Adhesive sheet and antenna structure including same

A pressure-sensitive adhesive sheet with tailored dielectric and modulus properties, using an acrylic copolymer blend, addresses dielectric loss and flexibility issues, enhancing antenna performance in flexible display devices.

JP2024537090APending Publication Date: 2024-10-10DONGWOO FINE CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024519872
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-07
Filing Date
2022-09-15
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing adhesive sheets for image display devices with high-frequency antennas suffer from dielectric loss and reduced radiation characteristics due to high dielectric constants, and they need to be flexible to accommodate bending and folding.

Method used

A pressure-sensitive adhesive sheet with a specific dielectric loss tangent and storage modulus range, composed of an acrylic copolymer blend with acrylate monomers of varying carbon lengths and polar monomers, ensuring reduced dielectric loss and improved flexibility.

Benefits of technology

The adhesive sheet maintains stable flexibility and bending properties, preventing antenna deterioration while promoting high-frequency radiation characteristics and reducing signal loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537090000001_ABST
    Figure 2024537090000001_ABST
Patent Text Reader

Abstract

An embodiment of the present invention provides a pressure-sensitive adhesive sheet, and an antenna structure and an image display device each including the pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet includes a pressure-sensitive adhesive layer having a dielectric loss tangent greater than 0 and not greater than 0.01 at 28 GHz measured at a thickness of 150 μm, a storage modulus of 10 to 50 kPa at 25° C., a first modulus ratio of 1.5 to 4.0, and a second modulus ratio of 1.0 to 3.5.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet and an antenna structure including the same, more particularly to a pressure-sensitive adhesive sheet including an acrylic copolymer and an antenna structure including the same. [Background technology]

[0002] In recent years, various information processing functions have been added to image display devices with combined communication functions such as smartphones, which allows one image display device to include structures such as a touch panel and an antenna, in addition to optical layers (e.g., polarizing plates, retardation plates, etc.) for implementing images.

[0003] For this reason, an adhesive layer or sheet is used to laminate the above-mentioned optical layers and structures on the display panel. For example, an adhesive sheet can be used to attach an antenna to the display panel.

[0004] Recently, high-frequency or ultra-high-frequency antennas have been adopted in image display devices, and the radiation characteristics of the antennas are easily hindered by the dielectric characteristics of the surroundings of the antennas. For example, if the dielectric constant of the adhesive sheet becomes high, dielectric loss or signal loss of the antenna occurs, and the impedance characteristics of the set antenna may be hindered.

[0005] In addition, with the development of flexible displays that can be folded or bent, adhesive layers or adhesive sheets applied to image display devices also need to be designed to have improved flexibility.

[0006] Therefore, it is necessary to develop an adhesive sheet that can be applied to flexible displays and has dielectric properties suitable for high-frequency and ultra-high-frequency communications.

[0007] For example, Korean Patent Publication No. 10-2021-0102035 discloses a pressure-sensitive adhesive composition for optical films containing a (meth)acrylic acid ester copolymer, but does not take into consideration the above-mentioned dielectric properties. Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a pressure-sensitive adhesive sheet having improved dielectric properties and flexibility.

[0009] It is an object of the present invention to provide an antenna structure including an adhesive sheet having improved dielectric properties and flexibility.

[0010] An object of the present invention is to provide an image display device to which the pressure-sensitive adhesive sheet is applied. [Means for solving the problem]

[0011] 1. The dielectric tangent at 28 GHz measured at a thickness of 150 μm is greater than 0 and is 0.01 or less, and the storage modulus at 25 ° C is 10 to 50 kPa; A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer having a first modulus ratio defined by the following formula 1 of 1.5 to 4.0 and a second modulus ratio defined by the following formula 2 of 1.0 to 3.5. [Formula 1] First modulus ratio = A / B [Formula 2] Second modulus ratio = B / C (In Equation 1 and Equation 2, A is the storage modulus of the pressure-sensitive adhesive layer at -20°C, B is the storage modulus of the pressure-sensitive adhesive layer at 25°C, and C is the storage modulus of the pressure-sensitive adhesive layer at 80°C.)

