Graphite steel wire rod with excellent cutting performance, steel wire, graphite steel, and manufacturing method thereof
A graphite steel with controlled composition and manufacturing process achieves high graphitization and uniform distribution, addressing the limitations of existing free-cutting steels by enhancing machinability and eliminating toxic emissions.
Patent Information
- Application Number
- JP2024522128
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-12
- Filing Date
- 2022-10-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-10-11
AI Technical Summary
Existing free-cutting steels face issues with harmful emissions and manufacturing difficulties due to the use of toxic elements like Pb, and irregular graphite distribution leads to poor machinability and tool wear, despite the advantages of graphite steel being underutilized due to challenges in precipitating stable graphite without long-term heat treatment.
A graphite steel composition with specific elements (C, Si, Mn, P, S, Al, Ti, B, N) and a manufacturing process involving controlled heating, hot rolling, and graphitization heat treatment at 700-800°C for 5 hours or more, ensuring a 95% graphitization degree and uniform graphite distribution.
The solution results in a graphite steel with superior cutting performance, replacing conventional free-cutting steels and eliminating harmful elements, while maintaining excellent machinability and tool life.
Smart Images

Figure 2024536913000001 
Figure 2024536913000002 
Figure 2024536913000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a graphite steel wire rod, steel wire, graphite steel having excellent cutting performance, and a manufacturing method thereof, and more particularly to a graphite steel wire rod, steel wire, graphite steel having sulfur added thereto and having better cutting performance than general free-cutting steel, and a manufacturing method thereof. [Background technology]
[0002] Generally, free-cutting steels with machinability-imparting elements such as Pb, Bi, and S are used as materials for machine parts and other objects that require machinability. To improve the machinability of steel materials, low-melting-point machinability-imparting elements such as Pb and Bi are added to the steel to use the liquid metal embrittlement phenomenon or to form a large amount of MnS in the steel. Such free-cutting steels are extremely excellent in terms of machinability, such as surface roughness during cutting, chip processing ability, and tool life.
[0003] However, free-cutting steels with added Pb, which has the best machinability, emit harmful substances such as toxic fumes during cutting, which are harmful to the human body, and also have problems with recycling the steel. Therefore, the addition of S, Bi, Te, Sn, etc. has been proposed as an alternative, but it has been known that there are problems with production being very difficult as cracks tend to occur during steel manufacturing, and there are also many problems with cracks occurring during hot rolling. Graphite steel is an example of a free-cutting steel that has been developed to solve the problems mentioned above. Graphite steel is a steel that contains fine graphite grains inside a ferrite matrix or a ferrite and pearlite matrix, and the fine graphite grains inside act as a crack supply source during cutting and act as chip breakers, resulting in a steel with good machinability.
[0004] However, despite these advantages of graphite steel, it is not currently commercially available because when carbon is added to steel, graphite is a stable phase, but a metastable phase of cementite precipitates, and it is difficult to precipitate graphite without a separate long-term heat treatment of at least 10 hours. During this long-term heat treatment, decarburization occurs, which has a detrimental effect on the performance of the final product.
[0005] Furthermore, even if graphite grains are precipitated through graphitization heat treatment, if they are irregularly shaped and unevenly distributed, the distribution of physical properties during cutting is uneven, resulting in poor chip processing and surface roughness, and shortened tool life, making it difficult to obtain the advantages of graphite steel. Therefore, there is a need to provide a method for producing graphite free-cutting steel with excellent cutting performance by using graphite grains and utilizing MnS-based inclusions. Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a graphite steel wire rod, a steel wire, and a graphite steel having excellent machinability, and a method for producing the same. [Means for solving the problem]
[0007] The graphite steel wire rod of the present invention is characterized by comprising, by weight, 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less (excluding 0) phosphorus (P), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the remainder being Fe and unavoidable impurities.
