contact time in step (a) is in the range of 10 to 30 minutes and the contact temperature is in the range of 50 to 85°C, more preferably, the contact time is in the range of 15 to 25 minutes and the contact temperature is in the range of 60 to 80°C.

[0075] As already mentioned above, the amount of solids contained in the cleaning and treatment composition of the present invention is in the range of 10 to 60 g / L, more preferably 15 to 50 g / L, and most preferably 20 to 45 g / L, for example 25 to 40 g / L.

[0076] After the contact step (a), in a second step (b), the washed and treated substrate is contacted with a rinsing composition, preferably water, to remove excess cleaning and treatment composition from the surface of the substrate. Typically, the rinsing step (b) is carried out by immersing the washed and treated substrate in water one or more times, preferably one water bath followed by another, preferably with increasing water purity. The first water bath may be contaminated with excess cleaning composition according to the invention, but the second and any subsequent baths will contain less and less of the components of the composition according to the invention, especially when the process is carried out as a continuous process utilizing one or more rinsing baths. However, this step (b) can also be carried out by spray application of the rinsing composition, the rinsing composition being preferably water.

[0077] Step (b) is preferably followed by a drying step (c) to remove excess water present on the surface of the washed, treated and rinsed metal substrate. Drying conditions can be, for example, drying at room temperature to a temperature of 100° C. or higher. Drying times depend on the drying temperature and can preferably range from 1 minute to 5 hours, or 10 minutes to 2 hours, etc. Typical drying conditions are drying at 100° C. for 15 minutes. Drying can also be accelerated, for example, by blowing a stream of air over the surface of the wet substrate.

[0078] After the drying step (c), the cleaned and treated metal substrate is ready for adhesive bonding or coating with a coating material and no further cleaning and / or treatment steps are required.

[0079] metal base material Preferably, the metal substrate treated in the method for cleaning and treating a metal substrate is selected from the group consisting of aluminum or aluminum-containing alloys, steel, such as cold rolled steel and galvanized steel, zinc-magnesium coated steel and magnesium alloys.

[0080] Use according to the invention The present invention further relates to the use of a composition according to the invention or obtained by a respective process according to the invention for cleaning a metal substrate and for treating the metal substrate by forming a Si-containing layer on the surface of the metal substrate.

[0081] The present invention will now be further described by way of examples and comparative examples. EXAMPLES

[0082] Solid mixture (M) Table 1 shows the solid inventive example mixtures (IM) used to prepare compositions according to the invention.

[0083] [Table 1]

[0084] All example mixtures (IM) contained metasilicate (A), diphosphate (C) and / or triphosphate (C), anionic surfactant, and nonionic surfactant (D), but example mixtures IM-3, IM-4 and IM-5 also contained orthophosphate, while example mixtures IM-1 and IM-2 did not contain orthophosphate. When mixtures IM-1 and IM-2 were dissolved to prepare the borate-free aqueous cleaning and treatment compositions according to the invention, the pH value was adjusted with phosphoric acid (IM-1: 5.30 g phosphoric acid (75%), IM-2: 5.60 g phosphoric acid (75%)), thus introducing orthophosphate into the respective cleaning and treatment composition.

[0085] Table 2 shows the components of comparative mixture CM-1.

[0086] [Table 2]

[0087] Comparative mixture CM-1 contained borate, which is to be avoided in the present invention. Comparative mixtures CM-1, CM-2 and CM-3 were completely free of P. CM-4 and CM-5 did not contain any phosphate (C). CM-5, CM-6 and CM-7 did not contain metasilicate, but instead contained disilicate.

[0088] Borate-free aqueous cleaning and treatment compositions Table 3 below shows the amounts of example mixture (IM) and comparative mixture (CM) used to prepare 1 liter of composition according to the invention (IC) and 1 liter of comparative composition (CC), respectively, as well as the amounts of pH adjusters, 50% by weight potassium hydroxide aqueous solution or 75% by weight phosphoric acid aqueous solution, and the final pH values ​​at 20° C. (room temperature).

[0089] [Table 3]

[0090] Table 4 shows the molar amounts in mmol / L of Si and P atoms and their respective origins (from solid components (A), (B), (C) and, where applicable, from phosphoric acid ("from acid")).

