Graphene oxide aerogel

A lightweight graphene oxide airgel crosslinked with metal ions addresses the limitations of existing desiccant materials by providing high porosity, large surface area, and fast adsorption/desorption rates, enhancing moisture management efficiency.

JP2024537631APending Publication Date: 2024-10-16NEWSOUTH INNOVATIONS PTY LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024515024
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-06
Filing Date
2022-09-06
Publication Date
2024-10-16

AI Technical Summary

Technical Problem

Existing desiccant materials such as silica gel and zeolite suffer from issues like large pore size distribution, low surface area to pore volume ratio, low hydrophilicity, and low hydrothermal stability, limiting their wide application in adsorption processes.

Method used

Development of a lightweight graphene oxide (GO)-based airgel material crosslinked with metal ions, which possesses a highly porous structure, large surface area, and high water adsorption capacity with fast adsorption and desorption rates, even at low temperatures.

Benefits of technology

The GO-based airgel exhibits superior adsorption and desorption performance, maintaining capacity and rate under varying humidity conditions, making it suitable for efficient moisture management in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537631000001_ABST
    Figure 2024537631000001_ABST
Patent Text Reader

Abstract

The present disclosure relates to aerogels comprising graphene oxide cross-linked with metal ions. The present disclosure also relates to methods and apparatus for using graphene oxide aerogels, particularly as desiccants.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to Australian Provisional Application No. 2021902883, filed September 6, 2021, the entire contents of which are incorporated herein by reference in their entirety.

[0002] The present invention relates to graphene oxide aerogels, and in particular to methods and apparatus for using same as desiccants, although it can be understood that the invention is not limited to this particular field of use. [Background technology]

[0003] The following description of the prior art is provided to place the present invention in an appropriate technical context and to enable a more complete understanding of the advantages of the present invention. However, it should be understood that any description of the prior art throughout this specification should not be taken as an explicit or implicit admission that such prior art is widely known or forms part of the common general knowledge in the field.

[0004] Nanoporous materials with large nano-sized pores and high surface area have attracted great interest worldwide for adsorption processes. Heterogeneous three-dimensional porous materials such as silica gel and zeolites are widely used as desiccant materials. However, problems such as large pore size distribution, low surface area to pore volume ratio, poor hydrophilicity and / or poor hydrothermal stability associated with the aforementioned materials limit their wide range of applications.

[0005] An ideal desiccant material for adsorption applications would have a large surface area and high porosity with chemical and mechanical stability. Therefore, there is a need to develop new desiccant materials that have one or more of these desirable properties.

[0006] The present invention is directed to overcoming or ameliorating one or more of the problems in the prior art, or at least providing a useful alternative. Summary of the Invention

[0007] The present inventors have surprisingly developed lightweight GO-based aerogel materials that may have a highly porous structure and large surface area suitable for adsorption applications. Due to their unique physicochemical properties, these GO-based aerogels may have high water adsorption capacity with fast adsorption rate and fast adsorption kinetics. Furthermore, the desorption process of these aerogel materials may be completed at low temperature (50°C) or room temperature with low humidity.

[0008] In a first aspect of the present invention, there is provided an aerogel comprising graphene oxide cross-linked with metal ions, the metal ions being selected from the group consisting of alkali metal ions, alkaline earth metal ions, transition metal ions and basic metal ions, the metal ions being selected from the group consisting of Fe 3+ , Co 2+ , Ni 2+ , Cu 2+ , Zr 4+ , Sn 4+ , Ti 4+ , V 5+ , La 3+ , Cr 3+ , Al 3+ , Zn 2+ and Ce 4+ The present invention provides an aerogel which is not selected from the group consisting of:

[0009] The following options may be used individually or in any combination in conjunction with the first aspect.

[0010] One skilled in the art will appreciate that the aerogel may be of any shape or size, and that the shape and / or size will depend on the application. For example, it may have a spherical, cubic, cylindrical, rectangular, tubular, or wire-like structure. In certain embodiments, the aerogel may be in the form of a sheet that is rolled, for example, to fit into a cylindrical device. In certain embodiments, the aerogel may be in the form of a cake, flake, or powder.

[0011] The weight ratio of graphene oxide to metal ions may be about 500:1 to about 1:20, or about 200:1 to about 1:20, about 100:1 to about 1:20, about 50:1 to about 1:20, about 20:1 to about 1:20, about 200:1 to about 1:10, about 200:1 to about 1:5, about 100:1 to about 1:10, about 50:1 to about 1:5, about 20:1 to about 1:2, about 5:1 to about 1:2, or about 5:1 to about 1:1. In certain embodiments, the weight ratio of graphene oxide to metal ions is about 200:1 to about 1:5. In certain embodiments, the weight ratio of graphene oxide to metal ions is about 5:1 to about 1:1. The weight ratio of graphene oxide to metal ions can be, for example, about 500:1, 200:1, 100:1, 50:1, 20:1, 10:1, 5:1, 2:1, 1:1, 1:2, 1:5, 1:10, or 1:20.

[0012] The metal ion may be any ion capable of cross-linking graphene oxide. In certain embodiments, the metal ion is selected from alkali metal ions and alkaline earth metal ions, and combinations thereof. In certain alternative embodiments, the metal ion is a basic metal ion or a transition metal ion. In certain embodiments, the metal ion is an ion selected from the group consisting of beryllium, magnesium, calcium, strontium, lithium, and barium. In certain embodiments, the metal ion may be an iron ion. In certain embodiments, the metal ion is a Be ion. 2+ , Mg 2+ , Ca 2+ , Sr 2+ , Li + and Ba 2+ In certain embodiments, the metal ion is an alkaline earth metal ion. In certain embodiments, the alkaline earth metal ion is Ca 2+ It is.

[0013] Without wishing to be bound by theory, the inventors hypothesize that graphene oxide cross-linked by certain metal ions may provide advantageous adsorption properties, in part, due to the high hydration number of the cross-linking ions attracting more water molecules to their surroundings and / or due to the fast exchange rate of water molecules in the first hydration shell of each metal ion, allowing for the rapid exchange of water molecules and thus increasing the adsorption rate of the cross-linked GO aerogel.

[0014] Graphene oxide itself (i.e., before it is crosslinked) is essentially a two-dimensional material. The size and shape of the graphene oxide can affect the properties of the aerogel. The average aspect ratio of graphene oxide is at least about 20, or at least about 50, 100, 200, 500, 1000, 2000, 5000, 10 4 Or 10 5 The average aspect ratio of the graphene oxide may be about 20 to about 10. 6 , or about 10 2 ~10 6 , 10 3 ~10 6 , 10 4 ~10 6 , 10 5 ~10 6 , 20~10 5 , 20~10 4 , 20~10 3 , 20~10 2 , 10 2 ~10 3 , 10 3 ~10 4 Or 10 4 ~10 5 For example, the average aspect ratio of graphene oxide may be about 20, 30, 40, 50, 100, 200, 500, 10 3 , 5×10 3 , 10 4 , 5×10 4 , 10 5 , 5×10 5 or 10 6The aspect ratio may be defined as the ratio of the smallest lateral dimension (i.e., in the plane of the graphene oxide) to the average non-lateral dimension (i.e., perpendicular to the plane of the graphene oxide). The graphene oxide may be non-uniform in shape, but may have, on average, a lateral dimension that is at least 20 times greater than its average non-lateral dimension.

[0015] In certain embodiments, the average lateral dimension of the graphene oxide may be less than about 10,000 nm, 5,000 nm, 2,000 nm, 1,000 nm, 500 nm, 200 nm, 100 nm, 50 nm, or less than about 20 nm, 10 nm, 5 nm, 2 nm, or 1 nm. In certain embodiments, the average lateral dimension of the graphene oxide is less than about 500 nm. The average lateral dimension of the graphene oxide may be from about 0.5 nm to about 10,000 nm, or from about 1 to 500, 2 to 500, 5 to 500, 10 to 500, 20 to 500, 0.5 to 200, 0.5 to 100, 0.5 to 50, 0.5 to 20, 2 to 50, 5 to 100, or 10 to 200 nm. For example, the average lateral dimension of the graphene oxide may be about 0.5, 1, 2, 5, 10, 20, 50, 100, 200, 500, or 1,000 nm. The graphene oxide may comprise particles formed from multiple sheets of layered material. The average number of individual sheets in each particle may be 1, or may be greater than about 1, or may be greater than about 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, or 50. The average number of individual sheets in each particle may be about 1 to about 1,000, or may be about 1-500, 1-200, 1-100, 1-50, 5-100, 5-1000, 10-1,000, 20-1,000, 50-1,000, 5-100, 10-200, or 20-500. For example, the average number of individual sheets in each particle may be about 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 40, 50, 60, 70, 80, 90, 100, 200, 500, or 100 sheets.

[0016] In certain embodiments, the aerogel may comprise a mixture of graphene oxides having different average lateral dimensions, for example, the aerogel may comprise a mixture of graphene oxides having average lateral dimensions of about 5 μm and graphene oxides having average lateral dimensions of about 300 nm (i.e., the graphene oxides may have a bimodal size distribution).

[0017] In other embodiments, the graphene oxide may have an average lateral dimension of greater than about 200 nm, 500 nm, 1,000 nm, 2,000 nm, or 5,000 nm. In certain embodiments, the average lateral dimension of the graphene oxide is greater than or equal to about 500 nm. The graphene oxide may have an average lateral dimension of about 0.2 μm to about 10 μm, or about 0.5-5, 0.5-2, 0.5-1, 0.2-10, 0.2-5, or 0.2-0.5 μm. For example, the average lateral dimension of the graphene oxide may be about 0.5, 1, 2, 5, or 10 μm. The graphene oxide may comprise particles formed from multiple sheets of layered material. The average number of individual sheets in each particle may be greater than about 20, 30, 40, 50, 60, 70, 80, 90, 100, or 200 sheets. The average number of individual sheets in each particle may be about 20 to about 1000, or about 50 to 500, 50 to 200, 50 to 100, 20 to 50, 20 to 100, 20 to 200, or 20 to 500. For example, the average number of individual sheets in each particle may be about 20, 25, 30, 40, 50, 60, 70, 80, 90, 100, 200, 500, or 1,000.

