Aluminum-containing nitride ceramic matrix composites, methods of making and using same
Patent Information
- Application Number
- JP2024520933
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-12
- Filing Date
- 2022-10-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024538022000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure generally relates to techniques for processing materials to produce polycrystalline ceramic composites, including aluminum-containing nitride matrix composites. More specifically, embodiments of the present disclosure include techniques for producing ceramic matrix composites incorporating one or more phosphor compositions in an aluminum-containing nitride matrix using a combination of processing techniques. Such ceramic matrix composites can be used in a variety of applications, including as phosphor components for powerful light sources such as laser diodes. [Background technology]
[0002] Solid-state lighting has grown significantly over the past two decades and is widely applied in many residential, commercial, and industrial environments. Typically, light from a blue and / or violet excitation source, for example emitted by a light-emitting diode (LED), is absorbed by one or more phosphor compositions, which then emit blue, green, yellow, and / or red light, resulting in an overall white light, where the color temperature and other properties, such as the color rendering index (CRI), can be controlled. Recently, laser diodes have been used as excitation sources, which offer the advantages of very high brightness and luminance, as well as very narrow beam angles, longer throwing distances, and higher contrast. However, to fully realize the benefits of laser-based lighting, phosphor compositions with very high thermal conductivity are required so that the heat generated by the light conversion process in the phosphor can be dissipated without degrading the performance of the phosphor or the package. In LEDs, the phosphor is typically dispersed in silicone, epoxy, or other polymer compositions, which have very low thermal conductivity. Although many groups have demonstrated phosphor-in-glass (PiG) compositions with good phosphor performance, the thermal conductivity of these compositions is still very low.
[0003] Ceramic phosphor compositions would, at least in principle, be ideal for laser-based lighting. Ideally, they would need to have high thermal conductivity and high internal and external quantum efficiency. However, currently only Ce-doped yttrium aluminum garnet (YAG) that emits yellow light is available. +3 ) is the only ceramic phosphor composition that is widely available commercially, and blue + YAG white light has a low CRI. Several groups have demonstrated other phosphor compositions in ceramic form, where sintering and densification have been achieved by conventional methods such as hot pressing, hot isostatic pressing, and spark plasma sintering. However, the high temperatures associated with these conventional ceramic processing methods often degrade the phosphor's performance. In addition, in many applications it is desirable to have multiple phosphor compositions in close proximity to one another, such as green and red phosphors, and co-sintering involves additional challenges beyond simple compositional sintering. Although the use of a matrix may be able to overcome some of the difficulties in co-sintering, the matrix materials demonstrated to date have important limitations with respect to the optical and thermal properties of the resulting ceramic matrix composite. Summary of the Invention [Problem to be solved by the invention]
[0004] Due to at least the above problems, there is a need for phosphor-containing ceramic matrix composites that have excellent phosphor performance and high thermal conductivity. [Means for solving the problem]
[0005] According to the present disclosure, further techniques are provided that relate to techniques for processing materials to produce aluminum-containing ceramic matrix composites. More specifically, embodiments of the present disclosure include:
[0006] An embodiment of the present disclosure may also provide a method of forming an aluminum-containing nitride ceramic matrix composite. The method may include forming at least one green body comprising a phosphor powder and an aluminum-containing composition, the at least one green body being characterized by a porosity between about 10% and about 80%; and heating a sealable container to a temperature between about 400°C and about 800°C and a pressure between about 10 MPa and about 1000 MPa. Prior to heating and pressurizing the sealable container, the at least one green body, ammonia, and a mineralizer composition are disposed in the sealable container. The phosphor powder comprises at least one phosphor composition, and the phosphor powder particles have a D50 diameter between about 100 nanometers and about 500 micrometers. The aluminum-containing composition has a purity between about 90% and about 99.9999%, based on the metal. Prior to heating and pressurizing the sealable container, a percentage of free volume in the sealable container filled with liquid ammonia is between about 10% and about 95%. The step of heating the sealable container includes heating the sealable container for a first period of time to form an aluminum-containing nitride ceramic matrix composite characterized by a phosphor to AlN volume ratio of between about 1% and about 99%, a porosity of between about 1% and about 50%, and a thermal conductivity of between about 1 W / (m·K) and about 320 W / (m·K).
[0007] The present disclosure may also provide an aluminum-containing composition. The aluminum-containing composition includes an aluminum-containing nitride matrix material and a plurality of secondary ceramic phase particles. The plurality of secondary ceramic phase particles are characterized by a particle size distribution having a D10 value between about 1 micrometer and about 10 micrometers and a D90 value between about 10 micrometers and about 100 micrometers. The aluminum-containing composition also includes at least 50% of the boundaries of the plurality of secondary ceramic phase particles bonded to the aluminum-containing matrix material; a ratio of the plurality of secondary ceramic phase particles to the aluminum-containing matrix material between about 1% and about 99%, and the aluminum-containing composition is characterized by a porosity between about 1% and about 50% and a thermal conductivity between about 1 W / (m·K) and about 320 W / (m·K). The plurality of secondary ceramic phase particles may also include at least one phosphor composition. The plurality of secondary ceramic phase particles may also include at least two phosphor compositions. In some embodiments, the aluminum-containing composition may also be characterized by a ratio of a plurality of secondary ceramic phase particles to aluminum-containing matrix material of between about 5% and about 95%, a porosity of between about 2% and about 50%, and a thermal conductivity of between about 5 W / (m·K) and about 260 W / (m·K). 12 :Ce 3+ , Lu3Al5O 12 :Ce 3+ , (Y,Gd,Tb,Sc,Lu,La)3(Al,Ga,In)5O 12 :Ce 3+ , β-SiAlON:Eu 2+ , α-SiAlON:Eu 2+ , and CaAlSiN3:Eu 2+ In some embodiments, secondary electron micrographs of polished portions of the aluminum-containing compositions reveal an absence of observable porosity within at least 50% of the boundaries between the plurality of secondary ceramic phase particles and the aluminum-containing matrix material.
[0008] A further understanding of the nature and advantages of the present disclosure may be realized by reference to the specification and the accompanying drawings.
[0009] So that the above-mentioned features of the present disclosure can be understood in detail, a more particular description of the present disclosure, briefly summarized above, can be had by reference to embodiments, some of which are illustrated in the accompanying drawings, in which it is noted, however, that the accompanying drawings depict only exemplary embodiments and therefore should not be considered limiting of its scope, other equally effective embodiments being permissible. [Brief description of the drawings]
[0010] [Figure 1A] FIG. 1 is a simplified schematic illustrating a plurality of phosphor particles having a coating according to one embodiment of the present disclosure. [Figure 1B] FIG. 1 is a simplified diagram showing a mixture of phosphor particles and aluminum-containing particles. [Figure 2A] FIG. 1 is a simplified diagram illustrating a process flow for tape casting a slurry composition according to one embodiment of the present disclosure. [Figure 2B] FIG. 1 is a simplified diagram illustrating a process flow for tape casting a slurry composition using a doctor blade and a stencil mask according to one embodiment of the present disclosure. [Figure 2C] FIG. 2B is a top view of the doctor blade and stencil mask portions of the tape casting device shown in FIG. 2A according to one embodiment of the present disclosure. [Figure 3A] FIG. 1 is a simplified diagram illustrating a method of forming a permeated composite material composition according to one embodiment of the present disclosure. [Figure 3B] FIG. 1 is a simplified diagram illustrating a method of forming a permeated composite material composition according to one embodiment of the present disclosure. [Figure 4A] 1 is a simplified diagram illustrating an alternative method of forming a permeated composite material composition, according to one embodiment of the present disclosure; [Figure 4B] 1 is a simplified diagram illustrating an alternative method of forming a permeated composite material composition, according to one embodiment of the present disclosure; [Figure 5A] FIG. 1 is a simplified diagram illustrating a process flow for forming a green body by tableting according to one embodiment of the present disclosure. [Figure 5B] FIG. 1 is a simplified diagram illustrating a process flow for forming a mixed dry powder composition from a slurry using a spray dryer, according to one embodiment of the present disclosure. [Figure 5C] FIG. 1 is a simplified diagram of a conveyor system used to form tablets according to one embodiment of the present disclosure. [Figure 6] FIG. 1 is a simplified diagram showing a cross-sectional view of a sealable container containing granules, pellets, tablets, or other green body forms according to one embodiment of the present disclosure. [Figure 7] FIG. 1 is a schematic diagram illustrating a pressure vessel apparatus according to one embodiment of the present disclosure. [Figure 8] FIG. 1 is a schematic diagram illustrating an internally heated pressure vessel, apparatus, according to one embodiment of the present disclosure. [Figure 9] FIG. 1 is a schematic diagram illustrating a mineralizer vessel and method of use according to one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] To facilitate understanding, wherever possible, identical reference numbers are used to designate identical elements common to the figures. It is contemplated that elements and features of one implementation may be beneficially incorporated in other implementations without further recitation.
[0012] According to the present disclosure, techniques are provided relating to material processing techniques for producing aluminum-containing nitride ceramic matrix composites that combine the functionality of incorporated particles, such as phosphor particles, with translucent optical properties and high thermal conductivity.
[0013] 1A and 1B are schematic cross-sectional views illustrating process steps within a method for manufacturing an aluminum-containing nitride ceramic matrix composite that overcomes the limitations discussed above. Referring to FIGs. 1A and 1B, a plurality of phosphor particles 101 are provided. In certain embodiments, the phosphor particles 101 are selected from one or more compositions having emission wavelengths in the blue region (430-490 nm), green region (490-560 nm), yellow region (560-600 nm), or red region (600-750 nm).