[0008] The method for producing graphite steel wire rod of the present invention is characterized by comprising the steps of producing a billet containing, by weight, 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less phosphorus (P) (excluding 0), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the balance being Fe and unavoidable impurities; heating the billet; hot-rolling the heated billet to produce a wire rod; and cooling the wire rod.
[0009] The graphite steel wire of the present invention is characterized by comprising, by weight, 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less phosphorus (P) (excluding 0), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the remainder being Fe and unavoidable impurities.
[0010] The graphite steel of the present invention is characterized in that it contains, by weight, 0.60 to 0.90% carbon (C), 2.0 to 2.5% silicon (Si), 0.1 to 0.6% manganese (Mn), 0.015% or less (excluding 0) phosphorus (P), 0.031 to 0.3% sulfur (S), 0.01 to 0.05% aluminum (Al), 0.005 to 0.02% titanium (Ti), 0.0005 to 0.0020% boron (B), 0.0030 to 0.0150% nitrogen (N), with the balance being Fe and unavoidable impurities, and has a microstructure in which graphite grains are distributed in a ferrite matrix, has a degree of graphitization of 95% or more, and contains a total of 5% or less of MnS inclusions and pearlite.
[0011] The method for producing graphite steel of the present invention is characterized by comprising the steps of: producing a wire rod consisting of, by weight, 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less (excluding 0) phosphorus (P), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the balance being Fe and unavoidable impurities; and subjecting the produced wire rod to a graphitization heat treatment. Effect of the Invention
[0012] INDUSTRIAL APPLICABILITY According to the present invention, the graphite steel of the present invention has excellent cutting performance and can replace conventional free-cutting steel materials, and can be used as an environmentally friendly free-cutting steel that is free of harmful elements such as Pb. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The graphite steel wire rod according to one embodiment of the present invention is composed, by weight, of 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less (excluding 0) phosphorus (P), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the remainder being Fe and unavoidable impurities.
[0014] Hereinafter, the graphite steel wire rod, steel wire, graphite steel, and a method for producing the same according to the present invention, which are excellent in cutting performance, will be described in detail. [Graphite steel wire] The graphite steel wire rod according to one embodiment of the present invention is composed, by weight, of 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less (excluding 0) phosphorus (P), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the remainder being Fe and unavoidable impurities. Hereinafter, unless otherwise specified, the unit is % by weight. Furthermore, when any part is said to "contain" a certain component, this does not mean that other components are excluded, but that other components may be further contained, unless otherwise specified to the contrary. [Range of ingredients]
[0015] Carbon (C): 0.60~0.90% by weight Carbon is an essential element for forming graphite grains. If the carbon content is less than 0.60% by weight, the effect of improving machinability is insufficient, and the distribution of graphite grains becomes non-uniform even after graphitization is completed. If the carbon content is excessively high, such as 0.90% by weight or more, the graphite grains are generated coarsely, the aspect ratio becomes large, and machinability, particularly surface roughness, may decrease. Therefore, the upper limit of the carbon content is preferably 0.90% by weight.
[0016] Silicon (Si): 2.0 to 2.5% by weight Silicon is a necessary component as a deoxidizer in the production of molten steel, and is a graphitization-promoting element that destabilizes cementite in steel and precipitates carbon as graphite, so it is added positively. In order to exhibit such effects in the present invention, the silicon content is preferably 2.0% by weight or more. On the other hand, if the content is excessive, not only the effect is saturated, but also the hardness increases due to the solid solution strengthening effect, tool wear is accelerated during cutting, brittleness is induced due to an increase in nonmetallic inclusions, and excessive decarburization is induced during hot rolling. Therefore, the upper limit of the silicon content is preferably 2.5% by weight.