[0018] The average non-lateral dimension (i.e., thickness) of the graphene oxide may be less than about 2,000 nm, or less than about 1,000, 500, 200, 100, 50, 20, 10, 5, 2, 1, or 0.5 nm. The average non-lateral dimension of the graphene oxide may be about 1-500, 2-500, 5-500, 10-500, 20-500, 0.5-200, 0.5-100, 0.5-50, 0.5-20, 2-50, 5-100, or 10-200 nm. For example, the average non-lateral dimension of the graphene oxide may be about 0.5, 1, 2, 5, 10, 20, 50, 100, 200, 500, or 1,000 nm.

[0019] The carbon:oxygen ratio of the graphene oxide may be about 0.1 to about 5, or about 0.5 to about 5, about 1 to about 4, about 1.5 to about 2.5, or about 2 to about 2.5. For example, the carbon:oxygen ratio of the graphene oxide may be about 0.1, 0.2, 0.5, 1, 1.5, 2, 2.1, 2.2, 2.25, 2.3, 2.35, 2.4, 2.5, 3, 4, or 5. In some embodiments, the graphene oxide has a carbon:oxygen ratio of about 0.5 to about 5. In certain embodiments, the graphene oxide has a carbon:oxygen ratio of about 2.25.

[0020] The adsorption capacity of the aerogel may be about 5% to about 1000% at 100% relative humidity, or may be about 5% to about 500%, about 10% to about 500%, about 20% to about 500%, about 50% to about 500%, about 100% to about 500%, about 20% to about 400%, about 50% to about 300%, about 50% to about 250%, or about 100% to about 250% at 100% relative humidity. In certain embodiments, the adsorption capacity of the aerogel is about 20 to about 400% at 100% relative humidity. The aerogel may have an adsorption capacity of, for example, about 5, 10, 15, 20, 50, 75, 100, 110, 120, 150, 200, 250, 300, 400, 500, 600, 700, 800, 900, or 1000% at 100% relative humidity. In certain embodiments, the aerogel may have an adsorption capacity of at least about 40% at 100% relative humidity, or at least about 50, 60, 70, 80, 90, 100, 110, 120, 150, or 200% at 100% relative humidity.

[0021] The adsorption capacity of the aerogel may be about 5% to about 500% at a relative humidity of 50%, or may be about 5% to about 200%, about 10% to about 500%, about 20% to about 500%, about 50% to about 500%, about 100% to about 500%, about 20% to about 400%, about 50% to about 300%, about 50% to about 250%, or about 100% to about 250% at a relative humidity of 50%. In certain embodiments, the adsorption capacity of the aerogel is about 20 to about 150% at a relative humidity of 50%. The adsorption capacity of the aerogel may be, for example, about 5, 10, 15, 20, 50, 75, 100, 110, 120, 150, 200, 250, 300, 400, or 500% at a relative humidity of 50%.

[0022] The density of aerogel is approximately 0.001 g / cm 3 ~ approx. 0.4g / cm 3 or about 0.002 g / cm 3 ~ approx. 0.4g / cm 3 , about 0.005g / cm 3 ~ approx. 0.4g / cm 3 , about 0.005g / cm 3 ~about 0.3g / cm 3 , about 0.005g / cm 3 ~Approx. 0.25g / cm 3 , about 0.01g / cm 3 ~about 0.2g / cm 3 , about 0.02g / cm 3 ~about 0.2g / cm 3 Or about 0.1g / cm 3 ~about 0.2g / cm 3 In certain embodiments, the density of the aerogel is about 0.005 g / cm 3 ~Approx. 0.25g / cm 3 The density of the aerogel is, for example, about 0.001, 0.002, 0.005, 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, or 0.4 g / cm 3 may be also possible.

[0023] The porosity of the aerogel may be about 50% to about 99.9%, or about 60% to about 99.9%, about 60% to about 99%, about 70% to about 99%, about 80% to about 99%, about 90% to about 99.9%, or about 70% to about 95%. In certain embodiments, the porosity of the aerogel is about 90% to about 99.9%. The porosity of the aerogel may be, for example, about 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 95, 97, 99, 99.5, or about 99.9%.

[0024] In some embodiments, the pore size of the aerogel may range from about 10 nm to about 500 μm. In some embodiments, the average pore size is at least about 20 nm, at least about 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, or 500 nm. In some embodiments, the average pore size is at least about 1 μm, 10 μm, 20 μm, 50 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, or 220 μm. In some embodiments, the average pore size may be about 500 μm or less, 400 μm or less, 300 μm or less, or 250 μm or less. In general, air is a pore size that is generally about 100 μm to 500 μm. The rogel may have an average pore size of about 100 to about 250 μm, about 110 to about 220 μm, about 120 to about 210 μm, or about 130 to 200 μm.

[0025] In certain embodiments, the metal ion is an ion of Li, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Sc, Y, Lu, Lr, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Mn, Tc, Re, Bh, Fe, Ru, Os, Hs, Co, Rh, Ir, Mt, Ni, Pd, Pt, Ds, Cu, Ag, Au, Rg, Zn, Cd, Hg, Cn, Al, Ga, Ge, In, Sn, Sb, Tl, Pb, Bi, Po, Nh, Fl, Mc, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, or Lv, or a combination thereof. In certain embodiments, the metal ion is an ion of Li, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Sc, Y, Lu, Lr, Hf, Rf, Nb, Ta, Db, Mo, W, Sg, Mn, Tc, Re, Bh, Ru, Os, Hs, Rh, Ir, Mt, Pd, Pt, Ds, Ag, Au, Rg, Cd, Hg, Cn, Ga, Ge, In, Sb, Tl, Pb, Bi, Po, Nh, Fl, Mc, or Lv, or a combination thereof.

[0026] In certain alternative embodiments, the metal ion is not one or more of the following ions: Li, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Sc, Y, Lu, Lr, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Mn, Tc, Re, Bh, Fe, Ru, Os, Hs, Co, Rh, Ir, Mt, Ni, Pd, Pt, Ds, Cu, Ag, Au, Rg, Zn, Cd, Hg, Cn, Al, Ga, Ge, In, Sn, Sb, Tl, Pb, Bi, Po, Nh, Fl, Mc, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and / or Lv.

[0027] In a second aspect of the present invention, there is provided a method for preparing an aerogel comprising graphene oxide cross-linked with metal ions, the metal ions being selected from the group consisting of alkali metal ions, alkaline earth metal ions, transition metal ions and basic metal ions, the metal ions being selected from the group consisting of Fe 3+ , Co 2+ , Ni 2+, Cu 2+ , Zr 4+ , Sn 4+ , Ti 4+ , V 5+ , La 3+ , Cr 3+ , Al 3+ , Zn 2+ and Ce 4+ and the method is not selected from the group consisting of (a) contacting graphene oxide with a cross-linker in the presence of a liquid; (b) removing the liquid to form an aerogel; The present invention provides a method for producing an aerogel, comprising:

[0028] The following options may be used individually or in any combination in conjunction with the second aspect.

[0029] The metal ions and / or the aerogel may be as described above in relation to the first embodiment.

[0030] The liquid may be an aqueous liquid, optionally including one or more salts. The liquid may include water. In certain embodiments, the liquid is substantially water. The liquid may include a polar solvent. The liquid may include an alcohol. The liquid may include one or more volatile organic solvents. The liquid may include, for example, ethanol, methanol, acetone, ethyl acetate, dichloromethane, chloroform, or propanol. The liquid may have a boiling point measured at 1 atmosphere of less than about 150° C., or less than about 130° C., 110° C., 90° C., or 70° C., measured at 1 atmosphere.

[0031] In certain embodiments, the liquid is removed by freeze-drying. The freeze-drying may be performed at temperatures between about -100°C and about -20°C, or between about -80°C and about -40°C, or at temperatures between about -100, -80, - The freeze-drying may be carried out at a temperature of -60°C for about 1 to about 48 hours, or for about 2 to about 24 hours, for about 3 to about 12 hours, for about 4 to about 10 hours, or for about 2 to about 5 hours. In certain embodiments, the freeze-drying step is carried out at a temperature of -60°C for about 2 to about 24 hours. Typically, the vacuum level for freeze-drying is between 50 mTorr and 300 mTorr, with 100 mTorr to 200 mTorr being the most common range.

[0032] In certain embodiments, after the contacting step, the graphene oxide is transferred to a mold prior to the freeze-drying step. The mold may be of any shape or size. One skilled in the art will understand that the shape and / or size of the mold will depend on the desired shape and / or size of the aerogel. The metal ion crosslinked graphene oxide in a mixture with a liquid may be transferred to a mold, and upon removal of the liquid, the mixture may form an aerogel having substantially the same volume as the mold.

[0033] In certain embodiments, the method includes providing an aqueous solution of graphene oxide at a predetermined concentration, followed by exposure to a cross-linking agent to provide cross-linked graphene oxide.

[0034] In certain embodiments, the crosslinking agent may be added to the aqueous solution of graphene for about 5 minutes to about 12 hours, or about 10 minutes to about 6 hours, about 30 minutes to about 5 hours, about 1 hour to about 4 hours, or about 1 hour to about 3 hours. The crosslinking agent may be added for about 5, 10, 15, 20, 30, 40, or 50 minutes, or about 1, 1.5, 2, 2.5, 3, 4, 5, 6, 7, 8, 9, 10, or 12 hours. In certain embodiments, the crosslinking agent may be added to the aqueous solution of graphene for about 10 minutes to about 6 hours.

[0035] In certain embodiments, the concentration of graphene oxide in the aqueous solution may be about 0.01% by weight to about 30% by weight, or about 0.02% by weight to about 30% by weight, about 0.05% by weight to about 30% by weight, or about 0.05% by weight to about 20% by weight, about 0.05% by weight to about 10% by weight, about 0.05% by weight to about 5% by weight, or about 0.05% by weight to about 1% by weight, or about 0.05% by weight to about 1.5% by weight. In certain embodiments, the concentration of graphene oxide in the aqueous solution is about 0.01 to about 20% by weight. In certain embodiments, the concentration of graphene oxide in the aqueous solution is about 0.05 to about 5% by weight. The concentration of graphene oxide in the aqueous solution may be about 0.01, 0.02, 0.05, 0.1, 0.2, 0.5, 1, 2, 5, 10, 20, or 30% by weight. In one particular embodiment, the concentration of graphene oxide in the aqueous solution is about 1% by weight.