[0091] [Table 4]

[0092] Method for cleaning and treating metal substrates As metal substrate panels AW-5005 (AlMg1) (aluminium / magnesium alloy; see also DIN EN573-3:2009-08) and AA6014 (aluminium / magnesium / silicon alloy) were used in oil form commercially available from Chemetall GmbH, Frankfurt, Germany, with dimensions of 10.5 x 19 cm.

[0093] The intrinsic silicon content of the panel surface, expressed as Si, is 1 mg / m for the aluminium-based alloy AW5005 (AlMg1), as measured by X-ray fluorescence analysis. 2 , and 10 mg / m for the aluminium-based alloy AA6014. 2 It was.

[0094] Compositions IC-1 to IC-5 of the invention and comparative compositions CC-1 to CC-7 were heated to 80° C. in separate baths. The panels were immersed in the separate compositions for 24 minutes by immersing the panels in the baths. The panels were then removed and immersion rinsed in a water bath for 6 minutes and immersion rinsed again in another water bath for 3 minutes to remove any excess cleaning and treatment composition. The panels were then dried at 100° C. for 15 minutes.

[0095] After drying, the panels were cut into 3.5×3.5 cm samples with a gate shear and analyzed for surface Si content by RFA analysis.

[0096] The RFA device used was a Panalytical Axios max (Rh tube 3 kW, channel Si K アルファ , measurement under vacuum, aperture 27 mm, collimator 300 μm, flow meter, excitation 24 kV-110 mA, crystal PE002, 2 theta angle maximum 109.1°, background 1 107.1° and background 2 110.4°, measurement time maximum 30 seconds, backgrounds 10 seconds each).

[0097] The Si content values ​​shown in Table 5 are baseline corrected values, i.e., 1 mg / m when AW-5005 (AlMg1) was used. 2 10mg / m2 when AA6014 is used 2 The amount of was subtracted from the value obtained by the RFA analysis. The average value of the two measurements is shown, rounded up to the nearest integer.

[0098] Additionally, the optical appearance was evaluated: As a control, comparative composition CC-1, which contained borate, was selected and rated as "good."

[0099] The final column of Table 5 provides notes regarding the overall rating, including the stability of the compositions and the processability of the mixtures used to prepare each composition.

[0100] [Table 5]

[0101] In addition to the above experiments, the composition IC-5 of the present invention was further investigated with respect to the relationship between the treatment time, treatment temperature and the composition component concentrations on the Si content of the substrate surface. For this study, the substrate panel was pre-cleaned, i.e., degreased with ligroin, before carrying out the method according to the present invention.

[0102] It was found that even a short treatment time of about 6 min (temperature 80 °C, concentration 40 g IM-5 / L) was enough to obtain a satisfactory Si content on the surface of the substrate AA6014: the Si content detected after 6 min of treatment compared to 24 min of treatment was still about 75% compared to 85%.

[0103] Even after reducing the component concentration to 10 g of IM-5 / L (fourfold reduction in components), reducing the treatment temperature to 50 °C, and shortening the treatment time to 1 min, the Si content detected on the surface of both substrates was still within the acceptable baseline-corrected range and was above 2 mg / m 2 It was.

[0104] From this study, the following was inferred: The longer the treatment time at a given temperature and concentration, the higher the Si content on the substrate surface. The higher the treatment temperature for a given treatment time and concentration, the higher the Si content on the substrate surface; The higher the concentration of the component at a given treatment time and temperature, the higher the Si content on the substrate surface can be.

[0105] Thus, all compositions prepared using IM-5 in the concentration range of 10 g / L to 40 g / L and at temperatures between 50°C and 85°C for up to 24 minutes showed satisfactory results in terms of Si content on the treated metal surface of both substrates. The higher the treatment time, temperature and concentration, the higher the Si content was, ranging from 2 to 7 mg / m 2 The lower the treatment time, temperature and concentration, the closer the Si content will be to the lower value of the aforementioned range.

Claims

1. at least one metasilicate (A), at least one orthophosphate (B); At least one phosphate (C) selected from the group consisting of diphosphates and triphosphates, At least one surfactant (D) selected from the group consisting of anionic surfactants and nonionic surfactants.

