Solid electrolyte for all-solid-state battery

A Li, K, and Bi oxide-based solid electrolyte for all-solid-state batteries addresses high-temperature sintering issues and low conductivity by enabling low-temperature sintering and enhanced ionic conductivity.

JP2024536978AActive Publication Date: 2024-10-10ベイス カンパニーリミテッド
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024512061
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-16
Filing Date
2022-10-24
Publication Date
2024-10-10
Estimated Expiration
2042-10-24

AI Technical Summary

Technical Problem

Existing oxide-based solid electrolytes for all-solid-state batteries face challenges with high sintering temperatures, leading to increased manufacturing costs and relatively low ionic conductivity, while sulfide-based electrolytes are prone to moisture reaction and hydrogen sulfide gas generation.

Method used

A solid electrolyte composed of Li, K, and Bi oxides with a specific molar ratio, forming a bismuth oxide crystal structure, allows for low-temperature sintering and enhanced ionic conductivity.

Benefits of technology

The electrolyte achieves excellent ionic conductivity with sintering temperatures between 540°C to 600°C, significantly improving manufacturing efficiency and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536978000001_ABST
    Figure 2024536978000001_ABST
Patent Text Reader

Abstract

The present invention relates to a solid electrolyte for an all-solid-state battery. The solid electrolyte for an all-solid-state battery according to one embodiment of the present invention is made of an oxide containing Li, K and Bi.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid electrolyte for an all-solid-state battery. [Background technology]

[0002] Recently, the use of secondary batteries has increased significantly in various fields, from IT devices such as mobile phones to electric vehicles and energy storage devices.

[0003] Lithium-ion batteries, which use liquid electrolytes, are the most widely used secondary batteries. However, liquid electrolytes pose a risk of tearing if the battery is subjected to external impact, and as a result, additional parts and devices are required to ensure safety.

[0004] Recently, in order to improve the safety of secondary batteries, active development of all-solid-state batteries that use solid electrolytes as electrolytes is underway. Solid electrolytes for all-solid-state batteries include polymer electrolytes, oxide electrolytes, and sulfide electrolytes. Of these, sulfide solid electrolytes have the highest ionic conductivity, but they react with moisture to generate hydrogen sulfide gas. Polymer electrolytes have the advantage of being relatively simple to process and can be used with existing lithium-ion battery processes, but have the disadvantage of significantly low ionic conductivity.

[0005] Oxide-based electrolytes have the advantage of being safer than sulfide-based electrolytes, but have relatively low ionic conductivity. In addition, oxide-based electrolytes generally require a high sintering temperature of 1,000°C or higher, which can significantly increase manufacturing costs. Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made to solve the above-mentioned problems of the prior art, and an object of the present invention is to provide a solid electrolyte for an all-solid-state battery that can be sintered at a low temperature and has excellent ionic conductivity. [Means for solving the problem]

[0007] A solid electrolyte for an all-solid-state battery according to an embodiment of the present invention is made of an oxide containing Li, K and Bi.

[0008] The solid electrolyte for an all-solid-state battery according to an embodiment of the present invention can satisfy, based on the molar ratio of each component, 0.2≦(Li+K) / Bi<1. Also, the solid electrolyte for an all-solid-state battery according to an embodiment of the present invention can satisfy, based on the molar ratio of each component, 0.2≦(Li+K) / Bi≦0.6.

[0009] The solid electrolyte for an all-solid-state battery according to an embodiment of the present invention may satisfy 0.1≦Li<0.5 based on the molar ratio. Also, the solid electrolyte for an all-solid-state battery according to an embodiment of the present invention may satisfy 0.10≦K≦0.15 based on the molar ratio.

[0010] The solid electrolyte for the all-solid-state battery according to an embodiment of the present invention may have a bismuth oxide crystal structure.

[0011] The solid electrolyte for the all-solid-state battery according to an embodiment of the present invention may have a softening point of 540°C to 600°C.