[0017] Manganese (Mn): 0.1 to 0.6% by weight Manganese improves the strength and impact properties of steel, and combines with sulfur in the steel to form MnS inclusions, thereby contributing to improved machinability. In order to achieve such effects in the present invention, manganese is preferably contained in an amount of 0.1% by weight or more. On the other hand, if the content is excessive, it may inhibit graphitization, delay the graphitization completion time, and increase strength and hardness, thereby reducing machinability. Therefore, the upper limit of the manganese content is preferably 0.6% by weight.
[0018] Phosphorus (P): 0.015% by weight or less (excluding 0) Phosphorus is an unavoidably contained impurity. Even though phosphorus weakens the grain boundaries of steel and aids machinability, it increases the hardness of ferrite through a significant solid solution strengthening effect, reduces the toughness and delayed fracture resistance of steel, and promotes the occurrence of surface defects, so it is preferable to control the phosphorus content as low as possible. Theoretically, it is advantageous to control the phosphorus content to 0% by weight, but it is inevitably contained in the manufacturing process. Therefore, it is important to control the upper limit, and in the present invention, the upper limit is controlled to 0.015% by weight.
[0019] Sulfur (S): 0.031~0.3% by weight Sulfur has an effect of improving machinability by generating MnS, but on the other hand, when it is contained in excess, mechanical anisotropy appears due to MnS elongated by rolling. In the present invention, sulfur is added in a range that does not cause mechanical anisotropy and can contribute to improving machinability, thereby inducing the generation of MnS. Specifically, when sulfur is contained in the range of 0.031 to 0.3 wt%, MnS is generated to improve machinability, and 100% cutting performance is achieved compared to lead free-cutting steel. However, when the sulfur content is controlled to less than 0.031 wt%, MnS inclusions cannot be formed to a degree that improves cutting performance. Also, when it exceeds 0.3 wt%, the anisotropy of the material increases, causing a phenomenon of breakage during cutting processing, which is dangerous for workers.
[0020] Aluminum (Al): 0.01 to 0.05% by weight Aluminum is the element that promotes graphitization next to silicon. This is because aluminum makes cementite unstable when it exists as solid solution Al. Therefore, it is necessary for aluminum to exist as solid solution Al. In order to exhibit such an effect in the present invention, it is preferable that aluminum is contained in an amount of 0.01% by weight or more. On the other hand, if the content is excessive, not only the effect is saturated, but there is also a risk of inducing nozzle clogging during continuous casting, and AlN is generated at the austenite grain boundary, and graphite with AlN as a nucleus is distributed unevenly at the grain boundary. Therefore, the upper limit of the aluminum content is preferably 0.05% by weight.
[0021] Titanium (Ti): 0.0051 to 0.02% by weight Titanium combines with nitrogen to form nitrides such as TiN, BN, and AlN, as with boron and aluminum, and these nitrides act as nuclei for graphite formation during isothermal heat treatment. However, since BN, AlN, and the like have a low formation temperature, they are unevenly precipitated at grain boundaries after austenite is formed. In contrast, TiN has a higher formation temperature than AlN and BN, so it crystallizes before austenite formation is completed, and is uniformly distributed at austenite grain boundaries and within grains. Therefore, the graphite grains formed using TiN as a nucleation agent are also finely and uniformly distributed. In order to exhibit such an effect, it is preferable that the content is 0.0051% by weight or more. On the other hand, if the content exceeds 0.02%, it becomes coarse carbonitrides, which consumes carbon necessary for graphite formation and inhibits graphitization. Therefore, the upper limit of the titanium content is preferably 0.02% by weight.
[0022] Nitrogen (N): 0.0030 to 0.0150% by weight Nitrogen combines with titanium, boron, and aluminum to form TiN, BN, AlN, etc., and nitrides such as BN and AlN are mainly formed at the austenite grain boundaries. During graphitization heat treatment, graphite is formed with these nitrides as nuclei, which can cause uneven distribution of graphite, so it is necessary to add an appropriate amount of nitrogen. If the amount of nitrogen added is too much and it does not combine with nitride-forming elements and exists in the steel as solid solution nitrogen, it has the disadvantageous effect of increasing strength, stabilizing cementite, and delaying graphitization. Therefore, in order to consume nitrogen to form nitrides that act as graphite nucleation sites and not remain as solid solution nitrogen, the nitrogen content is limited to 0.0030% by weight as the lower limit and 0.0150% by weight as the upper limit in the present invention.