[0012] 2. A pressure-sensitive adhesive sheet according to item 1 above, wherein the pressure-sensitive adhesive layer comprises an acrylic copolymer polymerized from a monomer blend including a first acrylate monomer having less than 18 carbon atoms and a second acrylate monomer having 18 or more carbon atoms.

[0013] 3. The pressure-sensitive adhesive sheet as recited in claim 2, wherein in the monomer blend, a ratio of the weight of the second acrylate monomer to the weight of the first acrylate monomer is 0.2 to 9.

[0014] 4. The pressure-sensitive adhesive sheet according to item 2, wherein the monomer blend further contains a polar monomer containing a carboxyl group or an amide group.

[0015] 5. The pressure-sensitive adhesive sheet according to item 4, wherein the monomer blend contains, per 100 parts by weight of the monomer blend, 10 to 75 parts by weight of the first acrylate monomer, 20 to 85 parts by weight of the second acrylate monomer, and 0.5 to 10 parts by weight of the polar monomer.

[0016] 6. The pressure-sensitive adhesive sheet according to item 5, wherein the amount of the hydroxyl group-containing monomer is 2 parts by weight or less per 100 parts by weight of the monomer blend.

[0017] 7. The pressure-sensitive adhesive sheet according to item 2 above, wherein the second acrylate monomer includes 2-decyl-1-tetradecanyl(meth)acrylate or stearyl(meth)acrylate.

[0018] 8. The pressure-sensitive adhesive sheet according to item 1, wherein the dielectric tangent of the pressure-sensitive adhesive layer is 0.005 or less.

[0019] 9. The pressure-sensitive adhesive sheet according to item 1, wherein the storage modulus of the pressure-sensitive adhesive layer at 25° C. is 20 to 40 kPa.

[0020] 10. The pressure-sensitive adhesive sheet according to item 1, further comprising a protective film formed on at least one surface of the pressure-sensitive adhesive layer.

[0021] 11. An antenna structure comprising an antenna dielectric layer, an antenna electrode layer disposed on a top surface of the antenna dielectric layer, and the adhesive sheet of the previous embodiment attached on a bottom surface of the antenna dielectric layer.

[0022] 12. An image display device comprising a display panel and an antenna structure according to any one of the preceding embodiments attached onto the display panel. Effect of the Invention

[0023] The adhesive sheet according to the embodiment of the present invention may have a room temperature modulus and a temperature-dependent modulus ratio within a predetermined range, thereby providing improved folding properties and stable flexibility and bending properties when applied to a flexible display.

[0024] According to an exemplary embodiment, the adhesive sheet may have a dielectric loss tangent value within a predetermined range, thereby preventing the antenna gain and radiation characteristics from being deteriorated by the adhesive sheet while having improved folding characteristics.

[0025] Therefore, an antenna structure or flexible display having improved flexibility while maintaining the radiation reliability of a high frequency / ultra high frequency antenna can be realized by using the pressure sensitive adhesive sheet.

[0026] In an exemplary embodiment, the pressure-sensitive adhesive sheet includes a copolymer of acrylic monomers, and the acrylic monomers may include both acrylate monomers having 18 or more carbon atoms and acrylate monomers having less than 18 carbon atoms.

[0027] This makes it possible to effectively achieve both reduced dielectric loss of the pressure-sensitive adhesive sheet and improved flexibility, as described above. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a pressure-sensitive adhesive sheet according to an exemplary embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view illustrating an antenna structure and an image display device according to an exemplary embodiment. [Diagram 3]FIG. 3 is a schematic plan view illustrating an antenna structure and an image display device according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] An embodiment of the present invention provides a pressure sensitive adhesive sheet having predetermined dielectric and modulus properties.

