Compositions containing resin from the canarium ovatum tree and methods for making same for sealants and flame retardants
A sealant composition using Canarium ovatum resin addresses the health and environmental issues of polysulfide-based sealants by providing enhanced mechanical and thermal properties, meeting aviation flammability standards while reducing hazards.
Patent Information
- Application Number
- JP2024545884
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-06
- Filing Date
- 2021-12-10
- Publication Date
- 2024-10-10
AI Technical Summary
Polysulfide-based sealants used in aerospace applications pose health and environmental hazards due to water absorption, antifreeze interaction, and flammability, while lacking effective alternatives with similar mechanical and thermal properties.
A sealant composition utilizing resin from the Canarium ovatum tree, combined with a solvent and an activator, such as manganese dioxide, to provide mechanical, thermal, and rheological properties suitable for aerospace applications, minimizing health and environmental risks.
The sealant composition demonstrates superior mechanical, thermal, and rheological properties, meets aviation flammability standards, and reduces health and environmental hazards compared to traditional polysulfide-based sealants.
Smart Images

Figure 2024537548000001 
Figure 2024537548000002 
Figure 2024537548000003
Abstract
Description
Detailed Description of the Invention
[0001] [Technical field] The present invention relates to sealant and flame retardant compositions, methods for their preparation and their application, particularly to aircraft fuel tanks.
[0002] [Background technology] There is a growing demand for aerospace adhesives and sealants for the commercial, military, and general aviation sectors, with the commercial sector being the largest group of these.
[0003] One of the most common sealing materials used in commercial end-user industries is polysulfide-based sealants. It was the first aerospace sealant and has been used in the aircraft industry for over 50 years. It is resistant to aviation fuels and therefore aids in sealing fuel tanks. Some of the advantages of polysulfide-based sealants are excellent adhesion to aluminum, titanium, other metals and composites, low permeability to fuel vapors, water vapor, and air, good low temperature flexibility, good heat resistance, good elasticity, moderate strength (in the presence of fuel), good elasticity, good adhesion of new sealant to old sealant (i.e. in repairs), and ease of application.
[0004] Naftoseal® MC-238 from Chemetall Company is an example of a polysulfide-based sealant. With a 75% concentration of polysulfide polymer as the base component, this type of sealant has the highest amount of polysulfide polymer of any sealant in its class.
[0005] Below, the complete composition including base material and hardener materials of Naftoseal® MC-238 is listed in tabular form along with its concentration percentage / percentage composition.
[0006] [Table 1]
[0007] Among the drawbacks of polysulfide-based sealants is the absorption of water and antifreeze, which leads to swelling, reduced effectiveness and properties, especially tearability and adhesion. In addition, these polysulfide-based sealants are listed in Section 3 (Composition / Ingredients Information) of the Material Safety Data Sheet (MSDS) as causing severe eye, respiratory and skin irritation, long-term harmful effects to aquatic animals, and as a source of flammable liquids and vapors. They also cause damage to organs and even genetic defects or cancer with prolonged or repeated exposure by inhalation or ingestion. The health hazards associated with polysulfide-based sealants pose problems for aircraft manufacturers, operators, and maintenance personnel.
[0008] There is an increasing need for sealants that are at least as effective as polysulfide-based sealants, but which pose minimal health and environmental hazards.
[0009] Prior art reference U.S. Patent No. 10,428,261 B2 ('261), entitled "Resin Composite with Overloaded Solids for Well Sealing Applications," teaches a seal material including one or more solid particles mixed into a fluid material to form a seal material, the one or more solid particles being about 22% to about 30% volume fraction of the seal material when mixed into the fluid material, and where hermetically sealed, the seal material includes a first portion having a first concentration of the one or more solid particles and a second portion having a second concentration of the one or more solid particles, the second concentration being less than the first concentration, the one or more solid particles further including at least one of magnesium oxide, sand, silicon carbide, and graphite. However, '261 does not teach a sealant having a composition consisting of a resin from the Canarium ovatum tree, and a method for making the same.
[0010] Objective of the invention It is an object of the present invention to provide a composition for a sealant for use in the aircraft industry, in particular a sealant for a fuel tank, which composition has the properties required for its function while at the same time minimizing health and environmental hazards. It is a further object of the present invention to provide a method for making said sealant.
[0011] Summary of the Invention The present invention aims to overcome the shortcomings of polysulfide-based sealants while providing the properties required for aerospace sealants. The present invention therefore provides a composition for a substrate for a sealant in which a resin from Canarium ovatum, also known as the piri tree, is used instead of synthetic polysulfide polymers. The present invention therefore comprises a combination of said resin with a solvent and an activator to provide the required mechanical, thermal and rheological properties of an aerospace sealant for use in fuel tanks while minimizing chemical components that pose health and environmental hazards. The present invention also provides a method for making said combination.