[0023] Boron (B): 0.0005 to 0.0020% BN is positively added because it bonds with N to form BN, which acts as a nucleus for the crystallization of graphite and promotes graphitization, but if it is added less than 0.0005% by weight, the effect is small, and if it is added in excess of 0.0020% by weight, BN is formed in excess at the austenite grain boundaries, which not only causes non-uniform distribution of graphite grains after graphitization heat treatment but also weakens the grain boundaries, causing a significant decrease in hot rolling properties. Therefore, it is preferable to add BN in the range of 0.0005 to 0.0020% by weight.
[0024] The remaining components of the present invention are iron (Fe) and inevitable impurities. However, in a normal steel manufacturing process, unintended impurities may be inevitably mixed in from raw materials or the surrounding environment, and it is not possible to exclude them. Since any engineer of a normal steel manufacturing process would know about these impurities, the contents of all of them will not be specifically mentioned in this specification.
[0025] According to one embodiment of the present invention, the wire for graphitization heat treatment may have an area fraction of pearlite of 95% or more. In the present invention, since graphite grains are generated by decomposition of pearlite, if the area fraction of pearlite is low, the graphite grain fraction is also low, which is undesirable since it shows a non-uniform distribution. Since a high area fraction of pearlite is advantageous for ensuring uniform and fine graphite grains, the upper limit is not particularly limited. [Wire rod manufacturing method]
[0026] A method for producing a graphite steel wire rod according to an embodiment of the present invention includes the steps of producing a billet containing, by weight percent, 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less phosphorus (P) (excluding 0), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the remainder being Fe and unavoidable impurities; heating the billet; hot rolling the heated billet into a wire rod; and Cooling the wire is included. Wire heating process
[0027] According to an embodiment of the present invention, the heating step may include performing heat treatment at a temperature in the range of 1050±100° C. for 60 minutes or more. Before rolling the billet into wire rod, the billet is maintained at a temperature in the range of 1050±100°C for 60 minutes or more. If the billet heating temperature is less than 950°C, the load increases during rolling and rolling productivity may decrease, so a low heating temperature is disadvantageous. If the heating temperature exceeds 1150°C, not only does the cost increase, but the decarburization is accelerated and the decarburized layer becomes thick and remains in the final product, which is undesirable. The heating maintenance time is set to 60 minutes or more because it is difficult to ensure a uniform temperature distribution inside and outside the billet for wire rod rolling if the heating time is less than 60 minutes. Wire rod rolling process
[0028] According to an embodiment of the present invention, the hot rolling to produce a wire rod may be performed at a temperature in the range of 900 to 1150°C. The wire rod rolling temperature is set in the range of 900 to 1150°C because, if the temperature is less than 900°C, surface defects are likely to occur during hot rolling or the rolling load is increased, making rolling difficult, whereas, if the temperature exceeds 1150°C, the AGS (austenite grain size) becomes coarse and the graphitization heat treatment time after wire rod rolling may become long. cooling process
[0029] According to an embodiment of the present invention, the cooling step may be performed to 500° C. at a cooling rate of 0.1 to 10.0° C. / s. According to an embodiment of the present invention, the method may further include a step of air-cooling after the step of cooling. A cooling rate of more than 10.0°C is not preferred because a hard phase such as martensite is generated, which may cause wire breakage during cold drawing, which is the next step after wire rolling.A cooling rate of less than 0.1°C is not preferred because an excessive amount of pro-eutectoid phase is generated, the pearlite fraction is reduced, the crystal grain size is coarsened, and the graphite grains generated after graphitization heat treatment have a non-uniform distribution. [Graphite steel wire]
[0030] The graphite steel wire according to one embodiment of the present invention is composed, by weight, of carbon (C): 0.60-0.90%, silicon (Si): 2.0-2.5%, manganese (Mn): 0.1-0.6%, phosphorus (P): 0.015% or less (excluding 0), sulfur (S): 0.031-0.3%, aluminum (Al): 0.01-0.05%, titanium (Ti): 0.005-0.02%, boron (B): 0.0005-0.0020%, nitrogen (N): 0.0030-0.0150%, and the remainder being Fe and unavoidable impurities. [Graphite steel]
[0031] Graphite steel according to one embodiment of the present invention is composed, by weight, of 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less phosphorus (P) (excluding 0), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), with the balance being Fe and unavoidable impurities. As a microstructure, graphite grains are distributed in a ferrite matrix, the degree of graphitization is 95% or more, and the steel contains a total of 5% or less MnS inclusions and pearlite.
