Sintering aid for solid electrolyte for all-solid-state battery and solid electrolyte containing same

A sintering aid of Li2O, V2O5, and Ag2O lowers the sintering temperature of oxide electrolytes to 550°C or lower, improving ionic conductivity and addressing the high-cost and low-conductivity issues of existing oxide-based electrolytes.

JP2024537602AInactive Publication Date: 2024-10-16ベイス カンパニーリミテッド
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024510491
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-09-13
Filing Date
2022-10-24
Publication Date
2024-10-16
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing oxide-based electrolytes for all-solid-state batteries require high sintering temperatures, leading to increased manufacturing costs and lower ionic conductivity, while sulfide-based electrolytes face issues with moisture reactivity and hydrogen sulfide gas generation.

Method used

A sintering aid composed of Li2O, V2O5, and Ag2O is used to lower the sintering temperature of oxide electrolytes with a NASICON crystal structure to 550°C or lower, enhancing ionic conductivity to 0.3×10-5 to 1.4×10-4 S/cm.

Benefits of technology

The solution enables low-temperature sintering of oxide electrolytes with excellent ionic conductivity, reducing manufacturing costs and maintaining high performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537602000001_ABST
    Figure 2024537602000001_ABST
Patent Text Reader

Abstract

The present invention relates to a sintering aid for a solid electrolyte for an all-solid-state battery and a solid electrolyte containing the same. The solid electrolyte for an all-solid-state battery according to one embodiment of the present invention includes a solid electrolyte having a NASICON type crystal structure and a sintering aid, and the sintering aid is an oxide containing Li, Ag, and V.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sintering aid for a solid electrolyte for an all-solid-state battery and a solid electrolyte containing the same. [Background technology]

[0002] Recently, the use of secondary batteries has increased significantly in various fields, from IT devices such as mobile phones to electric vehicles and energy storage devices.

[0003] Lithium-ion batteries, which use liquid electrolytes, are the most widely used secondary batteries. However, liquid electrolytes pose a risk of tearing if the battery is subjected to external impact, and as a result, additional parts and devices are required to ensure safety.

[0004] Recently, in order to improve the safety of secondary batteries, active development of all-solid-state batteries that use solid electrolytes as electrolytes is underway. Solid electrolytes for all-solid-state batteries include polymer electrolytes, oxide electrolytes, and sulfide electrolytes. Of these, sulfide solid electrolytes have the highest ionic conductivity, but they react with moisture to generate hydrogen sulfide gas. Polymer electrolytes have the advantage of being relatively simple to process and can be used with existing lithium-ion battery processes, but have the disadvantage of significantly low ionic conductivity.

[0005] Oxide-based electrolytes have lower but still relatively high ionic conductivity than sulfide-based electrolytes, and have the advantage of being extremely safe. However, oxide-based electrolytes generally require a high sintering temperature of over 1,000°C, which can significantly increase manufacturing costs. Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made to solve the above-mentioned problems of the prior art, and an object of the present invention is to provide a sintering aid that can sinter an oxide-based electrolyte at a low temperature and has excellent ionic conductivity, and a solid electrolyte containing the same. [Means for solving the problem]

[0007] The solid electrolyte for an all-solid-state battery according to one embodiment of the present invention includes a solid electrolyte having a NASICON-type crystal structure and a sintering aid, the sintering aid being made of an oxide containing Li, Ag, and V.

[0008] According to one embodiment of the present invention, the sintering aid may be made of 45-61 mol% Li2O, 25-40 mol% V2O5, and 6-25 mol% Ag2O.

[0009] According to one embodiment of the present invention, the sintering aid comprises Li2O, V2O5 and Ag2O, and the molar ratio of Li2O, V2O5 and Ag2O may be 2:1:1.

[0010] The sintering temperature of the solid electrolyte for the all-solid-state battery according to an embodiment of the present invention may be 550° C. or lower.

[0011] The ionic conductivity of the solid electrolyte for the all-solid-state battery according to one embodiment of the present invention at room temperature is 0.3×10 -5 ~1.4×10 -4 S / cm.

[0012] According to an embodiment of the present invention, the solid electrolyte having a NASICON type crystal structure may be a LAGP solid electrolyte or a LATP solid electrolyte.

[0013] The sintering aid in the solid electrolyte for an all-solid-state battery according to one embodiment of the present invention is made of an oxide containing Li, Ag, and V.

[0014] In addition, the solid electrolyte for an all-solid-state battery and the sintering aid according to the present invention may further include other additional components within a range that does not impair the technical concept of the present invention. Effect of the Invention

[0015] According to an embodiment of the present invention, low-temperature sintering of a solid electrolyte is possible through the use of a sintering aid containing Li, Ag, and V. In addition, a solid electrolyte containing such a sintering aid may have excellent ionic conductivity. [Brief description of the drawings]

[0016] [Figure 1] 1 is a diagram illustrating a cross section of an all-solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings to the extent that those skilled in the art to which the present invention pertains can easily carry out the present invention.