[0014] In a particular embodiment, the phosphor particles 101 are YAlO 12 :Ce 3+ , Lu3Al5O 12 :Ce 3+ , (Y,Gd,Tb,Sc,Lu,La)3(Al,Ga,In)5O 12 :Ce 3+ , β-SiAlON:Eu 2+ , α-c:Eu 2+ , SrSi2O2N2:Eu 2+ , SrGa2S4:Eu 2+ , SrS:Eu 2+ , and CaAlSiN3:Eu 2+ The composition may include one or more material compositions.
[0015] In one particular embodiment, the plurality of phosphor particles 101 can include a phosphor capable of emitting substantially red light. Such a phosphor can be selected from a material composition that can include one or more of the following: CaAlSiN3:Eu 2+ , (Gd,Y,Lu,La)2O3:Eu 3+ , Bi 3+ ;(Gd,Y,Lu,La)2O2S:Eu 3+ , Bi 3+ ;(Gd,Y,Lu,La)VO4:Eu 3+ , Bi 3+ ;Y2(O,S)3:Eu 3+ ;Ca 1-x Mo 1-y S yO4 (wherein 0.05≦x≦0.5, 0≦y≦0.1); (Li,Na,K)5Eu(W,Mo)O4; (Ca,Sr)S:Eu 2+ ;SrY2S4:Eu 2+ ;CaLa2S4:Ce 3+ ;(Ca,Sr)S:Eu 2+ ;3.5MgO*0.5MgF2*GeO2:Mn 4+ (MFG); (Ba, Sr, Ca)Mg x P2O7:Eu 2+ , Mn 2+ ;(Y,Lu)2WO6:Eu 3+ , Mo 6+ ;(Ba,Sr,Ca)3Mg x Si2O8:Eu 2+ , Mn 2+ (In the formula, 1 <x≦2である);(RE 1-y Ce y )Mg 2-x Li x S 3-x PxO 12 (Wherein, RE is at least one of Sc, Lu, Gd, Y, and Tb, and is 0.0001 <x<0.1、かつ0.001<y<0.1である);(Y、Gd、Lu、La) 2-x EU x W 1-y Mo y O6 (wherein 0.5≦x≦1.0, 0.01≦y≦1.0); (SrCa) 1-x EU x Si5N8 (wherein 0.01≦x≦0.3); SrZnO2: Sm +3 ;M m O n X, where M is selected from the group of Sc, Y, lanthanides, alkaline earth metals, and mixtures thereof; X is a halogen; 1≦m≦3; and 1≦n≦4, and the doping level of the lanthanides can range from 0.1 to 40% of the spectral weight; and Eu 3+ Activated phosphate or borate phosphors; and mixtures thereof.
[0016] In one particular embodiment, the phosphor particles 101 are α-SiAlON:Eu 2+, (Ba,Sr,Ca)5(PO4)3(Cl,F,Br,OH):Eu 2+ , Mn 2+ ;Sb 3+ ,(Ba,Sr,Ca)MgAl 10 O 17 :EU 2+ , Mn 2+ ;(Ba,Sr,Ca)BPO5:Eu 2+ , Mn 2+ ;(Sr,Ca) 10 (PO4)6*nB2O3:Eu 2+ ;2SrO*0.84P2O5*0.16B2O3:Eu 2+ ;Sr2Si3O8*2SrCl2:Eu 2+ ;(Ba,Sr,Ca)Mg x P2O7:Eu 2+ , Mn 2+ ;Sr4Al 14 O 25 :EU 2+ (SAE);BaAlO 13 :EU 2+ and blue phosphor compositions comprising one or more of the above mixtures.
[0017] In one particular embodiment, the phosphor particles 101 are β-SiAlON:Eu 2+ , (Ba,Sr,Ca)MgAl 10 O 17 :EU 2+ , Mn 2+ (BAMn);(Ba,Sr,Ca)Al2O4:Eu 2+ ;(Y,Gd,Lu,Sc,La)BO3:Ce 3+ ,Tb 3+ ;Ca8Mg(SiO4)4Cl2:Eu 2+ , Mn 2+ ;(Ba,Sr,Ca)2SiO4:Eu 2+ ;(Ba,Sr,Ca)2(Mg,Zn)Si2O7:Eu 2+ ;(Sr,Ca,Ba)(Al,Ga,In)2S4:Eu 2+ ;(Y,Gd,Tb,La,Sm,Pr,Lu)3(Al,Ga)5O 12 :Ce 3+;(Ca,Sr)8(Mg,Zn)(SiO4)4Cl2:Eu 2+ , Mn 2+ (CASI);Na2Gd2B2O7:Ce 3+ , Tb 3+ ;(Ba,Sr)2(Ca,Mg,Zn)B2O6:K,Ce,Tb; and mixtures thereof.
[0018] In certain embodiments, the phosphor particles 101 have a diameter or size between about 1 nanometer and about 1 millimeter, between about 100 nanometers and about 500 micrometers, between about 1 micrometer and about 200 micrometers, between about 1.5 micrometers and about 100 micrometers, or between about 2 micrometers and about 50 micrometers. Typically, the particles are not spherical, and the term "diameter" as used herein refers to the diameter of a sphere having the same volume as the volume of the particle. In certain embodiments, the phosphor particles 101 are characterized by a particle size distribution having a D10 value between about 1 micrometer and about 10 micrometers, and a D90 value between about 10 micrometers and about 100 micrometers. The particle size distribution can be measured by various methods known in the art, such as laser diffraction, dynamic light scattering, dynamic image analysis, sieve analysis, optical counting, electrical resistance counting, sedimentation, acoustic spectroscopy, laser occlusion time, etc. With respect to cumulative particle size distribution, the quantities D10, D50, and D90 refer to the diameter at which 10% of the particles by volume, 50% of the particles by volume, or 90% of the particles by volume, respectively, have a diameter less than or equal to the specified value. In this terminology, the quantities referred to as D10, D50, and D90 are sometimes referred to as Dv10, Dv50, and Dv90, respectively.
[0019] 1A, in certain embodiments, phosphor particles 101 may be coated with an aluminum-containing coating 103. In certain embodiments, aluminum-containing coating 103 has a thickness between about 10 nanometers and about 100 micrometers, between about 100 nanometers and about 25 micrometers, between about 150 nanometers and about 10 micrometers, or between about 0.25 micrometers and about 5 micrometers. In certain embodiments, aluminum-containing coating 103 is deposited by a physical vapor deposition (PVD) method, such as thermal evaporation, electron beam evaporation, or sputtering. In certain embodiments, aluminum-containing coating 103 is deposited by chemical vapor deposition (CVD). In certain embodiments, aluminum-containing coating 103 also includes other components, such as a getter composition, including one or more of beryllium, magnesium, calcium, strontium, barium, scandium, titanium, vanadium, chromium, yttrium, zirconium, niobium, rare earth metals, hafnium, tantalum, and tungsten. In certain embodiments, the aluminum-containing coating 103 also includes one or more of beryllium, magnesium, scandium, or yttrium. In this context, getter refers to a composition that has a higher affinity for oxygen than aluminum. Aluminum oxide forms a very stable passivation film on the surface of aluminum metal, which can be detrimental to the formation of aluminum nitride, and the presence of a getter can inhibit the formation of aluminum oxide by preferentially binding to available oxygen, reducing the concentration of oxides that form on the surface of the aluminum metal during processing. In preferred embodiments, the oxide of the getter material has a high thermal conductivity, with beryllium oxide being a prominent example.
[0020] In certain embodiments, the phosphor particles 101 are agitated on a surface, such as a vibrating table, while the aluminum-containing coating 103 is being deposited. In certain embodiments, the phosphor particles 101 are in a fluidized bed while the aluminum-containing coating 103 is being deposited. In certain embodiments, a nitrogen-containing gas is present during deposition of the aluminum-containing coating 103. In certain embodiments, the nitrogen-containing gas comprises or consists of ammonia or N2.
[0021] 1B, in certain embodiments, phosphor particles 101 are mixed with aluminum-containing particles 105. The mixing of particles, which can be used to form an aluminum-containing green body, discussed further below, can promote the formation of an aluminum-containing nitride matrix around the phosphor particles, which has high thermal conductivity. The aluminum-containing particles 105 can include or consist of aluminum nitride powder, aluminum nitride grit, aluminum powder, aluminum flakes, aluminum pellets, aluminum shavings, aluminum grit, aluminum evaporation slag, and the like. The aluminum-containing particles 105 can have a minimum dimension between about 10 millimeters and about 1 micrometer, between about 5 millimeters and about 2 micrometers, between about 2 millimeters and about 5 micrometers, between about 1 millimeter and about 10 micrometers, or between about 500 micrometers and about 20 micrometers. Larger sized aluminum-containing particles 105 can be more difficult to mix with phosphor particles 101, but can have benefits associated with reduced oxygen content, which can allow for higher thermal conductivity and improved translucency of the final ceramic matrix composite. The volume ratio of phosphor particles 101 to aluminum-containing particles 105 can be between about 1% and about 99%, between about 5% and about 95%, between about 10% and about 90%, or between about 20% and about 80%. In certain embodiments, phosphor particles 101 are mixed with aluminum-containing particles 105 in a ball mill, attrition mill, jet mill, or the like. In certain embodiments, a grinding medium, such as Si3N4, SiC, ZrO2, or AlN, is present during the mixing operation and can be separated from the mixture upon completion of grinding. In certain embodiments, the grinding process is performed under a dry nitrogen atmosphere. In certain embodiments, a shielding gas is used. In certain embodiments, the atmosphere present during the grinding operation includes or consists of ammonia. During the grinding process, a mechanical bond can be formed between at least a portion of phosphor particles 101 and aluminum-containing particles 105.