[0012] [Mode for carrying out the invention] The composition for the sealant of the present invention is prepared by first preparing a binder composition or mixture. This is done by mixing the resin harvested from the Canarium ovatum tree with a suitable solvent. One example of such a solvent is toluene.
[0013] The resin can be in either its green or used form, also known as never-dried or dried resin, respectively. Drying of the green resin is accomplished by a steam distillation process that separates the essential oils from the dried resin. Both the dried and never-dried resins are suitable for formulating fire-retardant sealants, as will be discussed further.
[0014] The ratio of resin to solvent can vary. Mixing is complete when the binder composition appears uniform. To prepare the sealant itself, the binder composition is then mixed with a suitable hardener, also known as an activator or activating agent. Manganese dioxide is used as an activator to prepare and test the sealant of the present invention. However, in practice, any suitable solvent for the resin and any suitable hardener or activator can be used. The examples herein should not be construed as limiting the selection in solvent and activator.
[0015] Detailed methods for making sealants using raw canarium ovatum resin are described in the following sections.
[0016] Extraction of raw Canarium ovatum sap is done by removing loose bark, dirt, and other foreign matter and lightly scraping the area to be tapped. The initial tapping is done no more than 60 cm above ground level as Canarium species are known for their high buttresses.
[0017] Carefully, to avoid damaging the cambium, use the knife to make a horizontal cut about 2 cm wide and 15 cm long. A space twice the width of the tapping should be maintained. Subsequent chippings, about 3 mm to 5 mm wide, should proceed vertically in a straight line. The first tapping cut should be 15 cm wide along the perimeter and 1 to 2 cm wide along the height of the tree.
[0018] A wooden mallet can be used to tap the knife to control the depth of the cut. Other cuts can be made at the same dimensions as the first cut at 15 cm, but the distance between the tapped portions should be approximately 30 cm or twice the length of the cut.
[0019] A plastic receptacle should be temporarily installed under the cut as the resin exuded from the tree will slowly harden. The tapped trunk should be covered with polyethylene sheeting and sealed with plastic roofing cement. This will prevent moisture, insects, and other debris such as dried leaves, bark, dust, etc. from entering the cut.
[0020] After extraction of raw resin from Canarium ovatum tree from Canarium ovatum bark, toluene is mixed and the resulting mixture is the base material for the experimental sealant. Manganese dioxide is then prepared in a separate container to act as a hardener.
[0021] The compounding process involves thoroughly mixing the base material with the hardener material, which is then cured prior to its application and testing.
[0022] The detailed method for making a sealant using dried canarium ovatum resin is as follows.
[0023] After the resin is extracted from the bark of Canarium ovatum, it may undergo a steam distillation process, which involves the separation of the essential oil from the spent or deoiled resin, since Canarium ovatum sap is olearin.
[0024] The used / deoiled resin, no longer dry resin, is ground and is the basic component of the flame retardant sealant formulation. In the dry process, the powdered resin can be easily dissolved by solvents.
[0025] Toluene is then mixed with the dry resin and serves as the base material for the flame retardant sealant. Manganese dioxide is then prepared in a separate container and serves as the curing agent.
[0026] The sealant formulation process involves thoroughly mixing the base material with the curing agent, then allowing it to cure before application and testing.
[0027] In verifying the effectiveness and applicability of the formulated sealant, five properties are used to analyze and determine the material properties by performing different standard tests: physical, chemical, mechanical, thermal, and rheological properties. For physical properties, sensory tests (color, odor, and appearance tests), instrumental colorimetry tests, and flash point tests are used. Chemical properties such as tack-free time test, cure time test, toxicity test, and Shore A hardness test are also performed. Additionally, for the mechanical properties of the sealant, shear strength test, tensile strength, tear strength test, peel strength test, knife test, and pull-off test are also of particular importance.
[0028] While Thermogravimetry-Differential Thermal Analysis, Differential Scanning Calorimetry, and Calorific Value refer to the thermal properties of the formulated sealant. The rheological properties of the sealant are quantified by viscosity tests.
[0029] Various results from the material characterization are discussed in the following sections.
[0030] Example 1: Sealant Bonding Formulation Consistency 22 binder compositions were preliminarily tested to quantify the homogeneity of the resulting mixtures for both dried and undried precursors. Various weights of pili sap are mixed with toluene. This initial test is used to quantify whether canarium ovatum sap has acceptable homogeneity characteristics when mixed with an organic solvent such as toluene.