[0030] Furthermore, an embodiment of the present invention provides an antenna structure and an image display device to which the pressure-sensitive adhesive sheet is applied.

[0031] Hereinafter, an embodiment of the present invention will be described in detail.

[0032] <Adhesive sheet> FIG. 1 is a schematic cross-sectional view showing a pressure-sensitive adhesive sheet according to an exemplary embodiment.

[0033] 1, the adhesive sheet 100 may include an adhesive layer 110. The adhesive sheet 100 may further include a protective film formed on at least one surface of the adhesive layer 110.

[0034] According to an exemplary embodiment, the dielectric loss tangent (dielectric loss or loss tangent; Df) value of the adhesive layer 110 measured at a thickness of 150 μm and 28 GHz may be 0.01 or less. For example, the dielectric loss tangent of the adhesive layer 110 may be greater than 0 and less than or equal to 0.01.

[0035] By suppressing the dielectric loss of the adhesive layer 110 within the above range, the dielectric properties of the antenna dielectric layer due to the adhesive layer 110 are not changed or impaired.

[0036] Preferably, the dielectric loss tangent of the pressure-sensitive adhesive layer 110 is greater than 0 and is 0.005 or less, more preferably 0.003 or less, and even more preferably 0.002 or less.

[0037] The elastic modulus of the adhesive layer 110 can be designed in consideration of the folding stability of the antenna structure or image display device including the adhesive layer 110 .

[0038] According to an exemplary embodiment, the storage modulus of the adhesive layer 110 at 25° C. may be 10 to 50 kPa. Within this range, the adhesive layer 110 can maintain mechanical stability while imparting sufficient folding properties.

[0039] In one embodiment, the storage modulus of the pressure-sensitive adhesive layer 110 at 25° C. may be 20 to 40 kPa, preferably 20 to 30 kPa.

[0040] According to an exemplary embodiment, the pressure-sensitive adhesive layer 110 may have a first modulus ratio defined by the following formula 1 of 1.5 to 4.0.

[0041] [Formula 1] First modulus ratio = A / B

[0042] In formula 1, A is the storage modulus of the pressure-sensitive adhesive layer 110 at -20°C, and B is the storage modulus of the pressure-sensitive adhesive layer 110 at 25°C.

[0043] According to an exemplary embodiment, the pressure-sensitive adhesive layer 110 may have a second modulus ratio defined by the following formula 2 of 1.0 to 3.5.

[0044] [Formula 2] Second modulus ratio = B / C

[0045] In formula 2, B is the storage modulus of the pressure-sensitive adhesive layer 110 at 25°C, and C is the storage modulus of the pressure-sensitive adhesive layer 110 at 80°C.

[0046] By forming the adhesive layer 110 so as to satisfy both the ranges of the first and second modulus ratios, it is possible to maintain sufficient flexibility and folding characteristics over a wide temperature range and suppress mechanical defects such as cracks and peeling during folding / bending. This makes it possible to prevent defects such as cracks from occurring even under severe bending conditions while maintaining sufficient mechanical strength and impact resistance of the adhesive layer 110.

[0047] For example, the adhesive layer 110 can be bent at -30° C. with a radius of curvature of 2 mm at a speed of 25 times per minute more than 10,000 times without cracking or peeling.

[0048] In one embodiment, the first modulus ratio of the pressure-sensitive adhesive layer 110 may be 2 to 3.5, preferably 2.4 to 3.3. In one embodiment, the second modulus ratio of the pressure-sensitive adhesive layer 110 may be 1.5 to 3.0, preferably 1.8 to 2.5.

[0049] The pressure-sensitive adhesive layer 110 may include an acrylic copolymer. For example, the pressure-sensitive adhesive layer 110 may be formed using a pressure-sensitive adhesive composition including the acrylic copolymer.