[0032] The degree of graphitization means the ratio of the carbon content present in the graphite state to the carbon content added to the steel, and is defined by the following [Relationship 1]. 95% or more graphitization means that most of the added carbon has been consumed to produce graphite (the amount of carbon dissolved in ferrite and in fine carbides is not taken into account since it is very small), and that there is no undecomposed pearlite, i.e., the steel has a fine structure in which graphite grains are distributed in the ferrite matrix. [Equation 1] Degree of graphitization (%) = (1 - carbon content in undecomposed pearlite / carbon content in steel) x 100 (If there is no undecomposed pearlite, the degree of graphitization is 100%) [Graphite steel manufacturing method]
[0033] A method for producing graphite steel according to one embodiment of the present invention includes the steps of producing a wire rod consisting of, by weight, 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less phosphorus (P) (excluding 0), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the balance being Fe and unavoidable impurities, and subjecting the produced wire rod to a graphitization heat treatment.
[0034] According to an embodiment of the present invention, the graphitization heat treatment may be performed at a temperature of 700 to 800° C. for 5 hours or more. If the heat treatment is maintained in the range of 700 to 800°C for 5 hours or more, a graphitization degree of 95% or more can be achieved. However, if the temperature is less than 700°C, the graphitization heat treatment time becomes long and exceeds 10 hours. If the temperature exceeds 800°C, not only does the graphitization time become long, but austenite is generated by reverse transformation of pearlite, and further pearlite may be generated during cooling, which is not preferable. The present invention will now be described more specifically with reference to examples. The following examples are presented to fully convey the concept of the present invention to those skilled in the art to which the present invention pertains, and the present invention is not limited to the examples presented herein and may be embodied in other forms. (Example)
[0035] A billet containing the components shown in Table 1 below was maintained at the heating temperature conditions for 90 minutes and then rolled at high speed into a wire rod having a diameter of 19 mm. The cooling rate of the wire rod, the area fraction of pearlite in the wire rod, the graphitization heat treatment time, and the degree of graphitization are shown in Table 1 below. In Tables 1 and 2, Examples 1 to 11 correspond to graphite steel wire rods that satisfy the alloy composition range and manufacturing conditions of the present invention, and Comparative Examples 1 to 7 correspond to wire rods that do not satisfy the alloy composition range and / or manufacturing conditions of the present invention.
[0036] [Table 1] *Cutting performance is a numerical value based on the cutting performance of lead free-cutting steel (100% means the same level).
[0037] [Table 2] *(100%-graphitization degree) structure is composed of MnS inclusions and pearlite, and graphitized structure is composed of ferrite + graphite grains. It can be confirmed that the pearlite area fraction and graphitization degree are achieved under the wire and graphitization manufacturing conditions shown in Table 2 above.