[0031] [Table 2]
[0032] It can be observed that all binder compositions for both dried and undried Canarium ovatum sap exhibited acceptable homogeneity and could be subsequently mixed with an activator to form a sealant.
[0033] Example 2: Flammability testing of sample formulations of [Flame Retardant Composition / Sealant] The 12 different sealant formulations that showed satisfactory suitable mixture consistency of base material and hardener materials were subjected to flammability testing, which is an important test and consideration as per aviation laws and regulations, especially 14 Code of Federal Regulation Appendix N to Part 25 - Fuel Tank Flammability Exposure and Reliability Analysis, to obtain the best formulation of the experimental sealant. Commercially available sealants are also tested under the same parameters and conditions as the 12 sealant formulations.
[0034] Based on the results, four sealant formulations, especially 18g, 18.50g, and 74g of undried canarium ovatum resin and 17.50g of dried canarium ovatum resin, passed the standard test showing the resistance of these experimental sealant formulations to flame. Furthermore, no ignition or flame occurred in the above four sealant formulations during the entire period of the test. Meanwhile, the remaining eight sealant formulations could not withstand the flammable conditions and caused the occurrence of flame and ignition. However, after this ignition, the eight sealant formulations could obtain a self-extinguishing state where the flame stopped burning.
[0035] [Table 3] JPEG2024537548000004.jpg51169
[0036] Of the various compositions of sealants containing resin from Canarium ovatum trees tested, four are found to exhibit properties that meet the flammability test of aviation regulations, specifically 14 Code of Federal Regulation Appendix N to Part 25 - Fuel Tank Flammability Exposure and Reliability Analysis. These four compositions, hereafter referred to as Experimental Sealant Samples 1-4, respectively, are summarized in Table 4. In this table, "wt" stands for "weight." Their other important properties are presented in Tables 3-10 and are discussed further thereafter.
[0037] [Table 4]
[0038] Example 3: Physical Description of Sample Formulations of [Flame Retardant Compositions / Sealants] The physical description of the sample formulations of the flame retardant composition / sealant and commercial sealants can be found in Table 5.
[0039] The essential advantage in the physical properties of the sample formulations over the commercial sealant is the odor: the formulated sealant was found to be more pleasant than the commercial sealant, which can be explained by the fact that the piri sap is of the oleaginous type, which contains essential oils that are used as perfume ingredients.
[0040] The results also show that the commercial sealant is brownish black in color, while the sealant sample is black in color.
[0041] According to L*a*b* color measurements, both the experimental and commercial sealants showed lower luminosity (L*) at the green value of the (a*) color chromaticity layer.
[0042] (b*) With regard to the color chromaticity layer, sample 3 and the commercial sealant exhibit yellow color values, while the remaining three resulting sealant formulations exhibit blue color values.
[0043] [Table 5]
[0044] Example 4: Physicochemical properties of sample formulations of [Flame Retardant Composition / Sealant] Table 6 shows three physicochemical chemical properties of the formulated sealant and Naftoseal® MC-238 samples. Tack-free time is the time when the sealant is judged to be properly adhered to the surface without interruption or damage. Cure time is the time when the chemical reaction that cures the sealant is complete and its mechanical strength is at its maximum. Short tack and cure times are desired. The durometer hardness of the sealant refers to its hardness and ability to resist indentation. A lower number indicates less resistance and a softer material. In Table 6, the values of chemical properties that are superior to the corresponding properties of Naftoseal® are shaded. As can be seen in this table, the durometer hardness of all compositions of the formulated sealant exceeds that of the commonly sold sealant Naftoseal® MC-238. However, in terms of tack-free time and cure time, samples 2 and 4 are superior to the commercially available sealant. Therefore, samples 2 and 4 are easily considered superior to Naftoseal® in tack-free time, cure time, and durometer hardness.
[0045] On the other hand, the flash point test is performed to show the quantitative aspects of the physical properties of both the experimental and commercial sealant formulations, since it is one of the important tests of this material property. The obtained results show that samples 1 and 2 have the highest flash points among the five sealants, and according to the MSDS, materials with high flash points are less flammable and hazardous. Moreover, these two experimental sealant samples exceeded the data results of the commercial sealant in the flash point test.