[0012] The solid electrolyte for the all-solid-state battery according to an embodiment of the present invention may have a half-ball temperature of 550°C to 660°C.

[0013] In addition, the solid electrolyte for an all-solid-state battery according to the present invention may further include other additional components within a range that does not impair the technical concept of the present invention. Effect of the Invention

[0014] According to an embodiment of the present invention, the solid electrolyte for the all-solid-state battery contains Li, K and Bi, and thus can have excellent ion conductivity while being capable of being sintered at a low temperature. [Brief description of the drawings]

[0015] [Figure 1]1 is a diagram illustrating a cross section of an all-solid-state battery. [Diagram 2] 1 shows a ternary diagram illustrating the composition ranges of solid electrolytes according to examples and comparative examples of the present invention. [Diagram 3] 1 shows an XRD graph of a solid electrolyte according to an embodiment of the present invention. [Figure 4] 3 shows an XRD graph of a solid electrolyte according to a comparative example of the present invention. [Diagram 5] 3 shows an XRD graph of a solid electrolyte according to a comparative example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings to such an extent that those skilled in the art to which the present invention pertains can easily carry out the present invention.

[0017] In order to clearly explain the present invention, the description of parts not related to the present invention will be omitted, and the same reference numerals will be used for the same components throughout the specification. It should be understood that the specific shapes, structures, and characteristics described in the specification may be changed from one embodiment to another without departing from the spirit and scope of the present invention, and the position or arrangement of individual components may also be changed without departing from the spirit and scope of the present invention.

[0018] Therefore, the following detailed description should not be taken in a limiting sense, and the scope of the present invention should be understood to encompass the scope of the appended claims and all equivalents thereof.

[0019] FIG. 1 is a drawing that illustrates a cross section of an all-solid-state battery.

[0020] 1, an all-solid-state battery 10 includes a positive electrode 11, a negative electrode 12, and a solid electrolyte layer 13. The solid electrolyte layer 13 is disposed between the positive electrode 11 and the negative electrode 12, and may be in contact with the positive electrode 11 and the negative electrode 12, respectively. The positive electrode 11 and the negative electrode 12 may each include a positive electrode active material layer and a negative electrode active material layer, and the positive electrode active material layer and the negative electrode active material layer may each be in contact with the solid electrolyte layer 13.

[0021] The positive electrode 11 and the negative electrode 12 can each be joined to the solid electrolyte layer 13 by sintering. That is, the positive electrode 11, the negative electrode 12 and the solid electrolyte layer 13 can be sintered together.

[0022] 1 illustrates an all-solid-state battery 10 including one layer each of a positive electrode 11, a negative electrode 12, and a solid electrolyte layer 13, but the present invention is not limited to this, and the all-solid-state battery may be configured such that the positive electrode, the negative electrode, and the solid electrolyte layer each include multiple layers. Alternatively, the all-solid-state battery may be configured as a so-called stacked type all-solid-state battery in which multiple positive electrodes, negative electrodes, and solid electrolyte layers are stacked alternately.

[0023] The solid electrolyte layer 13 according to an embodiment of the present invention includes an oxide-based electrolyte as a solid electrolyte.

[0024] Known oxide-based solid electrolytes include Nasicon-type solid electrolytes such as LAGP and Garnet-type solid electrolytes such as LLZO. Through continuous research and development, the ionic conductivity of these oxide-based solid electrolytes is expected to increase by 10 -4 It is known that the level has improved to S / cm.

[0025] However, there is a limit to how much the ionic conductivity can be improved with the Nasicon and Garnet types of oxide-based solid electrolytes.Moreover, these oxide-based solid electrolytes are sintered at high temperatures of over 1,000℃, and although they can achieve a certain level of excellent ionic conductivity, as mentioned above, the increase in manufacturing costs due to high temperature sintering is unavoidable.