[0036] In certain embodiments, the cross-linking agent comprises an alkaline earth metal ion and / or an alkali metal ion. In certain embodiments, the alkaline earth metal ion and / or the alkali metal ion is selected from the group consisting of beryllium, magnesium, calcium, strontium, lithium and barium. In certain embodiments, the cross-linking agent is selected from the group consisting of CaCl2 and MgCl2. In certain embodiments, the cross-linking agent is a salt of a metal ion as described above with respect to the first aspect.

[0037] In certain embodiments, after the removing step, the aerogel is compressed. The aerogel may be compressed to 95% or less of its original volume, or to 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, or 40% or less of its original volume. The aerogel may be compressed to about 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, or 20% of its original volume. In certain embodiments, the aerogel is compressed to about 50% of its original volume. The aerogel is compressed to about 0.01 bar to about 5 bar, or to about 0.01 bar to about 2 bar, about 0.02 bar to about 1.5 bar, about 0.05 bar to about 1 bar, about 0.05 bar to about 0.5 bar, or about 0.0 It may be compressed by exposure to a pressure of between about 5 bar and about 0.1 bar. For example, the aerogel may be exposed to a pressure of about 0.01, 0.02, 0.05, 0.1, 0.2, 0.5, 1, 2, 3, 4 or 5 bar.

[0038] In a third aspect of the present invention, there is provided a graphene oxide aerogel produced according to the method of the second aspect.

[0039] In certain embodiments, the graphene oxide aerogel may be as described above with respect to the first aspect.

[0040] In a fourth aspect of the present invention there is provided a method of adsorbing moisture from a gas stream or atmosphere containing said moisture, the method comprising the step of adsorbing said moisture from the gas stream or atmosphere by contacting the gas stream or the atmosphere with a graphene oxide aerogel.

[0041] The gas stream or atmosphere may be a waste gas stream. In certain alternative embodiments, the gas stream or atmosphere may be an inlet stream, particularly for processes where it is advantageous to remove water vapor from the inlet stream.

[0042] In certain embodiments, the aerogel may be contained within a porous packaging that allows moisture to pass through. The packaging may be used for storage applications, such as for storing dry food substances.

[0043] In certain embodiments, the graphene oxide aerogel is an aerogel according to the first or third aspect.

[0044] In a fifth aspect of the present invention, there is provided a use of graphene oxide aerogel for adsorbing moisture from a gas stream. The gas stream may be a waste gas stream. In certain alternative embodiments, the gas stream or atmosphere may be an inlet stream, particularly for a process where it is advantageous to remove water vapor from the inlet stream.

[0045] In certain embodiments, the graphene oxide aerogel is an aerogel according to the first or third aspect.

[0046] In a sixth aspect of the present invention, there is provided a method for desorbing water adsorbed in a graphene oxide aerogel, the method comprising the step of heating the graphene oxide aerogel sufficiently to release the adsorbed water and regenerate the graphene oxide aerogel.

[0047] Heating may be to a temperature of about 30° C. to about 250° C., or about 40° C. to about 250° C., about 40° C. to about 200° C., about 40° C. to about 150° C., about 40° C. to about 100° C., about 40° C. to about 80° C., or about 40° C. to about 60° C. Heating may be to a temperature of, for example, about 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 150, 200, or 250° C. In certain embodiments, heating may be at room temperature.

[0048] Heating may be for a period of about 10 minutes to about 48 hours, or about 20 minutes to about 48 hours, about 30 minutes to about 48 hours, about 60 minutes to about 48 hours, about 10 minutes to about 24 hours, about 10 minutes to about 12 hours, about 10 minutes to about 8 hours, about 10 minutes to about 6 hours, or about 30 minutes to about 8 hours. For example, heating may be for about 10, 20, 30, 40, or 50 minutes, or for about 1, 2, 4, 6, 8, 10, 12, 14, 16, 18, 20, 24, 36, or 48 hours.

[0049] In certain embodiments, the graphene oxide aerogel is an aerogel according to the first or third aspect.

[0050] In a seventh aspect of the present invention, there is provided a method for recovering water from a water-adsorbed graphene oxide aerogel, the method comprising the steps of heating the graphene oxide aerogel sufficiently to release the adsorbed water and recovering the water.

[0051] Heating may be to a temperature of about 30° C. to about 250° C., or about 40° C. to about 250° C., about 40° C. to about 200° C., about 40° C. to about 150° C., about 40° C. to about 100° C., about 40° C. to about 80° C., or about 40° C. to about 60° C. Heating may be to a temperature of, for example, about 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 150, 200, or 250° C. In certain embodiments, heating may be at room temperature.

[0052] Heating may be for a period of about 10 minutes to about 48 hours, or about 20 minutes to about 48 hours, about 30 minutes to about 48 hours, about 60 minutes to about 48 hours, about 10 minutes to about 24 hours, about 10 minutes to about 12 hours, about 10 minutes to about 8 hours, about 10 minutes to about 6 hours, or about 30 minutes to about 8 hours. For example, heating may be for about 10, 20, 30, 40, or 50 minutes, or for about 1, 2, 4, 6, 8, 10, 12, 14, 16, 18, 20, 24, 36, or 48 hours.

[0053] The method may include cooling the water vapor produced by the heating process. Cooling may be performed to a temperature of about 90° C. or less, or 80, 70, 60, 50, 40, 30, 20, 10, 0, −10, −20 or −30° C. or less.

[0054] In certain embodiments, the graphene oxide aerogel is an aerogel according to the first or third aspect.

[0055] In an eighth aspect of the present invention, there is provided an atmospheric water generating device comprising graphene oxide aerogel.

[0056] In certain embodiments, the atmospheric water generator includes an inlet for introducing a gas stream or atmosphere therein such that the gas stream or atmosphere contacts the graphene oxide aerogel, the gas stream or atmosphere may include moisture, and the graphene oxide aerogel may adsorb moisture from the gas stream or atmosphere.

[0057] In certain embodiments, the atmospheric water generator further comprises a heating element for heating the graphene oxide aerogel and releasing moisture adsorbed thereon. In certain embodiments, the atmospheric water generator further comprises a cooling element for cooling and condensing the moisture released in the heating process to form water. The atmospheric water generator may further comprise a container for collecting the condensed water.

[0058] In certain embodiments, the graphene oxide aerogel is an aerogel according to the first or third aspect. [Brief description of the drawings]