[0046] [Table 6]
[0047] Example 5: Mechanical properties of sample formulations of [Flame Retardant Composition / Sealant] Table 7 compares four mechanical properties of the sealant and Naftoseal® MC-238 samples. Tensile strength is the breaking strength of a specimen under the action of a force capable of breaking many threads simultaneously at a constant rate of 95 elongation / load. Tear strength is the maximum force required to tear a specimen in a direction perpendicular to the direction of stress. Shear strength is a measure of the maximum shear stress that a material can sustain before rupturing. Finally, peel strength is used to measure the bond strength of a material.
[0048] Table 7 shows the peel strength values for test panel lengths produced varying from 12.77 mm to 127 mm.
[0049] In Table 7, the shading highlights the properties of the experimental sealants that exceed the corresponding properties of Naftoseal® MC-238. The tensile strength of all the samples of the compounded sealants is higher compared to the same properties of the commercial sealants. Except for sample 1, all other samples of the experimental sealants show higher tear strength than the commercial sealants. This difference is more pronounced in the case of samples 2 and 4. In addition, all but sample 3 of the compounded sealants show higher shear strength. Finally, in terms of peel strength, samples 1 and 2 appear to be superior to Naftoseal® MC-238.
[0050] [Table 7]
[0051] Example 6. Knife test and pull-off strength evaluation of sample formulations of [Flame Retardant Composition / Sealant] Table 8 shows the knife test ratings and pull-off strength of the sealants and Naftoseal® MC-238. The knife test is used to determine the adhesion of organic coatings when applied to a smooth, flat panel surface using a cutting knife.
[0052] Pull-off strength measures the resistance of a sealant to separation from a substrate when a normal tensile force is applied.
[0053] In the tests carried out to compare the mechanical strength in Table 8, the substrate used is aluminum.
[0054] In the knife test, samples 3 and 4 have higher ratings than Naftoseal® MC-238, as can be seen in Table 8. However, over time, only sample 4 shows consistently higher pull-off strength compared to Naftoseal® MC-238. After 21 days or more of curing, samples 1 and 2 show higher pull-off strength.
[0055] [Table 8]
[0056] Example 7: Thermal property measurements of sample formulations of [Flame Retardant Composition / Sealant] Table 9 compares the results of three key thermal property tests, namely, thermogravimetry-differential thermal analysis, differential scanning calorimetry, and calorific value measurements, for the experimental sealant and Naftoseal® MC-238. These tests show how temperature affects the stability of both the experimental and commercial sealants.
[0057] [Table 9] JPEG2024537548000011.jpg100169
[0058] Differential thermogravimetric analysis showed that all sealant samples exhibited better thermal stability by not showing any dramatic weight loss during the entire temperature programmed period from 30° C. to 950° C. Similarly, the peak temperatures of all sealant samples show high temperature resistance ranging from 359° C. to 366° C., with an endothermic reaction before reaching the maximum amount of weight loss.
[0059] On the other hand, the commercial sealant exhibits the highest weight loss percentage, especially at its first peak, which is about 69.542% at a peak temperature of 284° C. Furthermore, it can also be seen in Table 9 that the commercial sealant exhibited thermal instability, as indicated by its significant weight loss, which is evident at its first peak temperature.
[0060] With respect to differential scanning calorimetry testing, the three experimental sealant samples (samples 1, 2, and 3) exhibited a high resistance temperature range of 123°C to 126°C before melting, compared to the commercial sealant, which has a melting point of 119.46°C.
[0061] Additionally, the three samples, along with sample 4, obtained higher total heat values based on the heat release test compared to the commercial sealant, demonstrating high temperature and heat resistance before total combustion occurs.
[0062] Thus, all the data from the thermal property tests reveal that the formulated sealant according to the invention is superior in terms of thermal stability and resistance to Naftoseal® MC-238. With regard to these thermal properties, the composition can be used as a flame retardant.
[0063] Example 8: Rheological properties of sample formulations of [Flame Retardant Composition / Sealant]
[0064] [Table 10]
[0065] The rheological properties of the experimental and commercial sealants are detailed in the table above. As a result, two experimental sealant samples, namely, Sample 1 and 3, exceed the viscosity values of the commercial sealant. Due to this property, the two mentioned sealant samples exhibited non-dripping or non-sagging properties. They can be used in applications where the sealant needs to stay in its place during application and curing. Thus, the viscosity results of Samples 1 and 3 prove that the rheological properties of the experimental sealant sample types are more efficient and effective as compared to the commercial sealant.