[0050] The acrylic copolymer may be prepared from a monomer blend in which a plurality of monomers are mixed, or from a monomer syrup.

[0051] The monomer blend can include a first acrylate monomer having less than 18 carbon atoms and a second acrylate monomer having 18 or more carbon atoms.

[0052] Non-limiting examples of the first acrylate monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isobornyl acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-pentafluorooctyl acrylate, 2-ethylhexyl diglycol acrylate, etc. These may be used alone or in combination of two or more.

[0053] Non-limiting examples of the second acrylate monomer include 2-decyl-1-tetradecanyl(meth)acrylate, stearyl(meth)acrylate, etc. These may be used alone or in combination of two or more.

[0054] The term "(meth)acryl-" as used in the present invention is intended to encompass both "acryl-" and "methacryl-".

[0055] According to an exemplary embodiment, the second acrylate monomer having a relatively large carbon number and a long molecular length is used to reduce the polarization characteristics of the adhesive layer 110. As a result, the dielectric constant of the adhesive layer 110 can be lowered and the dielectric loss tangent can be effectively reduced.

[0056] In addition, by using the first acrylate monomer together with the second acrylate monomer, the polarity in the monomer blend is increased, and the cohesive strength can be improved, thereby complementing or enhancing the folding property of the adhesive layer 110.

[0057] The contents of the first acrylate monomer and the second acrylate monomer may be adjusted in consideration of both the dielectric properties and the folding properties.

[0058] In some embodiments, the ratio of the weight of the second acrylate monomer to the weight of the first acrylate monomer may be about 0.2-9.

[0059] Preferably, from the viewpoint of realizing sufficient mechanical stability when the adhesive layer 110 is folded, the ratio of the weight of the second acrylate monomer to the weight of the first acrylate monomer may be 0.2 to 1, and preferably 0.3 or more and less than 1.

[0060] In some embodiments, the monomer blend may further include a polar monomer containing a carboxyl group or an amide group. The addition of the polar monomer may further increase the cohesive strength of the copolymer, thereby further improving the mechanical stability of the adhesive layer 110 when folded.

[0061] Examples of polar monomers containing a carboxyl group include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, crotonic acid, isocrotonic acid, maleic acid, itaconic acid, and fumaric acid.

[0062] Examples of polar monomers containing an amide group include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, and N-hydroxyethyl(meth)acrylamide.

[0063] In some embodiments, the monomer blend may contain 10 to 75 parts by weight of the first acrylate monomer, 20 to 85 parts by weight of the second acrylate monomer, and 0.5 to 10 parts by weight of the polar monomer, relative to 100 parts by weight of the monomer blend.

[0064] In some embodiments, an increase in the amount of hydroxyl groups in the monomer may increase the dielectric constant or dielectric loss due to an increase in polarization. Therefore, the amount of hydroxyl group-containing monomers can be restricted to 2 parts by weight or less, preferably 1 part by weight or less, per 100 parts by weight of the monomer blend.

[0065] In one embodiment, the monomer blend may be free of hydroxyl-containing monomers.

[0066] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl acrylate.

[0067] The pressure-sensitive adhesive composition may further include a photopolymerization initiator or a thermal curing agent to improve crosslinking or curing properties.

[0068] Examples of the photopolymerization initiator include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, 1-hydroxycyclohexyl-1-phenylmethanone, hydroxydimethylacetophenone, dimethylaminoacetophenone, dimethoxy-2-phenylacetophenone, 3-methylacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 4-chloroacetophenone, 4,4-dimethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 4-hydroxycyclophenyl ketone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, oligo[2-hydroxy-2-methyl-1-(4-(1-methylbiphenyl)methanone], 1-hydroxycyclohexyl phenyl ketone ... (2-hydroxyethyl)phenyl)propanone], 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4-diaminobenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, anthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, diphenyl ketone benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (TPO), fluorene, triphenylamine, carbazole, azobisisobutyronitrile (AIBN), and the like. These may be used alone or in combination of two or more kinds.