[0059] [Figure 1] Figure 1 shows an exemplary GO / Ca2+ solution (~30 mL) transferred to a 10 cm diameter glass Petri dish for the freeze-drying process, (a) top view, (b) side view. [Diagram 2] FIG. 1 shows an exemplary freeze-dryer dried GO-based aerogel. [Diagram 3] FIG. 1 shows a schematic diagram of an exemplary adsorption measurement setup for laboratory scale. [Figure 4] An example of the adsorption setup used in the laboratory is shown. [Diagram 5] Exemplary GO-based aerogels synthesized from GO solutions with lateral dimensions (a) >500 nm and (b) <500 nm, and (c) AFM image of GO nanosheets. [Figure 6] FIG. 1 shows images of exemplary GO-based aerogels with different weight ratios of GO to Ca2+: a) 1:1 and b) 5:1. [Figure 7] Figure 2 shows the water adsorption kinetics of GO-based aerogels with different weight ratios of GO to crosslinker: (a) GO:Ca2+=100:1, (b) GO:Ca2+=50:1, (c) GO:Ca2+=10:1, (d) GO:Ca2+=5:1, and (e) GO:Ca2+=1:1. [Figure 8] The schematic design of the canister for GO-based aerogel compression testing is shown. [Figure 9]Figure 3 shows the 3D-printed canister used for the aerogel compression test at its volumetric scale. The volume of the GO-based aerogel in the canister was 300 cm3 without compression. [Figure 10] FIG. 1 shows an exemplary GO-based aerogel after compression under high pressure (1.5 bar) into a thin film. [Figure 11] Figure 1 shows the percent adsorption capacity of an exemplary GO aerogel (a) without compression and (b) with compression at 0.07 bar. [Figure 12] Figure 2 shows the adsorption kinetics of exemplary GO-based aerogels with different concentrations of GO solution and weight ratios of crosslinker: (a) 1 wt%, GO:Ca2+1:1, (b) 1.5 wt%, GO:Ca2+1:1, (c) 1.5 wt%, GO:Ca2+2:1. [Figure 13] Figure 2 shows the adsorption kinetics of an exemplary GO-based aerogel at (a) RH 100%, (b) RH 80%, (c) RH 70%, and (d) RH 50%. [Figure 14] Figure 2 shows the adsorption capacity vs. relative humidity for (a) an exemplary GO aerogel, (b) an exemplary GO aerogel with a 50% reduction in volume, and (c) silica gel. [Figure 15] FIG. 1 shows the relationship between density, RH, and adsorption capacity of exemplary GO-based aerogels (a) without compression, (b) with 50% volume reduction, and (c) with 75% volume reduction. [Figure 16] Figure 2 shows the adsorption kinetics of eGO-based aerogels after four cycles. [Figure 17] 1 shows a schematic diagram of an exemplary desorption process. [Figure 18] 1 shows an exemplary experimental setup for laboratory-scale desorption testing. [Figure 19] We show that a simple exemplary desorption process can be used to recollect the adsorbed water. [Figure 20] (a) Exemplary prototype components; (b) Exemplary mold module for GO-based aerogel preparation. [Figure 21] An exemplary 3D printed mold module for GO aerogel preparation is shown. [Figure 22]Description of the laboratory-scale fabrication of exemplary GO aerogels: (a) metal ion cross-linked graphene oxide suspension, (b) freeze-drying of the cross-linked GO suspension, and (c) formation of GO aerogels. [Figure 23] Figure 1. Effect of GO flake size on the adsorption performance of an exemplary aerogel (GO:Ca2+1:1). Aerogel samples were prepared by using different GO flake sizes: (a) -5 μm (relative humidity -80%, maximum capacity -72.9%), (b) -1 μm (relative humidity -90%, maximum capacity -123.9%), and (c) -300 nm (relative humidity -90%, maximum capacity -123.3%). [Figure 24] Figure 2 shows the adsorption performance of exemplary GO aerogels prepared using a mixture of GO flakes of different sizes (~5 μm and ~300 nm) in the ratios of (a) 100:0 (max capacity 72.9%), (b) 75:25 (max capacity 33.3%), (c) 50:50 (max capacity 100.9%), and (d) 25:75 (max capacity 38.4%). Experimental conditions: GO:Ca2+=1:1, humidity=80%. [Diagram 25] Comparison of the adsorption performance of exemplary aerogels at different humidities: (a) 90% (maximum capacity ∼123.3%), (b) 75% (maximum capacity ∼68.5%), (c) 60% (maximum capacity ∼42.7%), and (d) 50% (maximum capacity 37.6%). The aerogels were generated from GO flakes with lateral dimensions of ∼300 nm. [Figure 26] Comparison of the adsorption performance of exemplary GO aerogels at different humidities: (a) 90% (maximum capacity ~123.9%), (b) 75% (maximum capacity ~94.4%), (c) 60% (maximum capacity ~62.9%), (d) 50% (maximum capacity ~39.4%), (e) 40% (maximum capacity ~23.4%), and (f) 30% (maximum capacity ~15.3%). [Figure 27] Relative humidity vs. adsorption performance of exemplary GO aerogels prepared by using Ca2+ crosslinker. The inset arrows indicate the decreasing trend of adsorption capacity (%). The adsorption capacity at 100 min was used for the comparison plot. [Figure 28]Adsorption performance of GO aerogels crosslinked with different metal ions: (a) Ca2+ (relative humidity ~80%, maximum capacity ~124%), (b) Al3+ (relative humidity ~90%, maximum capacity ~107.9%), (c) Mg2+ (relative humidity ~75%, maximum capacity ~42%), (d) K+ (relative humidity ~80%, maximum capacity ~30%). GO:crosslinker = 2:1. [Figure 29] Adsorption performance of GO aerogels crosslinked with different metal ions: (a) Ca2+ (maximum capacity ~120.9%), (b) Li+ (maximum capacity ~96%), and (c) Fe3+ (maximum capacity ~72.5%). GO:crosslinker = 1:1, relative humidity = 75-90%. [Diagram 30] Flake-shaped GO aerogels with a diameter of approximately 2 cm were prepared by scissors cutting. [Diagram 31] Comparison of the adsorption performance of exemplary GO aerogels with different shapes: (a) cake, (b) powder, and (c) flake (diameter about 2 cm) GO:Ca2+=1:1, relative humidity=about 90%. [Diagram 32] Figure 1 shows the adsorption performance of an exemplary eGO at different relative humidities (RH): (a) 100%, (b) 80-85%, and (c) 75-80%. (d) Comparative adsorption capacity curves of an exemplary eGO at different humidities. [Diagram 33] Exemplary eGO multiple adsorption cycles: A) 1st cycle, B) 2nd cycle, C) 3rd cycle, D) 4th cycle, E) 5th cycle, F) 6th cycle, G) 7th cycle, H) 8th cycle. eGO:Ca2+=1:1, RH=~100%. [Diagram 34] Comparative plot of the adsorption capacity of aerogels prepared by eGO (a) and eGO made by Armidale (b). eGO:Ca2+=1:1, relative humidity=~85~90%. [Diagram 35] Adsorption performance of eGO-UNE aerogels: (a) Sample 1 (maximum capacity approx. 177%) and (b) Sample 2 (maximum capacity approx. 125%). eGO:Ca2+ = 1:1, relative humidity = approx. 90–95%. [Diagram 36]Stepwise preparation of exemplary GO aerogels at large scale for freeze-drying: (a) Crosslinked GO suspension loaded into a metal tray (19 cm × 35 cm × 3 cm), (b–e) stacking trays in a -80 °C freezer, (f–h) visualization of frozen samples. [Figure 37] Adsorption performance of exemplary GO aerogels at large scale: (a) the first batch aerogel (~10.97 g), (b) the second batch aerogel (~8.22 g), (b) the third batch aerogel (~10.12 g) at RH 90%, GO:Ca2+=1:1. [Figure 38] Adsorption performance of GO aerogel on a small scale (~0.4 g) from the second batch sample. GO:Ca2+=1:1, relative humidity=85-95%. [Figure 39] Adsorption performance of exemplary aerogels (at a concentration of 1 wt%) with different weight ratios of GO to crosslinker: (a) 100:1, (b) 50:1, (c) 10:1, (d) 5:1, and (e) 1:1 in the range of relative humidity from 95 to 100%. (f) Comparative plot showing the increase in adsorption performance with increasing crosslinker ratio. The plot is based on 600 min measurements. The arrows represent the increasing trend of the adsorption performance of GO aerogels. [Diagram 40] Adsorption performance of exemplary GO aerogels with various thicknesses using external pressures: (a) ~0.07 bar, (b) ~1.5 bar, and (c) ~10 bar. (d) Design of the canister for compression of GO aerogels (left) and the 3D-printed canister containing GO aerogels for compression (right). Relative humidity ~95-100%. [Diagram 41] Analysis of the effect of ultrasonic treatment during sample preparation on the performance of GO aerogels. (a) No ultrasonic treatment was applied during sample preparation, (b) ultrasonic treatment was applied for 10 min during sample preparation. GO:Ca2+=2:1, relative humidity=approximately 95–100% [Diagram 42]Adsorption performance of exemplary GO aerogels (1.5 wt%) at different humidities: (a) about 95-100%, (b) about 80%, (c) about 70%, and (d) about 50%. The aerogel samples were prepared by crosslinking with Ca2+ at a weight ratio of GO to crosslinker of 2:1. [Diagram 43] Isotherm spectra of an exemplary GO aerogel: (a) adsorption isotherm (atmospheric pressure), (b) adsorption isotherm (vacuum), (c) fast readsorption upon ventilation. Adsorption was performed at 85% humidity and desorption was tested under two different conditions: atmospheric pressure and vacuum. Desorption tests by both techniques were carried out at ambient temperature. The grey highlighted area represents the isotherm under vacuum. Sample weight 2.7 g, room temperature, RH 85%. [Diagram 44] Isotherm spectra of an exemplary aerogel: (a) adsorption, (b) desorption. Sample mass = approx. 8.57 g, relative humidity = 85%, desorption test was performed in dry air at 30 °C. [Diagram 45] Isothermal curves of GO aerogel: (a) adsorption, (b) desorption. Sample mass = approx. 3.73 g, relative humidity = 85%, and desorption test was carried out in dry air at 40 °C. [Diagram 46] Isothermal curves of GO aerogel: (a) adsorption, (b) desorption. Sample mass = 2.91 g, relative humidity = 55%, desorption test was carried out in dry air at 40 °C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0060] definition In describing and claiming the present invention, the following terminology will be used in accordance with the definitions set out below. It is also to be understood that the terminology used herein is for the purpose of describing particular embodiments of the invention only, and is not intended to be limiting.

[0061] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0062] Unless the context clearly requires otherwise, throughout the specification and claims, the terms "comprise," "comprising," and the like are intended to be construed in an inclusive sense, i.e., "including, but not limited to," as opposed to an exclusive or exhaustive sense. For example, a composition, mixture, process, or method that includes a list of elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, mixture, process, or method.

[0063] The transitional phrase "consisting of" excludes any element, step, or ingredient not specified. When present in a claim, such would close the claim to the inclusion of materials other than those recited, except for impurities ordinarily associated with them. When the phrase "consisting of" appears in a clause in the body of a claim rather than immediately following a preamble, it limits only the elements recited in that clause and does not exclude other elements from the claim as a whole.

[0064] The transitional phrase "consisting essentially of" is used to define a composition, process, or method that includes materials, steps, features, components, or elements in addition to those literally disclosed, but where these additional materials, steps, features, components, or elements do not materially affect the basic and novel characteristic(s) of the claimed invention. The term "essentially consisting of" occupies a compromise between "comprising" and "consisting of."

[0065] It should be readily understood that where an applicant has defined an invention or a portion thereof using open-ended terms such as "comprising," the specification (unless otherwise stated) should also be construed as describing such invention using the terms "consisting essentially of" or "consisting of." In other words, with respect to the terms "comprising," "consisting of," and "consisting essentially of," where one of these three terms is used herein, the presently disclosed and claimed subject matter may also include the use of either of the other two terms. Thus, in some embodiments not expressly stated otherwise, any instance of "comprising" may be replaced with "consisting of" or "consisting essentially of."

[0066] Other than in the operating examples, or where otherwise indicated, all numbers expressing quantities of ingredients or reaction conditions used herein should be understood in all instances to be modified by the term "about." The examples are not intended to limit the scope of the invention. Hereinafter, or where otherwise indicated, "%" means "% by weight," "ratio" means "ratio by weight," and "parts" means "parts by weight."

[0067] As used herein, the terms "majority," "predominantly," and "substantially" are intended to mean including 50% by weight or more, unless otherwise indicated.

[0068] As used herein, in connection with a range of numerical values, the terms "about," "approximately," and "substantially" are understood to refer to a range of -10% to +10% of the referenced numerical value, preferably -5% to +5% of the referenced numerical value, more preferably -1% to +1% of the referenced numerical value, and most preferably -0.1% to +0.1% of the referenced numerical value. Moreover, with respect to numerical ranges, these terms should be construed as providing support for claims regarding any number or subset of numbers within that range. For example, a disclosure of 1 to 10 should be construed as supporting ranges of 1 to 8, 3 to 7, 1 to 9, 3.6 to 4.6, 3.5 to 9.9, 8 to 10, etc.

[0069] The terms "preferred" and "preferably" refer to embodiments of the invention that may provide certain benefits, under particular circumstances. However, other embodiments may also be preferred, under the same or other circumstances. Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.

[0070] As used herein, the term "aerogel" refers to a porous material derived from a gel in which the liquid component of the gel has been replaced by a gas without significant collapse of the gel structure. In certain embodiments, particularly when the material comprises graphene oxide, it has a density of about 0.5 g / cm. 3 Less than or about 0.2 g / cm 3 , about 0.1 or about 0.05 g / cm 3 By "density" is meant a material having a density less than

[0071] As used herein, the term "gel" means a soft, solid or solid-like material consisting of two or more components, one of which is liquid, present in significant amounts.

[0072] As used herein, the term "crosslinked" with respect to graphene oxide means that two or more graphene oxide sheets are bound together by a bond or a series of bonds via bridging groups, where the bridging groups are not themselves constituents of the graphene oxide sheets. In certain embodiments, the bridging groups are metal ions.