[0022] In certain embodiments, additional powder components are mixed with the phosphor particles 101. In certain embodiments, a getter composition may be mixed with the phosphor particles 101, such as one or more of beryllium, magnesium, calcium, strontium, barium, scandium, titanium, vanadium, chromium, yttrium, zirconium, niobium, rare earth metals, hafnium, tantalum, and tungsten, and their nitrides, oxynitrides, amides, imides, amideimides, halides, or oxyhalides. In certain embodiments, the getter composition includes one or more of beryllium, magnesium, scandium, and yttrium. In certain embodiments, the getter composition is included as an impurity in the aluminum-containing particles 105. In certain embodiments, the aluminum-containing particles 105 include or consist of between about 0.1% and about 20%, or between about 1% and about 10%, of the getter composition and an alloy including between about 80% and about 99.9%, or between about 90% and 99% aluminum.
[0023] In certain embodiments, as shown generally in FIG. 2A, phosphor particles 101 are mixed and dispersed in a slurry 201 as part of a processing system 200. The processing system 200 includes a mixing component 251 and a green body forming assembly 255. The mixing component 251 can include a mixing device 253, a slurry tank 254, a homogenizing device 259, and a pump 260. The green body forming assembly 255 can include a carrier film supply assembly 261 with a carrier film supply reel 211, an input tank 265, a doctor blade 266, a heating device 267, a green body take-up reel 213, and a carrier film take-up reel 212. In some embodiments, the slurry includes water. In certain embodiments, the slurry includes a polar, aprotic solvent. In certain embodiments, the slurry is substantially free of water and includes an aliphatic solvent, such as diethylamine, or an aromatic solvent, such as aniline. Avoidance of water and protic solvents can help minimize the formation of Al2O3 and other oxides on the surfaces of the phosphor particles 101, the aluminum-containing coating 103, and the aluminum-containing particles 105 (if present). In certain embodiments, the slurry includes one or more of binders, lubricants, wetting agents, plasticizers, dispersants, deflocculants, other additives, etc., as known in the art. In certain embodiments, the slurry includes one or more of a wax composition and urea.
[0024] Organic binders that can be used in the preparation of aluminum-containing nitride ceramic matrix composites as a component of the slurry or dry mixed powder include, but are not limited to, vinyl polymers (e.g., polyvinyl butyral (PVB), polyvinyl alcohol (PVA), polyvinyl chloride (PVC), polyvinyl acetate (PVAc), polyacrylonitrile, mixtures thereof and copolymers thereof, etc.), polyethyleneimine, polymethyl methacrylate (PMMA), vinyl chloride-vinyl acetate and mixtures thereof, preferably PVB. Plasticizers that can be used in the manufacture of aluminum-containing ceramic matrix composites include, but are not limited to, butyl benzyl phthalate, dicarboxylic acid / tricarboxylic acid ester based plasticizers (e.g., phthalic acid based plasticizers such as, but not limited to, bis(2-ethylhexyl) phthalate, diisononyl phthalate, bis(n-butyl) phthalate, butyl benzyl phthalate, diisodecyl phthalate, di-n-octyl phthalate, diisooctyl phthalate, diethyl phthalate, diisobutyl phthalate, di-n-hexyl phthalate, and mixtures thereof), adipic acid based plasticizers. (such as, but not limited to, bis(2-ethylhexyl) adipate, dimethyl adipate, monomethyl adipate, dioctyl adipate, and mixtures thereof), sebacic acid-based plasticizers (such as, but not limited to, dibutyl sebacate), and maleic acid-based plasticizers (such as, but not limited to, dibutyl maleate, diisobutyl maleate, and mixtures thereof); polyalkylene glycols (such as, but not limited to, polyethylene glycol, polypropylene glycol, and mixtures thereof).Other plasticizers that may be used include, but are not limited to, benzoic acids; epoxidized vegetable oils; sulfonamides (such as, but not limited to, N-ethyltoluenesulfonamide, N-(2-hydroxypropyl)benzenesulfonamide, and N-(n-butyl)benzenesulfonamide); organophosphates (such as, but not limited to, tricresyl phosphate and tributyl phosphate); glycols / polyethers (such as, but not limited to, triethylene glycol dihexanoate, triethylene glycol diheptanoate, and mixtures thereof); alkyl citrates (such as, but not limited to, triethyl citrate, acetyl triethyl citrate, tributyl citrate, acetyl tributyl citrate, trioctyl citrate, acetyl trioctyl citrate, trihexyl citrate, acetyl trihexyl citrate, butyryl trihexyl citrate, and trimethyl citrate); and alkyl sulfonic acid phenyl esters, and mixtures thereof.
[0025] Dispersants that can be used to form the slurry or dry mix powder include, but are not limited to, oxidized menhaden fish oil (MFO), dicarboxylic acids such as succinic acid, ethanedioic acid, propanedioic acid, pentanedioic acid, hexanedioic acid, heptanedioic acid, octanedioic acid, nonanedioic acid, decanedioic acid, sorbitan monooleate, o-phthalic acid, p-phthalic acid, and mixtures thereof.
[0026] In certain embodiments, as shown in Figures 2A, 2B, and 2C, a slurry 201 including phosphor particles 101 and / or aluminum-containing particles 105 is tape cast onto a flexible carrier film using tape casting or doctor blade techniques to form a green body 290 on the carrier film 202 using components in a processing system 200. In one example, the green body 290 can be formed as a continuous roll of material (referred to herein as green body 290A) that is received on a take-up reel 213, or as multiple green body disks 290B as shown in Figures 2B and 2C. The carrier film 202 is fed from a supply reel 211 to a take-up reel 212 of a carrier film supply assembly 261. In certain embodiments, the carrier film 202 includes or consists of Mylar™. In certain embodiments, the carrier film 202 comprises or consists of stainless steel or a metal composition having a melting point above about 600° C., or above about 660° C. In certain embodiments, the carrier film 202 comprises an aluminum-containing foil or coating. In certain embodiments, the aluminum-containing foil or coating also comprises a getter composition at a concentration of between about 0.1% and about 20%, or between about 1% and about 10%.
[0027] In certain embodiments, the carrier film with the layer of slurry applied thereto is subjected to a drying process to form a green body 290. In certain embodiments, an aluminum-containing layer 303 is deposited on the carrier film 202 with the layer of slurry 302 applied thereto, as shown generally in FIG. 3A. In certain embodiments, the dried slurry layer having the aluminum-containing coating 303 and / or including the aluminum-containing particles 105 is heated to a temperature above 660° C., for example, between about 660° C. and about 900° C., or between about 675° C. and about 750° C., to melt the aluminum-containing layer 303 and / or the aluminum-containing coating 103 and / or the aluminum-containing particles 105 and draw them into and through the dried slurry layer by capillary action to form the aluminum-containing coating 355 and aluminum-containing composite 359, as shown generally in FIG. 3B. In certain embodiments, the melting and infiltration process is performed in a vacuum for about 10 minutes. -2 Torr (approx. 1.3 Pa), approx. 10 -3 Torr (approx. 1.3 x 10 -1 Pa), approximately 10 -4 Torr (approx. 1.3 x 10 -2 Pa), approximately 10 -5 Torr (approx. 1.3 x 10 -3 Pa), approximately 10 -6 Torr (approx. 1.3 x 10 -4 Pa), approximately 10 -7 Torr (approx. 1.3 x 10 -5 Pa) or less than about 10 -8 Torr (approx. 1.3 x 10 -6 The melting and infiltration process is carried out at a pressure of less than 1000 Pa. In certain embodiments, the melting and infiltration process is carried out under a nitrogen-containing atmosphere, such as N2 or NH3, or an inert atmosphere, such as Ar, that is substantially free of oxygen and water. In certain embodiments, pores 357 are present in the composite. The presence of pores 357 can facilitate a subsequent nitridation process of the composite by providing a pore network that allows nitrogen-containing species (e.g., ammonia) to reach exposed aluminum-containing surfaces within the composite during processing.
[0028] In one particular embodiment, an aluminum-containing foil or coating 402 is present on a carrier film 202 with a dried slurry layer 403 underneath, as shown generally in Figure 4A. In one particular embodiment, the carrier film 202 and dried slurry layer 403 are heated to a temperature above 600°C, for example, between about 660°C and about 900°C, or between about 675°C and about 750°C, causing the aluminum-containing foil or coating 402 to melt and be drawn into the dried slurry layer by capillary action, forming an aluminum-containing coating 355 and an aluminum-containing composite 359, as shown generally in Figure 4B. In one particular embodiment, the melting and infiltration process is carried out in a vacuum for about 10 -2 Torr (approx. 1.3 Pa), approx. 10 -3 Torr (approx. 1.3 x 10 -1 Pa), approximately 10 -4 Torr (approx. 1.3 x 10 -2 Pa), approximately 10 -5 Torr (approx. 1.3 x 10 -3 Pa), approximately 10 -6 Torr (approx. 1.3 x 10 -4 Pa), approximately 10 -7 Torr (approx. 1.3 x 10 -5 Pa) or less than about 10 -8 Torr (approx. 1.3 x 10 -6 The melting and infiltration process is carried out at a pressure of less than 100 Pa. In certain embodiments, the melting and infiltration process is carried out under a nitrogen-containing atmosphere, such as N2 or NH3, or under an inert atmosphere, such as Ar, that is substantially free of oxygen and water. In certain embodiments, pores 357 are present in the composite.