1. A borate-free aqueous cleaning and treatment composition comprising: The aqueous cleaning and treatment composition comprises: i. has a pH value in the range of 11.0 to 12.8 at 20° C.; and ii. having a molar ratio of Si atoms to P atoms of 0.75:1 to 1:0.75 relative to the sum of the Si-containing metasilicate (A) and the sum of the P-containing orthophosphate (B), diphosphate (C) and triphosphate (C); A borate-free aqueous cleaning and treatment composition.

2. 10. The borate-free aqueous cleaning and treatment composition of claim 1 further comprising at least one carbonate salt in said aqueous cleaning and treatment composition.

3. 3. The borate-free aqueous cleaning and treatment composition of claim 1 or 2, containing at least one diphosphate (C) and at least one triphosphate (C).

4. 3. The borate-free aqueous cleaning and treatment composition according to claim 1 or 2, wherein the molar ratio of the sum of P atoms in the orthophosphate (B) to the sum of P atoms in the phosphate (C) is from 1:1.2 to 1:3.

5.

5. 3. The borate-free aqueous cleaning and treatment composition of claim 1 or 2, wherein the metasilicate (A), the orthophosphate (B) and the phosphate (C) are salts of alkali metals.

6. i. the molar concentration of the total Si atoms from the metasilicate (A) is in the range of 50 to 200 mmol / L; ii. the total molar concentration of P atoms from the orthophosphate (B) is in the range of 25-75 mmol / L; iii. The molar concentration of P atoms from the phosphate (C) is in the range of 30-130 mmol / L; iv. The concentration of the surfactant (D) is in the range of 0.5 to 10 g / L; and 3. The borate-free aqueous cleaning and treatment composition of claim 1 or 2, wherein the concentrations are per liter of said borate-free aqueous cleaning and treatment composition.

7. 3. A method for preparing the borate-free aqueous cleaning and treatment composition of claim 1 or 2, comprising: In the first step (I), at least one metasilicate (A), If no phosphoric acid is used in the second step (II), at least one orthophosphate (B), at least one diphosphate (C) and / or triphosphate (C), At least one surfactant (D) selected from the group consisting of anionic surfactants and nonionic surfactants. A solid mixture (M) comprising is dissolved in water to obtain an aqueous solution, and, if necessary, In the second step (II), The pH value of the aqueous solution obtained in the first step (II) is adjusted to the range specified in claim 1. method.

8. 8. The method for preparing a borate-free aqueous cleaning and treatment composition according to claim 7, wherein the solid mixture (M) further contains at least one carbonate (E).

9. A solid mixture (M) used in the method for preparing the borate-free aqueous cleaning and treatment composition of claim 7, comprising: at least one metasilicate (A), Preferably, at least one orthophosphate (B), At least one phosphate (C) selected from the group consisting of diphosphates and triphosphates, and At least one surfactant (D) selected from the group consisting of anionic surfactants and nonionic surfactants. wherein each of the species (A), (B) and (C) is a solid.

10. 10. The solid mixture (M) according to claim 9, further comprising at least one solid carbonate (E).

11. 1. A method for cleaning and treating a metal substrate, comprising: a. contacting a metal substrate with a borate-free aqueous cleaning and treatment composition as defined in claim 1 or prepared by the method as defined in claim 7 to obtain a cleaned metal substrate; and b. contacting the thus cleaned metal substrate with an aqueous rinsing composition to remove any excess cleaning and treating composition. A method comprising:

12. 12. The method of cleaning and treating a metal substrate according to claim 11, wherein in step (a), the metal substrate is contacted with the borate-free aqueous cleaning and treating composition by immersing the metal substrate in a bath containing the borate-free aqueous cleaning and treating composition for 1 to 45 minutes, the bath having a temperature in the range of 40 to 90° C.

13. 12. The method of cleaning and treating metal substrates according to claim 11, wherein the metal substrate is selected from aluminum or aluminum-containing alloys, steel, such as cold rolled steel and galvanized steel, and also zinc-magnesium coated steel and magnesium alloys.

14. 10. Use of the composition according to claim 1 or prepared by the method defined in claim 7 for cleaning a metal substrate and for treating the metal substrate by forming a Si-containing layer on the surface of the metal substrate.

Citation Information

Patent Citations

  • Metal pretreatment composition

    JP1985039171A

  • Improved bonding of paint or adhesive with aluminium or its alloys

    DE19642723A1

  • Method of surface preparation of aluminum substrates

    US5520768A

  • Improved method for nickel-free phosphating metal surfaces

    WO2019042951A1