[0073] As used herein, the term "lateral dimension" with respect to graphene oxide refers to the average width and length of the graphene oxide sheet in the plane of the sheet, i.e., the dimension perpendicular to the thickness of the sheet.

[0074] As used herein, the term "adsorption capacity" with respect to an aerogel can be calculated according to the following formula:

[0075]

number

[0076]

number

[0077] As used herein, the terms "adsorption" or "adsorb" or "adsorbed" should be interpreted broadly and include any process by which water molecules may be adsorbed onto or within an aerogel, including, for example, adsorption and / or adsorption processes.

[0078] As used herein, the term "basic metal" should be interpreted as including any metal in Groups 13 to 16 of the Periodic Table, including Al, Ga, Ge, In, Sn, Sb, Tl, Pb, Bi, Po, Nh, Fl, Mc, Lv.

[0079] As used herein, the term "transition metal" should be interpreted as including any metal in Groups 3 to 12 of the Periodic Table, including Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Rf, Db, Sg, Bh, Hs, Mt, Ds, Rg, Cn, the lanthanides and the actinides.

[0080] Abbreviation AFM: atomic force microscope, DI: deionized, eGO: electrochemically exfoliated graphene oxide, GO: graphene oxide, ICP-MS: inductively coupled plasma mass spectrometry, RH: relative humidity. EXAMPLES

[0081] Preferred features, embodiments and variations of the present invention can be discerned from the following examples, which provide sufficient information for one skilled in the art to practice the invention and should not be construed in any way as limiting the scope of the foregoing summary of the invention.

[0082] Preparation of graphene oxide-based aerogels Graphene oxide-based aerogels were prepared by cross-linking graphene oxide with calcium ions (CaCl2) and freeze-drying the resulting cross-linked graphene oxide. The detailed experimental procedures are described as follows. 1. A graphene oxide solution with a certain concentration was prepared. 2. A stock solution of CaCl2 in water was prepared with a concentration of 10 wt.%. The CaCl2 solution for aerogel preparation could be diluted to different concentrations with DI water to improve mixing (this may be optional for large scale aerogel formation). 3. CaCl2 solution with a certain weight ratio was gradually added to the GO solution with constant stirring for 30 min. 4. Next, GO / Ca 2+ The solution was transferred into a mold (e.g., see Figure 1) for a freeze-drying process (e.g., as shown in Figure 2) to form the GO-based aerogel.

[0083] Adsorption capacity measurement setup The adsorption capacity of GO-based aerogels was measured in a plastic glove bag. As shown in Figures 3 and 4, the glove bag (380 and 410) was connected to a flask (335 and 440) filled with water (330) to increase humidity. The relative humidity (RH) inside the glove bag was influenced by the moisture flow rate and temperature, which were controlled using an inlet valve (320, located near the inlet 310) and heaters (340 and 450). A balance (360 and 430) was placed inside the glove bag to continuously record the weight change of the aerogels (350 and 420) inside the cage 370. Two humidity sensors (390 and 460) were used to monitor the relative humidity inside the glove bag. The glove bag was connected to an outlet (395 and 470) through which the vapor could leave the bag.

[0084] Air entered the apparatus through inlet 310 via inlet valve 320, passed through water 330 in flask 335, into glove bag 380, and then exited through outlet 395. Water 330 was heated by heater 340. Sensor 390 measured the relative humidity inside the glove bag to which aerogel sample 350 in cage 370 was exposed. Balance 360 ​​was used to measure the mass change of aerogel 350.

[0085] Adsorption capacity calculation The adsorption capacity of GO-based aerogels was calculated based on the weight change of the aerogels. When the aerogels started to adsorb water, their weight increased. The aerogels that adsorbed water molecules reached a maximum weight when saturated. The adsorption capacity was calculated by the following equation:

[0086]

number

[0087]

number

[0088] Adsorption capacity of GO-based aerogels The adsorption capacity of GO-based aerogels was significantly affected by the physicochemical properties of GO used in the preparation of the aerogels. The lateral dimensions, C / O ratio, and concentration of GO significantly affected the adsorption capacity of GO-based aerogels. Different morphologies of GO-based aerogels have different adsorption capacities due to their influence on the formation.

[0089] Crosslinker Ca 2+ (CaCl2) was used to improve the mechanical properties of GO-based aerogels. 2+ The weight ratio of GO to GO is also an important factor that leads to the variation in performance. The weight ratio was adjusted according to the concentration of GO solution, which affects the formation process of GO-based aerogels, resulting in different adsorption capacities of the aerogels.

[0090] Some external factors, such as applied compression and relative humidity, may also play an important role in the adsorption capacity of GO-based aerogels. To reduce the volume of the aerogels, GO-based aerogels were compressed under various pressures. There was a limiting pressure to maintain the capacity of GO-based aerogels. High compression can damage the microstructure of GO-based aerogels and reduce the capacity of the desiccant.

[0091] It was found that GO-based aerogels have different adsorption capacities under different relative humidity conditions. In general, the adsorption capacity of GO-based aerogels increases under high relative humidity and decreases under low relative humidity.

[0092] Effect of lateral dimensions of GO The lateral dimension of GO, which can be adjusted by pre- or post-treatment of the synthesis process, is an important parameter for tuning the properties of GO-based aerogels. The C / O ratio of the GO used is about 2.25. Figure 5 shows the GO-based aerogels formed using GO solutions with different lateral dimensions. Figure 5a shows that GO with lateral dimensions >500 nm provided homogeneous morphology of the aerogels. Aerogels using GO solutions with GO lateral dimensions <500 nm have a porous structure, which could potentially increase the active sites for adsorbing water molecules. Figure 5c shows atomic force microscopy (AFM) images of GO nanosheets with different lateral dimensions.

[0093] Adsorption measurements were determined for these two aerogels. Table 1 shows how the lateral dimensions of GO affect the properties of the aerogel. Multiple adsorption cycles demonstrated the stability of the GO aerogels. The GO-based aerogels with smaller lateral dimensions performed better in terms of their stability and adsorption capacity, while the GO aerogels with larger lateral dimensions still had reasonable properties.

[0094] [Table 1]

[0095] GO and Ca 2+ Weight ratio of The GO used in the following experiments had lateral dimensions of <500 nm. As shown in Figure 6, the Ca 2+ There was no obvious difference in the morphology of the aerogel when GO:Ca was used (Figure 6 shows a) 1:1 and b) 5:1 GO:Ca 2+ However, Ca 2+ The weight ratio of GO and Ca influenced the adsorption capacity of GO-based aerogels. 2+ When the weight ratio of GO and Ca was changed from 100:1 to 10:1, the adsorption capacity of GO-based aerogels initially showed a decrease from 81% to 58%. 2+When the weight ratio of crosslinker was increased to 1:1, the adsorption capacity of the GO-based aerogels increased significantly by 258%. Table 2 shows the adsorption capacity of the GO-based aerogels with different weight ratios of crosslinker. The lateral dimensions of the GO used were <50 0 nm and the RH was in the range of 90 to 100%.

[0096] [Table 2]

[0097] Figure 7 shows the relationship between GO and Ca 2+ The adsorption kinetics of GO-based aerogels with different weight ratios of GO and Ca 2+ When the weight ratio of GO and Ca was in the range of 100:1 to 5:1 (Figure 1(a)-(d)), the adsorption rate did not change significantly. Within 60 min, the adsorption capacity reached about 40%. However, the adsorption rate of GO and Ca was significantly increased. 2+ The GO-based aerogel with a weight ratio of 1:1 had an adsorption capacity of 258% and a faster adsorption rate than the other aerogels. As shown in Figure 6(e), the adsorption capacity of the 1:1 GO-based aerogel reached 102% within 60 min.

[0098] Compression effect of GO-based aerogels The adsorption capacity of GO-based aerogel with and without compression was measured. The GO-based aerogel was compressed to save space during the packaging process for commercialization. A canister for compression testing was designed as shown in FIG. 8. The components of the canister include an outer body 810, a plunger arm 830, a plunger plate 840, a lid 820, and components 850 and 860 for fixing the position of the plunger plate during use. To assemble the canister, the plunger arm 830 is threaded through the square hole in the lid 820 and screwed onto the plunger plate 840. The plunger arm and plunger plate assembly is inserted into the outer body 810, and the lid 820 is screwed into place on the threads at the top of the outer body 810. This canister was designed for an aerogel with a diameter of 10 cm. After the aerogel is packed into the canister, the aerogel can be compressed by applying pressure to the plunger arm to reduce the volume according to the volume scale on the outer body 810 of the canister. Components 850 and 860 are then inserted through the openings in the outer body 810 of the canister and into the side openings of the plunger plate 840, thereby clamping the plunger plate 840 to hold it in place and keep the aerogel in a compressed form. Figure 9 shows the volume of 300 cm inside the 3D printed canister without compression. 3 Shown is a GO-based aerogel 930. Shown is a plunger arm 910 and an outer body 920 with volumetric graduations 940.

[0099] Table 3 shows the adsorption performance of GO-based aerogel under different compression forces. Moderate compression does not seem to impair the adsorption capacity of GO-based aerogel. For example, even when the volume is reduced by 48%, the adsorption capacity does not decrease at all compared to the uncompressed aerogel. However, there is a limit pressure to maintain the capacity of GO-based aerogel. High compression can damage the microstructure of GO-based aerogel and reduce its capacity. For example, when the aerogel was compressed into a thin film by applying high pressure as shown in Figure 10, the adsorption capacity was reduced by half (Table 3).

[0100] [Table 3]

[0101] Figure 11 shows the adsorption kinetics of GO-based aerogels without and with compression. These two GO-based aerogels had similar maximum adsorption capacities. Compared with the uncompressed aerogel (Figure 11a), the adsorption kinetics of the GO-based aerogel compressed at 0.07 bar decreased; however, it was still able to reach 50% of the adsorption capacity within 300 min (Figure 11b).

[0102] Concentration of GO solution The concentration of GO solution used for aerogel preparation can affect the mixing efficiency with the crosslinker and the adsorption capacity of the resulting aerogel. The weight ratio of GO to crosslinker could be adjusted depending on the concentration of the GO solution used. A GO solution with a concentration of 1.5 wt% was investigated. Compared to aerogels formed from a GO solution with a concentration of 1 wt%, the adsorption capacity of GO and Ca was significantly higher. 2+ A weight ratio of 2:1 resulted in aerogels with comparable adsorption capacity of 154% as shown in Table 4. The lateral dimensions of GO solutions with different concentrations were <500 nm and the adsorption tests were carried out at RH 100%.