[0029] 2A, in some embodiments, after formation of a green body 290A, such as an aluminum infiltrated composite green body, the green body can be stripped from the carrier film 202 and collected on a take-up reel 212 for further processing. The green body 290 can be characterized by a porosity of between about 10% and about 80%, or between about 20% and about 60%. A lower level of porosity can help increase the thermal conductivity of the aluminum-containing nitride matrix composite after nitridation, while a higher level of porosity can facilitate the nitridation process itself by providing easier access to ammonia during subsequent processing.
[0030] In a particular embodiment, as shown in FIG. 2B, the slurry 20 is screen printed or tape cast using tape casting or doctor blade techniques onto a flexible carrier film 202 overlying a stencil mask 271. In a particular embodiment, the stencil mask 271 is made of a polymer such as Mylar™ or silicone. In other embodiments, the stencil mask 271 is made of a metal or metal alloy, such as stainless steel. In a particular embodiment, the stencil mask 271 has openings 272 arranged in a square or hexagonal array across the surface of the stencil mask 271. In a particular embodiment, the openings 272 of the stencil mask 271 are circular and have a diameter between about 50 micrometers and about 100 millimeters, between about 200 micrometers and about 50 millimeters, between about 500 micrometers and about 20 millimeters, or between about 1 millimeter and about 10 millimeters. In certain embodiments, the stencil mask 271 has a thickness (i.e., vertically in FIG. 2B ) of between about 10 micrometers and about 1 millimeter, between about 20 micrometers and about 500 micrometers, or between about 50 micrometers and about 200 micrometers. In certain embodiments, a fixture is provided such that after the doctor blade 266 applies the slurry 201 composition into the openings 272 of the stencil mask 271, the stencil mask 271 is separated from the carrier film 202, leaving individual green body disks 290B on the carrier film 202, as shown diagrammatically on the left side of FIG. 2B .
[0031] In certain embodiments, rather than forming a green body 290 such as a continuous green body film 290A (FIG. 2A) or a green body disk 290B (FIG. 2B) by tape casting as shown generally in FIGS. 2A, 2B, and 2C, a green body including phosphor particles 101 can be formed by using a granulation and / or tableting process using a tableting system 500 as shown generally in FIG. 5A. The phosphor particles 101, with or without the aluminum-containing coating 103 and / or aluminum-containing particles 105, can be mixed with one or more of binders, lubricants, wetting agents, dispersants, deflocculants, other additives, and the like, by use of a material feeder 501 and one or more mixing and compacting components 505, as known in the art. In certain embodiments, the mixture includes one or more of a wax composition and urea. In certain embodiments, the mixture can also include any number of liquid components. In certain embodiments, avoidance of protic components such as polyvinyl alcohol and ethylene glycol can help minimize the formation of Al2O3 and other oxides on the surfaces of the phosphor particles 101, the aluminum-containing coating 103, and the aluminum-containing particles 105. In certain embodiments, the mixing process is performed using a V-blender, powder mixer, or the like. The mixed powder may be formed into granules by roller compaction, into ribbons, or into roughly spherical granules using a tableting device 551. In certain embodiments, the ribbons are broken into granules by a grinding process.
[0032] In one particular embodiment, as shown generally in Figure 5B, a slurry containing phosphor particles 101 is mixed in the form of a slurry and then dried into a powder (i.e., a powder product) by using a spray drying process. In some cases, the mixed powder with additional ingredients, such as one or more of a binder, lubricant, wetting agent, dispersant, deflocculating agent, and other additives, may be compressed into granules, and the like.
[0033] As shown diagrammatically in Figure 5C, granules 549 can be fed into a tablet press 551 and uniaxially pressed into tablets by methods known in the art. One or more doctor blades 266 can guide the granules 549 into a die cavity 547. The upper piston 533 is pushed downward by an upper cam 543 and the lower piston 531 is pushed upward by a lower cam 541 causing the formation of a tablet 535 which is then ejected.
[0034] In certain embodiments, the mixed powder is formed into pellets using a disk pelletizer, as known in the art. The pellets may or may not be further densified by a tableting process. In certain embodiments, the volatile components in the granules, pellets, or tablets are removed by a drying operation.
[0035] In certain embodiments, the granules, pellets, or tablets are infiltrated with the aluminum-containing composition by evaporation and heating, as shown generally in Figures 3A and 3B. In certain embodiments, the granules, pellets, or tablets are infiltrated with the aluminum-containing composition by placing them in contact with a foil or coating and heating, as shown generally in Figures 4A and 4B.
[0036] Other methods for incorporating the phosphor particles 101 into the aluminum-containing green body are also possible, including slip casting, uniaxial pressing, isostatic pressing, and screen printing.
[0037] In certain embodiments, the aluminum-containing coating or particle composition in the granules, pellets, tablets, or tape cast green bodies has a purity of between 99.9999% and 90%, between 99.9% and 95%, between 99.8% and 97%, or between 99.5% and 98% based on the metals. In certain embodiments, the aluminum-containing coating or particle composition includes Fe and / or Si as impurities, for example, in a concentration of between about 1 ppm and about 10% by weight, or between about 10 ppm and about 1% by weight.
[0038] As shown in Fig. 6, the aluminum-containing green body 609, whether in the form of granules, pellets, tablets, roll film, or other form, is disposed within the interior 621 of the sealable container 600. The sealable container 600 can include or consist of a capsule, an autoclave, or a liner within an autoclave. The capsule or liner can be composed of or include at least one of silver, a silver-based alloy, copper, a copper-based alloy, gold, palladium, platinum, iridium, ruthenium, rhodium, titanium, iron, an iron-based alloy, stainless steel, nickel, a nickel-based alloy, zirconium, niobium, molybdenum, tantalum, combinations thereof, and the like. The sealable container can include a fill tube, or one or more of a top inlet 623 and a bottom inlet 625.
[0039] At least one mineralizer composition can be added to the sealable container. The mineralizer composition can be composed of or include an alkali metal, such as Li, Na, K, Rb, or Cs, an alkaline earth metal, such as Be, Mg, Ca, Sr, or Ba, or an alkali or alkaline earth hydride, amide, imide, amide-imide, nitride, or azide. The mineralizer can be composed of or include an ammonium halide, such as NHF, NH4Cl, NH4Br, or NHI, an aluminum halide, such as AlF3, AlCl3, AlBr3, AlI3, or any compound that can be formed by the reaction of two or more of F, Cl, Br, I, HF, HCl, HBr, HI, Al, AlN, and NH3. The mineralizer can be composed of or include other alkali, alkaline earth, or ammonium salts, other halides, urea, sulfur or sulfide salts, or phosphorus or phosphorus-containing salts. In certain embodiments, the mineralizer comprises or consists of at least one of KN3 and NaN3, and is substantially free of moisture.
[0040] If the mineralizer is substantially free of the halogens Cl, Br, and I, silver may work well as a material of construction for the sealable container 600. However, if at least one of Cl, Br, and I is present in significant concentrations, gold, platinum, or platinum / iridium may be better choices.
[0041] A getter may also be added to the sealable container 600. The getter preferentially reacts with residual or extraneous oxygen or moisture present within the processing region 621, including oxygen that may be present on the surface of the phosphor particles and / or the aluminum-containing coating composition, to improve the purity, thermal conductivity, and optical transparency of the aluminum-containing nitride ceramic matrix composite. Examples of suitable getters include beryllium, magnesium, calcium, strontium, barium, scandium, titanium, vanadium, chromium, yttrium, zirconium, niobium, rare earth metals, hafnium, tantalum, and tungsten, as well as their nitrides, oxynitrides, amides, imides, amide-imides, halides, or oxyhalides. In certain embodiments, the getter includes at least one of Be, Mg, Ca, Ba, Y, or nitrides thereof. In preferred embodiments, the getter oxide formed during the gettering process, e.g., BeO, MgO, CaO, or YO, is characterized by a high thermal conductivity, e.g., greater than about 10 W / mK, greater than about 20 W / mK, greater than about 40 W / mK, or greater than about 100 W / mK.
[0042] In certain embodiments, in addition to the azide mineralizer and aluminum-containing coating or particle composition, optionally an additional metal, such as a getter in the form of a metal, for example as a component of an aluminum-containing alloy, is provided in a predetermined ratio such that the nitrogen produced by decomposition of the azide mineralizer and the hydrogen gas species produced by reaction of at least the metal with supercritical ammonia are in a ratio of about 1:3. For example, under ammonothermal reaction conditions, aluminum and other metals, if present, undergo one or more of the following reactions: Al+NH3=AlN+3 / 2H2 Na+NH3=NaNH2+1 / 2H2 K+NH3=KNH2+1 / 2H2 3Be+2NH3=Be3N2+3 / 2H2 3Mg+2NH3=Mg3N2+3 / 2H2 3Ca+2NH3=Ca3N2+3 / 2H2 Ca+2NH3=Ca(NH2)2+H2 Y+3NH3=Y(NH2)3+3 / 2H2 Y+NH3=YN+3 / 2H2 The use of azides as mineralizers is convenient in that they are often commercially available in high purity, can be further purified, and are much less hygroscopic than, for example, alkali metal or amide or alkaline earth nitrides. However, azides usually decompose under reaction conditions to produce nitrogen: 3KN3+2NH3=3KNH2+4N2 In a preferred embodiment, these two effects, i.e. the production of hydrogen by the reaction of the metal with ammonia and the formation of nitrogen by the decomposition of azide, are combined to counteract each other. The metal containing aluminum-containing coating and / or particle composition, the mineralizer, and the getter are added together with the azide mineralizer precursor so that H2 and N2 are produced in a ratio of about 3:1. The sealable container may further comprise a means for catalyzing the formation of NH3 from H2 and N2. The catalysis of the reaction between H2 and N2 liberated in the reaction of the metal with ammonia to reform ammonia, and the decomposition of azide, respectively, may be performed by the walls of the sealable container or by a catalyst also provided within the sealable container. The added catalyst may comprise a powder, granules, foil, coating, bulk material, or porous pellets. The added catalyst may include or consist of at least one of iron, cobalt, nickel, titanium, molybdenum, tungsten, aluminum, potassium, cesium, calcium, magnesium, barium, zirconium, osmium, uranium, or lanthanides, ruthenium, platinum, palladium, or rhodium. In a particular example, the added catalyst includes or consists of a ruthenium sponge. For example, the addition of 1 mole of KN3 mineralizer produces 4 / 3 moles of N2 while being converted to KNH2. Nitrogen production can be countered by adding 8 / 3 moles of Al and / or another metal, which produces 8 / 3 x 3 / 2 moles = 4 moles of H2, i.e., 3 times as many moles of N2 from KN3.