[0018] In order to clearly explain the present invention, the description of parts not related to the present invention will be omitted, and the same reference numerals will be used for the same components throughout the specification. It should be understood that the specific shapes, structures, and characteristics described in the specification may be changed from one embodiment to another without departing from the spirit and scope of the present invention, and the position or arrangement of individual components may also be changed without departing from the spirit and scope of the present invention.

[0019] Therefore, the following detailed description should not be taken in a limiting sense, and the scope of the present invention should be understood to encompass the scope of the appended claims and all equivalents thereof.

[0020] FIG. 1 is a drawing that illustrates a cross section of an all-solid-state battery.

[0021] 1, an all-solid-state battery 10 includes a positive electrode 11, a negative electrode 12, and a solid electrolyte layer 13. The solid electrolyte layer 13 is disposed between the positive electrode 11 and the negative electrode 12, and may be in contact with the positive electrode 11 and the negative electrode 12, respectively. The positive electrode 11 and the negative electrode 12 may each include a positive electrode active material layer and a negative electrode active material layer, and the positive electrode active material layer and the negative electrode active material layer may each be in contact with the solid electrolyte layer 13.

[0022] The positive electrode 11 and the negative electrode 12 can each be joined to the solid electrolyte layer 13 by sintering. That is, the positive electrode 11, the negative electrode 12 and the solid electrolyte layer 13 can be sintered together.

[0023] 1 illustrates an all-solid-state battery 10 including one layer each of a positive electrode 11, a negative electrode 12, and a solid electrolyte layer 13, but the present invention is not limited to this, and the all-solid-state battery may be configured such that the positive electrode, the negative electrode, and the solid electrolyte layer each include multiple layers. Alternatively, the all-solid-state battery may be configured as a so-called stacked type all-solid-state battery in which multiple positive electrodes, negative electrodes, and solid electrolyte layers are stacked alternately.

[0024] The solid electrolyte layer 13 according to an embodiment of the present invention includes an oxide-based electrolyte as a solid electrolyte. In one embodiment, the solid electrolyte includes an oxide having a Nasicon crystal structure. In one embodiment, the oxide having the Nasicon crystal structure is LAGP(Li 1+x Al x Ge 2-x (PO4)3) or LATP(Li 1+x Al x Ti 2-x (PO4)3).

[0025] The solid electrolyte contained in the solid electrolyte layer 13 according to an embodiment of the present invention further includes a sintering aid.

[0026] Generally, oxide electrolytes with NASICON type crystal structure are sintered at high temperatures of over 1,000℃. In this case, as mentioned above, it is possible to obtain a relatively good ion conductivity, but the increase in manufacturing costs due to high temperature sintering is unavoidable.

[0027] In one embodiment of the present invention, by adding a sintering aid to an oxide-based electrolyte having a NASICON type crystal structure, it is possible to significantly lower the sintering temperature while ensuring excellent ion conductivity.

[0028] The sintering aid according to an embodiment of the present invention may be a compound containing Li, V, and Ag. For example, the sintering aid according to an embodiment of the present invention may include Li2O, V2O5, and Ag2O.

[0029] Li2O, an oxide that acts as a sintering aid, provides Li ions and improves ion conductivity.

[0030] V2O5 is a low-temperature component that lowers the sintering temperature. In addition, V ions exist as pentavalent ions, and as the V ions increase, the nonbridging oxygen increases, creating additional ion flow paths in the network structure, which can improve ion conductivity.

[0031] Ag2O acts to lower the sintering temperature and also acts as a network modifier within the compound. Ag2O can improve ionic conductivity by breaking the connection of the main glass-forming network and allowing the flow of conductive ions.

[0032] As described above, the sintering aid according to an embodiment of the present invention includes Li2O, V2O5, and Ag2O, whereby V2O5 functions as a main glass former and can widen the flow path of Li ions, and Ag2O can cut the glass network and lower the sintering temperature.

[0033] The sintering temperature of the sintering aid according to one embodiment of the present invention is about 500° C. to about 600° C. When the sintering aid according to one embodiment of the present invention is sintered at the above temperature, it has a heat energy of about 1.5×10 -5 ~Approx. 1.6×10 -5 The ionic conductivity in S / cm is shown.

[0034] The solid electrolyte according to an embodiment of the present invention may contain 95% by mass or more of an oxide-based electrolyte having a NASICON type crystal structure and 5% by mass or less of a sintering aid. When the solid electrolyte according to an embodiment of the present invention is sintered at 500°C to 600°C, the ionic conductivity is about 1.4×10 -4 ~Approx. 1.5×10 -4 S / cm is indicated.

[0035] The present invention will now be described in more detail with reference to specific examples and test examples of the present invention.