[0103] [Table 4]

[0104] Figure 12 shows the cross-linking effect of different concentrations of the initial GO solution and the cross-linking agent Ca 2+ Figure 12(a-b) shows the adsorption kinetics of GO-based aerogels with different concentrations of initial GO solution but the same weight ratio of crosslinker. Aerogels with higher concentrations of GO showed faster adsorption kinetics and adsorption capacity, probably due to increased adsorption sites in the aerogel. Within 60 min, 1 wt% of Ca was adsorbed onto the aerogels with an initial concentration of 1 wt%. 2+The aerogel with a 1:1 weight ratio of GO and GO had an adsorption capacity of 52%, while the aerogel with an initial concentration of 1.5 wt% had a capacity of 67%. Figure 12(c) shows that by adjusting the weight ratio of the crosslinker, the adsorption rate and capacity of the different GO-based aerogels can be tuned to achieve similar performance (see Figure 12(a)). The GO-based aerogel used in Figure 12(c) was used in the following studies to allow comparison of the results.

[0105] Effect of relative humidity on the volume of aerogel The adsorption capacity of the optimized GO-based aerogel was measured under different relative humidity (RH). Table 5 shows that the adsorption capacity decreased from 154% to 31% as the RH decreased from 100% to 50%. The lateral dimensions of the GO used here were <500 nm.

[0106] [Table 5]

[0107] Figure 13 shows the relationship between time and the adsorption capacity of the GO-based aerogel under different RH. Under high humidity, the adsorption capacity showed a continuous and rapid increase. Under low humidity, the GO-based aerogel had a lower adsorption capacity. However, it still adsorbed quickly at the beginning and reached its maximum adsorption capacity under low RH. Comparing the adsorption performance of the aerogel under different RH (Figure 13(a-d)), the adsorption rate did not decrease significantly within 20 min from the start of each experiment.

[0108] Interactive effects of relative humidity and compression on the volume of aerogels The adsorption capacity of GO-based aerogels decreased as the relative humidity decreased. However, as shown in Figure 14, the adsorption capacity of GO aerogels was significantly higher than that of silica gel even when the volume was reduced by 50%. However, as shown in Figure 15, the capacity significantly decreased when the volume was reduced by 75%. The decrease in the adsorption capacity of the aerogels may be due to the high pressure, which the inventors hypothesize may have damaged the porous microstructure of the GO-based aerogels.

[0109] The detailed results of the adsorption capacity of GO-based aerogels under different compression and RH are shown in Table 6. The density of the aerogels was calculated to understand the effect of compression and RH on the adsorption properties of the aerogels.

[0110] [Table 6]

[0111] Optimized adsorption capacity of eGO-based aerogels Stable eGO-based aerogels with excellent adsorption capacity were synthesized from eGO produced by electrochemical method. The maximum adsorption capacity was 310% at 100% relative humidity. Table 7 shows that the adsorption capacity of eGO aerogels did not change significantly after four cycles. The difference in adsorption capacity was mainly due to the initial weight of the aerogel, which can be greatly affected by the drying process. This was caused by the fact that the adsorption rate decreased slightly after the first adsorption measurement. Figure 16 shows that the adsorption rate decreased slightly after the first adsorption measurement. In the first cycle, the adsorption capacity reached 100% within 60 min. Thereafter, the adsorption rate of the eGO-based aerogel remained relatively stable and reached 100% adsorption capacity within about 90 min.

[0112] [Table 7]

[0113] Desorption processes for water recycling After the adsorption capacity test, the GO-based aerogel was saturated with water molecules. Then, the desorption test was performed to release the water from the GO-based aerogel. The process included an evaporation step. A schematic diagram of the experimental setup is shown in Figure 17. The saturated GO-based aerogel 1770 was sealed in a clean container with a conical top 1710. Ice was placed on the top so that condensation 1780 could form as the water was released from the aerogel. The container was covered with a heat mat 1720 and heated by a heater 1730. A temperature controller 1740 and a probe 1750 were used to precisely monitor and provide heat for evaporation. Under the heating conditions, the water was evaporated and condensed at the conical top, which was then collected in the container 1760. After collecting the condensed water, the quality of the desorbed water was measured by inductively coupled plasma mass spectrometry (ICP-MS).

[0114] Setup for the desorption process Figure 18 shows the experimental setup for the lab-scale desorption process. The temperature of the heat mat was controlled at 50 °C by a temperature controller 1820 to prevent the GO-based aerogel from being reduced under high temperature. A balance 1810 was used to monitor the weight of water collected from the GO-based aerogel 1830. The efficiency of the desorption process was highly dependent on the temperature. Figure 19(a) shows that during the heating process, moisture was released from the aerogel 1910 and then condensed on the cooled top 1920 (Figure 19b). In this experiment, 1.4 g of water was collected out of 2.7 g of adsorbed water from the GO-based aerogel at 50 °C.

[0115] Reclaimed water quality The quality of the reclaimed water from GO-based aerogel was measured by ICP-MS. The characterization of water quality is very sensitive, so minor contaminations may cause unreliable results. Especially for the water from the desorption process, many steps are involved from the preparation of the aerogel to the final desorption test. Combining these steps can increase the possibility of contamination of the desorbed water. Table 8 shows the analysis results of the reclaimed water from the desorption process. The measurements of the reclaimed water were performed twice. The results show that there was a large amount of contamination in the recycled sample water-01, which was believed by the inventors to be due to improper cleaning of the container used in the desorption process. After proper cleaning of the container (sample water-02), the contaminants were significantly reduced, especially Ca, K, Zn and I. The concentrations of some common elements such as Mg and Na in the reclaimed water-02 were still higher than tap water, but were significantly reduced compared to the concentrations in the reclaimed water-01. This indicates that the contaminants can be effectively reduced by proper cleaning of the components used in the process. However, it was thought that the main issue causing the contamination could be the use of an oil pump for the freeze-drying step used in the preparation of the aerogel. We hypothesize that the oil vapors could be a source of contaminants, since the concentrations of some elements that were not used in the production of GO-based aerogels were abnormally high, as shown in Table 8 (highlighted in light gray). This problem could be solved by changing the pump system to an oil-free pump system, etc.

[0116] [Table 8-1]

[0117] [Table 8-2]

[0118] [Table 8-3]

[0119] Prototype of atmospheric water generator A prototype atmospheric water generator was constructed using aerogel. Figure 20 shows the components of the prototype and a mold for a GO-based aerogel that fits the prototype. The GO-based aerogel 2060 can be enclosed in a canister with an inlet and an outlet for moisture.

[0120] The prototype of the atmospheric water generating device includes a canister as shown in FIG. 20. The canister is divided into four parts: an outer shell 2040, a lid 2030, an insulating layer 2010, and a core layer 2050. The insulating layer 2010 is made of glass fiber and aluminum foil. The insulating layer is effective when the temperature is below 80° C. The core layer 2050 includes a heat mat, a temperature sensor, and a stainless steel mesh bag. The aerogel 2060 molded using a mold 2060 is first cut into small pieces and placed into a stainless steel mesh bag.

[0121] In certain embodiments, the canister described above may be connected to an inlet valve, an outlet valve, and a collection valve. When used in the "adsorption configuration," the collection valve is closed and the inlet and outlet valves are opened so that moisture-containing gas is sent into the canister through the inlet valve and exposed to the aerogel before being discharged from the canister as dry gas through the outlet valve. After a period of time during which the aerogel adsorbs a certain amount of water from the gas, the inlet and outlet valves are closed and the collection valve is opened in the "collection configuration," where a heat mat is used to heat the aerogel and drain the water through the collection valve into a water collection container. Once all the water has been drained, the collection valve is closed and the inlet and outlet valves are opened so that the system returns to the "adsorption configuration," thereby allowing more water to be adsorbed into the aerogel. This process may be repeated multiple times to increase the amount of water collected by the atmospheric water generator.

[0122] The assembly and disassembly procedures for the prototype are shown below. Assembly Instructions 1. The insulation layer 2010 is carefully and slowly pressed back onto the outer shell 2040. The layer is held in place with even pressure. 2. The heat mat and temperature sensor cables pass through the insulation layer 2010 and the outer shell 2040. 3. The core layer 2050 is pressed back into the outer shell 2040. The aluminum tube and mesh bag should be pressed carefully and slowly at the same time. The force on the stainless steel mesh bag should be uniform. 4. The nut 2020 on the bottom of the core layer 2050 is assembled to pull the core layer further down into the shell. The shell lid 2030 is assembled. Disassembly Procedure 1. Remove the shell lid 2030. Remove the nut at the bottom of the core layer. 2. The aluminum tube 2080 in the center of the core layer is carefully pushed out. At the same time, the stainless steel mesh bag is pulled out with needle-nose pliers. 3. The heat mat and temperature sensor cables are removed. 4. The insulation layer can be quickly and easily pulled off using needle-nose pliers.

[0123] 3D printed mold module for GO-based aerogel preparation The mold module for the preparation of GO-based aerogels allows the production of aerogels for incorporation into canisters. The shape of the aerogel module depends heavily on the internal structure of the canister. Figure 21 shows the module designed for GO aerogels for insertion into the canister as shown in Figure 20.

[0124] Preparation of graphene oxide aerogel Graphene oxide aerogels were produced by mixing GO with ionic crosslinkers in different weight ratios. 2+The detailed procedure for fabricating aerogels in is as follows. First, a stock solution of cationic crosslinker (calcium chloride, CaCl2) was prepared by dissolving 20 g of CaCl2 in 100 mL of ultrapure water at a concentration of 0.2 g / mL. Then, 7.5 mL (1.5 g) of CaCl2 was added to 100 mL of GO suspension (1.5 g, 1.5 wt%) and then mixed well for 15–20 min in a portable mixer. Subsequently, the resulting mixture was added to an appropriate Petri dish / metal tray for subsequent freeze-drying. All adsorption experiments of GO aerogels were performed in a glove bag with controlled relative humidity (RH). Figure 22 shows the stepwise preparation of GO aerogels. The mass of the small-scale aerogels was approximately 1–2 g.