[0043] The sealable container 600 is then closed and sealed except for one or more connections to a fluid manifold, including at least one of a gas, liquid, or vacuum manifold. The sealable container can then be evacuated to remove air, moisture, and other volatile contaminants. In some embodiments, the sealable container 600 is heated to a temperature between about 25° C. and about 500° C. during evacuation. In some embodiments, the sealable container is subjected to at least two, at least three, at least five, or at least ten evacuation cycles, and then refilled with an inert gas, such as argon or nitrogen. In one particular embodiment, referring to FIG. 6, the sealable container is provided with at least a bottom inlet 625 that can function as a gas phase inlet and a top inlet 623 that can function as a gas phase outlet, such that the sealable container can be purged with a continuous gas flow. Purging can provide superior removal of air, moisture, and other volatile contaminants compared to evacuation, since purging has limited conductance through the tubes to the interior of the sealable container. The efficiency of purging can be increased by flowing the purge gas from one end of the interior volume of the sealable container to the other. According to certain embodiments, the sealable container can be connected to a gas source in a fluid manifold by at least one fill or purge tube, preferably without exposing the contents of the sealable container to air. The gas source can include at least one of nitrogen, argon, hydrogen, helium, and ammonia, among others. Further details of configurations for purging the sealable container are described in U.S. Pat. No. 8,444,765, the entire contents of which are incorporated herein by reference.
[0044] In certain embodiments, as shown generally in FIG. 3B or 4B, infiltration of the phosphor-containing granules, pellets, tablets, or tape cast film with the aluminum-containing composition can be performed in situ in a sealable container under vacuum or while purging the sealable container with an inert gas, such as argon, or a nitrogen-containing gas, such as nitrogen or ammonia, at a temperature, for example, between about 660° C. and about 750° C.
[0045] After the pump-purge and / or flow-purge process is completed, the sealable vessel 600 can be cooled and filled with ammonia to a specified level. In certain embodiments, the sealable vessel 600 is cooled to dry ice temperatures, for example by immersion in a dry ice solvent bath or by using a heat exchanger, and a controlled amount of gaseous ammonia flows from the fluid manifold into the sealable vessel and is condensed to a liquid phase. In other embodiments, a controlled amount of liquid ammonia flows into the sealable vessel 600 at high pressure from a pumped fluid assembly in the fluid manifold, for example at pressures greater than about 7 atmospheres.
[0046] In certain embodiments, the mineralizer is added, for example in solution, to the sealable vessel 600 along with liquid ammonia. For example, referring to FIG. 9, the mineralizer composition can be weighed and added to the mineralizer vessel 951 in a glove box (not shown), and the mineralizer vessel 951 can be sealed and removed from the glove box. The mineralizer vessel 951 and the flash vessel 953 can be attached to an ammonia manifold 961. With valves 955 and 957 open, the mineralizer vessel 951 can be cooled to dry ice temperature and filled with a predetermined amount of ammonia. Then, with valve 957 open and valve 955 closed, the flash vessel 953 can be cooled and filled with a predetermined amount of ammonia. With valve 957 closed, the flash vessel 953 and the mineralizer vessel 951 can be disconnected from the ammonia manifold and allowed to warm to room temperature, producing a solution of mineralizer in ammonia in the mineralizer vessel 951 and connected to a pre-evacuated sealable vessel. Valve 959 can then be opened along with any additional valves between mineralizer vessel 951 and sealable vessel 600 to inject liquid ammonia mineralizer solution into sealable vessel 600. If necessary, sealable vessel 600 can be cooled or mineralizer vessel 951 can be heated, for example, to 5 to 25° C., to transfer the last residues of liquid ammonia to sealable vessel 600. Valve 959 can then be closed and valve 955 can be opened to transfer ammonia from flash vessel 953 to mineralizer vessel 951. If necessary, mineralizer vessel 951 can be cooled or the heater of flash vessel 953 can be cooled, for example, to 5 to 25° C., to transfer the last residues of liquid ammonia from flash vessel 953 to mineralizer vessel 951. Mineralizer vessel 951 can then be warmed to room temperature, which redissolves traces of mineralizer left by the initial ammonia transfer from mineralizer vessel 951 to sealable vessel 600. Valve 959, along with any additional valves (e.g., V4 and FV) between mineralizer vessel 951 and sealable vessel 600, can then be opened to inject the liquid ammonia mineralizer solution into sealable vessel 600. This process can be repeated as many times as necessary.As discussed above, additional ammonia can be added to the sealable vessel 600. After processing, the remaining ammonia can be discharged through outlet 965.
[0047] The percentage of free volume in the sealable container 600 that is filled with liquid ammonia can be between about 10% and about 95%, between about 20% and about 90%, between about 30% and about 80%, or between about 40% and about 70%. After the desired amount of ammonia has been added to the sealable container 600, the sealable container 600 can be closed and sealed. The sealing process can include one or more of closing valves, ultrasonically welding fill tubes, such as the top inlet 623 and / or the bottom inlet 625, and tungsten inert gas welding fill tubes, such as the top inlet 623 and / or the bottom inlet 625.
[0048] In certain embodiments, the ammonia charging process is performed while the sealable container is sealed within the pressure vessel (or pressure vessel if the sealable container is an autoclave). In certain embodiments, the sealable container 600 is placed within the pressure vessel after being charged with ammonia and sealed.
[0049] In one particular embodiment, the pressure vessel is an autoclave and the sealable vessel 600 is a liner or capsule 211 within the autoclave 200, as shown diagrammatically in Figure 7. The autoclave may be capable of processing materials in a fluid at pressures greater than about 5 MPa and less than about 800 MPa, less than about 500 MPa, less than about 400 MPa, less than about 300 MPa, less than about 200 MPa, or less than about 100 MPa, and temperatures between about 50°C and about 900°C, between about 100°C and about 600°C, between about 150°C and about 500°C, or between about 200°C and about 400°C. Referring to Figure 7, the autoclave 200 includes an autoclave body 201. An upper portion of the autoclave body 201 may be surrounded by an upper heater 205, and a lower portion of the autoclave body may be surrounded by a lower heater 207, each of which may include insulation. The upper heater 205 can include one, two, or more independently controllable hot zones, such as an upper tail zone 205a and an upper main zone 205b. The lower heater 207 can include one, two, or more independently controllable hot zones, such as a lower main zone 207a and a lower tail zone 207b. The upper heater 205 and the lower heater 207 can be physically combined into a single component, but are typically independently controllable. In a particular embodiment, a liner 211 is disposed within the cavity of the autoclave body 201. The liner 211 can be formed of or include one or more of platinum, palladium, iridium, Pt / Ir alloy, gold, or silver. The liner 211 can also include or be formed of one or more of titanium, rhenium, copper, stainless steel, zirconium, tantalum, molybdenum, niobium, alloys thereof, and the like.
[0050] In certain embodiments, the autoclave 200 further includes an autoclave cap 217 and a closure fixture 219 in addition to a gasket (not shown), as shown diagrammatically. The configuration shown in FIG. 7 is a schematic of a Grayloc™ seal. In other embodiments, the autoclave 200 includes one or more of an unsupported Bridgman seal, an o-ring seal, a trapped gasket seal, a bolted closure, an AE™ closure, an EZE-Seal™, a Keuntzel closure, a ZipperClave™ closure, a threadless pin closure, or a Gasche™ gasket seal. In certain embodiments, the autoclave 200 further includes a bottom cap, closure fixture, and seal in addition to a top cap, closure fixture, and seal.
[0051] The autoclave body 201, the autoclave cap 217, and the closure fixture 219 may each be manufactured from a material selected from the group consisting of steel, low carbon steel, SA723 steel, SA266 carbon steel, 4340 steel, A-286 steel, iron-based superalloys, nickel-based superalloys, cobalt-based superalloys, Inconel 718, Rene 41, 304 stainless steel, 310 stainless steel, 316 stainless steel, 340 stainless steel, 410 stainless steel, and 17-4 precipitation hardening stainless steel, zirconium and its alloys, titanium and its alloys, and other materials commonly known as Monel, Inconel, Hastelloy, Udimet 500, Stellite, Rene 41, and Rene 88. One or more of the components including the autoclave body 201, the autoclave cap 217, and the closure fixture 219 may be subjected to a heat treatment operation. In one particular embodiment, the autoclave body 201 includes removable seals on the bottom as well as the top.