[0069] In some embodiments, the photopolymerization initiator may be included in an amount of 0.01 to 3 parts by weight, preferably 0.2 to 2 parts by weight, based on 100 parts by weight of the acrylic copolymer.

[0070] The heat curing agent can, for example, appropriately crosslink the acrylic copolymer to strengthen the cohesive strength of the pressure-sensitive adhesive composition, and can include, for example, an isocyanate-based crosslinking agent.

[0071] Examples of the isocyanate crosslinking agent include tolylene diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, 2,4-diphenylmethane diisocyanate, 4,4-diphenylmethane diisocyanate, isophorone diisocyanate, tetramethylxylene diisocyanate, naphthalene diisocyanate, and isocyanurate trimer.

[0072] The heat curing agent may be contained in an amount of 0.1 to 1 part by weight, preferably 0.1 to 0.5 parts by weight, based on 100 parts by weight of the acrylic copolymer.

[0073] In some embodiments, the pressure-sensitive adhesive composition may further contain additives such as antioxidants, corrosion inhibitors, leveling agents, surface lubricants, defoamers, fillers, plasticizers, light stabilizers, reaction initiators, and solvents, within the range that does not impair the dielectric properties and folding properties of the acrylic copolymer.

[0074] Returning to FIG. 1, the adhesive sheet 100 may further include a protective film formed on the surface of the adhesive layer 110 .

[0075] For example, the adhesive sheet 100 may include a first protective film 120 and a second protective film 130 formed on the bottom and top surfaces of the adhesive layer 110, respectively.

[0076] The first protective film 120 may be provided as a base film for forming the adhesive layer 110. The second protective film 130 may be provided as a release film for attaching the adhesive layer 110 to a target body.

[0077] In some embodiments, the first protective film 120 may also be provided as a release film. In this case, the adhesive sheet 100 may be provided as a double-sided adhesive sheet.

[0078] The first protective film 120 and the second protective film 130 may include, for example, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, and polybutylene naphthalate; polyimide resins; acrylic resins; styrene-based resins such as polystyrene and acrylonitrile-styrene; polycarbonate resins; polylactic acid resins; polyurethane resins; polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers; vinyl-based resins such as polyvinyl chloride and polyvinylidene chloride; polyamide resins; sulfone-based resins; polyether-ether ketone-based resins; arylate-based resins, etc.

[0079] <Antenna structure and image display device> An embodiment of the present invention provides an antenna structure and an image display device, each including the above-mentioned pressure-sensitive adhesive sheet.

[0080] 2 and 3 are schematic cross-sectional and plan views, respectively, of an antenna structure and an image display device according to an exemplary embodiment.

[0081] 2 and 3, the antenna structure 300 may include an antenna electrode layer 160, an antenna dielectric layer 150, and the adhesive sheet 100 according to the above exemplary embodiment.

[0082] The antenna electrode layer 160 can be formed on the antenna dielectric layer 150. As shown in FIG. 3 , the antenna electrode layer 160 can include an antenna unit (AU), and multiple antenna units (AU) can be arranged on the antenna dielectric layer 150.

[0083] The antenna unit (AU) can include a radiator 162, a transmission line 164, and a signal pad 166. The signal pad 166 can be connected to an antenna driving IC chip via, for example, a flexible printed circuit board (not shown). This allows power supply and signal transmission to the radiator 162 via the transmission line 164.

[0084] A pair of ground pads 168 may be arranged around the signal pad 166 with the signal pad 166 in between.

[0085] According to an exemplary embodiment, radiator 162 may provide radio frequency or ultra-high frequency communications, for example, corresponding to bands of 5 GHz or higher, 10 GHz or higher, or 20 GHz or higher.

[0086] The antenna dielectric layer 150 may include an insulating material having dielectric properties to achieve the high frequency and ultra high frequency radiation characteristics.