[0125] Effect of GO flake size on the adsorption performance of aerogels The flake size of graphene oxide can affect the adsorption performance of aerogels by changing the porosity. Therefore, water absorption studies were carried out by using aerogel samples prepared by GO with different lateral dimensions of about 300 nm, about 1 μm, and about 5 μm. The aerogels were prepared by mixing Ca 2+ The aerogels were prepared by using a crosslinker with GO. The adsorption experiments were carried out in a glove bag with humidity controlled at 80-90%. According to the results shown in Figure 23, the adsorption capacity increased as the GO flake size decreased due to the higher porous structure of the aerogels.

[0126] Effect of mixture of GO flake sizes on the adsorption performance of aerogels GO aerogels with a flake size of approximately 5 μm (1:1 weight ratio with Ca 2+Aerogels with GO flakes (prepared by crosslinking with GO) showed an adsorption performance of about 73% within 6 hours under 80% humidity. This adsorption rate may be lower than that of the aerogels with smaller GO counterparts due to the less porous structure caused by the larger flakes. With this in mind, a series of experiments was conducted to better understand the effect of flake size on the performance of the aerogels. This was done by incorporating the above GO flakes with smaller stacks of about 300 nm in increasing ratios, namely, 100:0, 75:25, 50:50 and 25:75. As shown in Figure 24, significant changes were observed and aerogels with equal ratios of the two different flake sizes gave the best performance of about 100%.

[0127] Adsorption performance of aerogel at different humidity Considering the application of GO aerogels in water generation in different humid environments, a series of experiments on water absorption at various humidities were conducted. Two separate experiments were conducted on the aerogels using GO stacks with two different sizes, approximately 300 nm and approximately 1 μm, respectively.

[0128] Aerogels prepared by using small GO stacks (~300 nm) Adsorption tests using smaller stacks of about 300 nm were carried out under different humidity levels of 90%, 75%, 60% and 50%. All aerogel samples showed a high solubility in Ca 2+ The aerogels were prepared by using a crosslinker (1:1 weight ratio). It was observed that the relative humidity can play an important role in the adsorption performance of the aerogels. The adsorption capacity reached 125% at 9% humidity but decreased at lower relative humidity (Figure 25). A favorable performance of over 35% was still achieved even under 50% wet conditions.

[0129] Aerogels prepared by using larger GO stacks (~1 μm) The same experiment was performed with Ca 2+The experiment was repeated by using a different batch of GO aerogels, which was also prepared by crosslinking 1:1 GO with 1:1 weight ratio. The experiment was carried out at relative humidity ranging from 90%, 75%, 60%, 50%, 40%, and 30% for 5 hours. Similar to the previous experiment, a relatively high adsorption capacity of more than 35% was obtained at 50% humidity. It was also found that within 3 hours, an adsorption capacity of about 15% was obtained at 30% relative humidity as shown in Figure 26. Figure 27 shows a better visualization of the relationship between relative humidity and adsorption performance of the exemplary GO aerogels.

[0130] Adsorption performance of aerogels prepared by using different cationic crosslinkers A series of aerogel samples were prepared using Ca 2+ , K + , Mg 2+ and Al 3+ The weight ratio of GO to crosslinker was kept at 2:1, and the humidity ranged from 75 to 90%. 2+ The maximum adsorption capacity was achieved by using a crosslinker of about 124%, followed by Al 3+ It was observed that approximately 107.9% was achieved by using another crosslinker, Mg 2+ and K + provided approximately 42% and 30% of the maximum capacity, respectively. As mentioned above, the adsorption experiments were carried out in a glove bag with controlled relative humidity.

[0131] In addition, Li + and Fe 3+ Cations such as Ca were also considered for comparison with calcium crosslinkers. Here, the experimental setup involved preparing aerogels with a 1:1 weight ratio of GO and crosslinker (calcium chloride, lithium chloride or iron(III) chloride), and the adsorption tests were carried out at a relative humidity of about 85–95%. As in the previous experiments, Ca 2+ The aerogel prepared by using Li + and Fe 3+Aerogels prepared by using 1,2-dichlorophenyl 2,3-dichlorophenyl 1,3-dichlorophenyl 2,4-dichlorophenyl 1,5 ...

[0132] Adsorption performance of aerogels with different shapes The water absorption of GO aerogels in cake, flake (diameter about 2 cm), and powder form was measured. 2+ Three aerogel samples were prepared using crosslinker (1:1 weight ratio) and then freeze-dried. Aerogel in flake form was produced by cutting the freshly prepared aerogel with scissors. After cutting, aerogel flakes with diameter of about 2 cm were obtained (Figure 30). Aerogel in powder form was then produced by grinding one aerogel cake using a Breville coffee and spice grinder. Subsequently, water absorption studies of the three aerogel samples were carried out at 90% humidity. As shown in Figure 31, maximum adsorption capacity of up to about 127% was obtained by the aerogel cake, while about 111% and about 98% were achieved by the aerogel in powder and flake form, respectively.

[0133] Adsorption performance of eGO aerogel Adsorption performance of eGO at different humidity The eGO aerogel samples were prepared using Ca 2+ Crosslinker was 1:1 eGO:Ca 2+ The performance tests were then carried out in a glove bag at different humidities, 100%, 80-85%, and 75-80%, for 6 hours. The same trends as for standard GO were observed. That is, the humidity decreased from about 190% to about 150% and about 90% under the lower humidity conditions, as shown in FIG.

[0134] Performance of eGO during multiple cycles of adsorption Since reusability is an important property, the adsorption of eGO aerogel was carried out over multiple cycles. First, GO was adsorbed with Ca in a 1:1 weight ratio. 2+Samples were prepared by cross-linking with eGO and eight cycles of adsorption were performed for 5-6 h at 100% humidity. The water adsorption capacity of the aerogel at each cycle is shown in Figure 33, showing a slight decrease in water absorption after each cycle. However, the aerogel maintained desirable performance with over 120% maximum capacity even after eight cycles, indicating the potential of eGO aerogel as a carbon-based desiccant for industrial applications.

[0135] Adsorption performance of Armidale eGO eGO:Ca in a 1:1 weight ratio 2+ The adsorption performance of eGO aerogels (from Armidale) crosslinked with SiO was measured at 85–95% humidity. As shown in Figure 34, the adsorption rate reached 122% within 5 h and was observed to be similar to the other eGO samples.

[0136] Adsorption performance of eGO-UNE Ca in a 1:1 weight ratio 2+ Two eGO aerogel samples prepared by crosslinking with 1,2-dichlorophenyl ether were tested. The water absorption study was carried out in a glove bag with humidity controlled at 90-95%. As shown in Figure 35, the maximum capacity of sample 1 and sample 2 was about 177% and 125%, respectively.

[0137] Adsorption performance of GO aerogel on a large scale The performance of the large-scale produced GO aerogel was determined. The sample was prepared as follows: 40 g of GO was added to Ca in a 1:1 weight ratio. 2+ The suspension was stirred for 15-20 min, then divided into four metal trays (19 cm × 35 cm × 3 cm) and frozen in a -80 °C freezer (Figure 36). The frozen samples were then freeze-dried at Scitek. Figure 36 shows the preparation and freezing conditions of a large-scale GO suspension.

[0138] Three 40 g aerogel samples were prepared and are referred to as the first, second, and third batch aerogels, respectively. The first batch aerogel of about 11 g was subjected to water absorption study in a humidity chamber with a relative humidity of about 90%. It was observed that more than 300% water absorption was obtained within 4 hours, as shown in Figure 37a. The other two aerogels were tested in a glove bag with controlled humidity (85-95%). Before performance testing, the samples were thoroughly dried under nitrogen. A maximum capacity of about 160% was obtained for the second batch aerogel of about 8.22 g (Figure 37b). For the third batch aerogel (about 10.12 g), an adsorption capacity of about 130% was obtained (Figure 37c), similar to the second batch sample. It should be noted that the water absorption may vary depending on the environment set.

[0139] Next, the performance on a large scale was compared with that of a smaller one. A small piece of aerogel (about 0.4 g) was taken from a sample of the second batch and dried overnight under nitrogen before testing. The experimental conditions were set the same with humidity of 85-95% in a glove bag. Within 17 hours, an adsorption rate of 140% was reached, consistent with the results obtained with the second batch of aerogel on a large scale (Figure 38).

[0140] Adsorption performance of GO aerogel in GO suspensions with different concentrations A series of experiments was carried out using GO suspensions with concentrations of 1 wt% and 1.5 wt%. The aerogel samples were prepared by dissolving GO in calcium chloride (Ca 2+ ) crosslinking with a crosslinking agent.

[0141] 1 wt% GO suspension Changes in the weight ratio of GO to crosslinker Aerogels were prepared using GO suspensions with a concentration of 1 wt%. First, the aerogels were prepared using suspensions with different weight ratios (GO:Ca 2+ ), GO with Ca at 100:1, 50:1, 10:1, 1:5, and 1:1, respectively. 2+The aerogels were crosslinked with GO. The experiments were carried out in a glove bag at 95–100% relative humidity. It was found that the maximum adsorption capacity reached about 260% when the ratio of GO to crosslinker was equal. Figure 39 shows the adsorption performance of the aerogels by changing the weight ratio of GO to metal ions. As shown in Figure 39b, the capacity increases as the content of metal ions increases to reach the same mass ratio as GO.

[0142] Change in thickness of aerogel due to compression The adsorption properties of GO aerogels with different thicknesses were also tested. First, 1 wt% GO was mixed with Ca in a 1:1 weight ratio. 2+ The aerogels were cross-linked with 0.02% NaOH and then freeze-dried to form aerogels. The thickness of the aerogels was then adjusted by compressing them at different pressures of about 0.07 bar, about 1.5 bar, and about 10 bar using a 3D-printed canister, as shown in Figure 40d. The adsorption performance was then performed at 95-100% relative humidity. As shown in Figures 40a-c, the adsorption performance of the aerogels decreased from about 165% to about 79% and about 29% when compressed under high pressure.