[0052] The autoclave 200 may further comprise a bottom end heater 231 thermally coupled to the bottom of the autoclave body 201 and including thermal insulation 232. The bottom end heater 231 produces a substantially uniform power distribution azimuthally about the axis of the autoclave body 201. The power level of the bottom end heater 231 relative to the power levels of the lower heater 207 and the top heater 205 along with the radial dependence of the power density within the bottom end heater 231 is selected to maintain a uniform temperature distribution along the bottom surface 215 to within 10° C., 5° C., 2° C., 1° C., 0.5° C., or 0.2° C. In certain embodiments, the power level of the bottom end heater 231 relative to the power levels of the lower heater 207 and the top heater 205 along with the radial dependence of the power density in the bottom end heater 231 is selected to maintain an average temperature of the bottom surface 215 equal to the average temperature within a specified height within within 20° C., 10° C., 5° C., 2° C., or 1° C., as measured on the bottom surface 215, the inner surface of the liner 211, or the inner surface of the autoclave body 201 when the liner 211 is not present. In certain embodiments, the specified height is about 1 centimeter, 5 centimeters, 10 centimeters, 20 centimeters, or 25 centimeters. In certain embodiments, the bottom end heater 231 is configured with at least two or at least three independently controllable hot zones.
[0053] In certain embodiments, the autoclave 200 further includes an upper insulator / heater 209. In certain embodiments, the upper insulator / heater 209 includes or consists of a load-bearing thermal insulator, such as zirconia, or another ceramic material with low thermal conductivity. In certain embodiments, the upper insulator / heater also functions to generate heat, for example, by electrical connection through the autoclave cap 217. In certain embodiments, the upper insulator / heater 209 includes one or more of a cartridge heater, a cable heater, a disk heater, and the like. The upper insulator / heater 209 can have a surface that is finished to fit snugly against the underside of the autoclave cap 217 and the upper surface 245 of the liner 211, and sufficient radial clearance against the inner surface of the autoclave body 201 to facilitate insertion and removal without the top of the liner 211 being pushed out into the radial gap during high pressure operation. The dimensions of the upper insulator / heater 209 and its power level, if present, as well as the power levels of the lower heater 207 and upper heater 205, including the upper zone in the upper heater 205, and the radial dependence of the power density in the upper insulator / heater 209, can be selected to maintain a uniform temperature distribution along the top surface 245 to within 10° C., 5° C., 2° C., or 1° C. Additionally, the dimensions of the upper insulator / heater 209 and the upper heater 205 and lower heater 207 power levels can be selected to maintain the top surface 245 at an average temperature within 20° C., 10° C., 5° C., 2° C., or 1° C. equal to the average temperature within a specified height, as measured relative to the top surface 245, the inner surface of the liner 211, or the inner surface of the autoclave body 201 if the liner 211 is not present. In certain embodiments, the specified height is about 1 centimeter, 5 centimeters, 10 centimeters, 20 centimeters, or 25 centimeters. In one particular embodiment, the upper insulator / heater 209 is configured with at least two or at least three independently controllable hot zones.
[0054] In a particular embodiment, the sealable vessel 600 is placed in the internally heated high pressure apparatus 300 as a capsule 307, as shown diagrammatically in FIG. 8. The internally heated high pressure apparatus 300 provides adequate containment in all directions, which for a typical cylindrical vessel can be classified as radial and axial. Furthermore, depending on the details of the design parameters, the apparatus can operate at temperatures between 200° C. and 1500° C., and pressures between about 5 MPa and about 2000 MPa, for periods between about 1 hour and about 180 days. The internally heated high pressure apparatus 300 can include a stack of one or more ring assemblies with high strength enclosure rings 301 and ceramic rings 303 to provide radial containment. The stack can include more than 2, more than 5, more than 10, more than 20, more than 30, more than 50, or more than 100 ring assemblies. The stack surrounds the heater or heating element 305 and the capsule 307, and can be mechanically supported by at least one support plate (not shown). In other words, the heating element or heater can be positioned between the capsule and one or more radial restraining structures including the high strength enclosure ring and the ceramic ring 303. The stack can radially confine the pressure generated in the capsule 307 and transmitted outward through the heater 305. The heater 305 includes an upper heater 305a and a lower heater 305b. The upper heater 305a and the lower heater 305b can each include one, two, or more independently controllable hot zones. The upper heater 305a and the lower heater 305b can be physically combined into a single component, but are typically independently controllable. The interior of the heater 305 can define a process chamber within which the capsule 307 can be located. When the ring assemblies in the die stack are comprised of the high strength enclosure ring 301 and the ceramic ring 303, there can be an interference fit between the two members of each ring assembly. Means may be provided for externally cooling one or more of the ring assemblies or radial restraints. In one particular embodiment, capsule 307 includes an inner capsule member and an outer capsule member (not shown).
[0055] Axial containment of the pressure generated within the capsule 307 may be provided by the end plugs 311, the crown member 317, and the tie rods or tie rod fasteners 315. The end plugs 311 may include zirconium oxide or zirconia. Alternative end plug materials include magnesium oxide, aluminum oxide, silicon oxide, silicon carbide, tungsten carbide, steel, nickel alloys, titanium alloys, salts, and phyllosilicate minerals such as aluminum hydroxide silicate or pyrophyllite, according to certain embodiments. The end plugs 311 may be surrounded by an end plug jacket 313. The end plug jacket may provide mechanical support and / or radial containment for the end plugs 311. The end plug jacket 313 may also provide mechanical support and / or axial containment for the heater 305. The end plug jacket 313 may include steel, stainless steel, iron-based alloys, nickel-based alloys, etc. In certain embodiments, the tie rod fasteners 315 are arranged in a configuration to provide an axial load of two or more ring assemblies. Further details are provided in US Pat. Nos. 9,724,666 and 10,174,438, which are incorporated herein by reference in their entireties.
[0056] The crown member 317 and the tie rod fasteners 315 may comprise a material selected from the group consisting of steel, low carbon steel, SA723 steel, SA266 carbon steel, 4340 steel, A-286 steel, iron-based superalloys, 304 stainless steel, 310 stainless steel, 316 stainless steel, 340 stainless steel, 410 stainless steel, 17-4 precipitation hardened stainless steel, zirconium and its alloys, titanium and its alloys, and other materials known as Monel, Inconel, Hastelloy, Udimet 500, Stellite, Rene 41, and Rene 88.
[0057] The internally heated high pressure apparatus 300 may include a pressure transmission medium 309 proximate the axial end of the capsule 307 and the end plug 311, according to certain embodiments. The pressure transmission medium 309 may include multiple components, such as one or more disks. The pressure transmission medium may include sodium chloride, other salts, or phyllosilicate minerals, such as aluminum silicate hydroxide or pyrophyllite, or other materials, according to certain embodiments. In certain embodiments, the pressure transmission medium 309 may include one or more of metal halides, such as NaCl, NaBr, AgCl, AgBr, CaF2, SrF2, graphite, hexagonal boron nitride, talc, soapstone, gypsum, limestone, alabaster, molybdenum disulfide, calcium carbonate, magnesium oxide, zirconium oxide, melilinite clay, bentonite clay, or sodium silicate.
[0058] The internally heated high pressure apparatus 300 may further comprise a bottom end heater 331 and / or a top end heater 341 thermally coupled to the bottom and top, respectively, of the capsule 307. The bottom end heater 331 produces a nearly azimuthally uniform power distribution about the axis of the heater 305, and the relative power level of the bottom end heater 331 to the power levels of the lower heater 305b and the top heater 305a, along with the radial dependence of the power density within the bottom end heater 331, is selected to maintain a temperature distribution along the bottom surface 215 uniform to within 10°C, within 5°C, within 2°C, or within 1°C. In a particular embodiment, the relative power level of the bottom heater 331 to the power levels of the lower heater 305b and the top heater 305a, along with the radial dependence of the power density in the bottom heater 331, are selected to maintain an average temperature of the bottom surface 215, as measured relative to the bottom surface 215, within 10° C., 5° C., 2° C., or 1° C., equal to the average temperature within a specified height of the inner surface of the capsule 307. In a particular embodiment, the specified height is about 1 centimeter, 5 centimeters, 10 centimeters, 20 centimeters, or 25 centimeters. The top heater 341 produces a nearly azimuthally uniform power distribution about the axis of the heater 305, and the relative power level of the top heater 341 to the power levels of the bottom heater 305b and top heater 305a, along with the radial dependence of the power density in the top heater 341, is selected to maintain a temperature distribution along the top surface 345 uniform to within 10° C., 5° C., 2° C., or 1° C. In one particular embodiment, the relative power level of the top heater 341 to the power levels of the bottom heater 305b and top heater 305a, along with the radial dependence of the power density in the bottom heater 331, is selected to maintain an average temperature of the top surface 345 equal to the average temperature within a specified height of the inner surface of the capsule 307, as measured relative to the top surface 345, to within 10° C., 5° C., 2° C., or 1° C.