[0026] In one embodiment of the present invention, a new oxide-based solid electrolyte that overcomes the limitations of the conventional oxide-based solid electrolyte ensures excellent ion conductivity while lowering the sintering temperature.

[0027] According to an embodiment of the present invention, the solid electrolyte for the all-solid-state battery may be made of an oxide containing Li, K, and Bi. In one embodiment, the solid electrolyte for the all-solid-state battery may have a bismuth oxide crystal structure.

[0028] In the composition of the solid electrolyte, Bi forms a crystalline structure and is a low-temperature component that plays a role in lowering the sintering temperature.

[0029] In the composition of the solid electrolyte, Li and K can function as a network modifier and increase the lattice constant of the bismuth oxide crystal structure, which in turn can ensure a wider path for Li ions to move in the crystal structure, improving ion conductivity.

[0030] As described above, the solid electrolyte according to an embodiment of the present invention is composed of an oxide containing Li, K, and Bi, and thus Bi functions as a main component of the crystal structure, and Li and K can widen the flow path of Li ions to lower the sintering temperature.

[0031] According to one embodiment of the present invention, the components constituting the solid electrolyte may have a specific composition range.

[0032] The solid electrolyte according to an embodiment of the present invention may satisfy the following relational expression based on the molar ratio of each component.

[0033] 2≦(Li+K) / Bi<1

[0034] Preferably, the solid electrolyte according to an embodiment of the present invention may satisfy the following relational expression based on the molar ratio of each component.

[0035] (2) 0.2≦(Li+K) / Bi≦0.6

[0036] When the molar ratio of the alkaline components (Li and K) and the molar ratio of Bi in the solid electrolyte satisfy the above-mentioned relational formula, the ionic conductivity can be significantly improved.

[0037] The solid electrolyte according to an embodiment of the present invention may further satisfy the following relational expression based on the molar ratio.

[0038] (3) 0.10≦Li<0.5

[0039] (4) 0.10≦K≦0.15

[0040] When the molar ratio of the alkaline components (Li and K) in the solid electrolyte satisfies the above range, the ionic conductivity can be improved.

[0041] The sintering temperature of the solid electrolyte according to one embodiment of the present invention is about 500° C. to about 600° C. When sintered at the above temperature, the solid electrolyte according to one embodiment of the present invention has a melting point of about 2.4×10 -4 ~Approx. 5.8×10 -4 The ionic conductivity in S / cm is shown.

[0042] Working Example

[0043] Example 1

[0044] A precursor powder for manufacturing a solid electrolyte was prepared by mixing 10 mol% Li2O, 12.5 mol% K2O, and 77.5 mol% Bi2O3. After mixing the precursor powder, it was placed in a melting furnace and melted at a temperature of about 1,000°C for about 30 minutes. The homogenized melt was then poured into a quenching roller and cooled to room temperature, and was then crushed and sieved to obtain fine particles with a size of 10 μm or less. Finally, the obtained fine particles were sintered at about 500°C for about 6 hours to manufacture a solid electrolyte.

[0045] Additional Examples and Comparative Examples

[0046] Precursor powders were prepared with different composition ratios of Li2O and Bi2O3, and melted at temperatures of 800°C to 1,200°C for about 30 minutes depending on the composition ratio. Then, fine particles were obtained through the same process as in Example 1, and solid electrolytes were manufactured by sintering at about 500°C for about 6 hours.

[0047] The solid electrolyte composition ratios in each of the examples and comparative examples described above are as shown in Table 1.

[0048] [Table 1]

[0049] 2 is a ternary diagram illustrating the composition ranges of solid electrolytes according to examples and comparative examples of the present invention. In FIG. 2, 1 to 4 correspond to Examples 1 to 4, and 5 to 9 correspond to Comparative Examples 1 to 5.