[0036] [Example]

[0037] Example 1

[0038] A precursor powder for manufacturing a sintering aid was prepared by mixing 48 mol% Li2O, 527 mol% V2O, and 25 mol% Ag2O. After mixing the precursor powder, it was placed in a melting furnace and melted at a temperature of about 1,100°C for about 1 hour. The homogenized melt was then poured into a quenching roller and cooled to room temperature, then crushed and sieved to obtain the sintering aid in the form of cullets with a size of 200μm or less.

[0039] Additional Examples and Comparative Examples

[0040] Precursor powders were prepared by varying the composition ratio of Li2O, V2O525, and Ag2O, and melted at a temperature of 800°C to 1,200°C for about 1 hour according to the composition ratio. Then, the same process as in Example 1 was carried out to obtain sintering aids in the form of cullets.

[0041] The composition ratios of the sintering aids in the above-described examples and comparative examples are as shown in Table 1.

[0042] [Table 1]

[0043] The sintering aids of the Examples and Comparative Examples in Table 1 were mixed with LAGP and sintered to produce solid electrolytes. 1.5 Al 0.5 Ge 1.5 The solid electrolyte was prepared by mixing about 97% by mass of (PO4)3 and sintering at about 550° C. for about 12 hours. The transition temperature, crystallization temperature, and ionic conductivity of the solid electrolyte prepared as described above were measured, and the results are shown in Table 2.

[0044] [Table 2]

[0045] Referring to Table 2, it is confirmed that the solid electrolytes manufactured including the sintering aids according to Examples 1 to 4 of the present invention have transition points of 380°C or less and crystallization temperatures of 400°C or less. In comparison, the solid electrolytes manufactured including the sintering aids according to Comparative Examples 1 to 4 have transition points of 440°C or more and crystallization temperatures of 450°C or more. In other words, it can be confirmed that the solid electrolytes manufactured including the sintering aids according to Examples 1 to 4 have the property of being capable of low-temperature sintering. The solid electrolytes manufactured including the sintering aids according to Examples 1 to 4 of the present invention have a crystallization temperature of 3.19×10 -6 S / cm or more, whereas the solid electrolytes prepared including the sintering aids according to Comparative Examples 1 to 4 have lower ion conductivities. In particular, the solid electrolyte prepared including the sintering aid according to Example 1 (i.e., a sintering aid containing 50 mol% Li2O, 525 mol% V2O, and 25 mol% Ag2O in a molar ratio of 2:1:1) was confirmed to exhibit significantly excellent ion conductivity.

[0046] Although the present invention has been described above using specific details such as specific components and limited examples, the above examples are merely provided to facilitate a more general understanding of the present invention, and the present invention is not limited thereto. Those having ordinary knowledge in the technical field to which the present invention pertains may make various modifications and variations from such descriptions.

[0047] Therefore, the concept of the present invention should not be limited to the above-described embodiments, and all modifications equivalent to or similar to the scope of the claims, as well as the scope of the following claims, can be said to fall within the scope of the concept of the present invention.

Claims

1. Contains a solid electrolyte having a NASICON type crystal structure and a sintering aid, The sintering aid is composed of an oxide containing Li, Ag and V, Solid electrolyte for all-solid-state batteries.

2. The sintering aid is Li 2 O 45-61 mol%, V 2 O 5 25 to 40 mol% and Ag 2 The solid electrolyte for an all-solid-state battery according to claim 1, which is produced from 6 to 25 mol% O.

3. The sintering aid is Li 2 O.V. 2 O 5 and Ag 2 Contains O, Li 2 O.V. 2 O 5 and Ag 2 The solid electrolyte for an all-solid-state battery according to claim 1 or 2, wherein the molar ratio of O is 2:1:

1.

4. The solid electrolyte for an all-solid-state battery according to any one of claims 1 to 3, wherein the sintering temperature is 550°C or less.

5. Ionic conductivity at room temperature is 0.3 x 10 -5 ~1.4 x 10 -4 The solid electrolyte for an all-solid-state battery according to any one of claims 1 to 4, wherein the conductivity is 1.0 S / cm.

6. The solid electrolyte for an all-solid-state battery according to any one of claims 1 to 5, wherein the solid electrolyte having a NASICON type crystal structure is a LAGP solid electrolyte or a LATP solid electrolyte.

7. A sintering aid for a solid electrolyte for an all-solid-state battery, comprising: A sintering aid consisting of an oxide containing Li, Ag and V.

8. Li 2 O 45-61 mol%, V 2 O 525 to 40 mol% and Ag 2 The sintering aid according to claim 7, which is made from 6 to 25 mol% O.

9. Li 2 O.V. 2 O 5 and Ag 2 Contains O, Li 2 O.V. 2 O 5 and Ag 2 9. The sintering aid according to claim 7 or 8, wherein the molar ratio of O is 2:1:1.

Citation Information

Patent Citations

  • Solid electrolyte and all solid battery containing it

    JP2004335455A

  • Conductive material and positive electrode material for lithium ion secondary battery using the same

    JP2011014373A

  • All-solid secondary battery

    JP2012209256A