[0087] For example, the adhesive sheet 100 can be attached to the bottom surface of the antenna dielectric layer 150 after removing the first protective film 130. This allows the adhesive layer 110 to be in direct contact with the bottom surface of the antenna dielectric layer 150.

[0088] The image display device 400 may include a display panel 200 and an antenna structure 300 .

[0089] The display panel 200 may include a pixel electrode 210 , a pixel defining film 220 , a display layer 230 , a counter electrode 240 , and an encapsulation layer 250 disposed on a panel substrate 205 .

[0090] A pixel circuit including a thin film transistor (TFT) is formed on the panel substrate 205, and an insulating film covering the pixel circuit can be formed on the panel substrate 205. The pixel electrode 210 can be electrically connected to, for example, a drain electrode of the TFT on the insulating film.

[0091] A pixel defining layer 220 may be formed on the insulating layer to define a pixel region by exposing the pixel electrode 210. A display layer 230 may be formed on the pixel electrode 210, and the display layer 230 may include, for example, a liquid crystal layer or an organic light emitting layer.

[0092] A counter electrode 240 may be disposed on the pixel defining film 220 and the display layer 230. The counter electrode 240 may serve as, for example, a common electrode or a cathode of the image display device. An encapsulation layer 250 may be laminated on the counter electrode 240 to protect the display panel 200.

[0093] The antenna structure 300 can be attached onto the display panel 200 via the adhesive sheet 100. For example, after removing the first protective film 120, the antenna structure 300 can be attached onto the display panel 200 via the adhesive layer 110.

[0094] In some embodiments, the touch sensor layer 260 can be laminated on the display panel 200. For example, the touch sensor layer 260 can be attached onto the encapsulation layer 250 of the display panel 200 via the first adhesive layer 50.

[0095] In some embodiments, a polarizing layer 270 can be laminated on the touch sensor layer 260. For example, the polarizing layer 270 can be laminated on the touch sensor layer 260 via the second adhesive layer 60.

[0096] In some embodiments, the antenna structure 300 can be laminated onto the polarizing layer 270. For example, the first protective film 120 can be removed and the adhesive layer 110 can be attached onto the polarizing layer 270.

[0097] A cover window 280 can be laminated on the antenna structure 300. For example, the cover window 280 can be attached onto the antenna structure 300 via a third adhesive layer 70.

[0098] As described above, the antenna structure 300, the polarizing layer 270, and the touch sensor layer 260 can be arranged in this order from the user's viewing side. Alternatively, the antenna structure 300 may be arranged under the touch sensor layer 260, or between the polarizing layer 270 and the touch sensor layer 260.

[0099] 3, the image display device 400 can include a display area 410 and a peripheral area 420. The peripheral area 420 can correspond to a bezel area or a light-shielding area (non-display area).

[0100] The antenna structure 300 can be attached to the inside of the image display device 400 in the form of, for example, a patch using the adhesive sheet 100 so that the radiator 162 overlaps the display area 410 .

[0101] As described above, the adhesive sheet 100 can have reduced dielectric loss and improved folding characteristics, thereby promoting high-frequency and ultra-high-frequency radiation characteristics of the radiator 162 or antenna unit (AU) and suppressing signal loss. Also, the adhesive sheet 100 can be easily inserted in the form of a patch through the peripheral area 420 of the image display device 400 by folding and bending. EXAMPLES

[0102] Below, preferred embodiments are presented to aid in understanding the present invention. However, these embodiments are merely illustrative of the present invention and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the embodiments are possible within the scope of the scope and technical spirit of the present invention, and it is natural that such changes and modifications fall within the scope of the appended claims.