[0143] 1.5 wt% GO suspension The role of ultrasonic treatment on the performance of aerogels During sample preparation, i.e., GO was dissolved in Ca 2+ The effect of ultrasonic treatment during crosslinking was investigated. The two aerogel samples were mixed in a 2:1 weight ratio (GO:Ca 2+ ) and individually cross-linked with calcium chloride. One sample was then sonicated for 10 min, after which both suspensions were freeze-dried to form aerogels. As shown in Figure 41, no significant differences were observed between the aerogel samples prepared with and without sonication. The experiments were carried out in a glove bag with a relative humidity of 95–100%.

[0144] Adsorption performance at different humidity levels GO (1.5 wt%) in a 2:1 weight ratio with Ca 2+Aerogels were prepared by cross-linking with metal ions, and the adsorption performance of the aerogels was carried out at different humidities, 95-100%, 80%, 70%, and 50%, respectively. As shown in Figure 42, about 154% water absorption was obtained at 100% humidity, which decreased to about 56%, about 40%, and 30% when the relative humidity was decreased to 80%, 70%, and 50%, respectively.

[0145] Isotherm Test A number of aerogel samples in cake form were tested for their isothermal adsorption-desorption behavior.

[0146] Desorption under different conditions of atmospheric pressure and vacuum Ca in a 1:1 weight ratio 2+ About 2.7 g of GO aerogel was prepared by crosslinking with . The adsorption test was carried out at RH 85% for 42 h, followed by desorption under two different conditions: atmospheric pressure and vacuum. Figure 43 shows the first cycle of the adsorption-desorption process (desorption under atmospheric pressure), and the area highlighted in grey indicates the second cycle (desorption under vacuum). Although the adsorption was about 60% within the set time frame, the aerogel still showed good adsorption performance in the second cycle of the process. With regard to desorption, a gradual water release was observed under atmospheric pressure, while a significant enhancement was obtained under vacuum conditions.

[0147] Adsorption at 85°C and desorption in dry air at 30°C Another series of isotherm experiments using a second batch of 40 g aerogel samples were performed. Approximately 8.57 g of aerogel was thoroughly dried under nitrogen prior to the adsorption test at 85% humidity. As shown in Figure 44, the water absorption of the aerogel reached 100% within 2.5 hours. Desorption tests were then carried out under dry air at 30°C. The desorption spectrum shown in Figure 44 indicates complete water recovery from the aerogel under ambient conditions.

[0148] Adsorption at 85°C and desorption in dry air at 40°C The desorption performance at another mild temperature (40°C) was also investigated. The experimental conditions for the adsorption test were as follows: Approximately 3.73 g of aerogel was incubated at the same humidity (85%), and then desorption was carried out under dry air at 40°C. According to the isothermal curve shown in Figure 45, approximately 110% water absorption was achieved within 5 hours, and successful desorption was also observed.

[0149] Adsorption at 55% and desorption in dry air at 40°C After examining the desorption efficiency of the aerogel at low temperatures, another isotherm was carried out under mild conditions for both adsorption and desorption tests. In the experiment, Ca 2+ Approximately 2.91 g of aerogel prepared by crosslinking with GO was incubated at 55% humidity for 6 h and absorbed approximately 75% water. Desorption tests were then carried out under dry air at 40 °C. Figure 46 shows the isothermal curves indicating the desirable performance of GO aerogel under ambient conditions.

[0150] Although the aerogels described herein have been shown to adsorb water, one of ordinary skill in the art will appreciate that the aerogels may also be suitable for adsorption of other small molecules, such as organic solvents, such as methanol, ethanol, etc., and gases, such as carbon dioxide, nitrogen, sulfur dioxide, etc.

[0151] Although the present invention has been described with reference to specific embodiments, those skilled in the art will appreciate that the present invention may be embodied in many other forms. In particular, features of any one of the various described embodiments may be provided in any combination in any of the other described embodiments. Various modifications and alterations to the present invention will be apparent to those skilled in the art without departing from the scope and spirit of the present invention. It should be understood that the present invention is not intended to be unduly limited by the exemplary embodiments and examples set forth herein, and that such examples and embodiments are presented solely for illustrative purposes with respect to the scope of the present invention, which is intended to be limited only by the claims set forth herein below.

Claims

1. The graphene oxide is cross-linked with metal ions, the metal ions being selected from the group consisting of alkali metal ions, alkaline earth metal ions, transition metal ions and basic metal ions, and Fe 3+ , Co 2+ , Ni 2+ , Cu 2+ , Zr 4+ , Sn 4+ , Ti 4+ , V 5+ , La 3+ , Cr 3+ , Al 3+ , Zn 2+ and Ce 4+ An aerogel which is not selected from the group consisting of:

2. 10. The aerogel of claim 1, wherein the metal ions are selected from the group consisting of alkali metal ions and alkaline earth metal ions.

3. 3. The aerogel of claim 1, wherein the metal ions are selected from the group consisting of beryllium, magnesium, calcium, strontium, lithium and barium ions.

4. The metal ion is Be 2+ , Mg 2+ , Ca 2+ , Sr 2+ , Li + and Ba 2+ The aerogel according to any one of claims 1 to 3, selected from the group consisting of:

5. The aerogel according to any one of claims 1 to 4, wherein the metal ions are alkaline earth metal ions.

6. The alkaline earth metal ion is Ca 2+ 6. The aerogel of claim 5,

7. 2. The aerogel of claim 1, wherein the metal ions are basic metal ions or transition metal ions.

8. 8. The aerogel of claim 1, wherein a weight ratio of graphene oxide to metal ions is from about 200:1 to about 1:

5.

9. 9. The aerogel of claim 1, wherein a weight ratio of graphene oxide to metal ions is from about 5:1 to about 1:

1.

10. 10. The aerogel of claim 1, wherein the graphene oxide has an average lateral dimension of about 500 nm or less.

11. 11. The aerogel of any one of claims 1 to 10, wherein the graphene oxide has an average lateral dimension of about 500 nm or more.

12. 12. The aerogel of any one of claims 1 to 11, wherein the graphene oxide has a carbon:oxygen ratio of about 0.5 to about 5.

13. 13. The aerogel of claim 12, wherein the graphene oxide has a carbon:oxygen ratio of about 2.

25.

14. 14. The aerogel of any one of claims 1 to 13, wherein the aerogel has an adsorption capacity of about 20% to about 400% at about 100% relative humidity.

15. The density of the aerogel is about 0.005 g / cm 3 ~Approx. 0.25g / cm 3 The aerogel according to any one of claims 1 to 14,

16. 16. The aerogel of any one of claims 1 to 15, wherein the aerogel has a porosity of about 90% to about 99.9%.

17. 17. The aerogel of any one of claims 1 to 16, wherein the aerogel has an adsorption capacity of at least about 40% at about 100% relative humidity.

18. A method for producing an aerogel comprising graphene oxide cross-linked with metal ions, the metal ions being selected from the group consisting of alkali metal ions, alkaline earth metal ions, transition metal ions and basic metal ions, and further comprising: 3+ , Co 2+ , Ni 2+ , Cu 2+ , Zr 4+ , Sn 4+ , Ti 4+ , V 5+ , La 3+ , Cr 3+ , Al 3+ , Zn 2+ and Ce 4+ and wherein the method is not selected from the group consisting of (a) contacting graphene oxide with a cross-linking agent in the presence of a liquid; (b) removing the liquid to form the aerogel.

19. 20. The method of claim 18, wherein the removal of liquid is accomplished by freeze-drying.

20. 20. The method of claim 19, wherein the graphene oxide is transferred to a mold after the contacting step and before the freeze-drying step.

21. The method according to claim 19 or 20, wherein the freeze-drying step is carried out at a temperature of -60°C for 2 to 24 hours.

22. The method of any one of claims 18 to 21, wherein the liquid comprises water.

23. 23. The method of any one of claims 18 to 22, wherein the method comprises preparing cross-linked graphene oxide by providing an aqueous solution of graphene oxide at a predetermined concentration, followed by exposure to a cross-linking agent.

24. 24. The method of claim 23, wherein the cross-linking agent is added to the aqueous solution of graphene for a period of from 10 minutes to 6 hours.

25. 25. The method of claim 23 or 24, wherein the concentration of graphene oxide in the aqueous solution is from about 0.01% to about 20% by weight.

26. 26. The method of claim 25, wherein the concentration of graphene oxide in the aqueous solution is from about 0.05% to about 5% by weight.

27. 27. The method of claim 26, wherein the concentration of graphene oxide in the aqueous solution is about 1 wt%.

28. The method of any one of claims 18 to 27, wherein the cross-linking agent comprises the metal ion.

29. The method according to any one of claims 18 to 28, wherein the metal ions are selected from the group consisting of alkali metal ions and alkaline earth metal ions.

30. 30. The method of claim 29, wherein the alkaline earth metal ions and / or alkali metal ions are selected from the group consisting of beryllium, magnesium, calcium, strontium, lithium and barium.

31. The cross-linking agent is CaCl 2 and MgCl 2 The compound according to claim 18 to 3 is selected from the group consisting of 10. The method according to any one of claims 0 to 9.

32. The method according to any one of claims 18 to 28, wherein the metal ion is a basic metal ion or a transition metal ion.

33. The method of any one of claims 18 to 32, wherein after the removing step, the aerogel is compressed.

34. 34. The method of claim 33, wherein the aerogel is compressed to about 50% of its original volume.

35. Graphene oxide aerogel produced by the method according to any one of claims 18 to 34.

36. 1. A method for adsorbing moisture from a gas stream or atmosphere containing moisture, comprising the step of adsorbing the moisture from the gas stream or atmosphere by contacting the gas stream or atmosphere with a graphene oxide aerogel.

37. Use of graphene oxide aerogel to adsorb moisture from gas streams.

38. 1. A method for desorbing water adsorbed in a graphene oxide aerogel, comprising: heating the graphene oxide aerogel sufficiently to release the adsorbed water and regenerate the graphene oxide aerogel.

39. 1. A method for recovering water from a graphene oxide aerogel having adsorbed water, comprising: heating the graphene oxide aerogel sufficiently to release the adsorbed water and recovering the water.

40. Atmospheric water generator with graphene oxide aerogel.

41. The method according to claim 36, 38 or 39, the use according to claim 37 or the atmospheric water generator according to claim 40, wherein the graphene oxide aerogel is an aerogel according to any one of claims 1 to 17 and 35.

Citation Information

Patent Citations

  • A hydrophilic and compressible aerogel as draw agent for purity water in forward osmosis

    US20190001271A1