[0059] Next, the pressure vessel, e.g., autoclave 200 (FIG. 7) or internally heated high pressure apparatus 300 (FIG. 8), is closed and then the sealable vessel 600 is heated to a temperature above about 400° C. and pressurized to above about 10 MPa, and the ammonia in the sealable vessel 600 becomes a supercritical fluid. In certain embodiments, the temperature is increased to a first intermediate value, e.g., between about 100° C. and about 400° C., to allow the reaction of aluminum with other metals in the sealable vessel 600 to form hydrogen, as described above, and in the case of azide mineralizers, the azide mineralizer decomposes to amide and nitrogen, as described above, and in a catalytic reaction between hydrogen and nitrogen to form ammonia. The temperature can then be increased to a second value, for example, between about 400° C. and about 1000° C., between about 500° C. and about 800° C., or between about 600° C. and about 700° C., at a pressure between about 10 MPa and about 1000 MPa, between about 50 MPa and about 750 MPa, or between about 100 MPa and about 500 MPa. In one particular embodiment, referring to FIG. 8, the power levels of the bottom end heater 331, the top end heater 341, the top heater 305a, and the bottom heater 305b are adjusted to uniformly maintain the temperature within the capsule 307 (same as the sealable container 600) to within about 20° C., within about 10° C., within about 5° C., within about 2° C., or within about 1° C. The temperature can be maintained at this temperature for between about 1 hour and about 30 days, or between about 2 hours and about 7 days, or between about 3 hours and about 96 hours.
[0060] Referring to FIG. 6, while the sealable container 600 is held at high temperature in supercritical ammonia in the presence of a mineralizer, the aluminum present in the aluminum-containing green body 609 is converted to AlN and actually sinters with the phosphor particles 101 to form an aluminum-containing nitride ceramic matrix composite with high thermal conductivity. Without wishing to be bound by theory, the inventors believe that the supercritical ammonia enters the pores 357 of the aluminum-containing green body 609 (see FIGS. 3B and 4B) and also enters the cracks that form during the process of aluminum reacting with NH3 to form AlN, resulting in a local volume increase of about 25.7%. A portion of the AlN dissolves due to chemical reaction with the mineralizer. For example, in the case of a basic mineralizer, the following reversible reaction may occur: AlN+KNH2+2NH3=KAl(NH2)4 The dissolved intermediate (KAl(NH2)4 in the specific example) can then be transported through the pores 357, where a reverse reaction can occur, depositing AlN elsewhere. Thus, the supercritical fluid provides a mechanism by which Al atoms and AlN units within the ceramic composite can migrate. This is in many ways similar to the surface diffusion process that occurs during ceramic sintering processes at much higher temperatures. The grain coarsening and ceramic composite densification occurs for the same reason as occurs during normal sintering processes, i.e., due to the reduction in surface energy within the ceramic composite. However, because the supercritical fluid dissolution / redeposition process occurs at a much lower temperature than is required for sintering, it is much easier to maintain good properties within the phosphor particles 101, such as external quantum efficiency, and it is also much easier to incorporate two or more different types of phosphor particles in close proximity to each other within a single composite member with high thermal conductivity than is the case with conventional sintering processes. However, it is important to maintain a nearly uniform temperature within the sealable vessel 600, otherwise the molten intermediates may be transported to another location in the sealable vessel 600 that is hotter or colder, and AlN may deposit there instead of in the ceramic composite. For example, Peters [Journal of Crystal Growth 104, 411 (1990)] showed that AlN single crystals can form on the hottest surface in a pressure vessel by conversion of metallic Al to AlN, in conjunction with macroscopic transport in supercritical ammonia with KNH2 present as a mineralizer. In the present disclosure, the macroscopic transport of molten Al is suppressed by maintaining a nearly isothermal environment with limited conductance within the sealable vessel 600, for example, by densely packing the aluminum-containing green body 609 within the sealable vessel 600, or by the use of rolled layers of composite (see green body 290A in FIG. 2A).
[0061] Additionally, without wishing to be bound by theory, the inventors believe that the getter metal nitride, if present, formed by reaction with supercritical ammonia from the getter metal reacts with the oxide on the surface of the aluminum-containing coating or particle: Be3N2+Al2O3=3BeO+2AlN Mg3N2+Al2O3=3MgO+2AlN 2ScN+Al2O3=Sc2O3+2AlN 2YN+Al2O3=Y2O3+2AlN If a getter metal is included within the aluminum-containing coating or particle, the resulting nitrides and oxides of the getter metal will likely remain within the resulting aluminum-containing ceramic matrix composite. If the getter metal is added in slight excess relative to the oxygen content in the aluminum-containing coating or particle, and the getter metal oxide has a higher thermal conductivity than Al2O3 (e.g., BeO or MgO), the thermal conductivity of the aluminum-containing ceramic matrix composite can be significantly improved by the addition of the getter metal.
[0062] After a predetermined time at the second temperature, the sealable container can be cooled, the ammonia released therefrom, and removed from the pressure vessel and opened. The aluminum-containing ceramic matrix composite can then be removed. In certain embodiments, individual granules, pellets, or tablets of the ceramic matrix composite are prepared by one or more of jaw milling, cone milling, hammer milling, milling, grinding, vibrating, and other forms of comminution known in the art. In certain embodiments, the individual granules, pellets, or tablets of the ceramic matrix composite are subjected to one or more further processes, such as dicing, sawing, grinding, double-sided lapping, polishing, tumbling, etching, and the like, to form a finished aluminum-containing ceramic matrix composite part.
[0063] The finished aluminum-containing ceramic matrix composite part can include at least one, at least two, or at least three phosphor compositions having a phosphor to AlN volume ratio of between about 1% and about 99%, between about 5% and about 95%, between about 10% and about 90%, or between about 20% and about 80% in a matrix consisting essentially of AlN. The finished aluminum-containing ceramic matrix composite part can have a porosity of between about 1% and about 50%, between about 2% and about 25%, between about 3% and about 20%, or between about 4% and about 10%. The finished aluminum-containing ceramic matrix composite part may have a thermal conductivity of between about 1 W / (m·K) and about 320 W / (m·K), between about 5 W / (m·K) and about 260 W / (m·K), between about 10 W / (m·K) and about 170 W / (m·K), or between about 20 W / (m·K) and about 100 W / (m·K). At least one, at least two, or at least three phosphor components in the finished aluminum-containing ceramic matrix composite part may have an internal quantum efficiency of at least about 30%, at least about 50%, at least about 75%, or at least about 90%. At least one, at least two, or at least three phosphor components in the finished aluminum-containing ceramic matrix composite part may have a luminous efficiency of at least about 30 lumens / watt, at least about 50 lumens / watt, at least about 100 lumens / watt, or at least about 150 lumens / watt. The aluminum nitride matrix material has a wavelength of about 100 cm at wavelengths between about 400 nanometers and about 750 nanometers. -1 Less than 50cm -1 Less than 20cm -1 Less than 10cm -1 Less than 5cm -1 Less than 2cm -1 Less than or about 1 cm -1 It may have an optical absorption coefficient of less than .
[0064] In certain embodiments, one or more of the phosphor compositions in the phosphor particles 101 may have significant solubility in the supercritical fluid composition that includes ammonia and a mineralizer composition. In such cases, in addition to the bonds between the phosphor particles and the AlN matrix, direct bonds between adjacent phosphor particles may be formed. For example, β-SiAlON:Eu 2+ , α-SiAlON:Eu 2+ , and CaAlSiN3:Eu 2+ For example, direct "sintering" can occur within and between nitride and oxynitride phosphor compositions such as AlN. In certain embodiments, the methods described in this disclosure can be used to produce phosphor-containing ceramic composites that are completely free of AlN. For example, a green body containing phosphor particles and additives can be produced by slip casting (FIG. 2A) and / or tableting (FIG. 5A) processes. After placement, the phosphor-containing green body can be placed in a sealable container (FIG. 6) with a mineralizer and, optionally, one or more of a getter material to remove surface oxides and a catalyst to convert H2 and N2 to NH3. After pumping, purging, adding NH3, and sealing, the sealable container can then be heated to a first temperature, e.g., between about 100° C. and about 400° C., and a second temperature, e.g., between about 400° C. and about 1000° C., as described above. The resulting phosphor-ceramic composite can be processed into a finished phosphor-ceramic composite part, as described above.
[0065] The finished aluminum-containing nitride ceramic matrix composite formed by one or more of the processes described above can be incorporated into a package with one or more of a laser diode and a light emitting diode. For example, violet or blue light from a laser diode or light emitting diode can illuminate or focus the aluminum-containing nitride ceramic matrix composite, resulting in the emission of blue, green, yellow, orange, and / or red light. In certain embodiments, the overall light output from the package, including the reflected light from the laser diode or light emitting diode and the light emitted by the phosphor, is white light. In certain embodiments, the white light has a color rendering index (CRI) of greater than about 80, greater than about 85, greater than about 90, greater than about 95, greater than about 98, or greater than about 99. In certain embodiments, the white light has a CRI R9 value of greater than about 50, greater than about 70, greater than about 80, or greater than about 90. The aluminum-containing nitride ceramic matrix composite can be coupled to a heat sink to dissipate heat generated during light conversion within the phosphor. In certain embodiments, one or more aluminum-containing ceramic matrix composite components are incorporated into a surface mounted device (SMD), which can be advantageously provided as a compact, cost-effective package.
[0066] Example Method(s) The methods described herein provide a means for producing high performance ceramic matrix composites containing phosphor compositions that have high thermal conductivity and high internal quantum efficiency.