[0103] Production example: Production of acrylic copolymer Manufacturing Example 1 A monomer blend containing 50 parts by weight of 2-ethylhexyl acrylate (2-EHA), 45 parts by weight of 2-decyl-1-tetradecanyl acrylate (DTDA), and 5 parts by weight of acrylic acid (AA) was added to a 1L reactor, followed by 100 parts by weight of ethyl acetate (EAc) as a solvent. Nitrogen gas was purged for 1 hour to remove oxygen, and the temperature was maintained at 80°C. After the monomer blend was uniformly mixed, 0.1 parts by weight of azobisisobutyronitrile (AIBN) was added as a reaction initiator, and the mixture was reacted for 8 hours to produce an acrylic copolymer (weight average molecular weight: 950,000, PDI 4.1).

[0104] Manufacturing Examples 2 to 13 Acrylic copolymers were produced in the same manner as in Production Example 1, except that the monomer components and contents (parts by weight) were changed as shown in Table 1 below.

[0105] [Table 1]

[0106] The specific components shown in Table 1 are as follows: EHA: 2-Ethylhexyl acrylate (Sigma-Aldrich) EHDG-AT: 2-Ethylhexyl diglycol acrylate (Kyoeisha) DTDA: 2-decyl-1-tetradecanyl acrylate (Kyoeisha) DTDMA: 2-decyl-1-tetradecanyl methacrylate (Kyoeisha) SA: Stearyl acrylate (Kyoeisha) AA: Acrylic acid (Sigma-Aldrich) DMAA: N,N-Dimethylacrylamide (Sigma-Aldrich) 2-HEA: 2-hydroxyethyl acrylate (Sigma-Aldrich) 4-HBA: 4-hydroxybutyl acrylate (Sigma-Aldrich)

[0107] Experimental Example Using the acrylic copolymers synthesized in the above Preparation Examples, pressure-sensitive adhesive compositions according to Examples and Comparative Examples were prepared as shown in Tables 2 and 3. The pressure-sensitive adhesive compositions were applied to a thickness of 100 μm on a 50 μm release film coated with a silicone release agent, dried at 110° C. for 5 minutes, and then a release film was laminated to form pressure-sensitive adhesive sheets.

[0108] 1) Measurement of storage modulus The storage modulus at 25°C was measured for each adhesive sheet of the examples and comparative examples using a viscoelasticity measuring device (MCR-301, Anton Paar). Specifically, the size of the adhesive sheet was cut to 30 mm length x 30 mm width, and the release film attached to one side of the cut adhesive sheet was removed, and then the sheet was bonded to a glass substrate. Thereafter, the storage modulus was measured in a temperature range of -20 to 100°C under the conditions of a frequency of 1.0 Hz, a deformation of 2%, and a heating rate of 5°C / min while attached to a measuring tip. At this time, the measured values ​​at -20°C, 25°C, and 80°C were read, and the modulus ratio was calculated according to the above-mentioned formulas 1 and 2.

[0109] 2) Measurement of dielectric tangent The dielectric loss tangent of each of the pressure-sensitive adhesive sheets in the Examples and Comparative Examples was measured at 25° C. using a dielectric constant measuring device (Anritus, model number MS46522B). Specifically, a 150 μm pressure-sensitive adhesive sheet from which the release film had been removed was laminated between 40 μm COP films (Zeonor), and cut to a size of 30 mm length × 70 mm width.

[0110] The cut adhesive sheet was placed in the probe of a measuring device, and the dielectric loss tangent (Df) value at 28 GHz was measured.

[0111] <Evaluation criteria> ◎: 0.005 or less ○: Over 0.005 and 0.01 or less ×: Over 0.01

[0112] 3) Evaluation of folding properties The adhesive sheets produced in the examples and comparative examples were bonded to 50 μm PET to produce samples of 20 mm × 100 mm. The samples were fixed to a bending property evaluation device (COVOTECH, CFT-720C), folded 25 times per minute, held for 0.2 seconds after each folding, and evaluated for folding at -30°C under the conditions of a curvature radius of 2 mm. The number of foldings at which defects such as breakage, lifting, and peeling occurred at the folding site was measured, and the folding properties were evaluated as follows.