[0038] The Examples and Comparative Examples will be evaluated below with reference to Tables 1 and 2. In Examples 1 to 11, by satisfying the alloy composition range and manufacturing conditions of the present invention, it was confirmed that the graphite steel wire had a pearlite area fraction of 95% or more, a graphitization degree of 98.5% or more, and cutting performance that was 100% of that of lead free-cutting steel.
[0039] On the other hand, the cutting performance of the graphite steel of Comparative Example 1, which had a sulfur content of only 0.005% by weight and was substantially free of boron, was low at 88% compared to lead-based free-cutting steel, and the wire manufacturing method of Comparative Example 1 was cooled at a cooling rate of 0.05°C / s, producing a wire containing an area fraction of pearlite of 93%, and the heat treatment was maintained for 1.5 hours, resulting in a low graphitization degree of 75%. In addition, the cutting performance of the graphite steel of Comparative Example 2, which contains only 0.003% by weight of sulfur and only 0.0002% by weight of boron, is low at 95% compared to lead free-cutting steel, and the wire rod manufacturing method of Comparative Example 2 involves cooling at a cooling rate of 12.0°C / s. A wire rod containing a pearlite area fraction of 93.5% was manufactured and maintained for 2.5 hours in heat treatment, resulting in a low graphitization degree of 85%. In addition, the cutting performance of the graphite steel of Comparative Example 3, which had a sulfur content of only 0.006 wt% and a boron content of only 0.0004 wt%, was low at 89% compared to lead free-cutting steel, and the wire manufacturing method of Comparative Example 3 was cooled at a cooling rate of 11.5°C / s, producing a wire containing an area fraction of pearlite of 94.2%, and the heat treatment was maintained for 3.0 hours, resulting in a low graphitization degree of 86%.
[0040] In addition, the cutting performance of the graphite steel of Comparative Example 4, which had a carbon content of 0.95 wt%, a sulfur content of 0.007 wt%, and a boron content of 0.0025 wt%, was low at 92% compared to lead free-cutting steel, and in the wire manufacturing method of Comparative Example 4, a wire containing 93.2% pearlite area fraction was manufactured by cooling at a cooling rate of 0.07°C / s, and the heat treatment was maintained for 2.5 hours, resulting in a low graphitization degree of 85%.
[0041] In addition, the cutting performance of the graphite steel of Comparative Example 5, which had a carbon content of 0.55 wt%, a silicon content of 2.6 wt%, a sulfur content of 0.4 wt%, a titanium content of 0.025 wt%, and a boron content of 0.0025 wt%, was low at 91% compared to lead free-cutting steel, and the wire manufacturing method of Comparative Example 5 was cooled at a cooling rate of 15.5°C / s, produced a wire containing an area fraction of pearlite of 93.5%, and maintained the heat treatment for 3.4 hours, resulting in a low graphitization degree of 86%. In addition, the cutting performance of the graphite steel of Comparative Example 6, which had a silicon content of 2.75 wt%, a manganese content of 0.9 wt%, a sulfur content of 0.45 wt%, a titanium content of 0.03 wt%, and a boron content of 0.0024 wt%, was low at 93% compared to lead free-cutting steel, and the wire manufacturing method of Comparative Example 6 was cooled at a cooling rate of 14.0°C / s, producing a wire containing an area fraction of pearlite of 94.1%, and maintaining the wire in heat treatment for 4.2 hours, resulting in a low graphitization degree of 84%.
[0042] In addition, the graphite steel of Comparative Example 7, which had a silicon content of 2.8 wt%, a manganese content of 0.8 wt%, a sulfur content of 0.35 wt%, a titanium content of 0.002 wt%, and a boron content of 0.003 wt%, had cutting performance that was only 90% lower than that of the lead free-cutting steel. From the evaluation of each of the above-mentioned Examples and Comparative Examples, it is clear that when the range of the alloy composition and the manufacturing conditions of the present invention are satisfied, all of the properties of the graphite steel wire rod and graphite steel of the present invention can be satisfied. [Industrial Applicability]
[0043] INDUSTRIAL APPLICABILITY The graphite steel according to the present invention has excellent cutting performance and can replace conventional free-cutting steel materials. It can also be used as an environmentally friendly free-cutting steel that replaces harmful elements such as Pb, and therefore has industrial applicability.