[0066] Example 9: Toxicity parameters of sealant [flame retardant composition / sealant] formulations Table 11 compares the toxicity parameters of the experimental sealant samples and Naftoseal® MC-238. The meaning of the toxicity statements in this table is given in Table 12. The latter table first shows that there are three toxicity levels: harmful (H302, and in combination with other statements), toxic (H301, H311, H331, and in combination with other statements), and lethal (H300, H310, H330, and in combination with other statements). Examination of Table 11 reveals that Naftoseal® MC-238 can have fatal effects if swallowed, in contact with the skin, or inhaled as a vapor. On the other hand, four samples of the sealant formulation are classified only as "harmful" or "toxic". Moreover, the toxicity of the experimental sealant, expressed as "toxic concentration" and defined as the minimum concentration at which a particular substance produces a toxic effect, occurs at concentrations much higher than those of Naftoseal® MC-238. Thus, in summary, the toxicity of the samples is much lower than that of the commercially available sealants.
[0067] Among the sealant samples, sample 4 has the lowest rating in terms of toxicity, being listed only as "harmful" for oral and dermal toxicity, and only as "toxic" in its vapor form. In addition, its toxicity concentration is almost 25 times that of Naftoseal® MC-238. As far as table 11 goes, the best sample below is sample 1, whose toxicity concentration is 12 times that of Naftoseal® MC-238, or almost half that of sample 2. Finally, samples 2 and 3 differ slightly from each other, being only 5-6 times less toxic than Naftoseal® MC-238.
[0068] It will therefore be appreciated that the samples described above can be viewed as embodiments of the sealant composition. Sample 4 is one embodiment, while Sample 1 is preferred due to its superior peel strength and melting point. The most preferred embodiment with the most desirable properties is Sample 2. These embodiments compare favorably with Naftoseal® MC-238 in terms of physicochemical, mechanical, and thermal properties relevant to sealant function, with the added advantage of being less toxic than Naftoseal® MC-238.
[0069] [Table 11]
[0070] In addition, these embodiments point to an additional use of the composition, namely, flame retarding. In this application, sample 3 is an embodiment, while samples 1 and 2 are preferred, as they exceed the flash point and flammability results of commonly sold aviation sealants.
[0071] In pointing out these embodiments of the invention, it is not intended to limit the invention to these specific examples. Instead, the purpose is to illustrate the general spirit and scope of the invention. Although certain variations may occur in reproducing the compositions and methods described herein, the results should not be interpreted as departing from such spirit and scope.
[0072] [Table 12]
[0073] Preferred embodiments of the present invention are described in the above detailed description. It is understood that those skilled in the art may envision modifications and / or variations to the embodiments shown and described herein. Any such modifications or variations that are within the scope of this specification are intended to be included therein. Unless specifically stated otherwise, it is the intention of the inventors that the words and phrases in the specification and claims be given their ordinary and familiar meaning to those skilled in the applicable art. The foregoing description of the preferred embodiments and best mode of the invention known to the applicant at the time of filing has been presented and is intended for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed, and many modifications and variations are possible in light of the above teachings.
Claims
1. 1. A composition exhibiting flame retardant properties, comprising: A composition comprising Canarium ovatum sap and a solvent.
2. 2. The composition of claim 1, wherein the Canarium ovatum sap is 74 to 92.5% by weight.
3. The composition of claim 1, wherein the solvent is 6.8 to 26% by weight.
4. 2. The composition of claim 1, wherein the Canarium ovatum sap is either dried Canarium ovatum sap or undried Canarium ovatum sap.
5. The composition of claim 1 , wherein the solvent is an organic solvent.
6. A sealant comprising: A substrate, A sealant comprising a base material further comprising Canarium ovatum sap and a solvent, and an activator.
7. The sealant of claim 6, wherein the sealant comprises 88.0 to 90.9 wt. % of the substrate.
8. The sealant of claim 6, wherein the activator is 9.1 to 12.0 wt %.
9. The sealant of claim 6 wherein the activator is a metal oxide.
10. 7. The sealant of claim 6, wherein the weight ratio of the substrate to the solvent of the Canarium ovatum sap ranges from 5.29 to 12.
33.
11. 1. A method for making a Canarium ovatum sap sealant, comprising: a. Extracting Canarium ovatum sap from Canarium ovatum bark; b. adding a solvent to the extracted Canarium ovatum sap to create a substrate for the Canarium ovatum tree sealant; c. homogenizing the substrate; and d) adding an activator to the homogenized base material to produce the Canarium ovatum sap sealant.
Citation Information
Patent Citations
JP1973035462A
Fireproof sealant
JP2002363541A
Expandable fire-resistant sealing composition
JP2002540285A
Sealant resin composition
JP2016145370A
Flameproofed adhesive and sealing materials
US20080241529A1