[0113] <Evaluation criteria> ◎: No defects occurred when folded 30,000 times or more. ○: Defects occurred within the range of 10,000 to 30,000 folding times. ×: Defects occurred after less than 10,000 folding cycles.

[0114] The evaluation results are shown in the following Tables 2 and 3. In Tables 2 and 3, TDI-based Coronate-L (Nippon Urethane Co., Ltd.) was used as the crosslinking agent.

[0115] [Table 2]

[0116] [Table 3]

[0117] Referring to Tables 2 and 3, the pressure-sensitive adhesive sheets according to the examples had low dielectric tangents and satisfied the above-mentioned ranges of storage modulus and modulus ratio, thereby providing excellent durability even when folded at harsh low temperatures.

Claims

1. The dielectric loss tangent at 28 GHz measured at a thickness of 150 μm is greater than 0 and is 0.01 or less; The storage modulus at 25° C. is 10 to 50 kPa, A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer having a first modulus ratio defined by the following formula 1 of 1.5 to 4.0 and a second modulus ratio defined by the following formula 2 of 1.0 to 3.

5. [Formula 1] First modulus ratio = A / B [Formula 2] Second modulus ratio=B / C (In Formula 1 and Formula 2, A is the storage modulus of the pressure-sensitive adhesive layer at −20° C., B is the storage modulus of the pressure-sensitive adhesive layer at 25° C., and C is the storage modulus of the pressure-sensitive adhesive layer at 80° C.)

2. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer comprises an acrylic copolymer polymerized from a monomer blend including a first acrylate monomer having less than 18 carbon atoms and a second acrylate monomer having 18 or more carbon atoms.

3. The pressure-sensitive adhesive sheet according to claim 2, wherein in the monomer blend, a ratio of a weight of the second acrylate monomer to a weight of the first acrylate monomer is 0.2 to 9.

4. The pressure-sensitive adhesive sheet according to claim 2 , wherein the monomer blend further comprises a polar monomer containing a carboxyl group or an amide group.

5. 5. The pressure-sensitive adhesive sheet according to claim 4, wherein the monomer blend comprises, per 100 parts by weight of the monomer blend, 10 to 75 parts by weight of the first acrylate monomer, 20 to 85 parts by weight of the second acrylate monomer, and 0.5 to 10 parts by weight of the polar monomer.

6. 6. The pressure-sensitive adhesive sheet according to claim 5, wherein the amount of the hydroxyl group-containing monomer is 2 parts by weight or less per 100 parts by weight of the monomer blend.

7. The pressure-sensitive adhesive sheet according to claim 2, wherein the second acrylate monomer comprises 2-decyl-1-tetradecanyl(meth)acrylate or stearyl(meth)acrylate.

8. The pressure-sensitive adhesive sheet according to claim 1 , wherein the dielectric tangent of the pressure-sensitive adhesive layer is 0.005 or less.

9. The pressure-sensitive adhesive sheet according to claim 1, wherein the storage modulus of the pressure-sensitive adhesive layer at 25° C. is 20 to 40 kPa.

10. The pressure-sensitive adhesive sheet according to claim 1 , further comprising a protective film formed on at least one surface of the pressure-sensitive adhesive layer.

11. an antenna dielectric layer; an antenna electrode layer disposed on an upper surface of the antenna dielectric layer; and the adhesive sheet of claim 1 attached onto a bottom surface of the antenna dielectric layer.

12. A display panel; An image display device comprising: the antenna structure according to claim 11 attached onto the display panel.

Citation Information

Patent Citations

  • Transparent conductive film with adhesive layer

    JP2020142525A

  • Game machine

    JP2021166838A

  • Millimeter-wave antenna

    JP2022056353A

  • Adhesive sheet for oily surfaces

    JP7048467B2

  • Pressure-sensitive adhesive composition

    JP7785495B2