[0050] 2, Examples 1 to 4, Comparative Example 2, and Comparative Examples 3 to 5 have different crystal structures. Specifically, Examples 1 to 4 have a bismuth oxide crystal structure, Comparative Example 2 has a lithium-bismuth oxide crystal structure, and Comparative Examples 3 to 5 have a glass-ceramic structure. Comparative Example 1 is located at the boundary between the bismuth oxide crystal structure and the lithium oxide-bismuth oxide crystal structure.

[0051] FIG. 3 shows an XRD graph of a solid electrolyte according to one example (Example 3) of the present invention, and FIGS. 4 and 5 show XRD graphs of solid electrolytes according to comparative examples (Comparative Examples 2 and 4) of the present invention.

[0052] 3, it can be seen that the solid electrolyte according to the embodiment of the present invention has a single-phase bismuth oxide crystal structure, whereas the solid electrolyte according to the comparative example has a lithium oxide-bismuth oxide crystal structure (see FIG. 4) or a glass-ceramic structure (see FIG. 5).

[0053] The crystal structure, softening point, half-ball temperature, and ionic conductivity of the solid electrolytes according to the respective examples and comparative examples are shown in Table 2.

[0054] [Table 2]

[0055] Referring to Table 2, the solid electrolytes according to Examples 1 to 4 of the present invention have a softening point of 600° C. or less and a half-ball temperature of 660° C. or less. As described above, the solid electrolytes according to the examples of the present invention have excellent low-temperature properties compared to conventional oxide-based solid electrolytes, and therefore can be sintered at low temperatures.

[0056] The solid electrolytes according to Examples 1 to 4 of the present invention have a melting point of 2.4 × 10 -4 ~5.8×10 -4 In comparison, the solid electrolyte according to the comparative example exhibits low-temperature characteristics similar to those of the embodiment, but has an ionic conductivity of 0.97×10 -6 ~1.7×10 -5 S / cm, which shows a large difference from the embodiment of the present invention.

[0057] As described above, it can be confirmed that the solid electrolytes according to Examples 1 to 4 of the present invention can be sintered at low temperatures and have excellent ionic conductivity.

[0058] Although the present invention has been described above using specific details such as specific components and limited examples, the above examples are merely provided to facilitate a more general understanding of the present invention, and the present invention is not limited thereto. Those having ordinary knowledge in the technical field to which the present invention pertains may make various modifications and variations from such descriptions.

[0059] Therefore, the concept of the present invention should not be limited to the above-described embodiments, and all modifications equivalent to or similar to the scope of the claims, as well as the scope of the following claims, can be said to fall within the scope of the concept of the present invention.

Claims

1. A solid electrolyte for an all-solid-state battery, Consists of an oxide containing Li, K and Bi; Solid electrolyte for all-solid-state batteries.

2. 2. The solid electrolyte for an all-solid-state battery according to claim 1, which satisfies 0.2≦(Li+K) / Bi<1 based on the molar ratio of each component.

3. 3. The solid electrolyte for an all-solid-state battery according to claim 2, which satisfies 0.2≦(Li+K) / Bi≦0.6 based on the molar ratio of each component.

4. 4. The solid electrolyte for an all-solid-state battery according to claim 2, which satisfies 0.1≦Li<0.5 based on a molar ratio.

5. The solid electrolyte for an all-solid-state battery according to any one of claims 2 to 4, which satisfies 0.10≦K≦0.15 based on a molar ratio.

6. The solid electrolyte for an all-solid-state battery according to any one of claims 1 to 5, having a bismuth oxide crystal structure.

7. The solid electrolyte for an all-solid-state battery according to any one of claims 1 to 6, having a softening point of 540°C to 600°C.

8. The solid electrolyte for an all-solid-state battery according to any one of claims 1 to 7, wherein the half-ball temperature is 550°C to 660°C.

Citation Information

Patent Citations

  • Lithium ion conductor

    JP2021190206A

  • Novel lithium bismuth oxide compounds as li super-ionic conductor, solid electrolyte, and coating layer for li metal battery and li-ion battery

    US20200112052A1