[0067] Example 1 Aluminum powders having a particle size between about 10 micrometers and about 100 micrometers are prepared by filing high purity aluminum ingots in a glove box with oxygen and moisture concentrations less than 1 ppm. Green β-SiAlON:Eu powders, each having a particle size between about 5 micrometers and about 50 micrometers, are prepared by filing high purity aluminum ingots in a glove box with oxygen and moisture concentrations less than 1 ppm. 2+ Phosphor and red CaAlSiN3:Eu 2+The phosphor is prepared by preparing a blend of aluminum, green phosphor, and red phosphor in a weight ratio of 5:1:2 in a mortar and pestle in a glove box. The powder blend is pressed at a pressure of about 50 MPa into a disk with a diameter of 6 millimeters and a thickness of 1 mm, with a green porosity between about 10% and about 40%. The disk is placed in a silver-containing capsule with an outer diameter of 1.00 inches (2.54 cm) and a length of 5.25 inches (13.34 cm) in the glove box, and the capsule is welded closed using an orbital welder. 4.0 g of KN3 powder is placed in a stainless steel mineralizer container similar to that shown diagrammatically in FIG. 9 in the glove box, and the container is closed with a ConFlat® (CF) flange. The mineralizer container with attached flash container similar to that shown diagrammatically in FIG. 9 and the capsule are removed from the glove box. The mineralizer vessel is cooled to dry ice temperature and filled with 10.0 g of ammonia, the flash vessel is cooled to dry ice temperature and filled with 9.0 g of ammonia, then both vessels are warmed to room temperature and connected to the capsule. The capsule is cooled to dry ice temperature, the valve between the mineralizer vessel and the capsule is opened, and the liquid ammonia mineralizer solution is transferred to the capsule. The outlet valve of the mineralizer vessel is then closed, the valve between the flash vessel and the mineralizer vessel is opened, and liquid ammonia is transferred from the flash vessel to the mineralizer vessel. The flash vessel is gently warmed with a heat gun to drive the remaining liquid ammonia into the mineralizer vessel. The valve between the mineralizer vessel and the capsule is reopened, and the remaining ammonia is transferred to the capsule. The fill tube on the capsule is then welded closed and cut, and the capsule is loaded into an internally heated high pressure device.
[0068] The high pressure is ramped up to a temperature of 675 °C over 8 hours and held at this temperature for 24 hours without any intentional temperature gradient, then cooled. Ammonia is removed from the capsule, the capsule is removed from the high pressure apparatus, opened, and the disks are extracted. The disks are examined by optical microscopy, scanning electron microscopy (SEM) / energy dispersive spectroscopy (EDS), and powder X-ray diffraction, their porosity is measured by mercury intrusion, their thermal diffusivity is measured by laser flash method, their specific heat capacity is measured using a differential scanning calorimeter, and their thermal conductivity is calculated as the product of thermal diffusivity, specific heat capacity, and bulk density. X-ray diffraction shows the presence of the phosphor composition, AlN, with no additional phases above the detection limit. SEM images of fracture cross sections show that both types of phosphor particles are wetted by AlN, which forms a porous matrix. The porosity of the disks is measured to be 30%. The thermal conductivity is 30 W m -1 ·K -1 is measured.
[0069] While the above is a complete description of specific embodiments, various modifications, alternative constructions, and equivalents may be used. Accordingly, the above description and illustrations should not be construed as limiting the scope of the disclosure, which is defined by the appended claims. [Explanation of symbols]
[0070] 101 Phosphor particles 103, 355 Aluminum-containing coatings 105 Aluminum-containing particles 200 Processing System / Autoclave 201, 302 Slurry 202 Career Film 205 Upper heater 207 Lower Heater 209 Upper Insulator / Heater 211 Carrier film supply reel / liner 212 Carrier film take-up reel 213 Unfired body take-up reel 217 Autoclave Cap 251 Mixed Components 253 Mixed Devices 254 Slurry Tank 255 Green Body Forming Assembly 259 Homogenizing Device 260 Pump 261 Carrier Film Supply Assembly 265 Input Tank 266 Doctor Blade 267 Heating Devices 271 Stencil Mask 272 Opening 290, 290A Unfired 290B Unfired disc 303 Aluminum-containing layer 300 Internally heated high pressure device 307 Capsules 309 Pressure Transmission Medium 311 End plug 331 Bottom Heater 341 Top heater 357 Pore 359 Aluminum-containing composite materials 402 Aluminum-containing foil or coating 403 Dry Slurry Layer 501 Material supply device 505 Mixing and Compression Components 531 Lower Piston 533 Upper Piston 535 tablets 541 Lower Cam 543 Upper Cam 547 Die Cavity 549 Granules 551 Tableting Device 600 Sealable containers 609 Aluminum-containing unsintered bodies 621 Internal 623 Upper Entrance 625 Lower Entrance
Claims
1. 1. A method of forming an aluminum-containing nitride ceramic matrix composite, comprising: forming at least one green body comprising a phosphor powder and an aluminum-containing composition, the at least one green body is characterized by a porosity of between about 10% and about 80%; and the phosphor powder comprises at least one phosphor composition, and the phosphor powder particles have a D50 diameter between about 100 nanometers and about 500 micrometers; The process and heating the sealable container to a temperature of between about 400° C. and about 800° C. and a pressure of between about 10 MPa and about 1000 MPa; placing the at least one green body, ammonia, and a mineralizer composition in the sealable container prior to applying heat and pressure to the sealable container; the aluminum-containing composition has a purity, based on the metal, of between about 90% and about 99.9999%; the percentage of the free volume in the sealable container filled with liquid ammonia before heating and pressurizing the sealable container is between about 10% and about 95%; and heating the sealable container includes heating the sealable container for a first period of time to form an aluminum-containing nitride ceramic matrix composite characterized by a phosphor to aluminum nitride (AlN) volume ratio of between about 1% and about 99%, a porosity of between about 1% and about 50%, and a thermal conductivity of between about 1 W / (m·K) and about 320 W / (m·K); Process and A method comprising:
2. The phosphor composition is 3 A 5 O 12 : Ce 3+ , Lu 3 A 5 O 12 : Ce 3+ , (Y, Gd, Tb, Sc, Lu, La) 3 (Al, Ga, In) 5 O 12 : Ce 3+ , β-SiAlON:Eu 2+ , α-SiAlON:Eu 2+ , SrSi 2 O 2 N 2 :Eu 2+ , SrGa 2 S 4 :Eu 2+ , SrS:Eu 2+ , and CaAlSiN 3 :Eu 2+ The method of claim 1 , comprising one or more of:
3. 10. The method of claim 1, wherein the powder particles are characterized by a D50 diameter of between about 1 micrometer and about 200 micrometers.
4. 10. The method of claim 1, wherein the aluminum-containing composition comprises a coating having a thickness of between about 50 nanometers and about 100 micrometers disposed on at least a portion of the green body.
5. 10. The method of claim 1, wherein the aluminum-containing composition further comprises a getter composition, the getter composition comprising one or more of beryllium, magnesium, calcium, strontium, barium, scandium, titanium, vanadium, chromium, yttrium, zirconium, niobium, a rare earth metal, hafnium, tantalum, or tungsten.
6. The method of claim 5 , wherein the getter composition comprises one or more of beryllium, magnesium, scandium, or yttrium.
7. 10. The method of claim 1, wherein the green body further comprises aluminum-containing particles, the aluminum-containing particles comprising one or more of aluminum nitride powder, aluminum nitride grit, aluminum powder, aluminum flakes, aluminum pellets, aluminum shavings, aluminum grit, or aluminum evaporation slag.
8. 8. The method of claim 7, wherein the aluminum-containing particles are characterized by a maximum dimension between about 1 micrometer and about 10 millimeters.
9. The method of claim 1 , further comprising forming the at least one green body by a tape casting, screen printing, or doctor blading technique.
10. The method of claim 9 , wherein the tape casting, screen printing, or doctor blading technique further comprises the use of a stencil mask.
11. The method of claim 1 , wherein the green body is formed by one or more of a granulation, pelletizing, or tableting process.
12. forming supercritical ammonia in the sealable container while heating the sealable container; and heating the green body to above about 600° C. prior to exposing the green body to supercritical ammonia. The method of claim 1 further comprising:
13. 2. The method of claim 1, wherein the mineralizer comprises one or more of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, or Ba, or hydrides, amides, imides, amide-imides, nitrides, or azides thereof.
14. 14. The method of claim 13, wherein the mineralizer comprises at least one of sodium azide and potassium azide.
15. 14. The method of claim 13, wherein the sealable container further comprises a metal composition prior to heating the sealable container, and the metal composition disposed within the sealable container has a composition and amount such that nitrogen gas species are produced by decomposition of an azide mineralizer and hydrogen gas species are produced by reaction of at least the metal with supercritical ammonia in a molar ratio of about 1:
3.
16. The mineralizer is NH 4 F, N.H. 4 Cl, NH 4 Br, NH 4 I, AlF 3 , AlCl 3 , AlBr 3 , ALI 3 , or F, Cl, Br, I, HF, HCl, HBr, HI, Al, AlN, and NH 3 13. The method of claim 1, further comprising reacting any one or more of the compounds of formula (I) and formula (II).
17. The method of claim 1 , wherein the aluminum-containing nitride ceramic matrix composite is characterized by a porosity of between about 3% and about 20%.
18. The method of claim 1 , wherein the aluminum-containing nitride ceramic matrix composite material is characterized by a thermal conductivity of between about 10 W / (m·K) and about 170 W / (m·K).
19. The method of claim 1 , wherein the aluminum-containing nitride ceramic matrix composite comprises at least two phosphor compositions.
20. The method of claim 1 , wherein the aluminum-containing nitride ceramic matrix composite comprises at least one phosphor composition having an internal quantum efficiency of at least about 30%.
Citation Information
Patent Citations
Electroluminescent phosphor, its manufacturing method and device using the same
JP2006233134A
Ceramic composite
JP2011012215A
Inorganic molding article for color conversion, method of manufacturing the same and light-emitting device