Claims
1. Graphite steel wire rod having excellent cutting performance, characterized in that it consists, by weight, of 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less phosphorus (P) (excluding 0), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the remainder being Fe and unavoidable impurities.
2. 2. The graphite steel wire rod having excellent cutting performance according to claim 1, characterized in that the area fraction of pearlite is 95% or more.
3. producing a billet consisting of, in weight percent, 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less phosphorus (P) (excluding 0), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the balance being Fe and unavoidable impurities; heating the billet; hot rolling the heated billet to produce a wire rod; and The method for producing a graphite steel wire having excellent cutting performance, further comprising the step of cooling the wire.
4. 4. The method of claim 3, wherein the heating step comprises maintaining the temperature in the range of 1050±100° C. for 60 minutes or more.
5. 4. The method of claim 3, wherein the hot rolling to produce the wire is performed at a temperature in the range of 900 to 1150°C.
6. 4. The method of claim 3, wherein the cooling step comprises cooling the wire to 500° C. at a cooling rate of 0.1 to 10.0° C. / s.
7. 4. The method of claim 3, further comprising the step of air-cooling after the cooling step.
8. A graphite steel wire having excellent cutting performance, characterized in that it consists, by weight, of carbon (C): 0.60-0.90%, silicon (Si): 2.0-2.5%, manganese (Mn): 0.1-0.6%, phosphorus (P): 0.015% or less (excluding 0), sulfur (S): 0.031-0.3%, aluminum (Al): 0.01-0.05%, titanium (Ti): 0.005-0.02%, boron (B): 0.0005-0.0020%, nitrogen (N): 0.0030-0.0150%, and the remainder being Fe and unavoidable impurities.
9. In weight percent, carbon (C): 0.60-0.90%, silicon (Si): 2.0-2.5%, manganese (Mn): 0.1-0.6%, phosphorus (P): 0.015% or less (excluding 0), sulfur (S): 0.031-0.3%, aluminum (Al): 0.01-0.05%, titanium (Ti): 0.005-0.02%, boron (B): 0.0005-0.0020%, nitrogen (N): 0.0030-0.0150%, and the balance being Fe and unavoidable impurities. A graphite steel with excellent cutting performance, characterized in that the microstructure has graphite grains distributed in a ferrite matrix, has a graphitization degree of 95% or more, and contains a total of 5% or less of MnS inclusions and pearlite.
10. a step of manufacturing a wire consisting of, in weight percent, 0.60-0.90% carbon (C), 2.0-2.5% silicon (Si), 0.1-0.6% manganese (Mn), 0.015% or less phosphorus (P) (excluding 0), 0.031-0.3% sulfur (S), 0.01-0.05% aluminum (Al), 0.005-0.02% titanium (Ti), 0.0005-0.0020% boron (B), 0.0030-0.0150% nitrogen (N), and the balance being Fe and unavoidable impurities; The method for producing graphite steel having excellent cutting performance includes a step of graphitizing the produced wire rod by heat treatment.
11. 11. The method of claim 10, wherein the graphitization heat treatment is performed at a temperature of 700 to 800° C. for 5 hours or more.
Citation Information
Patent Citations
Steel material for graphitization and graphite steel with excellent machinability
CN106191710A
Production of hot forged steel parts excellent in machinability, the parts and hot rolled steel used therefor
JP1999350066A
Steel for machine structure superior in machinability
JP2003034840A
Hot forged product
US20190127817A1
Wire rod for graphitization heat treatment, graphite steel, and manufacturing method therefor
WO2021149849A1